Developing sleeve and electrophotographic image forming apparatus
An aluminum alloy with at least 0.6% silicon content in developing sleeves maintains surface roughness and durability, addressing wear issues and ensuring consistent developer conveyance and image quality.
Patent Information
- Application Number
- JP2023066090
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-25
AI Technical Summary
Developing sleeves made of aluminum wear out during long-term use, leading to a decrease in surface roughness and frictional force, which affects the conveyance of carrier and toner, resulting in uneven developer distribution and image quality issues.
The use of an aluminum alloy containing more than 0.6% by mass of silicon, which forms a sea-island structure with silicon microcrystals dispersed in the aluminum phase, maintaining appropriate surface roughness and durability, and optionally combined with sandblasting and grooves to enhance developer transportability.
The solution maintains excellent durability and developer conveyance ability, preventing surface wear and ensuring consistent image quality by retaining appropriate surface roughness and frictional force.
Smart Images

Figure 2024152110000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a developing sleeve and an electrophotographic image forming apparatus, and more particularly to a developing sleeve and an electrophotographic image forming apparatus that are excellent in durability of developer transport ability and can maintain good image quality. [Background technology]
[0002] In recent electronic image formation, members made of aluminum, which is inexpensive and easy to process, are increasingly being used as developer transport members.
[0003] An example of the above is Patent Document 1. In this document, an aluminum sleeve is used as the transport member to solve the problem of image defects when forming an image with a two-component developer.
[0004] However, since the unevenness described above becomes smaller as the developing sleeve wears during long-term use, there is room for improvement in order to maintain an appropriate roughness of the outer peripheral surface and excellent transportability. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 07-181809 Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in consideration of the above problems and circumstances, and the problem to be solved is to provide a developing sleeve and an electrophotographic image forming apparatus which have excellent durability in terms of developer transport ability and can maintain good image quality. [Means for solving the problem]
[0007] In order to solve the above problems, the present inventors have investigated the causes of the above problems and have found that the above problems can be solved by having a developing sleeve for an electrophotographic image forming apparatus, which transports a developer containing toner and a carrier, containing an aluminum alloy containing more than 0.6% by mass of silicon, thereby completing the present invention. That is, the above-mentioned problems of the present invention are solved by the following means.
[0008] 1. A developing sleeve for an electrophotographic image forming apparatus which transports a developer containing a toner and a carrier, said developing sleeve comprising an aluminum alloy containing more than 0.6% by weight of silicon.
[0009] 2. The developing sleeve according to claim 1, wherein the developing sleeve comprises an aluminum alloy containing more than 0.8% by weight of silicon.
[0010] 3. The developing sleeve according to claim 1, which has no resin layer on its surface.
[0011] 4. The developing sleeve according to claim 1, characterized in that it has grooves on its surface.
[0012] 5. The developing sleeve according to claim 1, wherein the surface of the developing sleeve is subjected to sandblasting.
[0013] 6. The developing sleeve according to item 1, wherein the average length RSm of the roughness curve elements of the surface of the developing sleeve is equal to or greater than the particle diameter of the carrier.
[0014] 7. The developing sleeve according to item 1, wherein the aluminum alloy contains magnesium, and the magnesium content is 5.0 mass % or less based on the total mass of the aluminum alloy.
[0015] 8. The developing sleeve according to item 1, wherein the aluminum alloy contains manganese, and the manganese content is 2.0 mass % or less based on the total mass of the aluminum alloy.
[0016] 9. The developing sleeve according to item 1, wherein the silicon content is in the range of more than 0.6 mass % and not more than 4.4 mass % based on the total mass of the aluminum alloy.
[0017] 10. An electrophotographic image forming apparatus having a developing sleeve for conveying a developer containing a toner and a carrier, the developing sleeve being made of an aluminum alloy containing more than 0.6% by mass of silicon. Effect of the Invention
[0018] According to the above-mentioned means of the present invention, it is possible to provide a developing sleeve and an electrophotographic image forming apparatus which are excellent in durability of developer transporting ability and capable of maintaining good image quality.
[0019] Although the mechanism by which the effects of the present invention are expressed or the mechanism by which the effects of the present invention are acted upon has not been clarified, it is speculated as follows.
[0020] The developing sleeve of the present invention is a developing sleeve for an electrophotographic image forming apparatus that transports a developer containing a toner and a carrier, and is characterized in that the developing sleeve comprises an aluminum alloy containing more than 0.6% by mass of silicon.
[0021] Conventionally, in order to provide a developing sleeve with excellent transportability, the surface of an aluminum developing sleeve is initially roughened by, for example, blasting the surface, etc. However, it has been found that the surface of the developing sleeve wears away with long-term use, making it impossible to maintain an appropriate roughness on the outer peripheral surface, and thus reducing the transportability of the carrier.
[0022] In a system in which the carrier and toner contained in a two-component developer are transported by an aluminum developing sleeve, the transportability of the carrier holding the toner is important in order to transport the toner to the development nip portion.
[0023] Conventionally, as a means for holding and transporting the carrier on the surface of the developing sleeve, a method for roughening the surface of the developing sleeve by sandblasting or the like has been used to increase the friction between the developing sleeve surface and the carrier. However, the initial roughness is worn down by the rubbing with the carrier, which is mainly made of ferrite, over a long period of use. This causes a problem in that the friction with the carrier decreases, making it difficult for the carrier to be transported.
[0024] Another factor that reduces the roughness of the developing sleeve surface is friction with external additives (such as Si) contained in the toner. When the roughness of the developing sleeve surface decreases and the frictional force between the developing sleeve surface and the carrier decreases, the carrier is not held on the developing sleeve surface and slips. This may cause a phenomenon in which the developer is not held on the developing sleeve surface and the developing sleeve surface is exposed.
[0025] When the developing sleeve surface is exposed without the developer, the developing property differs in the areas that are not exposed, resulting in uneven density. Mainly, the developing property of the exposed developing sleeve surface, where the developer is not held, is reduced, resulting in a reduction in density.
[0026] In the present invention, the developing sleeve contains an aluminum alloy containing more than 0.6% by mass of silicon, which forms a sea-island structure in which silicon crystallites (eutectic) are dispersed in the aluminum phase, forming appropriate irregularities on the outer peripheral surface of the developing sleeve.
[0027] In addition, since aluminum and silicon have different hardness, the surface roughness of the developing sleeve can be appropriately maintained even during long-term use by setting the silicon content within a certain range. This is believed to improve the durability of the carrier transport ability of the developing sleeve and maintain good image quality during image formation. [Brief description of the drawings]
[0028] [Figure 1] External view of a developing roller equipped with a developing sleeve [Diagram 2] Cross-sectional view of a developing roller with a shaft that does not pass through the magnet roller [Diagram 3] Cross-sectional view of a developing roller with a shaft passing through a magnet roller [Figure 4] Diagram to explain the state of silicon as a function of temperature [Diagram 5] (a) A photograph showing the eutectic state of a Si-Al alloy with a silicon content of 7 mass%. (b) A photograph showing the eutectic state of a Si-Al alloy with a silicon content of 12.6 mass%. (c) A photograph showing the eutectic state of a Si-Al alloy with a silicon content of 18 mass%. [Figure 6] A partial enlarged view of the undulations on the developing sleeve surface [Figure 7] Partially enlarged view of the cross section of the developing sleeve [Figure 8] FIG. 1 is an explanatory cross-sectional view showing an example of the configuration of an electrophotographic image forming apparatus according to the present invention; [Figure 9] (a) A three-dimensional schematic diagram showing the shape of the mask jig. (b) A schematic plan view showing the state before the mask jig is pressed against the developing sleeve. (c) A schematic plan view showing the state after the mask jig is pressed against the developing sleeve. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] The developing sleeve of the present invention is a developing sleeve for an electrophotographic image forming apparatus that conveys a developer containing a toner and a carrier, and is characterized in that the developing sleeve has an aluminum alloy containing more than 0.6% by mass of silicon. This characteristic is a technical characteristic common to or corresponding to each of the following embodiments (modes).
[0030] In an embodiment of the present invention, it is preferable that the developing sleeve comprises an aluminum alloy containing more than 0.8% by mass of silicon, from the viewpoints of durability of developer transport ability and maintaining good image quality.
[0031] From the viewpoint of imparting an appropriate surface roughness, it is preferable that the developing sleeve does not have a resin layer on the surface of the developing sleeve.
[0032] It is preferable that the developing sleeve has grooves on its surface from the viewpoint of improving the transportability of the developer.
[0033] From the viewpoint of improving the transportability of the developer, it is preferable that the surface of the developing sleeve is subjected to sandblasting.
[0034] It is preferable from the viewpoint of maintaining the transportability of the developer that the average length RSm of the roughness curve elements of the surface of the developing sleeve is equal to or greater than the particle diameter of the carrier.
[0035] It is preferable that the aluminum alloy contains magnesium and that the magnesium content is 5.0 mass % or less based on the total mass of the aluminum alloy, from the viewpoints of improving the strength of the developing sleeve and stabilizing the groove processing formed on the surface of the developing sleeve and the runout accuracy required of the developing roller.
[0036] It is preferable that the aluminum alloy contains manganese and that the manganese content is 2.0 mass % or less relative to the total mass of the aluminum alloy, from the viewpoints of improving the strength of the developing sleeve and stabilizing the groove processing formed on the surface of the developing sleeve and the runout accuracy required of the developing roller.
