Positive electrode active material, electrochemical device, and electronic device

A structured positive electrode active material with manganese-rich and manganese-poor gradients in secondary particles addresses manganese precipitation issues, enhancing energy density and cycle stability in batteries.

JP2024149363AInactive Publication Date: 2024-10-18AESC JAPAN LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023208541
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-07
Filing Date
2023-12-11
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Lithium manganese phosphate suffers from slow lithium ion migration, large charge polarization, and manganese precipitation during charging and discharging, leading to energy loss and poor cycle stability in batteries.

Method used

A positive electrode active material with a unique structure comprising secondary particles with manganese-rich primary particles inside and manganese-poor primary particles outside, forming a gradient, which reduces manganese dissolution and improves interfacial resistance.

Benefits of technology

Enhances energy density, cycle stability, and rate performance by mitigating manganese dissolution and reducing interfacial reactions, resulting in improved battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024149363000001_ABST
    Figure 2024149363000001_ABST
Patent Text Reader

Abstract

To provide a positive electrode active material.SOLUTION: A positive electrode active material includes a first lithium manganese iron phosphate in the form of primary particles inside secondary particles, and a second lithium manganese iron phosphate in the form of primary particles outside the secondary particles, the first lithium manganese iron phosphate having a general chemical formula LixMnaFe1-a-a'M1a'PO4, and 0.9≤x≤1.10, 0.4≤a≤0.9, and 0.001≤a'≤0.02 are satisfied, the second lithium manganese iron phosphate in the form of primary particles having a general chemical formula LiyMnbFe1-b-b'M2b'PO4, and 0.9≤y≤1.10, 0<b≤0.6, and 0.001≤b'≤0.02, and a>b are satisfied, and M1 and M2 are one or more of Mg, Ti, V, Ni, Co, and Al, respectively. The area ratio (S) of the first lithium manganese iron phosphate and the second lithium manganese iron phosphate satisfies S≥(0.4-b) / (a-0.4).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode active material, an electrochemical device, and an electronic device. [Background technology]

[0002] Lithium iron phosphate has the advantages of good structural stability, good temperature stability, good safety performance, and good cycle life, and its raw material resources are abundant. Therefore, the application of lithium iron phosphate in energy storage batteries and electric vehicle batteries is increasing. However, the plateau voltage of lithium iron phosphate is only 3.4V vs. Li / Li+, which limits the energy density. Lithium manganese phosphate has the same olivine structure as lithium iron phosphate. Compared with lithium iron phosphate, lithium manganese phosphate has a higher plateau voltage, but its inherent lithium ion solid phase migration speed is slow and its charging polarization is large.

[0003] In the related art, the energy density and electrical conductivity of lithium manganese phosphate or lithium iron phosphate are mainly improved by partially doping iron on the manganese sites of lithium manganese phosphate or partially replacing the manganese sites of lithium manganese phosphate with iron. However, the polarization problem caused by manganese is still serious. In addition, during the charge and discharge process, manganese in lithium iron phosphate is prone to precipitate and form manganese fluoride on the surface of the positive electrode, or dissolve in the electrolyte and precipitate on the negative electrode. This leads to energy loss during the battery cycle. Therefore, the preparation of lithium manganese iron phosphate materials with high capacity, low internal resistance, and good stability is very important for the research and development of electrochemical devices. Summary of the Invention [Problem to be solved by the invention]

[0004] In view of the drawbacks in the related art, an object of the present invention is to provide a positive electrode active material, a positive electrode sheet, an electrochemical device, and an electronic device. The positive electrode active material provided by the present invention is beneficial to reducing the dissolution of metal manganese during cycling, and further improving the cycle stability and energy density of the electrochemical device.

Means for Solving the Problems

[0005] To solve the problems in the related art, a first aspect of the present invention provides a positive electrode active material containing secondary particles. Inside the secondary particles, the first lithium iron manganese phosphate in the form of primary particles is included, and outside the secondary particles, the second lithium iron manganese phosphate in the form of primary particles is included.

