Manufacturing method of lithium metal complex oxide

The method stabilizes lithium metal composite oxide production by using low dew point gas and countercurrent oxygen flow to prevent condensation, ensuring continuous raw material supply and stable output.

JP2024153278APending Publication Date: 2024-10-29SUMITOMO CHEM CO LTD

Patent Information

Application Number
JP2023067067
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Fluidized firing furnaces face challenges in stably producing lithium metal composite oxide due to condensation issues that lead to blockages during the production process.

Method used

A method involving a firing device with a low dew point gas supply from the upstream side of the heating means, countercurrent oxygen-containing gas flow, and controlled gas ratios to prevent condensation and ensure stable production of lithium metal composite oxide.

Benefits of technology

Stable production of lithium metal composite oxide is achieved by minimizing condensation-related blockages, allowing continuous and efficient raw material supply.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153278000001
    Figure 2024153278000001
Patent Text Reader

Abstract

To provide a manufacturing method of a lithium metal complex oxide capable of stable raw material supply.SOLUTION: A manufacturing method of a lithium metal complex oxide includes a step of firing a processed object by using a firing apparatus to obtain a fired material. The firing apparatus includes: an input part where the processed object is input; a transportation part for transporting the processed object having been input from the input part; a cylindrical kiln main body; an exhaust port for exhausting the fired material; and gas supply means. In the step, a low dew point gas having a dew point of 10°C or under is supplied from an upstream than heating means, an oxygen-containing gas is supplied from a downstream side than the heating means, and a value represented by the following formula (A) is 0.0001 Nm3 / kg or over and 0.30 Nm3 / kg or under. Formula(A): a supply amount of the low dew point gas (Nm3 / time) / a supply amount of the processed object (kg / time)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a lithium metal composite oxide. [Background technology]

[0002] A method for producing a lithium metal composite oxide used as a positive electrode active material for a lithium secondary battery includes a step of mixing a metal composite compound precursor and a lithium compound, and calcining the mixture obtained. Such a calcination step is carried out using a continuous calcination furnace such as a tunnel furnace or a roller hearth kiln, or a fluidized calcination furnace such as a rotary kiln.

[0003] For the purpose of accelerating the firing reaction, Patent Document 1 discloses a method for producing a positive electrode active material using a firing furnace equipped with two air supply systems. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP-A-2019-75253 Summary of the Invention [Problem to be solved by the invention]

[0005] A fluidized bed sintering furnace has the problem that it is difficult to stably produce lithium metal composite oxide.

[0006] An object of the present invention is to provide a method for producing a lithium metal composite oxide that allows stable production. [Means for solving the problem]

[0007] The present invention encompasses the following [1] to [7]. [1] A method for producing a lithium metal composite oxide, comprising a step of calcining a material to be treated using a calcination device to obtain a calcined material, the material to be treated comprising a mixture of a metal composite compound and a lithium compound, the calcination device comprising an input section into which the material to be treated is input, a transport section for transporting the material to be treated input from the input section, a cylindrical kiln body, an outlet for discharging the calcined material, and a gas supply means, the kiln body comprising a heating means, in the step, a low dew point gas having a dew point of 10°C or less is supplied from the upstream side of the heating means, an oxygen-containing gas is supplied from the downstream side of the heating means, the material to be treated is calcined by countercurrent contact with the oxygen-containing gas, and a value represented by the following formula (A) is 0.0001 Nm 3 / kg or more 0.30Nm 3 / kg or less. Formula (A): Supply amount of low dew point gas (Nm 3 / hour) / supply amount of material to be treated (kg / hour) [2] The method for producing a lithium metal composite oxide according to [1], wherein the calcination apparatus is a rotary kiln. [3] The method for producing a lithium metal composite oxide according to [1] or [2], wherein the proportion of Li contained in the lithium compound is 5 mass % or more and 50 mass % or less. [4] The method for producing a lithium metal composite oxide according to [3], wherein the proportion of Li is 5 mass % or more and 30 mass % or less. [5] The value represented by the following formula (C) is 0.3 Nm 3 / kg or more 1Nm 3 The method for producing a lithium metal composite oxide according to any one of [1] to [4], wherein the amount of the lithium metal composite oxide is 1 / kg or less. Formula (C): Supply amount of oxygen-containing gas (Nm 3 / hour) / supply amount of material to be treated (kg / hour) [6] The method for producing a lithium metal composite oxide according to any one of [1] to [5], wherein the calcination apparatus has an exhaust port upstream of the heating means, and in the step, calcination is performed while exhausting the oxygen-containing gas in the calcination apparatus from the exhaust port. [7] The method for producing a lithium metal composite oxide according to any one of [1] to [6], wherein the lithium metal composite oxide satisfies the following compositional formula (I). Li[Li a (Ni (1-x-y) Co x M1 y ) 1-a O2 ··· Compositional formula (I) (In the compositional formula (I), M1 is at least one element selected from the group consisting of Mn, Fe, Cu, Ti, Mg, Ca, Al, Zn, Sn, Zr, W, Nb, B, Si, S, and P, and the compositional formula (I) satisfies -0.1 ≦ a ≦ 0.2, 0 ≦ x ≦ 0.7, 0 < y ≦ 0.7, and x + y < 1.)

