Composite active material and battery

A composite active material with silicon and a higher potential material like phosphorus addresses the issue of increased confining pressure in silicon-based batteries by having the higher potential material react first, thereby reducing local expansion and stabilizing the battery.

JP2024150150AActive Publication Date: 2024-10-23TOYOTA JIDOSHA KK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023063416
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-10-23
Estimated Expiration
2043-04-10

AI Technical Summary

Technical Problem

Batteries using silicon (Si) as the active material experience significant increases in confining pressure due to large volume changes during charging and discharging, which existing technologies have not adequately addressed.

Method used

A composite active material comprising silicon (Si) as the first active material and another material with a higher reaction potential, such as phosphorus (P), is used to reduce the increase in confining pressure by having the higher potential material react with lithium before Si, thereby reducing local expansion.

Benefits of technology

The composite active material effectively suppresses the increase in battery confining pressure by mitigating local reactions and expansions during charging, leading to a more stable battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150150000001_ABST
    Figure 2024150150000001_ABST
Patent Text Reader

Abstract

To disclose a composite active material containing Si capable of suppressing an increase in the restraint pressure of a battery at charging.SOLUTION: A composite active material of the present disclosure contains: a first active material; and a second active material. The first active material is Si, a reaction potential P2 of the second active material and Li is higher than a reaction potential P1 of the first active material and Li.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application discloses a composite active material and a battery. [Background technology]

[0002] Patent Document 1 discloses a negative electrode active material with a small expansion amount during charging. The negative electrode active material disclosed in Patent Document 1 is a nonwoven particle containing Si fiber, has an average particle diameter (D50) of 0.2 μm to 3.6 μm, and is amorphous. On the other hand, the volume change of the Si material as the active material of the battery is large during charging and discharging. For example, if the expansion amount of the Si material as the active material is large, the restraining pressure of the battery is likely to increase significantly. Although it is considered that the battery having the negative electrode active material disclosed in Patent Document 1 can suppress the increase in the restraining pressure during charging to some extent, there is still room for improvement. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2021-022554 Summary of the Invention [Problem to be solved by the invention]

[0004] For batteries with Si as the active material, new technologies are needed that can reduce the increase in confining pressure. [Means for solving the problem]

[0005] The present application discloses the following aspects as means for solving the above problems. <Aspect 1> a composite active material comprising a first active material and a second active material; The first active material is Si, The reaction potential P between the second active material and Li 2 is a reaction potential P between the first active material and Li 1 Higher than Composite active material. <Aspect 2> The composite active material of embodiment 1, The reaction potential P 2 and the reaction potential P 1 Difference with P 2 -P 1 is greater than 0V and less than or equal to 2.0V, Composite active material. <Aspect 3> The composite active material of embodiment 1 or 2, The first active material is porous Si. Composite active material. <Aspect 4> The composite active material according to any one of aspects 1 to 3, The second active material is P. Composite active material. <Aspect 5> A battery having a positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, The negative electrode active material layer contains the composite active material according to any one of aspects 1 to 4. battery. Effect of the Invention

[0006] According to the composite active material of the present disclosure, an increase in the confining pressure of the battery is likely to be reduced. [Brief description of the drawings]

[0007] [Figure 1] 1 shows a schematic diagram of an example of a composite active material. [Diagram 2] 1 shows a schematic diagram of an example of a battery configuration. [Diagram 3] 1 shows an SEM image of the composite active material according to Example 1 and EDX distributions of Si and P in the SEM image. [Figure 4] 1 shows an SEM image of the composite active material according to Example 2 and EDX distributions of Si and P in the SEM image. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] 1.Composite active material FIG. 1 shows a schematic configuration of a composite active material 1 according to an embodiment. As shown in FIG. 1, the composite active material 1 includes a first active material 1a and a second active material 1b. The first active material 1a is Si. The reaction potential P between the second active material 1b and Li is 2 is the reaction potential P between the first active material 1a and Li 1 Higher than.

[0009] 1.1 First active material The first active material 1a is Si. The first active material 1a may be amorphous Si or crystalline Si. Whether the first active material 1a is amorphous or crystalline can be determined by X-ray diffraction measurement or the like.

