Solid electrolyte layer, solid secondary battery and method for producing thereof
The solid electrolyte layer with a thermoplastic support and minimized voids addresses the short-circuit issue in solid secondary batteries, enhancing their safety and performance during high-current charging.
Patent Information
- Application Number
- JP2023066439
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-25
AI Technical Summary
Conventional solid secondary batteries using solid electrolyte sheets are prone to short circuits during charging with a large current, necessitating a solution to suppress such occurrences.
A solid electrolyte layer comprising a support body made of a thermoplastic material with a solid electrolyte filled between the support parts, where voids communicating across the support parts are minimized, and the length of these voids is less than the total thickness of the layer, optionally including layers without support and a binder, to enhance short-circuit resistance.
The proposed solid electrolyte layer effectively suppresses short circuits during high-current charging, ensuring the stability and safety of solid secondary batteries.
Smart Images

Figure 2024152318000001_ABST
Abstract
Description
[Technical Field]
[0001] The present invention relates to a solid electrolyte layer, a solid secondary battery using the solid electrolyte layer, and a method for manufacturing the solid secondary battery. [Background technology]
[0002] Lithium-ion secondary batteries are widely used as secondary batteries with high energy density. In recent years, the conversion of gasoline-powered vehicles to electric vehicles has been called for as a powerful means of achieving carbon neutrality, and therefore their use as batteries is accelerating.
[0003] However, when using lithium-ion secondary batteries in electric vehicles, the charging time is long compared to the time it takes to fill up a gasoline-powered vehicle with gasoline, which is an obstacle to their widespread use. Therefore, there is a demand for charging performance with a large current that allows charging in a shorter time.
[0004] Lithium-ion solid-state secondary batteries (hereinafter sometimes simply referred to as "solid-state secondary batteries") using solid electrolytes have been proposed as a technology that enables charging at large currents. Most solid electrolytes have a lithium ion transport number of 1, and with the recent improvement in ionic conductivity, they are essentially becoming batteries that are suitable for passing large currents.
[0005] In solid-state secondary batteries using solid electrolytes, the solid electrolyte may be in the form of a powder or a gel. The solid electrolyte layer containing such a solid electrolyte and serving as a separator is preferably formed thinly to improve energy density. At the same time, it is desirable that at least a portion of the solid electrolyte layer be self-supporting and easy to handle, similar to the polyolefin-based separators used in existing lithium-ion secondary batteries using organic electrolyte solutions. Having at least a portion of the solid electrolyte layer self-supporting makes it easier to handle the powder or gel-based solid electrolyte, which facilitates the creation of larger batteries and the improvement of mass productivity.
[0006] In this regard, a solid electrolyte layer using a sheet having many through-holes as a support has been proposed (see, for example, Patent Documents 1 to 4). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Japanese Patent Application Laid-Open No. 2016-31789 [Patent Document 2] Japanese Patent Application Laid-Open No. 2017-208250 [Patent Document 3] Patent Publication No. 2021-150204 [Patent Document 4] Japanese Patent Publication No. 2021-163759 Summary of the Invention [Problem to be solved by the invention]
[0008] However, conventional solid secondary batteries using the solid electrolyte sheets (solid electrolyte layers) described in Patent Documents 1 to 4 have a problem in that they are prone to short circuits, particularly during charging with a large current. Therefore, there has been a demand for a solid secondary battery that can suppress short circuits during charging with a large current, and a solid electrolyte layer that can achieve this.
[0009] Therefore, an object of the present invention is to provide a solid electrolyte layer that can realize a solid secondary battery that can suppress short circuits during charging with a large current, a solid secondary battery that includes such a solid electrolyte layer as a component, and a method for manufacturing the solid secondary battery. [Means for solving the problem]
[0010] One aspect of the present invention is as follows. [1] A solid electrolyte layer formed in a predetermined layer direction, The solid electrolyte layer is A layer (A) having a support including a support portion made of a thermoplastic material and a solid electrolyte filled between the support portions, When a cross section of the layer (A) is viewed, voids that communicate across a plurality of supporting portions may or may not be observed in the layer (A), When the voids are observed, the length (L1) of the voids and the plurality of supporting portions along the layer direction is equal to or less than the total thickness (T1) of the solid electrolyte layer. [2] 2. The solid electrolyte layer according to item 1, wherein the length (L1) is equal to or greater than 0 and is smaller than the total thickness (T1) of the solid electrolyte layer. [3] 3. The solid electrolyte layer according to item 1 or 2, wherein the solid electrolyte layer comprises a binder. [4] 4. The solid electrolyte layer according to any one of items 1 to 3, wherein the support is an electronically insulating nonwoven fabric, and the average diameter of the fibers constituting the support is 1 μm or more and 10 μm or less. [5] 5. The solid electrolyte layer according to any one of items 1 to 4, which does not have the support and has layer (B) disposed in contact with layer (A). [6] 6. The solid electrolyte layer according to any one of items 1 to 5, further comprising a layer (C) that does not have the support and is disposed in contact with the layer (A) on the opposite side of the layer (A) from the layer (B). [7] 7. The solid electrolyte layer according to any one of items 1 to 6, which has self-supporting strength. [8] A solid secondary battery comprising a positive electrode, a negative electrode, and the solid electrolyte layer according to any one of items 1 to 7. [9] a layer (B) that does not have the support and is disposed in contact with the layer (A), Item 9. The solid secondary battery according to item 8, wherein the layer (B) is disposed on the negative electrode side.
[10] A method for producing the solid electrolyte layer according to any one of items 1 to 7, comprising the following steps: filling the pores of the support with the solid electrolyte; applying pressure to the support at a temperature above the glass transition temperature of the support and below the decomposition temperature of at least one of the support and the solid electrolyte; The method for producing a solid electrolyte layer comprising the steps of:
[11] In the pressurizing step, Item 11. The method for producing a solid electrolyte layer according to Item 10, wherein the temperature during pressing is lower than the melting temperature of the support.
[12] In the filling step, Item 12. The method for producing a solid electrolyte layer according to Item 10 or 11, wherein a slurry of the solid electrolyte is introduced into the pores of the support in the presence of a predetermined solvent, and then the solvent is removed. [Effects of the Invention]
[0011] According to the present invention, it is possible to provide a solid electrolyte layer that can realize a solid secondary battery that can suppress short circuits during charging with a large current. Furthermore, the present invention can provide a solid secondary battery including such a solid electrolyte layer as a component, and a method for manufacturing the solid secondary battery. [Brief explanation of the drawings]
[0012] [Figure 1] FIG. 2 is a cross-sectional view showing an example of the configuration of a solid electrolyte layer according to the present embodiment. [Figure 2] FIG. 2 is a cross-sectional view showing an example of the configuration of a solid electrolyte layer according to the present embodiment. [Figure 3] FIG. 4 is a cross-sectional view illustrating a communicating gap and its length. DETAILED DESCRIPTION OF THE INVENTION
[0013] Hereinafter, an embodiment of the present invention (hereinafter referred to as "the present embodiment") will be described with reference to the drawings. The present invention is not limited to the present embodiment and the contents shown in the drawings, and various modifications are possible without departing from the spirit of the present invention. In this specification, the upper or lower limit of a numerical range described stepwise may be replaced with the upper or lower limit of another numerical range described stepwise, or may be replaced with a value shown in an example. The scale, shape, length, etc. shown in the drawings may be exaggerated for clarity.
[0014] [Solid electrolyte layer] [Schematic configuration] One aspect of this embodiment is a solid electrolyte layer formed in a predetermined layer direction, The solid electrolyte layer is A layer (A) having a support including a support portion made of a thermoplastic material and a solid electrolyte filled between the support portions, When a cross section of the layer (A) is viewed, voids that communicate across a plurality of support portions may or may not be observed in the layer (A), When such voids are observed, the length (L1) of the voids and the plurality of supports along the layer direction is equal to or less than the total thickness (T1) of the solid electrolyte layer. Such a solid electrolyte layer can be configured to realize a solid secondary battery that can suppress short circuits during charging with a large current. In this case, the solid electrolyte layer may have a predetermined layer (B) disposed in contact with the layer (A) on the negative electrode side, as described below.
[0015] An example of the solid electrolyte layer of this embodiment is shown in Fig. 1. Fig. 1 is a cross-sectional view that schematically shows a solid electrolyte layer 1 having a two-layer structure.
[0016] The solid electrolyte layer 1 has a layer 2 (layer (A)). The layer 2 has a support including a support portion made of a thermoplastic material, and a solid electrolyte filled between the support portions. The solid electrolyte layer 1 may further have a layer 3 (layer (B)). The layer 3 may have no support and be disposed in contact with the layer 2. When the solid electrolyte layer 1 is used in a solid secondary battery, the layer 2 may be located on the positive electrode side, and the layer 3 may be located on the negative electrode side.
[0017] Another example of the solid electrolyte layer of this embodiment is shown in Fig. 2. Fig. 2 is a cross-sectional view that schematically shows a solid electrolyte layer 100 having a three-layer structure. As shown in FIG. 2 , the solid electrolyte layer 100 has a layer 4 (layer (C)) in addition to the layer 3. The layer 4 does not have a support and can be disposed in contact with the layer 2. The layer 4 may be disposed on the opposite side of the layer 2 from the layer 3. That is, the layers 4, 2, and 3 may be stacked in this order. When the solid electrolyte layer 100 is used in a solid secondary battery, the layer 4 may be located on the positive electrode side, and the layer 3 may be located on the negative electrode side.
[0018] 1 and 2, layer 3 and layer 4 are referred to only in relation to the positive electrode and negative electrode when the solid electrolyte layer is used in a solid secondary battery. That is, in the case of a solid secondary battery in which layer 3 in FIG. 1 is located on the positive electrode side, layer 3 can be layer 4, and in the case of a solid secondary battery in which layer 4 in FIG. 2 is located on the negative electrode side, layer 4 can be layer 3.
[0019] Although not shown, the solid electrolyte layer may have four or more layers. For example, the solid electrolyte layer 100 shown in Fig. 2 may have a layer different from layer 3 on layer 3, and may have a layer different from layer 4 on layer 4. When the solid electrolyte layer has other layers in addition to layer 2, the absence of a support in the other layers can be confirmed, for example, by observing a predetermined image, etc., that the support is not observed in the other layers, and that porosity corresponding to the support is not observed in the other layers. Such other layers include "layers consisting only of a solid electrolyte." The image observation here may be performed in accordance with the observation method for determining "whether or not interconnected voids exist in the layer 2," which will be described later.
[0020] When solid electrolyte layer 1 has another layer in addition to layer 2, for example, when solid electrolyte layer 1 has layer 3 in addition to layer 2, or when solid electrolyte layer 1 has layers 3 and 4 in addition to layer 2, the composition of the solid electrolyte in each layer, the particle size if the solid electrolyte is in powder form, the type and content of the binder that can be contained in each layer, etc. may be the same or different. A binder is not necessarily required in each layer, but it is preferable that at least layer 2 contains a binder.
[0021] Layer 2 is the portion of solid electrolyte layer 1 where the support is composited with the solid electrolyte and exists as a layer, and its thickness can be considered to be substantially the same as the thickness of the support when the pores are filled with the solid electrolyte. Therefore, if there is a distribution in the thickness of the support, the thickness distribution of layer 2 will also reflect that distribution. The thickness of layer 3 is preferably 0.5 μm or more, and more preferably 1 μm or more, at the thinnest part, from the viewpoint of ensuring a suitable gap between the support and the negative electrode mixture layer in the solid secondary battery (e.g., to suitably avoid contact between the two). When the thickness of layer 3 at the thinnest part is less than 0.5 μm, the solid electrolyte layer is defined as not having layer 3 present over the entire surface, and such a configuration is excluded from the embodiment shown in FIG. The thickness of layer 4 is preferably 0.5 μm or more, and more preferably 1 μm or more, at the thinnest part, from the viewpoint of ensuring a suitable gap between the support and the positive electrode mixture layer in the solid secondary battery (e.g., to suitably avoid contact between the two). When the thickness of layer 4 at the thinnest part is less than 0.5 μm, the solid electrolyte layer is defined as not having layer 4 present over the entire surface, and such a configuration is excluded from the embodiment shown in FIG.