[0006] The general chemical formula of the first lithium iron manganese phosphate is Li x Mn a Fe 1-a-a’ M1 a’ PO4, where 0.9 ≦ x ≦ 1.10, 0.4 ≦ a ≦ 0.9, and 0.001 ≦ a' ≦ 0.02. The general chemical formula of the second lithium iron manganese phosphate in the form of primary particles is Li y Mn b Fe 1-b-b’ M2 b’ PO4, where 0.9 ≦ y ≦ 1.10, 0 < b ≦ 0.6, and 0.001 ≦ b' ≦ 0.02, a > b, and M1 and M2 are each one or more of Mg, Ti, V, Ni, Co, and Al. The area ratio S of the first lithium iron manganese phosphate to the second lithium iron manganese phosphate satisfies S ≧ (0.4 - b) / (a - 0.4).

[0007] A second aspect of the present invention provides a positive electrode sheet containing the above-mentioned positive electrode active material.

[0008] A third aspect of the present invention provides an electrochemical device containing the above-mentioned positive electrode sheet.

[0009] A fourth aspect of the present invention provides an electronic device containing the above-mentioned electrochemical device.

[0010] All reagents and raw materials used in the present invention are commercially available. Effect of the Invention

[0011] The positive and progressive effects provided by the present invention include:

[0012] (1) In the present invention, the secondary particles of lithium manganese iron phosphate with a special structure are used as the positive electrode active material. In the lithium manganese iron phosphate, from the inside to the outside, the manganese element content gradient decreases and the iron element content gradient increases. This is beneficial to reduce the dissolution problem of metal manganese during the lithium manganese iron phosphate cycle. The internal resistance of the interface can also be improved, which improves the rate performance of the positive electrode active material, and enhances the energy density and cycle stability.

[0013] (2) The secondary particle structure can prevent the electrolyte from penetrating into the inside of the particle, improving the cycle stability inside the particle. The inside is manganese-rich lithium manganese iron phosphate in the form of primary particles, and the outside is manganese-poor lithium manganese iron phosphate in the form of primary particles, so the positive electrode has fewer interfacial side reactions during cycling and a slower Mn dissolution rate. This significantly improves cycle performance and storage performance. [Brief description of the drawings]

[0014] [Figure 1] FIG. 2 is a schematic structural diagram of a positive electrode active material (reference numeral 1 is a first lithium manganese iron phosphate in the form of primary particles, and reference numeral 2 is a second lithium manganese iron phosphate in the form of primary particles). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present invention will be further described in conjunction with the following examples, but the present invention is not limited to the scope of the examples. For the experimental methods not specifying specific conditions in the following examples, they are selected based on the conventional methods and conditions or based on the product specifications.

[0016] Positive electrode active material

[0017] The present invention provides a positive electrode active material containing secondary particles. Inside the secondary particles, the first lithium iron manganese phosphate in the form of primary particles is included, and outside the secondary particles, the second lithium iron manganese phosphate in the form of primary particles is included.

[0018] The general chemical formula of the first lithium iron manganese phosphate is Li x Mn a Fe 1-a-a’ M1 a’ PO4, where 0.9 ≦ x ≦ 1.10, 0.4 ≦ a ≦ 0.9, and 0.001 ≦ a' ≦ 0.02. The general chemical formula of the second lithium iron manganese phosphate in the form of primary particles is Li y Mn b Fe 1-b-b’ M2 b’ PO4, where 0.9 ≦ y ≦ 1.10, 0 < b ≦ 0.6, and 0.001 ≦ b' ≦ 0.02, a > b, and M1 and M2 are each one or more of Mg, Ti, V, Ni, Co, and Al. The area ratio S of the first lithium iron manganese phosphate to the second lithium iron manganese phosphate satisfies S ≧ (0.4 - b) / (a - 0.4).

