Negative electrode material of lithium-ion battery, lithium-ion battery, manufacturing method of negative electrode material for lithium-ion batteries, and manufacturing system thereof

By surrounding silicon particles with graphite in a multi-layer petal or scale-like shape, the composite negative electrode material addresses volume change issues, enhancing lithium-ion battery performance and reducing manufacturing complexity and costs.

JP2024150525AActive Publication Date: 2024-10-23NISSHIN KASEI CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2024110950
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-10-23
Estimated Expiration
2036-04-06

AI Technical Summary

Technical Problem

Conventional lithium-ion batteries using silicon particles as negative electrode materials face issues with volume change and destruction during charging and discharging, leading to poor charge/discharge cycle characteristics and increased manufacturing complexity and costs.

Method used

A composite negative electrode material is created by surrounding silicon fine particles or their aggregates with graphite, forming a multi-layer petal or scale-like shape, which enhances the stability and collaboration of the silicon particles, thereby improving charge/discharge cycle characteristics.

Benefits of technology

The composite material results in a lithium-ion battery with stable charge/discharge capacity after repeated cycles, reducing manufacturing complexity and costs while increasing capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150525000001
    Figure 2024150525000001
  • Figure 2024150525000002
    Figure 2024150525000002
  • Figure 2024150525000003
    Figure 2024150525000003
Patent Text Reader

Abstract

To provide a hydrogen manufacturing system superior in economic and industrial property and capable of effectively using silicon waste.SOLUTION: A disclosed negative electrode material for lithium-ion batteries includes silicon fine particles and / or an aggregate or assembly of the silicon fine particles having a volume distribution with a mode diameter and a median diameter of 30 nm or less. The negative electrode material includes the aggregate or assembly in a state where it is folded into a compound petal-like or scale-like shape, and graphite surrounds at least a portion of the silicon fine particles and / or the aggregate or assembly.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a negative electrode material for a lithium ion battery, a lithium ion battery, and a method and apparatus for producing a negative electrode material for a lithium ion battery. [Background technology]

[0002] Conventionally used lithium ion batteries have a negative electrode with a mixture layer formed by mixing graphite (natural graphite, artificial graphite, etc.) as a negative electrode active material (hereinafter also referred to as "negative electrode material") and a negative electrode material using a binder on the negative electrode side. Also, the positive electrode side has a positive electrode with a mixture layer formed by mixing lithium (Li) oxide powder (LiCoO2, LiNiO2, LiMnO2, etc.) as a positive electrode active material and conductive graphite (mainly carbon black, etc.) using a binder (PVDF: polyvinylidene fluoride, etc.) and applying it. Also, the cell container of the lithium ion battery is filled with an electrolyte, and a separator (mainly a polyolefin-based porous material or a porous polypropylene sheet, etc.) is provided between the negative electrode material and the positive electrode material.

[0003] The separator described above is provided to allow the electrolyte to pass through and the movement of lithium ions to occur, and to separate the electrodes so as to prevent electrical short circuits from occurring.

[0004] Lithium-ion batteries are charged and discharged by the movement of lithium ions between the negative and positive electrode materials in the electrolyte. When charging, the lithium ions move to the negative electrode side, and when discharging, the lithium ions move to the positive electrode side. Charging is performed through an externally connected power source, and discharging is performed through an externally connected resistance (load).

[0005] Meanwhile, in the field of lithium ion batteries, a technology has been disclosed in recent years that uses silicon particles as a negative electrode active material instead of the graphite. For example, as an example of silicon particles, there is one in which single crystal silicon is crushed in a mortar and classified using a mesh to form a powder with a diameter of about 38 microns (μm) or less, which is heated to 150°C (attained temperature) at a heating rate of 30°C / min in an argon atmosphere (see Patent Document 1). In addition, as another example, liquid silicon tetrachloride is supplied into high-temperature and high-concentration zinc gas, and reacted at a high temperature of 1050°C or more to reduce silicon tetrachloride to form silicon particles, and the fine silicon is crystallized and aggregated at 1000°C or less, particularly 500 to 800°C, and then the particle size of the formed silicon particles is adjusted and collected in an aqueous zinc chloride solution. It has been disclosed that this operation allows high-purity silicon particles with a particle size of about 1 to 100 μm to be obtained, and that the particles are used (see Patent Document 2). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2005-032733 A [Patent Document 2] JP 2012-101998 A [Patent Document 3] International Publication No. WO2015 / 189926 Brochure [Patent Document 4] International Publication No. WO2013 / 027686 Brochure Summary of the Invention [Problem to be solved by the invention]

[0007] However, in the conventional technology, when silicon particles are used as the negative electrode material, the electric capacity during charging and discharging can be increased, but on the other hand, lithium is absorbed and released into the silicon particles, causing the volume of the silicon particles to change or be destroyed, resulting in a problem that the charge and discharge cycle characteristics cannot be maintained.

[0008] For example, in the case of the silicon particles disclosed in the above-mentioned Patent Documents 1 and 2, high-temperature synthesis and collection processes are required, so the manufacturing process for obtaining silicon particles as a negative electrode material becomes extremely complicated. As a result, it is inevitable that productivity will decrease and manufacturing costs will increase. In addition, the technology disclosed in Patent Document 3 is effective in that it is designed to prevent a part of the silicon particles from being electrically isolated due to, for example, expansion and contraction, but there is still room for improvement. In other words, the development of lithium-ion batteries using silicon particles is still in progress.

[0009] In light of the above-mentioned technical challenges, the inventors of the present application have conducted extensive research and analysis in order to find a higher performance negative electrode material that can be adapted to the mechanism of lithium ion batteries, without being limited to silicon particles as the material to be used as the negative electrode material.

[0010] As a result, the inventors of the present application have found that, in a unique embodiment, by incorporating certain characteristic fine silicon particles into an internal space formed by using graphite, surrounding and internalizing the particles, so to speak, integrating or combining the particles (hereinafter also referred to as "composite"), it is possible to realize a higher performance negative electrode material that significantly enhances the usefulness of the characteristic fine silicon particles. The present invention was created based on the above-mentioned viewpoint. [Means for solving the problem]

[0011] The present invention solves at least some of the problems associated with conventional negative electrode materials using silicon particles, such as problems with charge / discharge cycle characteristics, and is also expected to contribute greatly to the realization of higher performance negative electrode materials for lithium ion batteries, which are also expected to have a carbon dioxide reduction effect.

[0012] A negative electrode material for one lithium ion battery of the present invention comprises silicon fine particles and / or agglomerates or aggregates of the silicon fine particles having a volume distribution in which the mode diameter and median diameter are 30 nm or less, the agglomerates or aggregates being at least in a multi-layered petal-like or scale-like folded state, and graphite surrounds at least a portion of the silicon fine particles and / or the agglomerates or aggregates.

[0013] The above-mentioned negative electrode material contains a composite in which at least a part of the silicon fine particles and / or the aggregates or assemblies of the silicon fine particles in a state of being folded in a multi-layered petal-like or scale-like shape is surrounded by graphite. In addition, the silicon fine particles and / or the aggregates or assemblies are very fine aggregates or assemblies having a volume distribution with a mode diameter and a median diameter of 30 nm or less. Therefore, although the detailed mechanism is not yet clear, the silicon fine particles and / or the aggregates or assemblies are surrounded by graphite, in combination with the specificity of the multi-layered petal-like or scale-like shape of the aggregates or assemblies, which suppresses the degree of freedom of the silicon fine particles and / or the aggregates or assemblies to a certain extent, which leads to an increase in the cooperation between the graphite, the silicon fine particles and / or the graphite, and the aggregates or assemblies. As a result, by adopting this negative electrode material, a lithium ion battery with little change in charge / discharge capacity even when charging / discharging is repeated, in other words, with good charge / discharge cycle characteristics, can be realized. Alternatively, an increase in charge / discharge capacity can be realized.

[0014] In addition, one manufacturing apparatus for a negative electrode material for a lithium ion battery of the present invention includes a crushing unit that crushes crystalline silicon to form silicon fine particles and / or agglomerates or aggregates of the silicon fine particles having a volume distribution with a mode diameter and median diameter of 30 nm or less, the agglomerates or aggregates being in a state where the agglomerates or aggregates are folded at least into a multi-layered petal-like or scale-like shape, and a composite forming unit in which graphite surrounds at least a portion of the silicon fine particles and / or the agglomerates or aggregates, thereby forming a composite containing the graphite and the silicon fine particles, or a composite containing the graphite and the agglomerates or aggregates.

