Large format battery anode including silicon particles

The Si-cPAN anode addresses the scalability and stability issues of silicon-based lithium-ion batteries by using a conductive polymer binder and optimized manufacturing processes, resulting in high energy density and long-term performance.

JP2024150658AActive Publication Date: 2024-10-23SILLION INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024118430
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2016-10-13
Filing Date
2024-07-24
Publication Date
2024-10-23
Estimated Expiration
2037-10-13

AI Technical Summary

Technical Problem

Existing lithium-ion batteries face challenges in achieving high energy density and commercial scalability due to the volumetric expansion of silicon anodes, which leads to structural degradation and instability of the solid-electrolyte interface, limiting their performance and lifespan.

Method used

The development of a silicon-cyclized polyacrylonitrile (Si-cPAN) anode with a conductive polymer binder, processed through specific slurry preparation, coating, and thermal treatment methods, enabling high silicon payload and adhesion to current collectors, suitable for large-scale manufacturing.

Benefits of technology

The Si-cPAN anode achieves long-term cycling stability and high energy density, maintaining structural integrity and electrochemical performance, making it commercially viable for large format Li-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024150658000001_ABST
    Figure 2024150658000001_ABST
Patent Text Reader

Abstract

To provide a large-scale anode containing a high weight percentage of silicon suitable for use in a lithium ion energy storage device and a battery, and a method for making the same.SOLUTION: An anode material described herein can include a thin film cast onto a current collector substrate, the thin film includes a plurality of active material particles and a conductive polymer film coated on the active material particles. In some embodiments, the conductive polymer film includes polyacrylonitrile (PAN). A method of manufacturing an anode material can include preparing a slurry including active material particles and a conductive polymer material, casting the slurry onto a current collector substrate, and subjecting the composite material to drying and heat treatment.SELECTED DRAWING: Figure 1A
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATION(S) This application claims priority to U.S. Provisional Patent Application No. 62 / 407,938, filed October 13, 2016, the entirety of which is incorporated herein by reference.

[0002] STATEMENT REGARDING FEDERALLY FUNDED RESEARCH This invention was made with Government support under Grant No. DE-SC0013852 awarded by the Department of Energy. The Government has certain rights in this invention.

[0003] The present disclosure relates to energy storage devices such as lithium ion electrochemical cells and batteries. More specifically, the present disclosure relates to the scalable production of silicon anode electrode sheets suitable for use in, for example, lithium ion energy storage devices and batteries. [Background technology]

[0004] Batteries have become ubiquitous in today's society, powering everything from hearing aids to smartphones, forklifts, and even transportation equipment. Today's battery technologies range from heavy, bulky, and inexpensive lead-acid batteries to lighter, smaller, and more expensive lithium-ion batteries (LIBs). However, rechargeable LIBs have dominated the portable electronics market for nearly a decade, and in recent years they have gained significant traction in the electric transportation sector and specialty markets, including military applications. Minor improvements in materials processing and device manufacturing have allowed for energy density improvements of roughly 5 to 6% each year, a slow, incremental development. To date, improvements in Li-ion technology have primarily succeeded in modifying first-generation materials and fitting them into smaller, safer packages. Prior art batteries are still heavy, bulky, expensive, and unsafe, creating obstacles to the power / cost requirements of next-generation applications. Reaching future energy storage goals will require breakthroughs in next-generation electrode materials, incorporating active materials with higher energy density.

[0005] In recent years, silicon has been identified as one of the most attractive high-energy anode materials for LIBs. Its low operating voltage and high energy capacity (3579 mAhg) are nearly 10 times higher than that of prior art graphite anodes. -1The high theoretical specific capacity of Si has encouraged extensive research activities aimed at developing a viable Si-based electrode. Despite the advantages of Si electrodes, a number of challenges, mainly linked to the severe volume expansion of the material, have hindered their commercialization. While commercial graphite electrodes expand by roughly 10 to 13% during lithium intercalation, the expansion of Si reaches nearly 300%, causing structural degradation and instability of the critical solid-electrolyte intercalation (SEI). Such instability ultimately shortens the battery life to an insufficient level. The degradation of the active material can be mitigated by incorporating materials smaller than 150 nm or by nanostructural design of the electrode architecture, which can reduce the expansion. Unfortunately, the electrode architectures presented in previous works lack sufficiently high coulombic efficiency, mainly because the volume change during Si alloying and dealloying mechanically destabilizes the SEI at the Si-electrolyte interface.

[0006] Many activities aimed at the use of silicon in lithium-ion battery anodes have been working to combine silicon with traditional active materials, which provides higher capacity while minimizing the drawbacks of silicon materials (e.g., volume expansion, active material utilization, etc.). The incorporation of nanosilicon (nano-Si) particles in prior art graphite electrodes has been implemented in commercial practice to increase the capacity of today's anodes. However, this process is limited to the inclusion of only about 5% (by mass) nanosilicon active material. Any amount above the 5% limit would destroy the traditional network of the electrode due to the intense volume expansion and contraction of Si during lithiation and delithiation.