[0010] The first active material 1a may be porous Si. It is considered that the first active material 1a is porous and has voids, and thus the voids can absorb the expansion of Si, and the increase in the restraining pressure of the battery can be further reduced. The first active material 1a may be, for example, nanoporous Si. Nanoporous Si refers to Si having a plurality of pores with a pore diameter of nanometer order (less than 1000 nm, preferably 100 nm or less). The first active material 1a may be porous Si including pores with a diameter of 55 nm or less. Pores with a diameter of 55 nm or less are difficult to be crushed even by pressing. In other words, porous Si including pores with a diameter of 55 nm or less is likely to maintain a porous state even after pressing. For example, the first active material 1a may contain pores with a diameter of 55 nm or less in an amount of 0.21 cc or more and 0.30 cc / g or less per 1 g of the first active material 1a. The lower limit may be 0.22 cc / g or more, or 0.23 cc / g or more, and the upper limit may be 0.28 cc / g or less, or 0.26 cc / g or less. The amount of pores having a diameter of 55 nm or less contained in the first active material 1a can be determined from a pore size distribution by, for example, a nitrogen gas adsorption method or a DFT method.

[0011] The porosity of the first active material 1a is not particularly limited. The porosity of the first active material 1a may be, for example, 0% or more and 80% or less. The lower limit may be 1% or more, 5% or more, 10% or more, or 20% or more, and the upper limit may be 70% or less, 60% or less, 50% or less, 40% or less, or 30% or less. The porosity of the first active material 1a can be determined, for example, by observation using a scanning electron microscope (SEM). It is preferable to have a large number of samples, for example, 100 or more. The porosity can be an average value determined from these samples.

[0012] The first active material 1a may be particulate. That is, the composite active material 1 may have first particles containing Si as the first active material 1a. The first particles may contain Si as the first active material 1a, and the chemical composition thereof is not particularly limited. The ratio of the Si element to all elements contained in the first particles may be, for example, 50 mol% to 100 mol%, 70 mol% to 100 mol%, or 90 mol% to 100 mol%. The first particles may contain other elements in addition to the Si element. The other elements may be at least one of Li, Sn, Fe, Co, Ni, Ti, Cr, Al, and B. When the first particles are obtained by removing Li from Li-Si alloy particles, the first particles may contain Li as well as Si. The first particles may also contain impurities such as oxides. When the first active material 1a is particulate, the size thereof is not particularly limited. The particle diameter D of the first particles described above 1 The particle diameter D of the first particles may be, for example, 10 nm or more and 10 μm or less. The lower limit may be 30 nm or more, 50 nm or more, 100 nm or more, or 150 nm or more, and the upper limit may be 5 μm or less, 3 μm or less, 2 μm or less, or 1 μm or less. 1 can be obtained by observation with an electron microscope such as SEM, and is calculated as the number average value of the maximum Feret's diameter of each of a plurality of particles. The number of samples is preferably large, for example, 20 or more, or may be 50 or more, or may be 100 or more.1 can be appropriately adjusted, for example, by appropriately changing the manufacturing conditions of Si, which is the first active material 1a, or by performing a classification process. The composite active material 1 may have at least one of the above-mentioned first particles. The number of the above-mentioned first particles contained in one composite active material 1 may be 1 or more and 10,000 or less. The lower limit may be 2 or more, 5 or more, 10 or more, 50 or more, or 100 or more, and the upper limit may be 5,000 or less, 1,000 or less, or 500 or less.

[0013] 1.2 Second active material Reaction potential P between the second active material 1b and Li 2 is the reaction potential P between the first active material 1a and Li 1 is higher. That is, the charge / discharge potential of the second active material 1b is more noble than the charge / discharge potential of the first active material 1a, and during charging, the second active material 1b reacts with Li before the first active material 1a. According to the knowledge of the present inventor, when a composite active material 1 containing the second active material 1b together with the first active material 1a is used in a battery, the increase in the battery's restraining pressure during charging is smaller than when only the first active material 1a is used. This is presumed to be due to the following mechanism. That is, as described above, during charging of the battery, the second active material 1b reacts with Li before the first active material 1a. This is thought to reduce the local reaction between the first active material 1a and lithium, and to suppress the local expansion of the first active material 1a. As a result, the increase in the battery's restraining pressure is suppressed.

[0014] According to the above mechanism, the second active material 1b has a reaction potential P 2 is the reaction potential P between the first active material 1a and Li 1 Any material having a higher valence can be used. In one embodiment, the second active material 1b may be at least one selected from P, Sn, Al, and lithium titanate (LTO). For example, when the second active material 1b is P (simple phosphorus), a more excellent effect is likely to be exhibited.