[0015] According to this manufacturing apparatus for a negative electrode material for a lithium ion battery, the pulverizing unit forms very fine silicon fine particles and / or agglomerates or aggregates of the silicon fine particles having a volume distribution with a mode diameter and a median diameter of 30 nm or less. Here, the agglomerates or aggregates are formed in a state where they are folded at least in a multi-layered petal-like or scale-like shape. In addition, this manufacturing apparatus further includes a composite forming unit that surrounds at least a portion of the silicon fine particles and / or agglomerates or aggregates with graphite to form a composite containing the graphite and the silicon fine particles, or a composite containing the graphite and the agglomerates or aggregates. Therefore, although the detailed mechanism is not yet clear, the silicon fine particles and / or the aggregates or the aggregates are surrounded by graphite, which, combined with the specificity of the multi-layered petal-like or scale-like shape of the aggregates or the aggregates, suppresses the degree of freedom of the silicon fine particles and / or the aggregates or the aggregates to a certain extent, which leads to increasing the cooperation between the graphite and the silicon fine particles and / or the graphite and the aggregates or the aggregates. As a result, this manufacturing apparatus can contribute to the manufacture of a negative electrode material for a lithium ion battery that has little change in charge / discharge capacity even when charge / discharge is repeated, in other words, has good charge / discharge cycle characteristics, or a negative electrode material for a lithium ion battery that can increase the charge / discharge capacity.

[0016] Furthermore, one method for producing a negative electrode material for a lithium ion battery of the present invention includes a crushing step of crushing crystalline silicon to form silicon fine particles and / or agglomerates or aggregates of the silicon fine particles having a volume distribution with a mode diameter and median diameter of 30 nm or less, the agglomerates or aggregates being in a state where the agglomerates or aggregates are folded at least in a multi-layered petal-like or scale-like shape, and a composite formation step of using graphite to surround at least a portion of the silicon fine particles and / or the agglomerates or aggregates, thereby forming a composite containing the graphite and the silicon fine particles, or a composite containing the graphite and the agglomerates or aggregates.

[0017] According to this method for producing a negative electrode material for a lithium ion battery, a pulverization step is performed to form very fine silicon fine particles and / or agglomerates or aggregates of the silicon fine particles having a volume distribution with a mode diameter and a median diameter of 30 nm or less. Here, the agglomerates or aggregates are formed in a state where at least the agglomerates or aggregates are folded into a multi-layered petal-like or scale-like shape. In addition, this production method further includes a composite formation step in which graphite surrounds at least a portion of the silicon fine particles and / or the agglomerates or aggregates, thereby forming a composite containing the graphite and the silicon fine particles, or a composite containing the graphite and the agglomerates or aggregates. Therefore, although the detailed mechanism is not yet clear, the silicon fine particles and / or the aggregates or the aggregates are surrounded by graphite, which, combined with the specificity of the multi-layered petal-like or scale-like shape of the aggregates or the aggregates, suppresses the degree of freedom of the silicon fine particles and / or the aggregates or the aggregates to a certain extent, which leads to increasing the cooperation between the graphite and the silicon fine particles and / or the graphite and the aggregates or the aggregates. As a result, this manufacturing apparatus can contribute to the manufacture of a negative electrode material for a lithium ion battery that has little change in charge / discharge capacity even when charge / discharge is repeated, in other words, has good charge / discharge cycle characteristics, or a negative electrode material for a lithium ion battery that can increase the charge / discharge capacity.

[0018] By the way, the crystalline silicon in each of the above-mentioned inventions includes not only single crystal silicon but also polycrystalline silicon. In addition, metallic silicon can be selected as the crystalline silicon in each of the above-mentioned inventions. Note that, the crystalline silicon in each of the above-mentioned inventions is silicon cutting chips, silicon cutting waste, or polishing waste, which is usually waste in the cutting process of silicon in the production process of silicon wafers, for example, which is a very suitable embodiment from various viewpoints such as reduction in manufacturing cost, reduction in environmental load, and reuse of resources.

[0019] Therefore, from the viewpoint of reducing manufacturing costs, easiness of procurement of raw materials, reducing environmental load, and / or utilization of resources, etc., a negative electrode material for a lithium ion battery containing crystalline silicon chips or cutting chips and graphite surrounding at least a part of the chips or cutting chips is another embodiment that can be adopted. Also, a manufacturing device for a negative electrode material for a lithium ion battery including a composite forming part in which graphite surrounds at least a part of the crystalline silicon chips or cutting chips to form a composite containing the graphite and the chips or cutting chips is another embodiment that can be adopted. In addition, a manufacturing method for a negative electrode material for a lithium ion battery including a composite forming step in which graphite surrounds at least a part of the crystalline silicon chips or cutting chips to form a composite containing the graphite and the chips or cutting chips is another embodiment that can be adopted.

[0020] Further, in each of the above-mentioned inventions, in order to make it easier or more certain to store or release lithium ions in the above-mentioned aggregates or aggregates folded in a multi-layered petal-like or scale-like state, it is another preferred embodiment to adopt a negative electrode material for a lithium ion battery in which at least a part of the surface of the above-mentioned aggregates or aggregates, or the above-mentioned chips or cutting chips, is covered with carbon. From the viewpoint of ease of storing or releasing lithium ions, it is another preferred embodiment to adopt a manufacturing device for a negative electrode material for a lithium ion battery that includes a coating forming part that forms carbon that covers at least a part of the surface of the above-mentioned aggregates or aggregates, or the above-mentioned chips or cutting chips. Similarly, it is another preferred embodiment to adopt a manufacturing method for a negative electrode material for a lithium ion battery that includes a coating forming step that forms carbon that covers at least a part of the surface of the above-mentioned aggregates or aggregates, or the above-mentioned chips or cutting chips.

[0021] In each of the above-mentioned inventions, graphite, or more positively, a so-called "layer" of graphite (e.g., graphene or graphene sheet) surrounds the above-mentioned very fine aggregates or aggregates having a unique shape. However, the graphite does not necessarily completely surround the silicon microparticles and / or the aggregates or aggregates. Therefore, it can be said that the above-mentioned composite is one in which the aggregates or aggregates are surrounded by graphite, rather than one in which the aggregates or aggregates are encapsulated in graphite. Effect of the Invention

[0022] According to one of the lithium ion battery anode materials of the present invention, it is possible to realize a lithium ion battery with little change in charge / discharge capacity even when charging / discharging is repeated, in other words, with good charge / discharge cycle characteristics. Alternatively, it is possible to realize an increase in charge / discharge capacity. In addition, according to one of the lithium ion battery anode material manufacturing apparatuses of the present invention, it is possible to contribute to the manufacture of a lithium ion battery anode material with little change in charge / discharge capacity even when charging / discharging is repeated, in other words, with good charge / discharge cycle characteristics, or a lithium ion battery anode material that can increase charge / discharge capacity. In addition, according to one of the lithium ion battery anode material manufacturing methods of the present invention, it is possible to contribute to the manufacture of a lithium ion battery anode material with little change in charge / discharge capacity even when charging / discharging is repeated, in other words, with good charge / discharge cycle characteristics, or a lithium ion battery anode material that can increase charge / discharge capacity. [Brief description of the drawings]

[0023] [Figure 1] FIG. 2 is a flow chart showing a manufacturing process of the negative electrode material of the lithium ion battery according to the first embodiment. [Diagram 2] FIG. 1 is a schematic diagram showing a manufacturing apparatus and a manufacturing process for a negative electrode material for a lithium ion battery according to a first embodiment. [Diagram 3] FIG. 4 is a diagram showing a TEM (transmission electron microscope) image of an example of silicon fine particles and / or their aggregates or conglomerates that have been subjected to the coating formation step (S4) of the first embodiment. [Figure 4A] 2 is a SEM image of an example of silicon fine particles and / or aggregates or aggregates thereof according to the first embodiment. [Figure 4B] 2 is a SEM image of an example of enlarged silicon microparticles and / or aggregates or aggregates thereof in the first embodiment. [Figure 4C] 5A is an SEM image of another example of an aggregate or conglomerate of silicon fine particles in the first embodiment, and FIG. 5B is an enlarged view of a portion of FIG. 5A. [Diagram 5] FIG. 2 is a diagram showing a TEM image of a silicon microparticle of the first embodiment. [Figure 6]2 is a graph showing (a) crystallite size distribution in number distribution and (b) crystallite size distribution in volume distribution with respect to crystallite sizes of silicon fine particles etc. of the first embodiment. [Figure 7] 2 is a graph showing the results of X-ray diffraction measurement of silicon fine particles and / or their aggregates or conglomerates according to the first embodiment ((a) wide range, (b) limited range). [Figure 8] FIG. 1 is a schematic configuration diagram of a lithium ion battery according to a second embodiment. [Figure 9] FIG. 1 is a schematic diagram showing a manufacturing apparatus and a manufacturing process for a negative electrode material for a lithium ion battery according to another embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] The embodiments of the present invention will be described in detail with reference to the accompanying drawings. In this description, common parts are given common reference symbols throughout the drawings unless otherwise specified. In addition, in the drawings, the elements of each embodiment are not necessarily shown to scale. In addition, some symbols may be omitted in order to make each drawing easier to see.