Advantages of the Invention

[0008] According to the present invention, a method for producing a lithium metal composite oxide capable of stable production can be provided.

Brief Description of the Drawings

[0009] [Figure 1] It is a schematic cross-sectional view of a firing apparatus used in the method for producing a lithium metal composite oxide in one aspect of the present embodiment.

Embodiments for Carrying Out the Invention

[0010] In the present specification, a metal composite compound is hereinafter referred to as "MCC", a lithium metal composite oxide is hereinafter referred to as "LiMO", and a cathode active material for lithium secondary batteries is hereinafter referred to as "CAM".

[0011] "Ni" refers not to nickel metal but to nickel atoms. Similarly, "Co", "Li", etc. refer to cobalt atoms, lithium atoms, etc., respectively.

[0012] When a numerical range is described, for example, as "1-10 μm" or "1~10 μm", it means a range from 1 μm to 10 μm, that is, a numerical range including the lower limit value of 1 μm and the upper limit value of 10 μm.

[0013] <Method for manufacturing LiMO> This embodiment is a method for manufacturing LiMO, which includes a step of firing an object to be processed using a firing device to obtain a fired product (hereinafter sometimes referred to as step A). The firing device includes a charging section into which the object to be processed is charged, a conveying section for conveying the object to be processed charged from the charging section, a cylindrical kiln body, a discharge port for discharging the fired product, and a gas supply means. The kiln body includes a heating means. In step A, a low dew point gas with a dew point of 10°C or less is supplied from upstream of the heating means. Thereby, the water vapor staying near the supply section of the object to be processed can be dehumidified and dried. As a result, the generation of condensed water is less likely to occur, blockage near the supply section can be avoided, and stable production of LiMO becomes possible. Here, "upstream of the heating means" means the side of the charging section with respect to the heating means. For example, a low dew point gas can be supplied from a low dew point gas supply section 56 described later. The firing device used in the method for manufacturing LiMO will be described with reference to FIG. 1.

[0014] ≪Overall configuration≫ FIG. 1 is a schematic cross-sectional view of a firing device used in the method for manufacturing LiMO according to this embodiment. The firing device 50 shown in FIG. 1 includes a charging section 51, a conveying section 58, a kiln body 52, a discharge port 53, and a gas supply means 60. The conveying section 58 includes a conveying mechanism 581 and an electric motor 582.

[0015] The object to be processed is charged at the charging section 51 and supplied to the conveying section 58, and then is conveyed into the kiln body 52 by the conveying mechanism 581 of the conveying section 58. The conveying section 58 is, for example, a screw feeder. The conveying mechanism 581 is, for example, a conveying screw.

[0016] The kiln body 52 is a facility for burning the material to be treated. The material to be treated that is transported to the kiln body 52 is burned, and the obtained burned material is discharged from the discharge port 53.

[0017] As described above, the material to be treated is moved through the feeding section 51, the conveying section 58, and the kiln main body 52 toward the discharge outlet 53, where it is heated inside the kiln main body 52, and finally discharged from the discharge outlet 53.

[0018] The kiln body 52 is tubular, specifically cylindrical, and can rotate about an axis O. The kiln body 52 is equipped with a heating means 54. The material to be treated supplied to the inside of the kiln body 52 is fired by the heating means 54.

[0019] The calcination device 50 includes a gas supply means 60. The gas supply means 60 includes an oxygen-containing gas supply section 601 that supplies an oxygen-containing gas to the inside of the kiln body 52 from the downstream side of the heating means 54. "Downstream side of the heating means 54" means the discharge port 53 side of the heating means 54.

[0020] In order to make the oxygen-containing gas flow in the kiln body 52 in the opposite direction to the movement of the material to be treated, the calcination device 50 is provided with an exhaust port 55 upstream of the heating means 54, and in the step A, it is preferable to perform calcination while exhausting the oxygen-containing gas in the calcination device 50 from the exhaust port 55 (EG1 in Figure 1).

[0021] When the material to be treated is calcined inside the kiln body 52, moisture may be generated by a reaction that occurs during the calcination. Examples of reactions that generate moisture include the dehydration reaction of lithium hydroxide or MCC, and the desorption reaction of water molecules when a lithium compound reacts with MCC. The generated moisture becomes water vapor and rides on the countercurrent gas, flowing in the direction of the conveying section 58. The water vapor that reaches the upstream side of the heating means 54 condenses due to a drop in temperature.