[0037] It is preferable that the silicon content is in the range of more than 0.6 mass % and not more than 4.4 mass % relative to the total mass of the aluminum alloy, from the viewpoints of improving the transportability of the developer by maintaining the surface roughness of the developing sleeve during long-term use, and stabilizing the groove processing formed on the surface of the developing sleeve and the runout accuracy required of the developing roller.
[0038] The electrophotographic image forming apparatus of the present invention is an electrophotographic image forming apparatus equipped with a developing sleeve that transports a developer containing a toner and a carrier, and is characterized in that the developing sleeve comprises an aluminum alloy containing more than 0.6 mass % silicon.
[0039] The present invention, its components, and embodiments for carrying out the present invention will be described in detail below. In this application, the symbol "to" is used to mean that the numerical values before and after the symbol "to" are included as the lower and upper limits.
[0040] 1.Developing sleeve The developing sleeve of the present invention is a developing sleeve for an electrophotographic image forming apparatus that transports a developer containing a toner and a carrier, and is characterized in that the developing sleeve comprises an aluminum alloy containing more than 0.6% by mass of silicon.
[0041] It is preferable that the developing sleeve is mainly composed of an aluminum alloy, and more preferably, 80% by mass or more of the developing sleeve is an aluminum alloy, and even more preferably, 100% by mass of the developing sleeve is an aluminum alloy. In addition, it is preferable that the developing sleeve of the present invention has an aluminum alloy containing more than 0.8% by mass of silicon, from the viewpoint of maintaining durability of developer transport ability and good image quality.
[0042] The "developing sleeve" of the present invention is a means having a function of carrying a moderately charged developer and supplying the developer to another adjacent developing sleeve or a photoconductor on which an electrostatic image is formed, and may be, for example, a component part of a developing roller equipped in an electrophotographic image forming apparatus. The developing roller is composed of, for example, a developing sleeve, a flange, a shaft, and a magnet roller. However, a developing roller having the "developing sleeve" of the present invention as a part of its configuration does not need to include a magnet part as a part of its configuration, such as a magnet roller.
[0043] Fig. 1 is an example of an external view of a developing roller equipped with a developing sleeve. The developing sleeve is rotatable and cylindrical, and plays a role of carrying and transporting a developer on its surface. As shown in Fig. 1, a plurality of grooves 20 extending in the axial direction of the developing roller 10 are formed at predetermined intervals in the circumferential direction on the surface of the developing sleeve 11. Note that the surface of the developing sleeve of the present invention may be configured without the above-mentioned grooves.
[0044] 2 and 3 are examples of the developing sleeve of the present invention, each of which is a cross-sectional view in the axial direction of a developing roller having a magnet roller and a shaft configuration with different shapes. However, a developing roller having the developing sleeve of the present invention as a part of its configuration does not need to include a magnet part as a part of its configuration, such as a magnet roller, and is not limited to the configurations of FIGS. 2 and 3.
[0045] 2 is a cross-sectional view of a developing roller in which the shaft does not pass through the magnet roller. As shown in Fig. 2, the developing roller 10 has a shaft 16 fixed by inserting the shaft into a hole formed in the magnet roller 12, and is provided with a developing sleeve 11 made of a non-magnetic material on the outer periphery of the magnet roller 12.
[0046] 3 is a cross-sectional view of a developing roller in which the shaft passes through the magnet roller. As shown in Fig. 3, the developing roller 10 has a magnet roller 12 fixed around the periphery of a shaft 16 and a developing sleeve 11 made of a non-magnetic material attached to the outer periphery of the magnet roller 12.
[0047] The developing sleeve 11 is connected to the magnet roller 12 with a predetermined gap therebetween via a bearing portion 17 such as a bearing provided on the outside of the magnet roller 12. A non-driving side flange 18 and a driving side flange 19 are connected to the developing sleeve 11 on the outside of the axial bearing portion 17 of the developing sleeve 11. Note that the non-driving side flange 18 and the driving side flange 19 may be reversed, and are not limited to this. The non-driving side flange 18 and the driving side flange 19 are rotated together with the developing sleeve 11 while being held relative to the developing container.
[0048] (1.1) Aluminum alloy The aluminum alloy of the developing sleeve according to the present invention does not include the materials constituting the flange, shaft and magnet roller (see FIGS. 1, 2 and 3).
[0049] The aluminum alloy includes an aluminum alloy containing silicon, and the content of the silicon is more than 0.6 mass% based on the total mass of the aluminum alloy. By containing silicon in the developing sleeve of the present invention, roughness can be imparted to the surface of the developing sleeve. Furthermore, the difference in hardness between aluminum and silicon makes it possible to make the amount of wear of the surface of the developing sleeve during long-term use different between the two, and it is possible to impart and maintain an appropriate surface roughness to the surface of the developing sleeve.
[0050] If the silicon content is less than 0.6% by mass, sufficient roughness cannot be imparted to the surface of the developing sleeve due to wear of the developing sleeve during long-term use, resulting in a decrease in the conveying force.
[0051] Increasing the silicon content can impart roughness to the surface of the developing sleeve, and even when the surface wears away during long-term use, the effect of the contained silicon is such that the surface roughness is maintained, and the strength of the developing sleeve is also increased.
[0052] However, if the silicon content is 12.6% by mass or less, coarse crystals (protruding parts) due to the eutectic of silicon and aluminum are unlikely to occur, and the surface roughness of the developing sleeve is maintained during long-term use, making it easy to improve the carrier transportability. In addition, if the silicon content is increased too much, the strength increases, but processing such as forming grooves becomes difficult, so from the viewpoint of processability, the upper limit of the silicon content is preferably 4.4% by mass or less.
[0053] It is preferable that the silicon content be in the range of more than 0.6 mass % and not more than 4.4 mass % relative to the total mass of the aluminum alloy, from the viewpoints of making the resistance of the developing sleeve uniform and suppressing peeling of the layer formed on the surface of the developing sleeve.
[0054] The aluminum alloy contains magnesium and manganese in addition to silicon to ensure strength, but if the magnesium or manganese content is too high and the strength is increased too much, it will affect, for example, the grooves formed on the surface of the developing sleeve and the runout accuracy required for the developing roller. Therefore, it is preferable that the magnesium content is 5.0 mass% or less because the runout accuracy is stabilized. From the same viewpoint as above, it is also preferable that the manganese content is 2.0 mass% or less. Note that "runout accuracy" means the total runout intersection in the axial or circumferential direction as defined by JIS B0021.
[0055] (1.2) Surface From the viewpoint of providing an appropriate surface roughness, it is preferable that the surface of the developing sleeve of the present invention does not have a resin layer. As described above, in the present invention, a sea-island structure in which silicon microcrystals (eutectic) are dispersed in the aluminum phase constituting the developing sleeve is formed, and appropriate unevenness is formed on the outer peripheral surface of the developing sleeve, thereby improving the durability of the developer transport ability.
[0056] Figure 4 is a diagram for explaining the state of silicon as a function of temperature change. For example, an aluminum alloy containing silicon (hereinafter, "aluminum alloy containing silicon" is also simply referred to as "Si-Al alloy") is a eutectic system with a eutectic point at 577°C and a silicon content of 12.6 mass%, as shown in Figure 4, and when the alloy in a liquid state (L) is cooled, it undergoes eutectic solidification.
[0057] Figure 5 shows some images of the eutectic state of the microstructure of a powder sample of an aluminum alloy containing silicon. Figure 5(a) shows the eutectic state of a silicon content of 7 mass%, Figure 5(b) shows the eutectic state of a silicon content of 12.6 mass%, and Figure 5(c) shows the eutectic state of a silicon content of 18 mass%.
[0058] Silicon crystals that crystallize in a eutectic state barely dissolve aluminum and grow as thin, narrow plate-like crystals as shown in Figure 5(b).On the other hand, when the silicon content increases to a hypereutectic state, anisotropic coarse crystals are formed as shown in Figure 5(c).
[0059] The surface of a Si-Al alloy in the eutectic composition region has a sea-island structure as shown in Figure 5(a) or Figure 5(b), and gives the surface roughness according to the silicon content (see Kitaokayama Osamu et al., Light Metals, Vol. 38, (7), 426, (1988)).
[0060] Although there is no particular limitation on the method for imparting an appropriate roughness to the surface of the developing sleeve of the present invention, it is preferable that the surface of the developing sleeve is subjected to sandblasting from the viewpoint of improving the transportability of the developer. By performing sandblasting, unevenness is formed on the surface of the developing sleeve, so that the roughness of the outer peripheral surface can be appropriately maintained and excellent transportability can be ensured.
[0061] When silicon is contained, the silicon is removed differently on the surface of the developing sleeve during sandblasting in the areas containing silicon and the areas not containing silicon, so that an appropriate surface roughness can be imparted.
[0062] Sandblasting is a process in which a blasting material is projected onto the surface of a developing sleeve to indent the surface with the blasting material, thereby forming an uneven shape. More specifically, examples of sandblasting include air blasting, wet sandblasting, and shot blasting.
[0063] There are no particular limitations on the materials that can be used for sandblasting, and any known materials can be used as appropriate.Specific examples include glass beads, alumina particles, silica particles, titania particles, and zirconia particles.Organic fine particles can also be used, such as melamine resin particles, benzoguanamine resin particles, and crosslinked acrylic resin particles.
