Steel plate and method for manufacturing the same
A steel plate with a controlled microstructure and specific chemical composition enhances work hardenability, addressing strain concentration and hole formation during collisions by optimizing ferrite and pearlite content and reducing precipitation-strengthening particles.
Patent Information
- Application Number
- JP2023064195
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-11
- Publication Date
- 2024-10-24
AI Technical Summary
Existing steel plates used in structures like ships and offshore structures face challenges in suppressing strain concentration and hole formation during collisions, despite increasing thickness and ductility, which traditional methods of enhancing strength can exacerbate rather than mitigate damage.
A steel plate with a controlled microstructure composed mainly of ferrite and pearlite, limited martensite, and fine grain size, along with specific chemical compositions and manufacturing processes to enhance work hardenability, particularly in large strain regions, by limiting precipitation-strengthening particles and cementite density.
The solution effectively suppresses strain concentration and hole formation during collisions, improving the steel plate's ability to absorb impact and maintain structural integrity.
Smart Images

Figure 2024151070000001 
Figure 2024151070000002 
Figure 2024151070000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a steel plate and a manufacturing method thereof, and more particularly to a steel plate having improved work hardening ability, which is useful for suppressing strain concentration during deformation due to impact and suppressing the occurrence of fractures, and a manufacturing method thereof. [Background technology]
[0002] Ships, floating bodies, and marine structures are at risk of collision with ships that deviate from their course on the ocean, so their designs must ensure that they do not lose their stability even if they are hit by an anticipated collision. To ensure stability, fenders and other materials are used to mitigate the impact, and structures are divided into multiple blocks to minimize the impact of holes caused by a collision. Designs to prepare for such collisions are considered in addition to the design required for the original purpose, and they increase the construction costs of ships, floating bodies, and marine structures.
[0003] As with ships, floating bodies, and marine structures, automobiles are also required to control damage to the body during a collision and keep it within an acceptable range for anticipated collisions in order to protect the safety of passengers. As described in Non-Patent Document 1, one solution to this problem in automobiles is to improve the strength of the steel materials used. By applying high-strength steel materials that do not easily break to the body, it is possible to significantly improve safety during a collision even for a body that follows the same design as before.
[0004] Similarly, in ships, the degree of damage during collision can be reduced by improving the properties of materials. For example, Patent Document 1 proposes a high-strength, high-ductility steel plate that controls the microstructure, reduces the dislocation density in soft ferrite grains, and homogenizes the hardness distribution in the plate thickness direction as a means of suppressing the occurrence of holes in the side of the ship during a ship collision. Specifically, the high-strength, high-ductility steel plate described in Patent Document 1 has a lower limit of total elongation (T.EL) of 23% or more, which is 1.5 times that of general steel, a yield strength (YP) of 355 to 500 MPa, and a tensile strength (TS) of 490 to 620 MPa.
[0005] Furthermore, Patent Document 2 proposes a low-yield-ratio, high-strength steel plate with excellent ductile fracture resistance, in which island martensite structures are dispersed in bainite structures, suppressing the occurrence of ductile cracks under biaxial stress conditions, with a bainite area fraction of 30 to 90% and an island martensite area fraction of 2 to 10%.
[0006] Furthermore, Patent Document 3 proposes a thick steel plate for ship hulls that has a yield strength of 235 MPa or more, a tensile strength of 460 MPa or less, a uniform elongation of 15% or more, and a Charpy impact absorption energy of 100 J or more at 0° C. However, this steel plate is used for the purpose of reducing damage to the side receiving the collision by improving the properties of the steel plate on the side receiving the collision in the case of a collision of the ship hull, and is not necessarily intended as a means of controlling damage on the side receiving the collision.
[0007] On the other hand, from the viewpoint of promoting the strengthening of steel plates without the objective of reducing damage during collisions, Patent Document 4 discloses a manufacturing method for high-tensile steel plate with excellent large heat input weldability and ductility, in which the chemical composition, rolling conditions, and cooling conditions after rolling are controlled to finely disperse Ca-based inclusions in the steel, thereby achieving a yield strength of 460 MPa or more and a plate thickness of 50 mm or less, with the aim of reducing the weight of ships by using high-strength steel.
[0008] Patent Document 5 proposes a steel plate having a metal structure consisting of a first phase of ferrite and a second phase of pearlite, in which the hardness of the second phase is 260 HV or less, and which has a carbon content of 0.04 to 0.06 mass %, as a thick steel plate having excellent uniform elongation. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2016-125077 A [Patent Document 2] JP 2013-139602 A [Patent Document 3] International Publication No. 2011 / 062000 [Patent Document 4] JP 2015-193920 A [Patent Document 5] JP 2018-193605 A [Non-patent literature]
[0010] [Non-Patent Document 1] Manabu Takahashi: "100 Years of Sheet Technology - Sheet Steel and Manufacturing Technology that Developed Alongside the Automobile Industry", Tetsu-to-Hagane, Vol. 100, 2014, No. 1, p82-93 Summary of the Invention [Problem to be solved by the invention]
[0011] In order to promote high efficiency as a countermeasure against population decline and rising energy costs, ships, floating bodies, and marine structures are becoming larger, and the steel plates that make up these structures are also becoming thicker. Since the ductility of steel plates increases with increasing plate thickness, in structures that use thick steel materials, the effect of reducing damage during collisions due to improved ductility is saturated, and in order to further reduce damage during collisions, it is necessary to consider methods other than improving ductility. In addition, there is a concern that the high strength of steel plates proposed in Patent Documents 2 and 4, for example, excessively increases the yield strength, which hinders the absorption of impacts during collisions by plastic deformation, localizing deformation and increasing damage. In relation to this, in order to suppress damage due to collisions of structures, in addition to suppressing the occurrence of cracks in steel plates, the work hardening ability of the steel plates in the large strain region can be increased to suppress the concentration of deformation in specific areas after local deformation begins, widely dispersing the strain, and delaying the arrival of the critical strain for crack occurrence, thereby suppressing the occurrence of cracks.
[0012] Therefore, an object of the present invention is to provide a steel sheet having improved work hardening ability, particularly improved work hardening ability in the large strain region, and a manufacturing method thereof. [Means for solving the problem]
[0013] The present inventors have investigated the microstructural control of the steel sheet necessary for improving the work hardening ability in the large strain region of the steel sheet. As a result, they have found that the work hardening ability in the large strain region corresponding to the time after local deformation starts to progress can be improved by making the microstructure of the steel sheet a composite structure mainly composed of ferrite, containing pearlite as a hard structure, and limiting the total volume fraction of other structures, such as martensite, further making the average crystal grain size of the ferrite appropriately fine, limiting the density of the precipitation strengthening particles and coarse cementite contained in the ferrite grains, and further limiting the density of the precipitation strengthening particles contained in the ferrite that constitutes the pearlite, the pearlite being present in a fine island shape, the pearlite having a lamellar structure, and limiting the density of the precipitation strengthening particles contained in the ferrite that constitutes the pearlite.
[0014] Although the mechanism by which the above-mentioned microstructural features of steel sheet affect work hardening ability is unclear, it is presumed that by reducing the density of precipitation strengthening particles, the excessive development of dislocation substructures accompanying processing is suppressed, the number of disturbed lamellar structures in cementite in ferrite and pearlite, which are presumed to be sites of void generation when large strain is applied, is reduced, and the existence of regions of different strengths by forming a composite structure mainly composed of ferrite and including pearlite as a hard structure makes it difficult for the work hardening ability to deteriorate even if strain accumulates. Since voids can cause a deterioration of work hardening ability, suppressing the generation of voids in large strain regions is very effective in improving work hardening ability.
