Secondary battery
By using a positive electrode active material with an O2 type structure and a compliant inorganic solid electrolyte with a Young's modulus of 30 GPa or less, the battery maintains contact and reduces resistance during charging and discharging cycles, addressing the volume change issue in conventional secondary batteries.
Patent Information
- Application Number
- JP2023067241
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-17
- Publication Date
- 2024-10-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional secondary batteries experience increased resistance due to repeated charging and discharging cycles, primarily attributed to the inability of the solid electrolyte to maintain contact with the positive electrode active material layer as it undergoes significant volume changes.
Incorporating a positive electrode active material with an O2 type structure and an inorganic solid electrolyte having a Young's modulus of 30 GPa or less, which allows the electrolyte to deform and maintain contact with the active material despite volume changes, thereby reducing void formation and resistance.
The secondary battery exhibits a minimal increase in resistance during repeated charging and discharging cycles by ensuring consistent contact between the positive electrode active material and the electrolyte, thus enhancing its durability.
Smart Images

Figure 2024153377000001_ABST
Abstract
Description
[Technical field]
[0001] The present application discloses a secondary battery. [Background technology]
[0002] Patent Document 1 discloses that a solid electrolyte is used together with a positive electrode active material having an O2 type structure in a positive electrode active material layer of a secondary battery. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2022-085829 Summary of the Invention [Problem to be solved by the invention]
[0004] Conventional secondary batteries are prone to increasing resistance when repeatedly charged and discharged. [Means for solving the problem]
[0005] The present application discloses the following aspects as means for solving the above problems. <Aspect 1> A secondary battery having a positive electrode active material layer, a solid electrolyte layer, and a negative electrode active material layer, the positive electrode active material layer contains a positive electrode active material having an O2 type structure, The positive electrode active material layer contains an inorganic solid electrolyte having a Young's modulus of 30 GPa or less. Secondary battery. <Aspect 2> The secondary battery of aspect 1, The positive electrode active material contains, as constituent elements, at least one transition metal element selected from Mn, Ni, and Co, Li, and O. Secondary battery. <Aspect 3> The secondary battery according to aspect 1 or 2, The positive electrode active material is Lia Na b Mn x-p Ni y-q Co z-r M p+q+r O2 (where 0 < a ≤ 1.00, 0 ≤ b ≤ 0.20, x + y + z = 1, and 0 ≤ p + q + r ≤ 0.15, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W.) having a chemical composition represented by Secondary battery. <Aspect 4> A secondary battery according to any one of Aspects 1 to 3, wherein the inorganic solid electrolyte contains at least Li, P, S, and a halogen element as constituent elements. Secondary battery. <Aspect 5> A secondary battery according to any one of Aspects 1 to 4, wherein the Young's modulus of the inorganic solid electrolyte is 10 GPa or more and 30 GPa or less. Secondary battery.
Advantages of the Invention
[0006] The secondary battery of the present disclosure has a small increase in resistance when charge and discharge are repeated.
Brief Description of the Drawings
[0007] [Figure 1] An example of the configuration of a secondary battery is schematically shown. [Diagram 2] The relationship between the Young's modulus of the solid electrolyte contained in the positive electrode active material layer and the resistance increase rate of the secondary battery is shown.
Modes for Carrying Out the Invention
[0008] Hereinafter, an embodiment of the secondary battery of the present disclosure will be described, but the secondary battery of the present disclosure is not limited to the embodiments shown below.
[0009] 1, a secondary battery 100 according to one embodiment includes a positive electrode active material layer 10, a solid electrolyte layer 20, and a negative electrode active material layer 30. The positive electrode active material layer 10 includes a positive electrode active material having an O2 type structure. The positive electrode active material layer 10 also includes an inorganic solid electrolyte having a Young's modulus of 30 GPa or less.
