Seed coating agent, coated seed and seed coating method
The use of ascorbic acid and erythorbic acid as antioxidants in a seed coating agent for iron-based powder addresses the issue of seed damage from oxidative heat, enhancing seed density and coating strength in coated seeds.
Patent Information
- Application Number
- JP2023065400
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-04-13
AI Technical Summary
Existing coated seeds with increased seed density using iron-based powder face the risk of damage due to heat generated by oxidation of metallic iron, which is exacerbated by higher iron content.
A seed coating agent containing iron-based powder coated with ascorbic acid and erythorbic acid as antioxidants, applied in a ratio of 0.02% to 15% by mass, prevents seed damage from oxidative heat generation while maintaining high seed density.
The solution achieves increased seed density with reduced risk of seed damage, ensuring effective seed retention and improved coating strength.
Smart Images

Figure 2024151755000001 
Figure 2024151755000002 
Figure 2024151755000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a seed coating agent that contains an iron-based powder and coats the surface of a seed, a coated seed whose surface is coated with the seed coating agent, and a seed coating method for coating the surface of a seed using the seed coating agent. [Background technology]
[0002] With the aging of agricultural workers and the globalization of agricultural product distribution, labor saving in agricultural work and reduction of agricultural production costs have become issues that need to be resolved. To address these issues, for example, in rice cultivation, direct seeding, in which seeds are sown directly in fields, is becoming more widespread in order to save the labor of raising seedlings and transplanting. Among these, a technique that uses coated seeds with iron powder on the surface to increase seed density has attracted attention because it has the advantage of preventing seeds from floating or flowing out of paddy fields and preventing bird damage. Examples of coated seeds in which iron powder is coated as described above are disclosed in Patent Documents 1 and 2. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2005-192458 A [Patent Document 2] JP 2017-153427 A Summary of the Invention [Problem to be solved by the invention]
[0004] The coated seeds described above can remain in the location where they were sown by increasing the seed density (specific gravity). However, in actual farm fields, the seeds are exposed to various water currents, and may be washed away if the current is strong. Therefore, coated seeds with a higher seed density were required. In the coated seeds described in Patent Documents 1 and 2, the seed density can be increased by increasing the proportion of iron-based powder per unit mass of the seed. However, there is a problem in that increasing the seed density increases the risk of damage to the seeds due to heat generated by oxidation of metallic iron contained in the iron-based powder.
[0005] The present invention has been made to solve the above-mentioned problems, and aims to provide a seed coating agent, coated seeds, and a seed coating method that can increase the seed density per mass of the iron-based powder while preventing damage to the seeds caused by heat generation due to oxidation of the metallic iron contained in the iron-based powder. [Means for solving the problem]
[0006] In order to solve the above problems, the inventors have investigated various coatings of iron powder on seeds, and have found that coating the seed surface with a seed coating agent containing ascorbic acid, erythorbic acid, or these compounds as antioxidants prevents damage to the seeds caused by heat generation due to oxidation of metallic iron and increases the seed density. The present invention has been made based on the above findings, and has the following configuration.
[0007] (1) The seed coating agent according to the present invention contains an iron-based powder and is used to coat the surface of a seed, The present invention is characterized in that ascorbic acid, erythorbic acid, or one or more of these compounds are added as an antioxidant, and the ratio of the antioxidant to the mass of the iron-based powder is 0.02 mass% or more and 15 mass% or less.
[0008] (2) The coated seed according to the present invention is characterized in that the surface of the seed is coated with the seed coating agent described in (1) above.
[0009] (3) A seed coating method according to the present invention is characterized in that the seed surface is coated with the seed coating agent described in (1) above. Effect of the Invention
[0010] According to the present invention, coated seeds having a high seed density per mass of iron-based powder can be obtained while preventing damage to the seeds caused by heat generated by oxidation of metallic iron contained in the iron-based powder. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Before describing the seed coating agent, coated seed, and seed coating method according to the embodiment of the present invention, the seeds to which the present invention is applied will be described. In the following description, "mass%" will be simply written as "%".