[0015] The present invention which has achieved the above object is as follows. (1) Chemical composition, in mass%, C: 0.075-0.240%, Si: 1.25% or less, Mn: 0.50-2.00%, P: 0.030% or less, S: 0.0100% or less, N: 0.0150% or less, O: 0.0030% or less, Al: 1.000% or less, Ti: 0.004 to 0.030%, Nb: 0 to 0.015%, V: 0~0.100%, Cu: 0-0.10%, Ni: 0-3.00%, Cr: 0-1.50%, Mo: 0-1.00%, W: 0 to 1.00%, B: 0~0.0050%, Sn: 0~1.000%, Sb: 0 to 0.200%, The sum of one or more of Ca, Mg, Zr, La, Ce, Te, Hf and REM: 0 to 0.0050%, and The balance is composed of Fe and impurities. Satisfying the following formulas (1) and (2), The microstructure in the range from the surface to the position of 1 / 8 of the plate thickness in the plate thickness direction to the position of 3 / 8 of the plate thickness in the plate thickness direction from the surface is, in terms of volume fraction, Ferrite: 80~95%, Perlite: 5-20%, and The sum of martensite, bainite, bainitic ferrite and retained austenite: 0 to 5%. The average grain size of the ferrite is 2 to 16 μm, The density of the precipitation strengthening particles contained in the ferrite grains is 1.0×10 22 pieces / m 3 is as follows: The density of the cementite particles contained in the ferrite grains is 1.0×10 10 pieces / m 2 is as follows: The average equivalent circle diameter of the pearlite island regions is 8.0 μm or less, The ratio of the average long diameter of the cementite forming the lamellar structure of the pearlite to the circle equivalent diameter of the island regions of the pearlite in which the cementite is present is 0.20 or more on average, The density of the precipitation strengthening particles contained in the ferrite that forms the lamellar structure of the pearlite is 1.0×10 22 pieces / m 3 A steel plate, characterized in that: 2.44×10 -2 ×(1.00-0.20[Si]+7.00[Nb])×(1.00-10[B] 0.5 )×(117+17[Si]+11[Si] 2 -33[Mn]+4[Mn] 2 +79[Al]+59[Al] 2 -26[Ni]-12[Cr])×(1+1.3[Si]+12[Mo]+35[Nb]) -1 ≧1.00...Equation (1) -0.003≦[Ti]-3.42[N]≦0.015...Equation (2) Here, [Si], [Nb], [B], [Mn], [Al], [Ni], [Cr], [Mo], [Ti] and [N] are the contents [mass%] of each element, and are 0 when the element is not contained. (2) The chemical composition is, in mass%, Nb: 0.004 to 0.012%, V: 0.020~0.080%, Cu: 0.02-0.08%, Ni: 0.15-2.30%, Cr: 0.10~1.00%, Mo: 0.03-0.50%, W: 0.03 to 0.50%, B: 0.0005~0.0025%, Sn: 0.015~0.300%, Sb: 0.005 to 0.080%, and Sum of one or more of Ca, Mg, Zr, La, Ce, Te, Hf and REM: 0.0008~0.0030% The steel sheet according to the above (1), characterized in that it contains one or more selected from the following: (3) The steel sheet according to (1) or (2) above, characterized in that the average aspect ratio of crystal grains in the ferrite is 2.00 or less. (4) A casting step of casting a slab having the chemical composition described in (1) or (2) above, and then cooling it to 500°C or less; a heating step of heating the slab, the maximum heating temperature of the slab being 1000 to 1150°C, and the total residence time at a temperature of 1000°C or higher satisfying the following formula (3); a rough rolling step of subjecting the slab to rough rolling so that a cumulative rolling reduction rate in a temperature range of 1000° C. or higher is 25% or more, and then subjecting the slab to a retention time of 30 seconds or more; A finish rolling process in which the obtained rolled material is subjected to finish rolling so that the cumulative rolling reduction in a temperature range of 950°C or less is 30% or more, and the completion temperature of the finish rolling is 850 to 920°C; A cooling process for water-cooling the obtained steel sheet, in which the time elapsed from the completion of the finish rolling process until the temperature of the steel sheet reaches 630°C is 60 seconds or more, the water-cooling start temperature is 600 to 630°C, the water-cooling end temperature is 400 to 450°C, and the temperature of the steel sheet is controlled so as not to exceed 450°C by recuperation after water-cooling. A method for producing a steel sheet, comprising:
number
[0016] According to the present invention, it is possible to provide a steel plate and a manufacturing method thereof that are useful for increasing the work hardening capacity, particularly in a large strain region, suppressing strain concentration during local deformation, and therefore suppressing the occurrence of holes during collision. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, the steel sheet according to the embodiment of the present invention and the manufacturing method thereof will be described in more detail. However, these descriptions are intended to exemplify preferred forms of the present invention and are not intended to limit the present invention to specific embodiments.
[0018] [Chemical composition] Hereinafter, the chemical composition of the steel sheet according to the embodiment of the present invention will be described. In the following description, the unit of content of each element, "%", means "mass%" unless otherwise specified.
[0019] [C:0.075~0.240%] C is an element that forms pearlite, and if its content is less than 0.075%, a sufficient fraction of pearlite is not obtained, resulting in insufficient strength. On the other hand, if the C content exceeds 0.240%, the fraction of pearlite becomes excessive, and sufficient work hardening ability cannot be obtained in the high strain region. From this viewpoint, the C content is set to 0.075% or more and 0.240% or less. In order to sufficiently promote the growth of cementite inside pearlite and increase the work hardening ability in the high strain region, it is preferable that C is contained at 0.090% or more, and more preferably at 0.110% or more or 0.130% or more. On the other hand, C is an element that impairs weldability and the toughness of the welded part, and from this viewpoint, the C content is preferably 0.220% or less, and more preferably at 0.200% or less or 0.180% or less.
[0020] [Si:1.25% or less] Si is a deoxidizing element and also contributes to improving strength. The Si content may be 0%, but in order to obtain a sufficient deoxidizing effect by Si, the Si content is preferably 0.01% or more. In order to increase strength, the Si content is preferably 0.05% or more, and more preferably 0.10% or more or 0.30% or more. On the other hand, if the Si content is high, the eutectoid temperature at which pearlite formation begins increases, and the diameter of the pearlite islands increases excessively. From this viewpoint, the Si content is set to 1.25% or less. Also, Si is an element that impairs the toughness of the steel plate, and from this viewpoint, the Si content is preferably 1.00% or less or 0.80% or less, and more preferably 0.50% or less.
[0021] [Mn: 0.50~2.00%] Mn is an element that contributes to improving strength, and in order to fully obtain this effect, 0.50% or more is added. From the viewpoint of increasing strength, the Mn content is preferably 0.70% or more, and more preferably 1.00% or more or 1.20% or more. On the other hand, if Mn is contained excessively, Mn segregation stripes are generated and pearlite is formed along the segregation stripes, so the size of the island pearlite increases and the work hardening ability in the large strain region is impaired, so the amount of Mn added is limited to 2.00% or less. In addition, Mn is an element that impairs weldability and the toughness of the welded part, and from this viewpoint, the Mn content is preferably 1.85% or less, and more preferably 1.70% or less or 1.50% or less.
[0022] [P:0.030% or less] P is an element that is inevitably contained in general steelmaking methods, and limiting it to less than 0.001% places a large burden on the smelting process and is economically undesirable, so the P content is preferably 0.001% or more. On the other hand, P is an element that impairs toughness, and from this viewpoint, the P content is limited to 0.030% or less. Furthermore, P is an element that impairs weldability and the toughness of welded parts, and from this viewpoint, the P content is preferably 0.020% or less, and more preferably 0.010% or less.
[0023] [S:0.0100% or less] S is an element that is inevitably contained in general steelmaking methods, and limiting the S content to less than 0.0003% places a large burden on the smelting process and is economically undesirable, so the S content is preferably 0.0003% or more. On the other hand, S is an element that forms coarse sulfides and impairs toughness, and from this perspective, the S content is limited to 0.0100% or less. Furthermore, S is an element that impairs weldability and the toughness of welds, and from this perspective, the S content is preferably 0.0060% or less, and more preferably 0.0045% or less.
[0024] [N:0.0150% or less] N is an element that is inevitably contained in a general steelmaking process. If a large amount of N is contained, coarse nitrides are formed, which impairs the toughness of the steel plate, so the N content is limited to 0.0150% or less. N is also an element that impairs the toughness of a welded portion, and from this viewpoint, the N content is preferably 0.0100% or less, and more preferably 0.0060% or less. There is no particular lower limit for the N content, but excessive reduction places a large load on the smelting process and is economically undesirable, so the N content is preferably 0.0003% or more, and more preferably 0.0015% or more.
[0025] [O:0.0030% or less] O is an element that is inevitably contained in a general steelmaking process. If a large amount of O is contained, coarse oxides are formed, which impairs the toughness of the steel sheet, so the O content is limited to 0.0030% or less. O is also an element that impairs the toughness of a welded portion, and from this viewpoint, the O content is preferably 0.0020% or less, and more preferably 0.0010% or less. There is no particular lower limit for the O content, but since limiting it to less than 0.0002% places a large load on the smelting process and is economically undesirable, it is preferable to set it to 0.0002% or more.
