Steel plate and method for manufacturing the same

A steel plate with a controlled microstructure and manufacturing process improves bendability and suppresses crack formation in collision-prone structures by optimizing ferrite content and reducing elongated inclusions, addressing the limitations of existing steel plates in ships and offshore structures.

JP2024151088APending Publication Date: 2024-10-24NIPPON STEEL CORPORATION
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023064221
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-11
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Existing steel plates used in ships, floating bodies, and offshore structures face challenges in suppressing cracks during collisions due to strain concentration, despite improvements in ductility and strength, necessitating enhanced bendability to minimize damage.

Method used

A steel plate with a specific chemical composition and controlled microstructure, primarily composed of ferrite with limited hard structures and reduced elongated inclusions, achieved through precise manufacturing processes including controlled cooling and hot rolling, ensuring a homogeneous texture and improved bendability.

Benefits of technology

The solution significantly suppresses crack formation on strain-concentrated areas during collisions, enhancing both bendability and uniform elongation, making it suitable for structures prone to collisions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024151088000001
    Figure 2024151088000001
  • Figure 2024151088000002
    Figure 2024151088000002
  • Figure 2024151088000003
    Figure 2024151088000003
Patent Text Reader

Abstract

To provide a steel plate having improved bendability, and a method for manufacturing the same.SOLUTION: There are provided a steel plate that has a prescribed chemical composition, in which a micro structure in a depth region to 300 μm in a depth direction from the surface contains 90% or more ferrite, and 0 to 3% of the total of martensite, bainite, bainitic ferrite and retained austenite, in a volume fraction, a density of an elongation inclusion in the depth region is 1.0×105 pieces / m2 or less, and peak intensity in a 45-degree cross section in a three-dimensional crystal orientation distribution function of a BCC phase in the depth region is 5.0 or less; and a method for manufacturing the same.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a steel plate and a manufacturing method thereof, and more particularly to a steel plate having improved bendability and therefore useful for suppressing the occurrence of cracks on the surface of strain-concentrated areas during a collision, and a manufacturing method thereof. [Background technology]

[0002] Ships, floating bodies, and marine structures are at risk of collision with ships that deviate from their course on the ocean, so their designs must ensure that they do not lose their stability even if they are hit by an anticipated collision. To ensure stability, fenders and other materials are used to mitigate the impact, and structures are divided into multiple blocks to minimize the impact of holes caused by a collision. Designs to prepare for such collisions are considered in addition to the design required for the original purpose, and they increase the construction costs of ships, floating bodies, and marine structures.

[0003] As with ships, floating bodies, and marine structures, automobiles are also required to control damage to the body during a collision and keep it within an acceptable range for anticipated collisions in order to protect the safety of passengers. As described in Non-Patent Document 1, one solution to this problem in automobiles is to improve the strength of the steel materials used. By applying high-strength steel materials that do not easily break to the body, it is possible to significantly improve safety during a collision even for a body that follows the same design as before.

[0004] Similarly, in ships, the degree of damage during collision can be reduced by improving the properties of materials. For example, Patent Document 1 proposes a high-strength, high-ductility steel plate that controls the microstructure, reduces the dislocation density in soft ferrite grains, and homogenizes the hardness distribution in the plate thickness direction as a means of suppressing the occurrence of holes in the side of the ship during a ship collision. Specifically, the high-strength, high-ductility steel plate described in Patent Document 1 has a lower limit of total elongation (T.EL) of 23% or more, which is 1.5 times that of general steel, a yield strength (YP) of 355 to 500 MPa, and a tensile strength (TS) of 490 to 620 MPa.

[0005] Furthermore, Patent Document 2 proposes a high-strength thick steel plate having excellent toughness and brittle crack propagation arrestability in high heat input welds, the high-strength thick steel plate having a specified chemical composition, a (211) plane X-ray intensity ratio of 1.2 or more in a plane parallel to the plate surface of the steel plate, a (211) plane X-ray intensity ratio of 1.5 or more and a (222) plane X-ray intensity ratio of 2.5 or less in a plane parallel to the plate surface at the center of the plate thickness, and a plate thickness of more than 50 mm.

[0006] Furthermore, Patent Document 3 proposes a high-strength extra thick steel plate with a thickness of 70 mm or more, which has a predetermined chemical composition, a texture in which the (211) plane integration degree on the rolled surface at the center of the plate thickness is 1.7 or more, and a (200) plane integration degree on the steel plate surface is 1.3 or more, as a high-strength extra thick steel plate with excellent brittle crack propagation arresting properties.

[0007] Patent Document 4 proposes a steel plate having a metal structure consisting of a first phase of ferrite and a second phase of pearlite, in which the hardness of the second phase is 260 HV or less, and which has a carbon content of 0.04 to 0.06 mass %, as a thick steel plate having excellent uniform elongation. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2016-125077 A [Patent Document 2] International Publication No. 2018 / 030171 [Patent Document 3] International Publication No. 2016 / 143345 [Patent Document 4] JP 2018-193605 A [Non-patent literature]

[0009] [Non-Patent Document 1] Manabu Takahashi: "100 Years of Sheet Technology - Sheet Steel and Manufacturing Technology that Developed Alongside the Automobile Industry", Tetsu-to-Hagane, Vol. 100, 2014, No. 1, p82-93 Summary of the Invention [Problem to be solved by the invention]

[0010] In order to promote high efficiency as a countermeasure to the declining population and rising energy costs, ships, floating bodies, and marine structures are becoming larger, and the steel plates that make them up are also becoming thicker. Since the ductility of steel plates increases with increasing plate thickness, in structures that use thick steel materials, the effect of improving ductility in reducing damage during collisions is saturated, and in order to further reduce damage during collisions, it is necessary to consider methods other than improving ductility. In this regard, in order to reduce damage caused by collisions of structures, it is effective to improve the bendability of steel plates to suppress the occurrence of cracks on the surface of strain concentration areas during collisions.

[0011] Therefore, an object of the present invention is to provide a steel sheet having improved bendability through a novel configuration, and a manufacturing method thereof. [Means for solving the problem]

[0012] The present inventors have investigated the microstructural control of steel sheets necessary for improving bendability. As a result, the present inventors have found that the bendability of a steel sheet can be significantly improved by making the microstructure in the surface layer of a steel sheet having a predetermined chemical composition mainly comprise ferrite, which is a soft structure, and restricting hard structures such as martensite to a predetermined range, further making the texture of the ferrite homogenous, and further reducing the density of elongated inclusions contained in the surface layer, thereby completing the present invention.

[0013] The present invention which has achieved the above object is as follows. (1) Chemical composition, in mass%, C: 0.075-0.240%, Si: 1.25% or less, Mn: 0.50-2.00%, P:0.030% or less, S: 0.0100% or less, N: 0.0150% or less, O: 0.0030% or less, Al: 1.000% or less, Ti: 0 to 0.060%, Nb: 0 to 0.040%, V: 0 to 1.000%, Cu: 0-2.00%, Ni: 0-5.00%, Cr: 0-2.00%, Mo: 0-1.00%, W: 0 to 1.00%, B: 0~0.0050%, Sn: 0~1.000%, Sb: 0 to 0.200%, The sum of one or more of Ca, Mg, Zr, La, Ce, Te, Hf and REM: 0.0008 to 0.0050%, and The balance is composed of Fe and impurities. Satisfying the following formulas (1), (2) and (3), The microstructure in the depth region from the surface to 300 μm in the depth direction is, in terms of volume fraction, Ferrite: 90% or more, and Total of martensite, bainite, bainitic ferrite and retained austenite: 0-3% The density of the elongated inclusions in the depth region is 1.0×105 pieces / m2 or less, A steel sheet, characterized in that a peak intensity at a 45-degree cross section in a three-dimensional crystal orientation distribution function of the BCC phase in the depth region is 5.0 or less. 2.44×10-2×(1.00-0.20[Si]+7.00[Nb])×(1.00-10[B]0.5)×(117+17[Si]+11[Si]2-33[M n]+4[Mn]2+79[Al]+59[Al]2-26[Ni]-12[Cr])×(1+1.3[Si]+0.8[Mo]0.5+35[Nb])-1≧1.00 ...Equation (1) 0≦64+41[Si]-34[Mn]+95[Al]2+74[Al]-14[Cr]-43[Ni]≦100...Formula (2) 0.02≦[Mn]×[S]×(7.50[Ca]+12.50[Mg]+3.30[Zr]+2.16[La]+2.14[Ce]+2.34[Te]+1.68[Hf]+1.94[REM])-1≦1.00...Equation (3) Here, [Si], [Nb], [B], [Mn], [Al], [Ni], [Cr], [Mo], [S], [Ca], [Mg], [Zr], [La], [Ce], [Te], [Hf] and [REM] are the contents [mass%] of each element, and are 0 when the element is not contained. (2) The chemical composition is, in mass%, Ti: 0.008~0.030% Nb: 0.005 to 0.025% V: 0.050~0.600% Cu: 0.05-2.00%, Ni: 0.15-3.00%, Cr:0.10~2.00% or less, Mo: 0.03 to 1.00% or less W: 0.03~0.50% or less, B: 0.0005~0.0025% or less, Sn: 0.015 to 1.000% or less, and Sb:0.005~0.200% or less The steel sheet according to the above (1), characterized in that it contains one or more selected from the following: (3) The microstructure at a depth of 5.0 mm from the surface in the depth direction is, in terms of volume fraction, Ferrite: 80% or more, Perlite: 5% or more, and The sum of martensite, bainite, bainitic ferrite and retained austenite: 0 to 3%. The ferrite at the depth has an average crystal grain size of 8.0 to 20.0 μm, an average aspect ratio of 1.6 or less, and an intragranular orientation difference of 1.0 degree or less, The steel sheet according to (1) or (2) above, characterized in that the pearlite at the depth position has an average lamellar spacing of 0.30 μm or more. (4) The steel sheet according to any one of the above (1) to (3), characterized in that the density of spikes having a depth of 5.0 μm or more on the surface is 1.0 × 10 3 spikes / m or less. (5) a casting step of casting a slab having the chemical composition described in (1) or (2) above, and then cooling the slab at an average cooling rate of 100°C / h or more in a temperature range of 900 to 550°C until the surface temperature of the slab reaches the temperature range of 900 to 550°C; A heating step of heating the slab, the maximum heating temperature of the slab being 1050 to 1250° C. and satisfying the following formula (4): a hot rolling process in which the slab is subjected to high-pressure water descaling and then hot rolling, in which the end temperature of the high-pressure water descaling is 1000°C or higher, the time between each rolling pass at 1000°C or lower satisfies the following formula (5), and the end temperature of the hot rolling is 900°C or higher; A cooling process in which water cooling of the obtained steel plate is started within 10 seconds after the completion of the hot rolling process, and the surface temperature of the steel plate is cooled to a temperature range of 820°C or less. A method for producing a steel sheet, comprising:

