Inner electrode material for multilayered capacitor and multilayered capacitor including the same

The use of a compound in the chemical formula M1 a+1 M2M3 a as the internal electrode material in multilayer ceramic capacitors addresses cracking and delamination issues during high-temperature sintering, ensuring high electrical conductivity and cost-effective manufacturing by allowing oxidizing atmosphere firing.

JP2024152723APending Publication Date: 2024-10-25SAMSUNG ELECTRO MECHANICS CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
JP2024065414
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-27
Filing Date
2024-04-15
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing multilayer ceramic capacitors face issues such as cracking and delamination due to over-firing during high-temperature sintering, which is exacerbated by the use of nickel powder and requires additional additives like silicon dioxide or barium titanate, leading to decreased electrical conductivity and increased process costs.

Method used

A compound represented by the chemical formula M1 a+1 M2M3 a, where M1 is Ti, V, Sc, or Zr, M2 is Al, Si, or Sn, and M3 is C or N, is used as the internal electrode material, allowing for sintering shrinkage control without additional additives and enabling firing in an oxidizing atmosphere, thus preventing cracking and maintaining electrical conductivity.

Benefits of technology

The solution effectively suppresses sintering shrinkage, prevents cracking, maintains electrical conductivity comparable to nickel, and reduces manufacturing costs by eliminating the need for reducing atmospheres and additional additives.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024152723000001_ABST
    Figure 2024152723000001_ABST
Patent Text Reader

Abstract

To provide a new inner electrode material for a multilayered capacitor capable of suppressing sintering shrinkage without a separate additive during the firing process for manufacturing a capacitor, and capable of being fired even in an oxidizing atmosphere, and a multilayered capacitor including the same.SOLUTION: The present invention relates to a multilayered capacitor which includes a capacitor body including a dielectric layer and an inner electrode, and an external electrode disposed outside the capacitor body. The inner electrode includes a compound represented by the following Chemical Formula 1, and the compound has a BET specific surface area of 1.0 to 2.2 m2 / g. [Chemical Formula 1] M1a+1M2M3a In the Chemical Formula 1, M1 is Ti, V, Sc, Zr or Mo, M2 is Al, Si, Sn, Cd, In, Ga, Ge, Pb, As, S or P, M3 is C or N, and a is 1 to 3.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an internal electrode material for a multilayer capacitor and a multilayer capacitor including the same. [Background technology]

[0002] Multi-layered ceramic capacitors (MLCCs), a type of capacitor component, are chip-type capacitors that are mounted on printed circuit boards of various electronic products such as visual devices such as liquid crystal displays (LCDs) and plasma display panels (PDPs), computers, smartphones, and mobile phones, and serve to charge and discharge electricity.

[0003] Such multilayer ceramic capacitors are used as components of various electronic devices due to their advantages of being small in size, having a high capacitance, and being easy to mount.

[0004] The multilayer ceramic capacitor includes an internal electrode in a dielectric ceramic, and may be manufactured by laminating a conductive paste including an internal electrode material and a ceramic green sheet including a ceramic powder by a sheet method or a printing method, and then co-firing the laminate.

[0005] In this case, nickel (Ni) powder is generally used as the internal electrode material, and BaTiO3 is mainly used as the dielectric ceramic powder. However, to form the dielectric layer, the ceramic green sheet is fired at a high temperature of about 1100℃ or more, and the conductive paste can shrink during sintering at a lower temperature. Therefore, the internal electrode layer may be overfired during firing of the ceramic green sheet, which may cause problems such as cracks and delamination in the internal electrodes. This reduces the performance of the multilayer ceramic capacitor.

[0006] To solve this problem, attempts have been made to control high-temperature sintering shrinkage by adding silicon dioxide (SiO2) or nano-barium titanate (BaTiO3) to the internal electrode conductive paste, or by using metals such as tungsten (W). However, silicon dioxide and barium titanate are non-conductors, which can reduce the electrical conductivity of the electrode, and there are problems with the additives, which require additional processes and costs.

[0007] In addition, nickel powder needs to be sintered in a reducing atmosphere when it is sintered to manufacture a capacitor, but sintering in a reducing atmosphere increases process costs. Summary of the Invention [Problem to be solved by the invention]

[0008] An object of the present invention is to provide a new internal electrode material for a multilayer capacitor, which can suppress sintering shrinkage without additional additives during a sintering process for manufacturing a capacitor and can be sintered even in an oxidizing atmosphere, and a multilayer capacitor including the same. [Means for solving the problem]

[0009] One embodiment of the present invention includes a compound represented by the following chemical formula 1, and the BET specific surface area of ​​the compound is 1.0 to 2.2 m 2 / g of the internal electrode material for the multilayer capacitor. [Chemical formula 1] M1 a+1 M2M3 a In the above Chemical Formula 1, M1 is Ti, V, Sc, Zr or Mo, M2 is Al, Si, Sn, Cd, In, Ga, Ge, Pb, As, S or P, M3 is C or N, and a is 1 to 3.

[0010] In the above Chemical Formula 1, M1 may be Ti or V, M2 may be Al, Si or Sn, and M3 may be C.

[0011] The compound is Ti3AlC2, Ti2AlC, V2AlC, Ti3SiC2 or Ti3SnC 2- may be also possible.

[0012] The compound may have an average particle size (D50) of 400 to 700 nm.

[0013] When analyzed by a Thermomechanical Analyzer (TMA), the compound may have a volume reduction rate of 5% or less at a temperature of 1100° C. compared to a temperature of 800° C.

[0014] The compound has an electrical conductivity of 1.05×10 6 S / m or more.