[0012] <seed> As the seed to be coated with the seed coating agent according to the present invention, rice is preferably used. There is no particular restriction on the variety of rice, and any of Japonica, Indica, and Javanica rice can be used. Rice is often cultivated in paddy fields in hot and humid regions, so the effects of the present invention can be achieved.
[0013] <Seed coating agent> Next, the seed coating agent according to the embodiment of the present invention will be described. The seed coating agent according to the present embodiment contains iron-based powder and is used to coat the surface of seeds.
[0014] <Iron-based powder> The iron-based powder may be iron powder, iron oxide powder, or a mixture of iron powder and iron oxide powder. As the iron powder, powder of pure iron, ferroalloy, etc. can be used, and there is no particular limitation as long as the effects of the present invention can be obtained. As the iron oxide powder, iron oxide or partial iron oxide powder can be used. Examples of iron oxide include magnetite (Fe3O4), hematite (Fe2O3), wustite (FeO), and amorphous. The ratio of iron oxide in these is not particularly limited, but from the viewpoint of economy, iron oxide powder such as mill scale and iron ore is preferably used.
[0015] The iron powder and the iron oxide powder can be used in combination. From the viewpoint of preventing rust, it is preferable that the iron powder content in the mixed iron-based powder is 20% or more, and more preferably 40% or more.
[0016] The proportion (amount) of the iron-based powder contained in the seed coating agent is not particularly limited, but the mass ratio to the seeds (dry rice grains) is preferably 5% or more and 800% or less, and more preferably 10% or more and 500% or less.
[0017] In addition, the particle size of the iron-based powder is not particularly specified, but it is preferable for uniform coating that the iron-based powder having a particle size of 150 μm or less accounts for 80% or more of the total mass of the iron-based powder. The particle size distribution of the iron-based powder can be evaluated by sieving using the method specified in JIS Z2510-2004.
[0018] As the iron-based powder, the above-mentioned iron powder, iron oxide powder, and mixture of iron powder and iron oxide powder mixed with other metal powder can be used. However, from the viewpoint of rust formation, the metallic iron content in the iron-based powder is preferably 20% or more, more preferably 40% or more, based on the mass of the iron-based powder.
[0019] <Antioxidants> The seed coating agent according to the present embodiment contains ascorbic acid, erythorbic acid, and one or more of these compounds added as an antioxidant.
[0020] The form in which the antioxidant is added is not limited as long as ascorbic acid or erythorbic acid is added. Ascorbic acid or erythorbic acid and salts thereof, or anhydrides, hydrates, and isomers thereof can be used, and two or more types can be used in combination.
[0021] Specific examples of ascorbic acid include L-ascorbic acid, sodium L-ascorbate, calcium L-ascorbate, L-ascorbyl palmitate, and L-ascorbyl stearate. Specific examples of erythorbic acid include erythorbic acid and sodium erythorbate.
[0022] The antioxidant is presumed to have the function of suppressing excessive oxidation of high-density metallic iron contained in the iron-based powder, and of facilitating the production of high-density iron oxides (magnetite, wustite, etc.) rather than low-density iron hydroxides. As a result, it is believed that the addition of the antioxidant to the seed coating agent according to the present embodiment increases seed density while preventing damage to seeds due to oxidation heat.
[0023] The amount of the antioxidant is 0.01% or more and 15% or less based on the mass of the iron-based powder. If it is less than 0.01%, the effect of the present invention is reduced. If it exceeds 15%, the density decreases and the coating tends to become brittle.
[0024] When the antioxidant is added, it may be mixed with the iron-based powder in advance, or it may be sprayed onto the iron-based powder as an aqueous solution or suspension at the time of powder coating. Either method may be suitably employed.
[0025] If coarse iron-based powder particles remain on the seed surface, they can be removed using a sieve or the like, and the removed iron-based powder can be reused as a raw material for seed coating agents. On the other hand, when fine iron-based powder is used, unevenness in the coating is reduced, and the surface becomes smoother.