[0007] Preliminary work conducted by applicant has demonstrated impressive long-term cycling stability of a nano-Si electrode / room-temperature ionic liquid (RTIL or IL) system and its combination with a commercially available "L333" cathode for Li-ion cells that can deliver 1.35 times the specific energy of today's prior art technology normalized to the electroactive material mass. A nano-silicon-cyclized polyacrylonitrile (nSi-cPAN) electrode, when combined with an imide-based RTIL electrolyte, maintains an average half-cell coulombic efficiency of greater than 99.97% due to the synergistic effect of a robust electrode architecture and the formation of a stable solid-electrolyte intercalation (SEI) layer. US Pat. No. 6,399,433, which is incorporated herein by reference in its entirety, describes a composition formed during the combination and use of a nSi-cPAN electrode and a RTIL electrolyte of a particular composition in a Li-ion battery. Specifically, US Pat. No. 6,399,433 discloses the composition of the SEI formed between the nSi-cPAN electrode and the RTIL electrolyte.

[0008] Following the demonstration of the nSi-cPAN system, applicants developed a "micron-Si" (μSi) anode. The utilization of μSi is made possible by exploiting the mechanical strength of the cPAN coating. By encapsulating the μSi particles in a durable, conductive coating matrix, the pulverization of the larger Si particles is inhibited. This mechanism is called "self-inhibited fragmentation." The fragmented silicon particles remain attached to the cPAN coating matrix, allowing long-term full utilization of the material with minimal capacity fade. This mechanism is verified by the ability of the electrode to retain its capacity over many cycles, proving that the silicon particles maintain access to the electronically conductive cPAN matrix even after pulverization. This is demonstrated in FIG. 1 and described in US Pat. No. 5,339,363, which describes a composition formed by electrochemically pulverizing large silicon particles in a cPAN matrix.

[0009] While the development of the nSi-RTIL system and μSi-cPAN electrodes has resulted in world record performance of Li-ion full cells containing silicon anodes (high silicon loading mass, no pre-treated / pre-lithiated silicon anode, long cycle life, high energy), this performance has only been demonstrated on a laboratory scale. The anodes used to demonstrate those inventions, while containing more than 70% silicon relative to the total anode mass, were thin and not suitable for commercial applications. They were "bench-top" demonstrations done for proof-of-concept and demonstration of feasibility. The slurries used to fabricate those anodes contained 12.5 to 25 wt.% solids content (very low solids content, not suitable for commercial manufacturing). Laboratory standard current collector substrates (25 to over 30 microns thick), low electrode coating thickness (~2 mAh cm -2 The small electrode areas and low currents (suitable for coin cell demonstrations, in the microampere range) have made such demonstrations possible. Translating these technologies from the benchtop to commercial manufacturing lines presents an entirely new set of challenges.

[0010] Commercial anodes have a capacity of at least 2 mAhcm so that they can be paired with cathodes for improved energy density and cost in large format Li-ion batteries. -2 This means that previously developed anodes must be scaled up (by 2x in most metrics, including payload and thickness, to achieve attractive energy densities) and fabricated by commercially practical means. Commercial anodes must provide capacities per area (mAhcm) that adequately match the cathode capacities when stacked or wound into pouch or cylindrical cells, respectively. -2 ) must also be developed to remain consistent across the entire anode sheet. When the anode is scaled up to commercial levels, the adhesion between the coating and the current collector substrate, the physical properties of the coating, and even the anode electrochemistry change. -2It is well known that achieving realistic high performance silicon anodes with aerial loading capacities above 10 ... [Prior art documents] [Patent documents]

[0011] [Patent Document 1] International Publication No. 2016 / 123396 Summary of the Invention [Problem to be solved by the invention]

[0012] The present invention is directed to solving the problems of the background art. [Means for solving the problem]

[0013] This application describes various embodiments of processes and compositions used to facilitate a high quality commercial scale Si-cPAN anode for Li-ion batteries. In some embodiments, the anode comprises a thin film cast onto a current collector substrate, the thin film comprising active material particles (e.g., silicon particles) and a conductive polymer film coating on the active material particles. In some embodiments, the conductive polymer film coating comprises a thermoplastic processed to form a cyclized non-plastic ladder compound. Such an anode can be incorporated into an energy storage device in conjunction with a cathode and an electrolyte. Methods of manufacturing the anodes disclosed herein are also described. In some embodiments, the methods include preparing a slurry including active material, additive powder, polymer powder, and solvent. The slurry is then mixed for a period of time, and then the slurry is cast onto a current collector substrate. A drying and heating step is then performed. [Brief description of the drawings]

[0014] [Figure 1A] ~ [Figure 1B] FIG. 1 is a pair of graphs illustrating cycling data for a μSi-cPAN half-cell containing a fluorinated electrolyte additive, showing the rapid CE stabilization achieved by use of Applicant's previously disclosed μSi-cPAN / mRTIL system. [Figure 2A] ~ [Figure 2D] Provides high-resolution transmission electron microscopy images (HR-TEM) of nanospherical silicon particles coated with polyacrylonitrile. [Diagram 3] 1 is a graph illustrating a three-electrode experiment of a full cell pouch with micron silicon (anode) and NMC