[0025] <First embodiment> Fig. 1 is a flow diagram showing the manufacturing process of the negative electrode material for lithium ion batteries of this embodiment, and Fig. 2 is a schematic diagram showing the manufacturing device and manufacturing process of the negative electrode material for lithium ion batteries of this embodiment.

[0026] The method for producing the negative electrode material of the lithium ion battery of the present embodiment and the method for producing the lithium ion battery including the negative electrode material include various steps using silicon chips, silicon cutting chips, or polishing chips (hereinafter also referred to as "silicon chips, etc." or "chips, etc.") that are usually waste materials in the cutting process of silicon in the production process of silicon wafers used in semiconductor products such as solar cells as an example of a starting material. The chips, etc. also include fine chips obtained by pulverizing silicon wafers to be discarded with a known pulverizer. As shown in FIG. 1, the method for producing the lithium ion battery of the present embodiment includes the following steps (1), (2), (5), and (6), or the following steps (1), (2), (4), (5), and (6). The method for producing the lithium ion battery of the present embodiment can further include the following step (3) as another aspect that can be adopted. (1) Cleaning process (S1) (2) Grinding process (S2) (3) Oxide film removal process (S3) (4) Covering formation process (S4) (5) Complex formation step (S5) (6) Negative electrode formation process (S6)

[0027] 2, the manufacturing apparatus 100 for the negative electrode material (or negative electrode) of the lithium ion battery of this embodiment mainly includes a washer (cleaning and preliminary crusher) 10, a crusher 20, a dryer (not shown), a rotary evaporator 40, a coating forming section 60 for forming carbon that covers at least a part of the surface of silicon fine particles and / or their aggregates or conglomerates (hereinafter also referred to as "silicon fine particles, etc."), a composite forming section 70 for forming a composite containing graphite and silicon fine particles, etc. by surrounding at least a part of the silicon fine particles, etc. with graphite, and a mixing section 80 for performing a part of the negative electrode forming process of the lithium ion battery. Note that, among the above-mentioned configurations, the manufacturing apparatus 100 for the negative electrode material (or negative electrode) of the lithium ion battery that does not include the coating forming section 60 is another embodiment that can be adopted.

[0028] In addition, the lithium ion battery negative electrode material (or negative electrode) manufacturing apparatus 100 of this embodiment can be provided with an oxide film removal tank 50 and a centrifuge 58 as another embodiment that can be adopted. Note that only the pulverizer 20, or the washer 10 and the pulverizer 20, are referred to as a pulverizing section in this embodiment.

[0029] (1) Cleaning process (S1) In the cleaning step (S1) of this embodiment, for example, silicon chips formed in the cutting process of monocrystalline or polycrystalline silicon, that is, a lump or ingot of crystalline silicon (a lump or ingot of n-type crystalline silicon), are cleaned. Representative silicon chips are chips formed by cutting a silicon ingot with a known wire or the like (typically, a fixed abrasive wire). Therefore, in this embodiment, silicon chips, which have conventionally been considered waste material, are used as a starting material to form silicon fine particles constituting the negative electrode material of a lithium ion battery, which is excellent in terms of reducing manufacturing costs, facilitating procurement of raw materials, reducing the burden on the environment, and / or utilizing resources.

[0030] The cleaning step (S1) of this embodiment is mainly intended to remove organic matter that adheres during the formation process of the silicon chips, typically organic matter such as coolant and additives used in the cutting process. In this embodiment, as shown in FIG. 2, first, the chips 1 to be cleaned are weighed, and then the chips 1, a predetermined first liquid, and balls 11 are introduced into a cylindrical pot 13a with a bottom. After the pot 13a is sealed with a lid 13b, the pot 13a on the rotors 15 is rotated by rotating two cylindrical rotors 15 of a ball mill machine, which is a cleaning machine (cleaning and preliminary crushing machine) 10. As a result, in the pot 13a, the chips 1 to be cleaned are dispersed in the first liquid, so that cleaning and preliminary crushing of the chips 1 are performed.

[0031] Here, the ball mill of this embodiment is a grinding machine that applies physical impact force by rotating the pot 13a and the lid 13b, using steel balls, porcelain balls, boulders, and the like contained in the pot 13a and the lid 13b as balls 11 (grinding media). A suitable example of the first liquid is acetone. In a more specific aspect, for example, 300 milliliters (mL) of acetone is added to 100 grams (g) of silicon chips, etc., and the mixture is stirred for about one hour in the pot 13a and the lid 13b placed on the rotor 15 of the ball mill (Universal BALL MILL, manufactured by MASUDA Co., Ltd.) to disperse the silicon chips, etc. in the acetone. The ball types of the ball mill were alumina balls with a particle diameter of 10 millimeters (mm) and alumina balls with a particle diameter of 20 mm. In the cleaning step (S1) of this embodiment, the silicon chips, etc. are pre-ground and stirred in the first liquid in the ball mill, thereby dispersing the silicon chips, etc. Therefore, the cleaning efficiency is significantly improved compared to a process in which the material is simply immersed in the first liquid, and it is possible to obtain silicon particles that are suitable for improving the negative electrode characteristics of lithium ion batteries, in particular the charge / discharge cycle characteristics.

[0032] After the cleaning step (S1), the lid 13b is opened to discharge the silicon particles together with the first liquid, and the first liquid is removed by suction filtration using a known reduced pressure filtration means to become waste liquid. Meanwhile, the remaining silicon particles are dried in a known dryer. If necessary, the silicon particles obtained after the drying process are pre-crushed and washed again in the cleaning machine (cleaning and pre-crushing machine) 10 in the same process. Examples of other cleaning methods that can be adopted in the cleaning step (S1) include cleaning using the RCA cleaning method or cleaning using water (including pure water).

[0033] (2) Grinding process (S2) Then, in the crushing step (S2), a second liquid is added to the washed silicon particles, and the silicon particles are crushed in a bead mill. Therefore, in this embodiment, the silicon particles that have been subjected to the washing step (S1) are crushed further finely by the bead mill used after the ball mill, in other words, after the crushing by the ball mill.

[0034] A suitable example of the second liquid in this embodiment is IPA (isopropyl alcohol). As a pretreatment for the pulverization step, the second liquid and the silicon particles obtained in the cleaning step (S1) are placed in the pot 13a so that the weight ratio of the second liquid is 95% and the weight ratio of the silicon particles is 5%, and then the pot 13a and the lid 13b of the cleaning machine (cleaning and preliminary pulverizer) 10 are rotated to perform a preliminary pulverization process. The slurry containing the pre-pulverized silicon particles is passed through a mesh with an opening of 180 microns to remove relatively coarse particles, and the obtained slurry containing the silicon particles is further pulverized using a bead mill (in this embodiment, Star Mill LMZ015, manufactured by Ashizawa Finding Co., Ltd.) of the pulverizer 20. More specifically, the slurry containing the silicon chips from which silicon chips with a particle diameter of 180 microns or more have been removed is introduced into the inlet 21 of the pulverizer 20, and is guided to the filter 25 on the discharge port 24 side while or after the pulverization process is being performed in the pulverizer 20. Furthermore, if the pulverization is insufficient by this process, the slurry can be circulated by using pump 28 to return to the inlet 21 of the pulverizer 20 so that the pulverization can be carried out again. An example of a specific type of beads for the bead mill is zirconia beads with a particle size of φ0.5 mm. After collecting the slurry containing the pulverized silicon particles, the second liquid is removed using a rotary evaporator 40 that automatically performs reduced pressure distillation, thereby obtaining silicon fine particles and the like as the result of the pulverization process.

