Membrane-electrode assembly and fuel cell
By optimizing the pore size distribution in the cathode catalyst and gas diffusion layers of a fuel cell, the fuel cell's power generation performance is enhanced through improved water discharge and gas diffusion.
Patent Information
- Application Number
- JP2024136965
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-10-18
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The performance of a fuel cell is not adequately maintained by simply setting the peak pore size of the gas diffusion layer to a range of 0.01 to 1 μm, as it does not effectively manage water discharge and gas diffusion.
The cathode catalyst layer has a peak in the logarithmic differential pore volume dV/d (logD) distribution in a pore diameter D range of 0.01 μm to 1 μm, while the gas diffusion layer laminated on the cathode has a peak in the range of 0.01 μm to 5 μm, with the pore diameter at the peak of the gas diffusion layer being larger than that of the catalyst layer, facilitating effective water discharge and improved gas diffusion.
This configuration enhances the power generation performance of the fuel cell by effectively discharging produced water and ensuring efficient gas diffusion, thereby improving reaction efficiency.
Smart Images

Figure 2024149802000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a membrane electrode assembly and a fuel cell. [Background technology]
[0002] A fuel cell includes, for example, a membrane electrode assembly having an electrolyte membrane and a pair of electrodes sandwiching the electrolyte membrane. Each of the pair of electrodes includes, in order from the electrolyte membrane side, a catalyst layer and a gas diffusion layer.
[0003] As a configuration of the gas diffusion layer, Patent Document 1 discloses a gas diffusion layer in which a conductive agent containing boron-modified carbon black is filled in a fibrous porous substrate, and in a Log differential pore volume distribution graph measured by mercury intrusion porosimetry, there is only one peak, and the peak exists in the pore diameter range of 0.01 to 1 μm. It is said that by having the pore diameter peak of the gas diffusion layer in the above range, water generated at the positive electrode (cathode) can be retained inside, and the solid polymer membrane can be kept wet. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2011-108441 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the performance of a fuel cell depends not only on the gas diffusion layer but also on the configuration of, for example, the catalyst layer, etc. Simply setting the pore size peak of the gas diffusion layer to the range of 0.01 to 1 μm may not be enough to maintain the required performance. [Means for solving the problem]
[0006] One aspect of the present disclosure relates to a membrane electrode assembly including a cathode having a cathode catalyst layer, an anode having an anode catalyst layer, an electrolyte membrane interposed between the cathode and the anode, and a pair of gas diffusion layers laminated on the cathode and the anode, respectively, on a surface opposite to the electrolyte membrane, wherein the cathode catalyst layer has a peak in a logarithmic differential pore volume dV / d (logD) distribution in which a pore diameter D is in a range of 0.01 μm to 1 μm, and the gas diffusion layer laminated on the cathode has a peak in a logarithmic differential pore volume dV / d (logD) distribution in which a pore diameter D is in a range of 0.01 μm to 5 μm, and a pore diameter D1 at the peak of the cathode catalyst layer is smaller than a pore diameter D2 at the peak of the gas diffusion layer laminated on the cathode.
[0007] Another aspect of the present disclosure relates to a fuel cell including the above-mentioned membrane electrode assembly. Effect of the Invention
[0008] According to the present disclosure, the power generation performance of a fuel cell can be improved. [Brief description of the drawings]
[0009] [Figure 1] 1 is a graph showing an example of logarithmic differential pore volume distribution measured by mercury intrusion porosimetry for a gas diffusion layer of a fuel cell. [Diagram 2] 1 is a cross-sectional view showing a schematic structure of a single cell of a fuel cell according to an embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The fuel cell according to an embodiment of the present disclosure includes a cathode having a cathode catalyst layer, an anode having an anode catalyst layer, an electrolyte membrane interposed between the cathode and the anode, and a pair of gas diffusion layers respectively laminated on the surfaces of the cathode and the anode opposite to the electrolyte membrane, and has a membrane electrode assembly (hereinafter, also referred to as "MEA"). The fuel cell may further include, for example, a conductive cathode separator in contact with the cathode and a conductive anode separator in contact with the anode. One cell may be constituted by the MEA and a pair of separators. By laminating a plurality of cells such that the cathode separator and the anode separator are adjacent to each other, a stack in which the cells are connected in series can be formed.