[0022] When the condensed water produced by condensation comes into contact with the raw material supplied to the transport section 58, a lump of raw material is formed, causing blockage of the transport section 58. This blocks the supply of the subsequent raw material, which makes it difficult to stably produce LiMO. One way to solve this problem is to increase the rotation speed of the motor 582 of the conveying section 58 to keep the speed at which the raw material is supplied constant, but this makes it difficult to resolve the blockage when long-term operation is assumed.

[0023] In this embodiment, the low dew point gas is supplied to a position where condensation is likely to occur, i.e., upstream of the heating means 54, so that the water vapor remaining near the supply part of the material to be treated can be dehumidified and dried. As a result, clogging of the transport part 58 can be avoided, the raw material can be stably supplied, and LiMO can be stably produced.

[0024] Specifically, the gas supply means 60 includes a low dew point gas supply line 602 for supplying a low dew point gas, in addition to an oxygen-containing gas supply unit 601 . The supply amounts of the oxygen-containing gas and the low dew point gas are controlled by the control unit 61.

[0025] Here, the "low dew point gas" refers to a gas having a dew point of 10°C or less, specifically oxygen, nitrogen, air, and a mixed gas of two or more of the above three types having a dew point of 10°C or less. Moreover, the "oxygen-containing gas" is a gas that contains oxygen, and examples of such gas include oxygen and a mixed gas of oxygen and nitrogen.

[0026] The dew point of the low dew point gas is preferably not more than −10° C., and more preferably not more than −20° C. By using a low dew point gas having a dew point in the above range, LiMO can be produced more stably.

[0027] The low dew point gas is supplied to low dew point gas supply unit 56. In FIG. 1, low dew point gas supply unit 56 is installed above electric motor 582. However, the present invention is not limited to this as long as the low dew point gas supply unit 56 is located upstream of heating means 54. For example, the low dew point gas supply unit 56 may be installed in the circumferential direction upstream of heating means 54 of kiln body 52, or may be installed at the center of conveying mechanism 581. In addition, low dew point gas supply units may be installed in two or more locations.

[0028] As the calcination device, a rotary kiln, which is a fluidized calcination furnace, is preferred. In a rotary kiln, the kiln body rotates while sliding on the fixed part of the kiln body. Since gaps are likely to occur in the sliding part, a seal gas supply part is typically provided mainly for the purpose of sealing the sliding part. The seal gas supply part is installed near the sliding part, and is typically installed on either the upstream side or the downstream side or both of the heating means of the kiln body.

[0029] Since the rotary kiln is equipped with a seal gas supply unit as standard as described above, the manufacturing method of this embodiment can be carried out by simply changing the seal gas to a low dew point gas without modifying the calcination apparatus.

[0030] As the calcination device, in addition to a rotary kiln, a rocking type cylindrical furnace provided with a supply section and supply means for a low dew point gas can be used.

[0031] In addition, since a gas generally used as a seal gas has a dew point exceeding 10° C., the low dew point gas introduced in this embodiment is a gas different from the seal gas.

[0032] By using the seal gas supply unit installed upstream of the heating means of the kiln body as the low dew point gas supply unit, it is possible to supply low dew point gas from the upstream side of the heating means.

[0033] Next, the above-mentioned step A using the above-mentioned baking apparatus 50 will be described.

[0034] While the kiln body 52 is rotated, the material to be treated is supplied from the input section 51. In the calcination device 50, the material to be treated is moved from the feeding section 51 toward the kiln body 52 by the conveying section 58 while continuously calcining the material to be treated. In step A, a low dew point gas is supplied from the upstream side of the heating means 54, and an oxygen-containing gas is supplied from the downstream side of the heating means 54.

[0035] In step A, the value represented by the following formula (A) is 0.0001-0.30 Nm 3 / kg. Formula (A): Supply amount of low dew point gas (Nm 3 / hour) / supply amount of material to be treated (kg / hour)

[0036] The value expressed by formula (A) is 0.06-0.25Nm 3 / kg is preferred, 0.065-0.22Nm 3 / kg is more preferred.

[0037] When the value represented by formula (A) is equal to or greater than the above lower limit, a sufficient amount of low dew point gas is supplied to dehumidify and dry the water vapor that reaches the vicinity of the supply part of the workpiece, so that condensation is less likely to occur near the supply part of the workpiece and the raw material can be supplied stably.

[0038] When the value represented by formula (A) is equal to or less than the upper limit, the supply of oxygen-containing gas from the oxygen-containing gas supply unit 601 is unlikely to become excessive, and the heating energy of the heating means 54 is unlikely to increase.

