Hard coat resin composition and hard coating film

The hard coat resin composition with polyfunctional urethane (meth)acrylate, polythiophene compound, and fluorine-based antifouling agent addresses the issue of maintaining high water contact angle and abrasion resistance, enhancing durability and stain resistance for touch panels.

JP2024151788APending Publication Date: 2024-10-25AICA KOGYO CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023065496
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-13
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing hard coat films for touch panels do not maintain a high water contact angle and abrasion resistance when rubbed with an eraser or touch pen, leading to decreased stain resistance and durability.

Method used

A hard coat resin composition comprising polyfunctional urethane (meth)acrylate, polythiophene compound, fluorine-based antifouling agent, and photopolymerization initiator, with specific ratios to ensure high water contact angle and abrasion resistance.

Benefits of technology

The cured layer maintains a high water contact angle and exhibits excellent stain resistance even after extensive rubbing, ensuring durability and antifouling properties for touch panels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024151788000001
    Figure 2024151788000001
  • Figure 2024151788000002
    Figure 2024151788000002
  • Figure 2024151788000003
    Figure 2024151788000003
Patent Text Reader

Abstract

To provide a hard coat resin composition that exhibits minimal decrease in water contact angle even when rubbed with an eraser, while maintaining a high water contact angle, and a hard coating film with a resin cured layer thereof.SOLUTION: A hard coat resin composition includes a polyfunctional urethane (meth)acrylate, a polythiophene compound, a fluorine-based antifouling agent, and a photopolymerization initiator. The water contact angle of the fluorine-based antifouling agent alone is 115° or more, with its content being 0.3-1.1 pts.wt. relative to 100 pts.wt. of the photopolymerization component.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photocurable hard coat resin composition and a hard coat film having a cured layer formed thereon. [Background technology]

[0002] In recent years, touch panels that combine display devices and input devices have been used in a wide range of fields. In particular, touch panels that use a touch pen as an input device allow for more intuitive operation by directly inputting characters and complex figures, and are widely used in tablet PCs, pen tablets, smartphones, portable game devices, etc.

[0003] Touch panels have a problem in that the screen is exposed and is directly touched by fingers, skin, pens, etc., and is therefore susceptible to dirt such as sebum and scratches. To address such problems, technologies have been developed to make the surface of the touch panel less susceptible to dirt, easier to clean, smooth, and less susceptible to scratches, and for example, a hard coat film has been proposed in which a hard coat layer containing a hydrolyzable silyl group or silanol group, a radical polymerizable compound, and a polymerization initiator and a surface layer are laminated in this order (Patent Document 1).

[0004] By using such hard coat film, it has become possible to prevent the occurrence of dirt adhesion and scratches considerably, but especially when using a touch pen, high durability is required so that surface function can be maintained for a long time.However, there are not many hard coat films with sufficient abrasion resistance, and there are problems such as the water contact angle being greatly changed and the antifouling property being reduced when the film surface is rubbed with something that rubs the film surface, such as an eraser, and there is room for improvement. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 6519771 Summary of the Invention [Problem to be solved by the invention]

[0006] The object of the present invention is to provide a hard coat resin composition which exhibits a very small decrease in water contact angle even when rubbed with an eraser and can maintain a high water contact angle, and a hard coat (hereinafter referred to as HC) film having a cured resin layer thereof. [Means for solving the problem]

[0007] In order to solve the above problems, the invention of claim 1 provides a hard coat resin composition comprising a polyfunctional urethane (meth)acrylate (A), a polythiophene compound (B), a fluorine-based antifouling agent (C), and a photopolymerization initiator (D), wherein the water contact angle of (C) alone is 115° or more, and the blending amount of (C) is 0.3 to 1.1 parts by weight per 100 parts by weight of the photopolymerization component.

[0008] A second aspect of the present invention provides the hard coat resin composition according to the first aspect, characterized in that the blending amount of (B) is 0.18 to 1.4 parts by weight based on 100 parts by weight of the photopolymerizable component.

[0009] The invention of claim 3 provides a hard coat film comprising a plastic substrate and a cured layer of the hard coat resin composition of claim 1 or 2 formed on at least one surface of the plastic substrate. Effect of the Invention

[0010] The cured layer of the HC resin composition of the present invention has excellent stain resistance, in that the rate of decrease in water contact angle is very small even when rubbed with an eraser, and a high water contact angle can be maintained, making it useful as an HC resin for use in HC films for touch panels that use a touch pen as an input means. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will now be described in detail.