[0010] 1.Cathode active material layer The positive electrode active material layer 10 includes a positive electrode active material having an O2 type structure and an inorganic solid electrolyte having a Young's modulus of 30 GPa or less. The positive electrode active material layer 10 may also optionally include a conductive assistant or a binder. The positive electrode active material layer 10 may also optionally include other positive electrode active materials or other electrolytes. The positive electrode active material layer 10 may also optionally include various additives. The content of each component in the positive electrode active material layer 10 may be appropriately determined according to the intended battery performance. For example, the content of the positive electrode active material having an O2 type structure may be 40 mass% or more, 50 mass% or more, or 60 mass% or more, or 99 mass% or less, 95 mass% or less, 90 mass% or less, or 85 mass% or less, based on the entire positive electrode active material layer 10 (total solid content) being 100 mass%. In addition, the content of the inorganic solid electrolyte having a Young's modulus of 30 GPa or less may be 1 mass% or more, 5 mass% or more, or 10 mass% or more, and 60 mass% or less, 50 mass% or less, or 40 mass% or less, with the entire positive electrode active material layer 10 (total solid content) being taken as 100 mass%. The shape of the positive electrode active material layer 10 is not particularly limited, and may be, for example, a sheet having a substantially flat surface. The thickness of the positive electrode active material layer 10 is not particularly limited, and may be, for example, 0.1 μm or more or 1 μm or more, and 2 mm or less or 1 mm or less.
[0011] 1.1 Positive electrode active material with O2 structure The positive electrode active material layer 10 includes a positive electrode active material having an O2 type structure. The positive electrode active material has at least an O2 type structure (belonging to space group P63mc) as a crystal structure. The positive electrode active material may have a crystal structure other than the O2 type structure in addition to the O2 type structure. Examples of crystal structures other than the O2 type structure include a T♯2 type structure (belonging to space group Cmca) formed when Li is deintercalated from the O2 type structure and an O6 type structure (belonging to space group R-3m, with a c-axis length of 2.5 nm to 3.5 nm, typically 2.9 nm to 3.0 nm, and different from the O3 type structure also belonging to space group R-3m). The positive electrode active material may have an O2 type structure as a main phase, or may have a crystal structure other than the O2 type structure as a main phase. The positive electrode active material may have a crystal structure that is a main phase that changes depending on the charge / discharge state.
[0012] The positive electrode active material having an O2 type structure may contain at least one transition metal element selected from Mn, Ni, and Co, Li, and O as constituent elements. In particular, when the positive electrode active material contains at least Mn, at least one of Ni and Co, Li, and O as constituent elements, and especially when the positive electrode active material contains at least Li, Mn, Ni, Co, and O as constituent elements, it is easy to ensure higher performance. However, the positive electrode active material may, for example, release Li almost completely upon charging, and the molar concentration of Li may approach 0 to the limit. In addition, the positive electrode active material having an O2 type structure may contain Na as a constituent element due to its manufacturing process. In addition, the positive electrode active material may contain the element M described below. In addition, the positive electrode active material may contain other impurity elements. In one embodiment, the positive electrode active material having an O2 type structure contains Li a Na b Mn x-p Ni y-q Co z-r M p+q+rIt may have a chemical composition represented by O2 (where 0 < a ≤ 1.00, 0 ≤ b ≤ 0.20, x + y + z = 1, and 0 ≤ p + q + r ≤ 0.15, and the element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W). In the chemical composition, a may be greater than 0, 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, 0.50 or more, or 0.60 or more, and may also be 1.00 or less, 0.90 or less, 0.80 or less, or 0.70 or less. Also, b may be 0 or more or greater than 0, and may also be 0.15 or less, 0.10 or less, 0.05 or less, 0.04 or less, 0.03 or less, 0.02 or less, or 0.01 or less. Also, x may be 0 or more, 0.10 or more, 0.20 or more, 0.30 or more, 0.40 or more, or 0.50 or more, and may also be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, or 0.50 or less. Also, y may be 0 or more, 0.10 or more, or 0.20 or more, and may also be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, 0.30 or less, or 0.20 or less. Also, z may be 0 or more, 0.10 or more, 0.20 or more, or 0.30 or more, and may also be 1.00 or less, 0.90 or less, 0.80 or less, 0.70 or less, 0.60 or less, 0.50 or