Positive electrode active material, method of producing positive electrode active material, and lithium ion secondary battery
A method for producing Li-containing oxide particles with controlled composition and structure addresses capacity limitations in O2 type positive electrode active materials, resulting in enhanced performance in lithium ion secondary batteries.
Patent Information
- Application Number
- JP2023065097
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-12
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-04-12
AI Technical Summary
Conventional positive electrode active materials with an O2 type structure have limited capacity.
A positive electrode active material with a specific chemical composition and structure, including Li-containing oxide particles with a controlled particle size and X-ray diffraction peak intensity ratio, is produced through a method involving precursor preparation, Na coating, and ion exchange to achieve an O2 type structure.
The resulting material exhibits enhanced capacity due to reduced residual Na and minimized O3 type structure, leading to improved performance in lithium ion secondary batteries.
Smart Images

Figure 2024151614000001_ABST
Abstract
Description
[Technical field]
[0001] The present application discloses a positive electrode active material, a method for producing the positive electrode active material, and a lithium ion secondary battery. [Background technology]
[0002] Positive electrode active materials having an O2 type structure are known. As disclosed in Patent Document 1, a positive electrode active material having an O2 type structure is obtained by ion-exchanging at least a part of Na in a Na-containing oxide having a P2 type structure with Li. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2010-092824 A Summary of the Invention [Problem to be solved by the invention]
[0004] Conventional positive electrode active materials having an O2-type structure have room for improvement in terms of capacity. [Means for solving the problem]
[0005] The present application discloses the following aspects as means for solving the above problems. <Aspect 1> A positive electrode active material comprising Li-containing oxide particles, The Li-containing oxide particles have an O2 type structure, The Li-containing oxide particles are a Na b Mn x-p Ni y-q Co z-r M p+q+rO2 (where 0 < a ≤ 1.00, 0 ≤ b < 0.01, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W). It has a chemical composition represented by The particle size D50 of the Li-containing oxide particles is more than 0 μm and 3.0 μm or less, The particle size D90 of the Li-containing oxide particles is 2.0 μm or more and 6.0 μm or less, The X-ray diffraction pattern of the Li-containing oxide particles satisfies 0 ≤ I2 / I1 ≤ 0.5, The I1 is the X-ray diffraction peak intensity derived from the (002) plane of the O2-type structure, The I2 is the X-ray diffraction peak intensity derived from the (003) plane of the O3-type structure, A positive electrode active material. <Aspect 2> The positive electrode active material of Aspect 1, wherein The particle size D10 of the Li-containing oxide particles is more than 0 μm and 2.0 μm or less, A positive electrode active material. <Aspect 3> A method for manufacturing a positive electrode active material, comprising: Obtaining precursor particles containing at least one element among Mn, Ni, and Co; Coating the surface of the precursor particles with a Na source to obtain composite particles; Subjecting the composite particles to a main firing to obtain Na-containing oxide particles having a P2-type structure; and Contacting the Na-containing oxide particles with an ion exchange material to ion-exchange Na in the Na-containing oxide particles with Li to obtain Li-containing oxide particles having an O2-type structure. The main firing temperature is 700°C or more and less than 950°C, The particle size D50 of the Na-containing oxide particles is more than 0 μm and 3.0 μm or less, The particle size D90 of the Na-containing oxide particles is 2.0 μm or more and 6.0 μm or less, The ion exchange temperature is equal to or higher than the melting point of the ion exchange material and equal to or lower than 300° C. The ion exchange time is 30 minutes or more and less than 3 hours. Manufacturing method. <Aspect 4> The method of production of embodiment 3, The particle diameter D10 of the Na-containing oxide particles is more than 0 μm and 2.0 μm or less. Cathode active material. <Aspect 5> A lithium ion secondary battery having a positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, The positive electrode active material layer includes the positive electrode active material of embodiment 1 or 2. Lithium-ion secondary battery. Effect of the Invention
[0006] The positive electrode active material of the present disclosure has an O2 type structure and has a large capacity. [Brief description of the drawings]
[0007] [Figure 1] 1 shows an example of a flow of a method for producing a Li-containing oxide having an O2 type structure. [Diagram 2] 1 illustrates a schematic configuration of a lithium ion secondary battery. [Diagram 3] 1 shows an X-ray diffraction pattern of the positive electrode active material of Example 1. [Figure 4] 1 shows the X-ray diffraction patterns of the positive electrode active materials of Comparative Examples 1 to 3. [Diagram 5] 1 shows the X-ray diffraction patterns of the positive electrode active materials of Comparative Examples 4 and 5. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] 1.Cathode active material The positive electrode active material according to one embodiment includes Li-containing oxide particles. The Li-containing oxide particles have an O2 type structure. The Li-containing oxide particles include Li a Na b Mnx-p Ni y-q Co z-r M p+q+r O₂ (where 0 < a ≤ 1.00, 0 ≤ b < 0.01, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W). It has a chemical composition represented by the formula. The particle size D50 of the Li-containing oxide particles is more than 0 μm and 3.0 μm or less. The particle size D90 of the Li-containing oxide particles is 2.0 μm or more and 6.0 μm or less. The X-ray diffraction pattern of the Li-containing oxide particles satisfies 0 ≤ I2 / I1 ≤ 0.5. Here, I1 is the X-ray diffraction peak intensity derived from the (002) plane of the O₂-type structure, and I2 is the X-ray diffraction peak intensity derived from the (003) plane of the O3-type structure.)
[0009] 1.1 Crystal Structure The Li-containing oxide particles according to one embodiment have, as a crystal structure, at least an O₂-type structure (belonging to the space group P63mc). The Li-containing oxide particles according to one embodiment may have an O₂-type structure and a crystal structure other than the O₂-type structure. Examples of the crystal structure other than the O₂-type structure include, for example, the T♯2-type structure (belonging to the space group Cmca) formed when Li is deintercalated / inserted from the O₂-type structure, the O6-type structure (belonging to the space group R-3m, the c-axis length is 2.5 nm or more and 3.5 nm or less, typically 2.9 nm or more and 3.0 nm or less, and is different from the O3-type structure also belonging to the space group R-3m), and the like. However, as will be described later, the Li-containing oxide particles according to the embodiment substantially do not contain the O3-type structure, or even if they contain it, it is very small. The Li-containing oxide particles according to one embodiment may have an O₂-type structure as the main phase. The Li-containing oxide particles according to one embodiment may have a T♯2-type structure together with the O₂-type structure. The crystal structure that becomes the main phase of the Li-containing oxide particles according to the embodiment can also change depending on its charge / discharge state.)