[0622] (cathode) working electrodes and a lithium counter electrode with an N / P ratio of 0.9. [Figure 4] 1 is a pair of graphs illustrating pouch full cell cycling data comparing the impact of low N / P ratios to sufficient N / P ratios. [Figure 5A] ~ [Figure 5E] Figure 1 provides a graph showing half-cell cycle performance of silicon / PAN anodes highlighting the performance of 1 to 3 micrometer silicon particles (D50 size) on various coppers with different surface roughness, and (b)-(e) images of the surface topography of various copper materials with varying surface roughness. [Figure 6]Graph showing full cells (coins) containing silicon / carbon active material with PAN conductive binder (30-35% silicon normalized to total anode coating mass) and NMC

[0622] cathode comparing anode current collector roughness. [Figure 7] An overview of the different copper types, their associated roughness parameters, and a profilometer spectrum of a representative surface of the first copper type ("OM10um (coarse)" copper) are provided. [Figure 8] 1 illustrates a polyacrylonitrile heating process. [Figure 9] We provide SEM and EDS (with mapping) of silicon and PAN-containing polymer-driven nanocomposites after heat treatment under argon. [Figure 10A] ~ [Figure 10B] FIG. 1 is a pair of graphs illustrating the electrochemical performance of PAN / Si nanocomposite anodes, heat treated at 300° C. under argon (top) and air (bottom) environments, followed by heat treatment at 600° C. under argon. [Figure 11] 1 is a graph comparing cyclization in a vacuum oven and in a tube furnace under argon flow, showing high CE and high capacity when cyclized in either environment. [Figure 12A] ~ [Figure 12D] FIG. 1 is a series of graphs showing first cycle voltage profiles of full cells containing a nickel-rich NCM cathode and a Si-cPAN anode, in which the anode components were heat treated according to various procedures. [Figure 13] 1 is a graph illustrating an exemplary half-cell containing 30-35% silicon (normalized to total anode mass) anode produced by the methods described herein (6 mAh / cm2 loading). [Figure 14] 1 is a pair of graphs illustrating a full-cell single-stack pouch containing an exemplary anode described herein, mass-produced, suitable for commercial level performance (commercial payload, commercially realistic auxiliary components). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The following description details various embodiments of methods associated with producing commercial-scale Si-cPAN electrodes, electrochemical implications associated with some or all of those methods, and various embodiments of the resulting compositions. The description is divided into sections according to the steps used to fabricate the electrodes, and each step describes physical parameters that can be used to obtain improved battery performance.

[0016] Traditionally, Si-based electrodes are fabricated by mixing a polymer binder (e.g., polyvinylidene fluoride, polyacrylic acid, styrene-butadiene rubber, or carboxymethyl cellulose), a conductive additive (usually carbon black), and Si particles in an organic solvent such as N-methylpyrrolidone (NMP) to produce a viscous slurry. The slurry is then blade coated onto a copper foil current collector and dried to form the anode electrode. The embodiments described herein relate to the fabrication of a polymer-driven composite Si anode, which differs from conventional methods in significant ways.

[0017] Surprisingly, the method described herein is compatible with existing manufacturing infrastructure, enabling the first truly "drop-in" high-loading silicon anodes available to the Li-ion market. Other silicon anode production methods are cost and resource intensive, providing significant value to the methods discussed below. As described in more detail below, silicon active material is coated with a conductive polymer such as polyacrylonitrile (PAN), cast onto copper foil, and then thermally processed and paired with the cathode in a specific manner to enable full cell performance.

[0018] Although polyacrylonitrile is discussed in this application as an exemplary conductive polymer for application according to the disclosed method, other polymers may be used. Other suitable polymers include, but are not limited to, poly(acrylic acid) (PAA), carboxymethyl cellulose (CMC), and alginic acid. PAN is a resinous, fibrous organic polymer made from a mixture of monomers, the main component of which is acrylonitrile. PAN fibers, when appropriately modified, are chemical precursors to high-quality carbon fibers, which are found commercially in a number of high-tech and common everyday applications.

[0019] Numerous active material types may also be utilized with the methods described herein. Although silicon is discussed as an exemplary anode active material for application with this method, any silicon form may be incorporated into the anode slurry and electrode sheet. Silicon forms include, but are not limited to, nanospheres, nanowires, nanorods, whiskers, "coral-shaped" silicon, microspherical silicon, and various nanofeature-containing large particle silicon materials. Silicon-graphite, silicon-graphene, silicon-hard carbon, and other silicon-carbon composite materials are also non-exhaustive exemplary anode active materials for application with the methods described herein. Mixtures of silicon and carbonaceous materials such as graphite or hard carbon are also non-exhaustive exemplary anode active materials.

[0020] Bulk Slurry Mixing To fabricate Si-cPAN electrodes on a large scale, the methods described herein may generally begin by preparing a slurry. Generally, the slurry is prepared by mixing the active material, polymer, auxiliary materials, and additives in a solvent. Preferably, the resulting slurry has specific rheological properties to provide the highest electrochemical cycling performance of the Li-ion battery. In some embodiments, the composition added to the solvent includes about 10 to about 50 wt.% PAN and about 50 to about 90 wt.% active material. In some embodiments, the slurry includes about 30 to about 60 wt.% solids in about 70 to about 40 wt.% solvent.