less, 0.40 or less, or 0.30 or less. The element M has little contribution to charge and discharge. In this regard, in the above chemical composition, when p + q + r is 0.15 or less, it is easy to ensure a high charge and discharge capacity. p + q + r may be 0.12 or less, 0.10 or less, 0.08 or less, 0.06 or less, 0.05 or less, or 0.04 or less. On the other hand, when the element M is included, the O2 type structure is likely to be stabilized. In this regard, in the above chemical composition, p + q + r is 0 or more, and may also be greater than 0, 0.01 or more, 0.02 or more, or 0.03 or more. The composition of O is approximately 2, but is not necessarily exactly 2.0 and is indefinite. Also, in the above chemical composition of the positive electrode active material having an O type structure, when the valence of the element M is +n, the relationship 3.0 ≤ 4(x - p) + 2(y - q) + 3(z - r) + n(p + q + r) ≤ 3.5 may be satisfied.This is intended to mean a range in which the total valence of the metals in the positive electrode active material is close to 3.33 (charge neutrality when a is 0.67). A positive electrode active material having an O2 type structure is synthesized via a Na-containing transition metal oxide having a P2 type structure, and charge neutrality occurs when the Na composition at this time is in the range of 0.5 to 1.0, which corresponds to the case where the above relationship is satisfied.
[0013] The positive electrode active material having an O2 type structure may be, for example, particulate. The positive electrode active material particles may be solid particles, hollow particles, or may have voids. The positive electrode active material particles may be primary particles, or may be secondary particles formed by agglomeration of a plurality of primary particles. The average particle diameter (D50) of the positive electrode active material particles may be, for example, 1 nm or more, 5 nm or more, or 10 nm or more, and may be 500 μm or less, 100 μm or less, 50 μm or less, or 30 μm or less. The average particle diameter D50 in the present application is the particle diameter (median diameter) at an integrated value of 50% in a volume-based particle size distribution obtained by a laser diffraction / scattering method.
[0014] A protective layer containing an ion-conductive oxide may be formed on the surface of the positive electrode active material. This makes it easier to suppress reactions between the positive electrode active material and other battery materials (e.g., inorganic solid electrolytes, etc., described below). Examples of ion-conductive oxides include Li3BO3, LiBO2, Li2CO3, LiAlO2, Li4SiO4, Li2SiO3, Li3PO4, Li2SO4, Li2TiO3, and Li4Ti5O. 12 , Li2Ti2O5, Li2ZrO3, LiNbO3, Li2MoO4, Li2WO4, etc. The ion conductive oxide may be one in which some elements are replaced with a doping element such as P or B. The coverage (area ratio) of the protective layer to the surface of the positive electrode active material may be, for example, 70% or more, 80% or more, or 90% or more. The thickness of the protective layer may be, for example, 0.1 nm or more or 1 nm or more, and may be 100 nm or less, or 20 nm or less.
[0015] 1.2 Inorganic solid electrolyte with Young's modulus of 30 GPa or less The positive electrode active material layer 10 includes an inorganic solid electrolyte having a Young's modulus of 30 GPa or less together with the positive electrode active material having the O2 type structure. The Young's modulus of the inorganic solid electrolyte may be 10 GPa or more and 30 GPa or less, or 15 GPa or more and 25 GPa or less. In the present application, the "Young's modulus" refers to the Young's modulus at 25°C. The Young's modulus of the inorganic solid electrolyte can be measured by a nanoindenter. According to the knowledge of the present inventor, the positive electrode active material having an O2 type structure has a large volume change accompanying charge and discharge. Therefore, in a conventional secondary battery using a positive electrode active material having an O2 type structure and a solid electrolyte in combination, when charging and discharging are repeated, the contact between the positive electrode active material and the solid electrolyte cannot be maintained, or voids are generated in the positive electrode active material layer due to the volume change of the positive electrode active material, and the resistance of the secondary battery is likely to increase. In contrast, in the present embodiment, the positive electrode active material layer 10 contains an inorganic solid electrolyte having a Young's modulus of 30 GPa or less. Even if the volume of the positive electrode active material changes due to charging and discharging, the inorganic solid electrolyte deforms to follow the volume change, for example, thereby maintaining contact between the positive electrode active material and the inorganic solid electrolyte, and the inorganic solid electrolyte is replenished in voids generated by the volume change of the positive electrode active material, thereby reducing an increase in resistance of the secondary battery.