[0010] As described later, the Li-containing oxide particles having an O2 type structure are produced by ion-exchanging Na of the Na-containing oxide particles having a P2 type structure with Li. According to the findings of the present inventors, when the particle diameter of the Na-containing oxide particles is large, Na is likely to remain in the Li-containing oxide particles after ion exchange. On the other hand, when the particle diameter of the Na-containing oxide particles is small, Na is unlikely to remain, but if the ion exchange time is not appropriate, the O3 type structure is likely to be generated together with the O2 type structure in the Li-containing oxide particles after ion exchange. According to the findings of the present inventors, when the O3 type structure is contained in the Li-containing oxide particles in large amounts, the capacity as a positive electrode active material decreases. In other words, the lower the X-ray diffraction peak derived from the O3 type structure is relative to the X-ray diffraction peak derived from the O2 type structure, the higher the capacity as a positive electrode active material.
[0011] In the Li-containing oxide particles according to one embodiment, when the X-ray diffraction pattern is obtained, the ratio I2 / I1 of the X-ray diffraction peak intensity I2 derived from the (003) plane of the O3 type structure to the X-ray diffraction peak intensity I1 derived from the (002) plane of the O2 type structure is sufficiently small, 0.5 or less, so that the capacity as a positive electrode active material is large. The X-ray diffraction pattern may satisfy 0≦I2 / I1≦0.4, 0≦I2 / I1≦0.3, 0≦I2 / I1≦0.2, 0≦I2 / I1≦0.1, or I2 / I1=0. In the present application, the terms "X-ray diffraction pattern of the Li-containing oxide particles" and "X-ray diffraction peak intensity" refer to those obtained under the following conditions. That is, an X-ray diffraction pattern is obtained by performing 2θ / θ scanning with CuKα as a radiation source, a tube voltage of 45 kV, a tube current of 200 mA, a step width of 0.02°, and a scan speed of 1° / min, using an X-ray diffraction device (Rigaku, fully automated multipurpose X-ray diffraction device SmartLab). From the X-ray diffraction pattern, the X-ray diffraction peak derived from the (002) plane of the O2 type structure and the X-ray diffraction peak derived from the (003) plane of the O3 type structure are identified, and the I2 / I1 ratio can be calculated from the intensity of each X-ray diffraction peak after subtracting the background value near the peak. The position of the X-ray diffraction peak derived from the (002) plane of the O2 type structure and the position of the X-ray diffraction peak derived from the (003) plane of the O3 type structure may change depending on the Li amount and transition metal composition.
[0012] 1.2 Chemical composition The Li-containing oxide particles according to one embodiment include Li a Na b Mn x-p Ni y-q Co z-r M p+q+rO2 (where 0 < a ≤ 1.00, 0 ≤ b < 0.01, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W). When the Li-containing oxide particles have such a chemical composition, the O2-type structure is easily maintained. Also, since the composition ratio b of Na is less than 0.01, the Na remaining in the Li-containing oxide particles is sufficiently reduced, and the reversible capacity as a positive electrode active material increases. In the above chemical composition, a is greater than 0, and may be 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, 0.50 or more, or 0.60 or more, and is at most 1.00, and may be 0.90 or less, 0.80 or less, or 0.70 or less. Also, b is at most 0.01 and may be 0.00. Also, x is 0 or more, and may be 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, or 0.50 or more, and is at most 1.00, and may be 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, or 0.50 or less. Also, y is 0 or more, and may be 0.10 or more or 0.20 or more, and is at most 1.00, and may be 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, 0.30 or less, or 0.20 or less. Also, z is 0 or more, and may be 0.10 or more, 0.20 or more, or 0.30 or more, and is at most 1.00, and may be 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, or 0.30 or less. The element M has little contribution to charge and discharge. In this regard, in the above chemical composition, since p + q + r is less than 0.17, a high capacity is easily ensured. p + q + r may be 0.16 or less, 0.15 or less, 0.14 or less, 0.13 or less, 0.12 or less, 0.11 or less, or 0.10 or less. On the other hand, when the element M is included, the O2-type structure is easily stabilized. Also, the presence of the element M does not substantially affect the problem-solving mechanism by the positive electrode active material of the present disclosure. That is, regardless of the presence of the element M, since there is little O3-type structure and little remaining Na in the Li-containing oxide particles, the reversible capacity as a positive electrode active material can be improved.In the above chemical composition, p+q+r is 0 or more, and may be 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, 0.05 or more, 0.06 or more, 0.07 or more, 0.08 or more, 0.09 or more, or 0.10 or more. The composition of O is approximately 2, but is not necessarily exactly 2.0 and is indefinite.
[0013] 1.3 Particle size The particle diameter D50 of the Li-containing oxide particles according to an embodiment is more than 0 μm and 3.0 μm or less, and the particle diameter D90 is 2.0 μm or more and 6.0 μm or less. The Li-containing oxide particles having such D50 and D90 tend to have a small amount of Na remaining (the b in the chemical composition is less than 0.01) as described above. The particle diameter D50 of the Li-containing oxide particles may be 0.2 μm or more and 2.8 μm or less, 0.4 μm or more and 2.6 μm or less, 0.6 μm or more and 2.4 μm or less, 0.8 μm or more and 2.2 μm or less, or 1.0 μm or more and 2.0 μm or less. The particle diameter D90 of the Li-containing oxide particles may be 2.3 μm or more and 5.5 μm or less, 2.5 μm or more and 5.0 μm or less, 2.7 μm or more and 4.5 μm or less, or 2.9 μm or more and 4.0 μm or less. The particle diameter D10 of the Li-containing oxide particles according to an embodiment may be more than 0 μm and not more than 2.0 μm. The particle diameter D10 may be 0.1 μm or more and not more than 1.9 μm, 0.2 μm or more and not more than 1.8 μm, 0.3 μm or more and not more than 1.7 μm, 0.4 μm or more and not more than 1.6 μm, or 0.5 μm or more and not more than 1.5 μm. In the present application, the term "particle diameter D50" refers to a particle diameter (median diameter) at an integrated value of 50% in a volume-based particle size distribution by a laser diffraction / scattering method, the term "particle diameter D90" refers to a particle diameter at an integrated value of 90% in a volume-based particle size distribution by a laser diffraction / scattering method, and the term "particle diameter D10" refers to a particle diameter at an integrated value of 10% in a volume-based particle size distribution by a laser diffraction / scattering method.