[0019] In order to overcome the energy loss due to the easy dissolution of manganese during the charge and discharge process of the battery in the related art, through extensive research, the present invention has found that by adjusting the area ratio of the first lithium iron manganese phosphate to the second lithium iron manganese phosphate, the energy density and cycle performance of the positive electrode material can be improved. When the area ratio satisfies specific conditions, its electrical characteristics become better.

[0020] In the present invention, the area ratio refers to the cross-sectional area ratio of the first lithium manganese iron phosphate and the second lithium manganese iron phosphate in the CPSEM.

[0021] In the present invention, the secondary particles are formed by agglomeration of primary particles.

[0022] In the present invention, the mass ratio range of the first lithium iron manganese phosphate to the second lithium iron manganese phosphate may be (0.4-36.5:1).

[0023] In some embodiments, the mass ratio range of the first lithium iron manganese phosphate to the second lithium iron manganese phosphate may be 0.4:1, 1:1, 4.4:1, 11.2:1, 31.6:1, or 36.5:1.

[0024] In some embodiments, in the general chemical formula of the first lithium iron manganese phosphate, the value range of a is 0.6≦a≦0.8.

[0025] In some embodiments, in the general formula of the second lithium iron manganese phosphate, the value of b ranges from 0 <b<0.4である。

[0026] In some embodiments, in the general formula of the second lithium iron manganese phosphate, the value range of b is 0.2≦b<0.4.

[0027] The first lithium manganese iron phosphate is a manganese-rich lithium manganese iron phosphate. If the Mn content is too low, the Mn plateau potential cannot be realized, leading to low energy density; if the Mn content is too high, the LMFP has poor conductivity, low capacity, and low energy density. The first lithium manganese iron phosphate is a manganese-poor lithium manganese iron phosphate. If the Mn content is too low, the Mn plateau potential cannot be realized, leading to low energy density; if the Mn content is too high, the external Mn dissolution becomes serious, leading to poor cycle performance.

[0028] In some embodiments, the area ratio S of the first lithium iron manganese phosphate to the second lithium iron manganese phosphate satisfies the following: when 0 < b < 0.55 and 0.75 < a ≤ 0.9, (0.55 - b) / (a - 0.55) ≤ S ≤ (0.75 - b) / (a - 0.75).

[0029] In some embodiments, the area ratio S of the first lithium iron manganese phosphate to the second lithium iron manganese phosphate satisfies the following: when 0 < b < 0.5 and 0.5 < a ≤ 0.9, S ≥ (0.5 - b) / (a - 0.5).

[0030] In some embodiments, the area ratio S of the first lithium iron manganese phosphate to the second lithium iron manganese phosphate preferably satisfies b / a ≤ S ≤ 30b / a and preferably satisfies 7b / 3a ≤ S ≤ 15b / a.

[0031] In some embodiments, the area ratio S of the first lithium iron manganese phosphate to the second lithium iron manganese phosphate is preferably [(0.4 - b) / (a - 0.4)] ≤ S ≤ [(0.7 - b) / (a - 0.7)] when 0 < b < 0.4 and a > 0.7.

[0032] In some embodiments, the area ratio S of the first lithium iron manganese phosphate to the second lithium iron manganese phosphate is preferably [(0.5 - b) / (a - 0.5)] ≤ S ≤ [(0.7 - b) / (a - 0.7)] when 0 < b < 0.5 and a > 0.7.

[0033] In the present invention, the secondary particles are obtained by aggregation of primary particles. In the primary particles, there are particles rich in manganese and particles poor in manganese. During aggregation, the particles poor in manganese are distributed on the outside, and the particles rich in manganese are distributed on the inside, forming secondary particles with a poor manganese content on the outside and secondary particles with a rich manganese content on the inside.

[0034] In the present invention, in CPSEM, the number of primary particles of the secondary particles is 10 particles / μm2 ~30 particles / μm 2 It is.