[0015] The second active material 1b may be in a particulate form. That is, the composite active material 1 may have second particles containing the second active material 1b. When the second active material 1b is in a particulate form, its size is not particularly limited. The particle diameter D of the second particles is 2 The particle diameter D of the second particles may be, for example, 1 nm or more and 10 μm or less. The lower limit may be 5 nm or more, 10 nm or more, 30 nm or more, 50 nm or more, 100 nm or more, or 150 nm or more, and the upper limit may be 5 μm or less, 3 μm or less, 2 μm or less, or 1 μm or less. 2 can be obtained by observation with an electron microscope such as SEM, and is calculated as the number average value of the maximum Feret's diameter of each of a plurality of particles. The number of samples is preferably large, for example, 20 or more, or may be 50 or more, or may be 100 or more. 2 is the particle diameter D of the first particle 1 For example, as shown in FIG. 1, the composite active material 1 may have a first particle which is a relatively large particle, and a second particle which is a relatively small particle and adheres to the surface of the first particle.

[0016] Alternatively, the second active material 1b may be layered. For example, the composite active material 1 may have the above-mentioned first particle containing Si as the first active material 1a, and a coating layer that covers at least a part of the surface of the first particle and contains the second active material 1b. When the second active material 1b is layered, its thickness is not particularly limited. The layered second active material 1b may have a thickness of, for example, 1 nm or more and 10 μm or less. The lower limit may be 5 nm or more, 10 nm or more, 30 nm or more, 50 nm or more, 100 nm or more, or 150 nm or more, and the upper limit may be 5 μm or less, 3 μm or less, 2 μm or less, or 1 μm or less. The coating layer containing the second active material 1b may cover, for example, 10% or more and 100% or less of the surface of the first particle.

[0017] 1.3 Reaction potential of the first active material and the second active material with respect to Li As described above, the reaction potential P between the second active material 1b and Li 2 is the reaction potential P between the first active material 1a and Li 1 Higher than the reaction potential P 2 and reaction potential P 1 The difference between the reaction potential P 2 and reaction potential P 1 Difference with P 2 -P 1 When the difference P is greater than 0 V and equal to or less than 2.0 V, the increase in the battery restraining pressure during charging can be more significantly suppressed. 2 -P 1 may be 0.1V or more, 0.2V or more, or 0.3V or more, and may be 1.8V or less, 1.6V or less, 1.4V or less, 1.2V or less, or 1.0V or less. The reaction potential between the first active material 1a and Li may be, for example, 0.2V or more and 0.7V or less. The reaction potential between the second active material 1b and Li may be, for example, more than 0.7V and 1.2V or less. Here, the "reaction potential" refers to an average reaction potential. The reaction potential between the first active material 1a and Li can be calculated from a charging curve when only the first active material 1a is used as the active material of a lithium ion battery and charging is performed with Li metal as the counter electrode. Similarly, the reaction potential between the second active material 1b and Li can be calculated from a charging curve when only the second active material 1b is used as the active material of a lithium ion battery and charging is performed with Li metal as the counter electrode.

[0018] 1.4 Content ratio of first particles to second particles There is no particular limitation on the content ratio of the first active material 1a and the second active material 1b in the composite active material 1. For example, when the total of the first active material 1a and the second active material 1b is taken as 100 mass%, the content of the first active material 1a may be more than 50 mass% and less than 100 mass%, 60 mass% or more and 99 mass% or less, 70 mass% or more and 98 mass% or less, 80 mass% or more and 97 mass% or less, or 90 mass% or more and 95 mass% or less.