number

number

[0014] According to the present invention, it is possible to provide a steel plate having improved bendability and a manufacturing method thereof. Therefore, such a steel plate can suppress strain concentration near the surface layer and suppress crack generation on the surface of the strain concentrated portion, thereby significantly suppressing the generation of holes during a collision. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, the steel sheet according to the embodiment of the present invention and the manufacturing method thereof will be described in more detail. However, these descriptions are intended to exemplify preferred forms of the present invention and are not intended to limit the present invention to specific embodiments.

[0016] [Chemical composition] Hereinafter, the chemical composition of the steel sheet according to the embodiment of the present invention will be described. In the following description, the unit of content of each element, "%", means "mass%" unless otherwise specified.

[0017] [C:0.075~0.240%] C is an element that contributes to improving strength. To fully obtain this effect, the C content is set to 0.075% or more. From the viewpoint of increasing strength, the C content is preferably 0.090% or more, and more preferably 0.110% or more or 0.130% or more. On the other hand, if C is excessively contained, sufficient bendability and / or uniform elongation may not be obtained with high strength. Therefore, the C content is set to 0.240% or less. From the viewpoint of increasing bendability, the C content is preferably 0.220% or less, and more preferably 0.200% or less or 0.180% or less.

[0018] [Si:1.25% or less] Si is a deoxidizing element and also contributes to improving strength. The Si content may be 0%, but in order to obtain a sufficient deoxidizing effect by Si, the Si content is preferably 0.01% or more. In order to increase strength, the Si content is preferably 0.05% or more, and more preferably 0.10% or more or 0.30% or more. On the other hand, if the Si content is high, sufficient bendability and / or uniform elongation may not be obtained due to high strength. From this viewpoint, the Si content is set to 1.25% or less. Also, Si is an element that impairs the toughness of the steel plate, and from this viewpoint, the Si content is preferably 1.00% or less or 0.80% or less, and more preferably 0.50% or less.

[0019] [Mn: 0.50~2.00%] Mn is an element that contributes to improving strength, and in order to fully obtain this effect, 0.50% or more is added. From the viewpoint of increasing strength, the Mn content is preferably 0.70% or more, and more preferably 1.00% or more or 1.20% or more. On the other hand, if Mn is excessively contained, sufficient bendability and / or uniform elongation may not be obtained along with high strength. From this viewpoint, the amount of Mn added is limited to 2.00% or less. Furthermore, Mn is an element that impairs weldability and toughness of welded parts, and from this viewpoint, the Mn content is preferably 1.85% or less, and more preferably 1.70% or less or 1.50% or less.

[0020] [P:0.030% or less] P is an element that is inevitably contained in general steelmaking methods, and limiting it to less than 0.001% places a large burden on the smelting process and is economically undesirable, so the P content is preferably 0.001% or more. On the other hand, P is an element that impairs toughness, and from this viewpoint, the P content is limited to 0.030% or less. Furthermore, P is an element that impairs weldability and the toughness of welded parts, and from this viewpoint, the P content is preferably 0.020% or less, and more preferably 0.010% or less.

[0021] [S:0.0100% or less] S is an element that is inevitably contained in general steelmaking methods, and since limiting the S content to less than 0.0003% imposes a large load on the smelting process and is economically undesirable, the S content is preferably 0.0003% or more. On the other hand, S is an element that forms coarse sulfides that impair toughness, and forms elongated inclusions that reduce the bendability of steel sheets. For this reason, the S content is limited to 0.0100% or less. In addition, S is an element that impairs weldability and the toughness of welds, and from this perspective, the S content is preferably 0.0060% or less, and more preferably 0.0045% or less.

[0022] [N:0.0150% or less] N is an element that is inevitably contained in a general steelmaking process. If a large amount of N is contained, coarse nitrides are formed, which impairs the toughness of the steel plate, so the N content is limited to 0.0150% or less. N is also an element that impairs the toughness of a welded portion, and from this viewpoint, the N content is preferably 0.0100% or less, and more preferably 0.0060% or less. There is no particular lower limit for the N content, but excessive reduction places a large load on the smelting process and is economically undesirable, so the N content is preferably 0.0003% or more, and more preferably 0.0015% or more.

[0023] [O:0.0030% or less] O is an element that is inevitably contained in a general steelmaking process. If a large amount of O is contained, coarse oxides are formed, which impairs the toughness of the steel sheet, so the O content is limited to 0.0030% or less. O is also an element that impairs the toughness of a welded portion, and from this viewpoint, the O content is preferably 0.0020% or less, and more preferably 0.0010% or less. There is no particular lower limit for the O content, but since limiting it to less than 0.0002% places a large load on the smelting process and is economically undesirable, it is preferable to set it to 0.0002% or more.

[0024] [Al: 1.000% or less] Al is a deoxidizing element. The Al content may be 0%, but in order to obtain this effect, it is preferable to add 0.005% or more, and more preferably 0.010% or more. On the other hand, Al is an element that impairs toughness, and the Al content is limited to 1.000% or less. In addition, since Al impairs weldability and the toughness of the welded portion, the Al content is preferably 0.800% or less, and more preferably 0.500% or less or 0.200% or less.

[0025] [Ca, Mg, Zr, La, Ce, Te, Hf and REM: 0.0008~0.0050%] Ca, Mg, Zr, La, Ce, Te, Hf and REM are elements that refine sulfides and improve the deformability of steel sheets. In order to fully obtain this effect, the total content of Ca, Mg, Zr, La, Ce, Te, Hf and REM is 0.0008% or more, and may be, for example, 0.0010% or more or 0.0012% or more. On the other hand, if these elements are contained excessively, the effect is saturated, and therefore, the inclusion of Ca, Mg, Zr, La, Ce, Te, Hf and REM in the steel sheet more than necessary leads to an increase in manufacturing costs. In addition, these elements may combine with S in the steel to form elongated inclusions, which may reduce the bendability of the steel sheet. Therefore, the total content of Ca, Mg, Zr, La, Ce, Te, Hf and REM is limited to 0.0050% or less, preferably 0.0035% or less or 0.0030% or less, and more preferably 0.0015% or less. Here, REM is a general term for the lanthanoid group (Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb and Lu) excluding Sc, Y, La and Ce, and the total content of these 15 elements is the REM content.

[0026] The basic chemical composition of the steel sheet according to the embodiment of the present invention is as described above. Furthermore, the steel sheet may contain one or more of the following optional elements as necessary. The steel sheet may contain one or more selected from the group consisting of Ti: 0-0.060%, Nb: 0-0.040%, V: 0-1.000%, and Cu: 0-2.00%. The steel sheet may also contain one or more selected from the group consisting of Ni: 0-5.00%, Cr: 0-2.00%, Mo: 0-1.00%, and W: 0-1.00%. The steel sheet may also contain B: 0-0.0050%. The steel sheet may also contain one or two selected from the group consisting of Sn: 0-1.000% and Sb: 0-0.200%. These optional elements will be described in detail below.

[0027] [Ti: 0~0.060%] Ti is an element that contributes to improving strength. The Ti content may be 0%, but when it is contained, it may be 0.001% or more or 0.003% or more. From the viewpoint of increasing strength, the Ti content is preferably 0.008% or more, and more preferably 0.010% or more. On the other hand, if Ti is contained excessively, coarse Ti carbonitrides are generated, and there is a concern that the toughness of the steel plate and welded parts may be significantly deteriorated. From this viewpoint, the Ti content is preferably limited to 0.060% or less, and more preferably 0.030% or less or 0.020% or less.

[0028] [Nb: 0~0.040%] Nb is an element that contributes to improving strength, and may be contained in an amount of 0.040% or less. If the Nb content exceeds 0.040%, precipitation strengthening is excessively expressed, and there is a concern that bendability and / or uniform elongation may be impaired. The Nb content may be 0.025% or less, 0.015% or less, or 0.010% or less. On the other hand, the Nb content may be 0%, but from the viewpoint of increasing strength, the Nb content is preferably 0.001% or more, and more preferably 0.005% or more.