[0021] The active materials used to prepare the slurry may include combinations of materials in different compositions. For example, carbonaceous active materials (graphite, graphene, hard carbon, etc.) may be mixed to form a 10:90 silicon:carbonaceous material weight ratio or a 90:10 silicon:carbonaceous material weight ratio. An exemplary commercial Si:cPAN anode may include a 30:55:15 Si:carbonaceous material:PAN weight ratio. Other exemplary weight ratios include 40 to 80 wt.% silicon, with 5 to 50 wt.% carbonaceous material and 10 to 20 wt.% PAN. The carbonaceous material may include a mixture of active materials and conductive additives, including but not limited to carbon black or carbon nanotubes.

[0022] The mixture of active material and conductive binder powders is dispersed in a solvent to form a slurry. In some embodiments, the solvent is selected so that it can dissolve the conductive binder. For example, N,N-dimethylformamide (DMF, 99%) is an exemplary solvent for application according to the methods described herein when utilizing PAN polymer. Other suitable solvents include, but are not limited to, dimethylsulfone (DMSO2), dimethylsulfoxide (DMSO), N-methyl-2-pyrrolidone (NMP), N,N-dimethylacetamide (DMAc), ethylene carbonate (EC), and propylene carbonate (PC).

[0023] Slurry viscosity determines mixing quality, coating quality, and the ability to generate large thin films on the current collector substrate. Exemplary slurry viscosities can be determined using Brookfield Viscosity (spindle 64) (all measurements taken at room temperature 23° C.). Slurry viscosity is determined by the solvent / polymer mass ratio and polymer chain length, as well as by the mass of the solvent relative to the total slurry mass. Exemplary slurries made using the materials and methods described herein exhibit significantly more Newtonian behavior than conventional Li-ion anode slurries. A Newtonian fluid is a fluid in which the viscous stress resulting from fluid flow is linearly proportional to the range of change in strain rate or deformation of the fluid. This means that as shear forces are applied to the slurries described herein, the slurries exhibit less shear thinning relative to conventional Li-ion anode slurries. This has implications for the anode mixing and coating process, because the slurries can be mixed at much higher RPM and successfully coated at very low thicknesses. The low shear thinning properties of the slurries can be studied using a Brookfield Viscometer, which is a common instrument for rheological characterization. In some embodiments, the slurries have Brookfield viscosities ranging between 3000 and 6000 centipoise (cP) between 12 and 100 RPM spindle rotation (steel spindle #64) at room temperature, varying by less than 1000 cP for a given slurry mixture. The relatively low variation in viscosity over various shear forces (described by spindle rotation by RPM) suggests the Newtonian nature of the slurry. Other exemplary slurries have viscosities ranging from 3500 to 5000 cP between 20 and 100 RPM at room temperature.

[0024] Slurry mixing parameters are contributors to the resulting anode performance. Slurry mixing time and slurry volume, along with mass percentage, powder mixing, and slurry viscosity, are important factors in determining the polymer coating quality on the active material. Slurry time is important to allow for a uniform polymer coating on the suspended active material particles. In some embodiments, slurry mixing times of up to 12 hours are sufficient. In some embodiments, lower mixing times, such as 2 hours of mixing, are sufficient depending on the appropriate equipment.

[0025] Slurry mixing can be accomplished by a variety of equipment: vacuum and non-vacuum planetary centrifugal mixers (e.g., "Thinky" or "Ross" mixers), slurry planetary dispersing vacuum mixers, planetary double disperser mixers, homogenizers, and simple stirring in a beaker with a stir bar or stir plate can produce sufficient mixing conditions.

[0026] The slurry volume is important because there must be enough material present to produce adequate mixing. The slurry volume also affects the electrochemical performance of the resulting anode. If the slurry volume is too low, a relatively large portion of the material will not receive agitation / mixing and a uniform coating will not be applied. For example, a mixture of 200 mg active material plus polymer powder and 1.6 g solvent (87.5% total slurry weight solvent) will not mix properly. In this case, regardless of the mixing method, there is not enough slurry to produce adequate mixing. A slurry utilizing 1.2 g active material plus polymer powder in 8.4 g solvent (87.5% total slurry weight solvent) mixes as well and produces a uniform polymer coating on the active material as a slurry utilizing 1.2 g active material plus polymer powder in 4-6 g solvent. However, this solids content (12.5 wt.% solids) is not suitable for coating by large scale manufacturing equipment. These slurries have too low a viscosity to be coatable by roll-to-roll methods (e.g., comma bar, slot die, etc.).

[0027] The quality of the PAN coating on the silicon material, resulting from the aforementioned parameters, becomes increasingly important as the anode loading mass increases. Whether or not a sufficient coating has been achieved can be confirmed by identifying the uniformity and thickness of the coating using microscopy such as transmission electron microscopy. A PAN coating that provides strong shape retention over electrochemical cycling should be at least 3 to 5 nanometers thick and be found on the entire surface of the active material particles and be present throughout the electrode. An example of an exemplary coating formed using the method described above is shown in FIG. 2. Electron energy loss spectroscopy (EELS) highlights the silicon and PAN coating (d). A uniform 3 to 5 nm coating is present on the particles throughout the electrode matrix.