[0022] Here, the "total thickness (T1) of the solid electrolyte layer" in this specification refers to the total thickness of layers 2 and 3 in the solid electrolyte layer 1 in Fig. 1, and refers to the total thickness of layers 2, 3, and 4 in the solid electrolyte layer 100 in Fig. 2. That is, when the solid electrolyte layer has another layer (a layer containing a solid electrolyte) other than layer 2, the total thickness (T1) of the solid electrolyte layer refers to the total thickness of layer 2 and the other layer.
[0023] If the thickness of each of Layers 2, 3, and 4 is too thick, the energy density of the battery is likely to decrease, and if the thickness is too thin, the battery is likely to short-circuit. The thickness of Layer 2 is preferably 2 to 35 μm, more preferably 3 to 30 μm, and even more preferably 4 to 25 μm. The thickness of Layer 3 is preferably 3 to 50 μm, more preferably 4 to 40 μm, and even more preferably 5 to 35 μm. The thickness of Layer 4 is preferably 1 to 26 μm, more preferably 2 to 21 μm, and even more preferably 3 to 17 μm.
[0024] The solid electrolyte layer of this embodiment does not necessarily have to have a self-supporting strength. However, if the entire solid electrolyte layer or a part thereof has a self-supporting strength, it leads to an improvement in the strength of the solid electrolyte layer as a whole. Therefore, it is preferable from the viewpoints of preventing the solid electrolyte from falling off from the solid electrolyte layer, preventing cracking of the solid electrolyte layer, thereby facilitating the enlargement of the battery area, and improving mass productivity by improving handleability. Incidentally, having the solid electrolyte layer have a support is advantageous for strengthening the solid electrolyte layer itself and, ultimately, for preventing the solid electrolyte from falling off from the solid electrolyte layer.
[0025] [Layer (A)] Layer 2 (layer (A)) has supporting portions made of a thermoplastic material and a solid electrolyte filled between the supporting portions. When voids (sometimes referred to as "communicating voids" in this specification) that communicate across multiple supporting portions are observed in layer 2 when viewed from a cross section of layer 2, the length (L1) of the communicating voids and multiple supporting portions along the layer direction is less than the total thickness (T1) of the solid electrolyte layer. The length (L1) is preferably equal to or greater than 0 and less than the total thickness (T1) of the solid electrolyte layer, and it is particularly preferable that no communicating voids exist in the cross section of layer 2 (i.e., no communicating voids are observed).
[0026] <Communication gap> 3A to 3C are cross-sectional views illustrating the interconnected voids and their lengths. Figures 3A to 3C show solid electrolyte layers 1a to 1c, each having a support portion 5. In the solid electrolyte layers 1a to 1c, a solid electrolyte 6 is filled between the support portions 5. In each drawing, the gaps 7 (or holes 7) are shown between the support portions 5, and the openings to the surface associated with these gaps are shown as openings Op.
[0027] In the cross section of the layer 2, voids in contact with the support portions 5 may be observed. In each drawing, a void in contact with a specific support portion 5b that does not reach another support portion 5b is illustrated as "void 8," while a void in contact with a specific support portion 5a that reaches another support portion 5a is illustrated as "void 9." Here, the voids 9 correspond to the communicating voids 9. The communicating voids 9 include voids 9a whose both ends in the layer direction are connected to the supporting portion 5a, and voids 9b whose one end in the layer direction is connected to the supporting portion 5a, as shown in Figures 3(b) and 3(c), for example.
[0028] The length (L1) is defined as the length including not only the length of the communicating void 9 itself but also the length in the layer direction of the supporting portion 5a with which the communicating void 9 is in contact. 3(b), the length in the layer direction of the communicating voids 9 and the supporting portions 5a connected thereto is such that the communicating voids 9a form one end and the supporting portions 5a form the other end. In this case, the length (L1) is treated as the length having the communicating voids 9a at one end and the supporting portions 5a at the other end. 3(c), when the length in the layer direction of the communicating voids 9 and the supporting portions 5a to which they are connected is examined, the communicating voids 9 extend beyond the supporting portions 5, i.e., the communicating voids 9a constitute both ends. In this case, the length (L1) is treated as the length whose both ends are the communicating voids 9a.
[0029] Therefore, for example, in a support made of fibers such as a nonwoven fabric, when voids exist continuously in the layer direction through a plurality of fibers, the distance from one end of the void to the other end in the opposite direction corresponds to the above-mentioned length (L1). The gap 8 does not continue to another support portion 5b; and When the communicating void 9 is not connected to the support portion 5b to which the void 8 is connected; The voids 8 in are excluded from the communicating voids 9.
[0030] The present inventors have discovered that interconnected voids occur due to insufficient filling of the support with solid electrolyte. Conventionally, the cause of short circuits in solid secondary batteries has been believed to be continuous voids (penetrating cracks) in a direction perpendicular to the surface (current collecting surface) of the battery's current collecting foil (the direction in which the positive and negative electrodes face each other). To prevent such penetrating cracks and thus short circuits, for example, Patent Document 4 attempts to sandwich the support between a first solid electrolyte layer and a second solid electrolyte layer and press the support, thereby forcing the solid electrolyte into the through-holes in the support. However, it was found that the method described in Patent Document 4 tends to result in insufficient pressing of the solid electrolyte into the support. That is, it was found that even if the support is pressed with solid electrolyte layers from both sides, it is difficult to adequately fill the support with the solid electrolyte. As a result, interconnected voids are likely to form in the support, which may reduce the short-circuit resistance of the solid secondary battery. It has been found that interconnected voids are likely to remain in particular when the pore size of the support is small; when the support is thick or the pressure during pressing is low; when it does not contain a binder; when the support is prone to elastic deformation and therefore tends to return to its original shape after pressing even if it deforms during pressing; etc.
[0031] As a result of extensive efforts by the present inventors to examine the prior art including Patent Document 4, they have identified the following factors as the causes of short circuits that can occur in conventional solid secondary batteries. These elements are: The support restricts the migration and diffusion path of lithium (Li) ions to the solid electrolyte portion filled in the openings of the support (e.g., openings resulting from through-holes formed in the support), thereby causing Li ion current concentration; As a result of thinning the solid electrolyte layer to improve the energy density, the distance between the support and the negative electrode tends to become shorter, and in this case, Li ions that pass through the openings in the support are less likely to diffuse in the layer direction, which makes the above-mentioned Li ion current concentration effect more likely to occur; As a result, compared to a lithium solid state secondary battery without a support, the negative electrode active material is saturated on the negative electrode surface near the opening, and the operating potential is reduced, particularly during charging with a large current, which makes it more likely that Li metal will deposit and cause a short circuit; That is the thing.
[0032] Furthermore, as a result of their diligent efforts, the inventors have discovered that these short circuits are not caused solely by continuous voids (penetrating cracks) in the direction perpendicular to the surface of the current collecting foil (current collecting surface) (the direction in which the positive and negative electrodes face each other), or by the concentration of Li-ion current originating from the openings in the support.
[0033] In response to the above, the present inventors have newly focused on the above-mentioned interconnected voids as a cause of short circuits that can occur in solid secondary batteries, and have thereby achieved this embodiment.
[0034] The volume fraction of the solid electrolyte in layer 2 is not particularly limited, but if the volume fraction is too low, the resistance of the battery is likely to increase, which in turn leads to a decrease in capacity. Also, if the volume fraction is too high, the proportion of the support is likely to decrease, which in turn reduces the reinforcing effect of the support on the solid electrolyte layer. Therefore, the volume fraction is preferably 10 to 90%, more preferably 15 to 80%, and even more preferably 20 to 70%.
[0035] The solid electrolyte in layer 2 is preferably filled into the support without leaving any gaps. This support preferably undergoes plastic deformation when filled with the solid electrolyte, changing its shape from the shape before filling, and maintains that state after filling. This makes it easier to fill the support with the solid electrolyte without leaving any gaps, and therefore reduces the likelihood of interconnected voids being generated.
[0036] The support included in layer 2 may be of one type, may contain different materials, or may be a stack of multiple support layers of the types, materials, and structures described below. When stacking the layers, a layer consisting of only a solid electrolyte may be sandwiched between the layers. Even in this case, it is preferable that the solid electrolyte layer containing the multiple stacked support layers meets the requirements of this embodiment.
[0037] The presence or absence of interconnected voids in layer 2 can be confirmed by conventionally known methods, such as a method of cleaving the solid electrolyte layer to expose cross sections and observing the cross sections multiple times, or a method of obtaining a three-dimensional image of the support using a high-resolution X-ray CT, etc. For example, the presence or absence of interconnected voids can be determined by cleaving the solid electrolyte layer to obtain a predetermined cross section, polishing the cross section smoothly using a cross-section polisher and a focused ion beam, or the like, and then observing the cross section using an SEM, and performing these observations at multiple locations.
[0038] <Support> The support may be, for example, porous or sheet-shaped and have finite continuity. Any support may be used, such as a woven fabric, a nonwoven fabric, a microporous membrane, or a sheet with a large number of through-holes. The structure (composition, shape, etc.) of the support, and the structure (size, shape, etc.) of the openings on the surface of the support, are not limited. In this embodiment, it is preferable that the support includes a nonwoven fabric (in one aspect, the support is a nonwoven fabric). It is also preferable that the support be electronically insulating.
[0039] In this embodiment, the support is made of a thermoplastic material. Here, thermoplasticity refers to the property that, once the support is deformed by applying an external force above a certain temperature, it does not return to its original shape even when the external force is removed. Resin materials having a glass transition temperature (Tg) are particularly preferred because they possess this property. In a support made of a resin material having a Tg, the Tg is preferably below the decomposition temperature of the solid electrolyte, preferably 190°C or lower, more preferably 100°C or lower, and even more preferably 80°C or lower. The lower limit of Tg may be any temperature at which the support does not flow at room temperature and can maintain its shape; for example, a temperature above -130°C is preferred. Examples of such resin materials include polypropylene, polyethylene, polystyrene, polyethylene terephthalate (PET), polyacrylonitrile, polybutadiene, polyamide, polyacetal, polyvinyl chloride, polyvinyl acetate, and polymethyl methacrylate.
[0040] (nonwoven fabric) The support can be a nonwoven fabric made of an electronically insulating thermoplastic resin. Being electronically insulating means that electrons do not flow, but ion conductivity is acceptable. If the solid secondary battery is a lithium ion battery, the support may have lithium ion conductivity, and if the solid secondary battery is a sodium ion battery, the support may have sodium ion conductivity. The average fiber diameter of the fibrous material constituting the nonwoven fabric is not particularly limited, but if the average fiber diameter is too large, it tends to be difficult to densely fill the openings of the support with the solid electrolyte. On the other hand, if the average fiber diameter is too small, the strength of the support tends to decrease. Therefore, the average fiber diameter is preferably 0.3 to 20 μm, more preferably 0.5 to 15 μm, and even more preferably 1 μm to 10 μm. In particular, if the average fiber diameter exceeds 10 μm, the intersections of the fibers in the nonwoven fabric tend to act as "stops" during thermal compression, hindering compression, which may result in a decrease in the filling ability of the solid electrolyte.