[0015] Another embodiment of the present invention includes a capacitor body including a dielectric layer and an internal electrode; and an external electrode disposed on the outside of the capacitor body, the internal electrode including a compound represented by the following Chemical Formula 1, and the compound having a BET specific surface area of ​​1.0 to 2.2 m 2 / g. [Chemical formula 1] M1 a+1 M2M3 a In the above Chemical Formula 1, M1 is Ti, V, Sc, Zr or Mo, M2 is Al, Si, Sn, Cd, In, Ga, Ge, Pb, As, S or P, M3 is C or N, and a is 1 to 3.

[0016] In the above Chemical Formula 1, M1 may be Ti or V, M2 may be Al, Si or Sn, and M3 may be C.

[0017] The compound may be Ti3AlC2, Ti2AlC, V2AlC, Ti3SiC2 or Ti3SnC2.

[0018] The compound may have an average particle size (D50) of 400 to 700 nm.

[0019] When analyzed by a Thermomechanical Analyzer (TMA), the compound may have a volume reduction rate of 5% or less at a temperature of 1100° C. compared to a temperature of 800° C.

[0020] The compound has an electrical conductivity of 1.05×10 6 S / m or more.

[0021] The internal electrodes may be free of nickel (Ni), barium titanate (BaTiO3), silicon dioxide (SiO2) and tungsten (W).

[0022] The dielectric layer includes a plurality of dielectric crystal grains, and the dielectric crystal grains are mainly composed of Ba. m It contains TiO3 (0.995≦m≦1.010) and may further contain hafnium (Hf), manganese (Mn), chromium (Cr), silicon (Si), aluminum (Al), magnesium (Mg), tin (Sn), antimony (Sb), germanium (Ge), gallium (Ga), indium (In), or a combination thereof, as a minor component.

[0023] In still another embodiment of the present invention, a method for manufacturing a dielectric green sheet using a dielectric powder is provided. 2 forming a conductive paste layer containing a compound of 0.1 g / g; laminating the dielectric green sheets having the conductive paste layer formed thereon to form a dielectric green sheet laminate; firing the dielectric green sheet laminate in an oxidizing atmosphere to form a capacitor body including a dielectric layer and an internal electrode; and forming an external electrode on one surface of the capacitor body.

[0024] The oxidizing atmosphere can be air or oxygen (O2) atmosphere.

[0025] The firing can be carried out by a hot press method.

[0026] The conductive paste layer may be free of nickel (Ni), barium titanate (BaTiO3), silicon dioxide (SiO2) and tungsten (W). Effect of the Invention

[0027] The internal electrode material for a capacitor according to an embodiment of the present invention can suppress sintering shrinkage without additional additives during a sintering process for manufacturing a capacitor, can be sintered in an oxidizing atmosphere, and can achieve electrical conductivity similar to or improved from that of nickel, which has been commonly used as a conventional internal electrode material.

[0028] This reduces the manufacturing cost of the capacitor and improves the performance of the capacitor. [Brief description of the drawings]

[0029] [Figure 1] 1 is a perspective view of a multilayer capacitor according to an embodiment of the present invention; [Diagram 2] 2 is a cross-sectional view of the multilayer capacitor taken along line II' in FIG. [Diagram 3] 2 is an exploded perspective view showing a laminated structure of internal electrodes in the capacitor body of FIG. 1. [Figure 4] 1 is a graph showing the results of a Thermomechanical Analyzer (TMA) analysis in Experimental Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0030] Hereinafter, with reference to the accompanying drawings, an embodiment of the present invention will be described in detail so that a person having ordinary skill in the art to which the present invention belongs can easily carry out the present invention. In order to clearly explain the present invention in the drawings, parts that are not related to the description are omitted, and the same or similar components are given the same reference numerals throughout the specification. In addition, the attached drawings are intended to facilitate understanding of the embodiments disclosed in the present specification, and the technical ideas disclosed in the present specification are not limited by the attached drawings, and it should be understood that the drawings include all modifications, equivalents, or alternatives included in the idea and technical scope of the present invention.

[0031] Terms including ordinal numbers such as first, second, etc. may be used to describe various components, but the components are not limited by the terms. These terms are used only to distinguish one component from another.

[0032] When a component is described as being "coupled" or "connected" to another component, it should be understood that it may be directly coupled or connected to or face the other component, but that there may be other components between them. On the other hand, when a component is described as being "directly coupled" or "directly connected" to another component, it should be understood that there are no other components between them.

[0033] Throughout the specification, terms such as "comprise" or "have" are to be understood as specifying the presence of a feature, number, step, operation, component, part, or combination thereof described in the specification, but not precluding the presence or addition of one or more other features, numbers, steps, operations, components, parts, or combinations thereof. Thus, when a part is described as "comprising" certain elements, this means that it can further include other elements, rather than excluding other elements, unless specifically stated to the contrary.

[0034] FIG. 1 is a perspective view of a multilayer capacitor according to one embodiment of the present invention.

[0035] FIG. 2 is a cross-sectional view of the multilayer capacitor taken along line II' in FIG.

[0036] FIG. 3 is an exploded perspective view showing a laminated structure of internal electrodes in the capacitor body of FIG.

[0037] To clearly explain the present embodiment, the directions are defined as follows: the L axis, the W axis, and the T axis shown in the drawings indicate the length direction, the width direction, and the thickness direction of the capacitor body 110, respectively. Here, the thickness direction (T axis direction) is a direction perpendicular to the wide surface (main surface) of the sheet-shaped component, and can be used in the same concept as the lamination direction in which the dielectric layers 111 are laminated, for example. The length direction (L axis direction) is a direction extending parallel to the wide surface (main surface) of the sheet-shaped component, and can be a direction substantially perpendicular to the thickness direction (T axis direction), and can be a direction in which the first external electrode 131 and the second external electrode 132 are located on both sides, for example. The width direction (W axis direction) is a direction extending parallel to the wide surface (main surface) of the sheet-shaped component, and can be a direction substantially perpendicular to the thickness direction (T axis direction) and the length direction (L axis direction), and the length of the sheet-shaped component in the length direction (L axis direction) can be longer than the length in the width direction (W axis direction).