[0011] The cathode catalyst layer has a peak in the logarithmic differential pore volume dV / d(log D) distribution in the range where the pore diameter D is from 0.01 μm to 1 μm. On the other hand, the gas diffusion layer laminated on the cathode (hereinafter, also referred to as "cathode-side gas diffusion layer") has a peak in the logarithmic differential pore volume dV / d(log D) distribution in the range where the pore diameter D is from 0.01 μm to 5 μm. The pore diameter D1 at the peak of the cathode catalyst layer is smaller than the pore diameter D2 at the peak of the cathode-side gas diffusion layer (D1 < D2). D2 / D1 is, for example, 1.1 or more and 2.5 or less, and may be 1.1 or more and 1.7 or less, or 1.1 or more and 1.5 or less. D2 - D1 is, for example, 5 nm or more and 120 nm or less, and may be 5 nm or more and 60 nm or less, or 10 nm or more and 40 nm or less.
[0012] When the fuel cell generates electricity, water is generated at the cathode. The generated water is discharged from the cathode catalyst layer through the gas diffusion layer to the gas flow path. At this time, the generated water may be discharged in a form in which the water droplets combine and become larger as the water travels from the cathode catalyst layer to the cathode-side gas diffusion layer. Therefore, by making the peak pore diameter D2 of the cathode-side gas diffusion layer larger than the peak pore diameter D1 of the cathode catalyst layer, the generated water can be discharged more effectively. In addition, the generated water is prevented from blocking the gas diffusion path, and the gas required for the reaction is more easily diffused to the catalyst. As a result, the reaction efficiency is improved, and the performance of the fuel cell is easily improved.
[0013] The logarithmic differential pore volume dV / d(logD) distribution of the cathode catalyst layer and the cathode-side gas diffusion layer is measured by mercury intrusion porosimetry. Here, in the logarithmic differential pore volume distribution, when there are multiple peaks in a predetermined pore diameter range, the main peak is determined from among the multiple peak pore diameters. The main peak refers to the peak with the largest peak area (i.e., pore volume) among the multiple peaks in the predetermined pore diameter range. In the cathode catalyst layer, when there are multiple peaks in the logarithmic differential pore volume distribution in the range of 0.01 μm to 1 μm, the pore diameter of the main peak among the multiple peak pore diameters may be smaller than the peak pore diameter of the gas diffusion layer. Similarly, in the cathode-side gas diffusion layer, when there are multiple peaks in the logarithmic differential pore volume distribution in the range of 0.01 μm to 5 μm, the pore diameter of the main peak among the multiple peak pore diameters may be larger than the peak pore diameter of the cathode catalyst layer in the range of 0.01 μm to 1 μm.
[0014] FIG. 1 shows an example of logarithmic differential pore volume distribution. In FIG. 1, the logarithmic differential pore volume distribution of the gas diffusion layer shown by the solid line has one peak in the range of 0.01 μm to 5 μm (D2=0.09 μm). On the other hand, the logarithmic differential pore volume distribution of the gas diffusion layer shown by the dashed line has two peaks at the positions of pore diameters D of 0.04 μm and 0.2 μm in the range of 0.01 μm to 5 μm. Of these, the peak of 0.04 μm, which has a smaller pore diameter D, has a larger peak area (i.e., a larger pore volume) than the peak of 0.2 μm, which has a larger pore diameter, and is therefore considered to be dominant in the pore structure. Therefore, the pore diameter D2=0.04 μm of the main peak with the larger peak area is adopted as the peak pore diameter of the gas diffusion layer.
[0015] The peak pore diameter D1 of the cathode catalyst layer may be 0.05 μm or more. In this case, the peak pore diameter D2 of the gas diffusion layer is greater than 0.05 μm. This makes it easier for generated water to be discharged and improves gas diffusibility.