[0026] <Binding agent> In the present invention, a binder may be used, which is composed of sulfates and / or chlorides. The sulfates include calcium sulfate, potassium sulfate, magnesium sulfate, and hydrates thereof. Chlorides include potassium chloride, calcium chloride, magnesium chloride, and their hydrates. Plaster of Paris (calcium sulfate 1 / 2 hydrate) and gypsum (calcium sulfate dihydrate) are particularly preferred. Plaster of Paris and gypsum may be mixed or intermixed.
[0027] The mass ratio of the binder to the iron-based powder is not particularly limited, but in order to facilitate the progression of rust, it is preferably 0.1% or more and 33% or less.
[0028] The average particle size of the binder is not particularly specified, but is preferably 1 to 150 μm. If the average particle size of the binder is less than 1 μm, the amount of agglomerated particles generated during the coating operation increases, significantly reducing workability. On the other hand, if the average particle size of the binder exceeds 150 μm, the adhesive force to the iron-based powder decreases, and the strength of the coating tends to decrease.
[0029] <Finishing agent> A finishing agent is not required when coating the seed surface with a seed coating agent, but in order to further prevent the seeds from fusing together due to oxidation of the iron-based powder, it is preferable to apply a finishing agent such as calcined gypsum, gypsum, silica gel, etc.
[0030] ≪Third component≫ The seed coating agent according to the present invention may contain a third component to the extent that the effect of the present invention is not impaired. The third component includes inevitable impurities and additives that are intentionally added for some effect, and in any case, the amount of the third component is preferably up to about 30% of the seed coating agent.
[0031] <Coated seeds and seed coating method> Next, the coated seeds and seed coating methods according to the embodiments of the present invention will be described below.
[0032] The coated seeds according to the present embodiment are seeds whose surfaces are coated with the seed coating agent according to the present embodiment described above.
[0033] The seed coating method according to the present embodiment is for coating a seed surface with the seed coating agent according to the present embodiment. The seed coating method according to the present embodiment includes, for example, a step of attaching the seed coating agent to the seed surface (hereinafter, also referred to as "coating"), and a step of oxidizing the seed coating agent attached to the seed surface to form a coating layer.
[0034] There is no restriction on the specific method for coating the seed surface with the seed coating agent. For example, as shown in the "Iron-Coated Flooded Direct Seeding Manual 2010 (compiled by Kinki Chugoku Shikoku Agricultural Research Center, National Agriculture and Food Research Organization)," any method may be used, including manual coating and a method using a conventionally known mixer.
[0035] As the mixer, for example, a mixing blade type mixer (such as a Henschel mixer or concrete mixer) or a container rotation type mixer (such as a V-type mixer, a double cone mixer, an inclined rotation type pan mixer, a rotary hoe type mixer, etc.) can be used. In addition, a concrete mixer without the mixing blades can be preferably used.
[0036] When applying the seed coating agent using these mixers, the iron-based powder and seeds, and optionally the binder, separator, and additives may be placed in the mixer, and water may be added as appropriate. As a method for adding water, the mixer may be rotated while spraying water and / or a treatment liquid mainly composed of water, or the antioxidant may be sprayed as an aqueous solution or suspension without being mixed with the iron-based powder.
[0037] Regarding the step of forming the coating layer, there is no limitation on the method of oxidizing the seed coating agent. For example, as shown in the "Iron-Coated Flooded Direct Seeding Manual 2010 (compiled by the Kinki Chugoku Shikoku Agricultural Research Center, National Agriculture and Food Research Organization)," seeds may be spread out in seedling trays and watered, or an oxidation method using an oxidation regulator may be used. Alternatively, a method may be used in which the seeds are oxidized while flowing in a mixer and supplying water and air into the mixer (hereinafter referred to as the "mixed oxidation method"). The mixed oxidation method is more preferable because it can generate more divalent iron. The requirements for the mixed oxidation method are as follows:
[0038] To supply air, an electric fan, a fan, various types of dryers, a hot air blower, etc. can be used. The temperature of the air to be supplied is not particularly limited as long as the effects of the present invention can be obtained, but a temperature of -20 to 150°C is preferably applied, more preferably 0 to 100°C, and even more preferably 46 to 95°C. However, in order to maintain germination, the temperature of the seeds should be 50°C or lower, and even more preferably 40°C or lower. In order to prevent the seeds from freezing and to promote rusting, the temperature of the seeds should be 0°C or higher, and even more preferably 10°C or higher.