[0064] As materials applicable to sandblasting, from the viewpoint of applying an impact force that dents the elastic layer but does not tear the surface of the outer layer, spherical glass beads and alumina beads are particularly preferable. These materials may be used alone or in combination of two or more.
[0065] The volume average particle size of the above material varies depending on the size of the irregularities on the surface of the desired developing sleeve, but is preferably within the range of 3 to 200 μm, more preferably within the range of 10 to 100 μm, and even more preferably within the range of 20 to 80 μm.
[0066] From the viewpoint of maintaining the transportability of the developer, it is preferable that the average length RSm of the roughness curve element of the surface of the developing sleeve is equal to or greater than the particle diameter of the carrier. In this specification, the "average length RSm of the roughness curve element" refers to the average distance between roughness peaks, and is in accordance with JIS standard B0601-2013 (Geometric Product Specifications (GPS)-Surface Quality: Profile Curve Method-Terminology, Definitions and Surface Quality Parameters). Hereinafter, the "average length RSm of the roughness curve element" is also simply referred to as "RSm". The "average length RSm of the roughness curve element of the developing sleeve surface" is the length of an element that corresponds to one period of undulations in the roughness curve.
[0067] Fig. 6 is a partially enlarged view of a portion of the undulations on the surface of the developing sleeve, and the above-mentioned "RSm" is, for example, the length represented by Rs1 in Fig. 6. Note that "RSm" according to the present invention is not limited to the groove shape as shown in Fig. 6, and may be, for example, the surface roughness measured on a surface without grooves. "Rsm" can be measured, for example, by a surface roughness measuring instrument (model: SE700) manufactured by Kosaka Laboratory Co., Ltd.
[0068] When the above Rsm is equal to or greater than the carrier particle size on the surface of the developing sleeve, the developer transport ability of the developing sleeve surface is improved, a decrease in the transport amount is suppressed, and the occurrence of density unevenness in halftone images can be suppressed.
[0069] It is preferable to have grooves on the surface of the developing sleeve from the viewpoint of improving the transportability of the developer. Fig. 7 is a partially enlarged view of a cross section of the developing sleeve. The groove 20 is a V-shaped groove formed by an upstream wall surface 21 located on the upstream side with respect to the rotation direction X of the developing sleeve 11 and a downstream wall surface 22 located on the downstream side.
[0070] The cross-sectional shape of the developing sleeve of the present invention is not limited to a V-groove shape such as the groove 20 shown in Fig. 7, and may be a flat-bottom shape or an arc shape. The developing sleeve 11 having the groove 20 formed on its surface in this manner has excellent wear resistance and excellent transportability of the developer carried on its surface. For example, by forming a plurality of grooves extending in the axial direction of the developing sleeve at predetermined intervals in the circumferential direction, the durability of the developing sleeve during long-term use is improved, and the transportability of the developer is also improved.
[0071] The groove depth D is preferably within a range of 40 to 120 μm from the viewpoint of excellent transportability. The groove depth D can be calculated by photographing with a laser microscope (model: VKX-200) manufactured by Keyence Corporation. The groove apex angle α is preferably 80° or more from the viewpoint of suppressing a decrease in transportability due to clogging of the developer, and is preferably 120° or less from the viewpoint of improving transportability of the developer. The number of grooves in the circumferential direction of the developing sleeve is preferably within a range of 40 to 120. The groove angle β in FIG. 7 is 9° when the number of grooves is 40, and is 3° when the number is 120.
[0072] In addition, the groove angle β in FIG. 7 is calculated by drawing a perpendicular line from a direction perpendicular to the surface of the developing sleeve to a specific vertex (vertex A) of the groove, and then measuring the line L A Draw a perpendicular line from the direction perpendicular to the surface of the developing sleeve to the vertex (vertex B) adjacent to the specific vertex A of the groove, and define the straight line as L. B Then, the line is L A and the line L B The groove angle is less than 90°.
[0073] 2. Toner for developing electrostatic images (2.1) Toner base particles The toner base particles according to the present invention may contain external additives such as a binder resin, a release agent, a colorant, a charge control agent, inorganic fine particles, organic fine particles, a lubricant, etc. In the present invention, the term "toner particles" refers to toner base particles to which external additives have been added, and an aggregate of toner particles is called "toner".
[0074] Generally, the toner base particles can be used as they are as toner particles, but in the present invention, the toner base particles to which external additives are added are used as toner particles. In the following description, when there is no need to particularly distinguish between the toner base particles and the toner particles, they are also simply referred to as "toner particles". Hereinafter, the details of each of the constituent materials of the toner base particles according to the present invention will be described.
[0075] (2.2) Binder resin As the binder resin contained in the toner base particles contained in the electrostatic image developing toner of the present invention, conventionally known binder resins, such as crystalline resins and non-crystalline resins, can be used.
[0076] "Binding resin (also called "binder resin")" refers to a resin that is used as a medium or matrix (parent body) for dispersing and retaining internal additives (releasing agents, charge control agents, colorants, etc.) and external additives (silica, titanium oxide, etc.) contained in toner particles, and has the function of adhering to a recording medium (e.g. paper) during the fixing process of a toner image.
[0077] The binder resin preferably contains at least a styrene-acrylic resin. By containing a styrene-acrylic resin, excessive bleeding of the release agent during toner fixing can be suppressed, fixing separation can be improved, and contamination inside the machine caused by the release agent can be suppressed. In addition, other known resins may be contained within a range that does not impair the effects of the present invention.
[0078] (Hybrid crystalline polyester resin) The binder resin may contain a hybrid crystalline polyester resin (hereinafter, simply referred to as "hybrid resin"). By containing a hybrid crystalline resin, the affinity with the amorphous resin used in combination is improved, so that the low-temperature fixability of the toner is improved. In addition, the dispersibility of the crystalline resin in the toner is improved, so that bleeding out can be suppressed. The hybrid resin may be one or more kinds. In addition, the hybrid resin may replace the entire amount of the crystalline polyester resin, or may replace a part of the crystalline polyester resin, or may be used in combination.
[0079] The hybrid resin is a resin in which a crystalline polyester polymerized segment and an amorphous polymerized segment are chemically bonded. The crystalline polyester polymerized segment means a portion derived from the crystalline polyester resin. That is, it means a molecular chain having the same chemical structure as the molecular chain constituting the crystalline polyester resin described above. The amorphous polymerized segment means a portion derived from the amorphous resin. That is, it means a molecular chain having the same chemical structure as the molecular chain constituting the amorphous resin described above.
[0080] The hybrid resin may further have a functional group such as a sulfonic acid group, a carboxy group, a urethane group, etc. The functional group may be introduced into the crystalline polyester polymer segment or into the amorphous polymer segment.
[0081] [Weight average molecular weight] From the viewpoint of reliably achieving both sufficient low-temperature fixing ability and excellent long-term storage stability, the weight-average molecular weight (Mw) of the hybrid resin is preferably within the range of 5,000 to 100,000, more preferably within the range of 7,000 to 50,000, and particularly preferably within the range of 8,000 to 20,000.
[0082] By setting the weight average molecular weight (Mw) of the hybrid resin to 100,000 or less, sufficient low-temperature fixing property can be obtained. On the other hand, by setting the weight average molecular weight (Mw) of the hybrid resin to 5,000 or more, excessive progress of compatibility between the hybrid resin and the amorphous resin during toner storage can be suppressed, and image defects due to fusion of toner particles can be effectively suppressed.
[0083] (Method of manufacturing hybrid resin) The hybrid resin can be produced, for example, by the following first to third production methods.
[0084] [First manufacturing method] The first manufacturing method is a method for manufacturing a hybrid resin by carrying out a polymerization reaction to synthesize a crystalline polyester polymer segment in the presence of a previously synthesized amorphous polymer segment. In this method, first, the monomers constituting the above-mentioned amorphous polymer segment (preferably vinyl monomers such as styrene monomers and (meth)acrylic acid ester monomers) are subjected to an addition reaction to synthesize the amorphous polymer segment.
[0085] Next, a polycarboxylic acid and a polyhydric alcohol are polymerized in the presence of the amorphous polymerized segment to synthesize a crystalline polyester polymerized segment. At this time, the polycarboxylic acid and the polyhydric alcohol are condensed, and the amorphous polymerized segment is subjected to an addition reaction with the polycarboxylic acid or the polyhydric alcohol to synthesize a hybrid resin.
[0086] In the first method, it is preferable to incorporate a site in the crystalline polyester polymer segment or the amorphous polymer segment that allows these polymer segments to react with each other. Specifically, when synthesizing the amorphous polymer segment, in addition to the monomer constituting the amorphous polymer segment, the amphoteric compound described above is also used.
[0087] The amphoteric compound reacts with a carboxy group or a hydroxy group in the crystalline polyester polymer segment, so that the crystalline polyester polymer segment is chemically and quantitatively bonded to the amorphous polymer segment. In addition, when synthesizing the crystalline polyester polymer segment, the monomer may further contain the above-mentioned compound having an unsaturated bond.
[0088] According to the first method, a hybrid resin having a structure (graft structure) in which a crystalline polyester polymer segment is molecularly bonded to an amorphous polymer segment can be synthesized.