[0029] [V:0~1.000%] V is an element that contributes to improving strength, and may be contained in an amount of 1.000% or less. If the V content exceeds 1.000%, precipitation strengthening is excessively expressed, and there is a concern that bendability and / or uniform elongation may be impaired. The V content is preferably 0.600% or less or 0.300% or less. On the other hand, the V content may be 0%, but from the viewpoint of increasing strength, the V content is preferably 0.010% or more, and more preferably 0.050% or more.

[0030] [Cu:0~2.00%] Cu is an element that contributes to improving strength, and may be contained in an amount of 2.00% or less. If the Cu content exceeds 2.00%, precipitation strengthening is excessively expressed, and there is a concern that bendability and / or uniform elongation may be impaired. The Cu content is more preferably 1.00% or less or 0.50% or less. On the other hand, the Cu content may be 0%, but from the viewpoint of increasing strength, the Cu content is preferably 0.01% or more, and more preferably 0.05% or more.

[0031] [Ni:0~5.00%] Ni is an element that contributes to improving strength and / or heat resistance. The Ni content may be 0%, but in order to obtain this effect, it is preferably 0.01% or more or 0.10% or more, and more preferably 0.15% or more. On the other hand, if the Ni content exceeds 5.00%, the hardenability increases excessively, and the bendability and / or uniform elongation are impaired. From this viewpoint, the Ni content is limited to 5.00% or less, preferably 3.00% or less or 2.30% or less, and more preferably 1.50% or less or 1.00% or less.

[0032] [Cr:0~2.00%] Cr is an element that contributes to improving strength, and may be contained at 2.00% or less. The Cr content may be 0%, but from the viewpoint of increasing strength, the Cr content is preferably 0.01% or more or 0.10% or more. On the other hand, excessive Cr content may increase alloy costs and reduce toughness. Therefore, the Cr content is limited to 2.00% or less, and preferably 1.00% or less. Cr is an element that impairs weldability and the toughness of the welded portion, and from this viewpoint, the Cr content is more preferably 0.60% or less.

[0033] [Mo:0~1.00%] Mo is an element that contributes to improving strength. The Mo content may be 0%, but from the viewpoint of increasing strength, the Mo content is preferably 0.01% or more or 0.03% or more, and more preferably 0.08% or more. On the other hand, even if Mo is contained excessively, the effect becomes saturated, and there is a risk of causing an increase in manufacturing costs. Therefore, the Mo content is limited to 1.00% or less, preferably 0.50% or less, and more preferably 0.30% or less.

[0034] [W:0~1.00%] W is an element that contributes to improving strength. The W content may be 0%, but from the viewpoint of increasing strength, the W content is preferably 0.01% or more or 0.03% or more, and more preferably 0.08% or more. On the other hand, if W is contained excessively, the hardenability increases excessively, and the bendability and / or uniform elongation are impaired. From this viewpoint, the W content is limited to 1.00% or less, preferably 0.50% or less, and more preferably 0.30% or less.

[0035] [B: 0~0.0050%] B is an element that contributes to improving strength, and may be contained at 0.0050% or less. The content of B may be 0%, but from the viewpoint of increasing strength, the content of B is preferably 0.0001% or more or 0.0005% or more, and more preferably 0.0010% or more. On the other hand, if B is contained excessively, there is a concern that the weldability and toughness of the welded part may be impaired. From this viewpoint, the content of B is limited to 0.0050% or less, preferably 0.0025% or less, and more preferably 0.0015% or less.

[0036] [Sn:0~1.000%] Sn is an element that contributes to improving strength, and may be contained at 1.000% or less. The Sn content may be 0%, but from the viewpoint of increasing strength, the Sn content is preferably 0.005% or more or 0.015% or more, and more preferably 0.030% or more. On the other hand, if Sn is contained excessively, there is a concern that the weldability and toughness of the welded part may be impaired. From this viewpoint, the Sn content is limited to 1.000% or less, preferably 0.300% or less, and more preferably 0.100% or less.

[0037] [Sb: 0~0.200%] Sb is an element that contributes to improving strength, and may be contained in an amount of 0.200% or less. The Sb content may be 0%, but from the viewpoint of increasing strength, the Sb content is preferably 0.001% or more or 0.005% or more. On the other hand, if Sb is contained in an excessive amount, there is a concern that the hardenability will be excessively improved and the bendability and / or uniform elongation will be deteriorated. From this viewpoint, the Sb content is limited to 0.200% or less, preferably 0.080% or less, and more preferably 0.030% or less.

[0038] In the steel sheet according to the embodiment of the present invention, the balance other than the above elements consists of Fe and impurities. The impurities are components that are mixed in due to various factors in the manufacturing process, including raw materials such as ores and scraps, when the steel sheet is industrially manufactured.

[0039] The chemical composition of steel sheets can be measured by a general analytical method. For example, the chemical composition of steel sheets can be measured using inductively coupled plasma-atomic emission spectrometry (ICP-AES). C and S are measured using the combustion-infrared absorption method.

[0040] [Control of phase transformation by chemical composition] In order to obtain the steel sheet according to the embodiment of the present invention, it is necessary to form a predetermined microstructure by appropriately advancing the phase transformation. In order to control the behavior of the phase transformation, it is necessary to satisfy the following formula (1) in order to appropriately control the chemical composition of the steel sheet. 2.44×10-2×(1.00-0.20[Si]+7.00[Nb])×(1.00-10[B]0.5)×(117+17[Si]+11[Si]2-33 [Mn]+4[Mn]2+79[Al]+59[Al]2+26[Ni]-12[Cr])×(1+1.3[Si]+12[Mo]+35[Nb])-1≧1.00 ...Equation (1) Here, [Si], [Nb], [B], [Mn], [Al], [Ni], [Cr] and [Mo] are the contents [mass%] of each element, and are 0 when the element is not contained.

[0041] Formula (1) shows the range of chemical composition that allows the ferrite transformation to proceed sufficiently while not excessively promoting or inhibiting the transformation of other hard structures. To explain in more detail, equation (1) takes into account the driving force of ferrite transformation, the nucleation rate of ferrite transformation, and the interface mobility (degree of transformation progress). Specifically, the term 2.44 × 10-2 × (1.00-0.20[Si] + 7.00[Nb]) × (1.00-10[B]0.5) in equation (1) corresponds to the nucleation rate of ferrite transformation, the term (117 + 17[Si] + 11[Si]2-33[Mn] + 4[Mn]2 + 79[Al] + 59[Al]2-26[Ni]-12[Cr]) corresponds to the driving force of ferrite transformation, and (1 + 1.3[Si] + 0.8[Mo]0.5 + 35[Nb])-1 corresponds to the interface mobility. The larger the value of the left side of formula (1), the higher the temperature at which the ferrite transformation can proceed, and by proceeding with the ferrite transformation at a high temperature, the subsequent transformation of the hard structure can also proceed at a high temperature, making it possible to relatively easily form the desired structure fraction and structure morphology. From this viewpoint, the value of the left side of formula (1) is set to 1.00 or more, preferably 1.15 or more, and more preferably 1.30 or more.

[0042] [0≦64+41[Si]-34[Mn]+95[Al]2+74[Al]-14[Cr]-43[Ni]≦100] In the steel sheet according to the embodiment of the present invention, the microstructure of the surface layer, more specifically, the microstructure of the surface layer corresponding to a depth region from the surface of the steel sheet to a depth direction of 300 μm, is composed mainly of ferrite, and preferably, the microstructure inside the surface layer is also composed mainly of ferrite. Therefore, in order to generate ferrite sufficiently and appropriately, it is necessary to optimize the Ar3 point, which corresponds to the temperature at which the transformation from austenite to ferrite starts, and in this regard, the chemical composition of the steel sheet is controlled to satisfy the following formula (2). 0≦64+41[Si]-34[Mn]+95[Al]2+74[Al]-14[Cr]-43[Ni]≦100...Formula (2) Here, [Si], [Mn], [Al], [Cr] and [Ni] are the contents [mass %] of each element, and are 0 when the element is not contained.

[0043] If the value of formula (2) is less than 0, the Ar3 point becomes too low, and the desired ferrite fraction cannot be obtained due to the generation of other hard structures. On the other hand, if the value of formula (2) is more than 100, the ferrite becomes coarse and the strength decreases. The value of formula (2) may be, for example, 5 or more, 10 or more, 15 or more, or 20 or more. Similarly, the value of formula (2) may be, for example, 90 or less, 80 or less, or 70 or less.

[0044] [Control of elongated inclusions through chemical composition] In the steel plate according to the embodiment of the present invention, the chemical composition of the steel plate needs to satisfy the following formula (3), which makes it possible to reduce the density of elongated inclusions contained in the surface layer portion and significantly improve the bendability of the steel plate. 0.02≦[Mn]×[S]×(7.50[Ca]+12.50[Mg]+3.30[Zr]+2.16[La]+2.14[Ce]+2.34[Te]+1.68[Hf]+1.94[REM])-1≦1.00...Equation (3) Here, [Mn], [S], [Ca], [Mg], [Zr], [La], [Ce], [Te], [Hf] and [REM] are the contents [mass%] of each element, and are 0 when the element is not contained.