[0014] 1.4 Shape As described later, the Li-containing oxide particles having an O2 type structure can be obtained by substituting Li for Na in the Na-containing oxide particles having a P2 type structure. Here, the P2 type structure is a hexagonal crystal system, has a large diffusion coefficient of Na ions, and is prone to crystal growth in a specific direction. In particular, when at least one of Mn, Ni, and Co is included as a transition metal element constituting the P2 type structure, the crystals tend to grow in a plate-like shape in a specific direction. Therefore, the Na-containing oxide having the P2 type structure tends to become a plate-like particle with a large aspect ratio in which the crystal growth direction is biased in a specific direction. The Li-containing oxide according to one embodiment may be obtained based on such plate-like Na-containing oxide particles, or may be obtained based on spherical Na-containing oxide particles as described later. That is, the shape of the Li-containing oxide may be a plate-like particle or a spherical particle. When the Li-containing oxide is a spherical particle, the reaction resistance is reduced by reducing the crystallite size, and the diffusion resistance inside the particle is likely to be reduced. Furthermore, when applied to a secondary battery or the like, it is considered that the degree of bending is reduced by spheroidization, and the lithium ion conduction resistance is reduced. This, for example, improves the rate characteristics and tends to increase the reversible capacity. In the present application, the term "spherical particles" refers to particles having a circularity of 0.80 or more. The circularity of the particles may be 0.81 or more, 0.82 or more, 0.83 or more, 0.84 or more, 0.85 or more, 0.86 or more, 0.87 or more, 0.88 or more, 0.89 or more, or 0.90 or more. The circularity of the particles is 4πS / L 2 Here, S is the orthogonal projected area of the particle, and L is the perimeter of the orthogonal projected image of the particle. The circularity of a particle can be determined by observing the appearance of the particle with a scanning electron microscope (SEM), a transmission electron microscope (TEM), or an optical microscope. The circularity of multiple particles can be measured as an average value as follows. (1) First, the particle size distribution of the particles is measured. Specifically, the particle size at 10% cumulative value (D10) and the particle size at 90% cumulative value (D90) in the volume-based particle size distribution are determined by a laser diffraction / scattering method. (2) Regarding the appearance of the particles whose particle size distribution has been measured, images are observed using a SEM, TEM, or optical microscope, and from the particles contained in the images, 100 particles are randomly selected that have an equivalent circle diameter (the diameter of a circle having the same area as the orthogonal projected area of the particle) of not less than D10 and not more than D90, as determined in (1). (3) The circularity of each of the 100 extracted particles is determined by image processing, and the average value is regarded as the "circularity of the particle."
[0015] 1.5 Other As described above, the positive electrode active material according to one embodiment has a large capacity by including the specific Li-containing oxide particles. From the viewpoint of further improving the capacity as a positive electrode active material, the content of the Li-containing oxide particles included in the positive electrode active material may be 50% by mass or more and 100% by mass or less, 60% by mass or more and 100% by mass or less, 70% by mass or more and 100% by mass or less, 80% by mass or more and 100% by mass or less, 90% by mass or more and 100% by mass or less, 95% by mass or more and 100% by mass or less, or 99% by mass or more and 100% by mass or less, based on 100% by mass of the entire positive electrode active material, and the positive electrode active material may be made of the specific Li-containing oxide particles.
[0016] 2. Manufacturing method of positive electrode active material The Li-containing oxide particles according to the above embodiment can be produced, for example, by the following method. As shown in FIG. 1, the method for producing a positive electrode active material according to one embodiment includes the steps of: S1: Obtaining precursor particles containing at least one element of Mn, Ni and Co; S2: Coating the surface of the precursor particles with a Na source to obtain composite particles; S3: subjecting the composite particles to a main calcination process to obtain Na-containing oxide particles having a P2 type structure; and S4: contacting the Na-containing oxide particles with an ion exchange material to ion-exchange the Na in the Na-containing oxide particles with Li, thereby obtaining Li-containing oxide particles having an O2 type structure. The temperature of the main firing is 700° C. or more and less than 950° C., The particle diameter D50 of the Na-containing oxide particles is more than 0 μm and 3.0 μm or less, The particle diameter D90 of the Na-containing oxide particles is 2.0 μm or more and 6.0 μm or less, The ion exchange temperature is equal to or higher than the melting point of the ion exchange material and equal to or lower than 300° C. The ion exchange time is 30 minutes or more and less than 3 hours.