[0019] 1.5 Other ingredients The composite active material 1 includes at least the first active material 1a and the second active material 1b. The composite active material 1 may also include other components as desired. Examples of the other components include various solid components and liquid components. For example, the composite active material 1 may also include other active materials (third active materials). The composite active material 1 may include the first active material 1a and the second active material 1b in a total amount of more than 50% by mass and 100% by mass or less, 70% by mass or more and 100% by mass or less, or 90% by mass or more and 100% by mass or less. The third active material that may be included in the composite active material 1 may, for example, be one in which the reaction potential between the third active material and Li is lower than the reaction potential between the first active material 1a and Li. That is, the third active material may react with Li at a potential lower than that of the first active material 1a. The third active material may, for example, be at least one selected from graphite, lithium, and the like. The composite active material 1 may contain a binder in addition to the first active material 1a and the second active material 1b. The binder may have, for example, a function of binding the first active materials 1a together or a function of binding the first active material 1a and the second active material 1b together. The type of binder is not particularly limited. As the binder, various binders known as constituent materials of batteries may be adopted. For example, at least one binder selected from butadiene rubber (BR)-based binders, butylene rubber (IIR)-based binders, acrylate butadiene rubber (ABR)-based binders, styrene butadiene rubber (SBR)-based binders, polyvinylidene fluoride (PVdF)-based binders, polytetrafluoroethylene (PTFE)-based binders, polyimide (PI)-based binders, carboxymethyl cellulose (CMC)-based binders, polyacrylic acid-based binders, polyacrylic acid ester-based binders, etc. may be used. In particular, the performance of PVdF-based binders is high. The PVdF-based binder may be a copolymer having units derived from a monomer other than VdF. The binder may be used alone or in combination of two or more kinds.

[0020] 1.6 Size of composite active material As described above, the composite active material 1 may have a first particle as a first active material 1a and a second active material 1b (second particle or coating layer) attached to the surface of the first particle. In other words, the composite active material 1 can be regarded as a secondary particle formed by attaching the second active material 1b to the surface of the first particle. In this case, the average particle diameter of the composite active material 1 is not particularly limited. The average particle diameter of the secondary particles of the composite active material 1 may be 100 nm or more, 1 μm or more, 2 μm or more, or 3 μm or more, and may be 100 μm or less, 50 μm or less, 20 μm or less, 15 μm or less, or 10 μm or less. The average particle diameter of the secondary particles of the composite active material 1 can be obtained by observation with an electron microscope such as SEM, and is obtained, for example, as the number average value of the maximum Feret diameter of a plurality of secondary particles. The number of samples is preferably large, and may be, for example, 20 or more, 50 or more, or 100 or more. Alternatively, the average particle diameter (D50, median diameter) of the composite active material 1 measured using a laser diffraction particle distribution measurement device may be 100 nm or more, 1 μm or more, 2 μm or more, or 3 μm or more, and may be 100 μm or less, 50 μm or less, 20 μm or less, 15 μm or less, or 10 μm or less.

[0021] 1.7 Manufacturing method of composite active material The composite active material 1 can be produced, for example, by mixing the first active material 1a, the second active material 1b, and an optional component. There is no particular limitation on the mixing method, and it may be wet mixing using a solvent or dry mixing without using a solvent. There is also no particular limitation on the mixing means, and it may be mechanically mixed using various mixing devices or may be mixed manually.

[0022] 2.Battery A configuration of a battery 100 according to one embodiment is shown in Fig. 2. As shown in Fig. 2, the battery 100 has a positive electrode active material layer 20, an electrolyte layer 30, and a negative electrode active material layer 40. In the battery 100 according to one embodiment, the negative electrode active material layer 40 contains the composite active material 1 described above.

[0023] The problem of the increase in the confining pressure is more likely to become evident when the battery 100 contains a solid electrolyte. In this regard, in the battery 100, at least one of the positive electrode active material layer 20, the electrolyte layer 30, and the negative electrode active material layer 40 may contain a solid electrolyte. In the battery 100, at least the negative electrode active material layer 40 may contain a solid electrolyte. In the battery 100, all of the positive electrode active material layer 20, the electrolyte layer 30, and the negative electrode active material layer 40 may contain a solid electrolyte. Furthermore, the battery 100 may be a solid-state battery. A solid-state battery refers to a battery in which at least a part of an electrolyte having carrier ion conductivity is composed of a solid electrolyte. However, a liquid component may be included in a part of the battery. Alternatively, the battery 100 may be an all-solid-state battery that does not substantially contain a liquid component.