[0016] The gas diffusion layer (at least one of the cathode gas diffusion layer and the anode gas diffusion layer) may be produced without using a substrate. In order to maintain mechanical strength, the gas diffusion layer may have a configuration in which a water-repellent layer is formed on a conductive porous sheet such as carbon cloth and carbon paper. On the other hand, because the adhesion to the catalyst layer is good, the film thickness and porosity can be easily controlled, and a flow path can be formed directly on the gas diffusion layer, a configuration that does not have a conductive substrate and is mainly composed of a conductive material and a polymer resin has also been attempted. In the case of a gas diffusion layer having a substrate, the logarithmic differential pore volume distribution may have a peak in the range exceeding 5 μm due to the pore structure of the carbon fiber woven cloth and carbon paper. In contrast, a gas diffusion layer without a substrate does not have a peak in the logarithmic differential pore volume dV / d (logD) distribution in the range where the pore diameter exceeds 5 μm.
[0017] An example of the structure of a fuel cell according to this embodiment will be described below with reference to Fig. 2. Fig. 2 is a cross-sectional view that shows a schematic structure of a unit cell arranged in a fuel cell according to one embodiment. Normally, a plurality of unit cells are stacked and arranged in the fuel cell as a cell stack. For convenience, Fig. 2 shows one unit cell.
[0018] The single cell 200 includes a membrane electrode assembly 100 having an electrolyte membrane 110, a first catalyst layer 120A and a second catalyst layer 120B arranged to sandwich the electrolyte membrane 110, and a first gas diffusion layer 130A and a second gas diffusion layer 130B arranged to sandwich the electrolyte membrane 110 through the first catalyst layer 120A and the second catalyst layer 120B, respectively. The single cell 200 also includes a first separator 240A and a second separator 240B that sandwich the membrane electrode assembly 100. One of the first catalyst layer 120A and the second catalyst layer 120B functions as an anode, and the other functions as a cathode. The electrolyte membrane 110 is slightly larger than the first catalyst layer 120A and the second catalyst layer 120B, so that the peripheral portion of the electrolyte membrane 110 protrudes from the first catalyst layer 120A and the second catalyst layer 120B. The peripheral edge of the electrolyte membrane 110 is sandwiched between a pair of sealing members 250A, 250B.
[0019] Either the first catalyst layer 120A or the second catalyst layer 120B is an anode catalyst layer, and the other is a cathode catalyst layer. Here, the first catalyst layer 120A is the cathode catalyst layer, and the second catalyst layer 120B is the anode catalyst layer. In this case, the first gas diffusion layer 130A corresponds to the cathode side gas diffusion layer, and the logarithmic differential pore volume distribution of the first catalyst layer 120A and the logarithmic differential pore volume distribution of the first gas diffusion layer 130A satisfy the above-mentioned pore diameter peak relationship.
[0020] (Gas diffusion layer) The first gas diffusion layer 130A and the second gas diffusion layer 130B may have a structure with a substrate layer or may have a structure without a substrate layer. A structure without a substrate layer is more preferable. As a structure without a substrate layer, a microporous sheet formed from the above-mentioned conductive material and polymer resin can be used. As a structure with a substrate layer, for example, a structure having a substrate layer and a microporous layer provided on the catalyst layer side can be mentioned. A conductive porous sheet such as carbon cloth or carbon paper is used for the substrate layer. For the microporous layer, a mixture of a water-repellent resin such as a fluororesin, a conductive carbon material, and a proton-conductive resin (polymer electrolyte) is used.
[0021] The substrate-less gas diffusion layer contains, for example, a conductive material and a polymer resin. The polymer resin is preferably 10 to 40 parts by mass per 100 parts by mass of the conductive material and the polymer resin in total. The conductive material contains a particulate material and may further contain a fibrous material.
[0022] Examples of particulate materials include carbon black, spherical graphite, and activated carbon. Of these, it is preferable to use carbon black because of its high electrical conductivity and large pore volume. Examples of carbon black that can be used include acetylene black, ketjen black, and furnace black. Examples of fibrous materials include fibrous carbon materials such as vapor grown carbon fiber (VGCF (registered trademark)), carbon nanotubes, and carbon nanofibers.