[0038] 1 to 3, a multilayer capacitor 100 according to an embodiment of the present invention may include a capacitor body 110, and a first external electrode 131 and a second external electrode 132 arranged on opposite ends of the capacitor body 110 in a longitudinal direction (L-axis direction).

[0039] The capacitor body 110 may be, for example, generally hexahedral in shape.

[0040] For ease of explanation in this embodiment, the two surfaces of the capacitor body 110 that face each other in the thickness direction (T-axis direction) are defined as the first surface and the second surface, the two surfaces that are connected to the first surface and the second surface and face each other in the length direction (L-axis direction) are defined as the third surface and the fourth surface, and the two surfaces that are connected to the first surface and the second surface and are connected to the third surface and the fourth surface and face each other in the width direction (W-axis direction) are defined as the fifth surface and the sixth surface.

[0041] As an example, the first surface of the lower surface can be the surface facing the mounting direction. The first to sixth surfaces may be flat, but the present embodiment is not limited to this. For example, the first to sixth surfaces may be curved surfaces with a convex center, and the corners that are the boundaries between the surfaces may be rounded.

[0042] The shape and size of the capacitor body 110 and the number of laminated dielectric layers 111 are not limited to those shown in the drawings of this embodiment.

[0043] The capacitor body 110 is formed by stacking a plurality of dielectric layers 111 in the thickness direction (T-axis direction) and then firing the same, and includes first internal electrodes 121 and second internal electrodes 122 arranged alternately in the thickness direction (T-axis direction) between the plurality of dielectric layers 111.

[0044] At this time, the boundaries between the adjacent dielectric layers 111 of the capacitor body 110 may be integrated to such an extent that it is difficult to confirm the boundaries without using a scanning electron microscope (SEM).

[0045] The capacitor body 110 may also include an active area and a cover area 112 , 113 .

[0046] The active area is a portion that contributes to forming the capacitance of the multilayer capacitor 100. As an example, the active area may be an overlapping area of ​​the first internal electrode 121 or the second internal electrode 122 that are stacked along the thickness direction (T-axis direction).

[0047] The cover regions 112 and 113 may be located on the first and second surfaces of the active region in the thickness direction (T-axis direction) as thickness direction margins. The cover regions 112 and 113 may be a single dielectric layer 111 or two or more dielectric layers 111 stacked on the upper and lower surfaces of the active region, respectively.

[0048] In addition, the capacitor body 110 may further include a side cover region. The side cover region may be located on the fifth and sixth sides of the active region in the width direction (W-axis direction) as a width direction margin part. Such a side cover region may be formed by applying a conductive paste layer for forming an internal electrode to only a part of the surface of the dielectric green sheet when applying a conductive paste layer for forming an internal electrode to the surface of the dielectric green sheet, laminating dielectric green sheets on both sides of the surface of the dielectric green sheet without applying a conductive paste layer, and then firing the laminate.

[0049] The cover regions 112, 113 and the side cover regions serve to prevent the first internal electrode 121 and the second internal electrode 122 from being damaged by physical or chemical stress.

[0050] At this time, the internal electrode according to the present invention includes a compound represented by the following Chemical Formula 1 as an internal electrode material. [Chemical formula 1] M1 a+1 M2M3 a In the above Chemical Formula 1, M1 is Ti, V, Sc, Zr or Mo, M2 is Al, Si, Sn, Cd, In, Ga, Ge, Pb, As, S or P, M3 is C or N, and a is 1 to 3.

[0051] As described later, a multilayer capacitor can be manufactured by laminating ceramic green sheets containing a conductive paste and ceramic powder by a sheet method, a printing method, or the like, and co-firing the laminate.

[0052] Previously, nickel (Ni) powder was commonly used as the internal electrode material, and BaTiO3 was mainly used as the dielectric ceramic powder. However, to form the dielectric layer, the ceramic green sheet is fired at a high temperature of about 1100℃ or more, while the conductive paste containing nickel powder shrinks at a lower temperature. Therefore, the internal electrode layer can be overfired during firing of the ceramic green sheet, which can cause problems such as cracks and delamination in the internal electrode. This reduces the performance of the multilayer capacitor.

[0053] To solve this problem, attempts have been made to control high-temperature sintering shrinkage by adding silicon dioxide (SiO2) or nano-barium titanate (BaTiO3) to the internal electrode conductive paste, or by using metals such as tungsten (W). However, silicon dioxide and barium titanate are non-conductors, which can reduce the electrical conductivity of the electrode, and there are problems with the additives incurring additional processes and costs.

[0054] In addition, when nickel powder is sintered to manufacture a capacitor, the sintering atmosphere must be controlled to be a reducing atmosphere, but sintering in a reducing atmosphere increases the process cost.

[0055] Meanwhile, the internal electrode according to the present invention has a very high sintering shrinkage temperature and a low sintering shrinkage rate at high temperatures without the need for additional additives by including the compound represented by Formula 1 as an internal electrode material, thereby preventing cracks or peeling of the internal electrodes and preventing performance degradation of the multilayer capacitor.

[0056] In addition, the compound represented by Formula 1 can be sintered in an oxidizing atmosphere during the sintering process for manufacturing a capacitor, which eliminates the need to introduce reducing gas and reduces process costs.