[0035] In this embodiment, about 450 g of zirconia beads having a particle diameter of φ0.5 mm are introduced, and the pulverization process is performed at a rotation speed of 2900 rpm for 4 hours, thereby obtaining silicon fine particles and the like. In addition, in the pulverization step (S2), it is another embodiment that can be adopted to perform the pulverization process by any one of the pulverizers consisting of a ball mill, a bead mill, a jet mill, and a shock wave pulverizer group other than the above, or a combination of two or more of them. In addition, as the pulverizer used in the pulverization step (S2), not only an automatic pulverizer but also a manual pulverizer may be adopted. However, from the viewpoint of forming an aggregate or agglomerate of silicon fine particles in a state of being folded into a multi-layered petal shape or a scale shape as described later with high accuracy, it is preferable to adopt the pulverization step (S2) consisting of a process using a bead mill, or the pulverization step (S2) including a process using a bead mill.

[0036] In addition, another suitable embodiment that can be adopted is to further crush the silicon fine particles obtained in the above-mentioned crushing step (S2) using a known crushing machine (a representative crushing machine is Model 20D manufactured by Ishikawa Factory Co., Ltd.). This crushing treatment improves dispersibility when forming the negative electrode of a lithium ion battery, and therefore has the effect of preventing or suppressing destruction of the negative electrode due to the absorption and release of lithium with a high degree of certainty.

[0037] (3) Oxide film removal process (S3) In the present embodiment, the oxide film removing step (S3) is performed as a preferred aspect, however, even if the oxide film removing step (S3) is not performed, at least a part of the effects of the present embodiment can be achieved.

[0038] In the oxide film removal step (S3) of this embodiment, the silicon fine particles, etc. 2 obtained in the pulverization step (S2) are brought into contact with hydrofluoric acid or an aqueous ammonium fluoride solution. The silicon fine particles, etc. 2 obtained in the pulverization step (S2) are dispersed by immersing them in the hydrofluoric acid or ammonium fluoride aqueous solution. Specifically, in an oxide film removal tank 50, the silicon fine particles, etc. 2 are dispersed in the hydrofluoric acid or ammonium fluoride aqueous solution 55 using a stirrer 57, whereby oxides (mainly silicon oxide) on the surfaces of the silicon fine particles, etc. 2 are removed.

[0039] Thereafter, the silicon fine particles etc. from which the surface oxide has been partially or entirely removed are separated from the hydrofluoric acid aqueous solution by a centrifuge 58. Thereafter, the silicon fine particles etc. are immersed in a third liquid such as an ethanol solution. By removing the third liquid, silicon fine particles etc. from which the surface oxide (or oxide film) originally formed has been partially or entirely removed are obtained. When the process of removing oxides that may be present on the surface of the silicon fine particles etc. 2 is not performed, the silicon fine particles etc. are subjected to the process of coating formation step (S4), composite formation step (S5), and negative electrode formation step (S6) described below.

[0040] In the oxide film removing step (S3) of this embodiment, the silicon fine particles, etc. are immersed in hydrofluoric acid or an aqueous ammonium fluoride solution to bring the silicon fine particles, etc. into contact with hydrofluoric acid, but other methods for bringing the silicon fine particles, etc. into contact with hydrofluoric acid or an aqueous ammonium fluoride solution may also be used. For example, spraying the aqueous hydrofluoric acid solution onto the silicon fine particles, etc., in the manner of a so-called shower, is another embodiment that may be used.

[0041] (4) Covering formation process (S4) In this embodiment, the coating formation step (S4) is performed as a preferred embodiment. However, even if the coating formation step (S4) is not performed, at least a part of the effects of this embodiment can be achieved. Therefore, as already described, another embodiment that can be adopted is to perform the following (5) complex formation step (S5) without performing the coating formation step (S4) after the pulverization step (S2) or the oxide film removal step (S3).

[0042] In this embodiment, a coating forming step is performed in which a part or the whole of the surface of silicon fine particles or the like that has undergone or has not undergone the oxide film removal step (S3) is coated with a carbon film. Therefore, the silicon fine particles or the like that have undergone the coating forming step (S4) of this embodiment have at least a part of their surface covered with carbon, and therefore are thicker than silicon fine particles or the like that are not covered with carbon. In addition, since the carbon of this embodiment has electrical conductivity, a conductive negative electrode material can be formed. In addition, for example, by covering silicon fine particles or the like with carbon having a film thickness of several nm to several μm, not only a thin negative electrode is formed, but also a relatively thick negative electrode is easily formed. In addition, FIG. 3 is a TEM (transmission electron microscope) image of an example of silicon fine particles or the like (partially enlarged view) and / or their aggregates or aggregates (partially enlarged view) that have undergone the coating forming step (S4) of this embodiment. In the crystalline silicon shown in FIG. 3, a crystal plane orientation (111) (also simply referred to as "Si(111)" or "(111)"; the same applies to the notations for other plane orientations) was observed.

[0043] In addition, for example, carbon can contribute to alleviating internal stress in the negative electrode as a whole by covering silicon fine particles, and more microscopically, to alleviating internal stress in individual silicon fine particles, etc. As a result, it is possible to facilitate the manufacture of lithium ion batteries and also to improve the performance (e.g., charge / discharge cycle characteristics) of lithium ion batteries.

[0044] In addition, by forming a negative electrode material for a lithium ion battery using silicon fine particles, etc., at least a part of which is covered with carbon, it is possible to increase the charge capacity value and discharge capacity value compared to silicon fine particles, etc., that are not covered with carbon. For example, according to research by the present inventors, in the case of silicon fine particles, etc., that are not covered with carbon, when the thickness of the negative electrode material is about 30 μm, for example, the charge capacity value and discharge capacity value are less than 500 (mAh / g). However, by using silicon fine particles, etc., at least a part of which is covered with carbon, the charge capacity value and discharge capacity value can be increased by more than two times (typically about 3 to about 5 times).

[0045] In the coating formation step (S4) of this embodiment, the means for coating a part or all of the surface of the silicon fine particles, etc. (in other words, at least a part of the surface) with a carbon film is not particularly limited. For example, a method of covering at least a part of the surface of the silicon fine particles, etc. 2 with carbon by a thermal CVD method, which is an example of a chemical vapor deposition method, can be adopted. Specifically, at least a part of the surface of the silicon fine particles, etc. 2 can be coated with a carbon film by heating the silicon fine particles, etc. 2 at about 600°C or higher and about 1200°C or lower in an atmosphere containing an organic gas and / or its vapor. Therefore, a thermal CVD device, which is an example of a chemical vapor deposition device, is one aspect of the coating formation unit 60 that can be adopted in the coating formation step (S4) of this embodiment. In addition, examples of materials (or raw materials) that can be adopted in the thermal CVD method are one or more types of hydrocarbons selected from the group consisting of methane, ethane, acetylene, ethylene, propane, butane, butene, pentane, isobutane, and hexane, and / or one or more types of known aromatic hydrocarbons. Furthermore, by using copper or a copper alloy as a catalyst, acetylene can be thermally decomposed even at about 400° C., which can contribute to lowering the treatment temperature.

[0046] As described above, typically, a hydrocarbon gas is pyrolyzed on or near the heated silicon fine particles 2 to carbonize the gas, thereby covering at least a part of the surface of the silicon fine particles 2 with the carbon film, which is an example of a suitable carbon film in this embodiment and is a method with excellent productivity and industrial applicability. Note that reduced pressure thermal CVD or plasma CVD, which are other examples of chemical vapor deposition, may also be appropriately adopted.

[0047] Another example of the method for covering at least a part of the surface of the silicon fine particles, etc. 2 with a carbon film is as follows. First, a known organic compound (such as chlorinated polyethylene elastomer) or a mixture of the organic compound and graphite powder is attached or adsorbed to the silicon fine particles, etc. 2 that have been treated at least by the cleaning step (S1) and the pulverization step (S2) of this embodiment in the coating forming unit 60. Thereafter, the organic compound is heated to a temperature at which it is pyrolyzed, and the organic compound is carbonized to form the silicon fine particles, etc. 2 whose surface is at least partially covered with carbon (typically, graphene, graphite, and / or amorphous carbon). In addition, a step of baking the silicon fine particles, etc. 2 once formed in a nitrogen atmosphere or a hydrogen atmosphere at, for example, 400°C to 1200°C is additionally and / or previously performed, which is also one aspect of the modified embodiment of this embodiment. In addition, from the viewpoint of being able to highly reliably prevent, suppress, or remove the formation of an oxide film on the surface of the silicon fine particles, etc. 2, it is preferable to heat the silicon fine particles, etc. 2 in a hydrogen atmosphere.

