Steel plate and method for manufacturing the same
By optimizing the microstructure and composition of steel plates with ferrite and pearlite, the solution addresses the limitations of ductility in thick steel plates, improving uniform elongation and critical strain to prevent collision damage in marine structures.
Patent Information
- Application Number
- JP2023064410
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-11
- Publication Date
- 2024-10-24
AI Technical Summary
Existing steel plates used in structures such as ships, floating bodies, and offshore structures face limitations in suppressing damage from collisions due to saturation of ductility improvements with increasing plate thickness, necessitating methods to enhance uniform elongation and critical strain to prevent crack generation and propagation.
A steel plate composition primarily consisting of ferrite and pearlite with controlled microstructures, including specific chemical compositions and manufacturing processes to achieve uniform elongation and critical strain, characterized by reduced intragranular misorientation, maximum grain sizes, and inclusion densities.
The solution effectively suppresses crack generation and propagation during collisions, enhancing the steel plate's ability to withstand strain concentration areas, particularly in marine structures.
Smart Images

Figure 2024151196000001 
Figure 2024151196000002 
Figure 2024151196000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a steel plate and a manufacturing method thereof, and more particularly to a steel plate having improved uniform elongation and limiting strain amount, which is therefore useful for suppressing the initiation and propagation of cracks on the surface of strain concentrated areas during a collision, and a manufacturing method thereof. [Background technology]
[0002] Ships, floating bodies, and marine structures are at risk of collision with ships that deviate from their course on the ocean, so their designs must ensure that they do not lose their stability even if they are hit by an anticipated collision. To ensure stability, fenders and other materials are used to mitigate the impact, and structures are divided into multiple blocks to minimize the impact of holes caused by a collision. Designs to prepare for such collisions are considered in addition to the design required for the original purpose, and they increase the construction costs of ships, floating bodies, and marine structures.
[0003] As with ships, floating bodies, and marine structures, automobiles are also required to control damage to the body during a collision and keep it within an acceptable range for anticipated collisions in order to protect the safety of passengers. As described in Non-Patent Document 1, one solution to this problem in automobiles is to improve the strength of the steel materials used. By applying high-strength steel materials that do not easily break to the body, it is possible to significantly improve safety during a collision even for a body that follows the same design as before.
[0004] Similarly, in ships, the degree of damage during collision can be reduced by improving the properties of materials. For example, Patent Document 1 proposes a high-strength, high-ductility steel plate that controls the microstructure, reduces the dislocation density in soft ferrite grains, and homogenizes the hardness distribution in the plate thickness direction as a means of suppressing the occurrence of holes in the side of the ship during a ship collision. Specifically, the high-strength, high-ductility steel plate described in Patent Document 1 has a lower limit of total elongation (T.EL) of 23% or more, which is 1.5 times that of general steel, a yield strength (YP) of 355 to 500 MPa, and a tensile strength (TS) of 490 to 620 MPa.
[0005] Furthermore, Patent Document 2 proposes a low-strength thick steel plate excellent in elongation characteristics and corrosion resistance, the thick steel plate having a predetermined chemical composition, a metal structure containing ferrite at an area ratio of 70% or more relative to the total metal structure, the remainder being one or more types selected from the group consisting of pearlite, bainite and martensite, and a ferrite grain size of 3 μm or more and 40 μm or less.
[0006] Furthermore, Patent Document 3 proposes a low-yield-ratio, high-strength steel plate with excellent ductile fracture resistance, in which island martensite structures are dispersed in bainite structures, suppressing the occurrence of ductile cracks under biaxial stress conditions, with a bainite area fraction of 30 to 90% and an island martensite area fraction of 2 to 10%. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2016-125077 A [Patent Document 2] International Publication No. 2022 / 074933 [Patent Document 3] JP 2013-139602 A [Non-patent literature]
[0008] [Non-Patent Document 1] Manabu Takahashi: "100 Years of Sheet Technology - Sheet Steel and Manufacturing Technology that Developed Alongside the Automobile Industry", Tetsu-to-Hagane, Vol. 100, 2014, No. 1, p82-93 Summary of the Invention [Problem to be solved by the invention]
[0009] In order to promote high efficiency as a countermeasure against population decline and rising energy costs, ships, floating bodies, and marine structures are becoming larger, and the steel plates that make them up are also becoming thicker. Since the ductility of steel plates increases with increasing plate thickness, in structures that use thick steel materials, the effect of improving ductility in reducing damage during collisions is saturated, and in order to further reduce damage during collisions, it is necessary to consider methods other than improving ductility. In this regard, in order to reduce damage caused by collisions of structures, it is effective to improve the uniform elongation and limit strain in steel plates, which can suppress the occurrence of ductile cracks due to strain concentration due to the improvement in uniform elongation, and even if ductile cracks occur, it is possible to suppress the propagation of the ductile cracks due to the improvement in limit strain.
[0010] Therefore, an object of the present invention is to provide a steel sheet having improved uniform elongation and limit strain amount through a novel configuration, and a manufacturing method thereof. [Means for solving the problem]
[0011] The present inventors have studied the microstructural control of steel sheets necessary for improving uniform elongation and limit strain. As a result, the present inventors have found that both uniform elongation and limit strain can be improved by forming the microstructural structure of a steel sheet having a predetermined chemical composition with a composite structure in which ferrite, which is a soft structure, is the main component, pearlite is mainly contained as a hard structure, while other hard structures such as martensite are limited within a predetermined range. Furthermore, the present inventors have found that a ferrite structure with fewer dislocations can be realized by reducing the intragranular orientation difference of ferrite, and in this connection, the uniform elongation of the steel sheet can be significantly improved. In addition, the inventors have found that the limit strain of a steel plate can be significantly improved by reducing the maximum crystal grain size and maximum aspect ratio of ferrite within a predetermined range, reducing the maximum long axis of the island regions of pearlite that are dispersed in an island shape between ferrite grains within a predetermined range, reducing the Mn concentration in the cementite that forms the lamellar structure of the pearlite within a predetermined range, and reducing the density of elongated inclusions that serve as starting points for the generation of coarse voids in the microstructure within a predetermined range, and thus completed the present invention.