[0026] [Al: 1.000% or less] Al is a deoxidizing element. The Al content may be 0%, but in order to obtain this effect, it is preferable to add 0.005% or more, and more preferably 0.010% or more. On the other hand, Al is an element that impairs toughness, and the Al content is limited to 1.000% or less. In addition, since Al impairs weldability and the toughness of the welded portion, the Al content is preferably 0.800% or less, and more preferably 0.500% or less or 0.200% or less.
[0027] [Ti: 0.004~0.030%] Ti is an element that enhances the work hardening ability of a steel sheet in a high strain region by adding an appropriate amount of Ti, and since a sufficient work hardening ability improvement effect cannot be obtained when the Ti content is less than 0.004%, the Ti content in the steel sheet according to the embodiment of the present invention is set to 0.004% or more. On the other hand, when Ti is contained in an amount exceeding 0.030%, the work hardening ability of the steel sheet in a high strain region is deteriorated, so the Ti content is limited to 0.030% or less. Although the details of the manifestation of the effect of Ti are unclear, it is considered that the addition of an appropriate amount of Ti forms relatively coarse Ti carbonitrides in the ferrite that do not contribute to precipitation strengthening, and further, the solute carbon in the ferrite is absorbed by these Ti carbonitrides, thereby increasing the purity in the ferrite crystal grains and improving the work hardening ability in a high strain region. That is, by combining a Ti content of 0.004 to 0.030% with appropriate manufacturing conditions, which will be described in detail later, the solid solution carbon in ferrite, which adversely affects the work hardening ability, is absorbed by the formation of Ti carbonitrides, while the Ti carbonitrides are grown to a size that does not contribute to precipitation strengthening, and as a result, it becomes possible to limit the density of precipitation strengthening particles within a predetermined range. On the other hand, if Ti is added excessively, precipitation strengthening by Ti occurs, and it is considered that the characteristics are impaired. From the above viewpoints, the Ti content is preferably 0.007% or more, 0.010% or more, or 0.012% or more, and similarly, it is preferably 0.023% or less, 0.020% or less, or 0.017% or less. In this specification, Ti carbonitrides, i.e., Ti(CN), are particles consisting of one or more of TiC, TiN, TiC with part of C replaced by N, and / or TiN with part of N replaced by C.
[0028] The basic chemical composition of the steel sheet according to the embodiment of the present invention is as described above. Furthermore, the steel sheet may contain one or more of the following optional elements as necessary. The steel sheet may contain one or more selected from the group consisting of Nb: 0-0.015%, V: 0-0.100%, and Cu: 0-0.10%. The steel sheet may also contain one or more selected from the group consisting of Ni: 0-3.00%, Cr: 0-1.50%, Mo: 0-1.00%, and W: 0-1.00% or less. The steel sheet may also contain B: 0-0.0050%. The steel sheet may also contain one or two selected from the group consisting of Sn: 0-1.000% and Sb: 0-0.200%. The steel sheet may also contain 0 to 0.0050% in total of one or more of Ca, Mg, Zr, La, Ce, Te, Hf and REM. These optional elements will be described in detail below.
[0029] [Nb: 0~0.015%] Nb is an element that contributes to improving strength, and may be contained in an amount of 0.015% or less. If the Nb content exceeds 0.015%, precipitation strengthening is excessively expressed, and there is a concern that the work hardening ability in the high strain region may be impaired. In order to improve the work hardening ability in the high strain region, the Nb content is more preferably 0.012% or less or 0.010% or less. On the other hand, the Nb content may be 0%, but from the viewpoint of increasing strength, the Nb content is preferably 0.004% or more, and more preferably 0.007% or more.
[0030] [V:0~0.100%] V is an element that contributes to improving strength, and may be contained in an amount of 0.100% or less. If the V content exceeds 0.100%, precipitation strengthening is excessively expressed, particularly in pearlite, and there is a concern that the work hardening ability in the high strain region may be impaired. In order to improve the work hardening ability in the high strain region, the V content is more preferably 0.080% or less or 0.060% or less. On the other hand, the V content may be 0%, but from the viewpoint of increasing strength, the V content is preferably 0.020% or more, and more preferably 0.040% or more.
[0031] [Cu: 0~0.10%] Cu is an element that contributes to improving strength, and may be contained in an amount of 0.10% or less. If the Cu content exceeds 0.10%, precipitation strengthening is excessively expressed, particularly in ferrite, and there is a concern that the work hardening ability in the high strain region may be impaired. In order to improve the work hardening ability in the high strain region, the Cu content is more preferably 0.08% or less or 0.06% or less. On the other hand, the Cu content may be 0%, but from the viewpoint of increasing strength, the Cu content is preferably 0.02% or more, and more preferably 0.04% or more.
[0032] [Ni:0~3.00%] Ni is an element that improves the work hardening ability in a high strain region. The Ni content may be 0%, but in order to improve the work hardening ability, it is preferable to make it 0.15% or more. On the other hand, if the Ni content exceeds 3.00%, the hardenability increases excessively, and the work hardening ability in a high strain region is rather impaired. From this viewpoint, the Ni content is limited to 3.00% or less, preferably 2.30% or less, and more preferably 1.50% or less or 1.00% or less.
[0033] [Cr:0~1.50%] Cr is an element that contributes to improving strength, and may be contained in an amount of 1.50% or less. The Cr content may be 0%, but from the viewpoint of increasing strength, the Cr content is preferably 0.10% or more. On the other hand, if Cr is contained excessively, the connectivity of the lamellar structure of pearlite is impaired, and the work hardening ability in the high strain range is impaired. From this viewpoint, the Cr content is limited to 1.50% or less, and preferably 1.00% or less. In addition, Cr is an element that impairs weldability and the toughness of the welded part, and from this viewpoint, the Cr content is further preferably 0.60% or less.
[0034] [Mo:0~1.00%] Mo is an element that contributes to improving strength. The Mo content may be 0%, but from the viewpoint of increasing strength, the Mo content is preferably 0.03% or more, and more preferably 0.08% or more. On the other hand, if Mo is contained excessively, the connectivity of the lamellar structure of pearlite is impaired, and the work hardening ability in the high strain region is impaired. From this viewpoint, the Mo content is limited to 1.00% or less, and preferably 0.50% or less. In addition, Mo is an element that suppresses the growth of Ti carbonitrides, and may increase the density of Ti carbonitrides that contribute to precipitation strengthening, thereby impairing the work hardening ability in the high strain region. From this viewpoint, the Mo content is more preferably 0.30% or less.
[0035] [W:0~1.00%] W is an element that contributes to improving strength. The W content may be 0%, but from the viewpoint of increasing strength, the W content is preferably 0.03% or more, and more preferably 0.08% or more. On the other hand, if W is contained excessively, the hardenability increases excessively and the work hardening ability in the high strain range is impaired. From this viewpoint, the W content is limited to 1.00% or less, preferably 0.50% or less, and more preferably 0.30% or less.
[0036] [B: 0~0.0050%] B is an element that contributes to improving strength, and may be contained at 0.0050% or less. The B content may be 0%, but from the viewpoint of increasing strength, the B content is preferably 0.0005% or more, and more preferably 0.0010% or more. On the other hand, if B is contained excessively, there is a concern that the weldability and toughness of the welded part may be impaired. From this viewpoint, the B content is limited to 0.0050% or less, preferably 0.0025% or less, and more preferably 0.0015% or less.
[0037] [Sn:0~1.000%] Sn is an element that contributes to improving strength, and may be contained at 1.000% or less. The Sn content may be 0%, but from the viewpoint of increasing strength, the Sn content is preferably 0.015% or more, and more preferably 0.030% or more. On the other hand, if Sn is contained excessively, there is a concern that the weldability and toughness of the welded portion may be impaired. From this viewpoint, the Sn content is limited to 1.000% or less, preferably 0.300% or less, and more preferably 0.100% or less.
[0038] [Sb: 0~0.200%] Sb is an element that contributes to improving strength, and may be contained in an amount of 0.200% or less. The Sb content may be 0%, but from the viewpoint of increasing strength, the Sb content is preferably 0.005% or more. On the other hand, if Sb is contained in an excessive amount, there is a concern that the hardenability will be excessively improved and the work hardening ability in the high strain range will be deteriorated. From this viewpoint, the Sb content is limited to 0.200% or less, preferably 0.080% or less, and more preferably 0.030% or less.