[0045] More specifically, these elements combine with S in the steel to form inclusions, which are then rolled in the manufacturing process to form elongated inclusions that are elongated in the rolling direction. Since the elongated inclusions elongate along the surface direction of the steel sheet, if a relatively large number of such elongated inclusions are present in the surface layer of the steel sheet, the bendability of the steel sheet will decrease. In relation to this, the inventors have found that by controlling the chemical composition of the steel sheet to satisfy formula (3), the density of the elongated inclusions formed in the surface layer of the steel sheet can be reduced, and therefore the bendability of the steel sheet can be improved. If the value of formula (3) is too large, coarse Mn-based inclusions are formed. On the other hand, if the value of formula (3) is too small, the density of inclusions containing added elements such as Ca increases, and coarse inclusions are instead formed near the surface layer. In order to reduce inclusions in the surface layer and improve bendability, the value of formula (3) is preferably 0.05 or more and 0.90 or less, and more preferably 0.10 or more and 0.80 or less.

[0046] [Microstructure of the steel plate surface layer] [Ferrite: 90% or more] Since ferrite is a soft structure, it is possible to improve the bendability of the steel sheet by including the ferrite as the main structure constituting the surface layer portion of the steel sheet, that is, the depth region from the surface of the steel sheet to 300 μm in the depth direction. In an embodiment of the present invention, in order to achieve the desired bendability, the volume fraction of ferrite in the surface layer portion is controlled to 90% or more. From the viewpoint of improving the bendability of the steel sheet, the higher the volume fraction of ferrite in the surface layer portion, the more preferable it is, and it may be, for example, 92% or more, 94% or more, more than 95%, 96% or more, 97% or more, or 98% or more. The upper limit is not particularly limited, but for example, the volume fraction of ferrite in the surface layer portion may be 100% or 99% or less.

[0047] [Total of martensite, bainite, bainitic ferrite and retained austenite: 0~3%] In the steel sheet according to the embodiment of the present invention, the surface layer portion may contain one or more of martensite (including tempered martensite), bainite, bainitic ferrite, and residual austenite in addition to ferrite. However, if the surface layer portion contains a relatively large amount of these hard structures, sufficient bendability may not be obtained. Therefore, the total of martensite, bainite, bainitic ferrite, and residual austenite in the steel sheet surface layer portion is set to 3% or less in volume fraction. From the viewpoint of improving the bendability of the steel sheet, the total of martensite, bainite, bainitic ferrite, and residual austenite in the steel sheet surface layer portion is preferably set to 2% or less in volume fraction, and more preferably set to 1% or less. The lower limit is not particularly limited, but for example, the total of martensite, bainite, bainitic ferrite, and residual austenite in the steel sheet surface layer portion may be 0% or 0.5% or more.

[0048] [Remaining tissue] In the steel sheet according to the embodiment of the present invention, the surface layer portion may be composed of only ferrite, or may be composed of only ferrite and one or more of martensite, bainite, bainitic ferrite, and retained austenite, and therefore the remaining structure may be 0% in volume fraction. When a remaining structure is present in the steel sheet surface layer portion, the remaining structure is pearlite. The remaining structure in the steel sheet surface layer portion may be 10% or less, 8% or less, 7% or less, 5% or less, 3% or less, or 1% or less in volume fraction.

[0049] [The peak intensity at a 45-degree cross section in the three-dimensional crystal orientation distribution function of the BCC phase is 5.0 or less] In the steel sheet according to the embodiment of the present invention, the development of the texture of the surface layer portion mainly composed of ferrite is suppressed, and the texture is made more homogeneous, thereby improving the bendability of the steel sheet. More specifically, the bendability of the steel sheet can be improved by controlling the peak intensity at a 45-degree cross section in the three-dimensional crystallite orientation distribution function (hereinafter also abbreviated as ODF) of the BCC phase in the surface layer portion of the steel sheet to 5.0 or less. If the peak intensity at a 45-degree cross section in the ODF of the BCC phase in the surface layer portion of the steel sheet exceeds 5.0, the texture of the surface layer portion develops, and the desired bendability cannot be achieved. From the viewpoint of improving the bendability of the steel sheet, the lower the peak intensity at a 45-degree cross section in the ODF of the BCC phase in the surface layer portion of the steel sheet, the more preferable it is, and it may be, for example, 4.0 or less, 3.0 or less, 2.5 or less, or 2.0 or less. The lower limit is not particularly limited, but for example, the peak intensity at a 45-degree cross section in the ODF of the BCC phase in the surface layer portion of the steel sheet may be 0.5 or more, or 1.0 or more.

[0050] [Density of elongated inclusions: 1.0×105 pieces / m2 or less] Elongated inclusions are the starting points for the generation of coarse voids in the microstructure, and therefore, if a relatively large number of such elongated inclusions are present in the surface layer, they will reduce the bendability of the steel sheet. For this reason, in the steel sheet according to the embodiment of the present invention, the density of elongated inclusions in the surface layer, i.e., in the depth region from the surface of the steel sheet to 300 μm in the depth direction, is limited to 1.0×105 pieces / m2 or less to suppress the generation of coarse voids, thereby improving the bendability of the steel sheet. In the present invention, an elongated inclusion refers to any inclusion elongated in one direction (e.g., the rolling direction), having an aspect ratio defined by the major axis / minor axis of 5.0 or more, and an average of the major axis and minor axis of 5.0 μm or more. From the viewpoint of suppressing the generation of coarse voids, the density of such elongated inclusions is preferably as small as possible, and may be, for example, 0.8×105 pieces / m2 or less, 0.5×105 pieces / m2 or less, 0.3×105 pieces / m2 or less, or 0.1×105 pieces / m2 or less. The lower limit is not particularly limited, but the density of the elongated inclusions may be, for example, 0.01×105 pieces / m2 or more, or 0.02×105 pieces / m2 or more. Specific examples of the elongated inclusions are not particularly limited, but for example, the elongated inclusions may be sulfides containing at least one of Ca, Mg, and REM and S, and in particular MnS and / or MnS in which part of Mn is replaced with Ca, or may be composite inclusions in which these sulfides are mixed with oxides of Ti, Al, etc.

[0051] [Microstructure inside steel plate] As described above, the present invention aims to provide a steel sheet with improved bendability, and the objective is achieved by controlling the microstructure in the surface layer of the steel sheet having the above-mentioned predetermined chemical composition to contain ferrite: 90% or more, and the total of martensite, bainite, bainitic ferrite and retained austenite: 0 to 3% in volume fraction, and further controlling the peak intensity at 45-degree cross section in ODF of the BCC phase in the surface layer to 5.0 or less. Therefore, the microstructure in the steel sheet interior may be, for example, the same as or different from the microstructure in the steel sheet surface layer, and may be appropriately selected by a person skilled in the art in consideration of the properties of the steel sheet other than bendability, and therefore it is clear that it is not an essential technical feature for achieving the objective of the present invention. Below, a preferred microstructure in the steel sheet interior according to an embodiment of the present invention will be described in detail, but these descriptions are intended to be merely examples of microstructures in the steel sheet interior suitable for improving the uniform elongation of the steel sheet, and are not intended to limit the present invention to a steel sheet having an interior having such a specific microstructure.

[0052] [Ferrite: 80% or more] According to a preferred embodiment of the present invention, the microstructure inside the steel sheet is also composed of a structure mainly made of ferrite, similar to the surface layer of the steel sheet. By forming the microstructure inside the steel sheet mainly made of ferrite, the uniform elongation of the steel sheet can be improved. Therefore, by combining the bendability achieved mainly by the microstructure in the surface layer of the steel sheet and the uniform elongation achieved mainly by the microstructure inside the steel sheet, it is possible to significantly suppress the occurrence of cracks on the surface of the strain concentration part during collision. More specifically, in a preferred embodiment of the present invention, the microstructure at a depth position of 5.0 mm from the surface of the steel sheet in the depth direction is controlled to contain 80% or more of ferrite in volume fraction. From the viewpoint of improving the uniform elongation of the steel sheet, the higher the volume fraction of ferrite inside the steel sheet, the more preferable it is, and it may be, for example, 82% or more, 85% or more, 88% or more, or 90% or more. The upper limit is not particularly limited, but for example, the volume fraction of ferrite inside the steel sheet may be 95% or less, 94% or less, or 92% or less.

[0053] [Perlite: 5% or more] According to a preferred embodiment of the present invention, the microstructure inside the steel sheet contains 5% or more by volume of pearlite with an average lamellar spacing appropriately controlled, as will be described in detail later. When the microstructure inside the steel sheet, more specifically at a depth position of 5.0 mm from the surface of the steel sheet, contains 5% or more by volume of such pearlite in addition to ferrite, it becomes possible to further improve the uniform elongation of the steel sheet. The volume fraction of the pearlite may be, for example, 6% or more or 8% or more. Although there is no particular upper limit, the volume fraction of pearlite inside the steel sheet may be 20% or less, 18% or less, 15% or less, 12% or less, or 10% or less.

[0054] [Total of martensite, bainite, bainitic ferrite and retained austenite: 0~3%] According to a preferred embodiment of the present invention, the microstructure inside the steel sheet may be composed of only ferrite and pearlite, and therefore the remaining structure may be 0% in volume fraction. When the remaining structure exists inside the steel sheet, the remaining structure is one or more of martensite (including tempered martensite), bainite, bainitic ferrite, and retained austenite. However, if these hard structures are contained relatively in large amounts inside, sufficient uniform elongation may not be obtained. Therefore, the total of martensite, bainite, bainitic ferrite, and retained austenite inside the steel sheet is set to 3% or less in volume fraction. From the viewpoint of improving the uniform elongation of the steel sheet, the total of martensite, bainite, bainitic ferrite, and retained austenite inside the steel sheet is preferably set to 2% or less in volume fraction, and more preferably set to 1% or less. The lower limit is not particularly limited, but for example, the total of martensite, bainite, bainitic ferrite, and retained austenite inside the steel sheet may be 0% or 0.5% or more.