[0016] The Young's modulus of the inorganic solid electrolyte varies depending on the constituent elements. The inorganic solid electrolyte may be, for example, a sulfide solid electrolyte containing S as a constituent element, a halide solid electrolyte containing a halogen element as a constituent element, or a complex hydride solid electrolyte containing a complex ion. Among these sulfide solid electrolytes, halogenated solid electrolytes, and complex hydride solid electrolytes, one having a Young's modulus of 30 GPa or less may be adopted. In particular, when the inorganic solid electrolyte contains at least Li, P, S, and a halogen element as constituent elements, it is easy to have a Young's modulus of 30 GPa or less and excellent ion conductivity.
[0017] The sulfide solid electrolyte may be a glass-based sulfide solid electrolyte (sulfide glass), a glass ceramic-based sulfide solid electrolyte, or a crystalline sulfide solid electrolyte. The sulfide glass is amorphous. The sulfide glass preferably has a glass transition temperature (Tg). In addition, when the sulfide solid electrolyte has a crystalline phase, examples of the crystalline phase include a Thio-LISICON type crystalline phase, a LGPS type crystalline phase, and an Argyrodite type crystalline phase. The sulfide solid electrolyte preferably contains, for example, a Li element, an X element (X is at least one of P, As, Sb, Si, Ge, Sn, B, Al, Ga, and In), and an S element. In addition, the sulfide solid electrolyte may further contain at least one of an O element and a halogen element. In addition, the sulfide solid electrolyte preferably contains an S element as a main component of an anion element. As described above, the sulfide solid electrolyte may contain at least Li, P, S and a halogen element as constituent elements.
[0018] The halide solid electrolyte may be, for example, a compound represented by the formula (A): Li α M β X γ (A) Here, α, β, and γ are each independently a value greater than 0, M is at least one selected from the group consisting of metal elements and metalloid elements other than Li, and X is at least one selected from the group consisting of Cl, Br, and I. The "metalloid element" may be at least one selected from the group consisting of B, Si, Ge, As, Sb, and Te. The "metal element" may include (i) all elements included in Groups 1 to 12 of the periodic table (excluding hydrogen) and (ii) all elements included in Groups 13 to 16 of the periodic table (excluding B, Si, Ge, As, Sb, Te, C, N, P, O, S, and Se).
[0019] The complex hydride solid electrolyte may be composed of Li ions and complex ions containing H. The complex ion containing H may have, for example, an element A containing at least one of a nonmetallic element, a semimetallic element, and a metallic element, and H bonded to the element A. The complex ion containing H may have the element A as a central element and H surrounding the element A bonded to each other via a covalent bond. The complex ion containing H may be a complex ion containing Li ions, for example, an element A containing at least one of a nonmetallic element, a semimetallic element, and a metallic element, and H bonded to the element A via a covalent bond. m H n ) α- In this case, m is any positive number, and n and α can be any positive number depending on m and the valence of element A. Element A may be a nonmetallic element or a metallic element capable of forming a complex ion. For example, element A may contain at least one of B, C, and N as a nonmetallic element, or may contain B. Also, for example, element A may contain at least one of Al, Ni, and Fe as a metallic element. In particular, when the complex ion contains B, or contains C and B, softness and higher ionic conductivity are easily ensured. Specific examples of complex ions containing H include (CB9H 10 ) - , (C.B. 11 H 12 ) - , (B 10 H 10 ) 2- , (B 12 H 12 ) 2- , (BH4) - , (NH2) - , (AlH4) - , and combinations thereof. In particular, (CB9H 10 ) - , (C.B. 11 H 12 ) - In other words, the complex hydride solid electrolyte may contain Li, C, B, and H.