[0023] The conductive material may include a particulate material and a fibrous material, and may further include a plate-shaped material. The plate-shaped material may be provided in the gas diffusion layer so as to be oriented along the surface direction (direction perpendicular to the thickness direction) of the gas diffusion layer. The plate-shaped material acts to enhance the gas diffusibility in the surface direction of the gas diffusion layer. The plate-shaped material is particulate when viewed macroscopically, but is composed of plate-shaped particles when viewed microscopically. Specific examples of the plate-shaped material include flake graphite, graphitized polyimide film pulverized material, graphene, and the like. Among them, graphitized polyimide film pulverized material and graphene are easily oriented in the surface direction of the gas diffusion layer, are advantageous for forming a thin gas diffusion layer, and are suitable for enhancing the gas diffusibility in the surface direction of the gas diffusion layer.
[0024] The polymer resin functions as a binder that bonds the conductive materials together. From the viewpoint of suppressing water retention in the pores in the gas diffusion layer, it is preferable that 50% by mass or more, and further 90% by mass or more of the polymer resin is a water-repellent fluororesin. Examples of the fluororesin include PTFE (polytetrafluoroethylene), FEP (tetrafluoroethylene-hexafluoropropylene copolymer), PVdF (polyvinylidene fluoride), ETFE (tetrafluoroethylene-ethylene copolymer), PCTFE (polychlorotrifluoroethylene), and PFA (polyfluoroethylene-perfluoroalkyl vinyl ether copolymer). Among them, from the viewpoint of heat resistance, water repellency, and chemical resistance, it is preferable that the fluororesin is PTFE.
[0025] The gas diffusion layer is produced, for example, as follows. First, a mixture containing a conductive material, a polymer resin, a surfactant, and a dispersion medium is prepared. A kneader or a mixer may be used as the mixing device. At this time, it is preferable to add the conductive material, the surfactant, and the dispersion medium to the mixing device to uniformly disperse the conductive material in the dispersion medium, and then add the polymer resin to further disperse the conductive material. It is preferable to apply an appropriate shear force to the polymer resin to fibrillate the polymer resin. Examples of the dispersion medium include water, alcohol, and glycols. Examples of the surfactant include polyoxyethylene alkyl ether, alkylamine oxide, and the like.
[0026] Next, the mixture obtained is formed into a sheet by a molding method such as extrusion molding. The obtained sheet may be further rolled. A roll press machine can be used for rolling. The conditions of the roll press are not particularly limited, but a gas diffusion layer with high strength can be easily obtained by rolling at a linear pressure of 0.001 ton / cm to 4 ton / cm.
[0027] Next, the sheet is baked to obtain a baked sheet from which the surfactant and the dispersion medium are removed. The baking temperature may be any temperature at which the polymer resin does not deteriorate and at which the surfactant and the dispersion medium decompose or volatilize. When PTFE is used as the polymer resin, the baking temperature is preferably 280 to 340°C. The baking atmosphere may be an inert atmosphere, such as a nitrogen or argon atmosphere, or a reduced pressure atmosphere. It is sufficient that most of the surfactant and the dispersion medium are removed from the sheet, and it is not necessary to remove them completely.
[0028] (catalyst layer) The first catalyst layer 120A (cathode catalyst layer) contains, for example, a conductive material, catalyst particles, and a proton conductive resin. The catalyst particles are supported on the conductive material. The conductive material contains particulate conductive members and / or fibrous conductive members. By including the fibrous conductive members, the gas diffusibility of the catalyst layer can be improved.
[0029] (fibrous conductive material) Examples of the fibrous conductive member include fibrous carbon materials such as vapor-grown carbon fibers, carbon nanotubes, and carbon nanofibers. F is not particularly limited, but is preferably 200 nm or less, more preferably 5 nm or more and 200 nm or less, and even more preferably 10 nm or more and 170 nm or less. In this case, the volume ratio of the fibrous conductive members in the catalyst layer can be reduced while a sufficient gas path can be secured, and gas diffusibility can be improved. F is determined by randomly selecting 10 fibrous conductive members from the catalyst layer and averaging their diameters. The diameter is the length in the direction perpendicular to the longitudinal direction of the fibrous conductive members.