[0055] [Ferrite inside the steel sheet: average grain size of 8.0 to 20.0 μm, average aspect ratio of 1.6 or less, and intragranular misorientation of 1.0 degree or less] According to a preferred embodiment of the present invention, ferrite in the microstructure inside the steel sheet, more specifically, ferrite in the microstructure at a depth position of 5.0 mm in the depth direction from the surface of the steel sheet, is controlled to have an average crystal grain size of 8.0 to 20.0 μm, an average aspect ratio of 1.6 or less, and an intragranular orientation difference of 1.0 degree or less. By controlling the ferrite in the microstructure inside the steel sheet to satisfy these characteristics, the microstructure inside the steel sheet can be mainly composed of ferrite that has an appropriate grain size, isotropic, and has fewer dislocations, and therefore the uniform elongation of the steel sheet can be significantly improved.

[0056] For example, the average grain size of ferrite inside the steel sheet may be 10.0 μm or more, 12.0 μm or more, or 14.0 μm or more, and / or 18.0 μm or less, 16.0 μm or less, or 14.0 μm or less. From the viewpoint of improving the uniform elongation of the steel sheet, it is preferable that the ferrite inside the steel sheet is more isotropic. Therefore, it is preferable that the average aspect ratio of ferrite inside the steel sheet is, for example, 1.5 or less, 1.4 or less, or 1.3 or less. Although the lower limit is not particularly limited, the average aspect ratio of ferrite inside the steel sheet may be, for example, 1.0 or more or 1.1 or more. From the viewpoint of improving the uniform elongation of the steel sheet, it is preferable to reduce the dislocations contained in the ferrite grains. In this regard, by controlling the intragranular orientation difference of ferrite to 1.0 degree or less, a ferrite structure with fewer dislocations can be realized, and therefore the uniform elongation of the steel sheet can be significantly improved. From the viewpoint of improving the uniform elongation of the steel sheet, the smaller the misorientation of ferrite grains in the steel sheet, the more preferable, and it may be, for example, 0.8 degrees or less. Although there is no particular lower limit, for example, the misorientation of ferrite grains in the steel sheet may be 0 degrees or more, 0.1 degrees or more, or 0.2 degrees or more.

[0057] [Average lamellar spacing of pearlite inside steel sheet: 0.30 μm or more] According to a preferred embodiment of the present invention, the pearlite in the microstructure inside the steel sheet, more specifically, the pearlite in the microstructure at a depth position of 5.0 mm from the surface of the steel sheet in the depth direction, is controlled to have an average lamellar spacing of 0.30 μm or more. By increasing the lamellar spacing of the pearlite inside the steel sheet, the yield ratio can be further reduced, thereby improving the uniform elongation. According to a preferred embodiment of the present invention, such an effect is particularly remarkable when the lamellar spacing of the pearlite inside the steel sheet is 0.30 μm or more. From the viewpoint of improving the uniform elongation, the larger the average lamellar spacing of the pearlite inside the steel sheet, the more preferable it is, and it may be, for example, 0.35 μm or more or 0.40 μm or more. The upper limit is not particularly limited, but for example, the average lamellar spacing of the pearlite inside the steel sheet may be 1.00 μm or less, 0.80 μm or less, or 0.60 μm or less.

[0058] [Density of spikes with a depth of 5.0 μm or more on the steel plate surface: 1.0×103 spikes / m or less] According to a preferred embodiment of the present invention, the density of spikes having a depth of 5.0 μm or more on the steel sheet surface is controlled to 1.0×103 pieces / m or less. A spike is an area where scale has penetrated into the base steel, and by controlling the density of such irregularities having a penetration depth of 5.0 μm or more to 1.0×103 pieces / m or less, it is possible to significantly suppress or reduce strain concentration during bending deformation, and therefore it is possible to further improve bendability compared to a case where such control is not performed.

[0059] [Evaluation of microstructural features in the surface layer of steel sheets] The characteristics of the microstructure in the surface layer of the steel sheet are evaluated by detailed observation of the steel sheet. Specifically, a small piece including a depth region of 300 μm from the surface in the sheet thickness direction is cut out at a location of 1 / 2 the width of the steel sheet or processed steel sheet, and used as an observation sample. The volume fraction of the retained austenite is calculated by obtaining a diffraction peak of the fcc phase in the above depth region by X-ray diffraction. The observation and measurement of the volume fraction of each structure other than the retained austenite are performed using a field emission scanning electron microscope, and the cross section of the above depth region parallel to the rolling direction and perpendicular to the sheet surface is used as the observation surface, which is wet polished and polished with colloidal silica to make it a mirror surface, and then etched with nital (a mixture of ethanol and nitric acid) to make an observation sample. The above depth region is observed and evaluated at a magnification of 1000 to 3000 times. The volume fraction of materials other than retained austenite is evaluated by photographing the microstructure of a total area of ​​1.0 × 10-8 m2 or more using the above-mentioned electron microscope, determining the structure at 200 or more lattice points using the point counting method, and calculating the area fraction of each structure.

[0060] The peak intensity at a 45-degree cross section in the three-dimensional crystal orientation distribution function of the BCC phase in the surface layer of the steel sheet is measured by electron backscattered diffraction (EBSD). More specifically, a sample is first taken from the steel sheet so that the plate thickness cross section parallel to the rolling direction and perpendicular to the plate surface is the observation surface, and EBSD analysis is performed at a measurement interval of 1 μm in a depth region from the steel sheet surface to 300 μm in the plate thickness direction to obtain crystal orientation information of this depth region. The EBSD analysis is performed at an analysis speed of 50 to 300 points / second using an apparatus consisting of a thermal field emission scanning electron microscope (JEOL JSM-7001F) and an EBSD detector (TSL HIKARI detector). Next, from the crystal orientation information of this depth region, the three-dimensional crystal orientation distribution function (ODF) of this depth region is calculated using the software "OIM Analysis (registered trademark)" attached to the EBSD analysis device. The harmonic series expansion (spherical harmonic function method) is used to calculate the ODF. Finally, the peak intensity at the φ2=45 degree cross section in the Euler space is obtained in the ODF of the BCC phase.

[0061] The density of elongated inclusions in the surface layer of a steel sheet is determined by detailed observation of the steel sheet using an optical microscope or FE-SEM. Specifically, the observation surface is a surface parallel to the sheet surface at a depth of 300±30 μm from the surface in the sheet thickness direction at a location half the width of the steel sheet or processed steel sheet, and a small piece including this area is cut out and used as the observation sample. The observation surface is wet polished and polished with colloidal silica to make it a mirror surface, and the density of elongated inclusions is evaluated by observing an area of ​​5.0×10-5 m2 or more in total.

[0062] [Evaluation of microstructural features inside steel plate] The characteristics of the microstructure inside the steel sheet are evaluated by detailed observation of the steel sheet. Specifically, a small piece including a depth position of 5.0 mm from the surface of the steel sheet in the sheet thickness direction is cut out at a location of 1 / 2 the width of the steel sheet or processed steel sheet, and used as an observation sample. The volume fraction of the retained austenite is calculated by obtaining a diffraction peak of the fcc phase at the above-mentioned depth position by X-ray diffraction. The volume fraction of each structure other than the retained austenite, as well as the average crystal grain size and average aspect ratio of ferrite are observed and measured using a field emission scanning electron microscope, and a cross section including the above-mentioned depth position parallel to the rolling direction and perpendicular to the sheet surface is used as the observation surface, and the observation surface is wet polished and polished with colloidal silica to make it a mirror surface, and then etched with nital (a mixture of ethanol and nitric acid) to make an observation sample. The above-mentioned depth position is observed and evaluated at a magnification range of 1000 to 3000 times. The volume fraction of the non-retained austenite is evaluated by photographing the microstructure of a total area of ​​1.0×10-8 m2 or more centered at a depth of 5.0 mm from the steel plate surface in the plate thickness direction using the electron microscope, judging the structure at 200 or more lattice points using the point counting method, and calculating the area fraction of each structure. The average grain size of ferrite is calculated by drawing lines of 100 μm or more in the plate thickness direction, rolling direction, and 45 degrees between the plate thickness direction and rolling direction in the total area of ​​1.0×10-8 m2 or more centered at the depth position on the photograph observed with the electron microscope, and calculating the average grain size by the intercept method. Furthermore, the average aspect ratio of ferrite is calculated by calculating the aspect ratio, which is the ratio of the long axis to the short axis, for 10 or more ferrite grains randomly selected in the total area of ​​1.0×10-8 m2 or more from the photograph observed with the electron microscope, and taking the simple average of the aspect ratios as the average aspect ratio of ferrite.