[0089] [Second manufacturing method] The second manufacturing method is a method in which a crystalline polyester polymerized segment and an amorphous polymerized segment are formed in advance and then bonded to manufacture a hybrid resin. In this method, a polyvalent carboxylic acid and a polyhydric alcohol are first subjected to a condensation reaction to synthesize a crystalline polyester polymerized segment. In addition, the monomers constituting the above-mentioned amorphous polymerized segment are addition-polymerized to synthesize the amorphous polymerized segment, separately from the reaction system for synthesizing the crystalline polyester polymerized segment.
[0090] In this case, it is preferable to incorporate a site capable of reacting with the crystalline polyester polymer segment and the amorphous polymer segment into one or both of the crystalline polyester polymer segment and the amorphous polymer segment as described above.
[0091] Next, the synthesized crystalline polyester polymer segment and the amorphous polymer segment are reacted to synthesize a hybrid resin having a structure in which the crystalline polyester polymer segment and the amorphous polymer segment are molecularly bonded.
[0092] In addition, when the reactive site is not incorporated in either the crystalline polyester polymerization segment or the amorphous polymerization segment, a method may be adopted in which a compound having a site capable of bonding to both the crystalline polyester polymerization segment and the amorphous polymerization segment is added to a system in which the crystalline polyester polymerization segment and the amorphous polymerization segment coexist, thereby synthesizing a hybrid resin having a structure in which the crystalline polyester polymerization segment and the amorphous polymerization segment are molecularly bonded via the compound.
[0093] [Third manufacturing method] The third manufacturing method is a method for producing a hybrid resin by carrying out a polymerization reaction to synthesize an amorphous polymer segment in the presence of a crystalline polyester polymer segment. In this method, first, a polycarboxylic acid and a polyhydric alcohol are polymerized by a condensation reaction to synthesize a crystalline polyester polymer segment.
[0094] Next, in the presence of the crystalline polyester polymer segment, the monomers constituting the amorphous polymer segment are polymerized to synthesize the amorphous polymer segment. In this case, it is preferable to incorporate a site capable of reacting with each other in the crystalline polyester polymer segment or the amorphous polymer segment, as in the first production method.
[0095] By the above-mentioned method, a hybrid resin having a structure (graft structure) in which an amorphous polymerized segment is molecularly bonded to a crystalline polyester polymerized segment can be synthesized.
[0096] Among the first to third manufacturing methods, the first manufacturing method is preferred because it is easy to synthesize a hybrid resin having a structure in which a crystalline polyester resin chain is grafted to an amorphous resin chain and because it can simplify the production process. In the first manufacturing method, the amorphous polymerized segment is formed in advance and then the crystalline polyester polymerized segment is bonded to the amorphous polymerized segment, so that the orientation of the crystalline polyester polymerized segment is easily uniform.
[0097] (2.3) Release agent (wax) The release agent constituting the toner is not particularly limited, and known ones can be used.Specific examples thereof include polyolefin waxes such as polyethylene wax and polypropylene wax, branched chain hydrocarbon waxes such as microcrystalline wax, long chain hydrocarbon waxes such as paraffin wax and sazol wax, dialkyl ketone waxes such as distearyl ketone, carnauba wax, montan wax, behenyl behenate, trimethylolpropane tribehenate, pentaerythritol tetrabehenate, pentaerythritol diacetate dibehenate, glycerin tribehenate, 1,18-octadecanediol distearate, trimellitic acid tristearyl, distearyl maleate, and other ester waxes, and amide waxes such as ethylenediamine behenylamide and trimellitic acid tristearylamide.
[0098] The melting point of the release agent is preferably in the range of 60 to 100° C., more preferably in the range of 70 to 95° C. By setting the melting point within the above range, the heat-resistant storage property of the toner is ensured, and even when fixing is performed at a low temperature, a stable toner image can be formed without causing cold offset or the like. Here, in the present invention, the above-mentioned "melting point" refers to the endothermic peak temperature W 1 derived from the release agent observed during the first temperature rise in differential scanning calorimetry. (1) p (℃).
[0099] The content of the release agent in the toner is preferably within a range of 1 to 30% by mass, and more preferably within a range of 5 to 20% by mass.
[0100] (2.4) Colorants As colorants that can form the toner, carbon black, magnetic materials, dyes, pigments, etc. can be used arbitrarily. As carbon black, channel black, furnace black, acetylene black, thermal black, lamp black, etc. can be used.
[0101] As magnetic materials, ferromagnetic metals such as iron, nickel, and cobalt, alloys containing these metals, ferromagnetic metal compounds such as ferrite and magnetite, alloys that do not contain ferromagnetic metals but exhibit ferromagnetism when heat treated, such as alloys called Heusler alloys such as manganese-copper-aluminum and manganese-copper-tin, and chromium dioxide can be used.
[0102] Examples of black colorants that can be used include carbon black such as furnace black, channel black, acetylene black, thermal black, and lamp black, as well as magnetic powders such as magnetite and ferrite.
[0103] Examples of colorants for magenta or red include CI Pigment Red 2, 3, 5, 6, 7, 15, 16, 48:1, 53:1, 57:1, 60, 63, 64, 68, 81, 83, 87, 88, 89, 90, 112, 114, 122, 123, 139, 144, 149, 150, 163, 166, 170, 177, 178, 184, 202, 206, 207, 209, 222, 238, and 269.
[0104] Examples of colorants for orange or yellow include CI Pigment Orange 31, CI Pigment Orange 43, CI Pigment Yellow 12, 14, 15, 17, 74, 83, 93, 94, 138, 155, 162, 180, and 185.
[0105] Furthermore, examples of colorants for green or cyan include CI Pigment Blue 2, 3, 15, 15:2, 15:3, 15:4, 16, 17, 60, 62, 66, CI Pigment Green 7, and the like.
[0106] These colorants can be used alone or in combination of two or more, as required.
[0107] The amount of the colorant added is preferably within the range of 1 to 30% by mass, more preferably within the range of 2 to 20% by mass, based on the total amount of the toner, and a mixture of these may also be used, and within such a range, color reproducibility of the image can be ensured. The size of the colorant, in terms of volume average particle diameter, is preferably within the range of 10 to 1000 nm, more preferably within the range of 50 to 500 nm, and even more preferably within the range of 80 to 300 nm.
[0108] (2.5) Charge control agents As the charge control agent, various known compounds such as nigrosine dyes, metal salts of naphthenic acid or higher fatty acids, alkoxylated amines, quaternary ammonium salt compounds, azo metal complexes, and metal salicylate can be used.
[0109] The amount of the charge control agent added is usually within the range of 0.1 to 10% by mass, preferably within the range of 0.5 to 5% by mass, based on 100% by mass of the binder resin in the finally obtained toner particles. The size of the charge control agent particles is within the range of 10 to 1000 nm, preferably within the range of 50 to 500 nm, and particularly preferably within the range of 80 to 300 nm, in terms of number average primary particle diameter.
[0110] (2.6) External additives From the viewpoint of improving the charging performance, fluidity, or cleaning properties of the toner, known particles such as inorganic fine particles or organic fine particles, or lubricants can be added as external additives to the surface of the toner particles.
[0111] Preferable examples of the inorganic fine particles include inorganic fine particles made of silica, titania, alumina, strontium titanate, etc. If necessary, these inorganic fine particles may be subjected to a hydrophobic treatment.
[0112] As the organic fine particles, spherical organic fine particles having a number average primary particle diameter in the range of about 10 to 2000 nm can be used. Specifically, organic fine particles made of homopolymers such as styrene and methyl methacrylate, or copolymers thereof can be used.
[0113] The lubricant is used for the purpose of further improving the cleaning property and transfer property, and examples of the lubricant include metal salts of higher fatty acids such as salts of stearic acid such as zinc, aluminum, copper, magnesium, calcium, etc., salts of oleic acid such as zinc, manganese, iron, copper, magnesium, etc., salts of palmitic acid such as zinc, copper, magnesium, etc., salts of linoleic acid such as zinc, calcium, etc., and salts of ricinoleic acid such as zinc, calcium, etc. Various types of these external additives may be used in combination.
[0114] The amount of the external additive added is preferably within a range of 0.1 to 10.0% by mass relative to 100% by mass of the toner particles.
[0115] Examples of the method for adding the external additives include methods using various known mixing devices such as a Turbula mixer, a Henschel mixer, a Nauta mixer, and a V-type mixer.
[0116] (2.7) Toner particles (Core-shell structure) The toner base particles can be used as they are in a toner, but may also be toner particles having a multilayer structure such as a core-shell structure comprising the toner base particles as a core particle and a shell layer covering the surface of the core particle.
[0117] The shell layer does not have to cover the entire surface of the core particle, and the core particle may be partially exposed. The cross section of the core-shell structure can be confirmed by known observation means such as a transmission electron microscope (TEM) or a scanning probe microscope (SPM).
[0118] In the case of a core-shell structure, the core particle and the shell layer can have different properties such as glass transition point, melting point, and hardness, making it possible to design toner particles according to the purpose. For example, a shell layer can be formed by aggregating and fusing a resin with a relatively high glass transition point (Tg) to the surface of a core particle that contains a binder resin, a colorant, a release agent, etc. and has a relatively low glass transition point (Tg). The shell layer preferably contains an amorphous resin.