[0030] Length of fibrous conductive material L F Although there is no particular limitation, the length L of the fibrous conductive member is preferably 0.2 μm or more and 20 μm or less, and more preferably 0.2 μm or more and 10 μm or less. In this case, at least a part of the fibrous conductive member is oriented along the thickness direction of the catalyst layer, and it is easy to ensure a gas diffusion path. F is the average fiber length, and is determined by randomly selecting 10 fibrous conductive members from the catalyst layer and averaging the fiber lengths of these fibrous conductive members. Note that, in the case of a substantially linear fibrous conductive member, the fiber length of the fibrous conductive member refers to the length of a straight line connecting one end of the fibrous conductive member to the other end of the fibrous conductive member.
[0031] The fibrous conductive member may have a hollow space (hollow portion) inside. In this case, both ends in the longitudinal direction of the fibrous conductive member may be open in the catalyst layer. The fibrous conductive member having both ends in the longitudinal direction open means that the openings connect the hollow portion to the outside. In other words, the openings at both ends of the fibrous conductive member are not blocked by either the electrolyte membrane or the gas diffusion layer, and gas can enter and exit from both ends. The side wall of the fibrous conductive member having a hollow portion may be provided with a through hole that communicates the hollow portion with the outside. Catalyst particles can be arranged and fixed on the side wall of the fibrous conductive member so as to block at least a portion of the through hole. The catalyst particles supported on the side wall so as to block at least a portion of the through hole are more efficiently contacted with the reaction gas, and the reaction efficiency of the catalyst layer can be significantly improved.
[0032] (Particulate conductive material) The particulate conductive material is not particularly limited, but carbon black is preferred because of its excellent conductivity. Examples of carbon black include acetylene black, ketjen black, thermal black, furnace black, and channel black. The particle size (or the length of the structure composed of a plurality of connected primary particles) is not particularly limited, and any carbon black that has been used in the catalyst layer of a fuel cell can be used.
[0033] (catalyst particles) The catalyst particles are not particularly limited, and include catalyst metals such as alloys and simple substances selected from Sc, Y, Ti, Zr, V, Nb, Fe, Co, Ni, Ru, Rh, Pd, Pt, Os, Ir, lanthanide series elements, and actinide series elements. For example, catalyst particles used in the anode include Pt and Pt-Ru alloys. Catalyst particles used in the cathode include Pt and Pt-Co alloys. At least a part of the catalyst particles is supported on a particulate conductive member. The catalyst particles are preferably supported on a fibrous conductive member in addition to the particulate conductive member. This is because the catalyst particles are more likely to come into contact with the gas, and the efficiency of the oxidation reaction or reduction reaction of the gas is increased.
[0034] From the viewpoint of fixing the catalyst particles, the diameter X of the catalyst particles is preferably 1 nm or more and 10 nm or less, more preferably 2 nm or more and 5 nm or less. When X is 1 nm or more, the catalytic effect of the catalyst particles can be sufficiently obtained. When X is 10 nm or less, the catalyst particles can be easily supported on the side walls of the fibrous conductive member.
[0035] The diameter X of the catalyst particle is determined as follows. For any one catalyst particle observed in the TEM image of the catalyst layer, calculate the particle diameter when the particle is considered to be spherical. This is performed for 100 to 300 catalyst particles observed in the TEM image, and the particle diameter of each is calculated. The average value of these particle diameters is taken as the diameter X of the catalyst particle.
[0036] (Proton conductive resin) The proton conductive resin is not particularly limited, but examples thereof include perfluorocarbon sulfonic acid polymers and hydrocarbon polymers. Among them, perfluorocarbon sulfonic acid polymers and the like are preferred because of their excellent heat resistance and chemical stability. An example of a perfluorocarbon sulfonic acid polymer is Nafion (registered trademark). The proton conductive resin coats at least a portion of the particulate conductive member, the fibrous conductive member, and / or the catalyst particles.
[0037] The second catalyst layer 120B (anode catalyst layer) may be made of a known material and have a known structure. The anode catalyst layer may contain a conductive material, catalyst particles supported on the conductive material, and a proton conductive resin, similar to the cathode catalyst layer. The conductive material may contain a particulate conductive member and / or a fibrous conductive member.