[0028] When preparing the slurry, it may also be desirable to add electrode additives that can improve the performance of full-cell Li-ion batteries. Exemplary electrode additives include, but are not limited to, lithium metal powder (e.g., stabilized lithium metal powder SLMP) and lithium nitride (Li3N), as well as other high lithium content powders and salts. Dry powders such as these can be added directly to the slurry or mixed together with other slurry components. Oxalic acid can also be added to the slurry to improve dispersion and adhesion properties.

[0029] Generally speaking, a polymer is dissolved in a solvent, and the slurry is then mixed so that the polymer material thoroughly coats the active material powder that is dispersed in the polymer / solvent solution.

[0030] Electrode Coating After mixing the slurry, it is cast onto the current collector substrate, for example by roll-to-roll coating methods. Roll-to-roll coating machines can be used to produce electrodes of several hundred meters in one run. The roll-to-roll coating process is determined by the physical properties of the slurry (e.g., shear, viscosity, etc.). The current collector foil is pulled through a coater at a speed of 0.2 to 50 meters / min, and the coated foil passes through a dryer set at a temperature of 30 to 70° C. for water-based slurries and 110 to 160° C. for solvent-based slurries. In the case of the technology described here, the dryer temperature should be set at 30 to 70° C., despite the solvent-based system.

[0031] The important factors for the electrode coating are the area-based payload it provides per square centimeter of silicon, the capacity it provides, and how these numbers match the cathode used in the full cell. To pair with high energy cathode materials, including "nickel rich NMC" (nickel cobalt manganese oxide cathodes), the area-based capacity of the anode should be 1.3 to 2.0 times the area-based capacity of the cathode. This factor is known in the industry as the "N / P ratio" (negative electrode capacity / positive electrode capacity). In conventional Li-ion cells containing graphite anodes, the N / P ratio is typically 1.1 to 1.2 and is set to prevent lithium plating on the anode during cycling. The N / P ratios devised for the systems described herein are designed to cover the efficiency loss during initial cycles and to raise the anode half-cell voltage to Li / Li +The anode is designed to "pin" between 0.01 and 1.5 V relative to the total anode film mass. If the N / P ratio is too low, the anode half-cell voltage will drop below 0.01 V (due to full and over-lithiation of silicon) and the anode will be destroyed. This is illustrated in FIG. 3. FIG. 4 shows a cell with a poor N / P ratio compared to a cell with a strong N / P ratio. A higher relative N / P ratio also prevents wrinkling and deformation of the anode film due to expansion and contraction of the silicon material present in the film. The desired N / P ratio depends on the silicon loading mass relative to the total anode film mass. If the anode film contains 20 to 50 wt.% silicon, the N / P ratio should be 1.2 to 1.6. If the anode film contains more than 50 wt.% silicon, the N / P ratio should be greater than 1.6. In some embodiments, the weight percent of silicon in the anode can be added to "1" to obtain the minimum N / P ratio for the system. In other words, if the anode contains 40 wt.% silicon, the resulting N / P ratio of the full cell system should be greater than 1.4.

[0032] Current collector substrate A current collector substrate, typically a metal foil, is used to move electrons from outside the cell to the electrode and vice versa. The electrode slurry is cast onto the foil as a coating of uniform thickness. For Li-ion batteries to function properly, the electrode coating must be sufficiently adhered to the current collector foil and maintain this adhesion during cycling. This is particularly difficult when using large format electrodes (which tend to be very thick) given the expansion properties of the active materials when alloying electrodes such as silicon. The conductive binder is responsible for adhering the anode thin film to the current collector substrate. For large format electrodes, it is necessary to have enough binder present to allow adhesion. In the silicon plus PAN system described in this application, 10 to 25% PAN relative to the total anode coating mass is the minimum polymer content allowed. This is typical for large scaled large format silicon anodes with thicknesses greater than 5 micrometers.

[0033] Importantly and surprisingly, the physical properties of the current collector substrate are highly critical to the performance of the resulting anode sheet. In conjunction with the anode composition, the physical properties of the current collector substrate enable long cell life. Copper foil is an exemplary current collector substrate and is the most commonly used in conventional Li-ion cells. In this application, copper foil properties are discussed.

[0034] An important physical property of copper with respect to anodic thin film adhesion is its surface roughness. One measure of roughness is the 10-point height or maximum height (R z ) which is the root mean square value. R z is defined as the average number of peaks to valleys in a given scan area, with at least five consecutive points measured (5 highest peaks + 5 highest values ​​= 10 points). For some embodiments of the anodes described herein to remain adherent during cycling, the copper R z should be at least 1.5 micrometers. Other embodiments relying on larger active materials may require higher surface roughness, up to 6 to 7 micrometers. Other embodiments relying on nanoscale active materials may require R of greater than 0.5 micrometers. z Copper foils used in conventional / previously commercialized Li-ion anodes typically have an R value of 0.5 microns or less. z It has a value.