[0119] (particle size) The particle size of the toner particles is the volume-based median diameter (d 50 ) is preferably in the range of 3 to 10 μm, and more preferably in the range of 5 to 8 μm. Within the above range, high reproducibility can be obtained even for very fine dot images at a 1200 dpi level. The particle size of the toner particles can be controlled by the concentration of the coagulant used during production, the amount of organic solvent added, the fusion time, the composition of the binder resin, etc.
[0120] The volume-based median diameter of the toner particles (d 50 For the measurement of , a measuring device consisting of a Multisizer 3 (Beckman Coulter) connected to a computer system equipped with data processing software Software V3.51 can be used.
[0121] Specifically, the measurement sample (toner) is added to a surfactant solution (a surfactant solution prepared by diluting, for example, a neutral detergent containing a surfactant component 10 times with pure water in order to disperse toner particles) and allowed to mix, and then ultrasonic dispersion is performed to prepare a toner particle dispersion.
[0122] This toner particle dispersion is pipetted into a beaker containing ISOTON II (manufactured by Beckman Coulter) in a sample stand until the concentration indicated on the measuring device reaches 8%. By achieving this concentration, it is possible to obtain reproducible measurement values. Then, in the measuring device, the number of measured particles is set to 25,000, the aperture diameter is set to 100 μm, the measurement range of 2 to 60 μm is divided into 256 parts, and the frequency value is calculated. The particle diameters of the 50% with the largest volume cumulative fraction are taken as the volume-based median diameter (d 50 ) is obtained.
[0123] (Average circularity) From the viewpoint of improving the stability of the chargeability and the low-temperature fixability, the toner particles preferably have an average circularity in the range of 0.930 to 1.000, more preferably in the range of 0.950 to 0.995. When the average circularity is within the above range, the individual toner particles are less likely to be crushed. This makes it possible to suppress contamination of the frictional charge imparting member, stabilize the chargeability of the toner, and improve the image quality of the formed image.
[0124] The average circularity of the toner particles can be measured using an FPIA-2100 (manufactured by Sysmex Corp.) Specifically, a measurement sample (toner) is mixed with an aqueous solution containing a surfactant, and dispersed by ultrasonic dispersion treatment for 1 minute.
[0125] Then, an image is taken using an FPIA-2100 (manufactured by Sysmex) under the measurement conditions of HPF (high magnification imaging) mode at an appropriate density of 3,000 to 10,000 HPF detection numbers. If the HPF detection number is within the above range, reproducible measurement values can be obtained. From the captured particle images, the circularity of each toner particle is calculated according to the following formula (I), and the circularity of each toner particle is added and divided by the total number of toner particles to obtain an average circularity. Formula (I): Circularity = (perimeter of a circle with the same projected area as the particle image) / (perimeter of the projected particle image)
[0126] 3. Manufacturing method of toner for developing electrostatic images As a method for producing the toner for developing electrostatic images according to the present invention, for example, an emulsion polymerization aggregation method or an emulsion aggregation method can be suitably adopted.
[0127] The emulsion polymerization aggregation method is a method for producing toner particles by mixing a dispersion of fine particles of a binder resin (hereinafter also referred to as "binder resin fine particles") produced by the emulsion polymerization method with a dispersion of fine particles of a colorant (hereinafter also referred to as "colorant fine particles") and a dispersion of a release agent such as wax, aggregating the toner particles until they reach a desired particle size, and further controlling the shape by fusing the fine particles of the binder resin together.
[0128] The emulsion aggregation method is a method for producing toner particles by dropping a binder resin solution dissolved in a solvent into a poor solvent to prepare a resin fine particle dispersion, mixing this resin fine particle dispersion with a colorant dispersion and a release agent dispersion such as wax, aggregating the particles to a desired toner particle size, and further controlling the shape by fusing the binder resin fine particles together.
[0129] Either method can be applied to the toner of the present invention. An example of the method for producing the toner of the present invention using the emulsion polymerization aggregation method will be described below. (1) A step of preparing a dispersion liquid in which fine particles of a colorant are dispersed in an aqueous medium. (2) A step of preparing a dispersion in which binder resin particles, optionally containing an internal additive, are dispersed in an aqueous medium. (3) A process for preparing a dispersion of binder resin particles by emulsion polymerization. (4) A process of mixing a dispersion of colorant particles with a dispersion of binder resin particles, and forming toner base particles by agglomerating, associating, and fusing the colorant particles and the binder resin particles. (5) A process of filtering the toner base particles from the dispersion system (aqueous medium) and removing surfactants, etc. (6) Drying the toner base particles (7) A process of adding external additives to the toner base particles
[0130] When a toner is produced by the emulsion polymerization aggregation method, the binder resin particles obtained by the emulsion polymerization method may have a multi-layer structure of two or more layers made of binder resins with different compositions. Binder resin particles having such a configuration, for example, those having a two-layer structure, can be obtained by a method in which a dispersion of resin particles is prepared by a conventional emulsion polymerization process (first-stage polymerization), a polymerization initiator and a polymerizable monomer are added to this dispersion, and this system is polymerized (second-stage polymerization). In addition, toner particles having a core-shell structure can also be obtained by the emulsion polymerization aggregation method.
[0131] Specifically, toner particles having a core-shell structure are first prepared by aggregating, associating, and fusing binder resin particles for the core particles and colorant particles, and then adding binder resin particles for the shell layer to a dispersion of the core particles to aggregate and fuse the binder resin particles for the shell layer to the surface of the core particles, thereby forming a shell layer that covers the surface of the core particles.
[0132] An example of the method for producing the toner of the present invention using a pulverization method will be described below. (1) A process in which binder resin, colorant, and internal additives (if necessary) are mixed using a Henschel mixer or similar. (2) A step of kneading the obtained mixture while heating it using an extrusion kneader or the like. (3) A step of subjecting the obtained kneaded product to coarse pulverization using a hammer mill or the like, and then further pulverization using a turbo mill or the like. (4) A process of classifying the obtained pulverized material into fine powder using, for example, an air classifier utilizing the Coanda effect to form toner base particles. (5) A process of adding external additives to the toner base particles
[0133] The embodiments to which the present invention can be applied are not limited to the above-described embodiments, and can be modified as appropriate without departing from the spirit of the present invention.
[0134] 4. Developer The toner for developing electrostatic images of the present invention is mixed with a carrier to be used as a two-component developer, but various components can be added depending on the purpose, and the developer is not limited to being two-component.
[0135] When the toner is used as a two-component developer, the carrier may be magnetic particles made of conventionally known materials such as metals such as iron, ferrite, and magnetite, and alloys of these metals with metals such as aluminum and lead, with ferrite particles being particularly preferred.
[0136] The carrier may be a coated carrier in which the surface of magnetic particles is coated with a coating agent such as resin, or a dispersion type carrier in which magnetic fine powder is dispersed in a binder resin. 50 The volume-based median diameter (d 50 ) can be measured, for example, by a laser diffraction particle size distribution measuring device HELOS (manufactured by SYMPATEC) equipped with a wet disperser.
[0137] 5. Electrophotographic Image Forming Apparatus The electrophotographic image forming apparatus of the present invention is an electrophotographic image forming apparatus having a developing sleeve for conveying a developer containing a toner and a carrier, characterized in that the developing sleeve is made of an aluminum alloy containing more than 0.6% by mass of silicon, and further comprising, for example, a charging means, an exposure means, a developing means, and a transfer means.
[0138] 8 is an explanatory cross-sectional view showing an example of the configuration of an electrophotographic image forming apparatus of the present invention. The image forming apparatus 100 shown in FIG. 8 is called a tandem type color image forming apparatus, and has four image forming units 110Y, 110M, 110C, and 110Bk, a paper feed conveying means 150, and a fixing means 170.
[0139] An original image reading device SC is disposed on the upper portion of the main body of the image forming apparatus 100.
[0140] The image forming units 110Y, 110M, 110C, and 110Bk are arranged in a vertical line. The image forming units 110Y, 110M, 110C, and 110Bk each include a rotating drum-shaped photoconductor 111Y, 111M, 111C, and 111Bk, charging means 113Y, 113M, 113C, and 113Bk, exposure means 115Y, 115M, 115C, and 115Bk, developing means 117Y, 117M, 117C, and 117Bk, primary transfer rollers (primary transfer means) 133Y, 133M, 133C, and 133Bk, and cleaning means 119Y, 119M, 119C, and 119Bk, which are arranged in sequence along the rotation direction of the photoconductor in the outer circumferential surface area of the drum-shaped photoconductor 111Y, 111M, 111C, and 111Bk.
[0141] A configuration is adopted in which toner images of yellow (Y), magenta (M), cyan (C) and black (Bk) are formed on the photoconductors 111Y, 111M, 111C and 111Bk, respectively.
[0142] In the following description, the image forming unit 110Y will be taken as an example when referring to the drawings.
[0143] <Charging means> The charging means is a means for uniformly charging the surface of the photoreceptor. There are contact types such as a charging roller, a charging brush, and a charging blade, and non-contact types such as a corona charger (a corotron charger, a strocotton charger, etc.).
[0144] The contact type has the advantage that the amount of harmful ozone gas generated during the charging process is small. The non-contact type has the advantage that filming is less likely to occur because it is not a close-proximity discharge compared to the contact type. The charging means provided in the image forming system of the present invention may be of either a contact type or a non-contact type.
[0145] It is preferable that the charging means is a proximity charging roller or a contact charging roller, since this reduces the amount of harmful ozone gas generated during the charging process and is advantageous for achieving high image quality and miniaturization of the apparatus.