[0048] Another embodiment that can be adopted is to form silicon fine particles, etc. 2, at least a part of which is covered with carbon, using other known means. For example, it is also possible to use a carbon film formed by a known carbon black manufacturing method (furnace method or channel method). The furnace method is a method in which creosote oil obtained by distilling coal tar is partially burned in a specified chamber in a state in which the creosote oil is turbulently diffused, and then the droplets are water-cooled. The channel method is a method in which carbon is precipitated by colliding a flame formed by burning natural gas, for example, against the cooling surface of a channel steel. However, since sulfur components derived from petroleum are included, it is more preferable to adopt the above-mentioned thermal CVD method, which is a method in which such impurity components are less likely to be mixed in. In addition, when employing each of the above-mentioned methods, for example, employing a method of applying kinetic energy to silicon fine particles or the like by appropriately employing a known mechanical structure to cover at least a part of the surface of the silicon fine particles or the like 2 and / or their aggregates or aggregates with a carbon film is a preferred embodiment, since it enables a carbon film to be formed more uniformly (for example, with good uniformity in thickness and / or density) on the surface of the silicon fine particles or the like 2 and / or their aggregates or aggregates. More specifically, employing a method of applying a carbon film to at least a part of the surface of the silicon fine particles or the like 2 and / or their aggregates or aggregates with a carbon film while rotating a chamber or tube containing the silicon fine particles or the like 2 and / or applying ultrasonic vibration to the silicon fine particles or the like 2 and / or their aggregates or aggregates is a preferred embodiment, since it enables a carbon film to be formed more uniformly on the surface of the silicon fine particles or the like 2 and / or their aggregates or aggregates.

[0049] In the first embodiment when the coating formation process (S4) is performed, the weight ratio of carbon (C) in the silicon microparticles etc. 2 that constitute the negative electrode material or part of the negative electrode is 0.1 when silicon (Si) is taken as 1. However, if the weight ratio of carbon (C) when silicon (Si) is taken as 1 is 0.05 or more and less than 0.37, a lithium ion battery that is stable and has high charging capacity and discharging capacity values ​​can be obtained.

[0050] Further, as a result of further detailed analysis by the present inventor, the film thickness of the portion where carbon (C) adheres to silicon (Si) was about 2 nm to about 3 nm when the weight ratio of carbon (C) to silicon (Si) was 0.1 when the weight ratio of carbon (C) to silicon (Si) was 1 was about 5 nm to about 10 nm when the weight ratio of carbon (C) to silicon (Si) was 0.21 when the weight ratio of carbon (C) to silicon (Si) was 1 was also about 5 nm to about 10 nm. In addition, the film thickness of the portion where carbon (C) adheres to silicon (Si) was about 50 nm to about 90 nm when the weight ratio of carbon (C) to silicon (Si) was 0.37 when the weight ratio of carbon (C) to silicon (Si) was 1. Therefore, if the thickness of the carbon (C) film attached to the silicon (Si) is 1 nm or more and less than 50 nm, and in particular, if the thickness is 2 nm or more and 10 nm or less, a lithium ion battery that is stable and has high charge capacity and discharge capacity values ​​can be obtained.

[0051] Furthermore, the charge capacity and discharge capacity of a lithium-ion battery in which at least a portion of the surface of the silicon microparticles and / or their agglomerates or aggregates is not covered with carbon (i.e., has not been subjected to the coating formation step (S4)) can be at least two times (typically about three times) higher.

[0052] (5) Complex formation step (S5) As described above, after the pulverization step (S2) or the oxide film removal step (S3), the composite formation step (S5) is performed via the coating formation step (S4) or without the coating formation step (S4). The composite formation step (S5) of this embodiment is a step of forming a composite containing graphite and silicon fine particles, etc. 2 by surrounding at least a part of the silicon fine particles, etc. 2 with graphite.

[0053] Specifically, first, silicon fine particles etc. 2 and graphite (typically, flaky graphite or expanded graphite) are introduced into the composite forming section 70. The flaky graphite or expanded graphite of the present embodiment can be formed by a method disclosed in a publicly known method.

[0054] In addition, in this embodiment, since the pulverization step (S2) is performed, very fine aggregates or aggregates of silicon fine particles (silicon fine particles, etc. 2) having a volume distribution with a mode diameter and a median diameter of 30 nm or less are formed. In addition, the aggregates or aggregates are aggregates or aggregates of silicon fine particles in a state of being folded in a multi-layered petal-like or scale-like state. Since such very fine silicon fine particles, etc. 2 are adopted, a bead mill machine similar to the bead mill machine used in the pulverizer 20 can be adopted as an example of the complex forming section 70 in which the silicon fine particles, etc. 2 and graphite are mixed, the silicon fine particles, etc. 2 are taken into the internal space formed by using the graphite, and the silicon fine particles, etc. 2 are surrounded and internalized, so to speak, and integrated or united. Other examples of the complex forming section 70 are equipment groups that use a known dry process or a known wet process in combination with a pulverizer, typically a high-speed rotary impact pulverizer. However, from the viewpoint of reducing the actual number of steps, when combining silicon fine particles etc. 2 with graphite, it is preferable to employ, as the composite forming section 70, the above-mentioned bead mill machine alone or a composite processing device including at least a bead mill machine, or a composite processing device including a high-speed rotary impact grinder.

[0055] In particular, the scaly silicon fine particles and / or their aggregates or aggregates are advantageous for compositing the graphite and the silicon fine particles 2 when the graphite and the silicon fine particles 2 are introduced into the composite forming section 70 because the silicon fine particles 2 are easily taken in between layers of graphite (particularly, expanded graphite) having a moderate distance due to the specific shape, and / or are easily surrounded by the graphite. In addition, it is preferable to adopt the scaly silicon fine particles and / or their aggregates or aggregates that have undergone the coating formation step (S4) because the silicon fine particles 2 are easily taken in between layers of graphite (particularly, expanded graphite) having a moderate distance, and / or the silicon fine particles 2 are easily surrounded by the graphite. Also, as described above, from the viewpoint of having a higher charge capacity value and discharge capacity value, it is a preferable embodiment to adopt the scaly silicon fine particles and / or their aggregates or aggregates that have undergone the coating formation step (S4).

[0056] By carrying out the composite formation step (S5), it is possible to form a state in which the very fine silicon microparticles, etc. 2 having the above-mentioned aggregates or aggregates in a state of being folded into a multi-layered petal-like or scale-like shape are surrounded by graphite. In this embodiment, it is not necessarily required to go through a process (representatively, "spheroidization") in which the edge portions of the graphite are folded so that the silicon microparticles, etc. 2 are, so to speak, taken in by the sheet-like graphite, but it is also possible to adopt a mode in which the silicon microparticles, etc. 2 are surrounded by graphite after going through such a process.

[0057] (6) Negative electrode formation process (S6) The manufacturing apparatus 100 for the lithium ion battery negative electrode material (or negative electrode) of this embodiment includes a mixing section 80 that mixes, after the pulverization step (S2) or the oxide film removal step (S3), a negative electrode material that has been or has not been treated in the coating formation step (S4), in which at least a part of silicon fine particles or the like is surrounded by graphite, with a member that constitutes a part of the negative electrode (e.g., copper foil) using a binder (e.g., ammonium carboxyl methyl cellulose (CMC) and styrene butadiene rubber (SBR), or ammonium carboxyl methyl cellulose (CMC) and polyvinyl alcohol (PVA)). The negative electrode is formed using the mixture layer formed by this mixing section 80.

[0058] <Other processes> The silicon fine particles etc. obtained by the following steps (A) to (D) can be classified, for example, in order to reduce the variation in the number distribution and / or volume distribution of the crystallite diameter of each silicon fine particle etc. (A) Washing step (S1), crushing step (S2), and complex formation step (S5) (B) A cleaning step (S1), a crushing step (S2), an oxide film removal step (S3), and a complex formation step (S5) (C) Cleaning process (S1), crushing process (S2), coating formation process (S4), and composite formation process (S5) (D) Cleaning process (S1), crushing process (S2), oxide film removal process (S3), coating formation process (S4), and composite formation process (S5)

[0059] <Analysis results of silicon fine particles etc. obtained in the first embodiment> 1. Analysis of silicon microparticles using SEM and TEM images

[0060] FIG. 4A is a SEM (scanning electron microscope) image of an example of silicon fine particles and / or their aggregates or conglomerates after the pulverization step (S2) of the first embodiment. FIG. 4B is a diagram showing an enlarged SEM image of an example of silicon fine particles and / or their aggregates or conglomerates after the pulverization step (S2) of the first embodiment. FIG. 4C is (a) a diagram showing an SEM image of another example of an aggregate or conglomerate of silicon fine particles in the first embodiment, and (b) an enlarged view of a portion of (a). In addition, FIG. 5 is a diagram showing a transmission electron microscope (TEM) image of silicon fine particles of the first embodiment.