[0017] 2.1 S1 In S1, precursor particles containing at least one element of Mn, Ni, and Co are obtained. The precursor particles may contain at least Mn, one or both of Ni and Co, or may contain at least Mn, Ni, and Co. The precursor particles may be a salt containing at least one element of Mn, Ni, and Co. For example, the precursor particles may be at least one of carbonate, sulfate, nitrate, and acetate. Alternatively, the precursor particles may be a compound other than a salt. For example, the precursor particles may be a hydroxide. The precursor particles may be a hydrate. The precursor particles may be a combination of a plurality of types of compounds. The particle size of the precursor particles is not particularly limited. In S1, a precipitate as the precursor particles may be obtained by a coprecipitation method using an ion source capable of forming a precipitate in an aqueous solution with a transition metal ion and a transition metal compound containing at least one element of Mn, Ni, and Co. The "ion source capable of forming a precipitate in an aqueous solution together with transition metal ions" may be at least one selected from, for example, sodium salts such as sodium carbonate and sodium nitrate, sodium hydroxide, and sodium oxide. The transition metal compound may be the above-mentioned salts or hydroxides containing at least one element of Mn, Ni, and Co. Specifically, in S1, the ion source and the transition metal compound may be prepared as solutions, and the solutions may be dropped and mixed to obtain a precipitate as precursor particles. In this case, for example, water is used as the solvent. In this case, various sodium compounds may be used as bases, and an ammonia aqueous solution or the like may be added to adjust the basicity. In the case of the coprecipitation method, for example, an aqueous solution of a transition metal compound and an aqueous solution of sodium carbonate are prepared, and the aqueous solutions are dropped and mixed to obtain spherical precursor particles. Alternatively, the precursor particles can be obtained by a sol-gel method. In S1, the precursor particles may contain the element M. The element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W. The element M has a function of stabilizing, for example, the P2 type structure or the O2 type structure.The method for obtaining a precursor containing element M is not particularly limited. When obtaining a precursor by coprecipitation in S1, for example, an aqueous solution of a transition metal compound containing at least one of Mn, Ni, and Co, an aqueous solution of sodium carbonate, and an aqueous solution of a compound of element M are prepared, and each aqueous solution is dropped and mixed to obtain a precursor containing element M together with at least one element of Mn, Ni, and Co. Alternatively, in the manufacturing method of the present disclosure, element M may not be added in S1, and element M may be doped when Na-doping baking is performed in S2 and S3 described later.
[0018] 2.2 S2 In S2, the surface of the precursor particle obtained in S1 is coated with a Na source to obtain a composite particle. The Na source may be a salt containing Na, such as a carbonate or a nitrate, or a compound other than a salt, such as sodium oxide or sodium hydroxide. In S2, the amount of the Na source coated on the surface of the precursor particle may be determined taking into account the amount of Na lost during the subsequent firing. In S2, the coverage rate of the Na source on the surface of the precursor is not particularly limited. For example, in S2, the composite particle may be obtained by coating 40 area% or more, 50 area% or more, 60 area% or more, or 70 area% or more of the surface of the precursor particle with a Na source. If the coverage rate of the Na source is small, when the composite particle is fired, the P2 type crystals tend to grow in a specific direction on the surface of the composite particle, and the Na-containing oxide tends to become plate-like. If the coverage rate of the Na source is large, when the composite particle is fired, the crystallites of the P2 type crystals tend to become small, and the Na-containing oxide particles tend to correspond to the shape of the precursor particle. In S2, the method of coating the surface of the precursor particle with the Na source is not particularly limited. As described above, when 40% or more of the surface of the precursor particle is coated with the Na source, the method can be, for example, a rolling fluidized coating method or a spray drying method. That is, a coating solution in which a Na source is dissolved is prepared, and the coating solution is brought into contact with the surface of the precursor particle, and dried at the same time or after the contact. By adjusting the coating conditions (temperature, time, number of times, etc.), 40% or more of the surface of the precursor particle can be coated with the Na source. In S2, the precursor particle may be coated with the M source together with the Na source. For example, in S2, the precursor particle obtained by S1, the Na source, and the M source containing the element M may be mixed to obtain a composite particle. The M source may be, for example, a salt containing the element M, such as a carbonate or sulfate, or a compound other than a salt, such as an oxide or hydroxide.
[0019] 2.3 S3 In S3, the composite particles obtained in S2 are subjected to a main firing process to obtain Na-containing oxide particles having a P2 type structure. S3 may include the following S3-1 to S3-3.
[0020] In S3-1, the composite particles are pre-baked at a temperature of 300° C. or more and less than 700° C. for 2 hours or more and 10 hours or less. The pre-baking temperature may be 400° C. or more and less than 700° C., 450° C. or more and less than 700° C., 500° C. or more and less than 700° C., 550° C. or more and less than 700° C., or 550° C. or more and less than 650° C. The pre-baking time may be 2 hours or more and less than 8 hours, 3 hours or more and less than 8 hours, 4 hours or more and less than 8 hours, 5 hours or more and less than 8 hours, or 5 hours or more and less than 7 hours. The pre-baking atmosphere is not particularly limited, and may be, for example, an oxygen-containing atmosphere.
[0021] In S3-2, the composite particles are subjected to main firing following the above preliminary firing. The main firing temperature is 700°C or more and less than 950°C, and may be 800°C or more and 920°C or less. If the main firing temperature is too low, the P2 phase is not generated. If the main firing temperature is too high, Na is likely to remain after ion exchange in S4. The temperature rise condition from the preliminary firing temperature to the main firing temperature is not particularly limited. The main firing time is not particularly limited, and may be, for example, 30 minutes to 48 hours, 30 minutes to 24 hours, 30 minutes to 10 hours, or 30 minutes to 3 hours. However, the shape of the Na-containing oxide can be controlled by the main firing time. As described above, in the method of the present disclosure, when the coverage rate of the Na source in the composite particles is 40 area % or more, when the composite particles are fired, P2 type crystals with small crystallites are likely to be formed on the surface. In the method of the present disclosure, the P2 type crystals are grown along the surface of the particles so as to connect one P2 type crystallite with another P2 type crystallite, so that the shape of the Na-containing oxide particles corresponds to the shape of the precursor particles. For example, if the precursor particles are spherical, the Na-containing oxide particles may also be spherical. If the firing time is too short, the generation of the P2 phase is insufficient. On the other hand, if the firing time is too long, the P2 phase grows and the particles become plate-like rather than spherical. As far as the inventors have confirmed, if the firing time is 30 minutes or more and 3 hours or less, the Na-containing oxide particles are likely to become spherical. The Na-containing oxide particles obtained after firing may have a structure in which a plurality of crystallites are present on the surface and the crystallites are connected to each other.