[0035] Another measure of surface roughness is the arithmetic mean height (Sa), which expresses the magnitude of the difference in height of each point compared to the arithmetic mean of the surface. Yet another measure of surface roughness is the interfacial developed area ratio (Sdr), which is the percentage of the surface area contributed by the texture compared to the plane defined area (i.e., a perfectly flat surface has Sdr=0). Each of these parameters, along with their relative magnitudes, are important to the performance of the systems described herein.

[0036] As previously mentioned, the required copper surface roughness for realistic performance is highly dependent on the active material size. Current data suggest that a surface roughness R of more than 0.5 micrometers is required when the electrode film expansion is below 50% in the z-axis (orthogonal to the electrode substrate) and the active material particle size is above 500 nanometers. z It has been suggested that copper with a surface roughness R of more than 2 micrometers provides the best performance when the electrode film expansion is more than 50% in the z-axis (perpendicular to the electrode substrate) and the active material particle size is more than 500 nanometers. z Copper having a .DELTA..times ...

[0037] Unfortunately, higher surface roughness leads to a consequential higher thickness, which is detrimental to the battery energy density because the thicker current collector (ancillary material that does not contribute to the cell capacity) takes up space and does not provide energy. The improved adhesion on the rougher copper surface is explained by the increased surface area available for adhesion between the conductive polymer and the copper. Referring to FIG. 5, various copper surfaces were imaged by optical microscopy for comparison.

[0038] The performance of half cells containing silicon plus PAN anodes is also shown in Figure 5, demonstrating the clear need for adequate copper surface roughness to maintain adhesion to the anode thin film during many charge-discharge cycles based on the active material morphology and anode thin film structure. In the half cells, the first cycle coulombic efficiency (CE) is higher and the CE stabilizes much more quickly in the cells containing the rougher copper foil. This is attributed to the maintained electronic contacts and faster electron transport within the cell. The CE behavior and the combined electron transport / adhesion properties are manifested in the higher performance full cells due to the active material particles sized above 500 nanometers as shown in Figure 6. R at or below 1 micron is also evident. z In a full cell containing an anode current collector film having

[0039] A summary of the various copper types, their associated roughness parameters, and a profilometer spectrum of a representative surface of the first copper type ("OM10um(coarse)" copper) is provided in FIG. 7. The copper types denoted by shaded font ("OM10um(coarse)" and "VL10|23um" copper) provide the best performance with the various silicon material types and anode thin film microstructures. In general, the materials shown in FIG. 7 work best for the large scale electrode system described in this application. Therefore, a new parameter Sa / Sdr is used to describe the best performing copper foils based on the roughness parameters. Sa / Sdr describes the ratio of the average height of the peaks and valleys of the foil surface to the magnitude of the percentage of the surface caused by roughness. In other words, a high Sa / Sdr means that the copper surface has very high peaks and low frequency relative to the total roughness. Here, an Sa / Sdr closer to 1 suggests that the copper surface peak / valley heights are more evenly distributed. An Sa / Sdr closer to 1 is found to be advantageous, and an Sa / Sdr below 3 is found to be sufficient for high performance for a variety of silicon material types and anode thin film compositions and microstructures.

[0040] Electrode calendaring In some embodiments, the electrodes are dried after coating by roll-to-roll coating equipment, and the dryer temperature can be set at 30 to 70° C. under air flow. After slurry casting onto the current collector foil and solvent drying / evaporation, conventional graphite anodes are calendered to about 70% of their original thin film thickness. This calendering results in a porosity of about 40 to 50%. Such a process provides a higher degree of particle contact while still allowing sufficient electrolyte penetration. Above 50% porosity, conventional anodes lack sufficient mechanical strength to withstand battery production and operation. The system described in this application is different. The electrodes require a higher porosity to accommodate the volume expansion of the silicon material, and a higher inter-film surface area allows for the formation of a robust SEI layer and faster Li+ / - adsorption. +This is advantageous for ion transport. The anodes described herein, including silicon plus PAN anodes, are calendered to 40 to 70% porosity. An exemplary porosity for a Si-cPAN composite would be 50 to 60%. This is comparable to conventional graphite anodes, which have abot 30 to 40% porosity. Conventional electrodes (PAA, CMC, SBR, etc. binders) containing silicon today ranging up to 15 wt.% Si have porosities ranging from 40 to 50%. Active materials that exhibit higher expansion require electrodes with higher porosity.

[0041] Electrode heat treatment An important aspect of the anodes described herein is the ability of the conductive polymer binder to act both as a binder material and as an electronically conductive matrix that can provide efficient charge transport within the composite. Producing this type of high performance anode thin film on a large scale is indeed difficult and requires understanding of many complexities as described above, but another layer of complexity is added by the need to process many conductive polymers to achieve electronic conductivity. Exemplary conductive polymers discussed herein (e.g., PAN) can be heated in a reducing atmosphere or under vacuum to exhibit electronic conductivity. At the same time, the polymer can be processed so that the polymer matrix does not become too brittle for the mechanical effects of battery cycling (caused by heat treatment at very high temperatures or in an insufficient atmosphere). Moreover, the processing should be carried out so that the auxiliary components of the electrode (i.e., copper) are not affected and remain in the correct state for battery operation.