[0041] The basis weight of the nonwoven fabric is not particularly limited, but if the basis weight is too large, the opening diameter and opening ratio of the openings in the support tend to decrease, which in turn tends to increase the resistance of the battery. On the other hand, if the basis weight is too small, the strength of the support tends to decrease due to the low proportion of fibrous material. Therefore, the basis weight is preferably 1.0 to 10.0 g / m. 2 is preferred, and 1.5 to 8.0 g / m 2 More preferably, 2.0 to 6.0 g / m 2 is more preferred. The porosity relative to the membrane thickness is not particularly limited, but if the porosity is too small, the proportion of the solid electrolyte is likely to decrease, which in turn increases the resistance of the battery. Also, if the porosity is too large, the proportion of the fibrous material is likely to decrease, which in turn decreases the strength of the support. Therefore, the porosity of the support before filling with the solid electrolyte is preferably 30 to 90%, more preferably 40 to 85%, and even more preferably 50 to 80%.
[0042] (woven fabric) A woven fabric can be used as the support. The woven fabric is formed by bundling and weaving a plurality of monofilaments, which are the basic unit of fiber, using a sizing agent or the like as necessary. When a woven fabric is used as the support, the average value of the widths of the bundled monofilaments measured in a planar view from the thickness direction of the woven fabric is defined as the "aggregate fiber width" in this specification. The planar view may be obtained using an optical microscope or a scanning electron microscope (SEM). When there is a distribution in the aggregate fiber width, the width is measured multiple times, and the average value calculated is treated as the aggregate fiber width.
[0043] The fiber aggregate width and the number of fibers to be bundled are not particularly limited, but if the fiber aggregate width is too large, the opening ratio of the support tends to decrease, and if it is too small, the strength of the fibers tends to decrease, making it difficult to weave the woven fabric. Therefore, the fiber aggregate width is preferably 3 to 200 μm, more preferably 5 to 100 μm, and even more preferably 7 to 90 μm. Of course, the average fiber diameter of the monofilaments must be smaller than the fiber aggregate width. The weaving method for the woven fabric may be plain weave, twill weave, satin weave, leno weave, etc., as appropriate. However, there are no particular limitations as long as the shape can be maintained.
[0044] (microporous membrane) A microporous membrane can be used as the support. The pore structure (average pore size and its distribution width) of the microporous membrane is not particularly limited, but if the average pore size is too small, it is difficult to fill the openings, particularly in the case of a particulate solid electrolyte, and if the average pore size is too large, the particles are likely to fall out of the openings, particularly in the case of a particulate solid electrolyte. Therefore, the average pore size is preferably 0.5 to 5 μm, more preferably 1 to 4 μm.
[0045] (Sheet with many through holes) A mesh-like sheet (a sheet with many through-holes formed therein) can be used as the support. The configuration of the through-holes in the sheet (such as the average hole diameter and shape) is not particularly limited. For example, the shape of the through-holes is not limited to square, circle, etc., but may be rectangular, diamond, oval, etc. Methods for forming the through-holes include physical openings using a mold, drill, etc.; openings using a laser; openings using photolithography and thermal lithography; etc. Alternatively, a support may be used in which the through-holes are enlarged by making cuts in the sheet and pulling it to both sides.
[0046] (others) The thickness of the support is not particularly limited, but if the thickness is too thick, the energy density of the battery is likely to decrease, and if the thickness is too thin, the strength of the support is likely to decrease. Therefore, the thickness is preferably 2 to 40 μm, more preferably 3 to 35 μm, and even more preferably 4 to 30 μm.
[0047] The film thickness may be measured by a conventionally known method. For example, the support is clamped between a commercially available micrometer (e.g., MDH-25MB high-precision digimatic micrometer manufactured by Mitutoyo Corporation) and measurements are taken multiple times at different locations on the support, and the film thickness is obtained by calculating an average value from the results obtained.
[0048] When a fibrous material (such as a nonwoven fabric or a woven fabric) is used as the support, the average fiber diameter and its distribution may be measured by a conventionally known method. For example, the above can be determined by a step of cleaving the solid electrolyte layer to expose a cross section, a step of measuring the fiber portion of the cross section at multiple locations by cross-sectional observation using an SEM after smoothing and polishing with a cross-section polisher or the like, and a step of calculating the average value and distribution of the measured fiber diameters.
[0049] The aperture ratio of the support is not particularly limited, but if the aperture ratio is too small, it becomes difficult to fill with the solid electrolyte and the resistance of the battery is likely to increase, which is likely to result in a decrease in capacity. Also, if the aperture ratio is too large, the strength of the support is likely to decrease. Therefore, the aperture ratio is preferably 15 to 90%, more preferably 20 to 80%, and even more preferably 25 to 75%.
[0050] The aperture ratio of a support is defined as the ratio of the area of the surface treated as the object of observation when the support is viewed in a plane from the thickness direction to the area of the surface that can be seen through the support and opposite the observation surface of the support.
[0051] [Layer (B) and Layer (C)] With regard to layer 3 (layer (B)) and layer 4 (layer (C)), layer 3 is located on the negative electrode side of layer (A) in the solid secondary battery. Without being bound by theory, the inventors have found that the presence of the support causes state unevenness in the electrolyte potential, SOC, and the like inside the solid secondary battery, and that these unevenness accelerates the occurrence of short circuits associated with Li deposition, that the presence of layer 3 can suppress this, and that it is desirable for layer 3 to be thicker than layer 4. They have also found that the effects of this embodiment are greatly achieved by using layer 2 that does not have interconnected voids 9 and by arranging layer 3 on the negative electrode side of layer 2 in the solid secondary battery.
[0052] In addition, when the solid electrolyte layer has layer 4, the thickness of layer 3 is preferably 1.5 to 5 times that of layer 4. Furthermore, when the solid electrolyte layer of the present embodiment is a solid electrolyte sheet that has a self-supporting strength by itself, it may have the self-supporting strength when layer 3 is attached to layer 2, or it may have the self-supporting strength when layer 4 is attached to layer 2. Alternatively, a solid electrolyte layer may be obtained by joining layers 3 and 4, which are attached to the negative electrode and positive electrode, respectively, and finally attaching layer 3 and, if necessary, layer 4 to layer 2 in a solid secondary battery.
[0053] The thickness of the solid electrolyte layer may be measured by a conventionally known method, for example, by a process including a step of fracturing the solid electrolyte layer to expose a cross section, a step of polishing the cross section smoothly with a cross-section polisher or the like, a step of observing the cross section with an SEM, a step of measuring the thickness at a plurality of points, and a step of calculating an average value of the measured thicknesses.
[0054] [Solid electrolyte] The solid electrolyte is preferably one that can maintain a layered form by itself or by being held on the surface of a support or contained in a support, and more preferably one that can conduct ions. Generally, the higher the ionic conductivity of an electrolyte used in a battery, the better. The present invention is no exception. Examples of solid electrolytes include sulfide-based solid electrolytes, polymer-based solid electrolytes, gel-based electrolytes, hydride-based solid electrolytes, and oxide-based solid electrolytes. However, those that can be held on the surface of a support but cannot flow and maintain a layered form, and those that can be contained in a support but cannot flow and maintain a layered form, are excluded.
[0055] Even if the layer thickness decreases when the battery is pressurized due to constraints, etc., it can still be used as a solid electrolyte. However, if the solid electrolyte flows as the layer thickness decreases, causing more than half of the solid electrolyte to be extruded from the layer, this is not desirable.
[0056] The solid electrolyte to be filled into the support is preferably a sulfide-based solid electrolyte, a polymer solid electrolyte, a gel electrolyte, or a hydride-based solid electrolyte, which is soft and easily deformable and therefore easy to fill. If necessary, a binder component and components such as a viscosity adjuster required for filling and coating may be added.
[0057] Examples of sulfide-based solid electrolytes include, for example, glass-based and glass-ceramic-based electrolytes, Li2S-P2S5, Li2S-P2S3, Li2S-P2S3-P2S5, Li2S-P2S5-GeS2, Li2S-P2S5-B2S3, Li2S-SiS2, Li2S-SiS2-P2O5, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, LiI-Li2S-SiS2-P2S5, Li2S-SiS2-Li3PO4, LiBr-Li2S-SiS2, Examples include Li2S-GeS2, Li2S-GeS2-ZnS, Li2S-GeS2-Sb2S5, Li2S-GeS2-Ga2S3, Li2S-GeS2-Al2S3, LiI-Li2S-GeS2, Li2S-GeS2-Li3PO4, Li2S-Ga2S3, Li2S-B2S3, Li2S-Al2S3, Li2S-SiS2-Al2S3, LiI-Li2S-B2S3, Li2S-B2S3-Li3PO4, Li2S-P2S5-LiBr, Li2S-P2S5-Li3N, and Li2S-P2S5-LiBH4.
[0058] In the crystal system, Li6PS5X (where X = Cl, Br, I) is called argyrodite type, and Li 7-x PS 6-x X x (wherein X=Cl, Br, I, 0≦x≦1.8) and Li 3.4 P 0.6 Si 0.4 S4, Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 , Li 4-x Ge 1-x P x S4 (wherein 0≦x≦1), Li 10 GeP2S 11.7 O 0.3 etc.
[0059] Examples of polymer-based solid electrolytes and gel-based electrolytes include those in which an electrolyte salt is dissolved in a polymer compound to exhibit ionic conductivity, and those in which an electrolyte salt is dissolved in a solvent together with a polymer and a monomer to form a gel and exhibit ionic conductivity. Specifically, when a lithium salt is used as the electrolyte salt, examples of the lithium salt include conventionally known lithium salts such as lithium hexafluorophosphate (LiPF), lithium bis(fluorosulfonyl)imide (Li(FSO)N), lithium bis(trifluoromethanesulfonyl)imide (Li(CFSO)N), lithium perchlorate (LiClO), lithium arsenic hexafluoride (LiAsF), lithium tetrafluoroborate (LiBF), lithium trifluoromethanesulfonate (LiCFSO), and lithium bistrifluoromethylsulfonylimide [LiN(CFSO)].
[0060] Examples of polymers that can dissolve electrolyte salts and exhibit ionic conductivity include polyethylene glycol, polymers having polyacrylic acid, polymethacrylic acid, polyethylene oxide, polypropylene oxide, polyvinyl alcohol, polyphosphazene, polysilane, etc. in the main chain, and copolymers thereof having a polyoxyethylene structure in the side chain.
[0061] The electrolyte salt dissolves in an electrolyte solvent together with a polymer and a monomer to form a gel, which exhibits ionic conductivity. The polymers and monomers used in this gel electrolyte are not particularly limited. Examples of polymers include polyvinyl chloride, polyacrylonitrile, polyethylene, polypropylene, polyester, polyacrylate, and copolymers thereof. Examples of monomers include carborane-based materials such as ortho-carborane, meta-carborane, and para-carborane; adamantane-based materials such as 2-adamantanone, 1-adamantanone, 1-adamantanecarbonitrile, and 2-adamantanecarbonitrile; dinitrile compounds such as succinonitrile, methylsuccinonitrile, tetramethylsuccinonitrile, azobisisobutyronitrile, glutaronitrile, adiponitrile, pimelonitrile, octanedinitrile, azelanitrile, and sebaconitrile; and sulfolane compounds such as sulfolane, ethyl methyl sulfone, and 3-methylsulfolane sulfolane.
[0062] The electrolyte solvent may be a mixed solvent of a cyclic carbonate and a chain carbonate. Typical examples of the cyclic carbonate include ethylene carbonate (EC) and propylene carbonate (PC). Typical examples of the chain carbonate include dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC). However, the solvent is not limited to these.