[0057] In addition, the compound represented by Chemical Formula 1 has ionic conductivity that is equal to or even higher than that of conventional nickel (Ni). Therefore, unlike conventional nickel internal electrodes, the internal electrode according to the present invention does not require a separate additive for controlling sintering shrinkage, so that the internal electrode can be realized without a decrease in electrical conductivity, and excellent electrical conductivity can be achieved.

[0058] Accordingly, when analyzed by a Thermomechanical Analyzer (TMA), the compound may have a volume reduction rate of 5% or less at a temperature of 1100° C. compared to a temperature of 800° C.

[0059] The compound has an electrical conductivity of 1.05×10 6 S / m or more, more specifically, 1.5×10 6 S / m, 2.0×10 6 S / m, 2.5×10 6 S / m, 3.0×10 6 S / m, 3.5×10 6 S / m or more.

[0060] Specifically, in the formula 1, M1 may be Ti or V, M2 may be Al, Si or Sn, and M3 may be C. More specifically, the compound may be Ti3AlC2, Ti2AlC, V2AlC, Ti3SiC2 or Ti3SnC. 2- When the compound represented by Chemical Formula 1 is the same as this, the effect of suppressing high-temperature sintering shrinkage and the effect of improving ion conductivity described above are more preferably realized.

[0061] In addition, the compound represented by the above-mentioned Chemical Formula 1 has a BET specific surface area of ​​1.0 to 2.2 m 2 / g, more specifically, 1.2 to 2.1 m2 / g. If the BET specific surface area of ​​the compound represented by Chemical Formula 1 is too small, there are problems of an increase in the thickness of the internal electrode and a decrease in electrical conductivity. If the BET specific surface area of ​​the compound represented by Chemical Formula 1 is too large, there are problems of a decrease in connectivity and a decrease in density due to particle aggregation.

[0062] In this specification, the "BET specific surface area" can be measured using a BET (Surface area and Porosityan analyzer) method (Micromeritics, ASAP2020).

[0063] The average particle size (D50) of the compound represented by Chemical Formula 1 may be 400 to 700 nm. If the average particle size of the compound represented by Chemical Formula 1 is too small, a problem of particle aggregation may occur. If the average particle size of the compound represented by Chemical Formula 1 is too large, a problem of an increase in the thickness of the internal electrode may occur.

[0064] In this specification, the "average particle size (D50)" can be defined as the particle size corresponding to 50% of the cumulative volume in the particle size distribution curve of the particles. The average particle size (D50) can be measured, for example, by using a laser diffraction method. The laser diffraction method can generally measure particle sizes from the submicron range to several mm, and can obtain results with high reproducibility and high resolution.

[0065] On the other hand, the internal electrode does not have to contain nickel (Ni), that is, the internal electrode material according to the present invention can be used as a main internal electrode material, not as an additive or supplement to the conventional nickel-containing internal electrode.

[0066] Further, the internal electrode may not contain barium titanate (BaTiO3), silicon dioxide (SiO2), and tungsten (W). That is, the internal electrode according to the present invention may not contain another additive for controlling the high-temperature sintering shrinkage of nickel by using the compound of Chemical Formula 1 as the internal electrode material. Thereby, it is possible to prevent a decrease in electrical conductivity due to the use of an additive and to reduce the process cost.

[0067] On the other hand, the dielectric layer 111 may include a plurality of dielectric crystallites 1111.

[0068] The dielectric crystallites 1111 may include a main component and a sub-component.

[0069] The main component is Ba m TiO3 (0.995 ≦ m ≦ 1.010), (Ba 1-X Ca x ) m (Ti 1-y Zr y )O3 (0.995 ≦ m ≦ 1.010, 0 ≦ x ≦ 0.10, 0 < y ≦ 0.20), Ba m (Ti 1-x Zr x )O3 (0.995 ≦ m ≦ 1.010, x ≦ 0.10), (Ba 1-X Ca x ) m (Ti 1-y Sn y )O3 (0.995 ≦ m ≦ 1.010, 0 ≦ x ≦ 0.10, 0 < y ≦ 0.20), or a dielectric material including a combination thereof may be used.

[0070] The sub-component may include hafnium (Hf), manganese (Mn), chromium (Cr), silicon (Si), aluminum (Al), magnesium (Mg), tin (Sn), antimony (Sb), germanium (Ge), gallium (Ga), indium (In), or a combination thereof.

[0071] The secondary components may further include lanthanum (La), yttrium (Y), actinium (Ac), cerium (Ce), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), lutetium (Lu), or combinations thereof.

[0072] As an example, the average thickness of the dielectric layer 111 may be 0.5 μm to 10 μm.

[0073] Meanwhile, the first internal electrode 121 and the second internal electrode 122 are electrodes having different polarities, and are alternately arranged to face each other along the T-axis direction with the dielectric layer 111 therebetween, and one end can be exposed through the third and fourth surfaces of the capacitor body 110, respectively.

[0074] The first internal electrode 121 and the second internal electrode 122 can be electrically insulated from each other by a dielectric layer 111 disposed therebetween.

[0075] The ends of the first internal electrode 121 and the second internal electrode 122 alternately exposed through the third and fourth surfaces of the capacitor body 110 can be electrically connected to the first external electrode 131 and the second external electrode 132, respectively.

[0076] The first internal electrode 121 and the second internal electrode 122 may be formed using a conductive paste containing a conductive material. The conductive paste may be printed by screen printing or gravure printing.

[0077] As an example, the average thickness of the first internal electrode 121 and the second internal electrode 122 may be 0.1 μm to 2 μm.

[0078] The first external electrode 131 and the second external electrode 132 may be provided with voltages of different polarities and may be electrically connected to exposed portions of the first internal electrode 121 and the second internal electrode 122, respectively.