[0024] 2.1 Negative electrode active material layer The negative electrode active material layer 40 may have the same configuration as the conventional negative electrode active material layer 40, except that it contains the above-mentioned composite active material 1. The negative electrode active material layer 40 may contain, for example, the above-mentioned composite active material 1, and may optionally contain an electrolyte, a conductive assistant, a binder, and the like. The negative electrode active material layer 40 may also contain other active materials. The content of each component contained in the negative electrode active material layer 40 is not particularly limited. As described above, the negative electrode active material layer 40 may contain a solid electrolyte. As the solid electrolyte, a known one may be used as a solid electrolyte for batteries. The solid electrolyte may be an inorganic solid electrolyte or an organic polymer electrolyte. In particular, the inorganic solid electrolyte is excellent in ion conductivity and heat resistance. Examples of the inorganic solid electrolyte include an oxide solid electrolyte, a sulfide solid electrolyte, and an ion-bonded inorganic solid electrolyte. Among inorganic solid electrolytes, sulfide solid electrolytes, and sulfide solid electrolytes containing at least Li, S, and P as constituent elements, have high performance. Alternatively, among inorganic solid electrolytes, ion-bonded solid electrolytes, and among them, solid electrolytes containing at least Li, Y, and halogen (at least one of Cl, Br, I, and F) as constituent elements, have high performance. The solid electrolyte may be amorphous or crystalline. The solid electrolyte may be particulate. The average particle size (D50) of the solid electrolyte may be, for example, 10 nm or more and 10 μm or less. Only one type of solid electrolyte may be used alone, or two or more types may be used in combination.

[0025] The oxide solid electrolyte is lithium lanthanum zirconate, LiPON, Li 1+X Al X Ge 2-X (PO 4 ) 3 , Li-SiO-based glass, Li-Al-SO-based glass, etc. In addition, when an oxide solid electrolyte is combined with a liquid electrolyte, ion conductivity can be improved.

[0026] The sulfide solid electrolyte may be a glass-based sulfide solid electrolyte (sulfide glass), a glass ceramic-based sulfide solid electrolyte, or a crystalline sulfide solid electrolyte. The sulfide glass is amorphous. The sulfide glass may have a glass transition temperature (Tg). In addition, when the sulfide solid electrolyte has a crystalline phase, examples of the crystalline phase include a Thio-LISICON type crystalline phase, a LGPS type crystalline phase, and an Argyrodite type crystalline phase. The sulfide solid electrolyte may contain, for example, a Li element, an X element (X is at least one of P, As, Sb, Si, Ge, Sn, B, Al, Ga, and In), and an S element. In addition, the sulfide solid electrolyte may further contain at least one of an O element and a halogen element. In addition, the sulfide solid electrolyte may contain an S element as a main component of an anion element. The sulfide solid electrolyte may contain, for example, Li 2 SP 2 S 5 , Li 2 SP 2 S 5 - LiI, Li 2 SP 2 S 5 -GeS 2 , Li 2 SP 2 S 5 -Li 2 O, Li 2 SP 2 S 5 -Li 2 O-LiI, Li 2 SP 2 S 5 -LiI-LiBr, Li 2 S-SiS 2 , Li 2 S-SiS 2 - LiI, Li 2 S-SiS 2 -LiBr, Li 2 S-SiS 2 -LiCl, Li 2 S-SiS 2 -B 2 S 3 - LiI, Li 2 S-SiS 2 -P2 S 5 -LiI, Li 2 S-B 2 S 3 , Li 2 S-P 2 S 5 -ZmSn (where m, n are positive numbers. Z is any one of Ge, Zn, Ga.), Li 2 S-GeS 2 , Li 2 S-SiS 2 -Li 3 PO 4 , Li 2 S-SiS 2 -Li x MO y (where x, y are positive numbers. M is any one of P, Si, Ge, B, Al, Ga, In.) may be at least one selected therefrom. The composition of the sulfide solid electrolyte is not particularly limited. For example, xLi 2 S·(100 - x)P 2 S 5 (70 ≤ x ≤ 80), yLiI·zLiBr·(100 - y - z)(xLi 2 S·(1 - x)P 2 S 5 )(0.7 ≤ x ≤ 0.8, 0 ≤ y ≤ 30, 0 ≤ z ≤ 30), etc. may be mentioned. Alternatively, the sulfide solid electrolyte may have a composition represented by the general formula: Li 4-x Ge 1-x P x S 4 (0 < x < 1). In the above general formula, at least a part of Ge may be substituted with at least one of Sb, Si, Sn, B, Al, Ga, In, Ti, Zr, V, and Nb. In the above general formula, at least a part of P may be substituted with at least one of Sb, Si, Sn, B, Al, Ga, In, Ti, Zr, V, and Nb. In the above general formula, a part of Li may be substituted with at least one of Na, K, Mg, Ca, and Zn. In the above general formula, a part of S may be substituted with a halogen (at least one of F, Cl, Br, and I). Alternatively, the sulfide solid electrolyte is Li 7-a PS 6-a X a(X is at least one of Cl, Br, and I, and a is a number of 0 or more and 2 or less). a may be 0 or more than 0. In the latter case, a may be 0.1 or more, 0.5 or more, or 1 or more. Also, a may be 1.8 or less, or 1.5 or less.