[0063] Ionic liquids can also be used as electrolyte solvents. Specific examples include 1,2-ethylmethylimidazolium bis(fluorosulfonyl)imide, 1,2-ethylmethylimidazolium bis(trifluoromethanesulfonyl)imide, 1-ethyl-3-methylimidazolium bis(fluorosulfonyl)imide (abbreviated as EMImFSI), N-methylpropylpyrrolidinium bis(fluorosulfonyl)imide, N-methylpropylpyrrolidinium bis(trifluoromethanesulfonyl)imide, diethylmethylmethoxyethylammonium bis(trifluoromethanesulfonyl)imide, diethylammonium bis(fluorosulfonyl)imide, diallyldimethylammonium(trifluoromethanesulfonyl)imide, and diallyldimethylammonium(fluorosulfonyl)imide. However, they are not limited to these.
[0064] The hydride solid electrolyte is preferably one having ion conductivity, and examples thereof include LiBH4, LiAlH4, Li3AlH6, LiBH(Et)3, LiBH(s-Bu)3, LiNH2, Li2NH, Li[OC(CH3)3]3AlH, Li(OCH3)3AlH, Li(OC2H5)3H, a solid electrolyte in which the molar ratio of LiBH4 to LiI is 1:1 to 20:1, Li2B 12 H 12 and rotational complex ions such as Li3MoH9, and solid solutions of multiple of these.
[0065] Examples of oxide-based solid electrolytes include Li7La3Zr2O 12 (LLZ), Li x La y TiO3 (where x = 0.3 to 0.7, y = 0.3 to 0.7) (LLT), Li with LISICON (Lithium super ionic conductor) type crystal structure 3.5 Zn 0.25 GeO4, LiTi2P3O with NASICON (sodium super ionic conductor) type crystal structure 12 However, the present invention is not limited to these.
[0066] Phosphorus compounds containing Li, P, and O can also be used as solid electrolytes. Examples of preferred solid electrolytes include Li3PO4, LiPON, LiPOD (wherein D is at least one transition metal), and LiAON (wherein A is at least one selected from the group consisting of Si, B, Ge, Al, C, and Ga) in which some of the oxygen in Li3PO4 has been replaced with nitrogen. Li3N, which uses N instead of P, may also be used.
[0067] Among these, sulfide-based solid electrolytes are preferred as the solid electrolyte from the viewpoint of high ionic conductivity, and crystalline argyrodite-type sulfide-based solid electrolytes are more preferred from the viewpoint of electrochemical stability.
[0068] When a powdered sulfide-based solid electrolyte is used, a smaller average particle size makes it easier to fill the pores of the support with the solid electrolyte. On the other hand, when the solid electrolyte is treated as a slurry, its dispersibility in the solid electrolyte slurry tends to decrease, making it difficult to obtain a uniform solid electrolyte layer. Furthermore, a larger average particle size tends to increase the proportion of large-sized solid electrolyte particles, making it difficult not only to fill the pores of the support with the solid electrolyte but also to obtain a solid electrolyte layer of uniform thickness. Therefore, the average particle size of the sulfide-based solid electrolyte is preferably 0.1 to 10 μm.
[0069] The average particle size and particle size distribution of the powdered solid electrolyte can be determined by a known, general-purpose method. Specifically, for example, a dry particle size distribution analyzer using laser diffraction and scattering (e.g., HORIBA, Ltd.'s Laser Diffraction / Scattering Particle Size Distribution Analyzer LA-960V2) can be used. The solid electrolyte may be used alone or in combination of two or more.
[0070] <Binder> The solid electrolyte layer may contain a binder to improve the binding strength between the support and the solid electrolyte, between powdery solid electrolytes, and between solid electrolyte layers. In particular, it is preferable that the layer (A) having the support contains a binder. Known binders can be used, including, for example, styrene-based thermoplastic elastomers such as SBS (styrene butadiene block polymer), SEBS (styrene ethylene butadiene styrene block polymer), and styrene-styrene butadiene-styrene block polymer; styrene butadiene rubber; butadiene rubber; natural rubber; isoprene rubber; EPDM (ethylene-propylene-diene terpolymer); nitrile rubber; chloroprene rubber; and partially or fully hydrogenated versions thereof; cellulose such as carboxymethyl cellulose; copolymers of polyacrylic acid esters; PVDF (polyvinylidene fluoride); PVDF-HFP (polyvinylidene fluoride-hexafluoropropylene copolymer); and carboxylic acid-modified versions thereof; polymethacrylic acid esters; polyvinyl alcohol; ethylene-vinyl alcohol copolymers; acrylic latex; polyimides; polyamides; and polyamideimides. Other examples include polystyrene, polyolefins, olefin-based thermoplastic elastomers, polycycloolefins, and silicone resins. These may be used alone or in combination of two or more.
[0071] [Method for producing solid electrolyte layer] As a method for producing the solid electrolyte layer, a general production method can be adopted, for example, a method in which a solid electrolyte and a binder are dissolved or dispersed in a solvent to obtain a slurry or solution, and then this solid electrolyte slurry or solution is applied and then dried; a method in which a powder of a solid electrolyte material is applied and then excess powder is removed with a squeegee or the like; etc.
[0072] The method for producing the solid electrolyte layer of the present embodiment includes, for example, the following steps: a step of filling the pores of the support with the solid electrolyte (filling step); a step of pressing (heating) the support at a temperature above the glass transition temperature of the support and below the decomposition temperature of at least one of the support and the solid electrolyte; It has. The order of the filling step and the heating step is not limited as long as it is not contrary to the purpose of the step, and the steps may be repeated alternately.
[0073] In the pressurizing step, the temperature during pressurization is preferably lower than the melting temperature of the support. In the filling step, it is preferable to introduce a slurry of the solid electrolyte into the pores of the support in the presence of a predetermined solvent, and then remove the solvent. These points will be described later.
[0074] In a solid electrolyte layer having a support, the pores of the support must be filled with a solid electrolyte. In this case, the support may be held on a sheet or film serving as a base material, and a slurry or solution of the solid electrolyte may be applied or powder coated thereon to temporarily produce a solid electrolyte layer having a support integrated with the sheet and film while the pores of the support are filled with and retained by the solid electrolyte. In this case, the surfaces of the sheet and film that come into contact with the solid electrolyte layer are preferably subjected to a release treatment so that the sheet and film can be later peeled and removed from the solid electrolyte layer.
[0075] The method for forming a solid electrolyte layer without a support is the same as the method for forming a solid electrolyte layer with a support, that is, a method of applying a slurry or solution of the solid electrolyte onto the above-mentioned substrate sheet or film, a solid electrolyte layer with a support, another solid electrolyte layer without a support, a positive electrode composite layer, or a negative electrode composite layer, or a method of powder coating the solid electrolyte material can be used.
[0076] In particular, it is preferable to prepare a solid electrolyte layer (B) without a support on a substrate sheet or film, then place a support thereon, and then overlay the solid electrolyte by coating it with a slurry or solution, or by powder coating, to form a layer. As a result, a layer having the following composition with a desired thickness can be formed on the sheet or film: a solid electrolyte layer 3 (layer (B)) having no support; a solid electrolyte layer 2 (layer (A)) having a support, and a solid electrolyte layer 4 (layer (C)) having no support; Thereafter, the sheet and film may be peeled off to treat the solid electrolyte sheet as a free-standing solid electrolyte, or the solid electrolyte may be transferred to a positive electrode, a negative electrode, or the like and the sheet and film may be peeled off to treat the solid electrolyte layer.
[0077] Examples of the sheet or film that serves as the substrate include, but are not limited to, stainless steel foil, PET film, etc.
[0078] When a solid electrolyte sheet is prepared by sequentially stacking solid electrolyte layers using the above-described method, shrinkage stress during drying and residual stress after compression of the solid electrolyte material may cause the solid electrolyte sheet to warp after peeling off the sheet and film. The degree of warping depends on the type and material of the support, but warping is often significant when the difference in thickness between the unsupported solid electrolyte layers (the difference in thickness between layer 3 (layer (B)) and layer 4 (layer (C)) in Figure 2)) is large. When treating the solid electrolyte layer as a freestanding solid electrolyte sheet, this warping is likely to induce cracking and chipping of the solid electrolyte layer, restrict the manufacturing process, and cause a short circuit in the battery. Therefore, it is preferable to suppress warping.
[0079] Therefore, in this embodiment, a positive electrode or a negative electrode in which a solid electrolyte layer without a support is provided to one or both of the positive electrode composite layer and the negative electrode composite layer is laminated and joined with a solid electrolyte layer having a support, thereby finally obtaining a solid secondary battery having solid electrolyte layers in which the film thicknesses of Layer 3 (Layer (B)) and Layer 4 (Layer (C)) are significantly different.
[0080] In the solid electrolyte layer of this embodiment, applying pressure while heating compresses not only the solid electrolyte material but also the support, and compresses the support while thermoplastically deforming it. This makes it easier for the support to deform to conform to the shape of the particles when the solid electrolyte is composed of particles, thereby allowing the solid electrolyte to be filled without generating interconnected voids in the layer. In this case, in order to sufficiently thermoplastically deform the support and prevent elastic deformation so that it conforms to the shape of the particles, the temperature during pressing must exceed at least the Tg of the material constituting the support, preferably at least 50°C higher than the Tg, and more preferably at least 100°C higher than the Tg. However, if the support decomposes at high temperatures, the strength of the support will decrease or the layer will break due to gas generation, so it is preferable that the temperature be at least below the decomposition temperature of the support. While heating below the melting temperature of the support is generally more preferable, the support may be pressed in a molten state as long as it does not melt out of the layer and maintains its sheet-like form even after heating and pressing.
[0081] Since solid electrolytes tend to decompose at high temperatures, which can lead to a decrease in the performance of solid secondary batteries, it is preferable that the temperature during pressurization be equal to or lower than the decomposition temperature of the solid electrolyte. The decomposition temperature of a solid electrolyte depends on the type of solid electrolyte, but the temperature at which the performance of a solid secondary battery begins to decrease can be considered the decomposition temperature. For example, an argyrodite-type sulfide-based solid electrolyte begins to decompose and its performance begins to decrease when the temperature exceeds 190°C.
[0082] The method for pressing the solid electrolyte, the support, and the layer formed therefrom is not particularly limited, and for example, a hot roll press, a hot plate press, a hot isostatic press, etc. A hot roll press is preferable from the viewpoint of improving the productivity of the solid electrolyte layer because it allows continuous pressing.
[0083] The pressure applied to the solid electrolyte, the support, and the layer formed thereof is, for example, 30 to 1000 MPa in the case of a plate press, a hydrostatic press, etc., and, for example, 0.1 to 5 ton / cm in the case of a roll press.
[0084] [Solid electrolyte slurry or solution and method for forming a solid electrolyte layer using the same] The solid electrolyte slurry or solution contains a solid electrolyte, a solvent for dispersing or dissolving the solid electrolyte (the concept of "solvent" in this specification includes a dispersion medium), and additives (known additives such as a binder or a thickener) that are added as needed.