[0039] The wind speed of the supplied air is not particularly limited as long as the effects of the present invention are obtained, but is preferably 0.1 to 15 m / sec, and more preferably 0.5 to 10 m / sec. If it is less than 0.1 m / sec, oxidation and cooling do not proceed easily, and if it exceeds 15 m / sec, there is a risk that the seeds and the coating agent will be scattered.
[0040] Water can be added directly to the seeds or included in the air, for example, by spraying, misting, or adding water to the seeds or inside the mixer using a container such as a cup, or by supplying water as humidified air.
[0041] The moisture content is not particularly limited, but is preferably 10 to 1000% based on the mass of the iron-based powder, more preferably 20 to 500%, and even more preferably 50 to 200%. If it is less than 10%, rusting will be insufficient and the coating layer will peel off, while if it exceeds 1000%, there will be a problem that the time required for drying will be long. Furthermore, if a large amount of water is supplied at once, the seeds will clump together due to the moisture, so it is preferable to supply the amount of water in multiple batches while keeping the amount to a level that allows the seeds to flow within the mixer and maintaining the seeds in a wet state.
[0042] The oxidation treatment by the mixed oxidation method is preferably carried out after coating the seed surface with a seed coating agent, but it is also possible to supply air together with water to the flowing seeds in the step of coating the seeds with the seed coating agent, thereby carrying out the coating treatment and the oxidation treatment simultaneously.
[0043] After supplying water and air to the mixer, air is supplied to the mixer and the seeds are taken out after they have dried to a certain extent. After that, the seeds are transferred to a tray or the like and spread out, and excess water is removed and dried for storage.
[0044] As described above, according to the seed coating agent, coated seeds, and seed coating method of the present embodiment, it is possible to obtain coated seeds that have an increased seed density per unit mass of the iron-based powder coated on the seed surface while preventing damage to the seeds caused by heat generated by the oxidation of metallic iron.
[0045] Although the amount of the seed coating agent according to the present invention to be coated on the seed surface is not particularly limited, it is preferable to set the amount of the seed coating agent so that the iron-based powder is 5 to 800 parts by mass per 100 parts by mass of dry seeds. More preferably, in order to obtain a seed density (specific gravity) sufficient to sink the coated seeds to the bottom of the water, it is preferable to set the amount of the iron-based powder to about 10 to 500 parts by mass. In the present invention, even if the proportion of iron-based powder is increased, as long as it is within the above-mentioned range, coated seeds can be obtained that have an even higher seed density while preventing damage to the seeds caused by heat generated by the oxidation of metallic iron. EXAMPLES
[0046] An experiment was carried out to confirm the effect of the present invention, and the experiment will be described below. In the experiment, rice seeds were coated with the seed coating agent according to the present invention, and the coated seeds were subjected to an evaluation test.
[0047] The coating of the seed coating agent was carried out by a step of coating (dust dressing) the seed surface with the seed coating agent and a step of oxidizing the seed coating agent coated on the seed surface. The coating of the seed coating agent (dust dressing) was carried out according to the method described in the aforementioned "Iron-Coated Flooded Direct Seeding Manual 2010." In addition, the oxidation of the seed coating agent was carried out in two ways: mixed oxidation method and tray oxidation method. Specifically, the methods are as follows.
[0048] When using the mixed oxidation method, first, a seed coating agent premixed with rice seeds was prepared, and 100 g of seeds were coated with the seed coating agent in several batches using an inclined rotating pan mixer while spraying an appropriate amount of water (or L-ascorbic acid aqueous solution). Next, about 40 to 50 g of water was sprayed onto the seeds while supplying air at about 60°C to the seeds using a hot air blower. Unless otherwise specified, tap water was used as the water. In Example 14 of the invention shown in Table 1 below, the finishing agent was finally coated. After that, the coated seeds were spread on a tray and allowed to dry naturally.