[0027] The ion-bonded solid electrolyte may contain at least one element selected from the group consisting of, for example, Mg, Ca, Sr, Ba, Zn, Sn, Al, Sc, Ga, Bi, Sb, Zr, Hf, Ti, Ta, Nb, W, Y, Gd, Tb and Sm. These elements may generate cations in water. The ion-bonded solid electrolyte material may further contain, for example, at least one halogen element selected from the group consisting of Cl, Br, I and F. These elements may generate anions in water. The ion-bonded solid electrolyte may contain at least one element selected from the group consisting of Gd, Ca, Zr and Y, at least one element selected from the group consisting of Cl, Br, I and F, and Li. The ion-bonded solid electrolyte may contain Li and Y, and at least one element selected from the group consisting of Cl, Br, I and F. More specifically, the ionically bonded solid electrolyte may contain Li, Y, Cl, and Br, or may contain Li, Ca, Y, Gd, Cl, and Br, or may contain Li, Zr, Y, and Cl. 3 YBr 2 Cl 4 , Li 2.8 Ca 0.1 Y 0.5 Gd 0.5 Br 2 Cl 4 , and Li 2.5 Y 0.5 Zr 0.5 Cl 6 It may be at least one of the above.

[0028] 2.2 Other configurations In addition to the above configuration, the battery 100 may have a general configuration as a battery. For example, as shown in FIG. 2, the battery 100 may have a positive electrode active material layer 20, an electrolyte layer 30, a negative electrode active material layer 40, a positive electrode current collector 10 in contact with the positive electrode active material layer 20, and a negative electrode current collector 50 in contact with the negative electrode active material layer 40. In the battery 100, the configuration other than the negative electrode active material layer 40 is the same as that of the conventional battery, and may have a configuration such as that described in Patent Document 1 (JP Patent Publication 2021-022554). The battery 100 may have each of the above configurations housed inside an exterior body. Any known exterior body for a battery can be used as the exterior body. In addition, a plurality of batteries 100 may be electrically connected and stacked in any order to form an assembled battery. In this case, the assembled battery may be housed inside a known battery case. The battery 100 may also have other obvious configurations such as necessary terminals. The battery 100 may be a secondary battery. The shape of the battery 100 may be, for example, a coin type, a laminate type, a cylindrical type, a square type, or the like. The battery 100 may be manufactured by applying a known method. For example, the battery 100 may be manufactured as follows. However, the manufacturing method of the battery 100 is not limited to the following method, and each layer may be formed by, for example, dry molding or the like. (1) The composite active material constituting the negative electrode active material layer is dispersed in a solvent to obtain a negative electrode slurry. The solvent used in this case is not particularly limited, and water or various organic solvents can be used. Thereafter, the negative electrode slurry is applied to the surface of the negative electrode current collector or the electrolyte layer described below using a doctor blade or the like, and then dried to form a negative electrode active material layer on the surface of the negative electrode current collector or the electrolyte layer, thereby forming a negative electrode. Here, the negative electrode active material layer may be press-molded. (2) The positive electrode active material constituting the positive electrode active material layer is dispersed in a solvent to obtain a positive electrode slurry. The solvent used in this case is not particularly limited, and water or various organic solvents can be used. Thereafter, the positive electrode slurry is applied to the surface of the positive electrode current collector or the electrolyte layer described below using a doctor blade or the like, and then dried to form a positive electrode active material layer on the surface of the positive electrode current collector or the electrolyte layer, thereby forming a positive electrode. Here, the positive electrode active material layer may be press-molded. (3) The layers are laminated so as to sandwich the electrolyte layer between the negative electrode and the positive electrode, and a laminate having the negative electrode current collector, the negative electrode active material layer, the electrolyte layer, the positive electrode active material layer, and the positive electrode current collector in this order is obtained. The electrolyte layer may be obtained by, for example, molding an electrolyte mixture containing an electrolyte and a binder, or by press molding. Here, the laminate may be further press molded. Other members such as terminals are attached to the laminate as necessary. When an electrolytic solution is used, a separator may be used in the electrolyte layer. (4) The laminate is housed in a battery case and sealed to obtain a secondary battery. EXAMPLES

[0029] The technology of the present disclosure will be described in more detail below with reference to examples, but the technology of the present disclosure is not limited to the following examples.