[0085] The solvent is preferably one that can disperse or dissolve the solid electrolyte and additives well and does not significantly impair the battery characteristics of the solid electrolyte and the support.For example, methyl alcohol, ethyl alcohol, 1-propyl alcohol, 2-butanol, ethylene glycol, propylene glycol, glycerin, 1,6-hexanediol, 1,3-butanediol, 1,4-butanediol, ethylene glycol monomethyl ether, ethylene glycol monobutyl ether, diethylene glycol, dipropylene glycol, propylene glycol monomethyl ether, diethylene glycol monomethyl ether, triethylene glycol, polyethylene glycol, propylene glycol dimethyl ether, dipropylene glycol monomethyl ether, tripropylene glycol monomethyl ether, diethylene glycol monobutyl ether, diethylene glycol dibutyl ether, dimethyl ether, diethyl ether, dibutyl ether, tetrahydrofuran, dioxanes, N,N-dimethylformamide, 1-methyl-2-pyrrolidone, 2-pyrrolidinone, 1,3-dimethyl-2-imidazolidinone, ε-caprolactam, formamide, N-methylformamide, acetamide, N-methylacetamide, N, N-dimethylacetamide, N-methylpropanamide, triethylamine, tributylamine, acetone, methyl ethyl ketone, diethyl ketone, dipropyl ketone, dibutyl ketone, diisobutyl ketone, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, pentyl acetate, hexyl acetate, methyl propionate, ethyl propionate, propyl propionate, butyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate, butyl butyrate, isobutyl isobutyrate, pentyl butyrate, methyl valerate, ethyl valerate, propyl valerate, butyl valerate Examples of suitable solvents include toluene, methyl caproate, ethyl caproate, propyl caproate, butyl caproate, hexene, heptene, cyclohexene, toluene, various ortho-, meta- and para-xylenes, decalin, 1,2,3,4-tetrahydronaphthalene, mesitylene, methoxybenzene, hexane, pentane, heptane, 2-ethylhexane, cyclohexane, methylcyclohexane, ethylcyclohexane, decalin, octane, nonane, decane, pentane, cyclopentane, cyclooctane, acetonitrile, propylonitrile and butyronitrile.
[0086] In particular, when a sulfide-based solid electrolyte is used, a low-polarity solvent that has low reactivity with the sulfide-based solid electrolyte is preferred, and examples thereof include hexane, pentane, 2-ethylhexane, heptane, octane, nonane, decane, cyclohexane, hexene, heptene, cyclohexene, toluene, xylene, decalin, 1,2,3,4-tetrahydronaphthalene, mesitylene, and methoxybenzene.
[0087] The above solvents may be used alone or in combination of two or more. Furthermore, it is preferable that the water content of the solvent is low. The water content is preferably 50 ppm or less, more preferably 30 ppm or less, and even more preferably 10 ppm or less, and the closer to 0 ppm the better. In particular, when a sulfide-based solid electrolyte is used, a low water content is preferable.
[0088] The method for applying the solid electrolyte slurry or solution may be, for example, a commonly known method such as doctor blade coating, dip coating, spin coating, comma coating, gravure coating, spray coating, or bar coater coating.
[0089] When the solid electrolyte layer is produced using a known wet coating method, known thickeners may be added for the purpose of adjusting viscosity, for example, cellulose compounds such as carboxymethyl cellulose, methyl cellulose, ethyl cellulose, and hydroxypropyl cellulose; ammonium salts or alkali metal salts of the above cellulose compounds; polyvinyl alcohol-based polymers or copolymers thereof such as polyvinyl alcohol, modified polyvinyl alcohol, and ethylene-vinyl alcohol copolymer; saponified copolymers of vinyl esters and unsaturated carboxylic acids such as (meth)acrylic acid, maleic acid, and fumaric acid; and the like.
[0090] After applying a slurry or solution of the solid electrolyte, the solid electrolyte layer before thermal compression can be obtained by drying to remove the solvent. The drying temperature is, for example, preferably 30 to 300°C, more preferably 60 to 250°C, and particularly preferably 70 to 190°C. Drying may be carried out in vacuum or under reduced pressure. Heating within this temperature range makes it easy to suppress deterioration of the solid electrolyte and the support.
[0091] As described above, the method of pressurizing a solid electrolyte layer into pores in a support, as described in Patent Document 4, tends to result in insufficient pressurization of the solid electrolyte into the pores of the support. Therefore, such a method is generally unsuitable for the present embodiment. From the viewpoint of suppressing the generation of interconnected voids, it is considered effective to thermally compress a specific support and solid electrolyte under specific conditions.
[0092] [Solid secondary battery] [Positive electrode] The positive electrode functions as a positive electrode of a solid secondary battery and may be a known positive electrode. A preferred positive electrode contains a positive electrode active material and a solid electrolyte, and optionally further contains a conductive aid, a binder, and additives similar to those that may be contained in the solid electrolyte layer.
[0093] It is preferable that the positive electrode contains a material capable of electrochemically absorbing and releasing ions as a positive electrode active material, since this tends to enable high voltage and high energy density to be obtained. Examples of such materials include those represented by the following general formulas (2a) and (2b): Li x MO2(2a) Li y M2O4(2b) {wherein each M is independently one or more metals selected from transition metals, x is a number from 0 to 1.3, and y is a number from 0 to 2}, as well as other Li-containing compounds.
[0094] Examples of the Li-containing compounds represented by the general formulas (2a) and (2b) include lithium cobalt oxides such as LiCoO2; lithium manganese oxides such as LiMnO2, LiMn2O4, and Li2Mn2O4; lithium nickel oxides such as LiNiO2; z Examples include lithium-containing composite metal oxides represented by MO2 (wherein M is one or more elements selected from the group consisting of Ni, Mn, Co, Al, and Mg, and z is a number greater than 0.9 and less than 1.2). If necessary, other metal elements may be added to M.
[0095] The other Li-containing compounds may be any compounds containing Li. Examples of such other Li-containing compounds include composite oxides containing Li and a transition metal element, metal chalcogenides containing Li, phosphate compounds containing Li and a transition metal element, and metal silicate compounds containing Li and a transition metal element (e.g., Li t M u SiO4, M has the same meaning as in the above formula (2a), t is a number from 0 to 1, and u is a number from 0 to 2. From the viewpoint of obtaining a higher voltage, other Li-containing compounds are particularly preferably composite oxides containing Li and one or more transition metal elements selected from the group consisting of cobalt (Co), nickel (Ni), manganese (Mn), iron (Fe), copper (Cu), zinc (Zn), chromium (Cr), vanadium (V), and titanium (Ti), and phosphate compounds.
[0096] More specifically, other Li compounds include a composite oxide containing Li and a transition metal element, a metal chalcogenide containing Li and a transition metal element, and a metal phosphate compound containing Li, and further preferably a composite oxide containing Li and a transition metal element and a metal phosphate compound containing Li. For example, the compounds represented by the following general formulas (3a) and (3b), respectively: Li v M I O2(3a) Li w M II PO4(3b) {In formula, MI and M II are each one or more transition metal elements, the values of v and w vary depending on the charge / discharge state of the battery, v is a number from 0.05 to 1.10, and w is a number from 0.01 to 1.10.
[0097] The compound represented by the general formula (3a) has a layered structure, and the compound represented by the general formula (3b) has an olivine structure. From the viewpoint of stabilizing the structure, these compounds may be compounds in which a part of the transition metal element is substituted with Al, Mg, or another transition metal element, compounds in which these metal elements are contained in the crystal grain boundaries, compounds in which a part of the oxygen atoms is substituted with fluorine atoms, or compounds in which at least a part of the surface of the positive electrode active material is coated with another positive electrode active material.
[0098] As the positive electrode active material, the above-mentioned Li-containing compound may be used alone, or the Li-containing compound may be used in combination with other positive electrode active materials.
[0099] Examples of such other positive electrode active materials include metal oxides or metal chalcogenides having a tunnel structure and a layer structure, sulfur, conductive polymers, etc. Examples of metal oxides or metal chalcogenides having a tunnel structure and a layer structure include MnO2, FeO2, FeS2, VO5, and VO. 13 Examples of the conductive polymer include oxides, sulfides, and selenides of metals other than lithium, such as TiO2, TiS2, MoS2, and NbSe2. Examples of the conductive polymer include conductive polymers such as polyaniline, polythiophene, polyacetylene, and polypyrrole.
[0100] The positive electrode active material in this embodiment may be the above-mentioned positive electrode active material with an arbitrary coating applied to its surface. Examples of the coating material include, but are not limited to, ion-conductive materials containing Li, Nb, P, and O. The positive electrode active material may be used alone or in combination of two or more.
[0101] The mass proportion of the positive electrode active material in the positive electrode mixture layer is preferably 60 mass% or more, more preferably 70 mass% or more, and even more preferably 80 mass% or more. The average particle size (primary particle size) of the positive electrode active material is preferably 0.05 to 100 μm, more preferably 1 to 20 μm, and even more preferably 2 to 15 μm. The average particle size of the positive electrode active material can be measured using an existing particle size measuring device (for example, a laser diffraction / scattering particle size distribution analyzer, a dynamic light scattering particle size distribution analyzer, etc.).
[0102] The solid electrolyte may be the same as the solid electrolyte used in the solid electrolyte layer, and may be the same as that contained in the solid electrolyte layer. The mass proportion of the solid electrolyte is preferably 8 to 40 mass%, more preferably 12 to 35 mass%, and even more preferably 15 to 30 mass%.
[0103] Examples of conductive additives include carbon black, such as graphite, acetylene black, and ketjen black, activated carbon, various cokes, and carbon fibers such as carbon nanotubes. Metal powders such as aluminum, titanium, and stainless steel may also be used. The number-average particle size (primary particle size) of the conductive additive is preferably 10 nm to 10 μm, and more preferably 20 nm to 1 μm. The number-average particle size of the conductive additive is measured in the same manner as the number-average particle size of the positive electrode active material. The mass proportion of the conductive additive is preferably 0.5 to 10 mass%, more preferably 0.8 to 6 mass%, and even more preferably 1.1 to 4 mass%.
[0104] The binder may be the same as the binder species that may be contained in the solid electrolyte layer, and may be the same as that contained in the solid electrolyte layer. The mass proportion of the binder is preferably 0 to 4 mass%, more preferably 0.3 to 3 mass%, and even more preferably 0.6 to 2 mass%.
[0105] The positive electrode can be obtained, for example, as follows. First, a predetermined amount of positive electrode active material and solid electrolyte are mixed, and a conductive aid, binder, additive, etc. are added as needed. The resulting positive electrode mixture is dispersed in a solvent to prepare a positive electrode mixture-containing slurry. The solvent is not particularly limited, and any conventionally known solvent may be used. However, the solvents exemplified for wet production of the solid electrolyte layer can be suitably used. Next, the positive electrode mixture-containing slurry is applied to a positive electrode current collector and dried to form a positive electrode mixture layer.
[0106] The positive electrode current collector is made of, for example, a metal foil such as aluminum foil, nickel foil, titanium foil, or stainless steel foil, or a resin sheet containing a conductive material and having conductivity. The positive electrode current collector may have a carbon coating on its surface and may be processed into a mesh or foam shape. The thickness of the positive electrode current collector is preferably 5 to 35 μm, more preferably 7 to 30 μm, and even more preferably 9 to 25 μm.
[0107] The positive electrode can be produced, for example, by applying the positive electrode mixture-containing slurry to the current collector and drying the slurry. The production, application, and drying of the slurry can be carried out by conventionally known methods.
[0108] Examples of methods for producing the slurry include a rotary mixer, a planetary mixer, a bead mill, and a thin film rotary mixer. Examples of methods for applying the slurry include commonly known methods such as doctor blade coating, dip coating, spin coating, comma coating, gravure coating, spray coating, and bar coater coating.
[0109] The dried positive electrode mixture layer is optionally compressed by a roll press or the like to obtain a positive electrode in which the positive electrode mixture layer is formed on the positive electrode current collector. The thickness of the compressed positive electrode mixture is preferably 10 to 400 μm, more preferably 20 to 350 μm, and even more preferably 30 to 300 μm.
[0110] [Negative electrode] The negative electrode may be any known negative electrode that electrochemically absorbs and releases ions as a negative electrode for a solid secondary battery. A preferred negative electrode contains a negative electrode active material and a solid electrolyte, and optionally further contains a conductive aid, a binder, and additives similar to those that may be contained in the solid electrolyte layer.