[0061] As shown in Fig. 4A, not only individual silicon fine particles but also silicon fine particles and / or their aggregates or conglomerates shown in Y1 and Y2 were confirmed. Interestingly, when analyzed in more detail, it was confirmed that the silicon fine particles or their aggregates were aggregates or conglomerates in which thin-layer silicon fine particles were folded into a compound petal-like or scale-like shape, as shown in Fig. 4B and the Z portion of Fig. 4C(a) and (b). Furthermore, when observed in more detail, for example, when the width (minor axis) of one or a group of scale-like silicon fine particles was taken as 1, the range of the length (major axis) was 3.3 to 12.9.

[0062] Another interesting finding was obtained from the TEM image shown in FIG. 5, which focuses on individual silicon microparticles. Specifically, it was confirmed that the individual silicon microparticles shown in the areas surrounded by white lines in FIG. 5 are crystalline, that is, single crystal silicon. In addition, it was confirmed that at least a part of the silicon microparticles are irregular polygonal crystallites with sizes of about 2 nm to about 10 nm in cross-sectional view. In FIG. 5, the crystal plane orientation is shown in each area surrounded by white lines.

[0063] 2. Analysis of crystallite size distribution of silicon microparticles using X-ray diffraction method Figure 6 is a graph showing (a) the crystallite size distribution in number distribution and (b) the crystallite size distribution in volume distribution with respect to the crystallite size in the Si(111) direction of silicon fine particles etc. of the first embodiment. Figure 6 shows the results obtained by analyzing the crystallite size distribution of silicon fine particles etc. after the grinding step (S2) using an X-ray diffraction method. In both Figures 6(a) and 6(b), the horizontal axis represents the crystallite size (nm) and the vertical axis represents the frequency.

[0064] From the results of Figures 6(a) and 6(b), in the number distribution, the mode diameter was 1.6 nm and the median diameter (50% crystallite diameter) was 2.6 nm. In addition, in the volume distribution, the mode diameter was 6.3 nm and the median diameter was 9.9 nm. Therefore, it was confirmed that in the number distribution, both the mode diameter and the median diameter were 5 nm or less, more specifically, 3 nm or less. It is noteworthy that in the volume distribution, both the mode diameter and the median diameter were at least 50 nm or less, particularly 30 nm or less, and more narrowly 20 nm or less. Furthermore, in Figure 6, it was confirmed that an extremely small value of 10 nm or less was realized.

[0065] From the results of Figures 6(a) and 6(b), it was confirmed that the silicon fine particles obtained after the grinding step (S2) using the bead mill method have an average crystallite size of about 20 nm or less, more specifically, about 9.8 nm, which achieves 10 nm or less. The crystallite size distribution of the silicon fine particles after the oxide film removal step (S3) is also almost the same as that shown in Figure 6.

[0066] Therefore, by analyzing the results of Fig. 6 together with the results of each diagram in Fig. 4, it can be said that the aggregates or aggregates of silicon fine particles etc. at least after the crushing step (S2) or the oxide film removal step (S3) are in a state where thin-layered silicon fine particles etc. with a major axis of about 100 nm or less are piled up in a multi-layered petal-like or scale-like shape. Also, as can be seen from Figs. 5 and 6, the silicon fine particles etc. are mainly composed of crystallites with a major axis of 10 nm or less.

[0067] In addition, as shown in FIG. 6, the silicon fine particles of this embodiment contain silicon fine particles having a crystallite diameter of 1 nm or less. Interestingly, it was also confirmed that the average crystallite diameter in the volume distribution of the silicon fine particles of this embodiment is about 10 nm. This value can be said to be a very small value. As described above, further investigation confirmed that the apparent volume diameter of the silicon fine particles is in the range of about 100 nm or less. In particular, by containing a large number of extremely fine silicon particles having a crystallite diameter of 5 nm or less, the charge and discharge cycle characteristics derived from the silicon fine particles used as the negative electrode material of the lithium ion battery described later are more accurately improved. In addition, since at least a part of the surface of the extremely fine silicon particles described above is covered with carbon, it is possible to realize higher charge capacity values ​​and discharge capacity values, as well as excellent charge and discharge cycle characteristics.

[0068] 3. Analysis of crystallite plane orientation of silicon microparticles using X-ray diffraction method Fig. 7(a) shows the results of X-ray diffraction measurement (P) of silicon fine particles and / or their aggregates or aggregates before the grinding step (S2) of the first embodiment, and the results of X-ray diffraction measurement (Q) of silicon fine particles and / or their aggregates or aggregates after the grinding step (S2) in a wide angle range. Fig. 7(b) shows an enlarged view of a part of the result (P) of Fig. 7(a), and shows the results of X-ray diffraction measurement (R) of silicon fine particles and / or their aggregates or aggregates after the grinding step (S2) of the first embodiment, in a limited angle range. The peak intensities of the C(002) and C(003) planes shown in Fig. 7(b) indicate that about 1 wt% to about 3 wt% of graphite particles are contained in the silicon fine particle group or the aggregates or aggregates of silicon fine particles. As an example, the size of the graphite particles on the C(002) plane was approximately 50 nm or less, more specifically, approximately 35 nm, and the size of the graphite particles on the C(003) plane was approximately 100 nm or less, more specifically, approximately 75 nm.

[0069] As shown in Figs. 7(a) and (b), it was confirmed that the diffraction peak attributable to the Si (111) crystal plane (111) after the grinding step (S2) had a larger half-width than the diffraction peak attributable to the Si crystal plane (111) around 2θ = 28.4 ° before the grinding step (S2) of the first embodiment. The average crystallite size calculated using Scherrer's formula from the half-width of the Si (111) peak after the grinding step (S2) was 9.8 nm. Interestingly, it was revealed that the intensity of the diffraction peak attributable to Si (111) around 2θ = 28.4 ° after the grinding step (S2) was larger than the intensity of other diffraction peaks (for example, the peak intensity of Si (220) or Si (311)). The arrangement interval of Si (111) in the crystal lattice of the silicon fine particles after the grinding step (S2) is 0.31 nm (3.1 Å) as shown in Fig. 5.

[0070] Considering the above analytical results, it can be said that the silicon fine particles, etc. obtained after the crushing step (S2) of this embodiment are aggregates or conglomerates of crystalline silicon fine particles, etc. mainly having a (111) plane orientation, which are in a state of being multi-layered petal-like or scale-like and overlapping in multiple layers.

[0071] In this case, by using the silicon fine particles and / or their aggregates or aggregates after the crushing step (S2) or the oxide film removal step (S3) of this embodiment as a part of the negative electrode material of the lithium ion battery, the lithium ions (Li + When the lithium ions (Li + ) can easily penetrate into and escape from gaps between the folds of aggregates or aggregates in a state where the aggregates or aggregates are in a multi-layered petal-like or scale-like state.

[0072] In addition, in this embodiment, at least a part of the aggregates or aggregates of silicon fine particles in the above-mentioned multi-layered petal-like or scale-like folded state is surrounded by graphite. Therefore, the presence of the aggregates or aggregates in the multi-layered petal-like or scale-like folded state results in a negative electrode material or negative electrode in which lithium ions are easily stored and released. In addition, the aggregations or aggregates have a unique shape in the multi-layered petal-like or scale-like shape, and the aggregations or aggregates are surrounded by graphite, which suppresses the degree of freedom of the aggregations or aggregates to a certain extent, thereby increasing the cooperation between the graphite and the aggregations or aggregates, and thus realizing a high degree of stability in the movement state of lithium ions. As a result, by adopting this negative electrode material, a lithium ion battery with little change in charge and discharge capacity even when charging and discharging are repeated, in other words with good charge and discharge cycle characteristics, can be realized. Alternatively, an increase in charge and discharge capacity can be realized.

[0073] <Modification of the first embodiment> In the first embodiment, one of the possible variations is to perform a process of forming a complex by a complex formation step (S5) using a complex formation unit 70, for example, without performing a crushing step (S2) on silicon chips or the like (more specifically, chips or cutting chips of crystalline silicon) obtained as a result of performing only the cleaning step (S1). As in the first embodiment, an oxide film removal step (S3) may be performed after the cleaning step (S1). As in the first embodiment, a coating formation step (S4), i.e., a coating formation step using a coating formation unit 60, for example, for forming carbon that covers at least a part of the surface of the chips or cutting chips, may be performed after the cleaning step (S1), or after the cleaning step (S1) and the oxide film removal step (S3).