[0012] The present invention which has achieved the above object is as follows. (1) Chemical composition, in mass%, C: 0.060-0.240%, Si: 1.25% or less, Mn: 0.50-1.75%, P:0.030% or less, S: 0.0030% or less, N: 0.0150% or less, O: 0.0030% or less, Al: 1.000% or less, Ti: 0 to 0.060%, Nb: 0 to 0.040%, V: 0~1.00%, Cu: 0-2.00%, Ni: 0-5.00%, Cr: 0-2.00%, Mo: 0-1.00%, W: 0 to 1.00%, B: 0~0.0050%, Sn: 0~1.000%, Sb: 0 to 0.200%, Ca, Mg, Zr, La, Ce, Te, Hf, REM: 0.0008 to 0.0050% in total, and The balance is composed of Fe and impurities. Satisfying the following formula (1), The microstructure in the range from the surface to the position of 1 / 8 of the plate thickness in the plate thickness direction to the position of 3 / 8 of the plate thickness in the plate thickness direction from the surface is, in terms of volume fraction, Ferrite: 80% or more, Perlite: 5% or more, and The sum of martensite, bainite, bainitic ferrite and retained austenite: 0 to 3%. The maximum grain size of the ferrite is 30 μm or less, The maximum aspect ratio of the ferrite is 3.00 or less, The ferrite grain orientation difference is 1.0 degree or less, The maximum major axis of the island region made of pearlite is 20 μm or less, The Mn concentration in the cementite forming the lamellar structure of the pearlite is 0.050 or less, and The density of the elongated inclusion is 1.0×10 5 pieces / m 2 A steel plate characterized in that: 2.44×10 -2 ×(1.00-0.20[Si]+7.00[Nb])×(1.00-10[B] 0.5 )×(117+17[Si]+11[Si] 2 -33[Mn]+4[Mn] 2 +79[Al]+59[Al] 2 -26[Ni]-12[Cr])×(1+1.3[Si]+0.8[Mo] 0.5 +35[Nb]) -1 ≧1.00...Equation (1) Here, [Si], [Nb], [B], [Mn], [Al], [Ni], [Cr] and [Mo] are the contents [mass%] of each element, and are 0 when the element is not contained. (2) The chemical composition is, in mass%, Ti: 0.008 to 0.030%, Nb: 0.005 to 0.025%, V: 0.05-0.60%, Cu: 0.05-1.00%, Ni: 0.15-2.30%, Cr: 0.10~1.00%, Mo: 0.03-0.50%, W: 0.03 to 0.50%, B: 0.0005~0.0025%, Sn: 0.015~0.300%, Sb: 0.005 to 0.080%, The steel sheet according to (1) above, characterized in that it contains one or more selected from the following: (3) A casting process of casting a slab having the chemical composition described in (1) or (2) above, and rolling the slab by a cumulative amount of 20% or more after the center of the slab in the thickness direction is solidified without the temperature ever dropping below 1200°C; A heating step of heating the slab, the maximum heating temperature of the slab being 1120 to 1250° C., and satisfying the following formula (2): a rough rolling step of rough rolling the slab so that a cumulative rolling reduction in a temperature range of 1000° C. or higher is 35% or more; a finish rolling step in which the obtained rolled material is subjected to finish rolling, in which the rolling in a temperature range of 1000°C or less satisfies the following formula (3) and the finish rolling completion temperature is 900°C or higher; and The obtained steel sheet is air-cooled to 700°C, and then cooled in the temperature range of 700 to 450°C at an average cooling rate of 0.1 to 1.0°C / s. A method for producing a steel sheet, comprising:
number
number
[0013] According to the present invention, it is possible to provide a steel sheet having improved uniform elongation and critical strain amount, and a manufacturing method thereof. Therefore, with such a steel sheet, it is possible to suppress the generation and propagation of cracks on the surface of a strain concentrated portion during a collision, and therefore it is possible to significantly suppress the generation of holes during a collision. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Hereinafter, the steel sheet according to the embodiment of the present invention and the manufacturing method thereof will be described in more detail. However, these descriptions are intended to exemplify preferred forms of the present invention and are not intended to limit the present invention to specific embodiments.
[0015] [Chemical composition] Hereinafter, the chemical composition of the steel sheet according to the embodiment of the present invention will be described. In the following description, the unit of content of each element, "%", means "mass%" unless otherwise specified.
[0016] [C:0.060~0.240%] C is an element that contributes to improving strength. To fully obtain this effect, the C content is set to 0.060% or more. From the viewpoint of increasing strength, the C content is preferably 0.075% or more, and more preferably 0.090% or more or 0.110% or more. On the other hand, if C is excessively contained, sufficient uniform elongation and / or limit strain amount may not be obtained with high strength. Therefore, the C content is set to 0.240% or less. From the viewpoint of increasing bendability, the C content is preferably 0.220% or less, and more preferably 0.200% or less or 0.180% or less.
[0017] [Si:1.25% or less] Si is a deoxidizing element and also contributes to improving strength. The Si content may be 0%, but in order to obtain a sufficient deoxidizing effect by Si, the Si content is preferably 0.01% or more. In order to increase strength, the Si content is preferably 0.05% or more, and more preferably 0.10% or more or 0.30% or more. On the other hand, if the Si content is high, sufficient uniform elongation and / or limit strain amount may not be obtained with high strength. From this viewpoint, the Si content is set to 1.25% or less. Also, Si is an element that impairs the toughness of the steel plate, and from this viewpoint, the Si content is preferably 1.00% or less or 0.80% or less, and more preferably 0.50% or less.
[0018] [Mn: 0.50~1.75%] Mn is an element that contributes to improving strength, and in order to fully obtain this effect, 0.50% or more is added. From the viewpoint of increasing strength, the content of Mn is preferably 0.70% or more, and more preferably 1.00% or more or 1.20% or more. On the other hand, if Mn is excessively contained, the Mn concentration in cementite that forms the lamellar structure of pearlite cannot be reduced to within a desired range, and as a result, the limit strain amount of the steel sheet may not be sufficiently improved. From this viewpoint, the amount of Mn added is limited to 1.75% or less. Moreover, Mn is an element that impairs weldability and the toughness of the welded part, and from this viewpoint, the content of Mn is preferably 1.60% or less, and more preferably 1.50% or less or 1.40% or less.
[0019] [P:0.030% or less] P is an element that is inevitably contained in general steelmaking methods, and limiting it to less than 0.001% places a large burden on the smelting process and is economically undesirable, so the P content is preferably 0.001% or more. On the other hand, P is an element that impairs toughness, and from this viewpoint, the P content is limited to 0.030% or less. Furthermore, P is an element that impairs weldability and the toughness of welded parts, and from this viewpoint, the P content is preferably 0.020% or less, and more preferably 0.010% or less.
[0020] [S:0.0030% or less] S is an element that is inevitably contained in general steelmaking methods, and since limiting the S content to less than 0.0003% places a large load on the smelting process and is economically undesirable, the S content is preferably 0.0003% or more. On the other hand, S is an element that forms coarse sulfides that impair toughness, and forms elongated inclusions that reduce the limit strain of the steel plate. For this reason, the S content is limited to 0.0030% or less. In addition, S is an element that impairs weldability and the toughness of welds, and from this perspective, the S content is preferably 0.0025% or less, and more preferably 0.0020% or less.
[0021] [N:0.0150% or less] N is an element that is inevitably contained in a general steelmaking process. If a large amount of N is contained, coarse nitrides are formed, which impairs the toughness of the steel plate, so the N content is limited to 0.0150% or less. N is also an element that impairs the toughness of a welded portion, and from this viewpoint, the N content is preferably 0.0100% or less, and more preferably 0.0060% or less. There is no particular lower limit for the N content, but excessive reduction places a large load on the smelting process and is economically undesirable, so the N content is preferably 0.0003% or more, and more preferably 0.0015% or more.
[0022] [O:0.0030% or less] O is an element that is inevitably contained in a general steelmaking process. If a large amount of O is contained, coarse oxides are formed, which impairs the toughness of the steel sheet, so the O content is limited to 0.0030% or less. O is also an element that impairs the toughness of a welded portion, and from this viewpoint, the O content is preferably 0.0020% or less, and more preferably 0.0010% or less. There is no particular lower limit for the O content, but since limiting it to less than 0.0002% places a large load on the smelting process and is economically undesirable, it is preferable to set it to 0.0002% or more.
[0023] [Al: 1.000% or less] Al is a deoxidizing element. The Al content may be 0%, but in order to obtain this effect, it is preferable to add 0.005% or more, and more preferably 0.010% or more. On the other hand, Al is an element that impairs toughness, and the Al content is limited to 1.000% or less. In addition, since Al impairs weldability and the toughness of the welded portion, the Al content is preferably 0.800% or less, and more preferably 0.500% or less or 0.200% or less.
[0024] [Ca, Mg, Zr, La, Ce, Te, Hf and REM: 0.0008~0.0050%] Ca, Mg, Zr, La, Ce, Te, Hf and REM are elements that refine sulfides and improve the toughness and limit strain of steel sheets. In order to fully obtain this effect, the total content of Ca, Mg, Zr, La, Ce, Te, Hf and REM is 0.0008% or more, and may be, for example, 0.0010% or more or 0.0012% or more. On the other hand, if these elements are contained excessively, the effect is saturated, and therefore, the inclusion of Ca, Mg, Zr, La, Ce, Te, Hf and REM in the steel sheet more than necessary leads to an increase in manufacturing costs. In addition, Ca, Mg and REM in particular may combine with S in the steel to form elongated inclusions, which may reduce the limit strain of the steel sheet. Therefore, the total content of Ca, Mg, Zr, La, Ce, Te, Hf and REM is limited to 0.0050% or less, preferably 0.0035% or less or 0.0030% or less, and more preferably 0.0015% or less. Here, REM is a general term for the lanthanoid group (Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb and Lu) excluding Sc, Y, La and Ce, and the total content of these 15 elements is the REM content.