[0012] The HC resin composition of the present invention contains a polyfunctional urethane (meth)acrylate (hereinafter referred to as ureac) (A), a polythiophene-based compound (B), a fluorinated antifouling agent (C), and a photopolymerization initiator (D). In this specification, (meth)acrylate includes both acrylate and methacrylate.

[0013] The polyfunctional urea (A) used in the present invention is the main resin forming the HC layer, and is a binder with excellent scratch resistance due to the cohesive force of hydrogen bonds derived from urethane bonds. For example, it can be obtained by reacting polyisocyanate with (meth)acrylate having a hydroxyl group.

[0014] Examples of polyisocyanates used in the reaction (A) include hexamethylene diisocyanate (hereinafter referred to as HDI), isophorone diisocyanate, diphenylmethane diisocyanate, tolylene diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, hydrogenated xylylene diisocyanate, methylcyclohexylene diisocyanate, HDI isocyanurate, IPDI isocyanurate, etc., which may be used alone or in combination of two or more. Among these, aliphatic and alicyclic diisocyanates that have high weather resistance and are less likely to yellow are preferred, and among them, HDI, which has high extensibility, is particularly preferred.

[0015] Examples of (meth)acrylates having a hydroxyl group used in the reaction (A) include bifunctional trimethylolpropane di(meth)acrylate, glycerin di(meth)acrylate, pentaerythritol di(meth)acrylate, diglycerin di(meth)acrylate, ditrimethylolpropane di(meth)acrylate, dipentaerythritol di(meth)acrylate, and trifunctional or higher diglycerin tri(meth)acrylate, ditrimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, and dipentaerythritol penta(meth)acrylate. Among these, trifunctional pentaerythritol triacrylate (hereinafter referred to as PETA), which is highly curable, is preferred.

[0016] The blending amount of the (A) is preferably 55 to 98% by weight, more preferably 60 to 97% by weight, and particularly preferably 65 to 96% by weight, based on the total solid content. By setting the blending amount within this range, sufficient optical properties and low curling can be ensured, and the change rate of the water contact angle can be very small even when rubbed with an eraser.

[0017] The polythiophene compound (B) used in the present invention is a polymer of thiophene, a sulfur-containing heterocyclic compound, which becomes conductive when electrons are added to or removed from the conjugated n orbital by doping. In particular, poly(3,4-ethylenedioxythiophene) (hereinafter referred to as PEDOT) is preferable because it improves conductivity when combined with poly(4-styrenesulfonate) (hereinafter referred to as PSS), has high environmental stability, and has high light transmittance in a thin film. The inventors have found that by combining this polythiophene compound with a fluorine-based antifouling agent that has a specific water contact angle by itself, a high water contact angle can be stably maintained even after rubbing with an eraser more than 3,000 times.

[0018] The blending amount of (B) is preferably 0.18 to 1.4 parts by weight, more preferably 0.20 to 1.3 parts by weight, and even more preferably 0.25 to 1.1 parts by weight, based on 100 parts by weight of the photopolymerizable component. By making it 0.18 parts by weight or more, the decrease in the water contact angle after rubbing with an eraser can be sufficiently suppressed, and by making it 1.4 parts by weight or less, sufficient total light transmittance can be ensured.

[0019] The surface resistivity of the cured film containing (B) is initially 1.00×10 7 ~9.99×10 11 It is preferable that the conductivity is Ω / □. By setting the conductivity in this range, the water repellency can be stably maintained. Although the reason why the decrease in the water contact angle can be suppressed by improving the conductivity is not clear, it is presumed that the damage to the film can be reduced by making it difficult to generate static electricity that occurs when the eraser is rubbed, and as a result, the decrease in the water contact angle can be suppressed.

[0020] The fluorine-based antifouling agent (C) used in the present invention is blended for the purpose of lowering the surface tension of the cured film surface, improving the antifouling properties, and stabilizing the water contact angle. By blending (C), the water contact angle of the cured film becomes high, and even if it is rubbed with an eraser, the rate of change in the water contact angle before and after the rub can be made very small. This effect can be particularly enhanced when the photocuring is performed under nitrogen purging (deoxidation) conditions.

[0021] The water contact angle of the film of (C) when cured by itself is 115° or more, preferably 116° or more. If the water contact angle is 115° or more, sufficient water repellency can be ensured when the composition is cured to form a film, and even if the composition is rubbed with an eraser 3000 times or more, the change rate of the water contact angle before and after the rub is very small. Furthermore, when oleic acid is used, the contact angle is preferably 80° or more, more preferably 82° or more, and particularly preferably 84° or more. If the contact angle of oleic acid is 80° or more, sufficient water and oil repellency can be ensured when the composition is cured to form a film, and even if the composition is rubbed with an eraser 3000 times or more, the change rate of the water contact angle before and after the rub is very small.