[0039] [Ca, Mg, Zr, La, Ce, Te, Hf and REM: 0~0.0050%] Ca, Mg, Zr, La, Ce, Te, Hf and REM are elements that refine sulfides and improve the toughness of steel sheets, and may each be contained in an amount of 0.0050% or less. The content of each element and the total content may be 0%, but to obtain this effect, the content of Ca, Mg, Zr, La, Ce, Te, Hf and REM is preferably 0.0003% or more, and the total content is preferably 0.0008% or more. On the other hand, if these elements are contained in excess, the effect becomes saturated, and therefore, the inclusion of more Ca, Mg, Zr, La, Ce, Te, Hf and REM in the steel sheet than necessary leads to an increase in manufacturing costs. Therefore, the total content of Ca, Mg, Zr, La, Ce, Te, Hf and REM is limited to 0.0050% or less, preferably 0.0035% or less or 0.0030% or less, and more preferably 0.0015% or less. Here, REM is a general term for the lanthanoid group (Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb and Lu) excluding Sc, Y, La and Ce, and the total content of these 15 elements is the REM content.
[0040] In the steel sheet according to the embodiment of the present invention, the balance other than the above elements consists of Fe and impurities. The impurities are components that are mixed in due to various factors in the manufacturing process, including raw materials such as ores and scraps, when the steel sheet is industrially manufactured.
[0041] The chemical composition of steel sheets can be measured by a general analytical method. For example, the chemical composition of steel sheets can be measured using inductively coupled plasma-atomic emission spectrometry (ICP-AES). C and S are measured using the combustion-infrared absorption method.
[0042] [Control of phase transformation by chemical composition] In order to obtain the steel sheet according to the embodiment of the present invention, it is necessary to form a predetermined microstructure by appropriately advancing the phase transformation. In order to control the behavior of the phase transformation, it is necessary to satisfy the following formula (1) in order to appropriately control the chemical composition of the steel sheet. 2.44×10 -2 ×(1.00-0.20[Si]+7.00[Nb])×(1.00-10[B] 0.5 )×(117+17[Si]+11[Si] 2 -33[Mn]+4[Mn] 2 +79[Al]+59[Al] 2 -26[Ni]-12[Cr])×(1+1.3[Si]+12[Mo]+35[Nb]) -1 ≧1.00...Equation (1) Here, [Si], [Nb], [B], [Mn], [Al], [Ni], [Cr] and [Mo] are the contents [mass%] of each element, and are 0 when the element is not contained.
[0043] Formula (1) shows the range of chemical composition that allows ferrite transformation to proceed sufficiently while not excessively promoting or inhibiting pearlite transformation. To explain in more detail, formula (1) takes into consideration the driving force of ferrite transformation, the nucleation rate of ferrite transformation, and the interface mobility (degree of transformation progress). Specifically, the 2.44×10 -2 ×(1.00-0.20[Si]+7.00[Nb])×(1.00-10[B] 0.5 ) corresponds to the nucleation rate of the ferrite transformation, and (117+17[Si]+11[Si] 2 -33[Mn]+4[Mn] 2 +79[Al]+59[Al] 2 -26[Ni]-12[Cr]) corresponds to the driving force of the ferrite transformation, and (1+1.3[Si]+12[Mo]+35[Nb]) -1corresponds to the interface mobility. The larger the value of the left side of formula (1), the higher the temperature at which the ferrite transformation can proceed, and by proceeding with the ferrite transformation at a high temperature, the subsequent pearlite transformation can also proceed at a high temperature, making it possible to form a pearlite structure with a fully developed lamellar structure. From this viewpoint, the value of the left side of formula (1) is set to 1.00 or more, preferably 1.15 or more, and more preferably 1.30 or more.
[0044] [-0.003≦[Ti]-3.42[N]≦0.015] In the steel plate according to the embodiment of the present invention, the content of Ti and N must satisfy the following formula (2) in order to reduce the density of precipitation strengthening particles and fix the carbon (solubilized carbon) dissolved in ferrite as relatively coarse carbonitrides. If the value of [Ti]-3.42[N] is less than -0.003, Ti in the steel is insufficient to combine with N to absorb the solute carbon, and the work hardening ability in the large strain region is not obtained sufficiently. On the other hand, if the value of [Ti]-3.42[N] is more than 0.015, the amount of solute Ti remaining after fixing with N increases, and as a result, the density of fine precipitates that contribute to precipitation strengthening increases, and the work hardening ability in the large strain region is not obtained sufficiently. From the above viewpoints, the value of [Ti]-3.42[N] is preferably -0.003 or more and 0.015 or less, and more preferably 0.000 or more and 0.012 or less. -0.003≦[Ti]-3.42[N]≦0.015...Equation (2) Here, [Ti] and [N] are the contents [mass %] of each element.
[0045] Next, the characteristics of the microstructure of the steel sheet according to the embodiment of the present invention will be described. The steel sheet according to the embodiment of the present invention specifies a microstructure in the range from a position (1 / 8t) that is 1 / 8 of the thickness in the thickness direction from the surface to a position (3 / 8t) that is 3 / 8 of the thickness in the thickness direction from the surface. The reason for this is that the microstructure in the above range centered on a position (1 / 4t) that is 1 / 4 of the thickness in the thickness direction from the surface is a representative structure of the steel sheet, and is highly correlated with the mechanical properties of the steel sheet. The ratios of the following structures in the microstructure are all volume fractions.
[0046] [Ferrite: 80~95%] Ferrite is a structure rich in work hardening ability, and since it exhibits sufficient work hardening ability in the large strain region, it is necessary to include it as a main structure constituting the steel sheet. If the volume fraction of ferrite is less than 80%, the work hardening ability in the large strain region is insufficient, so the volume fraction of ferrite is 80% or more, preferably 82% or more, and more preferably 84% or more or 86% or more. On the other hand, if the fraction of ferrite increases and the fraction of the hard structure decreases excessively, the dislocation substructure that develops around the hard structure is not obtained, and the work hardening ability in the large strain region is reduced instead. In order to ensure a sufficient fraction of the hard structure, the volume fraction of ferrite is limited to 95% or less, preferably 93% or less, and more preferably 91% or less or 89% or less.
[0047] [Perlite: 5~20%] As a hard structure, pearlite promotes the development of dislocation substructures in adjacent ferrite, and furthermore, pearlite itself is strained and work-hardened, thereby enhancing the work-hardening ability in the large strain region. In addition, pearlite is a more preferable hard structure than other hard structures from the viewpoint of suppressing the generation of voids. Pearlite must be contained in the steel sheet at 5% or more, preferably 7% or more, and more preferably 9% or more or 11% or more. On the other hand, if the volume fraction of pearlite is excessively increased, the volume fraction of ferrite becomes insufficient, and the work-hardening ability in the large strain region is reduced, so the volume fraction of pearlite is limited to 20% or less, preferably 18% or less, and more preferably 16% or less or 14% or less.
[0048] [Total of martensite, bainite, bainitic ferrite and retained austenite: 0~5%] The steel sheet according to the embodiment of the present invention may be composed of only ferrite and pearlite, or, if a residual structure exists, the residual structure may include one or more of martensite (including tempered martensite), bainite, bainitic ferrite, and retained austenite. These hard structures promote the development of dislocation substructures in adjacent ferrite and enhance the work hardening ability in the large strain region. However, if a large amount of these hard structures is contained, voids are easily formed in the large strain region, which deteriorates the work hardening ability, so the total volume fraction of these structures is limited to 5% or less. The total volume fraction of these structures is preferably 2% or less or 1% or less, and may be 0%.
[0049] Next, the characteristics of the ferrite region will be described.
[0050] [Average grain size of ferrite: 2~16μm] In order to improve the work hardening ability in the large strain region, the average grain size of ferrite is controlled. If the average grain size of ferrite is excessively refined, the work hardening ability at the beginning of deformation increases excessively, and dislocation substructures develop during that time, resulting in a deterioration of the work hardening ability in the large strain region. For this reason, the average grain size of ferrite is set to 2 μm or more, preferably 4 μm or more, and more preferably 5 μm or more or 7 μm or more. On the other hand, if the grain size of ferrite is excessively coarse, strain is concentrated in a part of the microstructure, and voids are generated in the large strain region, resulting in a deterioration of the work hardening ability. For this reason, the grain size of ferrite is set to 16 μm or less, preferably 14 μm or less, and more preferably 13 μm or less or 11 μm or less.