[0063] The intragranular orientation misorientation of ferrite is determined as follows. Specifically, first, a sample is taken from a steel sheet so that the plate thickness cross section parallel to the rolling direction and perpendicular to the plate surface is the observation surface, and EBSD analysis is performed at measurement intervals of 1 μm on a rectangular region of 1000 μm in the rolling direction of the steel sheet and 100 μm in the normal direction to the rolling surface, centered at a depth position of 5.0 mm from the surface of the steel sheet in the plate thickness direction, to obtain crystal orientation information of this rectangular region. The EBSD analysis is performed at an analysis speed of 50 to 300 points / second using a device consisting of a thermal field emission scanning electron microscope (JSM-7001F manufactured by JEOL) and an EBSD detector (HIKARI detector manufactured by TSL). Next, the orientation misorientation (GAM value: Grain Average Misorientation) in the ferrite grains is calculated from the crystal orientation information of this rectangular region using the software "OIM Analysis (registered trademark)" attached to the EBSD analysis device.

[0064] The average lamellar spacing of pearlite is determined as follows. Specifically, first, a sample is taken from a steel sheet so that the plate thickness cross section parallel to the rolling direction and perpendicular to the plate surface is the observation surface. Next, the observation surface is mirror-polished and etched with a picral etchant, and then the structure is observed using a scanning electron microscope (SEM). The measurement area is a rectangular area (magnification is, for example, 5000 times) of 150 μm in the rolling direction of the steel sheet and 80 μm in the normal direction to the rolling surface, centered at a depth position of 5.0 mm from the steel sheet surface in the plate thickness direction, and 10 or more points where the cementite layer crosses perpendicularly to the paper surface of the structure photograph are selected. By measuring after etching with a picral etchant, information in the depth direction can be obtained, so that the points where the cementite layer crosses perpendicularly can be identified. By selecting and measuring 10 or more such points, the lamellar spacing S is obtained at each point, and the average of these is taken to obtain the average lamellar spacing. The method of measuring the lamellar spacing at each point is as follows. First, draw a straight line perpendicular to the cementite layer so as to cross 10 to 30 cementite layers, and define the length of the line as L. Also, define the number of cementite layers crossed by the line as N. In this case, the lamellar spacing S at that point is calculated by S = L / N.

[0065] [Spike density measurement] The spike density on the steel sheet surface is determined by detailed observation of the steel sheet using an optical microscope or FE-SEM. Specifically, a sample is taken from the steel sheet so that the observation surface is the sheet thickness cross section parallel to the rolling direction and perpendicular to the sheet surface, and the observation surface is wet polished and polished with colloidal silica to make it a mirror surface. The scale / base steel interface is observed over a total length of 5.0 x 10-3 m or more, and the number of spikes in which the scale has penetrated 5.0 μm or more in the sheet thickness direction from the scale / base steel interface is evaluated.

[0066] [Mechanical properties] [Tensile strength (TS), total elongation (EL), uniform elongation (UEL) and yield strength (YS)] According to the steel sheet having the above chemical composition and microstructure, a high tensile strength (TS), specifically a tensile strength of 380 MPa or more, can be achieved. The tensile strength is preferably 400 MPa or more, 420 MPa or more, 440 MPa or more, or 490 MPa or more. The upper limit is not particularly limited, but for example, the tensile strength may be 780 MPa or less, 700 MPa or less, or 650 MPa or less. Furthermore, according to the steel sheet according to the embodiment of the present invention, a total elongation (EL) of 20% or more can be achieved. The total elongation is preferably 22% or more, 25% or more, or 30% or more. The upper limit is not particularly limited, but for example, the total elongation may be 45% or less, 42% or less, or 40% or less. Furthermore, according to the steel sheet according to the embodiment of the present invention, a uniform elongation (UEL) of 15.0% or more can be achieved. The uniform elongation is preferably 16.0% or more, or 17.0% or more. The upper limit is not particularly limited, but for example, the uniform elongation may be 30.0% or less, 25.0% or less, or 22.0% or less. Moreover, according to the steel plate according to the embodiment of the present invention, a yield strength (YS) of 230 MPa or more can be achieved. The yield strength is preferably 250 MPa or more or 280 MPa or more. The upper limit is not particularly limited, but for example, the yield strength may be 550 MPa or less, 500 MPa or less, or 450 MPa or less. The tensile strength, total elongation, uniform elongation and yield strength are measured by taking a JIS 14A test piece from a direction (C direction) in which the longitudinal direction of the test piece is parallel to the rolling perpendicular direction of the steel plate, and performing a tensile test in accordance with JIS Z 2241:2011, and the yield strength means the 0.2% proof stress obtained by the above tensile test.

[0067] Plate Thickness The steel sheet according to the embodiment of the present invention generally has a thickness of 10 to 150 mm, although it is not particularly limited thereto. For example, the thickness may be 25 mm or more, 40 mm or more, or 50 mm or more, and / or 120 mm or less, or 100 mm or less.

[0068] [Steel plate manufacturing method] Next, a preferred method for manufacturing the steel plate according to the embodiment of the present invention will be described. The following description is intended to exemplify a characteristic method for manufacturing the steel plate according to the embodiment of the present invention, and is not intended to limit the steel plate to one manufactured by the manufacturing method described below.

[0069] The method for producing a steel sheet according to an embodiment of the present invention comprises: A casting process in which a slab having the chemical composition described above in relation to the steel plate is cast, and then the surface temperature of the slab is cooled in a temperature range of 900 to 550°C at an average cooling rate of 100°C / h or more; A heating step of heating the slab, the maximum heating temperature of the slab being 1050 to 1250° C. and satisfying the following formula (4): a hot rolling process in which the slab is subjected to high-pressure water descaling and then hot rolling, in which the end temperature of the high-pressure water descaling is 1000°C or higher, the time between each rolling pass at 1000°C or lower satisfies the following formula (5), and the end temperature of the hot rolling is 900°C or higher; A cooling process in which water cooling of the obtained steel plate is started within 10 seconds after the completion of the hot rolling process, the surface temperature of the steel plate is water-cooled to a temperature range of 820°C or less, and then cooled to 650°C. The present invention is characterized in that it includes:

number

number

[0070] [Casting process] First, a slab having the chemical composition described above in relation to the steel plate is manufactured, but the manufacturing method of the slab is not particularly limited, and for example, it can be manufactured by a continuous casting method or a blooming method. The manufactured slab is cooled at an average cooling rate of 100 ° C / h or more in the temperature range of 900 to 550 ° C. By cooling at such a relatively fast average cooling rate in the temperature range of 900 to 550 ° C, coarsening of the structure in the steel plate surface layer can be suppressed, and the microstructure of the present invention can be obtained in the surface layer through the subsequent process. If the average cooling rate in the temperature range of 900 to 550 ° C is less than 100 ° C / h, the peak strength at 45-degree cross section in the ODF of the BCC phase in the steel plate surface layer exceeds 5.0, and the texture of the surface layer develops, and the desired bendability may not be achieved. From this viewpoint, the average cooling rate in the temperature range of 900 to 550 ° C is 100 ° C / h or more, and preferably 120 ° C / h or more.

[0071] [Heating process] In order to hot roll the produced slab, a heat treatment is performed in which the maximum heating temperature is in the range of 1050 to 1250° C. and the following formula (4) is satisfied.

number

[0072] By carrying out such a heat treatment, the slab can be heated homogeneously and sufficiently, so that the development of the texture in the surface layer of the steel sheet can be suppressed, and the texture can be made more homogeneous. In addition, such a heat treatment is also effective in controlling the average grain size of ferrite in the steel sheet within a desired range. If the maximum heating temperature is below 1050°C or the value of formula (4) is excessively small, the development of the texture in the surface layer of the steel sheet cannot be sufficiently suppressed, the desired bendability cannot be obtained, and furthermore, the average grain size of ferrite in the steel sheet becomes small, and the desired uniform elongation cannot be obtained. Since the isotropy of the microstructure is improved by increasing the maximum heating temperature, the maximum heating temperature is preferably 1070°C or higher. On the other hand, if the maximum heating temperature exceeds 1250°C or the value of formula (4) is excessively large, the microstructure in the surface layer of the steel sheet becomes coarse, and recrystallization and / or phase transformation do not proceed appropriately in the subsequent hot rolling process and / or cooling process, resulting in deterioration of bendability. Furthermore, from the viewpoint of refining ferrite inside the steel sheet, the maximum heating temperature is preferably 1150° C. or less.

[0073] [Hot rolling process] Next, in the hot rolling process, the slab is subjected to high-pressure water descaling and then hot rolling, and the end temperature of the high-pressure water descaling is controlled to be 1000°C or higher, the time between each rolling pass at or below 1000°C satisfies the following formula (5), and the end temperature of the hot rolling is controlled to be 900°C or higher.

number

[0074] By completing the descaling before hot rolling at a relatively high temperature of 1000°C or more, preventing a decrease in the temperature of the slab surface, and then performing hot rolling with an appropriate interpass time, the recrystallization of the structure in the surface layer of the steel sheet can be sufficiently promoted, thereby randomizing the texture of the surface layer of the steel sheet to make it more homogeneous. As a result, in the surface layer of the finally obtained steel sheet, the peak intensity at a 45-degree cross section in the three-dimensional crystal orientation distribution function of the BCC phase can be controlled to 5.0 or less, and the desired bendability can be achieved. In addition, such a hot rolling process can also promote the recrystallization of the structure inside the steel sheet, and it becomes possible to reliably generate ferrite with an appropriate grain size, which is isotropic and has fewer dislocations in the microstructure inside the steel sheet.