[0039] In step A, the material to be treated is calcined by countercurrently contacting an oxygen-containing gas with the material to be treated. The supply amount of the oxygen-containing gas preferably satisfies the following formula (X). Formula (X): Supply amount of low dew point gas (Nm 3 / hour) < Oxygen-containing gas supply (Nm 3 / time)

[0040] By performing firing while exhausting the oxygen-containing gas in the firing device 50 from the exhaust port 55, firing can be performed under conditions in which the oxygen-containing gas flows in the opposite direction to the movement of the material to be treated in the kiln body 52. Under the condition that formula (X) is satisfied, the gas containing water vapor can be exhausted from the inside of the calcination device 50 including the transport part 58 to the exhaust port 55 in a short time (EG1 in FIG. 1). This shortens the time that the gas containing water vapor remains inside the calcination device 50, and water vapor is less likely to remain near the supply part of the material to be treated. As a result, clogging of the transport section 58 is avoided, so that the raw material is supplied stably, and LiMO can be produced stably.

[0041] In step A, the value represented by the following formula (C) is 0.3-1 Nm 3 It is preferable to calcinate the material to be treated while supplying an oxygen-containing gas into the kiln body 52 so that the calcination temperature becomes 100° C. / kg. Formula (C): Supply amount of oxygen-containing gas (Nm 3 / hour) / supply amount of material to be treated (kg / hour)

[0042] The value represented by the above formula (C) is 0.4-1Nm 3 / kg, preferably 0.5-1Nm 3 / kg is more preferred.

[0043] When the value represented by formula (C) is equal to or greater than the above lower limit, the dew point of the oxygen-containing gas in the kiln body 52 increases, making it difficult for condensation to occur. When the value represented by formula (C) is equal to or less than the upper limit, an increase in the supply amount of the oxygen-containing gas to be heated and an increase in heating energy can be suppressed.

[0044] In step A, the supply amount of oxygen-containing gas is 0.5 Nm 3 It is preferable that the time is 1 hour or more. When the supply amount of the oxygen-containing gas is equal to or greater than the lower limit, the reaction between the object to be treated and the oxygen-containing gas can be sufficiently enhanced. The upper limit of the supply amount of the oxygen-containing gas is, for example, 2 Nm 3 / hour. The supply rate of oxygen-containing gas is 0.5-2Nm 3 / hours is more preferable.

[0045] The firing temperature of the workpiece is, for example, 650-900°C, preferably 660-850°C, and more preferably 670-800°C. When the firing temperature is 650°C or higher, the growth of LiMO particles is promoted, and LiMO having a strong crystal structure can be obtained. When the heating temperature is 900°C or lower, cracks are prevented from being formed in the particles in LiMO, the strength of LiMO can be maintained, and the volatilization of lithium ions on the particle surfaces contained in LiMO can be reduced.

[0046] The firing temperature in this specification means the maximum temperature of the atmosphere inside the kiln body 52.

[0047] The retention time in the firing step is preferably 1 to 50 hours. When the retention time in the firing step is 1 hour or more, the crystals develop well. When the retention time in the firing step is 50 hours or less, the volatilization of lithium ions is unlikely to occur.

[0048] In this specification, the retention time in firing is defined as the time from when the workpiece reaches the area where the heating means 54 is provided until when it reaches the end of the area where the heating means 54 is provided.

[0049] The inner diameter of the kiln body 52 is preferably 0.05-10 m, more preferably 0.07-5 m, and even more preferably 0.09-2 m.

[0050] The filling rate of the material to be treated in the kiln body 52 is preferably 1 to 20%, more preferably 2 to 17%, and further preferably 3 to 15%.

[0051] The rotation speed of the kiln body 52 in the step A is preferably 0.003-0.5 rad / sec, more preferably 0.05-0.4 rad / sec, and further preferably 0.08-0.3 rad / sec.

[0052] (Item to be processed) The material to be treated includes a mixture of MCC and a lithium compound. The mixture of MCC and a lithium compound is a mixture of MCC and a lithium compound without calcination. The treated object may contain other materials as long as it mainly contains the mixture. For example, in addition to the mixture, it may contain a reaction product of MCC and a lithium compound. The reaction product of MCC and a lithium compound is a material obtained by calcining MCC and a lithium compound.

[0053] MCC is a compound that can produce LiMO by calcining with a lithium compound. MCC is, for example, a metal composite oxide or a metal composite hydroxide.

[0054] The proportion of Li contained in the lithium compound is preferably from 5 to 50 mass %, more preferably from 5 to 30 mass %, further preferably from 10 to 25 mass %, and particularly preferably from 15 to 20 mass %.

[0055] Specifically, the lithium compound may be at least one of lithium carbonate (Li ratio is 19% by mass), lithium nitrate (Li ratio is 5-10% by mass), lithium acetate (Li ratio is 7-11% by mass), lithium hydroxide (Li ratio is 16-30% by mass), lithium oxide (Li ratio is 46% by mass), lithium chloride (Li ratio is 16% by mass), and lithium fluoride (Li ratio is 27% by mass). Among these, lithium hydroxide (Li ratio is 16-30% by mass) is preferred because of its high reactivity with MCC.