[0051] [Density of precipitation strengthening particles contained in ferrite grains: 1.0×10 22 pieces / m 3 below] Ferrite is a soft structure with high work hardening ability, but ferrite containing a large amount of fine precipitates increases its strength through precipitation strengthening, but its work hardening ability is impaired. In ferrite grains, the density of fine precipitates with major diameters of 4 to 20 nm (hereinafter referred to as precipitation strengthening particles), which contribute particularly to precipitation strengthening, is 1.0 × 10 22 pieces / m 3 If the density exceeds 1.0×10, the work hardening ability in the large strain region is significantly degraded. 22 pieces / m 3 Limited to 0.3×10 22 pieces / m 3 It is preferable to keep it below 0.1×10 22 pieces / m 3 From the viewpoint of increasing the work hardening ability, the lower the density of the precipitation hardening particles, the more preferable it is, and therefore the lower limit is not particularly limited. In fact, in the measurement of the precipitation hardening particles, 22 pieces / m 3 In order to specify a specific density less than 100 nm, a large amount of measurements are required, and therefore it is not practical to specifically define the lower limit of the density. As described above, the precipitation strengthening particles are fine precipitates with a major axis of 4 to 20 nm, and include at least one selected from alloy carbonitrides, intermetallic compounds, and metal particles. The alloy carbonitride may be at least one selected from Nb(CN), Ti(CN), V(CN), and mixtures thereof. In this specification, Nb(CN) includes NbC, NbC in which part of C is replaced by N, and / or NbN in which part of N is replaced by C, and the same applies to V(CN). Nb(CN), Ti(CN), and V(CN) may also include other elements such as Mo in part of them. The intermetallic compound may be, for example, NiAl, etc. The metal particles may be, for example, Cu, etc.
[0052] [Density of cementite particles contained in ferrite grains: 1.0×10 10 pieces / m 2 below] Ferrite is a soft structure with high work-hardening capacity. However, when coarse cementite is included inside, voids are generated around the cementite in the large strain region, and the work-hardening capacity is deteriorated. From this point of view, the density of cementite particles with a major axis of 0.5 μm or more contained in ferrite grains is set to 1.0 × 10 10 pieces / m 2 Limited to 0.3×10 10 pieces / m 2 It is preferable to keep it below 0.1×10 10 pieces / m 2 From the viewpoint of increasing the work hardening ability, the lower the density of the cementite particles, the more preferable, and therefore the lower limit is not particularly limited. 10 pieces / m 2 In order to specify a specific density below this limit, a large amount of measurement would be required, and therefore it is not practical to specifically specify the lower limit of the density.
[0053] [Average aspect ratio of ferrite grains: 2.00 or less] According to a preferred embodiment of the present invention, the concentration of strain in a part of the microstructure is suppressed by making the crystal grains of ferrite isotropic, and the generation of voids in the large strain region is suppressed, thereby further improving the work hardening ability. From this viewpoint, the average aspect ratio, which is the ratio of the major axis to the minor axis of the crystal grains in ferrite, is preferably 2.00 or less, more preferably 1.70 or less or 1.50 or less. Although the lower limit is not particularly limited, for example, the average aspect ratio of the crystal grains in ferrite may be 1.00 or more, 1.10 or more, or 1.20 or more.
[0054] Next, the characteristics of the pearlite region will be described.
[0055] [Average circle equivalent diameter of pearlite island regions: 8.0 μm or less] In the embodiment of the present invention, pearlite is present in the form of islands dispersed among the ferrite grains that occupy the majority, i.e., 80% or more, of the microstructure of the steel sheet, but if the size of such pearlite islands is excessively large, strain is concentrated in a part of the microstructure, and voids are generated in the large strain region, resulting in deterioration of work hardening ability. For this reason, the average circle equivalent diameter of the pearlite island region, i.e., the pearlite islands, is limited to 8.0 μm or less, preferably 6.0 μm or less, and more preferably 4.0 μm or less. The lower limit is not particularly limited, but for example, the average circle equivalent diameter of the pearlite islands may be 0.5 μm or more or 1.0 μm or more.
[0056] [Average ratio of the average long diameter of the cementite that forms the lamellar structure of pearlite to the circle equivalent diameter of the island region of pearlite in which the cementite exists: 0.20 or more] If the lamellar structure of pearlite is broken inside, voids are generated at the broken parts of the lamellar structure in the large strain region, and the work hardening ability is deteriorated. For this reason, it is preferable that the cementite forming the lamellar structure of pearlite exists continuously in the island-like pearlite. From this viewpoint, as shown in the following formula (4), the average ratio of the average long diameter of the cementite forming the lamellar structure of pearlite to the circle equivalent diameter of the island-like region made of pearlite in which the cementite exists is set to 0.20 or more, preferably 0.35 or more, and more preferably 0.50 or more. The upper limit is not particularly limited, but for example, the average of the above ratio may be 0.90 or less or 0.80 or less.
number
[0057] [Density of precipitation strengthening particles contained within the ferrite that forms the lamellar structure of pearlite: 1.0×10 22pieces / m 3 below] The ferrite that forms the lamellar structure of pearlite is soft and highly deformable, but ferrite that contains a large amount of fine precipitates has increased strength due to precipitation strengthening, but its deformability is impaired. When the density of fine precipitates (hereinafter, precipitation strengthening particles) with a major axis of 4 to 20 nm, which contribute particularly to precipitation strengthening, in the ferrite that forms the lamellar structure of pearlite is 1.0 × 10 22 pieces / m 3 When the density exceeds 1.0×10, the deformability in the large strain region is greatly deteriorated, and voids are generated in the pearlite, deteriorating the work hardening ability. Therefore, the density of precipitation strengthening particles is 1.0×10 22 pieces / m 3 Limited to 0.3×10 22 pieces / m 3 It is preferable to keep it below 0.1×10 22 pieces / m 3 It is more preferable that the density of the precipitation strengthening particles is 0.001×10 or less. 22 pieces / m 3 or more than 0.01×10 22 pieces / m 3 or more. As described above, the precipitation strengthening particles are fine precipitates having a major axis of 4 to 20 nm, and include at least one selected from alloy carbonitrides, intermetallic compounds, and metal particles. The alloy carbonitrides may be at least one selected from Nb(CN), Ti(CN), V(CN), and mixtures thereof. Nb(CN), Ti(CN), and V(CN) may contain other elements such as Mo in part. The intermetallic compounds may be NiAl, for example. The metal particles may be Cu, for example.
[0058] The above-mentioned microstructural features are evaluated by detailed observation of the steel sheet. Specifically, a small piece is cut out from a 1 / 2 width portion of the steel sheet or processed steel sheet, covering a range from a position of 1 / 8 of the sheet thickness from the surface in the sheet thickness direction to a position of 3 / 8 of the sheet thickness from the surface in the sheet thickness direction, and used as an observation sample. The volume fraction of the retained austenite is calculated by obtaining a diffraction peak of the fcc phase in the above-mentioned range in the sheet thickness direction by X-ray diffraction. The volume fraction of each structure other than the retained austenite, the average crystal grain size of ferrite, the average aspect ratio of the crystal grains, the density of the cementite particles in the ferrite grains, the circle equivalent diameter of the island regions made of pearlite, and the average major axis of the cementite forming the lamellar structure of pearlite are observed and measured using a field emission scanning electron microscope, and a cross section parallel to the rolling direction and perpendicular to the sheet surface is used as the observation surface, and the observation surface is wet-polished and polished with colloidal silica to make it a mirror surface, and then corroded with nital (a mixture of ethanol and nitric acid) to prepare an observation sample. In the range of the plate thickness direction, the average long diameter of the cementite forming the lamellar structure of pearlite is observed and evaluated in the range of 5000 to 30000 times, and the rest is observed and evaluated in the range of 1000 to 3000 times. In addition, the observation of the precipitation strengthening particles is performed by preparing a needle-shaped test piece from the plate thickness region of the small piece, creating a three-dimensional atomic map using a three-dimensional atom probe, and identifying the precipitation strengthening particles to obtain the long diameter. Next, the density of the precipitation strengthening particles is calculated using the measurement field of view as the denominator and the number of precipitation strengthening particles as the numerator.