[0038] The anode catalyst layer is not exposed to as highly oxidizing an environment as the cathode catalyst layer, but since water is not produced by the reaction, the anode catalyst layer is more likely to be in a less humid environment than the cathode catalyst layer. As a result, the proton conductivity is more likely to decrease. The composition and content ratio of each of the particulate conductive member, the fibrous conductive member, and the proton conductive resin can be changed so as to obtain a proton conductivity higher than that of the cathode catalyst layer.
[0039] The thickness of the catalyst layer is preferably as thin as possible from the viewpoints of miniaturizing the fuel cell, maintaining low proton resistance, and obtaining high output. On the other hand, from the viewpoint of strength, it is preferable that the thickness is not excessively thin. In general, the thickness of the catalyst layer tends to increase as the blending ratio of the fibrous conductive member increases.
[0040] Thickness of the cathode catalyst layer T C The thickness T of the anode catalyst layer is, for example, 4 μm or more and 15 μm or less. A The thickness T of the catalyst layer is, for example, 2 μm or more and 12 μm or less. C and T A is the average thickness, and is obtained by averaging the distances when a straight line is drawn from one main surface to the other main surface along the thickness direction of the catalyst layer for any 10 points on the cross section of the catalyst layer.
[0041] Regarding the blending ratio of the fibrous conductive member in the catalyst layer, in both the anode catalyst layer and the cathode catalyst layer, the fibrous conductive member is contained in an amount of 20% or more relative to the particulate conductive member on a mass basis, thereby improving gas diffusibility. On the other hand, if the blending amount of the fibrous conductive member is increased, the catalyst layer is likely to become thicker and the proton transfer resistance is likely to increase. In addition, cracks are likely to occur in the catalyst layer. From the viewpoint of suppressing the increase in the proton transfer resistance and suppressing cracks, the blending amount of the fibrous conductive member may be 50% or less relative to the particulate conductive member on a mass basis in the anode catalyst layer and / or the cathode catalyst layer.
[0042] The catalyst layer is prepared, for example, as follows. First, catalyst particles and particulate conductive members are mixed in a dispersion medium (e.g., water, ethanol, propanol, etc.). Next, while stirring the obtained dispersion, a proton conductive resin and a fibrous carbon material are added in sequence to obtain a catalyst dispersion. The proton conductive resin may be added in two or more portions. In this case, the second and subsequent additions of the proton conductive resin may be added together with the fibrous carbon material. Thereafter, the obtained catalyst dispersion is applied to a uniform thickness on the surface of an electrolyte membrane or a suitable transfer substrate sheet, and dried to obtain a catalyst layer.
[0043] Examples of the coating method include conventional coating methods, such as spraying, screen printing, and coating methods using various coaters such as blade coaters, knife coaters, and gravure coaters. As the transfer substrate sheet, it is preferable to use a sheet having a smooth surface such as polyethylene terephthalate (PET) or polypropylene. When using the transfer substrate sheet, the obtained catalyst layer is transferred to the electrolyte membrane or gas diffusion layer described later.
[0044] The catalyst layer is transferred to the electrolyte membrane or gas diffusion layer by abutting the surface of the catalyst layer facing the transfer base sheet against the electrolyte membrane or gas diffusion layer. By abutting the smooth surface of the catalyst layer against the electrolyte membrane or gas diffusion layer, the interface resistance with the catalyst layer is reduced, improving the performance of the fuel cell. The catalyst dispersion may be applied directly to the electrolyte layer.
[0045] (electrolyte membrane) A polymer electrolyte membrane is preferably used as the electrolyte membrane 110. Examples of materials for the polymer electrolyte membrane include the polymer electrolytes exemplified as the proton conductive resin. The thickness of the electrolyte membrane is, for example, 5 to 30 μm.
[0046] (Separator) The first separator 240A and the second separator 240B are not particularly limited in material as long as they have airtightness, electronic conductivity, and electrochemical stability. Such materials are preferably carbon materials, metal materials, and the like. Metal materials may be coated with carbon. For example, the first separator 240A and the second separator 240B are obtained by punching a metal plate into a predetermined shape and performing a surface treatment.
[0047] In this embodiment, a gas flow channel 260A is formed on the surface of the first separator 240A that comes into contact with the first gas diffusion layer 130A. Meanwhile, a gas flow channel 260B is formed on the surface of the second separator 240B that comes into contact with the second gas diffusion layer 130B. The shape of the gas flow channel is not particularly limited, and may be a straight type, a serpentine type, or the like.