[0056] Lithium hydroxide is prone to generating water vapor during firing, but the LiMO production method described above allows for stable production of LiMO even when lithium hydroxide is used as the lithium compound.

[0057] The mixture of MCC and lithium compounds contains a lot of water attached and crystalline water, so water vapor is easily generated. However, the LiMO production method described above can stably produce LiMO even when using a mixture of MCC and lithium compounds.

[0058] The composition analysis of the lithium compound can be carried out, for example, by dissolving the lithium compound in hydrochloric acid and then using an ICP emission spectrometer (Optima 7300, manufactured by PerkinElmer Co., Ltd.).

[0059] The MCC preferably contains Ni and an element M1, and more preferably contains Ni, Co and an element M1. The element M1 represents one or more elements selected from the group consisting of Mn, Fe, Cu, Ti, Mg, Ca, Al, Zn, Sn, Zr, W, Nb, B, Si, S and P.

[0060] MCC is, for example, a metal composite hydroxide or metal composite oxide containing Ni, Co, and Al.

[0061] When MCC is a metal composite hydroxide, the metal composite hydroxide can be produced, for example, by the continuous coprecipitation method described in JP-A-2002-201028. For example, the metal composite hydroxide can be produced by the following procedure. First, at a temperature of 20-80°C in a reaction tank, an alkaline aqueous solution is added to a mixed solution containing a metal salt solution and a complexing agent so that the pH is in the range of 9-13. Next, the resulting reaction precipitate is washed, dehydrated, and dried to obtain a metal composite hydroxide. Examples of the metal salt solution include an aqueous nickel sulfate solution, an aqueous cobalt sulfate solution, and an aqueous aluminum sulfate solution, and examples of the complexing agent include ammonium sulfate. Examples of the alkaline aqueous solution that can be used include an aqueous sodium hydroxide solution, an aqueous potassium hydroxide solution, and the like.

[0062] When the MCC is a metal composite oxide, the metal composite oxide can be produced by heating the metal composite hydroxide at 300-700°C.

[0063] The lithium compound and MCC are mixed in consideration of the composition ratio of the final target product to produce a mixture. Specifically, the amount (molar ratio) of Li relative to the total amount of metal elements contained in MCC is preferably 0.98 or more, more preferably 1.04 or more, and even more preferably 1.05 or more. The amount of Li is preferably 1.20 or less. The amount of Li is preferably 0.98-1.20, more preferably 1.04-1.20, and even more preferably 1.05-1.20.

[0064] After the step A, a main firing may be performed. In this case, the fired product obtained by the step A is called a pre-fired product. The pre-fired product is fired to obtain a main fired product. The firing apparatus used for the main firing is not particularly limited, and may be, for example, a continuous stationary firing furnace or a fluidized firing furnace. As the fluidized firing furnace, a firing apparatus 50 may be used. The temperature and time during the main firing may be, for example, 650-950°C and 3-50 hours.

[0065] The fired product may be washed, dehydrated, and dried as necessary. LiMO is obtained through the above steps.

[0066] [Method for measuring the coefficient of variation of the impeller frequency] Whether or not a LiMO manufacturing method enables stable production is evaluated by measuring the coefficient of variation of the stirring blade frequency. In the calcination device 50, the stirring blades are rotated by an electric motor 582, and the material to be treated input from the input section 51 is transported.

[0067] If the desired raw material supply rate (kg / h) can be maintained without changing or barely changing the impeller frequency, stable production is possible. When the frequency is adjusted during operation to maintain the desired raw material supply rate (kg / h), the degree of frequency fluctuation is calculated as the "impeller frequency variation coefficient."

[0068] Specifically, the coefficient of variation of the stirring blade frequency is calculated by the following formula. Coefficient of variation of impeller frequency = standard deviation of impeller frequency of conveyor mechanism 581 / average impeller frequency of conveyor mechanism 581

[0069] In calculating the coefficient of variation of the agitator blade frequency, the standard deviation of the frequency after the material to be treated has been retained inside the kiln body 52 is used.

[0070] If the value of the above-mentioned coefficient of variation of the stirring blade frequency is large, it means that the frequency is adjusted each time during operation in order to maintain the desired raw material supply rate (kg / h), which means that production is unstable. In this embodiment, when the value of the coefficient of variation of the stirring blade frequency is 0.035 or less, the risk of clogging during long-term operation is unlikely to occur, and it is evaluated as being "possible for stable production."

[0071] <limo> The above LiMO has the following properties.

[0072] LiMO preferably contains Li, Ni and the element M1, and more preferably contains Li, Ni, Co and the element M1. LiMO is represented by, for example, the composition formula (I). Li[Li a (Ni (1-x-y) Co x M1 y ) 1-a O2 ··· Composition formula (I) (In the composition formula (I), M1 is the element M1, and the composition formula (I) satisfies -0.1 ≦ a ≦ 0.2, 0 ≦ x ≦ 0.7, 0 < y ≦ 0.7, and x + y < 1.)