[0074] In this modification, as described above, graphite surrounds at least a portion of the silicon chips, etc. obtained only by the cleaning step (S1). In addition, in this modification, the silicon chips, etc. and graphite (typically, flaky graphite or expanded graphite) are introduced into the composite forming section 70 used in the first embodiment. Thereafter, a process similar to the composite forming step (S5) in the first embodiment is performed to form a composite in which at least a portion of the silicon chips, etc. are surrounded by graphite.

[0075] Even when this modified example is adopted, the same effects as those of the first embodiment, or at least some of the effects, can be achieved.

[0076] <Second embodiment> The lithium ion battery of this embodiment uses silicon chips or silicon fine particles surrounded by graphite as the negative electrode material in the following modes (1) to (3). The configuration other than the negative electrode material is the same as that of a conventional CR2032 type coin cell lithium ion battery. (1) Silicon microparticles in a petal-like or scale-like folded state and / or aggregates or clusters of silicon microparticles, at least partially surrounded by graphite. (2) In (1), at least a portion of the surface of the silicon fine particles and / or the aggregates or conglomerates is covered with carbon. (3) Crystalline silicon chips or shavings at least partially surrounded by graphite.

[0077] 8 is a schematic diagram of a lithium ion battery 500 of this embodiment. The lithium ion battery 500 of this embodiment includes a negative electrode 512 electrically connected to a negative electrode material 514, a positive electrode 516 electrically connected to a positive electrode material 518, a separator 520 that electronically insulates the negative electrode material 514 from the positive electrode material 518, and an electrolyte 530 in a container 510 of a CR2032 coin cell. The lithium ion battery 500 of this embodiment also includes an external circuit including a power source 540 and a resistor 550 connected to the negative electrode 512 and the positive electrode 516 to realize charging and discharging.

[0078] The lithium ion battery 500 of this embodiment is manufactured as follows.

[0079] Regarding the method for producing the negative electrode, first, about 0.3 g of the silicon fine particles etc., at least a part of which is surrounded by graphite, or the silicon fine particles etc., at least a part of which is covered by carbon on the surface and at least a part of which is surrounded by graphite, as produced in the first embodiment (hereinafter collectively referred to as "negative electrode active material"), is dispersed in about 10 mL (milliliter) of a solution consisting of a 1 wt % CMC binder aqueous solution and an SBR binder aqueous dispersion (TRD2001, manufactured by JSR Corporation).

[0080] In this embodiment, the silicon fine particles, etc., carbon black, CMC binder aqueous solution, and SBR binder aqueous dispersion are mixed in this order in a dry weight ratio of 67:11:13:9 or 50:25:20:5. In one modification of this embodiment, the silicon fine particles, etc., carbon black, CMC binder aqueous solution, and PVA binder aqueous dispersion are mixed in this order in a dry weight ratio of 50:25:20:5.

[0081] Next, the slurry mixed and prepared using an agate mortar is applied to one side of a copper foil having a thickness of 15 μm and a size of about 9 cm (length) × 10 cm (width) so that the thickness after drying will be about 30 μm to about 200 μm, and then dried on a hot plate in the air at 80°C for about 1 hour. Then, the copper foil and the dried slurry are punched out into a circle having a diameter of 11.3 mm corresponding to the battery standard CR2032 type coin cell to form a working electrode. After measuring the weight of this working electrode, it is dried again by vacuum heating at 120°C for 6 hours in a glove box, and then attached to the inner surface of the negative electrode 512 made of copper foil, thereby producing the negative electrode of this embodiment.

[0082] Next, for the positive electrode, in order to evaluate the characteristics of the negative electrode material using a lithium ion battery with a half-cell structure, a lithium substrate was punched into a circle with a diameter of 13 mm and used as the positive electrode 516. Note that for the positive electrode of the lithium ion battery, a known positive electrode can be used instead of the above-mentioned positive electrode 516.

[0083] The separator 520 of this embodiment is a porous polypropylene sheet. In addition, the electrolyte 530 of this embodiment is an electrolyte in which 1 mole of lithium hexafluorophosphate (LiPF6) is dissolved in a solvent (1 L) of ethylene carbonate (EC) / diethyl carbonate (DEC) mixed at a volume ratio of 1 / 1, or an electrolyte to which fluoroethylene carbonate (FEC) is added, and is injected in an amount that is within the amount that fills the internal volume (about 1 mL) of a CR2032 coin cell.

[0084] The above-mentioned positive electrode material and positive electrode material 518, positive electrode 516, negative electrode material and negative electrode material 514, negative electrode 512, separator 520, and electrolyte 530 are placed in a container 510 of a CR2032 type coin cell. After that, in a glove box with an argon atmosphere, while insulating the positive electrode 516 and the negative electrode 512 of the outer frame of the coin cell, the components of the separator 520 and electrolyte 530 are sealed in the container 510, thereby producing a prototype lithium ion battery 500 of a CR2032 type coin cell.

[0085] In addition, examples of the electrolytic solvent constituting the electrolytic solution 530 in this embodiment are mixed solvents of cyclic carbonates such as ethylene carbonate (EC) and propylene carbonate (PC) (polypropylene sheet), and chain carbonate organic solvents such as dimethyl carbonate (DMC) and diethyl carbonate (DEC). In addition, supporting salts such as lithium hexafluorophosphate (LiPF) and lithium tetrafluoroborate (LiBF) can be dissolved in the above-mentioned electrolytic solvent and used.

[0086] By adopting the above-mentioned structure, the presence of the above-mentioned silicon fine particles, or the specificity of the multi-layered petal-like or scale-like shape of the aggregates or assemblies, combined with the fact that they are surrounded by graphite, suppresses the degree of freedom of the above-mentioned silicon fine particles and / or the aggregates or assemblies to a certain extent, which leads to increasing the cooperation between the graphite and the silicon fine particles and / or the graphite and the aggregates or assemblies. As a result, by adopting this negative electrode material, it is possible to realize a lithium ion battery with little change in charge / discharge capacity even when charging and discharging are repeated, in other words, with good charge / discharge cycle characteristics. Alternatively, it is possible to realize an increase in charge / discharge capacity.

[0087] <Other embodiment (1)> In the above-mentioned embodiments, silicon chips formed in the cutting process of a single crystal or polycrystalline silicon lump or ingot are exemplified as the starting material, but other forms of silicon chips can also be used as the starting material. Specifically, silicon chips are not limited to those inevitably formed in the cutting process of a silicon ingot in the production process of semiconductor products, but can also be produced by cutting a preselected crystalline silicon ingot uniformly or randomly with a cutting machine. In addition, so-called silicon waste materials such as silicon chips and silicon polishing chips, which are usually considered waste, can be the starting material for the silicon fine particles of the above-mentioned embodiments, but the silicon waste materials can also include fine chips obtained by crushing wafer fragments, waste wafers, etc. Furthermore, silicon fine particles using materials such as metallic silicon chips, metallic silicon polishing chips, or metallic silicon or other particulate materials as the starting material can also be used.

[0088] <Other embodiment (2)> In addition, the impurity concentration of the n-type crystalline silicon in each of the above-mentioned embodiments is not particularly limited. In addition, not only n-type but also p-type crystalline silicon can be adopted. Furthermore, crystalline silicon, which is a true semiconductor, can also be adopted as the crystalline silicon in each of the above-mentioned embodiments. Since the movement of electrons in the negative electrode material of the lithium ion battery is important, it is more preferable to use crystalline silicon containing n-type impurities. In addition, since about 1 wt% to about 3 wt% of graphite particles indicated by the peak intensities of the C(002) plane and the C(003) plane shown in the above-mentioned FIG. 7(b) are contained in the group of silicon fine particles or the aggregate of silicon fine particles, it is noted that a part or all of these graphite particles can contribute to improving the conductivity of the negative electrode material.

[0089] <Other embodiments (3)> Furthermore, the silicon microparticles and the lithium ion batteries including the same in the above-described embodiments are not limited to application to the coin cell type structure introduced in the second embodiment, and can therefore be applied to various devices or apparatuses that include or use lithium ion batteries with a larger electric capacity than those in the coin cell type structure.