[0075] If the end temperature of the high-pressure water descaling before hot rolling is less than 1000°C, the temperature of the surface layer of the steel sheet is excessively reduced, and the texture of the surface layer develops due to finish rolling, resulting in deterioration of bendability. For this reason, the end temperature of descaling is set to 1000°C or higher. In order to sufficiently suppress the development of the texture of the surface layer, it is preferable that the end temperature of descaling is 1010°C or higher. On the other hand, if the end temperature of descaling is excessively high, the texture of the surface layer is not affected, but the scale growth on the steel sheet surface may progress locally along the grain boundaries, resulting in the formation of spikes. Therefore, from the viewpoint of reducing the density of spikes with a depth of 5.0 μm or more on the steel sheet surface, it is preferable that the end temperature of descaling is 1050°C or lower.

[0076] After descaling, when the rolling conditions in the temperature range of 1000°C or less satisfy formula (5), the recrystallization of the surface layer progresses sufficiently, resulting in random crystal orientation. When the value of formula (5) is less than 1.0, the recrystallization does not progress sufficiently, and the texture of the surface layer is strengthened. From this viewpoint, the value of formula (5) is preferably 1.8 or more, and more preferably 2.5 or more. On the other hand, when the value of formula (5) exceeds 10.0, the structure inside the steel sheet becomes coarse and / or the anisotropy of the ferrite crystal grains increases, so the value of formula (5) is set to 10.0 or less, and preferably 8.0 or less.

[0077] If the hot rolling completion temperature is less than 900°C, the texture of the surface layer will be strengthened and the aspect ratio of ferrite inside the steel sheet will be large, so the hot rolling completion temperature is set to 900°C or higher, and preferably 915°C or higher. There is no particular upper limit for the hot rolling completion temperature, but if it exceeds 980°C, the average crystal grain size of ferrite inside the steel sheet will increase and / or the orientation difference within the ferrite grains will increase, so the hot rolling completion temperature is preferably 980°C or lower.

[0078] If the end temperature of the high-pressure water descaling before hot rolling is less than 1000°C, or the time between each rolling pass does not satisfy the following formula (5), and / or the end temperature of the hot rolling is less than 900°C, the recrystallization of the structure in the surface layer of the steel sheet cannot be sufficiently advanced, and the texture of the surface layer of the steel sheet cannot be randomized to make it more homogeneous. In addition, if the end temperature of the hot rolling is less than 900°C, the recrystallization of the structure inside the steel sheet does not sufficiently advance, so that the average crystal grain size, average aspect ratio, and / or intragranular orientation difference of ferrite inside the steel sheet increases, and the uniform elongation of the finally obtained steel sheet may decrease. The reduction rate in the hot rolling process is not particularly limited, but in order to make the microstructure inside the steel sheet fine and isotropic, it is preferable to set the cumulative reduction rate at a temperature of 1000°C or higher in the hot rolling process to 30% or more. If the cumulative rolling reduction is less than 30%, the average grain size and / or average aspect ratio of ferrite inside the steel sheet may become large, and the uniform elongation of the finally obtained steel sheet may decrease.

[0079] [Rough rolling] In the present manufacturing method, the heated slab may be subjected to rough rolling, for example, before high-pressure water descaling in order to adjust the plate thickness, etc. The conditions of the rough rolling are not particularly limited as long as the desired sheet bar dimensions can be secured.

[0080] [Cooling process] Next, water cooling of the obtained steel sheet is started within 10 seconds after the completion of the hot rolling process, and the surface temperature of the steel sheet is water-cooled to a temperature range of 820°C or less. By immediately water-cooling the steel sheet after the completion of rolling at a relatively high temperature in the previous hot rolling process, ferrite transformation is promoted, particularly in the surface layer of the steel sheet, and it is thereby possible to reliably achieve the desired ferrite fraction in the surface layer of the steel sheet. If the time from the completion of the hot rolling process to the start of water cooling exceeds 10 seconds, a relatively large amount of pearlite may be generated in the surface layer due to the diffusion of carbon from the inside of the steel sheet to the surface layer, and in such a case, it is not possible to achieve the desired ferrite fraction in the surface layer of the steel sheet. In addition, if the water-cooling stop temperature is higher than 820°C, a large amount of hard structure is generated in the surface layer of the steel sheet, and the bendability is reduced.

[0081] According to a preferred embodiment of the present manufacturing method, in the cooling step, the above water cooling is performed until the surface temperature of the steel sheet is in the temperature range of 820 to 770 ° C., and then the steel sheet is allowed to cool to 650 ° C. By using such a cooling history, it is possible to generate pearlite in the microstructure inside the steel sheet to improve the strength, while controlling the average lamellar spacing of the pearlite to a relatively wide range of 0.30 μm or more, thereby significantly improving the uniform elongation of the steel sheet. On the other hand, if water cooling is continued until the surface temperature of the steel sheet becomes lower than 770 ° C. due to excessive cooling, the grain orientation difference of ferrite inside the steel sheet may become large and / or the average lamellar spacing of pearlite may become too narrow, and the desired uniform elongation may not be obtained. In addition, if water cooling is performed again before the temperature drops to 650 ° C., a relatively large amount of hard structure may be generated inside the steel sheet, and the desired uniform elongation may not be obtained.

[0082] According to the steel sheet manufactured by the above manufacturing method, the microstructure in the surface layer of the steel sheet is mainly composed of ferrite, which is a soft structure, and the hard structure such as martensite is limited to a predetermined range, and the texture of the ferrite is homogenized, and the density of elongated inclusions contained in the surface layer can be reduced. As a result, the bendability of the steel sheet can be significantly improved. Furthermore, by optimizing the cooling process in the above manufacturing method by a combination of water cooling and natural cooling, the microstructure inside the steel sheet can be mainly composed of ferrite having a moderate grain size, which is isotropic and has fewer dislocations, and the microstructure can contain a predetermined amount of pearlite having a relatively wide average lamellar spacing. As a result, in addition to the above bendability, the uniform elongation of the steel sheet can also be significantly improved. Therefore, according to the steel sheet manufactured by the above manufacturing method, by combining the bendability achieved mainly by the microstructure in the surface layer of the steel sheet and the uniform elongation achieved mainly by the microstructure inside the steel sheet, it is possible to significantly suppress the occurrence of cracks on the surface of the strain concentration part during collision. Therefore, such a steel plate is useful for suppressing strain concentration during deformation due to collision and suppressing the occurrence of holes, and is particularly useful for application to structures that are at risk of collision with ships and the like on the ocean, such as ships, floating bodies, and marine structures.

[0083] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way. EXAMPLES

[0084] In the following examples, steel sheets according to the embodiments of the present invention were produced under various conditions, and the properties such as bendability and uniform elongation of the obtained steel sheets were examined.

[0085] Molten steel having the chemical composition shown in Table 1 was subjected to the casting, heating, hot rolling, and cooling steps under the conditions shown in Table 2 to obtain steel plates as examples including invention examples and comparative examples. In Table 2, the average cooling rate in the casting step indicates the average cooling rate in the temperature range where the surface temperature of the slab is 900 to 550°C, and the cumulative reduction in the hot rolling step indicates the cumulative reduction at temperatures of 1000°C or higher. The elapsed time until the start of water cooling in the cooling step indicates the elapsed time from the completion of the hot rolling step to the start of water cooling, and in the cooling step, the slab was allowed to cool to 650°C after water cooling was stopped.

[0086] [Table 1]

[0087] [Table 2]

[0088] [Characteristics evaluation] For the bending test, a test piece of 30 mm in the rolling direction of the steel plate, 100 mm in the width direction of the steel plate, and 5.0 mm in the thickness direction of the steel plate, including the surface of the steel plate, was taken, and a three-point bending test was performed with the ridge line in the rolling direction. The bending test was performed with a punch of 10 mm and 15 mm, with the surface opposite to the surface in contact with the punch being the surface of the steel plate, and the indentation depth was 10 mm. After the bending test, the pass / fail judgment was performed by visually observing the ridge line of the test piece for each of the 10 mm and 15 mm punches to confirm that no cracks had occurred. If no cracks occurred, it was judged as pass (◯), and if cracks occurred, it was judged as fail (×).

[0089] For the tensile tests, tensile test pieces with a parallel section diameter of 6.0 mm and a parallel section length of 32 mm (JIS No. 14A test pieces taken with the longitudinal direction in the C direction) were taken from 3 / 8 of the plate thickness of the steel plate, and the strain gauge length was set to 24.0 mm. The tensile properties, YS (0.2% yield strength), TS (tensile strength), EL (total elongation), and UEL (uniform elongation), were evaluated in accordance with JIS Z 2241:2011.

[0090] A steel sheet that passed the bending test using a 15 mmφ punch was evaluated as having improved bendability. The results are shown in Table 3. In Table 3, "surface microstructure" means the microstructure in the depth region from the surface of the steel sheet to 300 μm in the depth direction, and "internal microstructure" means the microstructure at a depth position of 5.0 mm in the depth direction from the surface of the steel sheet. In addition, the "hard structure" in the volume fraction of each microstructure means the sum of martensite, bainite, bainitic ferrite and retained austenite. In addition, in Table 3, "peak intensity" means the peak intensity at a 45-degree cross section in the three-dimensional crystal orientation distribution function of the BCC phase in the above depth region, and "spike density" means the density of spikes at a depth of 5.0 μm or more on the steel sheet surface.