[0035] In some specific embodiments, the primary particle count of secondary particles in a CPSEM is less than 20 particles / μm 2 It is.

[0036] The surfaces of the primary particles are preferably further coated with carbon.

[0037] Here, the amount of carbon coating is 1% to 3%, and the percentage in the amount of coating is the percentage of the mass of carbon in the mass of the primary particles.

[0038] In some particular embodiments, the carbon coverage of the first lithium iron manganese phosphate and the second lithium iron manganese phosphate are both 1.8%.

[0039] In the present invention, the method for preparing secondary particles preferably includes the following steps:

[0040] (1) Synthesis of the first lithium manganese iron phosphate precursor (MFP1): Manganese nitrate and iron nitrate are dissolved in ethanol in a specific molar ratio, and then the ethanol solution of the metal salts is poured into a phosphoric acid solution and reacted for 4 hours under stirring at 40°C, filtered, and then washed to obtain MFP1.

[0041] (2) The raw material solution of the second lithium manganese iron phosphate precursor (MFP2) is mixed with MFP1, ammonia water is added to control the pH=2, and the mixture is reacted by stirring at 50°C, filtered, and calcined in air at 550°C for 1 hour to obtain MFP1@MFP2.

[0042] (3) MFP1@MFP2 is mixed with a lithium source, a carbon source, and a doped metal source, wet-ground in water, spray-dried, and calcined at 650°C for 15 hours to obtain the product.

[0043] In step (1), the molar ratio of manganese nitrate to iron nitrate may be a:(1 - a - a'), where 0.4 ≦ a ≦ 0.9 and 0.001 ≦ a' ≦ 0.02.

[0044] In step (2), the raw material solution of MFP2 is obtained by mixing manganese nitrate, iron nitrate, and phosphoric acid in a specific molar ratio and dissolving them in water. The molar ratio of manganese nitrate, iron nitrate, and phosphoric acid is preferably b:(1 - b - b'):1, where 0 < b ≦ 0.6 and 0.001 ≦ b' ≦ 0.02.

[0045] In step (3), the molar ratio of the lithium source to MFP1@MFP2 may be 1.05:1.

[0046] In step (3), the addition amount of the carbon source may be 6% - 12% of the total mass of the lithium source and MFP1@MFP2.

[0047] Positive electrode sheet

[0048] The second aspect of the present invention provides a positive electrode sheet containing the above-described positive electrode active material.

[0049] The positive electrode sheet generally includes a positive electrode active material, a conductive agent, a binder, and a positive electrode current collector. The types of the conductive agent and the binder are not particularly limited in the present invention and may be selected according to actual requirements.

[0050] As an example, the conductive agent may be conductive carbon black (SP).

[0051] The binder may be polyvinylidene fluoride (PVDF).

[0052] The mass ratio of the positive electrode active material, the conductive agent, and the binder is (90 - 99):1:2, and may be, for example, 97:1.5:1.5.

[0053] Electrochemical device

[0054] A third aspect of the present invention provides an electrochemical device including the positive electrode sheet described above.

[0055] In the present invention, the electrochemical device may be a battery. The battery includes a positive electrode sheet, a negative electrode sheet facing the positive electrode sheet, a separator disposed between the positive electrode sheet and the negative electrode sheet, and an electrolyte. The positive electrode sheet is as described above. Furthermore, the battery may optionally include a battery case for housing the positive electrode sheet, the negative electrode sheet, and the separator, and a sealing member for sealing the battery case.

[0056] Negative electrode sheet

[0057] In the battery, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer formed on the negative electrode current collector. The negative electrode active material includes a negative electrode active material and, optionally, a binder and a conductive agent, and the amount of the binder and conductive agent may be adjusted within 1% to 50% of the total amount of the negative electrode active material layer according to different requirements.