[0073] From the viewpoint of obtaining a lithium secondary battery with a high cycle retention rate, a in the formula (I) is more preferably -0.05 or more, and even more preferably -0.01 or more. Also, from the viewpoint of obtaining a lithium secondary battery with a higher initial coulombic efficiency, a is preferably 0.08 or less, and more preferably 0.05 or less.

[0074] The upper and lower limit values of a can be arbitrarily combined. a is preferably -0.01 to 0.2, more preferably -0.05 to 0.08, and even more preferably -0.01 to 0.05.

[0075] From the viewpoint of improving cycle characteristics, x is preferably 0.01 or more, and more preferably 0.02 or more. From the viewpoint of obtaining a lithium secondary battery with a high charge capacity, x is preferably 0.5 or less, and more preferably 0.3 or less.

[0076] The upper and lower limit values of x can be arbitrarily combined. x is preferably 0.01 to 0.5, and more preferably 0.02 to 0.3.

[0077] From the viewpoint of improving cycle characteristics, y is preferably 0.01 or more, and more preferably 0.02 or more, and from the viewpoint of obtaining a lithium secondary battery with a high charging capacity, y is preferably 0.5 or less, and more preferably 0.3 or less.

[0078] The upper and lower limit values ​​of y can be arbitrarily combined. y is preferably 0.01 to 0.5, and more preferably 0.02 to 0.3.

[0079] x+y is greater than 0 and less than 1, preferably greater than 0 and not greater than 0.7, more preferably greater than 0 and not greater than 0.3, and even more preferably greater than 0 and not greater than 0.25.

[0080] From the viewpoint of obtaining a lithium secondary battery with a high cycle retention rate, M1 is preferably one or more elements selected from the group consisting of Mn, Ti, Mg, Al, W, Nb, B, and Zr, and more preferably one or more elements selected from the group consisting of Mn, Al, W, B, and Zr.

[0081] The composition analysis of LiMO can be carried out, for example, by dissolving LiMO in hydrochloric acid and then using an ICP emission spectrometer (Optima 7300, manufactured by PerkinElmer Co., Ltd.).

[0082] The crystal structure of LiMO is a layered structure, and is more preferably a hexagonal crystal structure or a monoclinic crystal structure.

[0083] The hexagonal crystal structure is P3, P31, P32, R3, P-3, R-3, P312, P321, P3112, P3121, P3212, P3221, R32, P3m1, P 31m, P3c1, P31c, R3m, R3c, P-31m, P-31c, P-3m1, P-3c1, R-3m, R-3c, P6, P61, P65, P62, P64, P63 , P-6, P6 / m, P63 / m, P622, P6122, P6522, P6222, P6422, P6322, P6mm, P6cc, P63cm, P63mc, P-6m2, P-6c2, P-62m, P-62c, P6 / mmm, P6 / mcc, P63 / mcm, and P63 / mmc.

[0084] In addition, the monoclinic crystal structure belongs to any one space group selected from the group consisting of P2, P21, C2, Pm, Pc, Cm, Cc, P2 / m, P21 / m, C2 / m, P2 / c, P21 / c, and C2 / c.

[0085] Among these, in order to obtain a lithium secondary battery with a high discharge capacity, the crystal structure is more preferably a hexagonal crystal structure belonging to the space group R-3m or a monoclinic crystal structure belonging to the space group C2 / m.

[0086] <cam> The LiMO can be suitably used as a CAM.

[0087] <Lithium secondary battery> An example of a suitable lithium secondary battery when LiMO is used as the CAM has a positive electrode, a negative electrode, a separator sandwiched between the positive electrode and the negative electrode, and an electrolyte solution disposed between the positive electrode and the negative electrode.

[0088] Further, an example of a lithium secondary battery has a positive electrode, a negative electrode, a separator sandwiched between the positive electrode and the negative electrode, and a solid electrolyte disposed between the positive electrode and the negative electrode. For the lithium secondary battery, the configuration, materials, and manufacturing method described in

[0104] to

[0181] of WO2022 / 113904A1 can be used.

[0089] The present invention may be the following

[10] to

[16] .

[10] A method for producing LiMO comprising the step A, wherein the material to be treated contains a mixture of MCC and a lithium compound, the calcination device comprises the charging section, the conveying section, a cylindrical kiln body, the discharge port, and the gas supplying means, and the kiln body comprises a heating means, and in the step A, a low dew point gas having a dew point of 10°C or less is supplied from the upstream side of the heating means, and an oxygen-containing gas is supplied from the downstream side of the heating means, and the material to be treated is calcined by countercurrent contact with the oxygen-containing gas, and the value represented by the formula (A) is 0.065-0.22 Nm 3 / kg,

[11] The method for producing LiMO described in

[10] , wherein the calcining apparatus is a rotary kiln.