[0049] In the case of using the tray oxidation method, first, the seed coating agent was mixed with rice seeds in advance, and then, using an inclined rotating pan mixer, the seed coating agent was coated in several batches per 100 g of seeds while spraying an appropriate amount of water, and finally, the finishing agent was coated. After that, the coated seeds were spread on a tray, sprayed with water six times, and then air-dried after sufficient oxidation.
[0050] In the experiment, rice seeds were coated by changing the type and amount of each ingredient contained in the seed coating agent and the seed coating method, as shown in Table 1. Tables 2 to 5 show each ingredient (Table 2: iron powder, Table 3: iron oxide, Table 4: binder, Table 5: antioxidant).
[0051] [Table 1]
[0052] [Table 2]
[0053] [Table 3]
[0054] [Table 4]
[0055] [Table 5]
[0056] In Table 1, in Examples 1 to 21, seeds were coated using the seed coating agent according to the present invention. In each of Examples 1 to 21, the ratio of the antioxidant to the mass of the iron-based powder was 0.02 mass% or more and 15 mass% or less.
[0057] Furthermore, for comparison, seeds were coated using the seed coating agents of Comparative Examples 1 and 2 shown in Table 1. Comparative Examples 1 and 2 are based on the prior art that does not contain an antioxidant. In Comparative Example 1, the seed coating was performed by the mixed oxidation method, and in Comparative Example 2, the seed coating was performed by the tray oxidation method.
[0058] The coated seeds coated with the seed coating agents according to the above-mentioned invention examples 1 to 21 and comparative examples 1 and 2 were subjected to evaluation tests for seed density and coating strength. These evaluation tests were carried out as follows. In addition, in the proportions of iron-based powder in the invention examples 1 to 21 and comparative examples 1 and 2, no damage to the seeds due to oxidation heat was observed.
[0059] <Seed density> The seed density of each coated seed was measured using an electronic specific gravity meter EW-300SG (Alpha Mirage Co., Ltd.).
[0060] <Coating strength> 100g of coated seeds were shaken for 1 minute using a 2mm mesh sieve in a Rotap sieve shaker to measure the weight loss rate. The weight loss rate was judged as follows: ◎: 1% or less, ○: over 1% and 5% or less, △: over 5% and 20% or less, ×: over 20%.
[0061] As shown in Table 1, the seed densities of the coated seeds of Comparative Examples 1 and 2 were 1.50 and 1.49. In contrast, the seed densities of the coated seeds of Invention Examples 1 to 21 were 1.52 to 1.60, which was an improvement over Comparative Examples 1 and 2. Here, in all of the invention examples 1 to 21 and the comparative examples 1 and 2, the iron-based powder was contained in a ratio of 50 parts by mass per 100 parts by mass of the seeds. Therefore, from the seed density results shown in Table 1, it can be seen that in the invention examples 1 to 21, the seed density per unit mass of the coated iron-based powder was increased even without increasing the ratio of the iron-based powder.
[0062] Furthermore, the coating strength of the coated seeds of Examples 1 to 21 was equivalent to that of Comparative Examples 1 and 2. This result shows that the seed coating agent according to the present invention, to which ascorbic acid, erythorbic acid, or a mixture of one or more of these compounds is added as an antioxidant, can provide coated seeds with improved seed density without reducing the coating strength.
Claims
1. A seed coating agent containing an iron-based powder and used to coat a seed surface, A seed coating agent characterized in that ascorbic acid, erythorbic acid, and one or more of these compounds are added as an antioxidant, and the ratio of the antioxidant to the mass of the iron-based powder is 0.02 mass% or more and 15 mass% or less.
2. A coated seed, the surface of which is coated with the seed coating agent according to claim 1.
3. A method for coating seeds, comprising coating the surface of a seed with the seed coating agent according to claim 1.
Citation Information
Patent Citations
Natural environment-friendly seed coating agent for non-heading Chinese cabbage and preparation method thereof
CN111466395A
Dressing agent for improving sprouting and growth of directly sowed rice plant seed
JP1989149704A
Method for treating plant seed
US20210015102A1
Method for producing iron powder coated rice plant seed
JP2005192458A
Seed coating agent, seed coating method, and coating agent coated seed
JP2017153427A