[0079] With the above-described configuration, when a predetermined voltage is applied to the first external electrode 131 and the second external electrode 132, charges are stored between the opposing first internal electrode 121 and second internal electrode 122. At this time, the capacitance of the multilayer capacitor 100 is proportional to the overlap area of ​​the first internal electrode 121 and the second internal electrode 122 that overlap each other along the T-axis direction in the active region.

[0080] The first external electrode 131 and the second external electrode 132 are arranged on the third and fourth surfaces of the capacitor body 110, respectively, and may include first and second connection portions connecting to the first internal electrode 121 and the second internal electrode 122, and first and second band portions arranged at the corners where the third and fourth surfaces of the capacitor body 110 meet with the first and second surfaces or the fifth and sixth surfaces.

[0081] The first and second band portions may extend from the first and second connection portions to parts of the first and second faces or the fifth and sixth faces of the capacitor body 110. The first and second band portions may serve to improve the bonding strength between the first external electrode 131 and the second external electrode 132.

[0082] As an example, the first external electrode 131 and the second external electrode 132 may each include a sintered metal layer in contact with the capacitor body 110, a conductive resin layer arranged to cover the sintered metal layer, and a plating layer arranged to cover the conductive resin layer.

[0083] The sintered metal layer can include a conductive metal and glass.

[0084] As an example, the sintered metal layer may include copper (Cu), nickel (Ni), silver (Ag), palladium (Pd), gold (Au), platinum (Pt), tin (Sn), tungsten (W), titanium (Ti), lead (Pb), alloys thereof, or combinations thereof, for example, copper (Cu) may include copper (Cu) alloys. When the conductive metal includes copper, the metal other than copper may include 5 molar parts or less per 100 molar parts of copper.

[0085] As an example, the sintered metal layer may include a composition in which an oxide is mixed with glass, and may be, for example, one or more selected from the group consisting of silicon oxide, boron oxide, aluminum oxide, transition metal oxide, alkali metal oxide, and alkaline earth metal oxide. The transition metal may be selected from the group consisting of zinc (Zn), titanium (Ti), copper (Cu), vanadium (V), manganese (Mn), iron (Fe), and nickel (Ni), the alkali metal may be selected from the group consisting of lithium (Li), sodium (Na), and potassium (K), and the alkaline earth metal may be one or more selected from the group consisting of magnesium (Mg), calcium (Ca), strontium (Sr), and barium (Ba).

[0086] The content of conductive metal and glass in the sintered metal layer is not particularly limited, but for example, the average area of ​​the conductive metal in cross sections (L-axis and T-axis cross sections) perpendicular to the thickness direction (W-axis direction) of the multilayer capacitor 100 may be 30% to 90%, or 70% to 90%, of the total area of ​​the sintered metal layer.

[0087] Alternatively, the conductive resin layer may be formed on the sintered metal layer, for example, to completely cover the sintered metal layer. Meanwhile, the first external electrode 131 and the second external electrode 132 may not include the sintered metal layer, in which case the conductive resin layer may be in direct contact with the capacitor body 110.

[0088] The conductive resin layer extends on the first and second surfaces or the fifth and sixth surfaces of the capacitor body 110, and the length of the region (i.e., band portion) where the conductive resin layer is disposed extending on the first and second surfaces or the fifth and sixth surfaces of the capacitor body 110 may be longer than the length of the region (i.e., band portion) where the sintered metal layer is disposed extending on the first and second surfaces or the fifth and sixth surfaces of the capacitor body 110. That is, the conductive resin layer may be formed on the sintered metal layer to completely cover the sintered metal layer.

[0089] The conductive resin layer includes a resin and a conductive metal.

[0090] The resin contained in the conductive resin layer is not particularly limited as long as it has adhesiveness and impact absorbency and can be mixed with the conductive metal powder to form a paste, and may include, for example, a phenolic resin, an acrylic resin, a silicone resin, an epoxy resin, or a polyimide resin.

[0091] The conductive metal contained in the conductive resin layer serves to electrically connect with the first internal electrode 121 and the second internal electrode 122 or the sintered metal layer.

[0092] The conductive metal contained in the conductive resin layer may have a spherical shape, a flake shape, or a combination thereof, i.e., the conductive metal may be only flake-shaped, only spherical, or a mixture of flake-shaped and spherical shapes.

[0093] Here, the spherical shape may include a shape that is not a perfect sphere, for example, a shape in which the ratio of the length of the major axis to the minor axis (major axis / minor axis) is 1.45 or less. The flake-type powder means a powder that is flat but has an elongated shape, and is not particularly limited, and may be, for example, a shape in which the ratio of the length of the major axis to the minor axis (major axis / minor axis) is 1.95 or more.

[0094] The first external electrode 131 and the second external electrode 132 may further include a plating layer disposed on the outer side of the conductive resin layer.

[0095] The plating layer may include nickel (Ni), copper (Cu), tin (Sn), palladium (Pd), platinum (Pt), gold (Au), silver (Ag), tungsten (W), titanium (Ti), lead (Pb), etc., alone or in alloys thereof. For example, the plating layer may be a nickel (Ni) plating layer or a tin (Sn) plating layer, and may be a form in which a nickel (Ni) plating layer and a tin (Sn) plating layer are sequentially laminated, or a form in which a tin (Sn) plating layer, a nickel (Ni) plating layer, and a tin (Sn) plating layer are sequentially laminated. The plating layer may also include a plurality of nickel (Ni) plating layers and / or a plurality of tin (Sn) plating layers.

[0096] The plating layer can improve the mountability of the multilayer capacitor 100 on a substrate, structural reliability, durability against the outside, heat resistance, and equivalent series resistance (ESR).