[0146] 8 is of a contact type. The charging means 113Y in this example is made up of a charging roller disposed in contact with the surface of the photoconductor 111Y, and a power source that applies a voltage to the charging roller.
[0147] <Exposure means> The exposure means is a means for exposing the photoconductor, which has been given a uniform potential by the charging means, based on an image signal to form an electrostatic latent image corresponding to the image. Examples of the exposure means include those consisting of LEDs and imaging elements in which light emitting elements are arranged in an array in the axial direction of the photoconductor, and those consisting of a laser optical system.
[0148] <Developing method> The developing means (developing machine) is a means for supplying a developer to the surface of the photoconductor to develop the electrostatic latent image formed on the surface of the photoconductor and form a toner image. The developer used is a developer containing the above-mentioned toner and carrier.
[0149] The developing means may be provided with a lubricant supplying means for supplying a lubricant to the developer, and it is preferable that the developer supplied by the developing means contains a lubricant from the viewpoint of improving abrasion resistance. It is more preferable that the lubricant is a metal soap from the viewpoint of improving abrasion resistance.
[0150] The developing means 117Y shown in FIG. 8 is specifically composed of a developing roller 118Y that has a built-in magnet and rotates while holding a developer, and a voltage application device (not shown) that applies a DC and / or AC bias voltage between the photoconductor 111Y and the developing roller 118Y.
[0151] The developing roller is composed of the developing sleeve, the flange, the shaft, and the magnet roller as described above. The aluminum alloy of the developing roller has a silicon content of more than 0.6 mass %.
[0152] The developer is transported to the photoconductor 111Y by the rotation of the developing roller 118Y. Then, a thin layer of toner on the developing roller 118Y comes into contact with the photoconductor 111Y to develop the electrostatic latent image on the photoconductor 111Y.
[0153] The developing roller 118Y is connected to a voltage application device. This voltage application device applies a DC and / or AC bias voltage to the developing roller 118Y. The developing bias can be adjusted to a desired value by controlling the voltage applied to the developing roller 118Y.
[0154] An electric field is formed in a development section where the development roller 118Y and the photoconductor 111Y face each other due to a potential difference (development potential difference) between the development roller 118Y and the potential of the electrostatic latent image carried by the photoconductor 111Y. The toner in the developer transported to the development section by the rotation of the development roller 118Y moves due to the force exerted by the electric field, and is attracted to the electrostatic latent image on the photoconductor 111Y.
[0155] The electrostatic latent image carried on the photoconductor 111Y is visualized, so that a toner image corresponding to the shape of the electrostatic latent image is formed on the surface of the photoconductor 111Y.
[0156] <Transfer Method> The transfer means is a means for transferring the toner image on the photoreceptor to a transfer body (intermediate transfer body or transfer material). When an intermediate transfer body is used, the primary transfer roller becomes the transfer means. Since the "transfer means" in the present invention is a means for transferring the "toner image on the photoreceptor", the secondary transfer roller used when transferring from the intermediate transfer body to the transfer material is not included in the "transfer means".
[0157] 8 transfers the toner image formed on the photoconductor 111Y onto the endless belt-like intermediate transfer body 131. The primary transfer roller 133Y is disposed in contact with the intermediate transfer body 131.
[0158] In the image forming apparatus 100 shown in FIG. 8, an intermediate transfer method is adopted in which the toner images formed on the photoconductors 111Y, 111M, 111C, and 111Bk are transferred to the intermediate transfer body 131 by primary transfer rollers (primary transfer means) 133Y, 133M, 133C, and 133Bk, and each toner image transferred to the intermediate transfer body 131 is transferred to the transfer material P by a secondary transfer roller (secondary transfer means) 217. However, a direct transfer method may also be adopted in which the toner images formed on the photoconductors are transferred directly to the transfer material P by a transfer means. EXAMPLES
[0159] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto. In the examples, the terms "parts" and "%" are used, but they represent "parts by mass" or "% by mass" unless otherwise specified.
[0160] A. Preparation of developing sleeve 1 (A.1) Preparation of hollow cylindrical tube made of aluminum alloy A hollow cylindrical tube was produced using an aluminum alloy containing silicon (Si), in which the silicon (Si) content was 0.65 mass%, the magnesium (Mg) content was 0.03 mass%, and the manganese (Mn) content was 0.01 mass%, relative to the total mass of the aluminum alloy.
[0161] (A.2) Groove formation The developing sleeve 1 was produced by forming V-groove surface shapes at equal intervals in the circumferential direction on the hollow cylindrical tube, and spraying glass beads with a blast gun to sandblast the outer peripheral surface of the cylinder. As shown in FIG. 7, for example, the V-groove has a groove depth D of 75±25 μm, a V-groove apex angle α of 100°, 40 grooves in the circumferential direction of the developing sleeve, and a groove angle β of 9°. The developing sleeve 1 has an outer diameter of 16 mm and a thickness of 1 mm. The processing conditions for the sandblasting treatment are as follows:
[0162] <Processing conditions> Glass bead type: FGB#80 (manufactured by Fuji Manufacturing) Glass beads feed rate: 200g / min Distance from blast gun to cylinder: 100mm Blast gun movement speed: 5.0cm / sec Compressed air pressure: 0.23MPa Cylinder rotation speed: 545 rpm
[0163] The surface of the developing sleeve 1 was photographed with a laser microscope (model: VKX-200) manufactured by Keyence Corporation, and the depth D of the grooves in the circumferential direction of the support was measured. Specifically, 12 points in total, 3 points in the axial direction of the support and 4 points in the circumferential direction, were photographed at 500x magnification. The photographed images were binarized using image analysis software, and the depth D of all linear grooves on the image was calculated. The range of the depth D of linear grooves that accounted for 90% or more of the total was calculated from the calculated linear groove depths, and was found to be 100 μm.
[0164] B. Preparation of developing sleeves 2 to 19 (B.1) Preparation of aluminum alloy and fabrication of hollow cylindrical tube The aluminum alloys containing silicon (Si) shown in Table I were used to prepare hollow cylindrical tubes.
[0165] (B.2) Groove formation Grooves were formed in the hollow cylindrical tube at equal intervals in the circumferential direction to form a V-groove surface shape. For the V-groove, a groove similar to that of developing sleeve 1 was formed with a groove depth D of 75±25 μm, a V-groove apex angle α of 100°, 40 grooves in the circumferential direction of the developing sleeve, and a groove angle β of 9°, as shown in Fig. 7. No V-grooves were formed in developing sleeves 5 and 6.
[0166] Further, the developing sleeves 2 to 17 and 19 were subjected to sandblasting treatment as shown in Table I. The developing sleeve 18 was not subjected to sandblasting treatment. The developing sleeves 2 to 19 all had an outer diameter of 16 mm and a thickness of 1 mm.
[0167] C. Preparation of developing rollers 1 to 19 A magnet roller, a shaft and a flange were attached to the above developing sleeves 1 to 19 to prepare developing rollers 1 to 19.
[0168] D. Toner Preparation (D.1) Preparation of resin particle dispersion (D.1.1) Preparation of crystalline resin [Preparation of crystalline resin (1a)] The raw material monomer (1a-1) of the following addition polymerization resin (styrene-acrylic resin) segment containing a bireactive monomer and 4 parts by mass of di-t-butyl peroxide as a radical polymerization initiator were placed in a dropping funnel.
[0169] <Raw material monomer (1a-1)> Styrene 20.0 parts by mass n-Butyl acrylate 8 parts by weight Acrylic acid 1.75 parts by mass
[0170] Furthermore, the raw material monomer (1a-2) of the polycondensation resin (crystalline polyester resin) segment described below was placed in a four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer and a thermocouple, and heated to 170° C. to dissolve.
[0171] <Raw material monomer (1a-2)> Sebacic acid (acid) 412.6 parts by mass 1,6-Hexanediol (alcohol) 152.6 parts by mass
[0172] Next, the monomers (1a-1) and (1a-2) were placed in a reaction vessel equipped with a stirrer, a thermometer, a cooling tube, and a nitrogen gas inlet tube, and the atmosphere in the reaction vessel was replaced with dry nitrogen gas to obtain a mixed liquid.
[0173] To the resulting mixture, 0.4 parts by mass of Ti(On-Bu)4 was added, the temperature was raised to 235°C, and the reaction was carried out under normal pressure (101.3 kPa) for 5 hours, and further under reduced pressure (8 kPa) for 1 hour to obtain a reaction liquid.
[0174] The resulting reaction liquid was cooled to 200° C., and then reacted under reduced pressure (20 kPa) until the acid value calculated by the above-mentioned measurement method became 20.0 mgKOH / g, thereby producing a crystalline resin (1a).
[0175] (D.1.2) Preparation of dispersion [Preparation of Crystalline Resin Particle Dispersion (1A)] 174.3 parts by mass of crystalline resin (1a) and 102 parts by mass of methyl ethyl ketone were placed in a reaction vessel and dissolved by stirring at 75° C. for 30 minutes, and 3.1 parts by mass of a 25% by mass aqueous sodium hydroxide solution was added to obtain a solution.
[0176] The above-mentioned solution was placed in a reaction vessel equipped with a stirrer, and 375 parts by mass of water heated to 70° C. was added dropwise to the solution while stirring over a period of 70 minutes. During the dropping, the liquid in the container became cloudy, and after the entire amount was dropped, the liquid became uniformly emulsified, giving an emulsion (1a).