[0030] 1. Preparation of negative electrode active material 1.1 Comparative Example 0.65g of Si particles (particle size 0.5μm, manufactured by Kojundo Chemical Co., Ltd.) and 0.60g of Li metal (manufactured by Honjo Metal Co., Ltd.) were mixed in an agate mortar under an Ar atmosphere to obtain a LiSi precursor. 1.0g of LiSi precursor and 125ml of dispersion medium (1,3,5-trimethylbenzene, manufactured by Nacalai Tesque) were mixed in a glass reactor under an Ar atmosphere using an ultrasonic homogenizer (UH-50, manufactured by SMT Co., Ltd.). The LiSi precursor dispersion obtained after mixing was cooled to 0°C, and 125ml of ethanol (manufactured by Nacalai Tesque) was dripped and reacted for 120 minutes. After the reaction, 50ml of acetic acid (manufactured by Nacalai Tesque) was further dripped and reacted for 60 minutes. After the reaction, the liquid and solid reactants (nanoporous Si particles) were separated by suction filtration. The obtained solid reaction product was vacuum dried at 120° C. for 2 hours to recover nanoporous Si particles (particle diameter: 500 nm).

[0031] 1.2 Example 1 The above nanoporous Si and P (simple phosphorus, manufactured by Nacalai Tesque) were weighed out so as to have a mass ratio of nanoporous Si:P=95:5, and were crushed and mixed in a mortar to obtain a composite active material according to Example 1.

[0032] 1.3 Example 2 The above nanoporous Si and P (simple phosphorus, manufactured by Nacalai Tesque) were weighed out so as to have a mass ratio of nanoporous Si:P=90:10, and were crushed and mixed in a mortar to obtain a composite active material according to Example 2.

[0033] 2. Preparation of Solid Electrolyte Li 2 S (Furuuchi Chemical Co., Ltd.) 0.550g and P 2 S 5 0.887g of LiI (manufactured by Aldrich), 0.285g of LiI (manufactured by Nippoh Chemical), and 0.277g of LiBr (manufactured by Kojundo Chemical) were mixed in an agate mortar for 5 minutes. 4g of n-heptane (dehydrated grade, manufactured by Kanto Chemical) was added to the resulting mixture, and mechanical milling was performed for 40 hours using a planetary ball mill to obtain a sulfide solid electrolyte.

[0034] 3. Preparation of Positive Electrode Composite LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 (manufactured by Nichia Corporation) and LiNbO 3 The positive electrode active material was surface-treated using a 0.023 g conductive additive (VGCF, manufactured by Showa Denko K.K.), 0.239 g of the above sulfide solid electrolyte, 0.011 g of binder (PVdF, manufactured by Kureha Corporation), and 0.8 g of butyl butyrate (manufactured by Kishida Chemical Co., Ltd.) were mixed using an ultrasonic homogenizer (UH-50, manufactured by SMT Corporation) to obtain a positive electrode composite material.

[0035] 4. Preparation of negative electrode mixture 1.0 g of the nanoporous Si according to the comparative example, 1.0 g of the composite active material according to Example 1, or 1.0 g of the composite active material according to Example 2, 0.04 g of a conductive additive (VGCF, manufactured by Showa Denko K.K.), 0.776 g of the sulfide solid electrolyte, 0.02 g of a binder (PVdF, manufactured by Kureha Corporation), and 1.7 g of butyl butyrate (manufactured by Kishida Chemical Co., Ltd.) were mixed using an ultrasonic homogenizer (UH-50, manufactured by SMT Corporation) to obtain a negative electrode composite material.

[0036] 5. Preparation of Evaluation Batteries 1cm 2 0.065 g of the above sulfide solid electrolyte was placed in a ceramic mold at 1 ton / cm 2 The solid electrolyte layer was prepared by pressing the electrode with a pressure of 1 ton / cm. 2 The positive electrode active material layer was prepared by pressing the negative electrode mixture (0.0054 g) at a pressure of 4 ton / cm. 2 The negative electrode active material layer was produced by pressing the positive electrode current collector with a pressure of 10 ...