[0042] Many conductive polymers can be chemically altered to provide electronic conductivity; however, most require the addition of a crosslinking agent to catalyze their chemical reaction. PAN and copolymers of PAN are unique in that they are self-catalyzing upon a heat treatment process. PAN has the molecular formula (C3H3N) nPAN is a unique linear, semi-crystalline organic polymer with a molecular structure consisting of carbon chains with coordinated nitrile groups. The chemistry of PAN is particularly interesting due to its unique autocatalytic cyclization and crosslinking due to thermal stabilization. PAN chains decompose before they reach a molten state, and the decomposition process, commonly referred to as "cyclization," converts the linear PAN chains into thermally stable conjugated ladder-like structures that do not flow or melt. This is illustrated in Figure 8. This thermal stabilization allows the fibers to withstand carbonization and graphitization temperatures (approximately 1000 to 3000°C) without excessive weight loss or chain scission, yielding high-performance carbon fibers.

[0043] Heat stabilization of PAN refers to the low temperature (typically 200 to 300°C) conversion of the polymer fibers into high temperature durable fibers. The conversion is necessary for the fibers to survive carbonization (800 to 1300°C) and graphitization (1300 to 3000°C) and have the highest possible carbon yield and superior properties. The main chemical reactions involved in this process are known as cyclization, dehydrogenation, oxidation, and crosslinking, which result in the formation of heat stable conjugated ladder structures.

[0044] Cyclization is a key reaction during the stabilization of PAN and is the main focus of the anodic treatment described in this application. Cyclization occurs when nitrile bonds (C≡N) react to develop crosslinks between PAN molecules, resulting in stable conjugated ladder polymers of double bonds (C═N) and fused pyridine rings. The thermal stability of stabilized fibers is attributed to the formation of ladder structures due to the cyclization of nitrile groups, allowing the operation of stabilized PAN at high temperatures with minimal volatilization of carbonaceous materials. Cyclization is the reason why stabilized fibers change color from white to yellow, brown, and black. Cyclization is exothermic and has the potential to damage the fibers if done too quickly. The fibers will shrink excessively, lose significant mass, and may even melt and condense together. Conversely, if the stabilization procedure is too conservative (both in terms of time and heat), the fibers will only be partially stabilized. Unlike dehydrogenation, cyclization does not require the presence of oxygen to occur, so it can occur in an inert atmosphere. The reaction atmosphere is important in the process described herein because the anode copper foil current collector is involved in the heat treatment of PAN, and any exposure to oxygen at temperatures above 100° C. will oxidize the foil and cause defect problems (electronic resistance and electrochemical side reactions).

[0045] In the embodiments described herein, PAN is processed only up to its stabilization (specifically "cyclization") stage, and then the resulting pyridine-based conjugated polymer is applied as an electrode binder / coating with robust mechanical and unique electronic properties. The reason for deviating from the conventional stabilization procedure (oxidation, dehydrogenation, and cyclization to carbonization and graphitization) for high carbon yield and high performance carbons is to prevent the formation of a highly oriented (basal plane to basal plane alignment), rigid, brittle coating around the active material that is prone to high expansion and contraction.

[0046] Stabilization of PAN from linear molecules to ladder polymer compounds by cyclization can be performed by heating in an inert environment from 100 to 500°C, with an exemplary temperature for PAN cyclization heat treatment being 300°C, with a rate of 5°C / min and a hold time at peak temperature of 2 to 12 hr. Running at various temperatures allows the best peak electrochemical performance of the PAN / silicon configuration to be determined. Figure 9 shows scanning electron microscopy (SEM) images and energy dispersive spectroscopy (EDS) analysis of some of the nanocomposite samples driven by those polymers. The PAN / silicon samples were tested using the method described above. Others were then processed for carbonization of the PAN and held at peak temperatures of 500°C, 600°C, 700°C, 800°C, 900°C, and 1000°C for 1 hr under the same argon atmosphere. For this second heating step, the heating rate was again kept at 5°C / min. Figures 10 and 11 illustrate the electrochemical data for the various heat treatment tests.

[0047] In addition to the processing parameters of heating time and temperature, the equipment utilized and the atmospheric conditions provided are important. As previously discussed, the anodes may be processed under vacuum or inert gas flow. Argon and nitrogen are exemplary inert gas atmospheres, with pressures of 20 to 80 PSI providing the most consistent heating conditions. Heat treatment under vacuum also allows for adequate cyclization conditions and high performance anodes. These atmospheres can be provided by a variety of equipment types, including tube furnaces, glove boxes, vacuum ovens, or other atmosphere-controlled ovens. Gas flow during heat treatment allows for improved heating and electrochemical performance because by-products of the polymer chemical reaction (including hydrogen outgassing during PAN cyclization) are flushed from the system and therefore cannot react with the electrode or current collector substrate. For best performance, the gas flow in the tube furnace should be set at a rate of 100 to 1,000 liters per hour. An entire roll of anodes or multiple rolls of anodes can be processed through a single oven. A controlled atmosphere furnace can also be added to the industry standard roll-to-roll coating systems utilized for electrode fabrication. Typically, the electrodes are conveyed through a drying oven immediately after coating. Following initial drying with conditions set to induce chemical changes in the polymer (i.e., PAN cyclization) before being wound onto a spool, the electrodes can also be passed through a controlled atmosphere furnace. In lieu of this equipment, a tube furnace provides a commercially viable means of processing large rolls of anodes containing silicon / polyacrylonitrile composites.