[0022] In step S3-3, following the main firing, the composite particles after the main firing are rapidly cooled (cooled at a temperature drop rate of 20°C / min or more) from a temperature T1 of 200°C or more to a temperature T2 of 100°C or less. The preliminary firing and main firing are performed, for example, in a heating furnace. In step S3-3, for example, after the main firing of the composite is performed in a heating furnace, it is cooled to an arbitrary temperature T1 of 200°C or more in the heating furnace, and after the temperature T1 is reached, the fired product is removed from the heating furnace and rapidly cooled to an arbitrary temperature T2 of 100°C or less outside the furnace. The temperature T1 may be an arbitrary temperature of 200°C or more, or an arbitrary temperature of 250°C or more. The temperature T2 may be an arbitrary temperature of 100°C or less, or an arbitrary temperature of 50°C or less, or may be the cooling end temperature. In a certain temperature range between the temperature T1 and the temperature T2, moisture is likely to penetrate between the layers of the P2 type structure due to atomic vibration, molecular motion, etc. When cooling the composite particles (Na-containing oxide particles having a P2 type structure) after the main firing, it is considered that the amount of moisture that penetrates between the layers of the P2 type structure is reduced by shortening the time in which the temperature range in which moisture easily penetrates (i.e., by cooling quickly). In this regard, in S3-3, when cooling the composite after the main firing, the cooling rate from temperature T1 of 200°C or higher to temperature T2 of 100°C or lower is high (e.g., 20°C / min or higher) during the period from temperature T1 to temperature T2 is high, moisture is less likely to penetrate between the layers of the P2 type structure, and the collapse of the P2 type structure can be suppressed. As a result, Na can be efficiently ion-exchanged with Li in S4, and the amount of Na remaining after ion exchange is easily reduced.
[0023] By the above method, it is possible to produce Na-containing oxide particles having a P2 type structure and a predetermined chemical composition. c Mn x-p Ni y-q Co z-r M p+q+rThe Na-containing oxide particles may have a chemical composition represented by O2. Here, 0.10≦c≦1.00, x+y+z=1, and 0≦p+q+r<0.17. M is at least one element selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W. When the Na-containing oxide particles have such a chemical composition, the P2 type structure is easily maintained. In the above chemical composition, c may be 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, 0.50 or more, or 0.60 or more, and may be 1.00 or less, 0.90 or less, 0.80 or less, or 0.70 or less. x, y, z, p, q, and r are as described above.
[0024] The Na-containing oxide particles obtained by the above method have a particle size distribution. In this embodiment, the precursor particles are classified by airflow classification, the composite particles are classified by airflow classification, or the Na-containing oxide particles are classified by airflow classification, to obtain Na-containing oxide particles having a predetermined D50 and D90, and the Na-containing oxide particles are used in S4 described below. This allows Li-containing oxide particles having a predetermined D50 and D90 to be obtained. Specifically, the particle diameter D50 of the Na-containing oxide particles used in S4 is more than 0 μm and 3.0 μm or less, and the particle diameter D90 is 2.0 μm or more and 6.0 μm or less. The particle diameter D50 may be 0.2 μm or more and 2.8 μm or less, 0.4 μm or more and 2.6 μm or less, 0.6 μm or more and 2.4 μm or less, 0.8 μm or more and 2.2 μm or less, or 1.0 μm or more and 2.0 μm or less. The particle diameter D90 may be 2.3 μm or more and 5.5 μm or less, 2.5 μm or more and 5.0 μm or less, 2.7 μm or more and 4.5 μm or less, or 2.9 μm or more and 4.0 μm or less. The particle diameter D10 of the Na-containing oxide particles may be more than 0 μm and 2.0 μm or less. The particle diameter D10 may be 0.1 μm or more and 1.9 μm or less, 0.2 μm or more and 1.8 μm or less, 0.3 μm or more and 1.7 μm or less, 0.4 μm or more and 1.6 μm or less, or 0.5 μm or more and 1.5 μm or less.
[0025] 2.4 S4 In S4, the Na-containing oxide particles obtained in S3 are brought into contact with an ion exchange material to ion-exchange Na in the Na-containing oxide particles with Li to obtain Li-containing oxide particles having an O2-type structure. Examples of the ion exchange material include a mixture of lithium halide and other lithium salts (e.g., molten salt). The lithium halide constituting the molten salt is preferably at least one of lithium chloride, lithium bromide, and lithium iodide. The other lithium salt constituting the molten salt is preferably lithium nitrate. By using the molten salt, the melting point becomes lower than when the lithium halide or other lithium salt is used alone, and ion exchange can be performed at a lower temperature. The temperature in the ion exchange is not lower than the melting point of the ion exchange material but not higher than 300°C. If the ion exchange temperature is too high, a stable O3-type structure is likely to be formed instead of an O2-type structure. On the other hand, from the viewpoint of shortening the ion exchange time, the ion exchange temperature is preferably as high as possible. The ion exchange time is 30 minutes or more and less than 3 hours. If the ion exchange time is too short, the amount of Na remaining in the Li-containing oxide particles increases, whereas if the ion exchange time is too long, O3 type structures and the like tend to form in addition to O2 type structures.
[0026] 3. Lithium-ion secondary battery FIG. 2 shows a schematic configuration of a lithium ion secondary battery according to an embodiment. As shown in FIG. 2, a lithium ion secondary battery 100 according to an embodiment has a positive electrode active material layer 10, an electrolyte layer 20, and a negative electrode active material layer 30. Here, the positive electrode active material layer 10 contains the positive electrode active material according to the above embodiment. As shown in FIG. 2, the lithium ion secondary battery 100 may include a positive electrode current collector 40 and a negative electrode current collector 50. In the lithium ion secondary battery 100, the configuration other than the positive electrode active material is the same as that of a conventional battery, and may adopt, for example, the configuration described in Patent Document 1 (JP Patent Publication 2010-092824). EXAMPLES
[0027] As described above, one embodiment of the positive electrode active material, the manufacturing method of the positive electrode active material, and the lithium ion secondary battery has been described, but the technology of the present disclosure can be modified in various ways other than the above embodiment without departing from the gist of the technology. Below, the technology of the present disclosure will be described in more detail while showing examples, but the technology of the present disclosure is not limited to the following examples.