[0091] [Table 3]

[0092] In the examples shown in Tables 1 to 3, Experiments Nos. 60 to 63 are comparative examples in which the chemical composition of the steel sheet did not satisfy formula (3) or the total of one or more of Ca, Mg, Zr, La, Ce, Te, Hf, and REM was not controlled within a predetermined range, resulting in excessive elongated inclusions in the surface layer of the steel sheet and impaired bendability. Experiment No. 59 is a comparative example in which the chemical composition of the steel sheet did not satisfy formula (1), resulting in excessive hard structure in the surface layer of the steel sheet and impaired bendability.

[0093] Test No. 8 is a comparative example in which the average cooling rate in the casting process was slow, causing the texture in the surface layer of the steel plate to develop and impairing the bendability.

[0094] Test No. 14 is a comparative example in which the maximum heating temperature in the heating process was low, which caused the texture to develop in the surface layer of the steel sheet, resulting in impaired bendability, whereas Test No. 46 is a comparative example in which the maximum heating temperature in the heating process was high, which caused the transformation in the surface layer of the steel sheet to not proceed properly, resulting in the generation of hard structures and impaired bendability. Test No. 55 is a comparative example in which the value of formula (4) was small in the heating process, texture developed in the surface layer of the steel sheet, and bendability was impaired. On the other hand, Test No. 4 is a comparative example in which the value of formula (4) was large in the heating process, recrystallization in the surface layer of the steel sheet did not progress sufficiently, texture developed, and bendability was impaired.

[0095] Test No. 52 is a comparative example in which the end temperature of descaling in the hot rolling process was low, and the texture in the surface layer of the steel sheet developed, resulting in impaired bendability. Test No. 58 is a comparative example in which the rolling completion temperature in the hot rolling process was low, and the texture in the surface layer of the steel sheet developed, resulting in impaired bendability. Experiments Nos. 3 and 7 are comparative examples in which the rolling conditions in the hot rolling process did not satisfy formula (5), and the texture in the surface layer of the steel sheet developed, resulting in impaired bendability.

[0096] Test No. 11 is a comparative example in which the time elapsed from the completion of rolling until the start of water cooling was long, and sufficient ferrite was not obtained in the surface layer of the steel sheet, resulting in impaired bendability. Test No. 17 is a comparative example in which the water cooling stop temperature in the cooling process was high, causing a large amount of hard structure to occur in the surface layer of the steel sheet, resulting in impaired bendability.

[0097] The other experimental examples are examples of the invention in which the steel sheets of the present invention can be obtained. Note that Experiments Nos. 23, 31, and 33 are cases in which the descaling end temperature in the hot rolling process was high, and a large number of spikes occurred on the surface layer of the steel sheet. Moreover, Experiments Nos. 27, 37, and 49 are cases in which the microstructure inside the steel sheet was outside the preferred range of the present invention, and therefore the bendability was good, but the uniform elongation was reduced. In the examples of the invention other than these, no cracks occurred not only in the bending test using a 15 mmφ punch, but also in the bending test using a 10 mmφ punch, and therefore, steel sheets with particularly excellent bendability and high uniform elongation were obtained.

Claims

1. The chemical composition, in mass%, is C: 0.075-0.240%, Si: 1.25% or less, Mn: 0.50-2.00%, P: 0.030% or less, S: 0.0100% or less, N: 0.0150% or less, O: 0.0030% or less, Al: 1.000% or less, Ti: 0 to 0.060%, Nb: 0 to 0.040%, V: 0-1.000%, Cu: 0-2.00%, Ni: 0-5.00%, Cr: 0-2.00%, Mo: 0-1.00%, W: 0-1.00%, B: 0 to 0.0050%, Sn: 0-1.000%, Sb: 0 to 0.200%, The total of one or more of Ca, Mg, Zr, La, Ce, Te, Hf, and REM: 0.0008 to 0.0050%, and The balance is composed of Fe and impurities. The following formulas (1), (2), and (3) are satisfied: The microstructure in the depth region from the surface to 300 μm in the depth direction is, in terms of volume fraction, Ferrite: 90% or more, and The sum of martensite, bainite, bainitic ferrite and retained austenite: 0 to 3%; The density of the elongated inclusions in the depth region is 1.0 × 10 pieces / m or less, The steel sheet is characterized in that a peak intensity at a 45-degree cross section in a three-dimensional crystal orientation distribution function of the BCC phase in the depth region is 5.0 or less. 2.44×10-2×(1.00-0.20[Si]+7.00[Nb])×(1.00-10[B]0.5)×(117+17[Si]+11[Si]2-33[M n]+4[Mn]2+79[Al]+59[Al]2-26[Ni]-12[Cr])×(1+1.3[Si]+0.8[Mo]0.5+35[Nb])-1≧1.00 ...Formula (1) 0≦64+41[Si]-34[Mn]+95[Al]2+74[Al]-14[Cr]-43[Ni]≦100...Formula (2) 0.02≦[Mn]×[S]×(7.50[Ca]+12.50[Mg]+3.30[Zr]+2.16[La]+2.14[Ce]+2.34[Te]+1.68[Hf]+1.94[REM])-1≦1.00...Formula (3) Here, [Si], [Nb], [B], [Mn], [Al], [Ni], [Cr], [Mo], [S], [Ca], [Mg], [Zr], [La], [Ce], [Te], [Hf] and [REM] are the contents [mass %] of each element, and are 0 when the element is not contained.

2. The chemical composition, in mass%, Ti: 0.008-0.030% Nb: 0.005-0.025% V:0.050~0.600% Cu: 0.05-2.00%, Ni: 0.15-3.00%, Cr: 0.10 to 2.00% or less, Mo: 0.03 to 1.00% W: 0.03 to 0.50% or less, B: 0.0005 to 0.0025% or less, Sn: 0.015 to 1.000% or less, and Sb: 0.005 to 0.200% or less The steel sheet according to claim 1 , further comprising one or more selected from the following:

3. The microstructure at a depth of 5.0 mm from the surface in the depth direction is, in terms of volume fraction, Ferrite: 80% or more, Perlite: 5% or more, and The sum of martensite, bainite, bainitic ferrite and retained austenite: 0 to 3%; The ferrite at the depth has an average crystal grain size of 8.0 to 20.0 μm, an average aspect ratio of 1.6 or less, and an intragranular orientation difference of 1.0 degree or less; 3. The steel plate according to claim 1, wherein the pearlite at the depth has an average lamellar spacing of 0.30 μm or more.

4. 3. The steel sheet according to claim 1, wherein the density of spikes having a depth of 5.0 μm or more on the surface is 1.0×10 3 / m or less.

5. A casting step of casting a slab having the chemical composition according to claim 1 or 2, and then cooling the slab at an average cooling rate of 100 ° C. / h or more in a temperature range of 900 to 550 ° C. A heating step of heating the slab, the maximum heating temperature of the slab being 1050 to 1250° C. and satisfying the following formula (4): A hot rolling process in which the slab is subjected to high-pressure water descaling and then hot rolling, in which the end temperature of the high-pressure water descaling is 1000° C. or higher, the time between each rolling pass at 1000° C. or lower satisfies the following formula (5), and the end temperature of the hot rolling is 900° C. or higher; A cooling step of starting water cooling of the obtained steel sheet within 10 seconds after the completion of the hot rolling step, and water cooling the steel sheet until the surface temperature of the steel sheet reaches a temperature range of 820° C. or less. A method for producing a steel sheet, comprising: [0010] Xi and ti are values ​​calculated for each of the ten equal intervals during which the temperature is 1050°C or higher. t is the length of each of the 10 equal time intervals [seconds], Ti is the slab temperature at the end of heating the i-th section out of 10 equal sections, A1, A2, A3, A4, A5, A1 and A7 are constants, which are 9.43×10-1, -3.50×104, 1.60×103, 1.12×100, 7.01×104, 5.46×102 and 9.50×103, X10 is obtained by calculating X1, X2, X3, ... in that order using the above formula. [0025] Equation (5) is an equation for evaluating and integrating the degree of recrystallization in the surface layer after the i-th rolling pass for n passes of rolling performed in a temperature range of 1000° C. or less, and is obtained using m, the elapsed time t [sec] between the i-th and (i+1)-th rolling passes, the sheet thickness h before the i-th rolling pass, and the sheet thickness h after the rolling pass, m is a value obtained from the steel sheet temperature Ti [°C] in the i-th rolling pass and the Nb content [Nb] [mass%] of the steel sheet, The elapsed time t [sec] until the next rolling pass for the nth rolling is the shorter of the elapsed time from the completion of the nth rolling until the steel sheet temperature reaches 900° C. or the elapsed time until water cooling is started, B1, B2, B3, B4, B5 and B6 are constants and are 1.00 x 102, 2.00 x 100, 8.43 x 10-11, 3.50 x 104, 2.73 x 102 and 4.75 x 101, respectively.

6. The method for producing a steel plate according to claim 5, characterized in that in the cooling step, the steel plate is water-cooled until the surface temperature reaches a temperature range of 820 to 770°C, and then allowed to cool to 650°C.

7. The maximum heating temperature in the heating step is 1050 to 1150° C., The method for producing a steel sheet according to claim 5, characterized in that a cumulative rolling reduction at a temperature of 1000°C or higher in the hot rolling step is 30% or more.

Citation Information

Patent Citations

  • High-strength and high-ductility thick steel plate and production method thereof

    JP2016125077A

  • Thick steel plate and manufacturing method therefor

    JP2018193605A

  • High-strength thick steel sheet and method for manufacturing same

    WO2016143345A1

  • High-strength thick steel plate and production method therefor

    WO2018030171A1