[0022] The conditions for preparing a cured film for measuring the contact angle of water and oleic acid with the (C) alone were as follows. Five parts of an α-hydroxyacetophenone-based photopolymerization initiator (Omnirad2959) were added to 100 parts by weight of a fluorine-based compound in terms of solid content ratio, and the mixture was applied to a PET film so that the thickness after drying was 3 μm. After drying at 80°C for 1 minute, the mixture was cured with ultraviolet light in a nitrogen purged environment. The ultraviolet curing conditions were an electrodeless UV irradiation device F300S / LC-6B manufactured by Fusion UV Systems Japan, with an output of 1200 mW / cm2 and an accumulated light amount of 200 mJ / cm2 with an H bulb. If the photopolymerization initiator is difficult to dissolve in the fluorine-based compound, it may be diluted with a solvent. The contact angle of water and oleic acid was measured according to the sessile drop method of JIS R 3257:1999, and the measurement was performed after dropping (2 μL) at room temperature and leaving it for 30 seconds using a DMs-400 manufactured by Kyowa Interface Science Co., Ltd.

[0023] The amount of (C) is 0.30 to 1.1 parts by weight, preferably 0.35 to 1.0 parts by weight, and more preferably 0.40 to 0.8 parts by weight, based on 100 parts by weight of the photopolymerizable component. If it is less than 0.3 parts by weight, the water contact angle after rubbing with an eraser tends to decrease, and the water repellency tends to be unable to be stably maintained, and if it exceeds 1.1 parts by weight, the water repellency tends to be unable to be stably maintained.

[0024] The photopolymerization initiator (D) used in the present invention generates radicals when irradiated with ultraviolet light or an electron beam, and the radicals trigger the polymerization reaction, and general-purpose photopolymerization initiators such as benzyl ketal, acetophenone, and phosphine oxide photopolymerization initiators can be used. By arbitrarily selecting the light absorption wavelength of the polymerization initiator, it is possible to impart curability over a wide wavelength range from the ultraviolet region to the visible light region. Specifically, 2.2-dimethoxy-1.2-diphenylethan-1-one is a benzyl ketal, 1-hydroxy-cyclohexyl-phenyl-ketone and 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one are α-hydroxyacetophenones, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one is α-aminoacetophenones, and 2.4.6-trimethylbenzoyl-diphenyl-phosphine oxide and bis(2.4.6-trimethylbenzoyl)-phenylphosphine oxide are acylphosphine oxides, which may be used alone or in combination of two or more. Among these, it is preferable to use an α-hydroxyacetophenone that is less prone to yellowing, and examples of commercially available products include Irgacure 184 and 2959 (trade name: BASF Japan, α-hydroxyacetophenones).

[0025] The amount of (D) is preferably 0.5 to 10 parts by weight, more preferably 3 to 8 parts by weight, based on 100 parts by weight of the photopolymerizable component. By adding 0.5 parts by weight or more, sufficient curability is achieved, and by adding 10 parts by weight or less, yellowing of the coating film and deterioration of storage stability can be prevented without excessive addition.

[0026] Furthermore, to the HC resin composition of the present invention, ultraviolet absorbers, antioxidants, colorants, defoamers, thickeners, suspending agents, antifogging agents, slip agents, antibacterial agents, antiviral agents, organic fine particles, inorganic fillers, and the like may be added as necessary.

[0027] The HC resin composition of the present invention is diluted with a solvent to a solid content of 10 to 90% in order to improve the coatability to a plastic substrate. Examples of the solvent include alcohol-based solvents such as ethanol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, isobutyl alcohol, and diacetone alcohol, ketone-based solvents such as acetone, methyl ethyl ketone (hereinafter referred to as MEK), methyl isobutyl ketone, and cyclohexanone, ester-based solvents such as methyl acetate and butyl acetate, and ether-based solvents such as PGM, diethyl ether, and diisopropyl ether, which can be used alone or in combination of two or more kinds.

[0028] Examples of plastic substrates to which the HC resin of the present invention can be applied include polyester films, polyethylene films, polypropylene films, diacetyl cellulose films, triacetyl cellulose (hereinafter referred to as TAC) films, acetyl cellulose butyrate films, polyvinyl chloride films, polyvinylidene chloride films, polyvinyl alcohol films, ethylene vinyl alcohol films, polystyrene films, polycarbonate films, polymethylpentene films, polysulfone films, polyether ether ketone films, polyether sulfone films, polyether imide films, polyimide films, fluorine resin films, nylon films, acrylic films, cycloolefin (co)polymer films, and the like.