[0177] While keeping the above emulsion at 70°C, the pressure was reduced to 15 kPa (150 mbar) using a diaphragm vacuum pump "V-700" (manufactured by BUCHI), and the mixture was stirred for 3 hours to distill off methyl ethyl ketone. Thereafter, the mixture was cooled at a cooling rate of 6° C. / min to prepare a crystalline resin particle dispersion (1A) in which fine particles of the crystalline resin (1a) were dispersed.
[0178] The volume average particle size of the crystalline resin (1a) in the crystalline resin microparticle dispersion (1A) was measured using a particle size distribution measuring instrument (laser diffraction particle size distribution measuring instrument "LA-750 (manufactured by HORIBA)"), and the volume average particle size of the crystalline resin (1a) was found to be 202 nm.
[0179] (D.1.3) Styrene-acrylic modified crystalline polyester composition ratio and melting point The melting point of the crystalline resin (1a) in the crystalline resin particle dispersion (1A) is 62°C.
[0180] The styrene-acrylic modified crystalline polyester composition ratio is 95 parts by mass of the crystalline polyester segment and 5 parts by mass of the styrene-acrylic copolymer segment. The styrene-acrylic modified crystalline polyester composition ratio is a value calculated from the total mass (29.75 parts by mass) of the raw material monomer (1a-1) and the total mass (565.2 parts by mass) of the raw material monomer (1a-2) when preparing the crystalline resin (1a).
[0181] As described above, in the present invention, the "melting point" refers to the endothermic peak temperature C of the crystalline resin observed during the first heating process in differential scanning calorimetry. (1) p (℃), and "melting point" is the above C (1) p(℃).
[0182] (D.2) Preparation of amorphous resin particle dispersion [Preparation of amorphous resin particle dispersion (1)] (First stage polymerization) A 5 L reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, and a nitrogen introducing device was charged with 8 parts by mass of sodium dodecyl sulfate and 3,000 parts by mass of ion-exchanged water, and the internal temperature was raised to 80° C. while stirring at a stirring speed of 230 rpm under a nitrogen stream. After the temperature was raised, a solution in which 10 parts by mass of potassium persulfate was dissolved in 200 parts by mass of ion-exchanged water was added, the liquid temperature was again raised to 80° C., and a mixed liquid of the following raw material monomer (1b-1) was added dropwise over 1 hour.
[0183] <Raw material monomer (1b-1)> Styrene 480.0 parts by mass n-Butyl acrylate 250.0 parts by mass Methacrylic acid 68.0 parts by mass
[0184] After the dropwise addition of the mixed liquid, the mixture was heated and stirred at 80° C. for 2 hours to polymerize the raw material monomer (1b-1) to prepare a vinyl resin particle dispersion (S1) as a first-stage polymerization liquid.
[0185] (Second stage polymerization) In a 5L reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, and a nitrogen introduction device, 1100 parts by mass of ion-exchanged water and 289 parts by mass of the vinyl resin microparticle dispersion (S1) (first-stage polymerization liquid) prepared by the first-stage polymerization were charged and heated to 87° C. Then, a mixture of the raw material monomer (1b-2), chain transfer agent, and release agent, which was dissolved at 85° C., was mixed and dispersed for 10 minutes using a mechanical disperser CLEARMIX (manufactured by M-Technique Co., Ltd.) with a circulation path, to prepare a dispersion containing emulsified particles (oil droplets).
[0186] <Raw material monomer (1b-2)> Styrene 253.0 parts by mass 2-Ethylhexyl acrylate 107.3 parts by mass Methacrylic acid 39.2 parts by mass
[0187] <Chain transfer agent> n-Octyl-3-mercaptopropionate 4.45 parts by mass
[0188] <Release agent> Behenic acid behenate 120.0 parts by mass
[0189] The above dispersion was added to the 5 L reaction vessel, and a solution of a polymerization initiator in which 5.5 parts by mass of potassium persulfate was dissolved in 103 parts by mass of ion-exchanged water was added. The system was heated and stirred at 87°C for 1 hour to polymerize, thereby preparing a vinyl resin microparticle dispersion (S1').
[0190] (Third stage polymerization) A solution of 7.4 parts by mass of potassium persulfate dissolved in 157.9 parts by mass of ion-exchanged water was added to the vinyl resin particle dispersion (S1') obtained by the second-stage polymerization. Further, a mixture of the following raw material monomer (1b-3) and a chain transfer agent was added dropwise over 90 minutes at a temperature of 84°C.
[0191] <Raw material monomer (1b-3)> Styrene 335.0 parts by mass n-Butyl acrylate 211.0 parts by mass Methacrylic acid 44.0 parts by mass n-Octyl-3-mercaptopropionate 8.1 parts by mass
[0192] After the dropwise addition was completed, polymerization was carried out by heating and stirring for 2 hours, and then the mixture was cooled to 28° C. to obtain a non-crystalline resin particle dispersion (1).
[0193] (D.3) Preparation of colorant particle dispersion 226 parts by mass of sodium dodecyl sulfate was added to 1600 parts by mass of ion-exchanged water, and 420 parts by mass of copper phthalocyanine (CI Pigment Blue 15:3) was gradually added while stirring the solution. A dispersion process was carried out using a stirring device Clearmix (manufactured by M Technique Co., Ltd., "Clearmix" is a registered trademark of the company) to prepare a colorant particle dispersion (P1). The volume-based median diameter of the colorant particles in the colorant particle dispersion (P1) was measured and found to be 110 nm.
[0194] (D.4) Preparation of toner particles Into a reaction vessel equipped with a stirrer, a temperature sensor, and a cooling tube, 480 parts by mass (solid content equivalent) of the amorphous resin particle dispersion (1) and 350 parts by mass of ion-exchanged water were added. At room temperature (25°C), a 5 mol / L aqueous sodium hydroxide solution was added to adjust the pH to 10. Furthermore, 36.4 parts by mass (solid content equivalent) of the colorant particle dispersion (P1) was added, and 80 parts by mass of a 50% by mass aqueous magnesium chloride solution was added over 10 minutes at 30°C while stirring to obtain a dispersion.
[0195] The resulting dispersion was allowed to stand for 5 minutes, then heated to 82°C over 60 minutes. After reaching 82°C, 59.3 parts by mass (solid content equivalent) of crystalline resin microparticle dispersion (1A) was added over 20 minutes, and the stirring speed was adjusted so that the particle size growth rate was 0.01 μm / min. The particles were allowed to grow until the volume-based median diameter measured using a Coulter Multisizer 3 (manufactured by Coulter Beckman) reached 6.0 μm.
[0196] Next, an aqueous solution of 80 parts by mass of sodium chloride dissolved in 300 parts by mass of ion-exchanged water was added to stop the growth of particle diameter. Next, the mixture was stirred at 82°C to allow the particles to fuse together until the average circularity of the toner particles reached 0.970, and then cooled at a temperature drop rate of 0.5°C / min or more to lower the liquid temperature to 30°C or lower. Next, solid-liquid separation was performed, and the dehydrated toner cake was redispersed in ion-exchanged water and washed by repeating the solid-liquid separation operation three times. After washing, the mixture was dried at 35°C for 24 hours to produce toner particles (1).
[0197] (D.5) Mixing of external additives 100 parts by mass of the obtained toner particles (1), 0.6 parts by mass of hydrophobic silica particles (number average primary particle size: 12 nm, hydrophobicity: 68), 1.0 part by mass of hydrophobic titanium oxide particles (number average primary particle size: 20 nm, hydrophobicity: 63), and 1.0 part by mass of sol-gel silica (number average primary particle size = 110 nm) were mixed in a Henschel mixer (manufactured by Nippon Coke and Engineering Co., Ltd.) at a rotor circumferential speed of 35 mm / sec and 32°C for 20 minutes. After mixing, coarse particles were removed using a sieve with 45 μm openings, and toner (1) was obtained.
[0198] E. Carrier Mixing Toner (1) and ferrite carrier with a volume average particle size of 33 μm coated with acrylic resin were added and mixed so that the concentration of toner (1) was 6 mass %. By the above process, a two-component developer [1] containing toner (1) was prepared.
[0199] F. Evaluation (RSm) [Preparation] Each of the developed sleeves was attached to the developing roller used in the developing means of the "bizhub C658" (Konica Minolta) in a normal temperature and humidity environment (NN environment: 23°C, 50% RH). In addition, two-component developer [1] was loaded.
[0200] [Evaluation method] After that, a durability test was conducted on the A3 size transfer material: "POD Gloss Coat (100g / m 2 After continuously printing 1 million sheets (1000 kp) of halftone images and solid images on a "Print Paper" (Oji Paper Co., Ltd.), the RSm values after the durability test (after continuous printing) were measured using the method described below. The RSm values were summarized in Table I together with the RSm values before the durability test for comparison.
[0201] The surface roughness of each of the developed sleeves thus produced was measured using a surface roughness measuring instrument (model: Surfcom 1400G) manufactured by Tokyo Seimitsu Co., Ltd. and a surface roughness measuring instrument (model: SE700) manufactured by Kosaka Laboratory Co., Ltd. under the following measurement conditions, and a roughness curve was calculated.