[0059] The volume fraction of the material other than the retained austenite was evaluated by the above-mentioned electron microscope observation, and the total volume fraction was 1.0 × 10 -8 m 2The microstructure of the above region is photographed, and the structure at 200 or more lattice points is determined by the point counting method, and the area fraction of each structure is obtained. The average crystal grain size of ferrite is obtained by drawing lines of 100 μm or more in the plate thickness direction, rolling direction, and 45-degree direction between the plate thickness direction and the rolling direction on the photograph observed with the electron microscope, and the average crystal grain size is obtained by the intercept method. Furthermore, the average aspect ratio of crystal grains in ferrite is obtained by calculating the aspect ratio, which is the ratio of the major axis to the minor axis, for 10 or more ferrite crystal grains randomly selected from the photograph observed with the electron microscope, and the simple average of the aspect ratio group is regarded as the average aspect ratio of crystal grains in ferrite. The circle equivalent diameter of pearlite islands is obtained by measuring the area of 10 or more pearlite islands randomly selected from the photograph observed with the electron microscope, converting it into a circle equivalent diameter, and the simple average of the circle equivalent diameter group is regarded as the average circle equivalent diameter of the pearlite island region. In addition to the circle-equivalent diameter of the island regions, the major axis of 10 or more randomly selected cementite particles forming lamellar structures in each island region is measured and the average value is calculated. From these values, the ratio of the average major axis of the cementite particles forming the lamellar structure of pearlite to the circle-equivalent diameter of the island region made of pearlite in which the cementite exists is calculated.
[0060] [Mechanical properties] [Tensile strength (TS), total elongation (EL) and yield strength (YS)] According to the steel sheet having the above chemical composition and microstructure, a high tensile strength (TS), specifically a tensile strength of 400 MPa or more can be achieved. The tensile strength is preferably 420 MPa or more, 440 MPa or more, or 490 MPa or more. The upper limit is not particularly limited, but for example, the tensile strength may be 780 MPa or less, 700 MPa or less, or 650 MPa or less. Furthermore, according to the steel sheet according to the embodiment of the present invention, a total elongation (EL) of 20% or more can be achieved. The total elongation is preferably 22% or more, 25% or more, or 30% or more. The upper limit is not particularly limited, but for example, the total elongation may be 45% or less, 42% or less, or 40% or less. Furthermore, according to the steel sheet according to the embodiment of the present invention, a yield strength (YS) of 280 MPa or more can be achieved. The yield strength is preferably 300 MPa or more, or 350 MPa or more. The upper limit is not particularly limited, but for example, the yield strength may be 550 MPa or less, 500 MPa or less, or 450 MPa or less. The tensile strength, total elongation and yield strength were measured by taking a JIS14A test piece from a direction in which the longitudinal direction of the test piece was parallel to the rolling direction perpendicular to the steel plate (C direction) and conducting a tensile test in accordance with JIS Z 2241:2011. The yield strength means the 0.2% proof stress obtained by the above tensile test.
[0061] [Steel plate manufacturing method] Next, a preferred method for manufacturing the steel sheet according to the embodiment of the present invention will be described. The following description is an example of a characteristic method for manufacturing the steel sheet according to the embodiment of the present invention, and is not intended to limit the steel sheet to one manufactured by the manufacturing method described below.
[0062] The method for producing a steel sheet according to an embodiment of the present invention comprises: casting a slab having the chemical composition described above in relation to the steel plate, followed by cooling to below 500°C; A heating step in which the maximum heating temperature of the slab is 1000 to 1150°C, and the total residence time at a temperature of 1000°C or higher satisfies the following formula (3): a rough rolling step of subjecting the slab to rough rolling so that a cumulative rolling reduction rate in a temperature range of 1000° C. or higher is 25% or more, and then subjecting the slab to a retention time of 30 seconds or more; A finish rolling process in which the obtained rolled material is subjected to finish rolling so that the cumulative rolling reduction in a temperature range of 950°C or less is 30% or more, and the completion temperature of the finish rolling is 850 to 920°C; A cooling process for water-cooling the obtained steel sheet, in which the time elapsed from the completion of the finish rolling process until the temperature of the steel sheet reaches 630°C is 60 seconds or more, the water-cooling start temperature is 600 to 630°C, the water-cooling end temperature is 400 to 450°C, and the temperature of the steel sheet is controlled so as not to exceed 450°C by recuperation after water-cooling. The present invention is characterized in that it includes:
number
[0063] [Casting process] First, a slab having the chemical composition described above in relation to the steel plate is manufactured, but the manufacturing method of the slab is not particularly specified, and it can be manufactured by, for example, a continuous casting method or a blooming method. The manufactured slab is cooled to 500 ° C or less in order to sufficiently grow Ti carbonitrides. If the cooling temperature exceeds 500 ° C, the growth of Ti carbonitrides becomes insufficient, and Ti carbonitrides melt excessively in the heating process, and many fine precipitates that contribute to precipitation strengthening are generated during the subsequent cooling process, and the work hardening ability in the large strain region is deteriorated. From this viewpoint, the cooling end temperature of the slab is preferably 450 ° C or less, and more preferably 400 ° C or less. There is no particular lower limit set for the cooling end temperature of the slab, but even if it is cooled below 300 ° C, the growth of Ti carbonitrides is saturated, while the amount of heat required for heating the slab in the subsequent heating process increases, which is economically undesirable.
[0064] [Heating process] The produced slab is subjected to a heat treatment with a maximum heating temperature in the range of 1000 to 1150 ° C. for hot rolling. If the maximum heating temperature is lower than 1000 ° C., coarse cementite remains unmelted, which impairs the work hardening ability in the large strain region. On the other hand, if the maximum heating temperature exceeds 1150 ° C., the Ti carbonitride in the slab melts excessively, and many fine precipitates that contribute to precipitation strengthening are generated in the cooling process, impairing the work hardening ability in the large strain region. Therefore, in the heating process, it is important to heat the slab within a range in which the Ti carbonitride melts but does not melt excessively, although some of the Ti carbonitride melts. From the above viewpoints, the maximum heating temperature is set to 1000 to 1150 ° C. Furthermore, since the isotropy of the microstructure is improved by increasing the maximum heating temperature, the maximum heating temperature is preferably set to 1070 ° C. or higher.
[0065] In order to heat the slab sufficiently, the total residence time at a temperature of 1000°C or higher must satisfy formula (3). If heating is insufficient and formula (3) is not satisfied, coarse cementite remains unmelted, which impairs the work hardening ability in the large strain region. Furthermore, since sufficient heating improves the isotropy of the microstructure, it is preferable that the value of the left side of formula (3) is 1.50 or more. There is no particular upper limit, but for example, the value of the left side of formula (3) may be 7.00 or less or 5.00 or less.
number
[0066] [Rough rolling process] The slab that has been subjected to the heat treatment is subjected to rough rolling at a temperature range of 1000°C or higher with a cumulative rolling reduction of 25% or more relative to the slab thickness. By performing a relatively high rough rolling of 25% or more in a temperature range of 1000°C or higher where recrystallization progresses, it is possible to promote the refinement of the microstructure. If the cumulative rolling reduction in the temperature range is less than 25%, the average crystal grain size of ferrite in the finally obtained microstructure becomes coarse, and the work hardening ability in the large strain region deteriorates. From this viewpoint, the cumulative rolling reduction in the temperature range is set to 25% or more, and preferably 30% or more. There is no particular upper limit for this cumulative rolling reduction, but since excessive rolling makes the steel sheet too thin, making it difficult to ensure a sufficient rolling reduction in the subsequent finish rolling process, it is preferable to set it to 70% or less.
[0067] After the rough rolling, a sufficient elapsed time (dwell time) is allowed to pass before the next rolling begins, to promote the coarsening of Ti carbonitrides and reduce excess solute Ti. If the elapsed time is less than 30 seconds, many fine precipitates that contribute to precipitation strengthening are formed, and the work hardening ability in the large strain region is deteriorated. Furthermore, recrystallization progresses during this elapsed time, and the structure becomes finer and isotropic. From this viewpoint, the elapsed time is preferably 45 seconds or more. The upper limit is not particularly limited, but the elapsed time may be, for example, 120 seconds or less or 100 seconds or less.