[0029] Among these, biaxially oriented polyester films are preferably used from the viewpoints of price, processability, dimensional stability, etc., acrylic films and polycarbonate films from the viewpoint of weather resistance, and TAC films from the viewpoint of good optical properties. The thickness of the film may be about 23 μm to 250 μm.

[0030] The method for applying the HC resin composition of the present invention is not particularly limited, and can be any of known coating methods such as spray coating, roll coating, die coating, air knife coating, blade coating, spin coating, reverse coating, gravure coating, wire bar coating, etc., or gravure printing, screen printing, offset printing, inkjet printing, etc. The dry film thickness is preferably 0.5 μm to 20 μm.

[0031] After the HC resin composition of the present invention is applied, it is dried at 60 to 120° C. and cured using an ultraviolet ray irradiator. Examples of light sources for irradiating ultraviolet rays include low pressure mercury lamps, high pressure mercury lamps, ultra-high pressure mercury lamps, carbon arc lamps, xenon lamps, metal halide lamps, electrodeless ultraviolet lamps, and LED lamps. The curing conditions are 500 mW / cm. 2 ~3000mW / cm 2 The irradiation intensity is 50 to 2,000 mJ / cm2 as the cumulative light quantity. 2 The irradiation atmosphere may be air, but is preferably an inert gas atmosphere such as nitrogen or argon.

[0032] The initial water contact angle of the HC film having a cured layer of the HC resin composition of the present invention is preferably 105° or more, more preferably 110° or more. In addition, the water contact angle after 3000 reciprocations with a load of 1 kgf using an eraser is preferably 100° or more, more preferably 103° or more, and particularly preferably 105° or more. Furthermore, the water contact angle after 8000 reciprocations is preferably 100° or more, more preferably 103° or more. If a water contact angle of 100° or more can be secured after rubbing with an eraser, it can be judged that the film has excellent antifouling properties and excellent abrasion resistance. In particular, if a water contact angle of 100° or more can be secured even after 8000 reciprocations, the film has very excellent antifouling properties and abrasion resistance.

[0033] In addition, the water contact angle after 3000 rubs with an eraser is preferably 90% or more of the initial value, more preferably 94% or more. If it is 90% or more of the initial value, it is considered that most of the antifouling components remain without being scraped off by the eraser test, so it can be judged that the antifouling properties are stable and abrasion resistant, and that the antifouling properties do not decrease over time when rubbed with a touch pen. The water contact angle after 8000 rubs is preferably 88% or more of the initial value, more preferably 90% or more.

[0034] The reason for using an eraser in the above is that the abrasion caused by an eraser is similar to that caused by a touch pen, and this evaluation allows for an approximate evaluation of the abrasion resistance to a touch pen. The abrasion resistance of optical films is generally evaluated using steel wool, but steel wool is literally a hard and thin metal wire, and the degree of abrasion caused by a touch pen is completely different, so the abrasion resistance caused by a touch pen cannot be evaluated using steel wool.

[0035] The eraser used in the above eraser test is manufactured by MINOAN Co., Ltd. in Korea (diameter 6 mm), and rubbed 3000 and 8000 times back and forth using a flat friction tester manufactured by Toyo Seiki Seisakusho Co., Ltd. under the conditions of a load of 1 kg, a rub speed of 40 rpm, and a stroke width of 30 mm, and the water contact angle is measured before and after. In this specification, the water contact angle is the value measured based on the sessile drop method of JIS R 3257:1999.

[0036] The present invention will be described in detail below based on examples and comparative examples, but these are specific examples and are not intended to be limiting. Unless otherwise stated, measurements were performed under conditions of room temperature of 25°C and relative humidity of 65%. The blend amounts are shown in parts by weight calculated as solid content.

[0037] Examples 1 to 7 Examples 1 to 7, which are HC resin compositions, were prepared by stirring the mixture as shown in Table 1 (dilution solvent was used in an amount to give a solid content of 30%) until uniformly dissolved and dispersed using ureac (6-functionality obtained by reacting HDI and PETA, Mw 2,600, solid content 90%) as (A), PEDOT / PSS dispersion (PEDOT / PSS content 0.4%) as (B), fluorine-based antifouling agent 1 (water contact angle 116.1°, oleic acid contact angle 84.1°) as (C), and Omnirad2959 (product name: manufactured by iGM, α-hydroxyacetophenone type) as (D) in the proportions shown in Table 1 (dilution solvent was used in an amount to give a solid content of 30%) as (A), and the like, respectively.