[0025] The basic chemical composition of the steel sheet according to the embodiment of the present invention is as described above. Furthermore, the steel sheet may contain one or more of the following optional elements as necessary. The steel sheet may contain one or more selected from the group consisting of Ti: 0-0.060%, Nb: 0-0.040%, V: 0-1.00%, and Cu: 0-2.00%. The steel sheet may also contain one or more selected from the group consisting of Ni: 0-5.00%, Cr: 0-2.00%, Mo: 0-1.00%, and W: 0-1.00%. The steel sheet may also contain B: 0-0.0050%. The steel sheet may also contain one or two selected from the group consisting of Sn: 0-1.000% and Sb: 0-0.200%. These optional elements will be described in detail below.
[0026] [Ti: 0~0.060%] Ti is an element that contributes to improving strength. The Ti content may be 0%, but when it is contained, it may be 0.001% or more or 0.003% or more. From the viewpoint of increasing strength, the Ti content is preferably 0.008% or more, and more preferably 0.010% or more. On the other hand, if Ti is contained excessively, coarse Ti carbonitrides are generated, and there is a concern that the toughness of the steel plate and welded parts may be significantly deteriorated. From this viewpoint, the Ti content is preferably limited to 0.060% or less, and more preferably 0.030% or less or 0.020% or less.
[0027] [Nb: 0~0.040%] Nb is an element that contributes to improving strength, and may be contained in an amount of 0.040% or less. If the Nb content exceeds 0.040%, precipitation strengthening is excessively expressed, and there is a concern that the uniform elongation and / or limit strain amount may be impaired. The Nb content may be 0.025% or less, 0.015% or less, or 0.010% or less. On the other hand, the Nb content may be 0%, but from the viewpoint of increasing strength, the Nb content is preferably 0.001% or more, and more preferably 0.005% or more.
[0028] [V:0~1.00%] V is an element that contributes to improving strength, and may be contained in an amount of 1.00% or less. If the V content exceeds 1.00%, precipitation strengthening is excessively expressed, and there is a concern that the uniform elongation and / or limit strain amount may be impaired. The V content is preferably 0.60% or less or 0.30% or less. On the other hand, the V content may be 0%, but from the viewpoint of increasing strength, the V content is preferably 0.01% or more, and more preferably 0.05% or more.
[0029] [Cu:0~2.00%] Cu is an element that contributes to improving strength, and may be contained in an amount of 2.00% or less. If the Cu content exceeds 2.00%, precipitation strengthening is excessively expressed, and there is a concern that the uniform elongation and / or limit strain amount may be impaired. The Cu content is more preferably 1.00% or less or 0.50% or less. On the other hand, the Cu content may be 0%, but from the viewpoint of increasing strength, the Cu content is preferably 0.01% or more, and more preferably 0.05% or more.
[0030] [Ni:0~5.00%] Ni is an element that contributes to improving strength and / or heat resistance. The Ni content may be 0%, but in order to obtain this effect, it is preferable to make it 0.01% or more or 0.10% or more, and more preferably 0.15% or more. On the other hand, if the Ni content exceeds 5.00%, the hardenability increases excessively, and the uniform elongation and / or limit strain amount is impaired. From this viewpoint, the Ni content is limited to 5.00% or less, preferably 2.30% or less, and more preferably 1.50% or less or 1.00% or less.
[0031] [Cr:0~2.00%] Cr is an element that contributes to improving strength, and may be contained at 2.00% or less. The Cr content may be 0%, but from the viewpoint of increasing strength, the Cr content is preferably 0.01% or more or 0.10% or more. On the other hand, excessive Cr content may increase alloy costs and reduce toughness. Therefore, the Cr content is limited to 2.00% or less, and preferably 1.00% or less. Cr is an element that impairs weldability and the toughness of the welded portion, and from this viewpoint, the Cr content is more preferably 0.60% or less.
[0032] [Mo:0~1.00%] Mo is an element that contributes to improving strength. The Mo content may be 0%, but from the viewpoint of increasing strength, the Mo content is preferably 0.01% or more or 0.03% or more, and more preferably 0.08% or more. On the other hand, even if Mo is contained excessively, the effect becomes saturated, and there is a risk of causing an increase in manufacturing costs. Therefore, the Mo content is limited to 1.00% or less, preferably 0.50% or less, and more preferably 0.30% or less.
[0033] [W:0~1.00%] W is an element that contributes to improving strength. The W content may be 0%, but from the viewpoint of increasing strength, the W content is preferably 0.01% or more or 0.03% or more, and more preferably 0.08% or more. On the other hand, if W is contained excessively, the hardenability increases excessively, and the uniform elongation and / or limit strain amount is impaired. From this viewpoint, the W content is limited to 1.00% or less, preferably 0.50% or less, and more preferably 0.30% or less.
[0034] [B: 0~0.0050%] B is an element that contributes to improving strength, and may be contained at 0.0050% or less. The content of B may be 0%, but from the viewpoint of increasing strength, the content of B is preferably 0.0001% or more or 0.0005% or more, and more preferably 0.0010% or more. On the other hand, if B is contained excessively, there is a concern that the weldability and toughness of the welded part may be impaired. From this viewpoint, the content of B is limited to 0.0050% or less, preferably 0.0025% or less, and more preferably 0.0015% or less.
[0035] [Sn:0~1.000%] Sn is an element that contributes to improving strength, and may be contained at 1.000% or less. The Sn content may be 0%, but from the viewpoint of increasing strength, the Sn content is preferably 0.005% or more or 0.015% or more, and more preferably 0.030% or more. On the other hand, if Sn is contained excessively, there is a concern that the weldability and toughness of the welded part may be impaired. From this viewpoint, the Sn content is limited to 1.000% or less, preferably 0.300% or less, and more preferably 0.100% or less.
[0036] [Sb: 0~0.200%] Sb is an element that contributes to improving strength, and may be contained in an amount of 0.200% or less. The Sb content may be 0%, but from the viewpoint of increasing strength, the Sb content is preferably 0.001% or more or 0.005% or more. On the other hand, if Sb is contained in an excessive amount, there is a concern that the hardenability will be excessively improved and the uniform elongation and / or the limit strain amount will decrease. From this viewpoint, the Sb content is limited to 0.200% or less, preferably 0.080% or less, and more preferably 0.030% or less.
[0037] In the steel sheet according to the embodiment of the present invention, the balance other than the above elements consists of Fe and impurities. The impurities are components that are mixed in due to various factors in the manufacturing process, including raw materials such as ores and scraps, when the steel sheet is industrially manufactured.
[0038] The chemical composition of steel sheets can be measured by a general analytical method. For example, the chemical composition of steel sheets can be measured using inductively coupled plasma-atomic emission spectrometry (ICP-AES). C and S are measured using the combustion-infrared absorption method.
[0039] [Control of phase transformation by chemical composition] In order to obtain the steel sheet according to the embodiment of the present invention, it is necessary to form a predetermined microstructure by appropriately advancing the phase transformation. In order to control the behavior of the phase transformation, it is necessary to satisfy the following formula (1) in order to appropriately control the chemical composition of the steel sheet. 2.44×10 -2 ×(1.00-0.20[Si]+7.00[Nb])×(1.00-10[B] 0.5 )×(117+17[Si]+11[Si] 2 -33[Mn]+4[Mn] 2 +79[Al]+59[Al] 2 -26[Ni]-12[Cr])×(1+1.3[Si]+0.8[Mo] 0.5 +35[Nb]) -1 ≧1.00...Equation (1) Here, [Si], [Nb], [B], [Mn], [Al], [Ni], [Cr] and [Mo] are the contents [mass%] of each element, and are 0 when the element is not contained.