[0068] [Finish rolling process] After the elapsed time, the steel sheet is subjected to finish rolling until the sheet thickness reaches the product sheet thickness. The finish rolling may be started at a temperature higher than 950°C after the elapsed time, but in a temperature range of 950°C or less, the finish rolling is performed with a cumulative reduction of 30% or more with respect to the sheet thickness at the time of reaching 950°C, with the finish rolling completion temperature being 850 to 920°C. If the cumulative reduction at 950°C or less is less than 30%, the average crystal grain size of ferrite becomes coarse, and the structure of the steel sheet according to the embodiment of the present invention cannot be obtained. Furthermore, in order to make the microstructure of the steel sheet fine and isotropic, the cumulative reduction is preferably 45% or more. Also, if the completion temperature of the finish rolling exceeds 920°C, the average crystal grain size of ferrite becomes coarse, and the structure of the steel sheet according to the embodiment of the present invention cannot be obtained. On the other hand, if the completion temperature of the finish rolling is lower than 850°C, the pearlite island regions become coarse, and the structure of the steel sheet according to the embodiment of the present invention cannot be obtained. In order to sufficiently advance recrystallization and increase the isotropy of the microstructure, the finish rolling is preferably completed at a temperature of 875° C. or higher.
[0069] [Cooling process] After the finish rolling process is completed, the steel sheet is cooled to 630°C for 60 seconds or more to advance the phase transformation and obtain a predetermined microstructure. Since the temperature drop behavior of the steel sheet differs depending on the sheet thickness, water cooling, gas cooling, air cooling, cooling, heat retention, heating, and other treatments may be appropriately performed within the range of satisfying the above conditions. In addition, descaling, which is performed by high-pressure spraying of a small amount of water for the purpose of removing scale from the steel sheet surface, and / or leveling processing for the purpose of shape correction may be performed before reaching 630°C, within the range of observing the above conditions. If the time to 630°C is less than 60 seconds, the phase transformation proceeds at an excessively low temperature, and the volume fraction of ferrite and / or pearlite is insufficient, or the volume fraction of structures other than ferrite and pearlite is excessively increased, or the development of the lamellar structure of pearlite is insufficient, and the microstructure of the steel sheet according to the embodiment of the present invention is not obtained. The upper limit is not particularly limited, but for example, the time to reach 630°C may be 200 seconds or less.
[0070] After reaching 630°C, water cooling is started before reaching 600°C, and the material is cooled to a water cooling stop temperature of 400 to 450°C. If water cooling is not performed, the water cooling start temperature is below 600°C, or the water cooling stop temperature is above 450°C, Ti forms many fine precipitates that contribute to precipitation strengthening, and the work hardening ability in the large strain region is deteriorated. On the other hand, if the water cooling start temperature is higher than 630°C, a lot of hard structures are generated, and voids are formed in the large strain region, and the work hardening ability is deteriorated. In addition, in the temperature range below 400°C after water cooling is stopped, it is necessary to grow the Ti carbonitrides and the like that have already precipitated to a size that does not contribute to precipitation strengthening. If the water cooling stop temperature is less than 400°C, the growth of such precipitates becomes insufficient, and a relatively large number of fine precipitates that contribute to precipitation strengthening may be formed in the microstructure finally obtained. Furthermore, in order to prevent Ti from forming fine precipitates that contribute to precipitation strengthening or to sufficiently reduce the formation of such precipitates, the temperature at which the steel is reheated after water cooling is controlled so as not to exceed 450°C.
[0071] Although the upper limit of the plate thickness of the steel plate according to the embodiment of the present invention is not particularly set, if the plate thickness exceeds 150 mm, there is a concern that casting defects remain even after rolling and act as cracks during local deformation to cause damage during collision, so the plate thickness is preferably 150 mm or less, and more preferably 120 mm or less. Similarly, although the lower limit of the plate thickness is not particularly set, there is a concern that if the steel plate is made too thin, the steel plate will naturally cool before pearlite with a regular lamellar structure is generated, so the plate thickness is preferably 10 mm or more or 25 mm or more, more preferably 40 mm or more, and even more preferably 50 mm or more.
[0072] According to the steel sheet manufactured by the above manufacturing method, the microstructure can be formed as a composite structure containing ferrite as a main component and pearlite as a hard structure in a predetermined ratio, and the average crystal grain size of the ferrite can be appropriately refined, and the density of the precipitation strengthening particles and coarse cementite contained in the ferrite grains, which may adversely affect the improvement of the work hardening ability, can be limited within a predetermined range. In addition, the pearlite exists in a fine island shape, and the connectivity of the lamellar structure of the pearlite is sufficiently ensured, and the density of the precipitation strengthening particles contained in the ferrite forming the lamellar structure can be limited. In addition, by containing an appropriate amount of Ti, the solid solution carbon in the ferrite, which may also adversely affect the work hardening ability, can be sufficiently absorbed by Ti, while the precipitates such as Ti carbonitrides related thereto can be grown to a size that does not contribute to precipitation strengthening, and as a result, the density of the precipitation strengthening particles can be limited within a predetermined range. Therefore, according to the steel plate manufactured by the above-mentioned manufacturing method, the work hardening ability in the large strain region corresponding to the time after local deformation begins to progress can be significantly improved. Therefore, such a steel plate is useful for suppressing strain concentration during deformation due to collision and suppressing the occurrence of holes, and is particularly useful for application to structures that are at risk of collision with ships and the like on the ocean, such as ships, floating bodies, and marine structures.
[0073] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way. EXAMPLES
[0074] In the following examples, steel sheets according to the embodiments of the present invention were produced under various conditions, and the work hardening ability of the resulting steel sheets in the large strain region was examined.
[0075] Molten steel having the chemical composition shown in Table 1 was processed in the casting process, heating process, rough rolling process, finish rolling process, and cooling process under the conditions shown in Table 2 to obtain steel plates as examples, including invention examples and comparative examples.
[0076] [Table 1]
[0077] [Table 2]
[0078] [Evaluation of work hardening capacity (WHR) in the large strain region] The work hardening capacity (hereinafter, WHR) in the large strain region was evaluated using a small round bar tensile test piece with a parallel part length of 2.0 mm and a parallel part diameter of 1.0 mmφ, and was calculated using the following formula. WHR i =(σ i -σ i-1 ) / (ε i -ε i-1 ) Here, σ i and ε i are the true stress and true strain obtained from the load and the cross-sectional area of the neck, respectively.
[0079] The WHR at a true strain of 0.6 was simulated as an indication of the work hardening capacity in the large strain region, and a value of 300 MPa or more was evaluated as a steel sheet with improved work hardening capacity in the large strain region.
[0080] [Table 3]
[0081] Table 3 shows the microstructure and WHR of the steel sheet obtained as an example. The "others" in the volume fraction in Table 3 means the total of martensite, bainite, bainitic ferrite and retained austenite. θ / D Pmeans the average ratio of the average long diameter of the cementite forming the lamellar structure of pearlite to the circle equivalent diameter of the island region of pearlite in which the cementite exists. As reference values, the tensile properties, i.e., YS (0.2% yield strength), TS (tensile strength), and EL (total elongation), evaluated in accordance with JIS Z 2241:2011 using a tensile test piece (JIS14A test piece taken in the direction of the longitudinal axis) with a strain gauge length of 24.0 mm and a parallel part diameter of 6.0 mmφ, are shown.
[0082] In the examples shown in Tables 1 to 3, Experiment No. 58 is a comparative example in which the value of formula (2) determined by the chemical composition was low, Ti was insufficient to absorb solute carbon, and WHR was low. Furthermore, Experiment No. 60 is a comparative example in which Ti content was low and WHR was low. Moreover, experiment No. 57 is a comparative example in which the value of formula (1), which is determined by the chemical composition, was low, so that sufficient ferrite was not obtained and the WHR was low. Furthermore, Test No. 59 is a comparative example in which the value of formula (2), which is determined by the chemical composition, was high, resulting in an increased density of precipitation strengthening particles in ferrite and a low WHR.
[0083] Experiment No. 9 is a comparative example in which the cooling end temperature in the casting process was high, which increased the density of precipitation strengthening particles in the ferrite and reduced the WHR.
[0084] Experiment No. 16 is a comparative example in which the maximum heating temperature in the heating process was low, the density of coarse cementite increased, and the WHR decreased. Experiment No. 25 is a comparative example in which the total residence time at temperatures of 1000°C or higher in the heating process did not satisfy formula (3), and the density of coarse cementite increased and the WHR decreased. Experiment No. 20 is a comparative example in which the maximum heating temperature in the heating process was high, the density of precipitation strengthening particles in ferrite increased, and the WHR decreased.