[0058] The negative electrode active material described in the present invention is a material capable of intercalating and deintercalating lithium. The negative electrode active material includes, but is not limited to, carbon materials such as crystalline carbon (natural graphite, artificial graphite), amorphous carbon, carbon-coated graphite, and resin-coated graphite, oxide materials such as indium oxide, silicon oxide, tin oxide, lithium titanate, zinc oxide, and lithium oxide, or lithium metal or metal materials capable of forming an alloy with lithium. Here, examples of metal materials capable of forming an alloy with lithium include Cu, Sn, Si, Co, Mn, Fe, Sb, and Ag. Binary alloys or ternary alloys containing these metals and lithium can also be used as the negative electrode active material. These negative electrode active materials may be used alone or in combination of two or more. From the viewpoint of increasing the energy density, a carbon material such as graphite may be used in combination with a Si-based material such as Si, a Si alloy, and a Si oxide.

[0059] Here, the conductive agent is a reagent used to ensure that the electrode exhibits good charge and discharge performance. The conductive agent may include, for example, graphite materials such as natural graphite and artificial graphite, carbon black materials such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black, conductive fibers such as carbon fibers and metal fibers, metal powders such as carbon fluoride powder, aluminum powder, and nickel powder, conductive whiskers such as metal powder, zinc oxide, and potassium titanate, and conductive metal oxides such as titanium dioxide and polyphenylene derivatives.

[0060] Here, the binder is a component that promotes the bond between the active material and the conductive agent and promotes the bond between the active material and the current collector. The binder may generally be selected from polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, fluororubber, and various copolymers.

[0061] Here, the negative electrode current collector as a substrate supporting the electrode active material is usually a metal foil having a thickness of 3 microns to 500 microns. There is no particular limitation on the material of the current collector as long as the material has high conductivity and does not cause a chemical reaction in the secondary battery system. For example, the material may be a foil material surface-treated with nickel, titanium, aluminum, silver, stainless steel, carbon, etc. The negative electrode current collector usually has a smooth surface, but fine lines may be formed on the surface to improve the adhesion between the negative electrode active material and the current collector. The negative electrode current collector may be one or a combination of various forms such as a foil, a film, a mesh, a porous material, a foam, and a nonwoven fabric.

[0062] Separator

[0063] The separator is placed between the positive electrode sheet and the negative electrode sheet, and is usually an insulating film having high ion permeability and high mechanical strength. The separator typically has a thickness of 9 μm to 18 μm, a pore size of 5 μm to 300 μm, an air permeability of 180 s / 100 mL to 380 s / 100 mL, and a porosity of 30% to 50%. As the separator, a sheet or nonwoven fabric made of an olefin polymer such as polypropylene, which is chemically resistant and hydrophobic, and glass fiber or polyethylene is used.

[0064] electrolyte

[0065] The electrolyte used in the lithium ion battery usually contains a non-aqueous solvent, a lithium salt, and an additive.

[0066] Here, the non-aqueous solvent may be a conventional non-aqueous solvent in the technical field, preferably an ester-based solvent, more preferably a carbonate-based solvent, where the carbonate-based solvent is preferably selected from at least one of ethylene carbonate, dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC).

[0067] Here, the lithium salt may be selected from at least one of LiPF6, LiBF4, LiN(SO2F)2 (abbreviated as LiFSI), LiClO4, LiAsF6, LiB(C2O4)2 (abbreviated as LiBOB), LiBF2(C2O4) (abbreviated as LiDFOB), LiN(SO2RF)2, and LiN(SO2F)(SO2RF). The content of the lithium salt in the electrolyte is preferably 5% to 20%.

[0068] Here, the additive is preferably selected from at least one of vinylene carbonate (VC), fluoroethylene carbonate (FEC), vinylethylene carbonate (VEC), vinyl sulfate (DTD), vinylene sulfate, 1,3-propane sultone (PS), propene sultone, 1,4-butane sultone. A typical amount of additive used in the electrolyte is 1% to 4% of the electrolyte, such as 2% of the electrolyte.