[0040] Formula (1) shows the range of chemical composition that allows ferrite transformation to proceed sufficiently while not excessively promoting or inhibiting pearlite transformation. To explain in more detail, formula (1) takes into consideration the driving force of ferrite transformation, the nucleation rate of ferrite transformation, and the interface mobility (degree of transformation progress). Specifically, the 2.44×10 -2 ×(1.00-0.20[Si]+7.00[Nb])×(1.00-10[B] 0.5 ) corresponds to the nucleation rate of the ferrite transformation, and (117+17[Si]+11[Si] 2 -33[Mn]+4[Mn] 2 +79[Al]+59[Al] 2 -26[Ni]-12[Cr]) corresponds to the driving force of the ferrite transformation, and (1+1.3[Si]+0.8[Mo] 0.5 +35[Nb]) -1corresponds to the interface mobility. The larger the value of the left side of formula (1), the higher the temperature at which the ferrite transformation can proceed, and by proceeding with the ferrite transformation at high temperatures, ferrite with a small misorientation within the crystal grains can be obtained. From this viewpoint, the value of the left side of formula (1) is set to 1.00 or more, preferably 1.15 or more, and more preferably 1.30 or more.
[0041] Next, the characteristics of the microstructure of the steel sheet according to the embodiment of the present invention will be described. The steel sheet according to the embodiment of the present invention specifies a microstructure in the range from a position (1 / 8t) that is 1 / 8 of the thickness in the thickness direction from the surface to a position (3 / 8t) that is 3 / 8 of the thickness in the thickness direction from the surface. The reason for this is that the microstructure in the above range centered on a position (1 / 4t) that is 1 / 4 of the thickness in the thickness direction from the surface is a representative structure of the steel sheet, and is highly correlated with the mechanical properties of the steel sheet. The ratios of the following structures in the microstructure are all volume fractions.
[0042] [Ferrite: 80% or more] Since ferrite is a soft structure, it is possible to improve the uniform elongation of the steel sheet by including the ferrite as the main structure of the steel sheet. In an embodiment of the present invention, in order to achieve a desired uniform elongation, the volume fraction of ferrite is controlled to 80% or more. From the viewpoint of improving the uniform elongation of the steel sheet, the higher the volume fraction of ferrite, the more preferable it is, and it may be, for example, 82% or more, 85% or more, 88% or more, or 90% or more. Although there is no particular upper limit, if the volume fraction of ferrite is too high, the hard structure such as pearlite will be insufficient, resulting in a decrease in strength. Therefore, for example, the volume fraction of ferrite is preferably 95% or less, and may be 94% or less or 92% or less.
[0043] [Perlite: 5% or more] In order to improve the limit strain amount in the steel sheet according to the embodiment of the present invention, it is important to suppress the generation and propagation of voids in the microstructure. From the viewpoint of suppressing the generation of voids, pearlite is a superior structure compared to other hard structures, and therefore, in the steel sheet according to the embodiment of the present invention, pearlite is contained at a volume fraction of 5% or more in order to suppress the generation of voids and thereby improve the limit strain amount. The volume fraction of pearlite may be, for example, 6% or more or 8% or more. Although there is no particular upper limit, if the volume fraction of pearlite becomes too high, ferrite, which is a soft structure, becomes insufficient, resulting in a decrease in uniform elongation. Therefore, for example, the volume fraction of pearlite is preferably 20% or less, and may be 18% or less, 15% or less, 12% or less, or 10% or less.
[0044] [Total of martensite, bainite, bainitic ferrite and retained austenite: 0~3%] The steel sheet according to the embodiment of the present invention may be composed of only ferrite and pearlite, and therefore the remaining structure may be 0% in volume fraction. When the remaining structure is present, the remaining structure is one or more of martensite (including tempered martensite), bainite, bainitic ferrite, and retained austenite. However, if these hard structures are contained in a relatively large amount, sufficient uniform elongation and / or limit strain may not be obtained. Therefore, the total of martensite, bainite, bainitic ferrite, and retained austenite is set to 3% or less in volume fraction. From the viewpoint of improving the uniform elongation and / or limit strain of the steel sheet, the total of martensite, bainite, bainitic ferrite, and retained austenite is preferably set to 2% or less in volume fraction, and more preferably set to 1% or less. The lower limit is not particularly limited, but for example, the total of martensite, bainite, bainitic ferrite, and retained austenite may be 0% or 0.5% or more.
[0045] Next, the characteristics of the ferrite region will be described.
[0046] [Maximum grain size of ferrite: 30 μm or less] As described above, in order to improve the critical strain of the steel sheet, it is important to suppress the generation and propagation of voids in the microstructure. In relation to this, the present inventors have found that by reducing the maximum aspect ratio of ferrite, which will be described in detail later, and the maximum long diameter of the island regions of pearlite dispersed in islands between ferrite grains, in addition to the maximum grain size of ferrite, each within a predetermined range, and further reducing the density of elongated inclusions, which are the starting points of coarse voids in the microstructure, within a predetermined range, the generation and / or propagation of voids in the microstructure can be sufficiently and reliably suppressed, thereby significantly improving the critical strain of the steel sheet. In particular, since coarse ferrite grains are the starting points of void generation, it is necessary to reduce the maximum grain size of ferrite in order to suppress the generation of voids. More specifically, in the steel sheet according to the embodiment of the present invention, the maximum grain size of ferrite must be controlled to 30 μm or less. For example, even if the average grain size of ferrite is controlled to a relatively small range, if coarse ferrite grains exceeding 30 μm are included, the limit strain amount of the steel sheet cannot be sufficiently improved. Therefore, in the steel sheet according to the embodiment of the present invention, it is extremely important to control the maximum grain size of ferrite, not the average grain size of ferrite. From the viewpoint of suppressing the generation of voids, the smaller the maximum grain size of ferrite, the more preferable it is, and for example, it may be 28 μm or less, 25 μm or less, 22 μm or less, 20 μm or less, 18 μm or less, or 16 μm or less. The lower limit is not particularly limited, but for example, the maximum grain size of ferrite may be 5 μm or more, 8 μm or more, or 10 μm or more.
[0047] [Maximum aspect ratio of ferrite: 3.00 or less] Ferrite grains with a large aspect ratio become the starting point of void generation, as in the case of coarse ferrite grains. Therefore, in the steel sheet according to the embodiment of the present invention, in order to suppress the generation of voids, it is important to control the maximum aspect ratio of ferrite, not the average aspect ratio, within a predetermined range, and more specifically, the maximum aspect ratio of ferrite is controlled to 3.00 or less. From the viewpoint of suppressing the generation of voids, the smaller the maximum aspect ratio of ferrite, the more preferable it is, and for example, it may be 2.80 or less, 2.50 or less, 2.20 or less, 2.00 or less, or 1.80 or less. The lower limit is not particularly limited, but for example, the maximum aspect ratio of ferrite may be 1.2 or more, 1.4 or more, or 1.5 or more.
[0048] [Ferrite grain orientation difference: 1.0 degree or less] In order to improve the uniform elongation of the steel sheet, it is necessary to make the microstructure of the steel sheet a ferrite-based structure, more specifically, a structure in which ferrite has a volume fraction of 80% or more, as described above, and to further reduce the dislocations contained in the grains of the ferrite. In relation to this, in the steel sheet according to the embodiment of the present invention, by controlling the intragranular orientation difference of ferrite to 1.0 degree or less, a ferrite structure with fewer dislocations is realized, and it is possible to significantly improve the uniform elongation of the steel sheet based on the combination with the feature that the volume fraction of ferrite is 80% or more. From the viewpoint of improving the uniform elongation of the steel sheet, the smaller the intragranular orientation difference of ferrite is, the more preferable it is, and for example, it may be 0.8 degrees or less. The lower limit is not particularly limited, but for example, the intragranular orientation difference of ferrite may be 0 degrees or more, 0.1 degrees or more, or 0.2 degrees or more.