[12] The method for producing LiMO according to

[10] or

[11] , wherein the proportion of Li contained in the lithium compound is 15 to 20 mass %.

[13] The value represented by the formula (C) is 0.3-1 Nm 3 The method for producing LiMO according to any one of

[10] to

[12] , wherein the LiMO content is 1 / kg.

[14] The method for producing LiMO according to any one of

[10] to

[13] , wherein the supply amount of the oxygen-containing gas satisfies the formula (X).

[15] The firing apparatus is provided with an exhaust port on the upstream side of the heating means, and in the step A, firing is performed while exhausting the oxygen-containing gas in the firing apparatus from the exhaust port, the method for producing LiMO according to any one of

[10] to

[14] .

[16] The LiMO satisfies the following compositional formula (I)-1, the method for producing LiMO according to any one of

[10] to

[16] . Li[Li a (Ni (1-x-y) Co x M1 y ) 1-a O2 ··· Compositional formula (I)-1 (In the compositional formula (I)-1, M1 is at least one element selected from the group consisting of Mn, Al, W, Zr, and B, and the compositional formula (I)-1 satisfies the relationships shown by -0.01 ≦ a ≦ 0.5, 0.02 ≦ x ≦ 0.3, 0.02 ≦ y ≦ 0.3, and 0 < x + y ≦ 0.7.)

Example

[0090] Next, the present invention will be described in more detail with reference to examples.

[0091] <Composition analysis> The composition analysis of LiMO and the lithium compound was performed using an ICP emission spectroscopic analyzer (Optima 7300, manufactured by PerkinElmer Co., Ltd.) after dissolving LiMO or the lithium compound in hydrochloric acid. <Coefficient of variation of stirring blade frequency> The coefficient of variation was measured according to the method described in the above [Method for measuring the coefficient of variation of stirring blade frequency].

[0092] ≪Example 1≫ After putting water into a reaction tank equipped with a stirrer and an overflow pipe, an aqueous sodium hydroxide solution was added, and the liquid temperature was maintained at 50°C.

[0093] An aqueous nickel sulfate solution, an aqueous cobalt sulfate solution, and an aqueous aluminum sulfate solution were mixed at a ratio such that the atomic ratio of Ni, Co, and Al was 0.88:0.09:0.03 to prepare a mixed raw material liquid.

[0094] Next, in the reaction vessel, an aqueous solution of ammonium sulfate was continuously added as a complexing agent to the mixed raw material solution under stirring. An aqueous solution of sodium hydroxide was added dropwise at appropriate times so that the pH of the mixed solution in the reaction vessel became 11.6 (measurement temperature: 40°C), and reaction precipitate 1 was obtained.

[0095] The reaction precipitate 1 was washed, dehydrated using a centrifuge, isolated, and dried at 105° C. to obtain a metal composite hydroxide 1 containing Ni, Co, and Al.

[0096] Metal composite hydroxide 1 was heated at 650° C. for 5 hours in an air atmosphere and then cooled to room temperature to obtain a metal composite oxide, MCC1.

[0097] Lithium hydroxide was weighed out so that the amount (molar ratio) of Li relative to the total amount of Ni, Co, and Al contained in MCC1 was 1.10. MCC1 and lithium hydroxide were mixed in a mortar to obtain mixture 1.

[0098] The proportion of Li contained in the lithium hydroxide used was 16.5 mass %.

[0099] This mixture 1 was placed in a fluidized-bed calcination furnace (manufactured by Noritake Company Limited, product name: desktop rotary kiln) corresponding to the calcination device 50. An oxygen-containing gas was supplied from the exhaust port side under conditions satisfying the relationship of formula (X), and while exhausting from an exhaust port corresponding to exhaust port 55, the oxygen-containing gas was brought into countercurrent contact with the mixture 1, and calcined at 680°C for 2 hours to obtain a calcined product 1.

[0100] At this time, the value of formula (A) is 0.20 (Nm 3 / kg), and the value represented by formula (C) is 0.67 (Nm 3 / kg), and oxygen with a dew point of -23.6°C was supplied as the low dew point gas from the low dew point gas supply unit.

[0101] In the calcination, the coefficient of variation obtained by the method described in the above [Method for measuring the coefficient of variation of the stirring blade frequency] was 0, confirming that LiMO can be produced stably.

[0102] Next, the obtained pre-fired product 1 was placed in a stationary batch-type firing furnace (manufactured by Motoyama Corporation, product name: oxidizing atmosphere furnace SKA-3050F-SP) and fired in an oxygen atmosphere at 720° C. for 5 hours to obtain a fired product 1.

[0103] The obtained fired product 1 was washed, dehydrated using a centrifuge, isolated, and dried at 250° C. under a nitrogen atmosphere to obtain LiMO1.