[0048] (Sealing material) The seal members 250A, 250B are made of an elastic material and prevent the fuel and / or oxidant from leaking from the gas flow paths 260A, 260B. The seal members 250A, 250B have, for example, a frame shape that surrounds the peripheral portions of the first catalyst layer 120A and the second catalyst layer 120B in a loop shape. The seal members 250A, 250B can each be made of a known material and have a known configuration.
[0049] The present disclosure will be described in more detail below based on examples, although the present disclosure is not limited to the following examples.
[0050] [Example] (1) Preparation of dispersion for cathode catalyst layer A particulate conductive member (carbon black) carrying catalyst particles (Pt-Co alloy) was added to an appropriate amount of water and stirred to disperse. An appropriate amount of ethanol was added to the obtained dispersion while stirring, and then 35 parts by mass of a fibrous conductive member (vapor-grown carbon fiber, average diameter 150 nm, average fiber length 10 μm) and 100 parts by mass of a proton conductive resin (perfluorocarbon sulfonic acid polymer) were added to 100 parts by mass of the particulate conductive member carrying catalyst particles, and stirred to prepare a catalyst dispersion for a cathode catalyst layer.
[0051] (2) Preparation of dispersion for anode catalyst layer A particulate conductive member (carbon black) carrying catalyst particles (Pt) was added to an appropriate amount of water and stirred to disperse it. An appropriate amount of ethanol was added to the obtained dispersion while stirring, and then 35 parts by mass of a fibrous conductive member (vapor-grown carbon fiber, average diameter 150 nm, average fiber length 10 μm) and 120 parts by mass of a proton conductive resin (perfluorocarbon sulfonic acid polymer) were added to 100 parts by mass of the particulate conductive member carrying catalyst particles, and stirred to prepare a catalyst dispersion for an anode catalyst layer.
[0052] (3) Preparation of gas diffusion layer A particulate conductive material (carbon black), a fibrous conductive material (carbon nanotubes, fiber diameter 50nm to 300nm, fiber length 1μm to 50μm), a surfactant, and a dispersion medium were added to a stirring device, and the materials were stirred and kneaded to uniformly disperse. Then, PTFE was further added as a polymer resin and uniformly dispersed to obtain a kneaded material. Next, the kneaded material was extruded and stretched into a sheet and dried. The obtained sheet was baked at 310°C to remove the surfactant and dispersion medium, and a gas diffusion layer was obtained.
[0053] The contents of the particulate conductive material, fibrous conductive material, and polymer resin in the gas diffusion layer were adjusted to be 5% to 35% by mass, 35% to 80% by mass, and 10% to 40% by mass, respectively. In this way, five types of gas diffusion layers A1 to A5 with different pore structures were produced.
[0054] (4) Preparation of a single cell Two PET sheets were prepared, and the obtained catalyst dispersion for the cathode catalyst layer was applied in a uniform thickness to the smooth surface of one PET sheet using a screen printing method, and the obtained catalyst dispersion for the anode catalyst layer was applied in a uniform thickness to the smooth surface of the other PET sheet. Then, they were dried to form two catalyst layers. The thickness of the cathode catalyst layer was 6 μm, and the thickness of the anode catalyst layer was 4.5 μm.
[0055] When the pore size distribution of the cathode catalyst layer was measured by mercury intrusion porosimetry, the logarithmic differential pore volume dV / dlogD had a peak when the pore diameter D was 80 nm.
[0056] The obtained catalyst layer was transferred onto both main surfaces of a 15 μm-thick electrolyte membrane, forming a cathode on one surface of the electrolyte membrane and an anode on the other surface. Then, two gas diffusion layers A1 to A5 were prepared, and one of the two was abutted against the anode and the other was abutted against the cathode, to produce five membrane electrode assemblies.
[0057] Next, a frame-shaped seal member was placed so as to surround the anode and the cathode. The whole was sandwiched between a pair of stainless steel flat plates (separators) having gas flow paths in the areas in contact with the gas diffusion layers to complete test cell X1 using gas diffusion layer A1, test cell X2 using gas diffusion layer A2, test cell X3 using gas diffusion layer A3, test cell X4 using gas diffusion layer A4, and test cell X5 using gas diffusion layer A5.