[0049] Next, the characteristics of the pearlite region will be described.
[0050] [Maximum long diameter of pearlite island regions: 20 μm or less] In the steel sheet according to the embodiment of the present invention, pearlite is present in the form of islands dispersed among the ferrite grains that occupy the majority of the microstructure, i.e., 80% or more in volume fraction. If such pearlite islands are excessively large in size, voids generated in the microstructure propagate relatively easily, and the limit strain of the steel sheet decreases. Therefore, in the steel sheet according to the embodiment of the present invention, the maximum major axis of the pearlite island region is controlled to 20 μm or less to suppress the propagation of voids, thereby improving the limit strain of the steel sheet. As in the case of the maximum grain size and maximum aspect ratio of ferrite, it is important to control the maximum major axis of the pearlite island region, rather than the average diameter. For example, even if the average diameter of the pearlite island region is controlled to a relatively small range, if the pearlite island region with the maximum major axis exceeding 20 μm is included, the limit strain of the steel sheet cannot be sufficiently improved. From the viewpoint of suppressing the propagation of voids, the smaller the maximum major axis of the pearlite island regions, the more preferable, and may be, for example, 18 μm or less, 15 μm or less, 12 μm or less, 10 μm or less, or 8 μm or less. Although there is no particular lower limit, for example, the maximum major axis of the pearlite island regions may be 2 μm or more, 3 μm or more, or 5 μm or more.
[0051] [Mn concentration in cementite forming the lamellar structure of pearlite: 0.05 or less] Pearlite is basically composed of two phases, ferrite and cementite, and various elements may be concentrated in cementite (Fe3C). The present inventors have found that when the Mn concentration in the cementite forming the lamellar structure of pearlite is controlled within a predetermined range, more specifically, when the Mn concentration in the cementite forming the lamellar structure of pearlite is controlled to 0.05 or less, the limit strain amount of the steel sheet can be significantly improved. Although not intending to be bound by any particular theory, it is believed that when the Mn concentration in the cementite forming the lamellar structure of pearlite is greater than 0.05, such a relatively high Mn concentration makes it easier for fracture or peeling to occur between the cementite in pearlite and the surrounding ferrite, and as a result, the limit strain amount of the steel sheet is reduced. Therefore, from the viewpoint of preventing fracture or peeling of cementite in pearlite and improving the critical strain of the steel sheet, the smaller the Mn concentration in the cementite forming the lamellar structure of pearlite, the more preferable, and it may be, for example, 0.04 or less, 0.03 or 0.02 or less. The lower limit is not particularly limited, but for example, the Mn concentration in the cementite forming the lamellar structure of pearlite may be 0 or 0.01 or more.
[0052] [Density of elongated inclusions: 1.0×10 5 pieces / m 2 below] The elongated inclusions become the starting points for the generation of coarse voids in the microstructure, and therefore, if a relatively large number of such elongated inclusions are present, the critical strain of the steel sheet is reduced. For this reason, in the steel sheet according to the embodiment of the present invention, the density of the elongated inclusions is set to 1.0×10 5 pieces / m 2 or less to suppress the occurrence of coarse voids, thereby improving the critical strain of the steel sheet. In the present invention, an elongated inclusion refers to any inclusion that is elongated in one direction (e.g., the rolling direction) and has an aspect ratio, defined by the major axis / minor axis, of 5.0 or more. From the viewpoint of suppressing the occurrence of coarse voids, the smaller the density of such elongated inclusions, the more preferable it is, and a density of 0.8×10 5 pieces / m2 Below, 0.5 x 10 5 pieces / m 2 Below, 0.3 × 10 5 pieces / m 2 Less than or equal to 0.1×10 5 pieces / m 2 The lower limit is not particularly limited, but for example, the density of the elongated inclusions is 0.01×10 5 pieces / m 2 or more than 0.02×10 5 pieces / m 2 Specific examples of the elongated inclusions are not particularly limited, but for example, the elongated inclusions may be sulfides containing at least one of Ca, Mg, and REM and S, in particular MnS and / or MnS in which part of Mn is substituted with Ca, or may be composite inclusions in which these sulfides are mixed with oxides of Ti, Al, etc.
[0053] [Evaluation of microstructural characteristics] The characteristics of the microstructure are evaluated by detailed observation of the steel sheet. Specifically, a small piece is cut out from a 1 / 2 width portion of the steel sheet or processed steel sheet, covering a range from a position of 1 / 8 of the sheet thickness from the surface in the sheet thickness direction to a position of 3 / 8 of the sheet thickness from the surface in the sheet thickness direction, and used as an observation sample. The volume fraction of the retained austenite is calculated by obtaining a diffraction peak of the fcc phase in the above-mentioned range in the sheet thickness direction by X-ray diffraction. The volume fraction of each structure other than the retained austenite, the maximum crystal grain size and maximum aspect ratio of ferrite, and the maximum long diameter of the island region consisting of pearlite are observed and measured using a field emission scanning electron microscope, and the cross section parallel to the rolling direction and perpendicular to the sheet surface is used as the observation surface, and the observation surface is wet-polished and polished with colloidal silica to make it a mirror surface, and then etched with nital (a mixture of ethanol and nitric acid) to obtain an observation sample. The range in the sheet thickness direction is observed and evaluated at a magnification of 1000 to 3000 times. The volume fraction of the material other than the retained austenite was evaluated by the above-mentioned electron microscope observation, and the total volume fraction was 1.0 × 10 -8 m 2The microstructure of the above-mentioned regions is photographed, and the structure at 200 or more lattice points is determined by the point counting method, and the area fraction of each structure is calculated.
[0054] The maximum grain size of ferrite is determined by calculating the average value of the long diameter and the short diameter of 100 or more ferrite grains randomly selected from the photograph observed with the electron microscope, and determining the grain size of each ferrite grain as the maximum grain size of ferrite. Furthermore, the maximum aspect ratio of ferrite is determined by calculating the aspect ratio, which is the ratio of the long diameter to the short diameter, of the top 20 grains with the largest grain size among the 100 or more ferrite grains randomly selected from the photograph observed with the electron microscope, and determining the maximum of these aspect ratios as the maximum aspect ratio of ferrite. The maximum long diameter of the pearlite island region is determined by calculating the long diameter of each of the 100 or more pearlite island regions randomly selected from the photograph observed with the electron microscope, and determining the maximum of all the long diameters obtained as the maximum long diameter of the pearlite island region.
[0055] The intragranular orientation misorientation of ferrite is determined as follows. Specifically, first, a sample is taken from a steel sheet so that the plate thickness cross section parallel to the rolling direction and perpendicular to the plate surface is the observation surface, and EBSD analysis is performed at measurement intervals of 1 μm on a rectangular region of 1000 μm in the rolling direction of the steel sheet and 100 μm in the normal direction to the rolling surface, centered at a position 3 / 8 of the plate thickness from the surface of the steel sheet, to obtain crystal orientation information of this rectangular region. The EBSD analysis is performed at an analysis speed of 50 to 300 points / second using a device consisting of a thermal field emission scanning electron microscope (JSM-7001F manufactured by JEOL) and an EBSD detector (HIKARI detector manufactured by TSL). Next, the orientation misorientation (GAM value: Grain Average Misorientation) in the ferrite grains is calculated from the crystal orientation information of this rectangular region using the software "OIM Analysis (registered trademark)" attached to the EBSD analysis device.
[0056] The Mn concentration in the cementite that forms the lamellar structure of pearlite is measured by a three-dimensional atom probe. The cementite that forms the lamellar structure of pearlite is identified from the measured carbon concentration distribution, and the concentrations of Fe, Si, Mn, Ni, Cu, Cr, Mo, W, Nb, Ti, V, B, Sn, and Sb at that location are calculated, and the measured Mn concentration is divided by the sum of the concentrations of all the elements including Mn to obtain the Mn concentration.