[0069] In the present invention, the shape of the battery is not particularly limited, and the shape may be cylindrical, rectangular, or any other shape.

[0070] electronic equipment

[0071] The electronic device of the present invention includes the electrochemical device according to the third embodiment.

[0072] By way of example, the electronic device in the present invention may be, but is not limited to, a mobile device (e.g., a mobile phone, a tablet computer, a notebook computer, a video recorder, a portable printer / copier, etc.), an electric vehicle (e.g., a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric locomotive, a marine vessel, a satellite, an energy storage system, a backup power source, etc.

[0073] Based on common general knowledge in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain preferred embodiments of the present invention.

[0074] Example 1

[0075] (1) Preparation of positive electrode sheet

[0076] The positive electrode active material, Super P, and PVDF were mixed in a mass ratio of 97:1.5:1.5. The positive electrode active material was secondary particles of LiMn 0.75 Fe 0.25 PO4@C and LiMn 0.25 Fe 0.75PO4@C, and S=2.7. The carbon coating amount of the first lithium manganese iron phosphate and the second lithium manganese iron phosphate was both 1.5%. Nitrogen methyl pyrrolidone (NMP) was gradually added with high speed stirring to prepare a positive electrode slurry of a specific viscosity. Next, the prepared slurry was uniformly coated on an aluminum foil and dried at 120°C for 10 minutes in a blower drying oven. Finally, the dried electrode sheet was rolled and cut to prepare a positive electrode sheet. Here, the structure of the positive electrode active material is illustrated.

[0077] (2) Preparation of negative electrode sheet

[0078] The negative electrode active material graphite, conductive agent acetylene black, thickener sodium carboxymethylcellulose, and binder styrene-butadiene rubber were mixed in a mass ratio of 97:1:1:1, and deionized water was added to obtain a negative electrode slurry under the action of a vacuum mixer. The negative electrode slurry was uniformly coated on a copper foil current collector with a thickness of 8 μm, dried at room temperature, transferred to an oven for drying, and then cold pressed and slit to obtain a negative electrode sheet.

[0079] (3) Preparation of electrolyte

[0080] The organic solvent was a mixture of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC), with a volume ratio of EC, DMC, and EMC of 3:3.5:3.5. In an argon atmosphere glove box with a moisture content of less than 10 ppm, completely dried lithium ion salt (LiPF6) was dissolved in the above organic solvent and mixed uniformly to obtain an electrolyte solution, with a LiPF6 concentration of 1 mol / L.

[0081] (4) Preparation of the separator

[0082] A 12 μm thick polypropylene separator was chosen.

[0083] (5) Battery construction

[0084] The positive electrode sheet, separator, and artificial graphite negative electrode sheet obtained above were stacked in order so that the separator was placed between the positive electrode sheet and the negative electrode sheet for insulation. Then, it was covered with an aluminum-plastic film, transferred to a vacuum oven at 120°C for drying, and sealed after injecting 3.0g / Ah of electrolyte. After standing, hot pressing, cold pressing, 4.5V molding, fixing, screening, and other processes, a pouch battery (i.e., a lithium-ion battery) with a capacity of 1Ah was finally obtained.

[0085] The parameter settings for Examples 2 to 16 and Comparative Examples 1 to 10 are as shown in Table 1.

[0086] Comparative Example 2

[0087] LiMn 0.75 Fe 0.245 Ti 0.005 PO4@C and LiMn 0.25 Fe 0.745 Ti 0.005 Only physical mixing of PO4@C was performed.

[0088] Example of effect

[0089] (1) Test of the area ratio (S) of the first lithium manganese iron phosphate to the second lithium manganese iron phosphate: the electrode sheet was cut by CP and photographed with SEM and EDS. The first lithium manganese iron phosphate and the second lithium manganese iron phosphate in the form of primary particles were confirmed in the SEM and EDS images, and then the particle areas were statistically analyzed with Image J.