[0202] <Measurement conditions> Measurement length 8.000mm Measurement speed 0.150mm / s Measurement range: ±64.000μm Calculation standard JIS B 0601:2013 Measurement type: Roughness measurement Shape removal Least squares Straight line evaluation length 8.000mmλs No filter Cutoff type: Gaussian Cutoff wavelength (λc) 0.08mm Pickup Type Standard Pickup The measurements were performed under the conditions of a cutoff value of 0.8 mm, a measurement length of 8,000 mm, and a data interval of 1.6 μm.
[0203] From the calculated surface roughness curve of each developing sleeve, the average length Rsm of the roughness curve element of the developing sleeve surface was calculated in accordance with JIS B 0601:2013.
[0204] (Developer transport amount) [Preparation] Each of the developed sleeves was attached to the developing roller used in the developing means of the "bizhub C658" (Konica Minolta) in a normal temperature and humidity environment (NN environment: 23°C, 50% RH). In addition, two-component developer [1] was loaded.
[0205] [Evaluation method] After that, a durability test was conducted on the A3 size transfer material: "POD Gloss Coat (100g / m 2 After continuously printing 1 million sheets (1000 kp) of halftone images and solid images on a "Printer Printer" (Oji Paper Co., Ltd.), the developer transport amount after the durability test (after continuous printing) was calculated using the following method, and was summarized in Table I together with the value before the durability test for comparison.
[0206] The developer transport amount before the durability test was calculated as follows.
[0207] Before starting the actual evaluation, the developing unit was removed from the main body of the "bizhub C658" (Konica Minolta). The developing unit contained developer, and developer was already held on the surface of the developing sleeve, so the amount of developer held per unit area was sucked in by a suction mechanism such as a pump while pressing a mask jig shaped as shown in Figure 9(a). The amount of developer transported per unit area [g / m 2 ] was calculated from the mass before and after suction. 2 The suction mechanism used was a pump shaped like a straw with a diameter of about 1 mm. The area of the surface S of the mask jig applied to the surface of the developing sleeve (the area of the mask jig facing the surface of the developing sleeve) was 10 cm 2 It was.
[0208] Fig. 9(a) is a schematic three-dimensional diagram showing the shape of the mask jig. Fig. 9(b) is a schematic plan view showing the state before the mask jig is pressed against the developing sleeve, and Fig. 9(c) is a schematic plan view showing the state after the mask jig is pressed against the developing sleeve. In Figs. 9(a), (b) and (c), surface S represents the area that comes into contact with the surface of the developing sleeve 11 when the mask jig M is pressed against the surface of the developing sleeve 11, and this portion is hollow. Moreover, the surface S is arc-shaped to match the surface of the developing sleeve 11. Note that T represents the developer.
[0209] Regarding the amount of developer transported after the durability test, the developing unit was removed from the machine body of the "bizhub C658" (manufactured by Konica Minolta) after the durability test (after continuous printing), and the amount of developer transported after the durability test was calculated in the same manner as the amount of developer transported before the durability test.
[0210] (Uneven density) [Preparation] Each of the developed sleeves was attached to the developing roller used in the developing means of the "bizhub C658" (Konica Minolta) in a room temperature and humidity environment (NN environment: 23°C, 50% RH). In addition, two-component developer [1] was loaded.
[0211] [Evaluation method] Before the durability test at the beginning of printing, A3 size transfer material: "POD Gloss Coat (100g / m 2 A halftone image and a solid image were printed on the entire surface of a transfer sheet of "POD Gloss Coat (100g / m 2 After printing halftone and solid images on 1 million sheets (1000kp) of paper (Oji Paper Co., Ltd.), the paper was immediately transferred onto a new A3-sized transfer material, "POD Gloss Coat (100g / m 2 A halftone image and a solid image were printed on the entire surface of a paper (manufactured by Oji Paper Co., Ltd.) to prepare a print for evaluating image unevenness after the durability test.
[0212] For the above printed matter, the image quality of the printed halftone image and solid image was measured using the following color difference ΔE * The evaluation was performed by determining the change in ab between the initial printing stage and after the durability test.
[0213] Halftone and solid images are measured using a spectrophotometer. * a * b * Expressed in a color space, ΔE from the measured value * ab was calculated. * a * b * A "color system" is a useful means of quantifying and representing color. * The axis direction indicates brightness, and * The axis direction indicates the red-green hue, and b * The axis direction indicates the hue from yellow to blue. * ab is the L before the durability test * a * b * The value is (L1, a1, b1), and the L * a * b * When the values are (L2, a2, b2), the value was calculated by substituting each value into the following formula.
[0214] ΔE = [(L1 - L2) 2 +(a1-a2) 2 +(b1-b2)2 〕 0.5
[0215] L * , a * , and b * The measurements were made using a spectrophotometer "Gretag Macbeth Spectrolino" (manufactured by Gretag Macbeth). A D65 light source was used as the light source, and a Φ4mm aperture was used as the reflection measurement aperture, with the measurement wavelength range of 380 to 730 nm at 10 nm intervals and a viewing angle of 2°. For reference alignment, measurements were made under conditions where a dedicated white tile was used.
[0216] The evaluation criteria for density unevenness were as follows. In the following evaluation criteria, A and B were deemed acceptable for practical use and were considered to be acceptable. C was deemed to be unacceptable.
[0217] (Evaluation Criteria) A: The color difference (ΔE) is 10 or less (pass). B: Color difference (ΔE) is more than 10 and less than 11 (pass). C: The color difference (ΔE) is more than 11 (failure).
[0218] [Table 1]
[0219] <<Overall Review>> As can be seen from Table I, in the comparative examples in which the silicon content of the aluminum alloy of the developing sleeve is 0.6 mass% or less, the Rsm value after the durability test is significantly reduced compared to the Rsm value before the durability test. In contrast, when the silicon content exceeds 0.6 mass% as in the examples, the Rsm value after the durability test does not significantly reduce compared to the Rsm value before the durability test.
[0220] As the silicon content increases, the decrease in the Rsm value after the durability test is suppressed, and the decrease in the amount of transported developer is also suppressed, which is thought to further suppress density unevenness. When the silicon content exceeds 0.8 mass%, the decrease in the Rsm value is further suppressed, and the decrease in the amount of transported developer is also suppressed.
[0221] To improve the developer transportability, it is preferable to form grooves by sandblasting, but by increasing the silicon content as in Examples 5 and 6, it is possible to maintain the Rsm value of the surface of the developing roller within an appropriate range without forming grooves, and it is possible to maintain the amount of developer transport. It is also found that this makes it possible to prevent uneven concentration.
[0222] From the above, it is understood that the developer transporting ability of the examples is superior in durability to that of the comparative examples, and good image quality can be maintained. [Explanation of symbols]
[0223] 10 Developing roller 11 Developing sleeve 12 Magnet Roller 16 Shaft 17 Bearing section 18 Non-drive side flange 19 Drive side flange 20 grooves 21 Upstream wall of the groove 22 Downstream wall of the groove 100 Image forming device 110Y, 110M, 110C, 110Bk Image forming unit 111Y, 111M, 111C, 111Bk photoconductor 113Y, 113M, 113C, 113Bk Charging means (charging roller) 115Y, 115M, 115C, 115Bk Exposure means 117Y, 117M, 117C, 117Bk developing means 118Y, 118M, 118C, 118Bk developing roller 119Y, 119M, 119C, 119Bk Cleaning means 131 Intermediate transfer body 133Y, 133M, 133C, 133Bk Transfer means (primary transfer roller) 150 Paper feed conveying means 170 Fixing means 217 Secondary transfer roller (secondary transfer means) SC Original Image Scanner P Transfer material α Groove apex angle β Groove angle Rs1 Length of an example of Rsm A, B groove apex M Mask fixture S: The area of contact between the mask jig and the surface of the developing sleeve when the mask jig is pressed against the surface of the developing sleeve. T Developer
Claims
1. A developing sleeve for an electrophotographic image forming apparatus, which conveys a developer containing a toner and a carrier, The developing sleeve has an aluminum alloy containing more than 0.6% by weight of silicon. The developing sleeve is characterized by the above.
2. The developing sleeve has an aluminum alloy containing more than 0.8% by weight of silicon.
2. The developing sleeve according to claim 1,
3. No resin layer on the surface 2. The developing sleeve according to claim 1,
4. Has grooves on the surface 2. The developing sleeve according to claim 1,
5. The surface is sandblasted 2. The developing sleeve according to claim 1,
6. The average length RSm of the roughness curve elements of the surface of the developing sleeve is equal to or greater than the particle diameter of the carrier.
2. The developing sleeve according to claim 1,
7. The aluminum alloy contains magnesium, The magnesium content is 5.0 mass% or less based on the total mass of the aluminum alloy.
2. The developing sleeve according to claim 1,
8. The aluminum alloy contains manganese, The manganese content is 2.0 mass% or less based on the total mass of the aluminum alloy.
2. The developing sleeve according to claim 1,
9. The silicon content is in the range of more than 0.6 mass% and not more than 4.4 mass% based on the total mass of the aluminum alloy.
2. The developing sleeve according to claim 1,
10. An electrophotographic image forming apparatus including a developing sleeve for conveying a developer containing a toner and a carrier, The developing sleeve has an aluminum alloy containing more than 0.6% by weight of silicon.
2. An electrophotographic image forming apparatus comprising:
Citation Information
Patent Citations
Developing method and device
JP1995181809A