[0057] The density of elongated inclusions is determined by detailed observation of the steel plate using an optical microscope or FE-SEM. Specifically, the observation surface is a surface parallel to the plate surface at a position 3 / 8 of the plate thickness from the surface in the plate thickness direction in a location that is 1 / 2 the width of the steel plate or processed steel plate, and a small piece including this region is cut out and used as the observation sample. The observation surface is wet polished and polished with colloidal silica to make it a mirror surface, and a total of 5.0 × 10 -5 m 2 The above area is observed to evaluate the density of the elongated inclusions.
[0058] [Mechanical properties] [Tensile strength (TS), total elongation (EL), uniform elongation (UEL) and yield strength (YS)] According to the steel sheet having the above chemical composition and microstructure, a high tensile strength (TS), specifically a tensile strength of 400 MPa or more can be achieved. The tensile strength is preferably 420 MPa or more, 440 MPa or more, or 490 MPa or more. The upper limit is not particularly limited, but for example, the tensile strength may be 780 MPa or less, 700 MPa or less, or 650 MPa or less. Furthermore, according to the steel sheet according to the embodiment of the present invention, a total elongation (EL) of 20% or more can be achieved. The total elongation is preferably 22% or more, 25% or more, or 30% or more. The upper limit is not particularly limited, but for example, the total elongation may be 45% or less, 42% or less, or 40% or less. Furthermore, according to the steel sheet according to the embodiment of the present invention, a uniform elongation (UEL) of 15.0% or more can be achieved. The uniform elongation is preferably 16.0% or more, or 17.0% or more. The upper limit is not particularly limited, but for example, the uniform elongation may be 30.0% or less, 25.0% or less, or 20.0% or less. Moreover, according to the steel plate according to the embodiment of the present invention, a yield strength (YS) of 260 MPa or more can be achieved. The yield strength is preferably 280 MPa or more or 300 MPa or more. The upper limit is not particularly limited, but for example, the yield strength may be 550 MPa or less, 500 MPa or less, or 450 MPa or less. The tensile strength, total elongation, uniform elongation and yield strength are measured by taking a JIS 14A test piece from a direction (C direction) in which the longitudinal direction of the test piece is parallel to the rolling perpendicular direction of the steel plate, and performing a tensile test in accordance with JIS Z 2241:2011, and the yield strength means the 0.2% proof stress obtained by the above tensile test.
[0059] Plate Thickness The steel sheet according to the embodiment of the present invention generally has a thickness of 10 to 150 mm, although it is not particularly limited thereto. For example, the thickness may be 25 mm or more, 40 mm or more, or 50 mm or more, and / or 120 mm or less, or 100 mm or less.
[0060] [Steel plate manufacturing method] Next, a preferred method for manufacturing the steel plate according to the embodiment of the present invention will be described. The following description is intended to exemplify a characteristic method for manufacturing the steel plate according to the embodiment of the present invention, and is not intended to limit the steel plate to one manufactured by the manufacturing method described below.
[0061] The method for producing a steel sheet according to an embodiment of the present invention comprises: casting a slab having the chemical composition described above in relation to the steel sheet, and rolling the slab after the center of the slab has solidified by a cumulative total of 20% or more without the temperature ever dropping below 1200°C; A heating step of heating the slab, the maximum heating temperature of the slab being 1120 to 1250° C., and satisfying the following formula (2): a rough rolling step of rough rolling the slab so that a cumulative rolling reduction in a temperature range of 1000° C. or higher is 35% or more; a finish rolling step in which the obtained rolled material is subjected to finish rolling, in which the rolling in a temperature range of 1000°C or less satisfies the following formula (3) and the finish rolling completion temperature is 900°C or higher; and The obtained steel sheet is air-cooled to 700°C, and then cooled in the temperature range of 700 to 450°C at an average cooling rate of 0.1 to 1.0°C / s. The present invention is characterized in that it includes:
number
number
[0062] [Casting process] First, a slab having the chemical composition described above in relation to the steel plate is manufactured, but the manufacturing method of the slab is not particularly limited, and it can be manufactured by, for example, a continuous casting method or a blooming method. In this manufacturing method, it is important to perform rolling by a cumulative 20% or more while the temperature does not fall below 1200 ° C. once after the center of the slab in the thickness direction is solidified. This makes it possible to suppress the generation of coarse grains and elongated grains, and to reduce the maximum crystal grain size and maximum aspect ratio of ferrite, the maximum long diameter of the island region made of pearlite, and the density of elongated inclusions to within the desired range in the microstructure of the finally obtained steel plate. To explain in more detail, coarse grains and elongated grains are likely to occur in the part where solidification segregation, i.e., center segregation, occurs. Therefore, it is important to suppress center segregation in the casting process, and more specifically, it is important to gradually solidify from the surface of the molten steel, and finally, by performing sufficient reduction in a state where the temperature immediately after the center part solidifies is relatively high, recrystallization is firmly promoted at the center segregation part. By performing such an operation, it is possible to homogenize the structure of the center segregation part.
[0063] Although it is not intended to be bound by any particular theory, usually, in the casting process, there are relatively many coarse grains, and therefore the movement of elements along the grain boundaries is difficult to occur. However, it is considered that the grain boundaries move as the recrystallization proceeds, and the structure is further refined by the recrystallization, so that the movement of elements along the grain boundaries also occurs relatively easily, and as a result, the structure in the central segregation part can be homogenized. On the other hand, if the temperature of the center part in the thickness direction of the slab falls below 1200°C even once after solidification, the recrystallization cannot be sufficiently advanced and / or the movement of elements along the grain boundaries becomes difficult to occur, and the structure in the central segregation part cannot be sufficiently homogenized. As a result, in the microstructure of the finally obtained steel sheet, it becomes impossible to control the maximum grain size and maximum aspect ratio of ferrite, the maximum long diameter of the island region made of pearlite, and / or the density of the elongated inclusions within the desired range. In addition, it is preferable to perform rolling of 20% or more in the casting process in multiple steps rather than once in order to avoid cracks during rolling. More specifically, for example, it is preferable to perform rolling so that the cumulative rolling reduction in three or more rolling passes is 20% or more.
[0064] [Heating process] In order to hot roll the produced slab, the slab is subjected to a heat treatment in which the maximum heating temperature is 1120 to 1250° C. and the following formula (2) is satisfied.
number
[0065] By carrying out such a heat treatment, the slab can be heated homogeneously and sufficiently, and this is also effective in controlling the maximum major axis of the pearlite island region within a desired range. If the maximum heating temperature is below 1120°C or the value of formula (2) is less than 1.0, the maximum major axis of the pearlite island region cannot be controlled within a desired range, and as a result, the desired limit strain amount cannot be obtained. Since the isotropy of the microstructure is improved by increasing the maximum heating temperature, the maximum heating temperature is preferably 1150°C or higher. On the other hand, if the maximum heating temperature exceeds 1250°C or the value of formula (2) exceeds 3.5, the maximum grain size of ferrite becomes too large, and the desired limit strain amount may not be obtained. From the viewpoint of fine ferrite, the maximum heating temperature is preferably 1200°C or lower.
[0066] [Rough rolling process] The heat-treated slab is subjected to rough rolling in a temperature range of 1000°C or higher so that the cumulative reduction ratio relative to the slab thickness is 35% or more. In addition to the casting process, the rough rolling process can also be performed at a relatively high rough rolling rate of 35% or more in a temperature range of 1000°C or higher where recrystallization progresses, thereby further promoting the refinement of the microstructure. As a result, it is possible to control the maximum grain size of ferrite in the finally obtained microstructure within a desired range. If the cumulative reduction ratio in the above temperature range is less than 35%, coarse ferrite grains are formed in the finally obtained microstructure, and the desired limit strain amount cannot be obtained. From this perspective, the cumulative reduction ratio in the above temperature range is set to 35% or more, and preferably 40% or more. Although there is no particular upper limit, excessive reduction makes the steel sheet too thin, making it difficult to ensure a sufficient reduction ratio in the subsequent finish rolling process. For this reason, the cumulative reduction ratio in the above temperature range of rough rolling is preferably set to 70% or less.