[0090] (2) Energy density test: Charge and discharge were performed at 25° C., 0.33 C, 2.5 V to 4.2 V (charge cutoff current: 0.05 C), and the discharge energy was divided by the mass of the positive electrode active material to obtain the energy density.

[0091] (3) Cycle test: 500 cycles of charge and discharge were performed at 1C at 45° C. in the range of 2.5 V to 4.2 V, and the capacity ratio of the 500th cycle to the 1st cycle was recorded as the capacity retention rate.

[0092] [Table 1] JPEG2024149363000003.jpg243166JPEG2024149363000004.jpg243166JPEG2024149363000005.jpg93166

[0093] [Table 2]

[0094] From the data in Table 2, it can be seen that when the positive electrode active materials of Examples 1 to 16 are applied to batteries, the energy density exceeds 461 Wh / kg in all cases, and the capacity retention rate after 500 charge / discharge cycles at 1C exceeds 91.5%, indicating that good electrochemical performance can be obtained.

[0095] Compared with the examples, Comparative Example 1 has only the first lithium manganese iron phosphate, and there is no gradient change of manganese element, which leads to poor cycle performance. This is because the Mn dissolution phenomenon in the lithium manganese iron phosphate is alleviated when a gradient structure with manganese-rich inside and manganese-poor outside exists. Comparative Example 1 does not have such a structure, so its cycle performance is poor.

[0096] Although the same positive electrode active material is provided in Comparative Example 2 as in Example 1, the particles are formed by physically mixing two positive electrode active materials, and therefore no gradient change of manganese element is formed, and the phenomenon of Mn dissolution cannot be alleviated, and the cycle performance is relatively poor.

[0097] The values ​​of a and b in Comparative Example 3 are not within the range of the present invention, and are the opposite of the manganese concentration of the present invention, with the structure being rich in manganese on the outside and poor in manganese on the inside. The active material has a high energy density, but does not have the structure provided by the present invention, and therefore cannot mitigate the Mn dissolution phenomenon. The cycle performance is far inferior to that of the Examples.

[0098] Comparative Examples 4 to 6 show that when the value of a or b is too high or too low, the effect on cycle performance is unclear, but it may affect the energy density to a certain extent. When the Mn content in the lithium manganese iron phosphate is 0.9 or more, the electrical properties are particularly poor, and the energy density of Comparative Example 5 is poor. Within a specific range, the higher the Mn content, the higher the energy density. In Comparative Examples 4 to 6, the Mn content is generally low, and therefore the energy density is low.

[0099] In Comparative Examples 7 to 9, the area ratio (S) is all less than (0.4-b) / (a-0.4), and the energy density is low. This is because the Mn content is lower than the expected range when the area ratio (S) of the first lithium manganese iron phosphate to the second lithium manganese iron phosphate is < the above formula, and therefore the energy density is low. The iron content in the second lithium manganese iron phosphate of Comparative Example 10 is not within the range provided by the present invention, and the cycle performance is poor. [Industrial Applicability]

[0100] Furthermore, the positive electrode active material, the electrochemical device, and the electronic device including the same of the present invention can be used in the electronics field, and has high industrial applicability.

[0101] In addition, it should be noted that each specific technical feature described in the above specific embodiments can be combined in any suitable manner unless inconsistent, and in order to avoid unnecessary repetition, the various possible combinations are not described herein.