[0028] 1. Preparation of Positive Electrode Active Material 1.1 Example 1 1.1.1 Preparation of precursor particles (1) MnSO4·5H2O, NiSO4·6H2O, and CoSO4·7H2O were weighed out to obtain the desired composition ratio, and dissolved in distilled water to obtain a concentration of 1.2 mol / L to obtain a first solution. In a separate container, Na2CO3 was dissolved in distilled water to obtain a concentration of 1.2 mol / L to obtain a second solution. (2) 1000 mL of pure water was placed in a reaction vessel (with a baffle plate), and 500 mL of the first solution and 500 mL of the second solution were each added dropwise at a rate of about 4 mL / min. (3) After the dropwise addition was completed, the mixture was stirred at room temperature at a stirring speed of 150 rpm for 1 hour to obtain a product. (4) The product was washed with pure water, subjected to solid-liquid separation using a centrifuge, and the precipitate was collected. (5) The obtained precipitate was dried overnight at 120°C, crushed in a mortar, and then separated into coarse particles and fine particles by air classification. Here, both the coarse particles and the fine particles are composite salts containing Mn, Ni, and Co. In Example 1, the above fine particles were used as precursor particles.
[0029] 1.1.2 Preparation of composite particles The precursor particles and Na2CO3 are mixed together to obtain a target composition after calcination, which will be described later. 0.7 Mn 0.5 Ni 0.2 Co 0.3 The surfaces of the precursor particles were coated with Na2CO3 to obtain composite particles.
[0030] 1.1.3 Sintering of composite particles The composite particles were placed in an alumina crucible and sintered in an air atmosphere to obtain a Na-containing oxide having a P2 structure under the following sintering conditions (1) to (7). (1) The alumina crucible containing the composite particles is placed in a heating furnace in an air atmosphere. (2) The temperature inside the heating furnace is raised from room temperature (25°C) to 600°C in 115 minutes. (3) The temperature in the heating furnace is kept at 600°C for 360 minutes to perform pre-baking. (4) After preliminary firing, the temperature inside the heating furnace is raised from 600°C to 900°C in 60 minutes. (5) The temperature in the heating furnace is kept at 900°C for 60 minutes to perform the main firing. (6) After the main firing, the temperature in the heating furnace is lowered from 900°C to 250°C in 130 minutes. (7) At 250°C, the alumina crucible is removed from the heating furnace and allowed to cool in a dry atmosphere outside the furnace.
[0031] The fired product after cooling was pulverized in a mortar under a dry atmosphere to obtain Na-containing oxide particles A having a P2 type structure. The chemical composition and particle diameters D10, D50 and D90 of the Na-containing oxide particles A are shown in Table 1 below.
[0032] 1.1.4 Ion exchange (1) LiNO3 and LiCl were weighed out to have a molar ratio of 50:50, and mixed with the above-mentioned Na-containing oxide particles A in a molar ratio that was 10 times the minimum Li amount required for ion exchange to obtain a mixture. (2) Using an alumina crucible, ion exchange was carried out at 280°C for 1 hour in an air atmosphere to obtain a product containing Li-containing oxide particles. (3) The salt remaining in the product was washed with pure water, and solid-liquid separation was performed by vacuum filtration to obtain a precipitate. (4) The obtained precipitate was dried overnight at 120° C. to obtain the positive electrode active material according to Example 1.
[0033] 1.2 Comparative Example 1 1.2.1 Preparation of precursor particles and composite particles In the same manner as in Example 1, precursor particles and composite particles were obtained.
[0034] 1.2.2 Sintering of composite particles The composite particles were placed in an alumina crucible and sintered in an air atmosphere to obtain Na-containing oxide particles having a P2 structure under the following sintering conditions (1) to (7). (1) The alumina crucible containing the composite particles is placed in a heating furnace in an air atmosphere. (2) The temperature inside the heating furnace is raised from room temperature (25°C) to 600°C in 115 minutes. (3) The temperature in the heating furnace is kept at 600°C for 360 minutes to perform pre-baking. (4) After preliminary firing, the temperature inside the heating furnace is raised from 600°C to 950°C in 70 minutes. (5) The temperature in the heating furnace is kept at 950°C for 60 minutes to perform the main firing. (6) After the main firing, the temperature in the heating furnace is lowered from 950°C to 250°C in 140 minutes. (7) At 250°C, the alumina crucible is removed from the heating furnace and allowed to cool in a dry atmosphere outside the furnace.
[0035] The fired product after cooling was pulverized in a mortar under a dry atmosphere to obtain Na-containing oxide particles B having a P2 type structure. The chemical composition and particle sizes D10, D50 and D90 of the Na-containing oxide particles B are shown in Table 1 below.
[0036] 1.2.3 Ion exchange Ion exchange was carried out under the same conditions as in Example 1, except that the Na-containing oxide particles B were used instead of the Na-containing oxide particles A, to obtain a positive electrode active material according to Comparative Example 1.
[0037] 1.3 Comparative Example 2 1.3.1 Preparation of precursor particles and composite particles In the same manner as in Example 1, precursor particles and composite particles were obtained.
[0038] 1.3.2 Sintering of composite particles The composite particles were placed in an alumina crucible and sintered in an air atmosphere to obtain a Na-containing oxide having a P2 structure under the following sintering conditions (1) to (7). (1) The alumina crucible containing the composite particles is placed in a heating furnace in an air atmosphere. (2) The temperature inside the heating furnace is raised from room temperature (25°C) to 600°C in 115 minutes. (3) The temperature in the heating furnace is kept at 600°C for 360 minutes to perform pre-baking. (4) After preliminary firing, the temperature inside the heating furnace is raised from 600°C to 1000°C in 80 minutes. (5) The temperature in the heating furnace is kept at 1000°C for 60 minutes to perform the main firing. (6) After the main firing, the temperature in the heating furnace is lowered from 1000°C to 250°C in 150 minutes. (7) At 250°C, the alumina crucible is removed from the heating furnace and allowed to cool in a dry atmosphere outside the furnace.
[0039] The fired product after cooling was pulverized in a mortar under a dry atmosphere to obtain Na-containing oxide particles C having a P2 type structure. The chemical composition and particle diameters D10, D50 and D90 of the Na-containing oxide particles C are shown in Table 1 below.
[0040] 1.3.3 Ion exchange Ion exchange was carried out under the same conditions as in Example 1, except that the Na-containing oxide particles C were used instead of the Na-containing oxide particles A, to obtain a positive electrode active material according to Comparative Example 2.
[0041] 1.4 Comparative Example 3 1.4.1 Preparation of precursor particles and composite particles Precursor particles and composite particles were obtained in the same manner as in Example 1, except that the above-mentioned coarse particles were used as the precursor particles.