[0111] The negative electrode preferably contains, as the negative electrode active material, one or more materials selected from the group consisting of materials capable of absorbing and releasing Li ions and metallic Li. Examples of such materials include metallic Li, amorphous carbon (hard carbon), artificial graphite, natural graphite, pyrolytic carbon, coke, glassy carbon, sintered organic polymer compounds, mesocarbon microbeads, carbon fiber, activated carbon, graphite, carbon colloid, and carbon black; and materials containing elements capable of forming an alloy with Li. Examples of the coke include pitch coke, needle coke, and petroleum coke. Sintered organic polymer compounds are carbonized by sintering polymer materials such as phenolic resins and furan resins at an appropriate temperature. The carbon material may contain, in addition to carbon, heteroelements or heterocompounds such as O, B, P, N, S, Si, SiC, SiO, SiO2, and BC. The content of the heteroelements or heterocompounds is preferably 0 to 10% by mass.
[0112] The material containing an element capable of forming an alloy with Li may be a metal or semimetal element, alloy, or compound, and may have one or more of these phases at least in part.
[0113] In this specification, the term "alloy" includes not only those composed of two or more metallic elements, but also those containing one or more metallic elements and one or more metalloid elements. Furthermore, as long as the alloy as a whole has metallic properties, it may contain non-metallic elements. The alloy structure may be a solid solution, a eutectic (eutectic mixture), or an intermetallic compound, or two or more of these may coexist.
[0114] Examples of metal elements and metalloid elements that can form an alloy with Li include titanium (Ti), tin (Sn), lead (Pb), aluminum (Al), indium (In), silicon (Si), zinc (Zn), antimony (Sb), bismuth (Bi), gallium (Ga), germanium (Ge), arsenic (As), silver (Ag), hafnium (Hf), zirconium (Zr), and yttrium (Y). Among these, metal elements and metalloid elements in Group 4 or Group 14 of the long-form periodic table are preferred. Titanium, silicon, and tin are particularly preferred because they have a high ability to absorb and release Li and can achieve high energy density.
[0115] Examples of tin alloys include those having, as a second constituent element other than tin, one or more elements selected from the group consisting of silicon, magnesium (Mg), nickel, copper, iron, cobalt, manganese, zinc, indium, silver, titanium (Ti), germanium, bismuth, antimony, and chromium (Cr).
[0116] Examples of silicon alloys include those having, as a second constituent element other than silicon, one or more elements selected from the group consisting of magnesium, nickel, copper, iron, cobalt, manganese, zinc, indium, silver, titanium, germanium, bismuth, antimony, and chromium.
[0117] Examples of titanium compounds, tin compounds, and silicon compounds include those containing oxygen (O) or carbon (C), which may contain the above-mentioned second constituent element in addition to titanium, tin, or silicon.
[0118] The negative electrode is made of anode active material, 0.4 to 3V vs. Li / Li + The lithium ion-absorbing material may contain a metal compound capable of absorbing Li ions within the range of 1 to 4. Examples of such metal compounds include metal oxides, metal sulfides, and metal nitrides.
[0119] Examples of metal oxides include titanium oxide, lithium titanium oxide (lithium titanium-containing composite oxide), tungsten oxide (e.g., WO3), amorphous tin oxide (e.g., SnB 0.4 P 0.6 O 3.1 ), tin silicon oxide (for example, SnSiO3), and silicon oxide (SiO). Among these, titanium oxide and lithium titanium oxide are preferred.
[0120] Examples of lithium titanium oxides include lithium titanate having a spinel structure {e.g., Li4+aTi5O 12 (wherein a can vary within the range of -1≦a≦3 due to charge-discharge reactions)}, lithium titanate with a ramsdellite structure {for example, Li2+bTi3O7 (wherein b can vary within the range of -1≦b≦3 due to charge-discharge reactions)}, and the like.
[0121] The titanium oxide may or may not contain Li before charge and discharge. Examples of titanium oxides that do not contain Li before charge and discharge (at the time of synthesis) include titanium oxides (e.g., TiO, HTi 12 O 25 Examples of suitable titanium composite oxides include TiO2-P2O5, TiO2-V2O5, TiO2-P2O5-SnO2, and TiO2-P2O5-MeO (wherein Me is at least one element selected from the group consisting of Cu, Ni, and Fe). Titanium composite oxides preferably have low crystallinity and are of the anatase type, and are heat-treated at a temperature of 300 to 500°C. Examples of suitable titanium composite oxides include TiO2-P2O5, TiO2-V2O5, TiO2-P2O5-SnO2, and TiO2-P2O5-MeO (wherein Me is at least one element selected from the group consisting of Cu, Ni, and Fe). Titanium composite oxides preferably have low crystallinity and a microstructure in which a crystalline phase and an amorphous phase coexist, or in which only an amorphous phase exists. Having such a microstructure can significantly improve the cycle performance of solid-state secondary batteries.
[0122] Examples of titanium oxides that contain Li before charge and discharge (at the time of synthesis) include Li cTiO2 (where 0 < c ≤ 1.1) and the like can be mentioned.
[0123] Examples of metal sulfides include titanium sulfide (e.g., TiS2), molybdenum sulfide (e.g., MoS2), and iron sulfide (e.g., FeS, FeS2, Li g FeS2 (where g is 0 ≤ g ≤ 1)). Examples of metal nitrides include lithium cobalt nitride (e.g., Li d Co e N, 0 < d < 4, 0 < e < 0.5).
[0124] From the viewpoint of increasing the battery voltage, the negative electrode of the solid secondary battery in the present embodiment preferably contains a material that occludes lithium ions at a potential lower than 0.4V vs. Li / Li + More inferior potential. Examples of such materials include carbon materials typified by amorphous carbon (hard carbon), artificial graphite, natural graphite, graphite, pyrolytic carbon, coke, glassy carbon, fired bodies of organic polymer compounds, mesocarbon microbeads, carbon fibers, activated carbon, graphite, carbon colloids, and carbon black. In addition, metallic lithium, metal oxides, metal nitrides, lithium alloys, tin alloys, silicon alloys, intermetallic compounds, organic compounds, inorganic compounds, metal complexes, organic polymer compounds, etc. can be mentioned.
[0125] The negative electrode active material is used alone or in combination of two or more. The mass ratio of the negative electrode active material in the negative electrode composite material layer is preferably 50% by mass or more, more preferably 60% by mass or more, and still more preferably 65% by mass or more.
[0126] The number average particle diameter (primary particle diameter) of the negative electrode active material is preferably 0.1 to 30 μm, and more preferably 1 to 20 μm. The number average particle diameter of the negative electrode active material is measured in the same manner as the number average particle diameter of the positive electrode active material. As the solid electrolyte, conductive assistant, binder, and additive that the negative electrode may contain, the same ones as those used for the positive electrode composite material layer described above can be used.
[0127] The mass proportion of the solid electrolyte is preferably 10 to 50 mass%, more preferably 15 to 40 mass%, and even more preferably 20 to 35 mass%. The mass proportion of the conductive additive is preferably 0 to 10 mass%, more preferably 0.5 to 6 mass%, and even more preferably 1 to 4 mass%. The mass proportion of the binder is preferably 0 to 5 mass%, more preferably 0.5 to 4 mass%, and even more preferably 1 to 3 mass%.
[0128] The negative electrode can be obtained, for example, as follows. First, a predetermined amount of the negative electrode active material and solid electrolyte are mixed, and a conductive aid, binder, additive, etc. are added as needed. The resulting negative electrode mixture is dispersed in a solvent to prepare a negative electrode mixture-containing slurry. The solvent is not particularly limited, and any conventionally known solvent may be used. However, the solvents exemplified for wet preparation of the solid electrolyte layer can be suitably used. Next, the negative electrode mixture-containing slurry is applied to a negative electrode current collector and dried to form a negative electrode mixture layer.
[0129] The negative electrode current collector is made of, for example, a metal foil such as copper foil, nickel foil, or stainless steel foil. The negative electrode current collector may have a carbon coating on its surface or may be processed into a mesh. The thickness of the negative electrode current collector is preferably 5 to 40 μm, more preferably 6 to 35 μm, and even more preferably 7 to 30 μm.
[0130] The slurry can be applied by any commonly known method, such as doctor blade coating, dip coating, spin coating, comma coating, gravure coating, spray coating, or bar coater coating.
[0131] The negative electrode mixture layer obtained after drying is compressed as needed using a roll press or the like to obtain a negative electrode in which the negative electrode mixture layer is formed on the negative electrode current collector. The thickness of the compressed negative electrode mixture layer is preferably 10 to 300 μm, more preferably 20 to 280 μm, and even more preferably 30 to 250 μm.
[0132] [Solid-state secondary battery exterior] The structure of the exterior of the solid secondary battery is not particularly limited, and for example, either a battery can or a laminate film exterior can be used. As the battery can, for example, a metal can made of steel or aluminum can be used. As the laminate film exterior, for example, two laminate films each having a three-layer structure of heat-melting resin / metal film / resin can be stacked with the heat-melting resin side facing inward and the edges can be heat-sealed.
[0133] When a laminate film exterior body is used, a positive electrode terminal (or a lead tab connected to the positive electrode terminal) and a negative electrode terminal (or a lead tab connected to the negative electrode terminal) may be connected to the positive electrode current collector and the negative electrode current collector, respectively, and the laminate film exterior body may be sealed with the ends of both terminals (or lead tabs) extended to the outside of the exterior body.
[0134] [Method for manufacturing solid secondary batteries]
[0135] The solid secondary battery of this embodiment has the solid electrolyte layer of this embodiment between the positive electrode and the negative electrode. In this embodiment, layer 3 is bonded to layer 2 so as to be located on the negative electrode side, and if layer 4 is included, layer 4 is bonded to layer 2 so as to be located on the positive electrode side. The solid electrolyte layer may be formed as a solid electrolyte sheet having self-standing strength, and the positive electrode, the solid electrolyte sheet, and the negative electrode may be laminated and bonded in this order. Alternatively, the sheet serving as a substrate and the solid electrolyte layer formed on a film may be transferred to the positive electrode or the negative electrode, laminated, and then bonded. When bonding, the solid electrolyte layer may be wrapped in a laminate film exterior or the like as needed, and then pressed by roll pressing, plate pressing, cold isostatic pressing, or warm isostatic pressing, for example.
[0136] Next, the above layers are housed in a battery case (battery exterior) and sealed to produce the solid secondary battery of this embodiment. The shape of the solid secondary battery of this embodiment is not particularly limited, and suitable shapes include, for example, a cylindrical shape, an elliptical shape, a rectangular tube shape, a button shape, a coin shape, a flat shape, and a laminate shape.
[0137] The solid secondary battery of this embodiment can function as a battery after initial charging. There are no particular limitations on the method of initial charging in this embodiment, but the initial charging is preferably performed at 0.01 to 1 C, more preferably at 0.05 to 0.5 C, and even more preferably at 0.1 to 0.2 C. Here, 1 C refers to a current that can discharge the rated capacity of a specified battery (capacity equivalent to a fully charged battery) in one hour. The above initial charging may be performed multiple times.
[0138] The solid secondary battery of this embodiment can also be used as a battery pack by connecting a plurality of batteries in series or parallel. From the viewpoint of controlling the charge / discharge state of the battery pack while suppressing deterioration of the active material and solid electrolyte, the operating voltage range per battery is preferably 2.25 to 5 V, more preferably 2.5 to 4.75 V, and particularly preferably 2.75 V to 4.5 V. [Example]
[0139] The present invention will be illustrated below by way of examples, but the present invention is not limited to these examples.