[0048] Of particular importance, especially as this relates to commercial-scale manufacturing, is the knowledge that the heating time and heating ramp rate should be tuned according to the anode microstructure and size. Specifically, anode thickness, PAN weight percentage, and the amount of anode material undergoing processing influence such processing parameters. As illustrated in Figure 12, a heating time of only 2 hours may be sufficient for adequate electrochemical performance.

[0049] Electrochemical performance Figure 13 presents exemplary data for a micron silicon:polyacrylonitrile (Si:PAN) anode half cell made by the methods described herein. The payload, processing, and resulting composition are sufficient for commercial use. Figure 14 presents exemplary data for a full cell including an exemplary anode described herein and a "nickel-rich" high energy cathode ("NMC

[0622] ").

[0050] From the foregoing it will be appreciated that specific embodiments of the invention have been described herein for purposes of illustration and that various modifications may be made without departing from the scope of the invention. Accordingly, the invention is not to be limited except as by the appended claims.

Claims

1. A cathode; An electrolyte; Surface roughness R of more than 1.5 microns z an anode comprising a thin film having a thickness of 10 to 80 micrometers cast on a current collector substrate having a Including, The thin film, A) a plurality of active material particles (the active material particles include at least one of silicon, hard carbon, graphite, graphene, germanium, titanium oxide, tin, magnesium, antimony, and lead); B) a conductive polymer film coating on the active material particles, the conductive polymer film coating comprising a thermoplastic polymer that has been treated to form a cyclized non-plastic ladder compound; Including, Energy storage devices.

2. 10. The energy storage device of claim 1, wherein the anode comprises 30-60 wt. % silicon particles and the gravimetric capacity per area of ​​the anode is 1.3 to 1.6 times that of the gravimetric capacity per area of ​​the cathode.

3. 10. The energy storage device of claim 1, wherein the anode comprises greater than or equal to 60 wt. % silicon particles and the gravimetric capacity per area of ​​the anode is 1.6 to 2.0 times that of the gravimetric capacity per area of ​​the cathode.

4. 10. The energy storage device of claim 1, wherein the thermoplastic polymer processed to become a cyclized non-plastic ladder compound comprises polyacrylonitrile.

5. 10. The energy storage device of claim 1, wherein the electrolyte comprises an imide-based room temperature ionic liquid.

6. 10. The energy storage device of claim 1, wherein the porosity of the anode thin film is between 50 and 70%.

7. 2. The energy storage device of claim 1, wherein the magnitude of the arithmetic mean height Sa is less than three times the expansion ratio Sdr of the interface.

8. the thin film includes a plurality of active materials and a thermoplastic polymer that is processed to form a cyclized non-plastic ladder compound; The method is A) preparing a slurry having a Brookfield viscosity of 2000-6000 cP at room temperature with a #64 spindle at 20-100 RPM by placing a mixture of active material, additive powder, and polymer powder in a solvent capable of dissolving the polymer powder; B) mixing the slurry for a period of 1 to 4 hours; C) casting the slurry onto a current collector substrate; D) drying the cast film; and E) applying heat to the cast film at a temperature of 200 to 400° C. for a time period of 1 to 12 hours; Including, A method of making an anode comprising casting a thin film thickness of 10 to 80 micrometers on a current collector substrate.

9. The method of claim 8 , wherein the active material comprises at least one of silicon, hard carbon, graphite, germanium, titanium oxide, tin, magnesium, antimony, and lead.

10. 9. The method of claim 8, wherein the thermoplastic polymer that is treated to become a cyclized non-plastic ladder compound comprises polyacrylonitrile.

11. The method of claim 8 , wherein the additive powder comprises lithium metal powder.

12. The method of claim 8 , wherein the additive powder comprises lithium nitride.

13. The method of claim 8 , wherein the additive powder comprises oxalic acid.

14. 9. The method of claim 8, wherein the application of heat at 200 to 400° C. is completed under vacuum or inert gas flow.

15. 10. An energy storage device comprising an anode, a cathode, and an electrolyte produced according to the method of claim 8, wherein the gravimetric capacity per area of ​​the anode is 1.3 to 2.0 times that of the gravimetric capacity per area of ​​the cathode.

Citation Information

Patent Citations

  • Nano combination electrode material Li3N / Si used for lithium ion battery and its preparation method

    CN101222041A

  • Cathode for lithium secondary battery and lithium secondary battery

    JP2005285581A

  • Non-aqueous electrolyte secondary battery

    JP2009252705A

  • Nanocomposite electrodes and related devices

    JP2009538495A

  • Negative electrode for nonaqueous secondary battery, and process for production thereof

    JP2011086427A