[0090] <Other embodiments (4)> Also, as an alternative to the lithium ion battery negative electrode material (or negative electrode) manufacturing apparatus 100 shown in FIG. 2 in the first embodiment described above, a lithium ion battery negative electrode material (or negative electrode) manufacturing apparatus 200 shown in FIG. 9 may be adopted. Specifically, from the viewpoint of simplifying the equipment and / or reducing manufacturing costs, in the lithium ion battery negative electrode material (or negative electrode) manufacturing apparatus 200, a cleaning machine 10 for cleaning silicon chips formed in the silicon cutting process also serves as a crusher 20 for forming silicon fine particles 2 by crushing the cleaned silicon chips. Therefore, in the apparatus / method shown in FIG. 9, for example, beads with a relatively large diameter are used in the cleaning process and beads with a relatively small diameter are used in the crushing process to obtain silicon fine particles 2 to be used as a lithium ion battery negative electrode material. However, in order to obtain the silicon fine particles 2 described in the first embodiment with a higher degree of accuracy, it is preferable to form the silicon fine particles 2 by a bead mill machine after processing using a ball mill machine as in the first embodiment.

[0091] <Other embodiments (5)> Furthermore, according to the analysis by the present inventors, it has become clear that the amount of fluoroethylene carbonate (FEC) added to the electrolyte 530 in the second embodiment can affect the charge capacity value, the discharge capacity value, and the charge / discharge cycle characteristics. This is because a good (e.g., low-resistance and / or thin) solid electrolyte interface (SEI) is formed on the surface of the negative electrode material.

[0092] The disclosure of each of the above-mentioned embodiments is described for the purpose of explaining the embodiments, and is not described for the purpose of limiting the present invention. In addition, modifications within the scope of the present invention, including other combinations of each embodiment, are also included in the scope of the claims. [Industrial Applicability]

[0093] The negative electrode material for a lithium ion battery of the present invention and a lithium ion battery including the same can be suitable for a wide variety of devices or apparatuses including, for example, various power generation or storage devices (including small home power storage devices and large power storage systems), smartphones, personal digital assistants, portable electronic devices (mobile phones, portable music players, notebook computers, digital cameras and videos), electric vehicles, hybrid electric vehicles (HEVs) or plug-in hybrid electric vehicles (PHEVs), motorcycles powered by a motor as a power source, three-wheeled vehicles powered by a motor as a power source, other transportation machines or vehicles, and the like. [Explanation of symbols]

[0094] 1 Chips etc. 2. Fine silicon particles, etc. 10. Washing machine (washing and pre-grinding machine) 11. Ball 13a Pot 13b Lid 15 Rotating Body 20 Crusher 21 Introduction 22 Processing Room 24 Outlet 25 Filters 40 Rotary Evaporator 50 Oxide film removal tank 55 Hydrofluoric acid or ammonium fluoride aqueous solution 57 Mixer 58 Centrifuge 60 Covering Formation Division 70 Complex formation part 80 Mixing section 100 Manufacturing equipment for negative electrode materials (or negative electrodes) of lithium ion batteries 500 Lithium-ion battery 510 Container 512 Negative electrode 514 Anode materials and anode materials 516 Positive electrode 518 Cathode materials and cathode materials 520 Separator 530 Electrolyte 540 Power supply 550 Resistance

Claims

1. Silicon fine particles having a volume distribution in which the mode diameter and the median diameter are 30 nm or less and / or aggregates or conglomerates of the silicon fine particles, the aggregates or conglomerates being in a state where they are folded at least in a multi-layered petal-like or scale-like shape, Graphite surrounds at least a portion of the silicon fine particles and / or the aggregates or conglomerates. A negative electrode material for lithium-ion batteries.

2. At least a portion of the surface of the silicon fine particles and / or the aggregates or conglomerates is covered with carbon. The negative electrode material for a lithium ion battery according to claim 1.

3. The silicon fine particles and / or the aggregates or the conglomerates have a volume distribution in which the mode diameter and the median diameter are 20 nm or less. The negative electrode material for a lithium ion battery according to claim 1 or 2.

4. In an X-ray diffraction measurement of the silicon fine particles and / or the aggregates or the conglomerates, the intensity of a diffraction peak attributable to Si(111) near 2θ=28.4° is greater than the intensities of other diffraction peaks. The negative electrode material for a lithium ion battery according to any one of claims 1 to 3.

5. The graphite is expanded graphite. The negative electrode material for a lithium ion battery according to any one of claims 1 to 4.

6. containing swarf or cuttings of crystalline silicon, and Graphite surrounds at least a portion of the chips or cutting debris; A negative electrode material for lithium-ion batteries.

7. At least a portion of the surface of the chip or cutting chip is covered with carbon. The negative electrode material for a lithium ion battery according to claim 6.

8. The negative electrode material of a lithium ion battery according to any one of claims 1 to 7 is provided. Lithium-ion battery.

9. A device comprising the lithium ion battery of claim 8.

10. a grinding section for grinding crystalline silicon to form silicon fine particles having a volume distribution with a mode diameter and a median diameter of 30 nm or less and / or aggregates or conglomerates of the silicon fine particles, the aggregates or conglomerates being in a state of being folded at least in a multi-layered petal-like or scale-like shape; and a composite forming portion in which the graphite surrounds at least a portion of the silicon fine particles and / or the agglomerates or the aggregates to form a composite containing the graphite and the silicon fine particles, or the graphite and the agglomerates or the aggregates. Equipment for manufacturing negative electrode materials for lithium-ion batteries.

11. A coating forming unit that forms carbon to cover at least a portion of the surface of the silicon fine particles and / or the aggregates or the conglomerates. The apparatus for producing a negative electrode material for a lithium ion battery according to claim 10.

12. The crystalline silicon is chips or shavings cut by a fixed abrasive wire. An apparatus for producing a negative electrode material for a lithium ion battery according to claim 10 or 11.

13. The grinding unit includes a ball mill and a bead mill used after the ball mill. An apparatus for producing a negative electrode material for a lithium ion battery according to any one of claims 10 to 12.

14. A composite forming portion in which the graphite surrounds at least a portion of the crystalline silicon chips or cutting chips to form a composite containing the graphite and the chips or cutting chips. Equipment for manufacturing negative electrode materials for lithium-ion batteries.

15. The complex forming section includes a bead mill. The apparatus for producing a negative electrode material for a lithium ion battery according to claim 14.

16. A coating forming unit that forms carbon to cover at least a portion of the surface of the chip or the cutting chip is further provided. An apparatus for producing a negative electrode material for a lithium ion battery according to claim 14 or 15.

17. a grinding step of grinding crystalline silicon to form silicon fine particles having a volume distribution with a mode diameter and a median diameter of 30 nm or less and / or aggregates or conglomerates of the silicon fine particles, the aggregates or conglomerates being in a state of being folded at least in a multi-layered petal-like or scale-like shape; A composite forming step in which the graphite surrounds at least a portion of the silicon fine particles and / or the agglomerates or the aggregates to form a composite containing the graphite and the silicon fine particles, or the graphite and the agglomerates or the aggregates. A method for producing negative electrode materials for lithium-ion batteries.

18. A coating formation step of forming carbon to cover at least a portion of the surface of the silicon fine particles and / or the aggregates or conglomerates, A method for producing the negative electrode material of a lithium ion battery according to claim 17.

19. The crystalline silicon is chips or shavings cut by a fixed abrasive wire. A method for producing the negative electrode material of a lithium ion battery according to claim 17 or 18.

20. In the pulverization step, the crystalline silicon is pulverized by a ball mill and then pulverized by a bead mill to form the aggregates or the conglomerates. A method for producing the negative electrode material of a lithium ion battery according to any one of claims 17 to 19.

21. A composite forming step in which the graphite surrounds at least a portion of the crystalline silicon chips or cuttings to form a composite containing the graphite and the chips or cuttings; A method for producing negative electrode materials for lithium-ion batteries.

22. In the complex formation step, the complex is formed by a bead mill. A method for producing the negative electrode material of a lithium ion battery according to claim 21.

23. The coating step further includes forming carbon to cover at least a portion of the surface of the chip or the cutting chip; A method for producing the negative electrode material of a lithium ion battery according to claim 21 or 22.

Citation Information

Patent Citations

  • High-capacity negative electrode materials for lithium secondary batteries

    JP2006525625A

  • Negative electrode material for lithium secondary battery, negative electrode for lithium ion secondary battery, and lithium ion secondary battery

    JP2012043546A

  • METHOD FOR MANUFACTURING SILICON FINE PARTICLE, AND Si INK, SOLAR CELL AND SEMICONDUCTOR DEVICE USING THE SILICON FINE PARTICLE

    JP2012229146A

  • Method for producing negative electrode material of lithium ion battery, lithium ion battery, method of manufacturing negative electrode material of lithium ion battery, and manufacturing apparatus thereof

    JP2017188329A

  • Anode material for lithium ion battery, lithium ion battery, method for manufacturing anode material for lithium ion battery and manufacturing device thereof

    JP7525191B2