[0042] 1.4.2 Sintering of composite particles The composite particles were placed in an alumina crucible and sintered in an air atmosphere to obtain a Na-containing oxide having a P2 structure under the following sintering conditions (1) to (7). (1) The alumina crucible containing the composite particles is placed in a heating furnace in an air atmosphere. (2) The temperature inside the heating furnace is raised from room temperature (25°C) to 600°C in 115 minutes. (3) The temperature in the heating furnace is kept at 600°C for 360 minutes to perform pre-baking. (4) After preliminary firing, the temperature inside the heating furnace is raised from 600°C to 1000°C in 80 minutes. (5) The temperature in the heating furnace is kept at 1000°C for 1440 minutes to carry out the main firing. (6) After the main firing, the temperature in the heating furnace is lowered from 1000°C to 250°C in 150 minutes. (7) At 250°C, the alumina crucible is removed from the heating furnace and allowed to cool in a dry atmosphere outside the furnace.
[0043] The fired product after cooling was pulverized in a mortar under a dry atmosphere to obtain Na-containing oxide particles D having a P2 type structure. The chemical composition and particle diameters D10, D50 and D90 of the Na-containing oxide particles D are as shown in Table 1 below.
[0044] 1.4.3 Ion exchange Ion exchange was carried out under the same conditions as in Example 1, except that Na-containing oxide particles D were used instead of Na-containing oxide particles A, to obtain a positive electrode active material according to Comparative Example 3.
[0045] 1.5 Comparative Example 4 1.5.1 Preparation of precursor particles and composite particles, and calcination of composite particles Precursor particles and composite particles were obtained in the same manner as in Example 1, and then the composite particles were fired and pulverized under the same conditions as in Example 1 to obtain Na-containing oxide particles E having a P2 type structure. The chemical composition and particle diameters D10, D50 and D90 of the Na-containing oxide particles E are as shown in Table 1 below.
[0046] 1.5.2 Ion exchange Ion exchange was performed under the same conditions as in Example 1, except that Na-containing oxide particles E were used instead of Na-containing oxide particles A and the ion exchange time was changed from 1 hour to 3 hours, to obtain a positive electrode active material according to Comparative Example 4.
[0047] 1.6 Comparative Example 5 1.6.1 Preparation of precursor particles and composite particles, and calcination of composite particles Precursor particles and composite particles were obtained in the same manner as in Comparative Example 3, and then the composite particles were fired and pulverized under the same conditions as in Comparative Example 3 to obtain Na-containing oxide particles F having a P2 type structure. The chemical composition and particle diameters D10, D50 and D90 of the Na-containing oxide particles F are as shown in Table 1 below.
[0048] 1.6.2 Ion exchange Ion exchange was performed under the same conditions as in Example 1, except that Na-containing oxide particles F were used instead of Na-containing oxide particles A and the ion exchange time was changed from 1 hour to 3 hours, to obtain a positive electrode active material according to Comparative Example 5.
[0049] 2. Evaluation of positive electrode active material 2.1 Elemental analysis Elemental analysis was carried out to identify the chemical composition of each of the positive electrode active materials of Example 1 and Comparative Examples 1 to 5. The results are shown in Table 2 below.
[0050] 2.2 Particle size distribution measurement Particle size distribution measurement was carried out for each of the positive electrode active materials of Example 1 and Comparative Examples 1 to 5, and the particle diameters D10, D50 and D90 were determined. The results are shown in Table 2 below.
[0051] 2.2 Identification of crystal structure by X-ray diffraction measurement For each of the positive electrode active materials of Example 1 and Comparative Examples 1 to 5, an X-ray diffraction measurement was performed using CuKα as a radiation source to obtain an X-ray diffraction pattern. Figures 3 to 5 show the X-ray diffraction patterns of Example 1 and Comparative Examples 1 to 5. As shown in Figures 3 to 5, it can be seen that all of the positive electrode active materials of Example 1 and Comparative Examples 1 to 5 have an O2 type structure. Table 3 below shows the crystal structure contained in each of the positive electrode active materials of Example 1 and Comparative Examples 1 to 5, and the ratio I2 / I1 of the X-ray diffraction peak intensity I2 derived from the (003) plane of the O3 type structure to the X-ray diffraction peak intensity I1 derived from the (002) plane of the O2 type structure.
[0052] 3. Preparation of evaluation cells Coin cells were produced using the positive electrode active materials of Examples 1 and 2 and Comparative Examples 1 and 2. The coin cell was produced as follows. (1) The positive electrode active material, acetylene black (AB) as a conductive additive, and polyvinylidene fluoride (PVdF) as a binder were weighed out so that the mass ratio of the positive electrode active material:AB:PVdF=85:10:5, and dispersed and mixed in N-methyl-2-pyrrolidone to obtain a positive electrode mixture slurry. The positive electrode mixture slurry was applied onto an aluminum foil and vacuum dried overnight at 120°C to obtain a positive electrode, which is a laminate of a positive electrode active material layer and a positive electrode current collector. (2) TDDK-217 (manufactured by Daikin Industries, Ltd.) was prepared as the electrolyte. (3) Metallic lithium foil was prepared as the negative electrode. (4) A coin cell (CR2032) was prepared using the positive electrode, electrolyte, and negative electrode.
[0053] 4.Charge / Discharge Characteristics Evaluation Each coin cell was charged and discharged at 0.1 C (1 C = 220 mA / g) in a voltage range of 2.0-4.8 V in a thermostatic chamber maintained at 25° C., and the discharge capacity was measured. The results are shown in Table 3 below.
[0054] 5. Evaluation Results Table 1 below shows the firing temperature, chemical composition, particle diameters D10, D50, and D90 for each of the Na-containing oxide particles A to F used in Example 1 and Comparative Examples 1 to 5. Table 2 below also shows the ion exchange time, chemical composition, particle diameters D10, D50, and D90 for each of the positive electrode active materials in Example 1 and Comparative Examples 1 to 5. Table 3 below also shows the crystal structure contained in the positive electrode active material, I2 / I1 determined from the X-ray diffraction pattern, and the discharge capacity of the evaluation cell for each of Example 1 and Comparative Examples 1 to 5.