[0097] In still another embodiment of the present invention, a method for manufacturing a dielectric green sheet using a dielectric powder is provided. 2 forming a conductive paste layer containing a compound of 0.1 g / g; laminating the dielectric green sheets having the conductive paste layer formed thereon to form a dielectric green sheet laminate; firing the dielectric green sheet laminate in an oxidizing atmosphere to form a capacitor body including a dielectric layer and an internal electrode; and forming an external electrode on one surface of the capacitor body. [Chemical formula 1] M1 a+1 M2M3 a In the above Chemical Formula 1, M1 is Ti, V, Sc, Zr or Mo, M2 is Al, Si, Sn, Cd, In, Ga, Ge, Pb, As, S or P, M3 is C or N, and a is 1 to 3.

[0098] Hereinafter, a method for manufacturing a multilayer capacitor according to another embodiment of the present invention will be described in more detail.

[0099] First, the manufacture of the capacitor body will be described.

[0100] In the manufacturing process of the capacitor body, a dielectric paste that will become the dielectric layer after firing and a conductive paste that will become the internal electrode after firing are prepared.

[0101] The dielectric paste is produced, for example, by the following method: Dielectric powder is mixed uniformly by means of wet mixing or the like, dried, and then heat-treated under predetermined conditions to obtain a plastic powder. An organic vehicle or an aqueous vehicle is added to the obtained plastic powder and kneaded to prepare the dielectric paste.

[0102] The obtained dielectric paste is formed into a sheet by a technique such as a doctor blade method to obtain a dielectric green sheet. The dielectric paste may contain additives selected from various dispersants, plasticizers, dielectrics, subcomponent compounds, glass, etc., as necessary.

[0103] The conductive paste for the internal electrodes is prepared by kneading the compound represented by Chemical Formula 1, that is, the powder of the internal electrode material, with a binder and a solvent.

[0104] At this time, the conductive paste for the internal electrodes may not contain nickel (Ni), barium titanate (BaTiO3), silicon dioxide (SiO2) and tungsten (W). That is, since the multilayer capacitor according to the present invention uses the compound of Chemical Formula 1 as the internal electrode material, it does not contain nickel, which is a conventional internal electrode material, and does not need to contain a separate additive used to control the sintering shrinkage of nickel. This makes it possible to prevent a decrease in electrical conductivity due to the use of additives and reduce process costs.

[0105] A conductive paste for internal electrodes is applied in a predetermined pattern to the surface of a dielectric green sheet by various printing methods such as screen printing or transfer methods. Then, the dielectric green sheets on which the internal electrode patterns are formed are laminated in multiple layers, and pressed in the lamination direction to obtain a dielectric green sheet laminate. At this time, the dielectric green sheets and the internal electrode patterns can be laminated so that the dielectric green sheets are located on the upper and lower surfaces of the dielectric green sheet laminate in the lamination direction.

[0106] Optionally, the resulting dielectric green sheet laminate can be cut to a predetermined size by dicing or the like.

[0107] Furthermore, the dielectric green sheet laminate can be solidified and dried to remove plasticizers and the like as necessary, and after solidification and drying, can be barrel polished using a horizontal centrifugal barrel machine or the like. In barrel polishing, the dielectric green sheet laminate is placed in a barrel container together with media and a polishing liquid, and rotational motion, vibration, or the like is applied to the barrel container, thereby polishing away unnecessary parts such as burrs generated during cutting. After barrel polishing, the dielectric green sheet laminate can be washed with a cleaning liquid such as water and dried.

[0108] The dielectric green sheet laminate is subjected to binder removal and firing to obtain a capacitor body.

[0109] The conditions of the binder removal treatment can be appropriately adjusted according to the main component composition of the dielectric layer and the main component composition of the internal electrode. For example, the temperature rise rate during the binder removal treatment may be 5°C / hour to 300°C / hour, the support temperature may be 180°C to 400°C, and the temperature maintenance time may be 0.5 hours to 24 hours. The binder removal atmosphere may be air or a reducing atmosphere.

[0110] The firing conditions can be appropriately adjusted depending on the main component composition of the dielectric layer and the main component composition of the internal electrodes. For example, the firing temperature can be 1200°C to 1350°C or 1220°C to 1300°C, and the firing time can be 0.5 hours to 8 hours, or 1 hour to 3 hours.

[0111] In particular, the sintering atmosphere may be an oxidizing atmosphere. When nickel is used as the conventional internal electrode material, sintering is performed in a reducing atmosphere. For example, in the conventional case, the sintering atmosphere is a humidified mixture of nitrogen gas (N2) and hydrogen gas (H2) with an oxygen partial pressure of 1.0×10 -14 MPa~1.0×10 -10 The firing was performed in an atmosphere controlled at MPa. Meanwhile, the multilayer capacitor according to the present invention can be fired in an oxidizing atmosphere by using the compound of Formula 1 as the internal electrode material, which has the advantage of reducing process costs.

[0112] For example, the oxidizing atmosphere can be an air or oxygen (O2) atmosphere.

[0113] In addition, the firing can be performed by a hot press method. When the compound of Formula 1 is used as the internal electrode material, the firing can be performed by a hot press method to prevent gas release due to high temperature firing and prevent cracks in the internal electrode.

[0114] Optionally, the third and fourth faces of the obtained capacitor body may be subjected to a surface treatment such as sandblasting, laser irradiation, or barrel polishing. By carrying out such a surface treatment, the ends of the first and second internal electrodes may be exposed on the outermost surfaces of the third and fourth faces, which improves the electrical connection between the first and second external electrodes and the first and second internal electrodes, making it easier to form an alloy part.

[0115] A paste for forming a sintered metal layer is applied to the outer surface of the obtained capacitor body by using an external electrode, and then sintered to form a sintered metal layer.