[0102] Furthermore, the various embodiments of the present invention can be arbitrarily combined unless they are contrary to the spirit of the present invention, and such combinations should also be considered as part of the disclosure of the present invention. [Explanation of symbols]

[0103] 1: First lithium manganese iron phosphate 2: Secondary lithium manganese iron phosphate

Claims

1. A positive electrode active material including secondary particles, The inside of the secondary particles contains a first lithium manganese iron phosphate in the form of a primary particle, The secondary particles include a second lithium manganese iron phosphate in the form of the primary particles, The general chemical formula of the first lithium manganese iron phosphate is Li x Mn a Fe 1-a-a’ M1 a’ P.O. 4 where 0.9≦x≦1.10, 0.4≦a≦0.9, and 0.001≦a′≦0.02; The general chemical formula of the second lithium manganese iron phosphate is Li y Mn b Fe 1-b-b’ M2 b’ P.O. 4 where 0.9≦y≦1.10, 0<b≦0.6, and 0.001≦b′≦0.02, and a>b; M1 and M2 are each one or more of Mg, Ti, V, Ni, Co, and Al, and the area ratio of the first lithium manganese iron phosphate to the second lithium manganese iron phosphate satisfies S≧(0.4−b) / (a−0.4), where S is the area ratio; Cathode active material.

2. (a) in the general chemical formula of the first lithium manganese iron phosphate, the value range of a is 0.6≦a≦0.8; and (b) in the general chemical formula of the second lithium manganese iron phosphate, the value range of b is 0<b<0.4; At least one of the following conditions is satisfied: The positive electrode active material according to claim 1 .

3. The area ratio of the first lithium manganese iron phosphate to the second lithium manganese iron phosphate satisfies b / a≦S≦30b / a. The positive electrode active material according to claim 1 .

4. the area ratio of the first lithium manganese iron phosphate to the second lithium manganese iron phosphate satisfies (0.55-b) / (a-0.55)≦S≦(0.75-b) / (a-0.75) when 0<b<0.55 and 0.75<a≦0.9; The positive electrode active material according to claim 1 .

5. the area ratio of the first lithium manganese iron phosphate to the second lithium manganese iron phosphate satisfies S≧(0.5−b) / (a−0.5) when 0<b<0.5 and 0.5<a≦0.9; The positive electrode active material according to claim 1 .

6. the area ratio of the first lithium manganese iron phosphate to the second lithium manganese iron phosphate satisfies (0.4-b) / (a-0.4)≦S≦(0.7-b) / (a-0.7) when 0<b<0.4 and a>0.7; The positive electrode active material according to claim 1 .

7. the surface of the primary particle is coated with carbon, the amount of the carbon coated is 1% to 3%, and the percentage of the amount of the carbon coated is the percentage of the mass of the carbon in the mass of the primary particle; The positive electrode active material according to claim 1 .

8. A positive electrode sheet, a negative electrode sheet, and a separator Including, The positive electrode sheet comprises the positive electrode active material according to claim 1. Electrochemical devices.

9. The electrochemical device according to claim 8, electronic equipment.

10. A positive electrode sheet, a negative electrode sheet, and a separator Including, The positive electrode sheet contains the positive electrode active material according to claim 2. Electrochemical devices.

11. A positive electrode sheet, a negative electrode sheet, and a separator Including, The positive electrode sheet contains the positive electrode active material according to claim 3. Electrochemical devices.

12. A positive electrode sheet, a negative electrode sheet, and a separator Including, The positive electrode sheet contains the positive electrode active material according to claim 4. Electrochemical devices.

13. A positive electrode sheet, a negative electrode sheet, and a separator Including, The positive electrode sheet contains the positive electrode active material according to claim 5. Electrochemical devices.

14. A positive electrode sheet, a negative electrode sheet, and a separator Including, The positive electrode sheet contains the positive electrode active material according to claim 6. Electrochemical devices.

15. A positive electrode sheet, a negative electrode sheet, and a separator Including, The positive electrode sheet contains the positive electrode active material according to claim 7. Electrochemical devices.

Citation Information

Patent Citations

  • Secondary battery

    JP2013062082A

  • Positive electrode active material, nonaqueous electrolyte battery, and battery pack

    JP2014209463A

  • Positive electrode active material for lithium-ion secondary battery

    JP2022094473A

  • Battery positive electrode material, preparation method therefor, and application thereof