[0067] [Finish rolling process] Next, the steel plate is subjected to finish rolling until the plate thickness reaches the product plate thickness. The finish rolling is performed so that the rolling temperature of the rolled material obtained by rough rolling in a temperature range of 1000°C or less satisfies the following formula (3) and the completion temperature of the finish rolling is 900°C or more.
number
[0068] If the value of formula (3) is too small, recrystallization does not proceed sufficiently, and a coarse structure elongated in one direction is obtained. On the other hand, if the value of formula (3) is too large, crystal grain growth after recrystallization proceeds excessively, the microstructure becomes coarse on average, the progress of subsequent phase transformation is suppressed, ferrite is formed at a lower temperature, and the orientation difference within the crystal grains becomes large. From these viewpoints, the value of formula (3) is set to 1.0 or more and 10.0 or less. In order to advance the refinement of the microstructure and increase the isotropy, the value of formula (3) is preferably set to 2.0 or more and 8.5 or less, and more preferably set to 3.0 or more and 7.0 or less.
[0069] By satisfying formula (3), the finish rolling can be performed at a relatively low temperature without excessively lengthening the interpass time, and such rolling can promote the refinement of the microstructure. In addition, by setting the finishing temperature of the finish rolling to 900°C or higher, recrystallization can also be promoted, and as a result, the maximum grain size and in-grain orientation difference of ferrite can be controlled within a desired range. On the other hand, if formula (3) is not satisfied, the refinement of the microstructure by rolling becomes insufficient, and if the finishing temperature of the finish rolling is less than 900°C, recrystallization cannot be promoted sufficiently. In these cases, the maximum grain size and / or in-grain orientation difference of ferrite becomes large, and the uniform elongation and / or limit strain of the finally obtained steel sheet decreases. In order to promote recrystallization sufficiently and thereby increase the isotropy of the microstructure, it is preferable to set the finishing temperature of the finish rolling to 925°C or higher.
[0070] [Cooling process] Next, the obtained steel sheet is air-cooled to 700 ° C. in the cooling process, and then cooled in the temperature range of 700 to 450 ° C. at an average cooling rate of 0.1 to 1.0 ° C. / sec. By using such a cooling history, it is possible to achieve the desired structure fraction and ferrite grain orientation difference, and to reduce the Mn concentration in the cementite that forms the lamellar structure of pearlite to within a desired range. If water cooling is performed at a temperature higher than 700 ° C. after the previous finish rolling process, the ferrite grain orientation difference becomes large, and the desired uniform elongation may not be obtained. In addition, if the temperature range of 700 to 450 ° C. is cooled at an average cooling rate slower than 0.1 ° C. / sec after air cooling, Mn concentration in the cementite will proceed excessively, and such relatively high Mn concentration will easily cause fracture or peeling between the cementite in the pearlite and the surrounding ferrite, and as a result, the limit strain amount of the steel sheet may be reduced. On the other hand, if the temperature range of 700 to 450°C is cooled at an average cooling rate faster than 1.0°C / sec, the formation of pearlite becomes insufficient and structures other than ferrite and pearlite are formed excessively, and the desired microstructure in the steel sheet cannot be obtained.
[0071] According to the steel sheet manufactured by the above manufacturing method, the microstructure of the steel sheet can be composed of a composite structure containing mainly ferrite and hard pearlite in a predetermined ratio, i.e., ferrite: 80% or more and pearlite: 5% or more, thereby improving both the uniform elongation and the limit strain. Furthermore, since the intragranular orientation difference of ferrite can be reduced to 1.0 degree or less, a ferrite structure with fewer dislocations can be realized, and in connection with this, the uniform elongation of the steel sheet can be significantly improved. In addition, the maximum crystal grain size and maximum aspect ratio of ferrite can be reduced to 30.0 μm or less and 3.00 or less, respectively, while the maximum long diameter of the island regions of pearlite that are dispersed in an island shape between ferrite grains can be reduced to 20.0 μm or less, further, the Mn concentration in the cementite that forms the lamellar structure of the pearlite can be reduced to 0.05 or less, and the density of elongated inclusions that are the starting points of the generation of coarse voids in the microstructure can be reduced to 1.0×105 pieces / m 2 Since the strain of the steel plate can be reduced to or below 100%, the critical strain of the steel plate can be significantly improved. Therefore, according to the steel plate manufactured by the above manufacturing method, the occurrence of ductile cracks due to strain concentration can be suppressed due to the improvement in uniform elongation, and even if ductile cracks occur, the propagation of the ductile cracks can be suppressed due to the improvement in the critical strain. Therefore, such a steel plate can significantly suppress the occurrence and propagation of cracks on the surface of the strain concentration part during a collision, so it is useful for suppressing the occurrence of holes during a collision, and is particularly useful for application to structures that are at risk of collision with ships or the like on the ocean, such as ships, floating bodies, and marine structures.
[0072] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way. EXAMPLES
[0073] In the following examples, steel sheets according to the embodiments of the present invention were produced under various conditions, and the properties of the resulting steel sheets, such as uniform elongation and limit strain amount (reduction of area), were investigated.
[0074] Molten steel having the chemical composition shown in Table 1 was subjected to the casting process, heating process, rough rolling process, finish rolling process, and cooling process under the conditions shown in Table 2 to obtain steel plates as examples including invention examples and comparative examples. In Table 2, the cumulative reduction in the casting process indicates the cumulative reduction during the period from when the center of the slab in the thickness direction solidified to when the temperature never dropped below 1200°C, and the cumulative reduction in the rough rolling process indicates the cumulative reduction in the temperature range of 1000°C or higher. In the cooling process, the obtained steel plate was air-cooled to 700°C, and then cooled in the temperature range of 700 to 450°C at the average cooling rate shown in Table 2.
[0075] [Table 1]
[0076] [Table 2]
[0077] [Characteristics evaluation] For the tensile tests, tensile test pieces (JIS14A test pieces taken with the longitudinal direction in the C direction) with a parallel part diameter of 6.0 mm and a parallel part length of 32 mm were taken from 3 / 8 of the plate thickness of the steel plate, the strain gauge length was set to 24.0 mm, and the tensile properties of YS (0.2% yield strength), TS (tensile strength), EL (total elongation), UEL (uniform elongation), and reduction of area were evaluated in accordance with JIS Z 2241:2011. Examples with a UEL of 15% or more and a reduction of area of 75% or more were judged to pass (steel plates with improved uniform elongation and ultimate strain).
[0078] [Table 3]
[0079] The evaluation results of the microstructure and properties are shown in Table 3. In the volume fraction in Table 3, "other" refers to the total of martensite, bainite, bainitic ferrite, and retained austenite. Additionally, the "maximum long diameter" of pearlite in Table 3 refers to the maximum long diameter of the island regions made of pearlite, and similarly, "Mn enrichment" refers to the Mn enrichment in the cementite that forms the lamellar structure of pearlite.
[0080] Among the examples shown in Tables 1 to 3, Experiment No. 58 is a comparative example in which the chemical composition of the steel sheet did not satisfy formula (1), the misorientation in the ferrite grains became excessively large, and uniform elongation was impaired. Experiments Nos. 59 and 60 are comparative examples in which the total amount of elements such as Ca and Mg was not controlled within the desired range, resulting in the occurrence of coarse elongated inclusions and impaired reduction of area. Experiments Nos. 61 and 62 are comparative examples in which the C and Si contents were high, respectively, so that the desired volume fraction of the microstructure associated with high strength was not obtained, and uniform elongation and reduction of area were impaired.