[0020] 1.3 Other ingredients Examples of the conductive assistant that may be included in the positive electrode active material layer 10 include carbon materials such as vapor grown carbon fiber (VGCF), acetylene black (AB), ketjen black (KB), carbon nanotubes (CNT), and carbon nanofibers (CNF); and metal materials such as nickel, titanium, aluminum, and stainless steel. The conductive assistant may be, for example, particulate or fibrous, and the size thereof is not particularly limited. Only one type of conductive assistant may be used alone, or two or more types may be used in combination.
[0021] Examples of binders that can be included in the positive electrode active material layer 10 include butadiene rubber (BR)-based binders, butylene rubber (IIR)-based binders, acrylate butadiene rubber (ABR)-based binders, styrene butadiene rubber (SBR)-based binders, polyvinylidene fluoride (PVdF)-based binders, polytetrafluoroethylene (PTFE)-based binders, polyimide (PI)-based binders, etc. Only one type of binder may be used alone, or two or more types may be used in combination.
[0022] The positive electrode active material layer 10 may contain various additives in addition to the above components, such as a dispersant, a lubricant, etc. The positive electrode active material layer 10 may also contain other positive electrode active materials and other electrolytes.
[0023] 2.Solid electrolyte layer The solid electrolyte layer 20 is disposed between the positive electrode active material layer 10 and the negative electrode active material layer 30. The solid electrolyte layer 20 includes at least a solid electrolyte. The solid electrolyte included in the solid electrolyte layer 20 may be an inorganic solid electrolyte or an organic polymer electrolyte. In particular, inorganic solid electrolytes, particularly sulfide solid electrolytes, have high performance. The solid electrolyte layer 20 may include a liquid component together with the solid electrolyte, and may further include a binder and various additives. The content of the solid electrolyte and the like in the solid electrolyte layer 20 is not particularly limited. The thickness of the solid electrolyte layer 20 is not particularly limited, and may be, for example, 0.1 μm or more and 2 mm or less, the lower limit may be 1 μm or more, and the upper limit may be 1 mm or less. The solid electrolyte layer 20 may be made of one layer or may be made of multiple layers. For example, the solid electrolyte layer 20 may include a first layer disposed on the positive electrode active material layer 10 side and a second layer disposed on the negative electrode active material layer 30 side, and the first layer may include a first electrolyte, and the second layer may include a second electrolyte. The first electrolyte and the second electrolyte may be different from each other. The first electrolyte and the second electrolyte may each be at least one selected from the above-mentioned various inorganic solid electrolytes. For example, the first layer may include a halide solid electrolyte, and the second layer may include at least one of a halide solid electrolyte and a sulfide solid electrolyte.
[0024] 3.Negative electrode active material layer The negative electrode active material layer 30 includes at least a negative electrode active material, and may further include an electrolyte, a conductive assistant, a binder, various additives, and the like. The content of each of the negative electrode active material, electrolyte, conductive assistant, binder, and the like in the negative electrode active material layer 30 may be appropriately determined according to the intended battery performance. The shape of the negative electrode active material layer 30 is not particularly limited, and may be, for example, a sheet-like negative electrode active material layer having a substantially flat surface. The thickness of the negative electrode active material layer 30 is not particularly limited, and may be, for example, 0.1 μm or more or 1 μm or more, and may be 2 mm or less or 1 mm or less. Examples of the negative electrode active material include silicon-based active materials such as Si, Si alloys, and silicon oxide; carbon-based active materials such as graphite and hard carbon; various oxide-based active materials such as lithium titanate; metallic lithium, lithium alloys, and the like. Only one type of negative electrode active material may be used alone, or two or more types may be used in combination. The electrolyte, conductive assistant, and binder that can be contained in the negative electrode active material layer 30 may be appropriately selected from, for example, those exemplified as those that can be contained in the positive electrode active material layer 10 described above.
[0025] 4.Other configurations As shown in FIG. 1, the secondary battery 100 may include a positive electrode collector 40 electrically connected to the positive electrode active material layer 10 and a negative electrode collector 50 electrically connected to the negative electrode active material layer 30. A known configuration may be adopted as the configuration of the collector. In addition to the above configuration, the secondary battery 100 may include a general configuration as a secondary battery. For example, a tab or a terminal. The secondary battery 100 may be one in which each of the above configurations is housed inside an exterior body. Any known exterior body for a battery can be adopted as the exterior body. In addition, a plurality of batteries 100 may be electrically connected in any way and stacked in any way to form a battery pack. Examples of the shape of the secondary battery 100 include a coin type, a laminate type, a cylindrical type, and a square type. The secondary battery 100 can be manufactured, for example, through a process of forming each of the above layers in a dry or wet manner. EXAMPLES
[0026] The technology of the present disclosure will be described in more detail below with reference to examples, but the technology of the present disclosure is not limited to the following examples.
[0027] 1. Preparation of Positive Electrode Active Material 1.1 Preparation of precursor particles MnSO4·5H2O, NiSO4·6H2O and CoSO4·7H2O were weighed out to obtain the desired composition ratio, and dissolved in distilled water to a concentration of 1.2 mol / L to obtain the first liquid. In a separate container, Na2CO3 was dissolved in distilled water to a concentration of 1.2 mol / L to obtain the second liquid. Next, 500 mL of the first and second liquids were dropped at a rate of about 4 mL / min into a reaction container that had already been filled with 1000 mL of pure water. After the dropwise addition, the mixture was stirred at room temperature for 1 h at a stirring speed of 150 rpm. The precipitate was washed with pure water and separated into solid and liquid using a centrifuge. The obtained precipitate was dried overnight at 120°C, crushed in a mortar, and fine particles were removed by air classification to obtain precursor particles containing Mn, Ni and Co.
[0028] 1.2 Preparation of coated particles Na2CO3 was dissolved in distilled water to prepare an aqueous solution of Na2CO3. The precursor particles were mixed into the aqueous solution of Na2CO3 to obtain a slurry. The Na2CO3 and the precursor particles were dried and then mixed with Na 0.7 Mn 0.5 Ni 0.2 Co 0.3 The mixture was mixed so as to have a composition of 0.02. The obtained slurry was dried by spray drying. Specifically, a DL410 spray dryer was used, with a slurry delivery rate of 30 mL / min, an inlet temperature of 200°C, and a circulating air volume of 0.8 m 3 The surfaces of the above precursor particles were coated with Na2CO3 at a spray air pressure of 0.3 MPa, to obtain coated particles.
[0029] 1.3 Preparation of Na-containing oxides with P2 structure The coated particles were fired in an electric furnace using an alumina crucible under an atmospheric air. Specifically, the alumina crucible containing the coated particles was placed in an electric furnace, and the "first heating step", "pre-firing step", "second heating step", "main firing step", "in-furnace cooling step" and "out-furnace cooling step" shown in Table 1 below were carried out. The "in-furnace cooling step" refers to a cooling step in an electric furnace, and the "out-furnace cooling step" refers to a step of cooling outside the electric furnace. Thereafter, the particles were pulverized in a mortar at a dew point of -30°C or lower to obtain a Na-containing oxide (Na 0.7 Mn 0.5 Ni 0.2 Co 0.3 O2) was obtained.
[0030] [Table 1]
[0031] 1.4 Ion exchange LiNO3 and LiCl were weighed out to have a molar ratio of 50:50, and mixed with the above-mentioned Na-containing oxide in a molar ratio that was 10 times the minimum Li amount required for ion exchange to obtain a mixture. Next, the mixture was fired at 280°C for 1 hour in an alumina crucible under air. The salt remaining after firing was washed with pure water and subjected to solid-liquid separation by vacuum filtration. The obtained precipitate was dried overnight at 120°C to obtain the Li-containing oxide (Li 0.6 Mn 0.5 Ni 0.2 Co 0.3 When the Li-containing oxide was subjected to X-ray diffraction measurement, it was found that the Li-containing oxide had an O2 type structure as a crystal structure.