[0140] [Example 1] [Preparation of solid electrolyte layer] As a sulfide-based solid electrolyte, argyrodite-type sulfide solid electrolyte Li 7-x PS 6-x Cl x (wherein x≈1) powder (average particle size 3 μm); a binder solution in which 5% by mass of rubber-based resin is dissolved in a low-polarity organic solvent that does not react with the sulfide-based solid electrolyte; The sulfide solid electrolyte and the rubber-based resin were weighed out so that the mass ratio was 96.0:4.0, and the low-polarity organic solvent was further added to adjust the viscosity, followed by kneading with a planetary mixer to obtain a solid electrolyte slurry.
[0141] A polyethylene terephthalate (PET) film with a thickness of approximately 38 μm and one side of which had been treated for release was placed on a tabletop coater with the release-treated side facing up as a substrate. Then, to create layer (B), a solid electrolyte slurry was applied to the release-treated side using an applicator while leaving a predetermined clearance. This was then dried in a dryer at normal pressure and a temperature of 70°C for 1 hour, thereby obtaining a sheet in which a solid electrolyte layer was laminated on a PET film. Next, the sheet was placed on the tabletop coater with the solid electrolyte layer facing up, and a nonwoven fabric (support: average fiber width of approximately 7 μm, thickness of approximately 22 μm, and basis weight of 5 g / m) made of PET resin with a Tg of approximately 75°C and a decomposition temperature of approximately 250°C was laid on top of it. 2 ) was placed on the nonwoven fabric. Next, the solid electrolyte slurry was further applied onto the nonwoven fabric using an applicator while leaving a predetermined clearance. The resultant was then dried in a dryer at normal pressure and a temperature of 70°C for 1 hour, and then reduced pressure and dried in a dryer at a temperature of 70°C for 20 hours. This resulted in a solid electrolyte layer in which a solid electrolyte layer (layer (B)), a nonwoven fabric-containing solid electrolyte layer (layer (A)), and a solid electrolyte layer (layer (C)) were sequentially laminated on the PET film.
[0142] [Fabrication of solid electrolyte sheet] The solid electrolyte layer obtained on the PET film was pressed at a pressure of 392 MPa to peel off the PET film from the layer, thereby obtaining a solid electrolyte sheet with no warping and sufficient self-standing strength.
[0143] [Preparation of positive electrode] The positive electrode active material is LiNi, which has a composite oxide of Li and Nb formed on its surface. 0.5 Co 0.2 Mn 0.3 O2 powder (average particle size 5 μm); Argyrodite-type sulfide solid electrolyte Li 7-x PS 6-x Cl x (wherein x≈1) powder (average particle size 0.6 μm); As a conductive additive, carbon fiber ("VGCF" (product name) manufactured by Showa Denko Co., Ltd.) a binder solution in which 5% by mass of rubber-based resin is dissolved in a low-polarity organic solvent that does not react with the sulfide-based solid electrolyte; The positive electrode active material, sulfide solid electrolyte, carbon fiber, and rubber-based resin were weighed out so that the mass ratio was 82.7:15.3:1.2:0.8, and the low-polarity organic solvent was further added to adjust the viscosity, followed by kneading with a planetary mixer to obtain a positive electrode slurry.
[0144] A 20 μm thick aluminum foil was placed on a tabletop coater, and the positive electrode slurry was applied to the aluminum foil with a predetermined clearance using an applicator. The applied aluminum foil was then dried in a dryer at 100°C under normal pressure for 1 hour, and then dried in a dryer at 100°C under reduced pressure for 20 hours to obtain a positive electrode.
[0145] [Preparation of negative electrode] As the negative electrode active material, natural graphite powder (average particle size 16 μm) and Argyrodite-type sulfide solid electrolyte Li 7-x PS 6-x Cl x (wherein x≈1) powder (average particle size 0.6 μm); a binder solution in which 5% by mass of rubber-based resin is dissolved in a low-polarity organic solvent that does not react with the sulfide-based solid electrolyte; The negative electrode active material, sulfide solid electrolyte, and rubber-based resin were weighed out so that the weight ratio was 67.5:30.5:2, and the low-polarity organic solvent was further added to adjust the viscosity, followed by kneading with a planetary mixer to obtain a negative electrode slurry.
[0146] A stainless steel foil with a total thickness of 10 μm and a carbon coating was placed on a tabletop coater. The negative electrode slurry was applied to the carbon-coated surface using an applicator with a predetermined clearance. The resulting mixture was dried in a dryer at 100°C under normal pressure for 1 hour, and then dried again in a dryer at 100°C under reduced pressure for 20 hours to obtain a negative electrode.
[0147] [Fabrication of solid-state secondary batteries] The positive electrode, the negative electrode, and the solid electrolyte sheet were each punched to a predetermined size. Then, layers were obtained by stacking these in the order of positive electrode composite layer, solid electrolyte sheet, and negative electrode composite layer. The solid electrolyte sheet was positioned on the negative electrode side relative to layer (A), with the layer that had been in contact with the PET film substrate becoming layer (B). The resulting layer was wrapped in stainless steel foil, and the outside was further wrapped in aluminum laminate film, and the layer was then vacuum-sealed to place the layer in a packaging material. This packaging material was heated and compressed at 980 MPa at 190°C, which is 100°C or more higher than the Tg of the support, just before the decomposition of the solid electrolyte begins, and below the melting temperature of the support. This compressed the support in the solid electrolyte layer while thermoplastically deforming it, densifying the laminate and pressing the bonding surfaces.
[0148] After removing the pressed layer from the packaging, lead tabs were ultrasonically welded to the positive and negative electrodes, respectively, and the layer with the attached lead tabs was then wrapped in aluminum laminate and vacuum-sealed to produce a solid-state secondary battery.
[0149] [Structure of solid electrolyte layer] The resulting solid-state secondary battery was cut with a sharp razor blade, and then the cross section was smoothed using a cross-section polisher with an argon ion beam in an air-protected environment. The cross section was then observed using an SEM. Three cross-section samples were prepared and observed (e.g., at 1500x magnification or less). In all cross-sections, the pores of the support in the solid electrolyte layer were completely filled with solid electrolyte, and no interconnected voids were observed in the layer direction (parallel to the sheet surface of the support). Furthermore, because the melting point of the support was approximately 250°C, the shape of the support deformed to conform to the shape of the solid electrolyte particles, but they did not melt and diffuse into the solid electrolyte. In other words, the continuity of the sheet-like support was ensured. Furthermore, the average thickness of layer (A) was 23 μm, the average thickness of layer (B) was 29 μm, and the average thickness of layer (C) was 9 μm. In other words, the support was sufficiently separated from the composite layers of the positive and negative electrodes.
[0150] [Charge / discharge evaluation of solid secondary batteries] The fabricated solid-state secondary battery was tested under a confining pressure of 0.15 ton / cm 2 The battery was restrained with a stainless steel restraining jig so that the battery was in this state. In this state, charge / discharge evaluation was carried out.
[0151] (Initial charge / discharge) In this section, "Initial Charge and Discharge," the 1C current was determined based on the reference capacity of the positive electrode active material, 204mAh / g, at 4.35V. The 1C current value, "1.0C," is the current value at which a fully charged battery can discharge its electrical charge in 1 hour.
[0152] Using a charge / discharge device (Toyo Systems Co., Ltd., product name: TOSCAT-3000) in a thermostatic chamber at a constant temperature of 25°C, the battery was charged at a constant current of 0.1 C followed by a constant voltage of 4.35 V until the end current reached 0.01 C. Thereafter, the battery was discharged at a constant current of 0.1 C followed by a constant voltage of 3.0 V until the end current reached 0.01 C (first cycle of charge / discharge). The second and third cycles of charge / discharge were carried out under the same conditions as the first cycle.
[0153] (Charging load characteristic evaluation) In this section, "Charge Load Characteristics Evaluation," the discharge capacity from full charge to 3.0 V in the 0.1 C constant current discharge at the third initial charge / discharge cycle was determined as the rated capacity of the battery, and the 1 C current was determined based on this. The 1 C current in this charge load characteristics evaluation is approximately 2.9 mA / cm in current density notation. 2 It was.
[0154] After the initial charge and discharge, the battery was charged at a constant current of 0.1 C using the same charge / discharge device in the same thermostatic chamber at 25°C, followed by a charge at a constant voltage of 4.35 V until the cutoff current reached 0.01 C. After that, the battery was discharged at a constant current of 0.1 C and then at a constant voltage of 3.0 V until the cutoff current reached 0.01 C. The charge / discharge efficiency (%) = [(discharge capacity) / (charge capacity)] × 100 was 99.5% or higher.
[0155] The battery was then charged at a constant current of 1 C until the cut-off voltage reached 4.35 V, then discharged at a constant current of 0.1 C, and then discharged at a constant voltage of 3.0 V until the cut-off current reached 0.01 C (charge-discharge condition A). The charge-discharge efficiency at this time was 100.2%.
[0156] Thereafter, charging and discharging were repeated in the same manner as under charge-discharge condition A, except that the charging current values were changed to 2C, 3C, 4C, 5C, and 6C. The charge-discharge efficiency at each charging current value is shown in Table 1. The battery was considered to have short-circuited when the charge-discharge efficiency at each charging current fell below 95% or when a voltage drop of 40mV or more occurred during charging. The results of the charge-discharge evaluation are shown in Table 1. At 5C, approximately 14.4mA / cm 2 A charge / discharge efficiency of over 95% was obtained up to 1000 sq m, demonstrating that the battery has high short-circuit resistance even at high current densities.
[0157] [Example 2] The support was a nonwoven fabric made of PET resin with a Tg of approximately 75°C and a decomposition temperature of approximately 250°C (support: average fiber width of approximately 5 μm, thickness of approximately 18 μm, and basis weight of 4 g / m 2 A solid secondary battery was fabricated in the same manner as in Example 1, except that ) was used.
[0158] Three cross-sectional samples were observed using the same method as in Example 1. In all cross-sectional observations, the pores of the support in the solid electrolyte layer were completely filled with solid electrolyte, and no interconnected voids were observed in the layer direction (parallel to the sheet surface of the support). The shape of the support was deformed to conform to the shape of the solid electrolyte particles, and no melting or diffusion into the solid electrolyte occurred. This ensured the continuity of the sheet-like support. The average thickness of layer (A) was 11 μm, the average thickness of layer (B) was 34 μm, and the average thickness of layer (C) was 12 μm. No voids were observed in layers (B) and (C), and their density was unchanged from Example 1. This meant that the support was sufficiently separated from the composite layers of the positive and negative electrodes.
[0159] The results of charge / discharge evaluation carried out in the same manner as in Example 1 are also shown in Table 1. The charge / discharge current was approximately 14.4 mA / cm at 5 C. 2 A charge / discharge efficiency of over 95% was obtained up to 1000 sq m, demonstrating that the battery has high short-circuit resistance even at high current densities.
[0160] [Example 3] The support was a nonwoven fabric made of PET resin with a Tg of approximately 75°C and a decomposition temperature of approximately 250°C (support: average fiber width approximately 19 μm, thickness approximately 28 μm, basis weight 8 g / m 2 , and an average opening diameter of 71 μm). A polyethylene terephthalate (PET) film with a thickness of approximately 38 μm and a release-treated surface on one side was placed on a tabletop coater as a substrate, with the release-treated surface facing up. Then, to create layer (B), a solid electrolyte slurry was applied to the release-treated surface using an applicator while leaving a predetermined clearance. This was then dried in a dryer at 70°C under normal pressure for 1 hour, thereby obtaining a sheet in which a solid electrolyte layer was laminated on a PET film. Next, the sheet was placed on the tabletop coater with the solid electrolyte layer facing up, and a nonwoven fabric was placed on top of it. Next, the solid electrolyte slurry was further applied to the nonwoven fabric using an applicator while leaving a predetermined clearance, and the surface slurry was then scraped off with a squeegee or the like to expose the nonwoven fabric. This was then dried in a dryer at normal pressure and a temperature of 70°C for 1 hour, and then reduced pressure and dried in a dryer at a temperature of 70°C for 20 hours, thereby obtaining a solid electrolyte layer in which a layer consisting of only a solid electrolyte and a nonwoven fabric-containing solid electrolyte layer (layer (A)) were sequentially laminated on the PET film.