[0081] Experiment No. 8 is a comparative example in which the rolling in the casting process was insufficient, the microstructure was coarsened, and a large amount of coarse elongated inclusions was included, resulting in a loss of reduction in area.
[0082] Experiment No. 4 is a comparative example in which the maximum heating temperature in the heating process was low, coarse island pearlite was generated, and the reduction in area was impaired. On the other hand, Experiment No. 34 is a comparative example in which the maximum heating temperature in the heating process was high, coarse ferrite was generated, and the reduction in area was impaired. Experiment No. 27 is a comparative example in which the value of formula (2) was small in the heating process, coarse island pearlite was generated, and the reduction in area was impaired. On the other hand, Experiment No. 47 is a comparative example in which the value of formula (2) was large in the heating process, coarse and elongated ferrite was generated, and the reduction in area was impaired.
[0083] Experiment No. 52 is a comparative example in which the reduction ratio in the rough rolling step was small, resulting in the generation of coarse ferrite and the reduction in area being impaired.
[0084] Test No. 55 is a comparative example in which the value of formula (3) was small in the finish rolling process, resulting in the generation of coarse ferrite elongated in one direction and the reduction in area was impaired. On the other hand, Test No. 24 is a comparative example in which the value of formula (3) was large in the finish rolling process, resulting in a large misorientation within the ferrite grains and the impairment of uniform elongation. Experiment No. 13 is a comparative example in which the rolling completion temperature in the finish rolling process was low, causing a large misorientation within the ferrite crystal grains and impairing uniform elongation.
[0085] Experiment No. 42 is an example in which water cooling was performed after the completion of finish rolling (an example in which air cooling to 700°C was not performed), and is a comparative example in which the orientation difference within the ferrite crystal grains became large and uniform elongation was impaired. Experiment No. 31 is a comparative example in which the cooling rate in the cooling process was slow, causing excessive Mn concentration in the cementite that constitutes the pearlite lamellae, and thus impairing the reduction of area. On the other hand, Experiment No. 18 is a comparative example in which the cooling rate in the cooling process was fast, causing a large amount of structures other than ferrite and pearlite to be generated, and thus impairing the reduction of area.
[0086] The other examples are steel sheets manufactured under the conditions of the present invention, and are examples (invention examples) that exhibit excellent properties.
Claims
1. The chemical composition, in mass%, is C: 0.060-0.240%, Si: 1.25% or less, Mn: 0.50 to 1.75%, P: 0.030% or less, S: 0.0030% or less, N: 0.0150% or less, O: 0.0030% or less, Al: 1.000% or less, Ti: 0 to 0.060%, Nb: 0 to 0.040%, V: 0-1.00%, Cu: 0-2.00%, Ni: 0-5.00%, Cr: 0-2.00%, Mo: 0-1.00%, W: 0-1.00%, B: 0 to 0.0050%, Sn: 0-1.000%, Sb: 0 to 0.200%, The total of one or more of Ca, Mg, Zr, La, Ce, Te, Hf, and REM: 0.0008 to 0.0050%, and The balance is composed of Fe and impurities. The following formula (1) is satisfied: The microstructure in the range from the surface to the position of 1 / 8 of the plate thickness in the plate thickness direction to the position of 3 / 8 of the plate thickness in the plate thickness direction from the surface is, in terms of volume fraction, Ferrite: 80% or more, Perlite: 5% or more, and The sum of martensite, bainite, bainitic ferrite and retained austenite: 0 to 3%; The maximum grain size of the ferrite is 30 μm or less, The maximum aspect ratio of the ferrite is 3.00 or less, The ferrite grain orientation difference is 1.0 degree or less, The maximum major axis of the island region made of pearlite is 20 μm or less, The Mn concentration in the cementite forming the lamellar structure of the pearlite is 0.050 or less, and The density of the elongated inclusion is 1.0×10 5 pieces / m 2 A steel plate characterized in that: 2.44×10 -2 ×(1.00 - 0.20[Si] + 7.00[Nb])×(1.00 - 10[B] 0.5 )×(117 + 17[Si] + 11[Si] 2 - 33[Mn] + 4[Mn] 2 + 79[Al] + 59[Al] 2 - 26[Ni] - 12[Cr])×(1 + 1.3[Si] + 0.8[Mo] 0.5 + 35[Nb]) -1 ≥1.00 ··· Formula (1) Here, [Si], [Nb], [B], [Mn], [Al], [Ni], [Cr] and [Mo] are the contents [mass %] of each element, and are 0 when the element is not contained.
2. The chemical composition, in mass%, Ti: 0.008-0.030%, Nb: 0.005-0.025%, V: 0.05-0.60%, Cu: 0.05-1.00%, Ni: 0.15-2.30%, Cr: 0.10-1.00%, Mo: 0.03-0.50%, W: 0.03-0.50%, B: 0.0005-0.0025%, Sn: 0.015-0.300%, Sb: 0.005-0.080%, The steel sheet according to claim 1 , further comprising one or more selected from the following:
3. A casting process comprising: casting a slab having the chemical composition according to claim 1 or 2; and rolling the slab by a cumulative amount of 20% or more while the temperature of the slab is never lowered below 1200°C after the central portion of the slab in the thickness direction is solidified; A heating step of heating the slab, the maximum heating temperature of the slab being 1120 to 1250° C., and satisfying the following formula (2): a rough rolling step of rough rolling the slab so that a cumulative rolling reduction in a temperature range of 1000° C. or higher is 35% or more; A finish rolling step in which the obtained rolled material is subjected to finish rolling, in which the rolling in a temperature range of 1000° C. or less satisfies the following formula (3) and the finish rolling completion temperature is 900° C. or more; and A cooling process in which the obtained steel plate is air-cooled to 700°C, and then cooled in the temperature range of 700 to 450°C at an average cooling rate of 0.1 to 1.0°C / sec. A method for producing a steel sheet, comprising: [0010] X i and t i is a value calculated for each of ten equal intervals during which the temperature is 1100° C. or higher, t is the length of each of the 10 equal time intervals [seconds], T i is the slab temperature at the end of heating the i-th section among 10 equal sections, [Nb] is the Nb content [mass%] of the steel plate, R is the cumulative rolling reduction rate [%] in the casting process, A 1 , A 2 , A 3 , A 4 , A 5 , A 6 , A 7 and A 8 are constants, 9.43×10 -1 , −3.50×10 4 , 1.65×10 3 , 1.12×10 0 , 7.01×10 4 , 5.46×10 2 , 4.30×10 2 and 1.10 x 10 1 and X 10 According to the above formula, 1 From X 2 , X 3 This can be obtained by calculating in this order. [0025] Formula (3) is a formula for evaluating and integrating the degree of recrystallization and grain growth after the i-th rolling pass for n passes of rolling performed in a temperature range of 1000 ° C. or less, and m i , the elapsed time t between the i-th and i+1-th rolling passes i [sec], plate thickness h before the i-th rolling i-1 Plate thickness after the above process h i is obtained using m i is the steel plate temperature T in the i-th rolling pass i [°C] and the Nb content [Nb] [mass%] of the steel sheet, The elapsed time t until the next rolling pass for the nth rolling n [Seconds] is the elapsed time from the completion of the nth rolling until the steel sheet temperature reaches 900°C, B 1 , B 2 , B 3 , B 4 , B 5 and B 6 are constants, each of which is 1.50 × 10 1 , −5.00×10 -1 , 7.50 x 10 -11 , 3.50×10 4 , 2.73×10 2 and 4.75 x 10 1 It is.
Citation Information
Patent Citations
Low-yield-ratio high-strength steel sheet excellent in ductile fracture resistance performance
JP2013139602A
High-strength and high-ductility thick steel plate and production method thereof
JP2016125077A
Low-strength thick steel sheet having excellent elongation properties and corrosion resistance