[0116] The paste for forming the sintered metal layer may include a conductive metal and glass. The conductive metal and glass are the same as those described above, and therefore will not be described again. The paste for forming the sintered metal layer may optionally include a subcomponent such as a binder, a solvent, a dispersant, a plasticizer, or an oxide powder. For example, the binder may be ethyl cellulose, acrylic, or butyral, and the solvent may be an organic solvent such as terpineol, butyl carbitol, alcohol, methyl ethyl ketone, acetone, or toluene, or an aqueous solvent.

[0117] The method of applying the paste for forming the sintered metal layer to the outer surface of the capacitor body can be a dipping method, various printing methods such as screen printing, an application method using a dispenser, a spraying method using a spray, etc. The paste for the sintered metal layer is applied to at least the third and fourth surfaces of the capacitor body, and can also be applied selectively to a part of the first surface, the second surface, the fifth surface, or the sixth surface on which the band portions of the first external electrode and the second external electrode are formed.

[0118] Thereafter, the capacitor body on which the paste for forming a sintered metal layer has been applied is dried and sintered at a temperature of 700° C. to 1000° C. for 0.1 to 3 hours to form a sintered metal layer.

[0119] Alternatively, a conductive resin layer forming paste may be applied to the outer surface of the obtained capacitor body and then cured to form a conductive resin layer.

[0120] The paste for forming the conductive resin layer may include a resin, and optionally a conductive metal or a non-conductive filler. The conductive metal and the resin are the same as those described above, and therefore will not be described again. The paste for forming the conductive resin layer may optionally include a subcomponent such as a binder, a solvent, a dispersant, a plasticizer, or an oxide powder. For example, the binder may be ethyl cellulose, acrylic, or butyral, and the solvent may be an organic solvent such as terpineol, butyl carbitol, alcohol, methyl ethyl ketone, acetone, or toluene, or an aqueous solvent.

[0121] As an example, the conductive resin layer may be formed by dipping the capacitor body 110 into a paste for forming the conductive resin layer and then curing it, by printing the paste for forming the conductive resin layer on the surface of the capacitor body 110 using a screen printing method or a gravure printing method, or by applying the paste for forming the conductive resin layer on the surface of the capacitor body 110 and then curing it.

[0122] Next, a plating layer is formed on the outside of the conductive resin layer.

[0123] For example, the plating layer may be formed by a plating method, such as sputtering or electroplating.

[0124] Hereinafter, the present invention will be described in more detail with reference to the following examples, but the following examples are merely preferred embodiments of the present invention and the present invention is not limited to these examples.

[0125] Example 1: Ti3AlC2 internal electrode material preparation Ti3AlC2 powder was produced by solid-state method (ball milling).

[0126] Example 2: Ti2AlC inner electrode material fabrication Ti2AlC powder was produced by a solid-state method (ball milling).

[0127] Example 3: V2AlC internal electrode material fabrication V2AlC powder was produced by a solid-state method (ball milling).

[0128] Example 4: Ti3SiC2 internal electrode material preparation Ti3SiC2 powder was prepared by solid-state method (ball milling).

[0129] Example 5: Ti3SnC2 internal electrode material preparation Ti3SnC2 powder was prepared by a solid-state method (ball milling).

[0130] Comparative example 1: Ni internal electrode material prepared Nickel powder (Guangbo Company) was prepared.

[0131] Comparative Example 2 Mo2GaC powder was prepared by solid-state method (ball milling).

[0132] Comparative Example 3 Zr2TiC powder was produced by a solid-state method (ball milling).

[0133] Comparative Example 4 Cr2AlC powder was produced by solid-state method (ball milling).

[0134] Comparative Example 5 Ta4AlC3 powder was prepared by solid-state method (ball milling).

[0135] Comparative Example 6 Nb4AlC3 powder was produced by solid-state method (ball milling).

[0136] Comparative Example 7 Hf2InC powder was produced by a solid-state method (ball milling).

[0137] Experimental example 1: Internal electrode material BET specific surface area evaluation The specific surface area of ​​the internal electrode material powders manufactured according to the examples and comparative examples was measured using a BET (Surface area and Porosity analyzer) (Micromeritics, ASAP2020). The results are shown in Table 1.

[0138] Experimental example 2: Evaluation of high temperature firing shrinkage characteristics of internal electrode material The volume reduction rate of the internal electrode materials manufactured according to the examples and comparative examples was measured according to the heat treatment temperature in order to evaluate the shrinkage characteristics during high-temperature firing.

[0139] More specifically, the volume reduction rate at a temperature of 1100° C. compared to a temperature of 800° C. was measured using a Thermomechanical Analyzer (TMA). The results are shown in Table 1 and FIG.

[0140] Experimental example 3: Evaluation of electrical conductivity of internal electrode material The electrical conductivity of the internal electrode materials manufactured according to the examples and comparative examples was evaluated, and the results are shown in Table 1.

[0141] More specifically, the electrical conductivity was measured using a four point probe meter.

[0142] Experimental Example 4: Density Ratio Evaluation The density ratio of the internal electrode materials manufactured according to the examples and comparative examples was evaluated, and the results are shown in Table 1.

[0143] More specifically, the density ratio (experimental / theoretical, %) was measured using the Archimedes method.

[0144] [Table 1]

[0145] Referring to Table 1, it was confirmed that in Examples 1 to 5, in which the type of the internal electrode material compound was appropriately selected and the BET specific surface area was appropriately controlled, the volume reduction rate was small and the electrical conductivity was good. On the other hand, in the case of Comparative Example 1, it was confirmed that the electrical conductivity was good but the volume reduction rate was too large.