[0104] A composition analysis of LiMO1 revealed that in the composition formula (I), a=0.02, x=0.09, y=0.03, and the element M1 was Al.

[0105] Example 2 The value of formula (A) is 0.07 (Nm 3 A calcined product 2 was obtained in the same manner as in Example 1, except that the amount of the calcined product was changed to 1 / kg.

[0106] In the preliminary calcination, the coefficient of variation was 0.034, confirming that LiMO could be produced stably.

[0107] LiMO2 was obtained in the same manner as in Example 1, except that pre-calcined product 2 was used.

[0108] A composition analysis of LiMO2 revealed that in the composition formula (I), a=0.02, x=0.09, y=0.03, and the element M1 was Al.

[0109] Comparative Example 1 Without supplying low dew point gas, the value expressed by formula (C) is 1.72 (Nm 3 A calcined product 11 was obtained in the same manner as in Example 1, except that the amount of calcined product was changed to 1 / kg.

[0110] In the calcination, the coefficient of variation was 0.058. Since this value was large and there was a high risk of clogging if the operation was continued, the calcination was stopped midway.

[0111] Comparative Example 2 Without supplying low dew point gas, the value expressed by formula (C) is 0.10 (Nm 3 A calcined product 12 was obtained in the same manner as in Example 1, except that the amount of calcined product was changed to 1 / kg.

[0112] In the calcination, the coefficient of variation was 0.040. Since this value was large and there was a high risk of clogging if the operation was continued, the calcination was stopped midway.

[0113] As shown by the above results, in a countercurrent contact calcination method, when a low dew point gas with a dew point of 10°C or less is supplied from the upstream side of the heating means and calcination is performed under conditions that satisfy formula (A), it has been confirmed that blockages due to condensation near the raw material supply section are unlikely to occur and LiMO can be stably produced. [Explanation of symbols]

[0114] 50: burning device, 51: input section, 52: kiln body, 53: exhaust port, 54: heating means, 55: exhaust port, 56: low dew point gas supply section, 58: conveying section, 581: electric motor, 582: conveying mechanism, 60: gas supply means, 601: oxygen-containing gas supply section, 602: low dew point gas supply line, 61: control section< / cam> < / limo>

Claims

1. A method for producing a lithium metal composite oxide, comprising the step of calcining a material to be treated using a calcination device to obtain a calcined material, the workpiece includes a mixture of a metal complex compound and a lithium compound, The calcination device includes an input section into which the material to be treated is input, a transport section for transporting the material to be treated input from the input section, a cylindrical kiln body, an outlet for discharging the calcined material, and a gas supply means. The kiln body is provided with a heating means, In the above process, A low dew point gas having a dew point of 10° C. or less is supplied from the upstream side of the heating means, supplying an oxygen-containing gas from a downstream side of the heating means; calcining the material to be treated by countercurrently contacting the material with the oxygen-containing gas; The value represented by the following formula (A) is 0.0001 Nm 3 / kg or more 0.30Nm 3 / kg or less. Formula (A): Supply amount of low dew point gas (Nm 3 / hour) / supply amount of material to be treated (kg / hour)

2. The method for producing a lithium metal composite oxide according to claim 1 , wherein the calcination apparatus is a rotary kiln.

3. 3. The method for producing a lithium metal composite oxide according to claim 1, wherein the proportion of Li contained in the lithium compound is 5% by mass or more and 50% by mass or less.

4. The method for producing a lithium metal composite oxide according to claim 3 , wherein the proportion of Li is 5 mass % or more and 30 mass % or less.

5. The value represented by the following formula (C) is 0.3 Nm 3 / kg or more 1Nm 3 3. The method for producing a lithium metal composite oxide according to claim 1, wherein the total amount of the lithium metal composite oxide is 100% or less. Formula (C): Supply amount of oxygen-containing gas (Nm 3 / hour) / supply amount of material to be treated (kg / hour)

6. 3. The method for producing a lithium metal composite oxide according to claim 1, wherein the calcination apparatus is provided with an exhaust port upstream of the heating means, and in the step, the calcination is performed while exhausting the oxygen-containing gas in the calcination apparatus from the exhaust port.

7. The method for producing a lithium metal composite oxide according to claim 1 or 2, wherein the lithium metal composite oxide satisfies the following composition formula (I): Li[Li a (Ni (1-x-y) Co x M1 y ) 1-a O 2 ... Composition formula (I) (In the composition formula (I), M1 is at least one element selected from the group consisting of Mn, Fe, Cu, Ti, Mg, Ca, Al, Zn, W, Nb, Sn, Zr, B, Si, S, and P, and the composition formula (I) satisfies −0.1≦a≦0.2, 0≦x≦0.7, 0<y≦0.7, and x+y<1.)

Citation Information

Patent Citations

  • Method for manufacturing positive electrode active material for lithium secondary battery

    JP2019075253A

Cited By

  • Avalanche photodiode