[0085] Experiment No. 3 is a comparative example in which the cumulative reduction rate in the rough rolling process was small, the average grain size of ferrite became coarse, and the WHR was low. Experiment No. 35 is a comparative example in which the residence time after rolling in the rough rolling step was short, the density of precipitation strengthening particles in ferrite increased, and the WHR was low.
[0086] Test No. 49 is a comparative example in which the cumulative reduction rate in the finish rolling process was small, the average grain size of ferrite became coarse, and the WHR was low. Experiment No. 5 is a comparative example in which the rolling completion temperature in the finish rolling process was low, the average circular equivalent diameter of the island pearlite became coarse, and the WHR was low. Test No. 42 is a comparative example in which the rolling completion temperature in the finish rolling process was high, the average grain size of ferrite became coarse, and the WHR was low.
[0087] Experiments Nos. 4, 10, and 23 are comparative examples in which the time elapsed from the completion of the finish rolling process in the cooling process until the temperature of the steel plate reached 630°C was short, resulting in low WHR. More specifically, Experiment No. 4 is an example in which the connectivity of cementite in pearlite was poor. Experiments Nos. 10 and 23 are examples in which the volume fraction of ferrite and / or pearlite was insufficient, or the volume fraction of structures other than these was excessively increased. Experiment No. 29 is a comparative example in which the water-cooling start temperature in the cooling process was low, which increased the density of precipitation strengthening particles in ferrite and reduced the WHR. Experiment No. 14 is a comparative example in which the water-cooling start temperature in the cooling process was high, a large amount of hard structure was generated, and the WHR was low. Experiment No. 33 is a comparative example in which the water cooling stop temperature in the cooling process is low, the density of precipitation strengthening particles in ferrite is increased, and the WHR is low. Experiment No. 27 is a comparative example in which the water cooling stop temperature in the cooling process was high, and therefore the temperature reached by reheating after water cooling was stopped was high, increasing the density of precipitation strengthening particles in ferrite and resulting in a low WHR. Test No. 46 is a comparative example in which the temperature reached by reheating after water cooling was stopped in the cooling process was high, the density of precipitation strengthening particles in ferrite increased, and the WHR was low. Experiment No. 38 is an example in which water cooling was not performed in the cooling process, and is a comparative example in which the density of precipitation strengthening particles in pearlite increased and the WHR decreased.
[0088] The examples other than these comparative examples are examples of the present invention (invention examples), and all of them show high WHR. In the invention examples and comparative examples, all of the ones in which the presence of precipitation strengthening particles was clearly confirmed contained Ti(CN) or the like.
Claims
1. The chemical composition, in mass%, is C: 0.075-0.240%, Si: 1.25% or less, Mn: 0.50-2.00%, P: 0.030% or less, S: 0.0100% or less, N: 0.0150% or less, O: 0.0030% or less, Al: 1.000% or less, Ti: 0.004 to 0.030%, Nb: 0 to 0.015%, V: 0-0.100%, Cu: 0 to 0.10%, Ni: 0-3.00%, Cr: 0-1.50%, Mo: 0-1.00%, W: 0-1.00%, B: 0 to 0.0050%, Sn: 0-1.000%, Sb: 0 to 0.200%, The total of one or more of Ca, Mg, Zr, La, Ce, Te, Hf, and REM: 0 to 0.0050%, and The balance is composed of Fe and impurities. The following formulas (1) and (2) are satisfied, The microstructure in the range from the surface to the position of 1 / 8 of the plate thickness in the plate thickness direction to the position of 3 / 8 of the plate thickness in the plate thickness direction from the surface is, in terms of volume fraction, Ferrite: 80-95%, Perlite: 5-20%, and The sum of martensite, bainite, bainitic ferrite and retained austenite: 0 to 5%; The average grain size of the ferrite is 2 to 16 μm, The density of the precipitation strengthening particles contained in the ferrite grains is 1.0×10 22 pieces / m 3 is as follows: The density of the cementite particles contained in the ferrite grains is 1.0×10 10 pieces / m 2 is as follows: The average circular equivalent diameter of the island regions made of pearlite is 8.0 μm or less, The ratio of the average long diameter of the cementite forming the lamellar structure of the pearlite to the circle equivalent diameter of the island regions consisting of the pearlite in which the cementite is present is 0.20 or more on average, The density of the precipitation strengthening particles contained in the ferrite forming the lamellar structure of the pearlite is 1.0×10 22 pieces / m 3 A steel plate, characterized in that: 2.44×10 -2 ×(1.00 - 0.20[Si] + 7.00[Nb])×(1.00 - 10[B] 0.5 )×(117 + 17[Si] + 11[Si] 2 - 33[Mn] + 4[Mn] 2 + 79[Al] + 59[Al] 2 - 26[Ni] - 12[Cr])×(1 + 1.3[Si] + 12[Mo] + 35[Nb]) -1 ≥1.00 ··· Formula (1) -0.003≦[Ti]-3.42[N]≦0.015...Formula (2) Here, [Si], [Nb], [B], [Mn], [Al], [Ni], [Cr], [Mo], [Ti] and [N] are the contents [mass %] of each element, and are 0 when the element is not contained.
2. The chemical composition, in mass%, Nb: 0.004 to 0.012%, V: 0.020-0.080%, Cu: 0.02-0.08%, Ni: 0.15-2.30%, Cr: 0.10-1.00%, Mo: 0.03-0.50%, W: 0.03-0.50%, B: 0.0005-0.0025%, Sn: 0.015-0.300%, Sb: 0.005 to 0.080%, and Sum of one or more of Ca, Mg, Zr, La, Ce, Te, Hf, and REM: 0.0008 to 0.0030% The steel sheet according to claim 1 , further comprising one or more selected from the following:
3. The steel sheet according to claim 1 or 2, characterized in that the average aspect ratio of crystal grains in the ferrite is 2.00 or less.
4. A casting step of casting a slab having the chemical composition according to claim 1 or 2 and then cooling it to 500°C or less; A heating step of heating the slab, the maximum heating temperature of the slab being 1000 to 1150°C, and the total residence time at a temperature of 1000°C or higher satisfying the following formula (3); a rough rolling step of subjecting the slab to rough rolling so that a cumulative rolling reduction in a temperature range of 1000° C. or higher is 25% or more, and then subjecting the slab to a retention time of 30 seconds or more; A finish rolling process in which the obtained rolled material is subjected to finish rolling so that the cumulative rolling reduction in a temperature range of 950° C. or less is 30% or more, and the completion temperature of the finish rolling is 850 to 920° C.; A cooling process for water-cooling the obtained steel plate, in which the time elapsed from the completion of the finish rolling process until the temperature of the steel plate reaches 630°C is 60 seconds or more, the water-cooling start temperature is 600 to 630°C, the water-cooling end temperature is 400 to 450°C, and the temperature of the steel plate is controlled so as not to exceed 450°C by recuperation after water-cooling. A method for producing a steel sheet, comprising: [0010] X 10 is a value obtained by dividing the total residence time at a temperature of 1000° C. or higher by 10 according to the above calculation formula, t is the total residence time at a temperature of 1000° C. or higher divided into 10 equal parts [seconds], T i is the temperature [°C] after the i-th time of the residence time divided into 10 equal parts has elapsed, A 1 , A 2 , A 3 , A 4 , A 5 and A 6 are constants, and each is 4.04 × 10 3 , −3.14×10 4 , 1.55×10 3 , 6.12 x 10 -8 , 6.28×10 4 and 5.46 x 10 2 and X i and t i is a numerical value obtained by calculating from 1 to i in order according to the above formula.
5. The maximum heating temperature in the heating step is 1070 to 1150° C., The method for producing a steel plate according to claim 4, characterized in that the cumulative rolling reduction in the finish rolling step is 45% or more, and the finish rolling completion temperature is 875 to 920°C.
Citation Information
Patent Citations
Low-yield-ratio high-strength steel sheet excellent in ductile fracture resistance performance
JP2013139602A
Method for producing non-heat-treated high tensile strength steel plate excellent in high input welding characteristic and ductility
JP2015193920A
High-strength and high-ductility thick steel plate and production method thereof
JP2016125077A
Thick steel plate and manufacturing method therefor
JP2018193605A
Thick steel plate for ship hull and process for production thereof
WO2011062000A1