[0037] 6. Evaluation 6.1 Observation of composite active materials The appearance of each of the composite active materials of Examples 1 and 2 was observed by SEM, and the elements contained in the composite active materials were analyzed by EDX. Figure 3 shows an SEM image of the composite active material of Example 1 and the EDX distribution of each of Si and P in the SEM image, and Figure 4 shows an SEM image of the composite active material of Example 2 and the EDX distribution of each of Si and P in the SEM image. As shown in Figures 3 and 4, in the composite active materials of Examples 1 and 2, it can be seen that P as the second active material is dispersed and attached to at least a part of the surface of the nanoporous Si particles as the first active material.

[0038] 6.2 Confirmation of increase in confinement pressure of evaluation battery The evaluation batteries of the Comparative Example and Examples 1 and 2 were restrained at a restraining pressure of 5 MPa. The restrained evaluation batteries were CC / CV charged to 4.55 V at a 1 / 10 C rate. The negative electrode expanded due to charging, and an increase in the restraining pressure was confirmed. The increase in the restraining pressure after charging relative to the restraining pressure before charging was measured. The results are shown in Table 1 below. In Table 1 below, the increase in the restraining pressure of the evaluation battery according to the Comparative Example is set to 100, and the increase in the restraining pressure of the evaluation batteries according to Examples 1 and 2 is shown relative to each other. The smaller the value shown in Table 1, the smaller the increase in the restraining pressure.

[0039] [Table 1]

[0040] As is clear from the results shown in Table 1, in Examples 1 and 2 in which a composite active material of Si and P is used as the negative electrode active material of the battery, the battery's confining pressure during charging is less likely to increase than in the comparative example in which Si is used alone as the negative electrode active material of the battery. Here, it is known that the reaction potential between P and Li is higher than the reaction potential between Si and Li. That is, in Examples 1 and 2, it is considered that P reacts with Li before nanoporous Si reacts with Li during battery charging. In this case, it is considered that the presence of P suppresses the nanoporous Si from reacting with Li locally during battery charging, and as a result, it is considered that the local and rapid expansion of nanoporous Si is suppressed during battery charging, and the increase in the battery's confining pressure is suppressed.

[0041] In the above embodiment, the composite active material is composed of only the first active material and the second active material, but the composite active material may contain other components that do not impair the above-mentioned effects. In the above embodiment, the composite active material is composed of the first active material, porous Si, and the second active material, P, but the technology of the present disclosure is not limited to this embodiment. For example, the first active material may be non-porous Si. The second active material may be one that has a relatively high reaction potential with Li (reacts with Li before Si during charging), and an active material other than P may be used. That is, if the composite active material has the following configurations (1) to (3), it is considered that a certain effect is exhibited by the same mechanism as above. However, it is considered that the effect is more likely to be enhanced when porous Si is used as the first active material and P is used as the second active material. (1) The composite active material includes a first active material and a second active material. (2) The first active material is Si. (3) The reaction potential P between the second active material and Li 2 is a reaction potential P between the first active material and Li 1 Higher than. [Explanation of symbols]

[0042] 1 Composite active material 1a First active material 1b Second active material 100 Battery 10 Positive current collector 20 Positive active material layer 30 Electrolyte layer 40 Negative active material layer 50 Negative current collector

Claims

1. a composite active material comprising a first active material and a second active material; The first active material is Si, The reaction potential P between the second active material and Li 2 is the reaction potential P between the first active material and Li 1 Higher than Composite active material.

2. The composite active material according to claim 1 , The reaction potential P 2 and the reaction potential P 1 Difference with P 2 -P 1 is more than 0 V and 2.0 V or less; Composite active material.

3. The composite active material according to claim 1 , The first active material is porous Si; Composite active material.

4. The composite active material according to claim 1 , The second active material is P; Composite active material.

5. A battery having a positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, The negative electrode active material layer comprises the composite active material according to any one of claims 1 to 4. battery.

Citation Information

Patent Citations

  • Phosphorus-contained negative electrode composite material and preparation method therefor, and lithium ion battery

    CN105845906A

  • Phosphorus-coated negative electrode material and preparation method and application thereof

    CN114784251A

  • High-capacity high-magnification lithium ion battery negative electrode

    CN210576213U

  • Group iva functionalized particles and methods of use thereof

    JP2018138511A

  • Modified silicon particle electrodes and methods