[0055] [Table 1]
[0056] [Table 2]
[0057] [Table 3]
[0058] As is clear from the results shown in Tables 1 to 3, in Comparative Examples 1 to 3, the firing temperature in preparing the Na-containing oxide particles having a P2 structure was too high, so that the ion exchange after firing did not proceed sufficiently, and Na remained in the Li-containing oxide particles. Among them, in Comparative Examples 2 and 3, the particle size of the Na-containing oxide particles after firing was too large, so that the ion exchange did not proceed further, and the amount of Na remaining in the Li-containing oxide particles increased. In Comparative Example 5, the particle size of the Na-containing oxide particles after firing was too large, so that Na remained in the Li-containing oxide particles after ion exchange even if the ion exchange time was extended. In Comparative Example 4, while the particle size of the Na-containing oxide particles after firing was small, the ion exchange time after firing was too long, so that the O3 phase was generated in the Li-containing oxide after ion exchange. Due to these factors, the Li-containing oxide particles according to Comparative Examples 1 to 5 had a lower capacity as a positive electrode active material than the Li-containing oxide particles according to Example 1. In contrast, the Li-containing oxide particles according to Example 1 had a suitable chemical composition, particle size and crystal structure, and therefore had a high capacity as a positive electrode active material.
[0059] 6. Supplementary Information In the above embodiments, the case where precursor particles are obtained by the coprecipitation method has been exemplified. However, the precursor particles can also be obtained by other methods. Further, in the above embodiments, the case where composite particles are obtained by mixing the precursor particles and a Na source (Na2CO3) has been exemplified. However, the composite particles can also be obtained by other methods. Further, in the above embodiments, as the Na-containing oxide having a P2-type structure or the Li-containing oxide having an O2-type structure, those having a predetermined chemical composition have been exemplified. However, the chemical compositions of the Na-containing oxide and the Li-containing oxide are not limited thereto. For example, the Na-containing oxide and the Li-containing oxide may be doped with an element M other than Mn, Ni, and Co. The element M is as described in the embodiment.
[0060] From the above results, it can be said that the Li-containing oxide particles satisfying the following requirements (1) to (5) have a high capacity as a positive electrode active material. (1) The Li-containing oxide particles have an O2-type structure. (2) The Li-containing oxide particles are Li a Na b Mn x-p Ni y-q Co z-r M p+q+r O2 (where 0 < a ≤ 1.00, 0 ≤ b < 0.01, x + y + z = 1, and 0 ≤ p + q + r < 0.17, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W). (3) The particle size D50 of the Li-containing oxide particles is more than 0 μm and 3.0 μm or less. (4) The particle size D90 of the Li-containing oxide particles is 2.0 μm or more and 6.0 μm or less. (5) The X-ray diffraction pattern of the Li-containing oxide particles satisfies 0 ≤ I2 / I1 ≤ 0.5, where I1 is the X-ray diffraction peak intensity derived from the (002) plane of the O2-type structure, and I2 is the X-ray diffraction peak intensity derived from the (003) plane of the O3-type structure.
Explanation of Reference Numerals
[0061] 100 Lithium-ion secondary battery 10 Cathode active material layer 20 Electrolyte layer 30 Negative electrode active material layer 40 Positive electrode current collector 50 Negative electrode current collector
Claims
1. A positive electrode active material comprising Li-containing oxide particles, The Li-containing oxide particles have an O2 type structure, The Li-containing oxide particles include Li a Na b Mn x-p Ni y-q Co z-r M p+q+r O 2 (wherein 0<a≦1.00, 0≦b<0.01, x+y+z=1, and 0≦p+q+r<0.17; and element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W), The particle diameter D50 of the Li-containing oxide particles is more than 0 μm and 3.0 μm or less, The particle diameter D90 of the Li-containing oxide particles is 2.0 μm or more and 6.0 μm or less, The X-ray diffraction pattern of the Li-containing oxide particles is 0≦I 2 / I 1 ≦0.5 is satisfied, I 1 is the X-ray diffraction peak intensity derived from the (002) plane of the O2 type structure, I 2 is the X-ray diffraction peak intensity due to the (003) plane of the O3 type structure, Cathode active material.
2. The positive electrode active material according to claim 1 , The particle diameter D10 of the Li-containing oxide particles is more than 0 μm and 2.0 μm or less. Cathode active material.
3. A method for producing a positive electrode active material, comprising the steps of: Obtaining precursor particles comprising at least one element of Mn, Ni and Co; Coating the surface of the precursor particles with a Na source to obtain composite particles; The composite particles are subjected to a main calcination process to obtain Na-containing oxide particles having a P2 type structure; and and bringing the Na-containing oxide particles into contact with an ion exchange material to ion-exchange the Na in the Na-containing oxide particles with Li to obtain Li-containing oxide particles having an O2-type structure. The temperature of the main firing is 700° C. or more and less than 950° C., The particle diameter D50 of the Na-containing oxide particles is more than 0 μm and 3.0 μm or less, The particle diameter D90 of the Na-containing oxide particles is 2.0 μm or more and 6.0 μm or less, The ion exchange temperature is equal to or higher than the melting point of the ion exchange material and equal to or lower than 300° C. The ion exchange time is 30 minutes or more and less than 3 hours. Manufacturing method.
4. The method according to claim 3, The particle diameter D10 of the Na-containing oxide particles is more than 0 μm and 2.0 μm or less. Cathode active material.
5. A lithium ion secondary battery having a positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer, The positive electrode active material layer comprises the positive electrode active material according to claim 1 or 2. Lithium-ion secondary battery.
Citation Information
Patent Citations
Non-aqueous electrolyte secondary battery
JP2011228273A
Method for producing positive electrode active material and method for manufacturing lithium ion battery
JP2021068555A
All-solid-state battery
JP2022085829A
Positive electrode active material for secondary battery, and secondary battery
WO2021085112A1
Cathode active material for nonaqueous electrolyte secondary battery and nonaqueous electrolyte secondary battery using the same, and method of manufacturint cathode active material for nonaqueous electrolyte secondary battery
JP2010092824A
Cited By
Secondary battery positive electrode active material, secondary battery positive electrode, and secondary battery
WO2026110767A1