[0058] <Evaluation> The single cell was heated to 80°C, and fuel gas with a relative humidity of 100% was supplied to the anode, and oxidant gas (air) with a relative humidity of 100% was supplied to the cathode. The fuel gas and oxidant gas were pressurized to a cell inlet gas pressure of 70 to 90 kPa at each current density and supplied. The load control device was controlled so that the current flowed constantly, and the voltage (initial voltage) and resistance value of the single cell were measured while changing the current density relative to the electrode area of the anode and cathode.
[0059] The maximum power density W1 was evaluated for each of the unit cells X1 to X5. The evaluation results are shown in Table 1. In Table 1, the maximum power density W1 is shown as a relative value with the measured value of the maximum power density W1 for the unit cell X5 taken as 100. Table 1 also shows the pore diameters D2 at which the logarithmic differential pore volume distribution has a main peak in the range of 0.01 μm to 5 μm for the gas diffusion layers A1 to A5 used in the unit cells X1 to X5.
[0060] As can be seen from Table 1, the pore diameter D2 at the main peak of the gas diffusion layers A1 to A4 is larger than the pore diameter peak D1 (80 nm) of the cathode catalyst layer. In contrast, in the unit cell X5, the pore diameter D2 at the main peak of the gas diffusion layer A5 is smaller than the pore diameter peak (80 nm) of the cathode catalyst layer. In the unit cells X1 to X4, the drainage of water generated at the cathode is improved, and the maximum power density is improved from the cell X5.
[0061] [Table 1] [Industrial Applicability]
[0062] The fuel cell according to the present disclosure can be suitably used as a power source for a stationary type home cogeneration system or a power source for a vehicle. The present disclosure is suitable for application to a polymer electrolyte fuel cell, but is not limited thereto, and can be applied to fuel cells in general. [Explanation of symbols]
[0063] 100: membrane electrode assembly, 110: electrolyte membrane, 120: catalyst layer, 120A: first catalyst layer, 120B: second catalyst layer, 130A: first gas diffusion layer, 130B: second gas diffusion layer, 200: fuel cell (single cell), 240A: first separator, 240B: second separator, 250A, 250B: sealing members, 260A, 260B: gas flow path
Claims
[Claim 1] a cathode having a cathode catalyst layer; an anode having an anode catalyst layer; an electrolyte membrane interposed between the cathode and the anode; a pair of gas diffusion layers laminated on the cathode and the anode, respectively, on the opposite side of the electrolyte membrane; the cathode catalyst layer includes a particulate conductive member, a fibrous conductive member, catalyst particles supported on at least the particulate conductive member among the particulate conductive member and the fibrous conductive member, and a proton conductive resin, and has a peak in a logarithmic differential pore volume dV / d (logD) distribution in a pore diameter D range of 0.01 μm to 1 μm, The gas diffusion layer laminated on the cathode includes a particulate conductive material, a fibrous conductive material, and a polymer resin, the particulate conductive material includes at least one selected from the group consisting of carbon black, spherical graphite, and activated carbon; the fibrous conductive material includes at least one selected from the group consisting of vapor-grown carbon fiber, carbon nanotube, and carbon nanofiber; The polymer resin includes a fluororesin, The gas diffusion layer laminated on the cathode has a peak in a logarithmic differential pore volume dV / d (logD) distribution in a pore diameter D range of 0.01 μm to 5 μm, and does not have a peak in a logarithmic differential pore volume dV / d (logD) distribution in a pore diameter range exceeding 5 μm, The pore diameter D at the peak of the cathode catalyst layer 1 is the pore diameter D at the peak of the gas diffusion layer laminated on the cathode 2 The membrane electrode assembly is smaller than
Citation Information
Patent Citations
Fuel cell electrode, manufacture thereof and fuel cell
JP2000182626A
Electrode for fuel cell and fuel cell
JP2001338651A
Gas diffusion layer, membrane-electrode conjugant, and fuel cell
JP2011108441A
Membrane-electrode assembly and fuel cell
JP2020140908A