[0038] Comparative Examples 1 to 4 In addition to the materials used in the examples, fluorine-based antifouling agent 2 (water contact angle 110.2°, oleic acid contact angle 75.2°) and fluorine-based antifouling agent 3 (water contact angle 112.1°, oleic acid contact angle 76.0°) were used, and PGMAC was used as a dilution solvent. The compositions shown in Table 2 (dilution solvent in an amount to give a solids content of 30%) were stirred until uniformly dissolved and dispersed to prepare Comparative Examples 1 to 4, which are HC resin compositions.

[0039] Adjustment of HC film The coating was applied to an A4-sized polyethylene terephthalate film U403 (product name: Toray Industries, 50 μm, with easy-adhesion layers on both sides) so that the film thickness when cured would be 5 μm, and after drying at 80°C for 1 minute in a thermostatic chamber, the film was purged with nitrogen and cured with ultraviolet light using an electrodeless UV irradiation device F300S / LC-6B manufactured by Fusion UV Systems Japan, with an output of 1200 mW / cm2 using an H bulb and an accumulated light quantity of 200 mJ / cm2.

[0040] Table 1 JPEG2024151788000001.jpg52133

[0041] Table 2 JPEG2024151788000002.jpg74129

[0042] The evaluation method was as follows.

[0043] Water contact angle (initial): The water contact angle was measured according to the sessile drop method of JIS R 3257:1999 using a DMs-400 manufactured by Kyowa Interface Science Co., Ltd., after dropping water (2 μL) at room temperature and leaving it for 30 seconds. The water contact angle was evaluated as × for less than 105°, ◯ for 105° to 110°, and ◎ for more than 110°.

[0044] Water contact angle (after rubbing): Using an eraser (diameter 6 mm) manufactured by South Korea's MINOAN Co., Ltd., and a flat friction tester manufactured by Toyo Seiki Seisakusho, the material was rubbed back and forth 3,000 times and 8,000 times under the conditions of a load of 1 kg, a rubbing speed of 40 rpm, and a stroke width of 30 mm, and the water contact angle was measured after that. 3000 times: Less than 100° is ×, 100° to 105° is 〇, over 105° is ◎ 8,000 times: Less than 100° was marked as ×, 100° to 103° was marked as 〇, and over 103° was marked as ◎.

[0045] Water contact angle reduction rate: The ratio of the water contact angle after rubbing with an eraser to the initial value of the water contact angle. 3000 times: Less than 90% is ×, 90-94% is 〇, and over 94% is ◎ 8,000 times: Less than 88% was marked as ×, 88-90% as 〇, and over 90% as ◎.

[0046] Total light transmittance: Measured in accordance with JIS K7361-1 using Haze-GARD2 manufactured by Toyo Seiki Seisakusho, with less than 89% being rated as "X" and 89% or more being rated as "O."

[0047] Surface resistivity: The coated surface of the HC film prepared above was measured in accordance with JIS K6911 using a high resistivity meter HIRESTA-UX manufactured by Nitto Seiko Analytech Co., Ltd.

[0048] Evaluation result 1 JPEG2024151788000003.jpg112137

[0049] Evaluation result 2 JPEG2024151788000004.jpg196160

[0050] The examples were satisfactory without any problems in all respects, including the initial water contact angle, the water contact angle after rubbing with an eraser, the rate of decrease in the contact angle, the total light transmittance, and the surface resistivity.

[0051] On the other hand, in Comparative Example 1, where (C) was below the lower limit, and Comparative Example 2, where (C) was above the upper limit, the water contact angle decreased after rubbing with an eraser 8,000 times or more. In Comparative Examples 3 and 4, where (C) was used, where the water contact angle of the single substance was less than 115°, the water contact angle decreased after rubbing with an eraser 3,000 times or more, and neither of these were suitable for the present invention.

Claims

1. A hard coat resin composition comprising a polyfunctional urethane (meth)acrylate (A), a polythiophene compound (B), a fluorine-based antifouling agent (C), and a photopolymerization initiator (D), the composition being characterized in that the water contact angle of the (C) alone is 115° or more, and the blending amount of the (C) is 0.3 to 1.1 parts by weight per 100 parts by weight of the photopolymerization component.

2. 2. The hard coat resin composition according to claim 1, wherein the blending amount of said (B) is 0.18 to 1.4 parts by weight based on 100 parts by weight of the photopolymerizable component.

3. 3. A hard coat film comprising a plastic substrate and a cured layer of the hard coat resin composition according to claim 1 or 2 formed on at least one surface of the substrate.

Citation Information

Patent Citations

  • Hard coated film and information display device

    JP6519771B2