[0161] A solid secondary battery was produced in the same manner as in Example 1, except that the above solid electrolyte layer was used, and the layer consisting of only the solid electrolyte layer that was in contact with the PET film substrate was positioned on the negative electrode side with respect to layer (A) so as to play the role of layer (B).
[0162] Three cross-sectional samples were observed using the same method as in Example 1. In all cross-sectional observations, the pores of the support in the solid electrolyte layer were filled with solid electrolyte. However, voids in the layer direction (parallel to the sheet surface of the support) were observed, particularly extending from the center of the support where the fiber diameter was large. This is presumably because, despite the large aperture ratio, the average fiber diameter of the nonwoven fabric was large. During thermal compression, the fibers acted as "stop bars," especially at their intersections, resulting in insufficient compression of the solid electrolyte, which involved thermoplastic deformation. However, the length (L1) was short, less than 50 μm, i.e., shorter than the average thickness (T1) of the entire solid electrolyte layer, which was 62 μm. Furthermore, the support was not observed to melt and diffuse into the solid electrolyte, ensuring the continuity of the sheet-like support. The average thickness of layer (A) was 24 μm, and the average thickness of layer (B) was 38 μm. No voids were observed in layer (B), its density was the same as in Example 1, and the support was sufficiently separated from each negative electrode. On the other hand, the positive electrode mixture layer and the support were in contact in many places, i.e., layer (C) was substantially absent.
[0163] The results of charge / discharge evaluation carried out in the same manner as in Example 1 are also shown in Table 1. The charge / discharge current was approximately 8.7 mA / cm at 3 C. 2 A charge-discharge efficiency of 95% or more was obtained up to 4C, which indicated that the battery had high short-circuit resistance even at high current densities. On the other hand, the charge-discharge efficiency was less than 95% at 4C, and a sudden voltage drop due to short circuit occurred at 5C. This indicates that the short-circuit resistance of Example 3 is slightly lower than that of Examples 1 and 2.
[0164] [Comparative Example 1] The support was a nonwoven fabric made of polyarylate resin with a Tg of 193°C and a decomposition temperature of over 300°C (support: average fiber width of approximately 4 μm, thickness of approximately 7 μm, and basis weight of 4 g / m 2 A solid secondary battery was fabricated in the same manner as in Example 1, except that ) was used.
[0165] When three cross-sectional samples were observed using the same method as in Example 1, many gaps were observed in the pores of the support in the solid electrolyte layer. These gaps were long and interconnected in the layer direction (parallel to the sheet surface of the support), with their length (L1) exceeding 100 μm and extending widely into the support, longer than the average thickness (T1) of the entire solid electrolyte layer, which was 58 μm. Furthermore, many of the interfaces between the support and the solid electrolyte were also delaminated. This is presumably because the Tg was higher than the temperature during thermal compression, so the support was unable to undergo thermoplastic deformation during thermal compression, only elastic deformation, resulting in springback of the support after compression, which created interconnected voids in the support. The support was not observed to melt and diffuse into the solid electrolyte, ensuring the continuity of the sheet-like support. The average thickness of layer (A) was 12 μm, the average thickness of layer (B) was 35 μm, and the average thickness of layer (C) was 11 μm. No voids were observed in the layers (B) and (C), and the density was the same as in Example 1. The support was sufficiently separated from the composite layers of the positive and negative electrodes.
[0166] The results of charge / discharge evaluation performed in the same manner as in Example 1 are also shown in Table 1. The voltage dropped during charging at 1 C, and a slight short circuit occurred, i.e., the charge / discharge efficiency decreased, resulting in a sudden voltage drop due to a short circuit at 3 C. From the above, it was found that in Comparative Example 1, a short circuit easily occurred as the current density was increased.
[0167] Comparative Example 2 The support is a composite nonwoven fabric made of thick and thin fibers, consisting of PET resin with a Tg of approximately 75°C and a decomposition temperature of approximately 250°C (support: average fiber width approximately 12 μm, thickness approximately 28 μm, basis weight 8 g / m 2 A solid secondary battery was fabricated in the same manner as in Example 1, except that a pore size of 20 μm was used.
[0168] When three cross-sectional samples were observed using the same method as in Example 1, many gaps were observed in the pores of the support in the solid electrolyte layer. The voids were long and interconnected in the layer direction (parallel to the sheet surface of the support), with some of the voids exceeding 100 μm in length (L1), longer than the average thickness (T1) of the entire solid electrolyte layer, which was 65 μm. However, the gap spacing was smaller than in Comparative Example 1, and there was only slight delamination at the interface between the support and the solid electrolyte. This is thought to be because the nonwoven fabric had a composite structure consisting of thick and thin fibers. In addition to the presence of thick fibers as in Example 3, the average opening diameter was smaller compared to Example 3 despite the same basis weight. This resulted in a decrease in the filling of the pores with the solid electrolyte, resulting in more voids remaining and interconnected, even in a thermoplastic support. The support did not melt and diffuse into the solid electrolyte, ensuring the continuity of the sheet-like support. The average thickness of layer (A) was 25 μm, the average thickness of layer (B) was 30 μm, and the average thickness of layer (C) was 10 μm. No voids were observed in layers (B) and (C), and their density was unchanged from that in Example 1. The support was sufficiently separated from the composite layers of the positive and negative electrodes.
[0169] The results of charge / discharge evaluation performed in the same manner as in Example 1 are also shown in Table 1. During charging at 2C, the voltage dropped, and a slight short circuit occurred, i.e., the charge / discharge efficiency decreased. As a result, a sudden voltage drop due to a short circuit occurred at 3C. After the short circuit, the voltage did not increase, and further charging became difficult. From the above, it was found that in Comparative Example 2, a short circuit easily occurred as the current density increased. That is, even when a thermoplastic support was used for thermal compression, depending on the support structure, particularly in the case of nonwoven fabrics, when the average fiber diameter was large and / or the average opening diameter was small, the solid electrolyte was not compressed or filled sufficiently, which resulted in the generation of interconnected voids and caused a short circuit.
[0170] Comparative Example 3 The same nonwoven fabric as in Example 2 was used as the support, and a solid electrolyte layer in which the nonwoven fabric was exposed on the surface was obtained in the same manner as in Example 3.
[0171] A solid secondary battery was fabricated in the same manner as in Example 1, except that the above solid electrolyte layer was used, and the solid electrolyte sheet was arranged so that the layer consisting of only the solid electrolyte layer that had been in contact with the PET film substrate faced the positive electrode side and played the role of layer (C).
[0172] Three cross-sectional samples were observed using the same method as in Example 1. In all cross-sectional observations, the pores of the support in the solid electrolyte layer were completely filled with solid electrolyte, and no interconnected voids were observed in the layer direction (parallel to the sheet surface of the support). Furthermore, the shape of the support was deformed to conform to the shape of the solid electrolyte particles, and no melting or diffusion into the solid electrolyte was observed. Therefore, the continuity of the sheet-like support was ensured. Furthermore, the average thickness of layer (A) was 11 μm, and the average thickness of layer (C) was 34 μm. No voids were observed in layer (C), and its density was unchanged from Example 1. Furthermore, the support was sufficiently separated from the positive electrode composite layer. On the other hand, the negative electrode composite layer and the support were in contact in many places; that is, layer (B) was substantially absent.
[0173] A charge-discharge evaluation was carried out in the same manner as in Example 1, but a voltage drop occurred immediately after the start of initial charge-discharge, and as a result, the voltage did not increase and further charging became difficult. From the above, it was found that Comparative Example 3, in which the negative electrode mixture layer and the support were in contact, did not function well as a battery, even if there were no interconnected voids in the support. [Table 1]
[0174] From the above, it was confirmed that the solid electrolyte layer and the solid secondary battery in the Examples are superior in suppressing short circuits when a large current flows compared to the Comparative Examples. [Industrial Applicability]
[0175] A solid secondary battery using the solid electrolyte layer of the present invention can be used as a storage battery for electric vehicles, hybrid electric vehicles, electric motorcycles, electric bicycles, stationary power storage systems, mobile communication devices, portable electronic devices, etc. [Explanation of symbols]
[0176] 1, 1a~c, 100: Solid electrolyte layer 2: Solid electrolyte layer with support (layer (A)) 3: Solid electrolyte layer without support (layer (B)) 4: Solid electrolyte layer without support (layer (C)) 5, 5a, 5b: Support part (support body) 6: Solid electrolyte 7: Gap (hole) 8 :Void 9, 9a, 9b: voids (communicating voids) Op: Opening L1: Length of the communicating gap and support part T1: Thickness of the solid electrolyte layer
Claims
1. A solid electrolyte layer formed in a predetermined layer direction, The solid electrolyte layer is A layer (A) having a support including a support portion made of a thermoplastic material and a solid electrolyte filled between the support portions, When a cross section of the layer (A) is viewed, voids that communicate across a plurality of support portions may or may not be observed in the layer (A); When the void is observed, a length (L1) of the void and the plurality of supports along the layer direction is equal to or less than a total thickness (T1) of the solid electrolyte layer.
2. The solid electrolyte layer according to claim 1 , wherein the length (L1) is equal to or greater than 0 and is smaller than a total thickness (T1) of the solid electrolyte layer.
3. The solid electrolyte layer of claim 1 , wherein the solid electrolyte layer comprises a binder.
4. 2. The solid electrolyte layer according to claim 1, wherein the support is an electronically insulating nonwoven fabric, and the average diameter of the fibers constituting the support is 1 μm or more and 10 μm or less.
5. The solid electrolyte layer according to claim 1 , further comprising a layer (B) that does not have the support and is disposed in contact with the layer (A).
6. 6. The solid electrolyte layer according to claim 5, further comprising a layer (C) which does not have a support and is disposed in contact with the layer (A) on the opposite side of the layer (A) from the layer (B).
7. The solid electrolyte layer according to claim 1 , which has self-supporting strength.
8. A solid secondary battery comprising a positive electrode, a negative electrode, and the solid electrolyte layer according to any one of claims 1 to 7.
9. The optical film has no support and has a layer (B) disposed in contact with the layer (A), The solid secondary battery according to claim 8 , wherein the layer (B) is disposed on the negative electrode side.
10. A method for producing the solid electrolyte layer according to any one of claims 1 to 7, comprising the following steps: filling the pores of the support with the solid electrolyte; applying pressure to the support at a temperature above the glass transition temperature of the support and below a decomposition temperature of at least one of the support and the solid electrolyte; The method for producing a solid electrolyte layer comprising the steps of:
11. In the pressurizing step, The method for producing a solid electrolyte layer according to claim 10 , wherein the temperature during pressing is lower than the melting temperature of the support.
12. In the filling step, The method for producing a solid electrolyte layer according to claim 10, further comprising introducing a slurry of the solid electrolyte into the pores of the support in the presence of a selected solvent, followed by removal of the solvent.
Citation Information
Patent Citations
Solid electrolyte sheet and all-solid type secondary battery
JP2016031789A
All-solid type lithium secondary battery and method for manufacturing the same
JP2017208250A
All-solid-state lithium secondary battery and manufacturing method thereof
JP2021150204A
Method for manufacturing solid-state battery sheet and method for manufacturing laminate to be used for the same
JP2021163759A