[0146] Also, in the case of Comparative Example 2, even if the type of the internal electrode material compound was appropriately selected, it was confirmed that the density was too low as a result of the BET specific surface area being too large.

[0147] In addition, in the case of Comparative Example 5, even if the type of the internal electrode material compound was appropriately selected, it was confirmed that the BET specific surface area was too small, resulting in low electrical conductivity.

[0148] Although the above describes a preferred embodiment of the present invention, the present invention is not limited thereto, and various modifications can be made within the scope of the claims, the detailed description of the invention, and the attached drawings, and it is natural that these also fall within the scope of the present invention.

[0149] Therefore, the true scope of the invention is defined by the appended claims and their equivalents. [Explanation of symbols]

[0150] 100 Stacked Capacitor 110 Capacitor Body 111 Dielectric layer 112, 113 Coverage area 121 1st internal electrode 122 Second internal electrode 131 First external electrode 132 Second external electrode

Claims

1. The compound includes a compound represented by the following chemical formula 1: The BET specific surface area of ​​the compound is 1.0 to 2.2 m 2 / g of an internal electrode material for a multilayer capacitor: [Chemical formula 1] M1 a+1 M2M3 a In Formula 1, M1 is Ti, V, Sc, Zr, or Mo, M2 is Al, Si, Sn, Cd, In, Ga, Ge, Pb, As, S, or P, M3 is C or N, and a is 1 to 3.

2. 2. The internal electrode material for a multilayer capacitor according to claim 1, wherein in Formula 1, M1 is Ti or V, M2 is Al, Si or Sn, and M3 is C.

3. The compound is Ti 3 AIC 2 , Ti 2 AlC, V 2 AlC, Ti 3 SiC 2 Or Ti 3 SnC 2 The internal electrode material for a multilayer capacitor according to claim 1 ,

4. 2. The internal electrode material for a multilayer capacitor according to claim 1, wherein the compound has an average particle size (D50) of 400 to 700 nm.

5. 2. The internal electrode material for a multilayer capacitor according to claim 1, wherein the compound has a volume reduction rate of 5% or less at a temperature of 1100° C. compared to a temperature of 800° C. when analyzed by a Thermomechanical Analyzer (TMA).

6. The compound has an electrical conductivity of 1.05×10 6 2. The internal electrode material for a multilayer capacitor according to claim 1, having a dielectric constant of at least 1.0 S / m.

7. a capacitor body including a dielectric layer and an internal electrode; and an external electrode disposed outside the capacitor body; The internal electrode includes a compound represented by the following Chemical Formula 1, and the BET specific surface area of ​​the compound is 1.0 to 2.2 m 2 / g, [Chemical formula 1] M1 a+1 M2M3 a In Formula 1, M1 is Ti, V, Sc, Zr, or Mo, M2 is Al, Si, Sn, Cd, In, Ga, Ge, Pb, As, S, or P, M3 is C or N, and a is 1 to 3.

8. 8. The multilayer capacitor according to claim 7, wherein in Formula 1, M1 is Ti or V, M2 is Al, Si or Sn, and M3 is C.

9. The compound is Ti 3 AIC 2 , Ti 2 AlC, V 2 AlC, Ti 3 SiC 2 Or Ti 3 SnC 2 8. The multilayer capacitor according to claim 7, wherein

10. 8. The multilayer capacitor according to claim 7, wherein the compound has an average particle size (D50) of 400 to 700 nm.

11. 8. The multilayer capacitor of claim 7, wherein the compound has a volume reduction rate of 5% or less at a temperature of 1100° C. compared to a temperature of 800° C. when analyzed by a Thermomechanical Analyzer (TMA).

12. The compound has an electrical conductivity of 1.05×10 6 8. The multilayer capacitor according to claim 7, wherein the capacitance is equal to or greater than S / m.

13. The internal electrodes are made of nickel (Ni), barium titanate (BaTiO 3 ), silicon dioxide (SiO 28. The stacked capacitor of claim 7, which is free of tungsten (W) and tungsten (H).

14. The dielectric layer includes a plurality of dielectric crystal grains, and the dielectric crystal grains are mainly composed of Ba. m TiO 3 (0.995≦m≦1.010) and further comprising hafnium (Hf), manganese (Mn), chromium (Cr), silicon (Si), aluminum (Al), magnesium (Mg), tin (Sn), antimony (Sb), germanium (Ge), gallium (Ga), indium (In), or a combination thereof, as a minor component. The stacked capacitor according to claim 7.

15. forming a dielectric green sheet using the dielectric powder; The dielectric green sheet has a surface having a BET specific surface area of ​​1.0 to 2.2 m2 and is represented by the following formula 1: 2 forming a conductive paste layer containing 0.1 g of a compound; laminating the dielectric green sheets having the conductive paste layers formed thereon to form a dielectric green sheet laminate; Firing the dielectric green sheet laminate in an oxidizing atmosphere to form a capacitor body including dielectric layers and internal electrodes; and forming an external electrode on one surface of the capacitor body; [Chemical formula 1] M1 a+1 M2M3 a In Formula 1, M1 is Ti, V, Sc, Zr, or Mo, M2 is Al, Si, Sn, Cd, In, Ga, Ge, Pb, As, S, or P, M3 is C or N, and a is 1 to 3.

16. The oxidizing atmosphere is air or oxygen (O 2 16. The method for producing a multilayer capacitor according to claim 15, wherein the atmosphere is 1000.degree.

17. The method of claim 15, wherein the sintering is performed by a hot press method.

18. The conductive paste layer is made of nickel (Ni), barium titanate (BaTiO 3 ), silicon dioxide (SiO 2 16. The method for producing a multilayer capacitor according to claim 15, wherein the method does not include any of the following: