Method of producing positive electrode active material, positive electrode active material, positive electrode plate, and nonaqueous electrolyte secondary battery
By treating aggregated particles with a fluorine-based compound and lithium-containing oxide, and mixing with single particles, the method addresses gas generation issues in nonaqueous electrolyte secondary batteries, improving storage characteristics.
Patent Information
- Application Number
- JP2023067148
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-04-17
AI Technical Summary
The increase in gas generation during storage affects the storage characteristics of nonaqueous electrolyte secondary batteries when using single particles in the positive electrode plate, leading to deterioration.
A method for producing a positive electrode active material involving the treatment of aggregated particles with a fluorine-based compound and a lithium-containing metal oxide, followed by mixing with single particles, to form a barrier that suppresses gas generation and improves storage characteristics.
The method effectively reduces gas generation to 6.0 cm³/Ah or less after 60 days at 60°C, thereby enhancing the storage characteristics of the battery.
Smart Images

Figure 2024153330000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing a positive electrode active material, and further to a positive electrode active material, a positive electrode plate, and a nonaqueous electrolyte secondary battery. [Background technology]
[0002] Patent Document 1 discloses a lithium metal composite oxide composed of secondary particles formed by agglomerations of primary particles and single particles that exist independently of the secondary particles, and proposes suppressing particle cracking by making the particle size of the single particles relatively small. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-87879 A Summary of the Invention [Problem to be solved by the invention]
[0004] When single particles are used in the positive electrode plate of a non-aqueous electrolyte secondary battery (hereinafter also referred to as a battery), the amount of gas generated when the battery is stored (hereinafter also referred to as a stored gas amount) increases, and the storage characteristics of the battery tend to deteriorate.
[0005] An object of the present disclosure is to provide a positive electrode active material that suppresses deterioration of battery storage characteristics, a method for producing the same, a positive electrode plate including the same, and a nonaqueous electrolyte secondary battery. [Means for solving the problem]
[0006] The present disclosure provides the following method for producing a positive electrode active material, a positive electrode active material, a positive electrode plate including the same, and a nonaqueous electrolyte secondary battery. [1] A method for producing a positive electrode active material, comprising: A preparation step of preparing agglomerated particles containing a nickel-cobalt-manganese compound having a nickel ratio of 75 mol % or more; a first treatment step of treating the surfaces of the aggregated particles with a fluorine-based compound at a temperature of 80° C. or higher; and A second treatment step in which the surface of the aggregated particles after the first treatment step is treated with at least one selected from the group consisting of lithium-containing metal oxides and lithium borate. A method for producing a positive electrode active material comprising the steps of: [2] The method for producing a positive electrode active material according to [1], wherein the fluorine-based compound is a compound containing a perfluoroalkyl group. [3] The method for producing a positive electrode active material according to [1], wherein the lithium-containing metal oxide is at least one selected from the group consisting of lithium tungstate, lithium zirconate, lithium titanate, and lithium aluminate. [4] The method for producing a positive electrode active material according to [1], further comprising a mixing step of mixing the agglomerated particles obtained after the second treatment step with single particles containing a nickel-cobalt-manganese-based compound having a nickel ratio of 70 mol % or more. [5] The method for producing a positive electrode active material according to [4], wherein a mass ratio of the aggregated particles to the single particles is 20:80 to 50:50. [6] After a storage test at 60°C for 60 days, the amount of gas generated was 6.0 cm 3 / Ah or less, and the positive electrode active material includes agglomerated particles containing a nickel-cobalt-manganese compound having a nickel ratio of 75 mol % or more. [7] A positive electrode plate comprising the positive electrode active material according to [6]. [8] A non-aqueous electrolyte secondary battery comprising the positive electrode plate according to [7]. Effect of the Invention
[0007] According to the present disclosure, there are provided a positive electrode active material in which deterioration of storage characteristics is suppressed, a method for producing the same, a positive electrode plate including the same, and a nonaqueous electrolyte secondary battery. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a schematic flow chart of a method for producing a positive electrode active material in this embodiment. [Diagram 2]FIG. 2 is a schematic diagram showing an example of a battery according to this embodiment. [Diagram 3] FIG. 3 is a schematic diagram showing an example of an electrode body in this embodiment. [Figure 4] FIG. 4 is a conceptual diagram showing the positive electrode plate in this embodiment. [Diagram 5] FIG. 5 is a schematic flowchart of a method for producing a positive electrode plate in this embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present disclosure (hereinafter may be abbreviated as "the present embodiment") and an example of the present disclosure (hereinafter may be abbreviated as "the present embodiment") will be described. However, the present embodiment and the example do not limit the technical scope of the present disclosure.
[0010] In this specification, elements expressed in the singular form include the plural form unless otherwise specified. For example, a "particle" can mean not only "one particle" but also "an aggregate of particles (powder, powder, particle group)."
[0011] <Method of manufacturing positive electrode active material> As shown in FIG. 1 , a method for producing a positive electrode active material according to an embodiment of the present disclosure includes a preparation step (A) of preparing agglomerated particles containing a nickel-cobalt-manganese-based compound (hereinafter also referred to as a first NCM compound) having a nickel ratio of 75 mol % or more, a first treatment step (B) of treating the surfaces of the agglomerated particles using a fluorine-based compound at a temperature of 80° C. or more, and a second treatment step (C) of treating the surfaces of the agglomerated particles after the first treatment step with at least one selected from the group consisting of lithium-containing metal oxides and lithium borate.
[0012] Since single particles require a higher temperature treatment than aggregated particles during production, the value of cation mixing is likely to be large, and in order to suppress this, Li / Me is generally set to 1 or more in many cases. In this case, this leads to an increase in the alkaline components present on the surface of the single particles, and the amount of storage gas increases due to the alkaline components remaining on the surface of the single particles, and the storage characteristics tend to deteriorate. It is presumed that this is because one form of the alkaline component changes from LiOH to LiHCO3 to Li2CO3, and as a result, CO2 gas is generated during storage at high temperatures. In addition, not only the decomposition of the alkaline components present on the surface of the positive electrode active material, but also the decomposition of the electrolyte due to contact between the electrolyte and the positive electrode active material tends to occur easily. In the manufacturing method of the positive electrode active material of the present disclosure, a barrier layer that suppresses gas generation is formed between the surface of the aggregated particles and the coating layer by treating the surface of the aggregated particles with a fluorine-based compound and then performing element coating, which makes it easier to suppress the generation of gas due to the above-mentioned alkaline components, and as a result, it is possible to suppress the deterioration of the storage characteristics. In this specification, the storage characteristics are evaluated according to the method described in the Examples section below.
[0013] The aggregated particles prepared in the preparation step (A) may be aggregates of primary particles. The aggregated particles may have any size. The average particle diameters D50, D70, and D30 of the aggregated particles may be, for example, 1 μm or less and 40 μm or less, preferably 1 μm or less and 30 μm or less, and more preferably 1 μm or more and 20 μm or less. The average particle diameters D50, D70, and D30 represent particle diameters at which the cumulative particle volume from the small particle size side in the volume-based particle size distribution is 50%, 70%, and 30%, respectively, of the total particle volume. The average particle diameter can be measured by a laser diffraction / scattering method.
[0014] A primary particle refers to a particle in which grain boundaries cannot be visually confirmed in an SEM image of the particle, and has an average primary particle diameter of less than 0.5 μm. The average primary particle diameter refers to the distance between the two most distant points on the contour line of the primary particle. The average primary particle diameter of the primary particles may be, for example, 0.05 μm to 0.2 μm or 0.1 μm to 0.2 μm. When 10 or more primary particles randomly extracted from an SEM image of one agglomerated particle have an average primary particle diameter of 0.05 μm to 0.2 μm, all of the primary particles contained in the agglomerated particle are considered to have an average primary particle diameter of 0.05 μm to 0.2 μm. The primary particles may have an average primary particle diameter of, for example, 0.1 μm to 0.2 μm.
[0015] The first NCM compound has a nickel ratio of 75 mol % or more, preferably 78 mol % or more, and more preferably 81 mol % or more. The nickel ratio is the nickel content ratio relative to the metal elements excluding lithium.
[0016] The first NCM compound preferably contains a nickel-cobalt-manganese composite hydroxide, more preferably a lithium-nickel-cobalt-manganese composite oxide. The nickel-cobalt-manganese composite hydroxide may be obtained by, for example, a coprecipitation method. The nickel-cobalt-manganese composite hydroxide may be, for example, a compound represented by the general formula: x Co y Mn z It may be a compound represented by (OH)2 (wherein x+y+z=1). The lithium nickel cobalt manganese composite oxide may have a molar ratio of lithium to nickel, cobalt and manganese, Li:(Ni+Co+Mn), of, for example, 1.0 to 1.2:1.0.
[0017] The first NCM compound is, for example, represented by the following formula (1): Li 1-a1 Ni x1 Me 1 1-x1 O2(1) [In formula (1), “a1” satisfies the relationship: −0.3≦a1≦0.3. “x1” satisfies the relationship 0.75≦x1≦1.0. "Me 1 " represents at least one selected from the group consisting of Co, Mn, Al, Zr, Ti, V, Cr, Fe, Cu, Zn, Mo, Sn, Ge, Nb, and W. The layered metal oxide may contain one or more first layered metal oxides represented by the following formula:
[0018] For example, the aggregate particles (primary particles) are LiNi 0.75 Co 0.15 Mn 0.1 O2, and LiNi 0.75 Co 0.1 Mn 0.15 O2 and LiNi 0.8 Co 0.1 Mn 0.1 For example, the aggregate particles (primary particles) may contain at least one selected from the group consisting of LiNi 0.75 Co 0.15 Mn 0.1 O2, and LiNi 0.75 Co 0.1 Mn 0.15 O2 and LiNi 0.8 Co 0.1 Mn 0.1 O2.
[0019] When the agglomerated particles contain a lithium nickel cobalt manganese composite oxide, the agglomerated particles can be obtained, for example, by mixing a lithium source such as lithium hydroxide with a nickel cobalt manganese composite hydroxide, firing the mixture, and then wet-pulverizing the mixture using a ball mill or the like, and drying the mixture.
[0020] The fluorine-based compound used to treat the surfaces of the aggregated particles in the first treatment step (B) is not particularly limited in the length of the main chain, and it is sufficient that at least one of the atoms present in the side chain is a fluorine atom. For example, the compound may have a functional group such as an aliphatic hydrocarbon group (e.g., a methyl group, an ethyl group, etc.) or an aromatic hydrocarbon group (e.g., a benzene ring), and at least one of the hydrogen atoms of the functional group may be substituted with fluorine. Examples of fluorine-containing compounds include compounds containing perfluoroalkyl groups. Specific examples thereof include trimethoxysilane (CH 16 O3Si), perfluorohexylethyltriethoxysilane (CF3(CF2)5CH2CH2Si(OEt)3), perfluorohexylethyltrimethoxysilane (CF3(CF2)5CH2CH2Si(OMe)3), perfluorohexylethyltrichlorosilane (CF3(CF2)5CH2CH2SiCl3), CF3(CF2)9CH2CH2Si(OCH3)3, and CF3(CF2)3(C6H4)CH(OH)CH3. Examples of the fluorine-based compound include surfactants containing fluorine.
[0021] The temperature for treating the surface of the aggregated particles with a fluorine-based compound is 80° C. or higher, and from the viewpoint of storage properties, is preferably 80° C. or higher and 160° C. or lower. The method for treating the surface of the aggregated particles with a fluorine-based compound may be any method that can cause the fluorine-based compound to be present on part of the surface of the aggregated particles, and examples of the method include coating treatments such as mechanochemical treatments. The mechanochemical treatment can be, for example, a dry treatment in which a base material (aggregated particles) and coating material particles (fluorine-based compound) are rotated at high speed in a container together with media (e.g., zirconia beads, etc.), and the coating material particles are crushed and bonded to the surface of the base material to coat them.
[0022] The lithium-containing metal oxide used in the second treatment step (C) may include at least one selected from the group consisting of lithium tungstate (Li2WO4), lithium zirconate (Li2ZrO3), lithium titanate (Li2TiO3) and lithium aluminate (LiAlO2). From the viewpoint of storage characteristics, lithium borate is preferably used.
[0023] In the second treatment step (C), the surface of the aggregated particles after the first treatment step is treated with at least one selected from the group consisting of lithium-containing metal oxides and lithium borate, for example, a method of heat treating the aggregated particles using at least one selected from the group consisting of metal oxides and boric acid and a lithium salt, etc. For example, a method of mixing the aggregated particles after the first treatment step with at least one selected from the group consisting of metal oxides and boric acid and a lithium salt, and heating at a temperature of 200°C to 400°C for 1 hour, etc. Examples of the lithium salt include lithium carbonate, etc. Examples of the metal oxide include tungstic acid (H3BO3), zirconic acid (H4O4Zr), titanic acid (H4TiO4), aluminic acid (HAlO2), etc. The heat treatment time is preferably 10 minutes to 60 minutes from the viewpoint of storage characteristics.
[0024] The method for producing a positive electrode active material may further include a mixing step of mixing the aggregated particles after the second treatment step with single particles containing an NCM compound having a nickel ratio of 70 mol% or more (hereinafter also referred to as a second NCM compound). The single particles may have any size. The average particle diameter D50 of the single particles may be, for example, 1 μm or more and 20 μm or less, preferably 1 μm or less and 10 μm or less, and more preferably 1 μm or more and 5 μm or less.
[0025] The nickel content in the second NCM compound is 70 mol % or more, preferably 73 mol % or more, and more preferably 76 mol % or more.
[0026] The second NCM compound preferably contains a nickel-cobalt-manganese composite hydroxide, more preferably a lithium-nickel-cobalt-manganese composite oxide. The nickel-cobalt-manganese composite hydroxide may be obtained by, for example, a coprecipitation method. The nickel-cobalt-manganese composite hydroxide may be, for example, a compound represented by the general formula: x Co y Mn z It may be a compound represented by (OH)2 (wherein x+y+z=1). The lithium nickel cobalt manganese composite oxide may have a molar ratio of lithium to nickel, cobalt and manganese, Li:(Ni+Co+Mn), of, for example, 1.0 to 1.2:1.0.
[0027] The single particle may be, for example, a particle represented by the following formula (2): Li 1-a2 Ni x2 Me 2 1-x2 O2(2) [In formula (2), “a2” satisfies the relationship: −0.3≦a2≦0.3. “x2” satisfies the relationship 0.7≦x2<1.0. "Me 2 " represents at least one selected from the group consisting of Co, Mn, Al, Zr, Ti, V, Cr, Fe, Cu, Zn, Mo, Sn, Ge, Nb, and W. The layered metal oxide may contain one or more second layered metal oxides represented by the following formula:
[0028] For example, a single particle is LiNi 0.7 Co 0.2 Mn 0.1 O2, and LiNi 0.7 Co 0.1 Mn 0.2 O2 and LiNi 0.8 Co 0.1 Mn 0.1 For example, the single particle may substantially contain at least one selected from the group consisting of LiNi 0.7 Co 0.2 Mn 0.1 O2, and LiNi 0.7 Co 0.1Mn 0.2 O2 and LiNi 0.8 Co 0.1 Mn 0.1 O2.
[0029] When the single particle contains a lithium nickel cobalt manganese composite oxide, the single particle can be obtained by mixing a lithium source such as lithium hydroxide and a nickel cobalt manganese composite hydroxide, firing the mixture, and then wet-pulverizing the mixture using a ball mill or the like and drying the mixture. The single particle may be surface-treated.
[0030] In the mixing step, the single particles can be mixed so that the mass ratio of the agglomerated particles to the single particles is, for example, 20:80 to 50:50, and is preferably 30:70 to 50:50. When the positive electrode active material contains the single particles and the agglomerated particles in the above-mentioned mass ratio, particle cracking tends to be easily suppressed. The positive electrode active material layer formed from the positive electrode active material containing the single particles and the agglomerated particles in the above-mentioned mass ratio has a density of 3.7 g / cm. 3 Even if the amount is more than this, particle cracking tends to be easily suppressed.
[0031] <Cathode active material> In another embodiment of the positive electrode active material of the present disclosure, the amount of gas generated after a storage test at a temperature of 60° C. and a storage period of 60 days was 6.0 cm 3 / Ah or less and includes an NCM compound having a nickel ratio of 75 mol% or more. The positive electrode active material of the present disclosure includes the agglomerated particles, which tend to suppress the generation of storage gas and to easily suppress deterioration of storage characteristics by including the agglomerated particles. The agglomerated particles can be agglomerated particles obtained by the above-mentioned method for producing a positive electrode active material. The above-mentioned explanations regarding the agglomerated particles and the first NCM compound in the method for producing a positive electrode active material are applied to the agglomerated particles and the NCM compound having a nickel ratio of 75 mol% or more, respectively. The amount of gas generated after a storage test at a temperature of 60°C and a storage period of 60 days is measured by a method described later in the Examples section.
[0032] The positive electrode active material may further include single particles containing an NCM compound having a nickel ratio of 70 mol% or more. The explanations for the single particles and the second NCM compound in the method for producing a positive electrode active material described above are applied to the single particles and the NCM compound having a nickel ratio of 70 mol% or more (hereinafter also referred to as the second NCM compound), respectively. The mass ratio of the agglomerated particles to the single particles in the positive electrode active material may be, for example, 20:80 to 50:50, and is preferably 30:70 to 50:50. When the mass ratio of the single particles to the agglomerated particles in the positive electrode active material is within the above range, particle cracking tends to be easily suppressed.
[0033] <Nonaqueous electrolyte secondary battery> Fig. 2 is a schematic diagram showing an example of a nonaqueous electrolyte secondary battery in this embodiment. The battery 100 shown in Fig. 2 may be, for example, a lithium ion battery used as a main power source or a power assist power source for an electric vehicle.
[0034] The battery 100 includes an exterior body 90. The exterior body 90 houses an electrode assembly 50 and an electrolyte (not shown). The electrode assembly 50 is connected to a positive terminal 91 by a positive current collecting member 81. The electrode assembly 50 is connected to a negative terminal 92 by a negative current collecting member 82. FIG. 3 is a schematic diagram showing an example of an electrode assembly in this embodiment. The electrode assembly 50 is of a wound type. The electrode assembly 50 includes a positive electrode plate 20, a separator 40, and a negative electrode plate 30. That is, the battery 100 includes a positive electrode plate 20. The positive electrode plate 20 includes a positive electrode active material layer 22 and a positive electrode substrate 21. The negative electrode plate 30 includes a negative electrode active material layer 32 and a negative electrode substrate 31.
[0035] <Positive electrode plate> As shown in FIG. 4, a positive electrode plate 20 may have a positive electrode active material layer 22 formed directly or indirectly on one or both sides of a positive electrode substrate 21. The positive electrode substrate 21 may be, for example, a conductive sheet made of an Al alloy foil, a pure Al foil, or the like. The positive electrode active material constituting the positive electrode active material layer 22 contains aggregated particles 12. As shown in FIG. 4, the positive electrode active material may contain single particles 11. The positive electrode active material can be produced by the above-mentioned method for producing a positive electrode active material. The positive electrode active material layer 22 may further contain a conductive material, a binder, and the like.
[0036] The positive electrode active material layer 22 may have a thickness of, for example, 10 μm or more and 200 μm or less. The positive electrode active material layer 22 may have a high density. The density of the positive electrode active material layer 22 is, for example, 3.65 g / cm 3 or more, 3.7 g / cm 3 or more than 3.8g / cm 3 The positive electrode active material layer 22 may have a density of, for example, 4.0 g / cm 3 It may have the following densities:
[0037] <Manufacturing method of positive electrode plate> The manufacturing method of the positive electrode plate 20 in this embodiment includes the preparation of a positive electrode slurry (A), application (B), and rolling (C) as shown in FIG. 5. In the preparation of the positive electrode slurry (A), a positive electrode slurry containing the positive electrode active material manufactured by the manufacturing method of the positive electrode active material described above is prepared. The positive electrode slurry is prepared by dispersing the positive electrode active material in a dispersion medium. The dispersion medium may be an organic solvent, such as N-methyl-2-pyrrolidone (NMP), tetrahydrofuran (THF), dimethylformamide (DMF), methyl ethyl ketone (MEK), and dimethyl sulfoxide (DMSO). The positive electrode slurry may contain a conductive material and a binder. Examples of the conductive material include carbon nanotubes, carbon black such as acetylene black (AB), and other carbon materials (e.g., graphite, etc.). Examples of the binder include polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), polyimide (PI), polyamide (PA), polyamideimide (PAI), butadiene rubber (BR), styrene butadiene rubber (SBR), nitrile-butadiene rubber (NBR), styrene-ethylene-butylene-styrene block copolymer (SEBS), carboxymethyl cellulose (CMC), or a combination thereof. The slurry may have a solids concentration of, for example, 40% to 80%. Any stirring device, mixing device, or dispersing device may be used for mixing.
[0038] In coating (B), the positive electrode slurry is coated on the surface of the positive electrode substrate 21 to form a positive electrode active material layer 22. In rolling (C), the positive electrode active material layer 22 and the positive electrode substrate 21 are rolled to produce the positive electrode plate 20. A raw sheet of the positive electrode plate 20 is produced by rolling. The raw sheet can be cut to a predetermined planar size according to the specifications of the battery 100. EXAMPLES
[0039] The present invention will be described in more detail below with reference to examples. In the examples, "%" and "parts" are by mass % and parts by mass unless otherwise specified.
[0040] <Example 1> [Preparation of aggregated particles] Obtained by coprecipitation, with the composition Ni 0.83 Co 0.05 Mn 0.12 The nickel-cobalt-manganese composite hydroxide of (OH)2 was baked together with lithium hydroxide in an oxygen atmosphere at a temperature of 800°C for 10 hours, and then crushed to obtain agglomerated particles of lithium composite oxide (preparation step). 0.05 wt% of trimethoxysilane solvent having a perfluoroalkyl group containing fluorine (hereinafter also referred to as trimethoxysilane solvent) was added to the agglomerated particles, and mixed with φ2 mm zirconia balls using a P5 planetary mill manufactured by Flitch. The temperature after 30 minutes of mixing was 80°C (first treatment step). Next, 0.6 wt% of boric acid and an equal molar amount of lithium carbonate were added to the obtained agglomerated particles of the lithium composite oxide in a dispersed state, and the mixture was heat-treated at a temperature of 300°C to obtain an active material (first composite oxide) with an agglomerated structure coated with lithium borate (second treatment step). The particle size distribution of the first composite oxide was D50 12 μm, D70 14 μm, and D30 10 μm. The cross section of the first composite oxide after the CP processing was observed by SEM, and the average primary particle size of the first composite oxide was found to be 0.13 μm.
[0041] <Example 2 and Comparative Example 2> The aggregated particles of Example 2 and Comparative Example 2 were prepared in the same manner as in Example 1, except that the treatment temperature in the first treatment step in Example 1 was changed to the treatment temperatures shown in Table 1. <Example 3> The aggregated particles of Example 3 were prepared in the same manner as in Example 1, except that the fluorine-based compound shown in Table 1 was used instead of the fluorine-based compound used in Example 1, and the treatment temperature in the first treatment step in Example 1 was changed to the treatment temperature shown in Table 1. <Examples 4 to 6> The aggregated particles of Examples 4 to 6 were prepared in the same manner as Example 1, except that the fluorine-based compound used in Example 1 was replaced with the fluorine-based compound shown in Table 1, the treatment temperature of the first treatment step in Example 1 was replaced with the treatment temperature shown in Table 1, and tungstic acid, titanic acid, and zirconic acid were used in Examples 4 to 6 in place of boric acid in Example 1, in the same molar amounts as in Example 1.
[0042] <Comparative Example 1> Aggregated particles were prepared in the same manner as in Example 1, except that after the preparation step in Example 1, the second treatment step was carried out without carrying out the first treatment step.
[0043] [Preparation of single particles] Obtained by coprecipitation, with the composition Ni 0.78 Co 0.11 Mn 0.11 The nickel-cobalt-manganese composite hydroxide of (OH)2 was calcined at 500°C to obtain a nickel-cobalt-manganese composite oxide (Z1). Next, lithium hydroxide and the nickel-cobalt-manganese composite oxide (Z1) were mixed so that the molar ratio of Li to the total amount of Ni, Co, and Mn was 1.05:1, and the mixture was calcined at 900°C for 72 hours in an oxygen atmosphere, and then wet-pulverized in a ball mill and dried to form a single particle structure. The mixture was then heat-treated again at 750°C for 10 hours in an oxygen atmosphere to obtain a lithium composite oxide (second composite oxide) with a single particle structure. When the particle size distribution of the second composite oxide was measured, the particle diameter (D50) was 3.6 μm, and when the structure was observed by SEM, the second composite oxide was found to be almost a particle with a single particle structure, and the particle diameter was 2.5 to 3.8 μm.
[0044] [Preparation of positive electrode plate] The mixture of the aggregated particles obtained in the Examples and Comparative Examples and the above single particles in a 1:1 ratio was further mixed with acetylene black and polyvinylidene fluoride (PVdF) to a solid content mass ratio of 96.3:2.5:1.2, and an appropriate amount of N-methyl-2-pyrrolidone (NMP) was added, followed by kneading to prepare a positive electrode composite slurry. The positive electrode composite slurry was applied to both sides of a 1N30 aluminum foil core having a thickness of 13 μm, the coating was dried, and then the coating was rolled using a rolling machine until the composite density of the coating became 3.7 g / cm. 3 Then, the positive electrode core was compressed so as to have a predetermined electrode size, and then cut to obtain a positive electrode plate having a positive electrode mixture layer formed on both sides of the positive electrode core.
[0045] [Production and evaluation of small lithium-ion batteries] The positive electrode plate and the carbon negative electrode were combined with a separator, placed in a laminate outer bag, and sealed with electrolyte to create a small laminated battery. The size of the battery was 8 layers of electrodes stacked together to obtain a charging capacity of 600mAh.
[0046] [Evaluation of storage characteristics] The fabricated battery was charged and then stored in a thermostatic chamber at 60° C. for 60 days, after which the amount of gas generated was measured. The results are shown in Table 1.
[0047] [Table 1]
[0048] As shown in Table 1, in Examples 1 to 6, the DTG peak values after the storage test at a temperature of 60° C. for a storage period of 60 days were lower than those in Comparative Examples 1 and 2. It is clear that according to the present disclosure, a positive electrode active material with excellent storage characteristics can be produced. [Explanation of symbols]
[0049] 11 single particle, 12 agglomerated particle, 20 positive electrode plate, 21 positive electrode substrate, 22 positive electrode active material layer, 30 negative electrode plate, 31 negative electrode substrate, 32 negative electrode active material layer, 40 separator, 50 electrode body, 81 positive electrode current collector, 82 negative electrode current collector, 90 exterior body, 91 positive electrode terminal, 92 negative electrode terminal, 100 battery.
Claims
1. A method for producing a positive electrode active material, comprising: A preparation step of preparing agglomerated particles containing a nickel-cobalt-manganese compound having a nickel ratio of 75 mol % or more; a first treatment step of treating the surfaces of the aggregated particles with a fluorine-based compound at a temperature of 80° C. or higher; and a second treatment step of treating the surface of the aggregated particles after the first treatment step with at least one selected from the group consisting of lithium-containing metal oxides and lithium borate; A method for producing a positive electrode active material comprising the steps of:
2. The method for producing a positive electrode active material according to claim 1 , wherein the fluorine-based compound is a compound containing a perfluoroalkyl group.
3. 2. The method for producing a positive electrode active material according to claim 1, wherein the lithium-containing metal oxide is at least one selected from the group consisting of lithium tungstate, lithium zirconate, lithium titanate, and lithium aluminate.
4. 2. The method for producing a positive electrode active material according to claim 1, further comprising a mixing step of mixing the aggregated particles obtained after the second treatment step with single particles containing a nickel-cobalt-manganese based compound having a nickel ratio of 70 mol % or more.
5. The method for producing a positive electrode active material according to claim 4, wherein a mass ratio of the aggregated particles to the single particles is 20:80 to 50:
50.
6. After a storage test at 60°C for 60 days, the amount of gas generated was 6.0 cm 3 / Ah or less, and the positive electrode active material includes agglomerated particles containing a nickel-cobalt-manganese compound having a nickel ratio of 75 mol % or more.
7. A positive electrode plate comprising the positive electrode active material according to claim 6.
8. A non-aqueous electrolyte secondary battery comprising the positive electrode plate according to claim 7.
Citation Information
Patent Citations
Cathode active material for lithium secondary battery, method for manufacturing the same and lithium secondary battery having positive electrode including cathode active material
JP2019200991A
Positive electrode for secondary battery
JP2022170190A
Positive electrode active material for lithium secondary battery and lithium secondary battery containing the same
JP2023553058A
Positive electrode active material powder for lithium secondary battery, its manufacturing method, positive electrode for lithium secondary battery, and lithium secondary battery
JP2024535751A
Positive electrode active material for secondary cells
WO2012081348A1