[0032] 2. Preparation of Positive Electrode The above positive electrode active material, the solid electrolyte shown in Table 2 below, vapor grown carbon fiber (VGCF), a PVdF-based binder, and butyl butyrate were stirred and mixed by an ultrasonic dispersion device to obtain a positive electrode slurry. Here, the mass ratio of the positive electrode active material, the solid electrolyte, the VGCF, and the PVdF-based binder was positive electrode active material: solid electrolyte: VGCF: PVdF-based binder = 82.1: 14.9: 2.5: 0.6. The obtained positive electrode slurry was applied onto an Al foil as a positive electrode current collector by a blade method, and dried on a hot plate at 120 ° C for 30 minutes to obtain a positive electrode having a positive electrode active material layer and a positive electrode current collector.
[0033] 3. Preparation of the Negative Electrode A negative electrode slurry was obtained by stirring and mixing lithium titanate as a negative electrode active material, a sulfide solid electrolyte (Li2S-P2S5-LiI-LiBr), VGCF, a PVdF-based binder, and butyl butyrate using an ultrasonic dispersion device. Here, the mass ratio of the negative electrode active material, the sulfide solid electrolyte, the VGCF, and the PVdF-based binder was negative electrode active material:sulfide solid electrolyte:VGCF:PVdF-based binder=72.1:22.7:1.7:3.5. The obtained positive electrode slurry was applied onto Ni foil as a negative electrode current collector by a blade method, and dried on a hot plate at 120°C for 30 minutes to obtain a negative electrode having a negative electrode active material layer and a negative electrode current collector.
[0034] 4. Preparation of Solid Electrolyte Layer A solid electrolyte slurry was obtained by stirring and mixing the sulfide solid electrolyte (Li2S-P2S5-LiI-LiBr), PVdF-based binder, and butyl butyrate using an ultrasonic dispersion device. The mass ratio of the sulfide solid electrolyte to the PVdF-based binder was sulfide solid electrolyte:PVdF-based binder=99.4:0.4. The obtained solid electrolyte slurry was applied onto Ni foil as a substrate by the blade method, and dried on a hot plate at 120°C for 30 minutes to obtain a transfer laminate having a solid electrolyte layer on the surface of the substrate.
[0035] 5. Preparation of Evaluation Batteries The positive electrode active material layer of the positive electrode and the solid electrolyte layer of the transfer laminate were overlapped and pressed with a roll press at a pressure of 50 kN / cm and a temperature of 160°C. The Al foil as the substrate was then peeled off and a 1 cm 2 By punching out the sheet to a size of 100 mm, a positive electrode laminate having a structure of a positive electrode current collector, a positive electrode active material layer, and a solid electrolyte layer was obtained.
[0036] The negative electrode active material layer of the negative electrode and the solid electrolyte layer of the transfer laminate were overlapped and pressed with a roll press at a pressure of 50 kN / cm and a temperature of 160°C. The Al foil as the base material was then peeled off to obtain a first negative electrode laminate having a configuration of solid electrolyte layer / negative electrode active material layer / negative electrode current collector.
[0037] The solid electrolyte layer of the transfer laminate was further superimposed on the solid electrolyte layer side of the first negative electrode laminate, and the laminate was pre-pressed with a flat uniaxial press at a pressure of 100 MPa and a temperature of 25° C., after which the Al foil as the substrate was peeled off, and a 1.08 cm 2 By punching out the laminate to a size of 100 mm, a second negative electrode laminate having a structure of solid electrolyte layer / solid electrolyte layer / negative electrode active material layer / negative electrode current collector was obtained.
[0038] The above positive electrode laminate and the second negative electrode laminate were laminated such that the solid electrolyte layers overlapped each other, and pressed with a flat uniaxial press at a pressure of 200 MPa and a temperature of 120°C, to obtain a battery laminate having a configuration of positive electrode current collector / positive electrode active material layer / solid electrolyte layer / solid electrolyte layer / solid electrolyte layer / negative electrode active material layer / negative electrode current collector.
[0039] The above battery laminate was sandwiched between a laminate material having a positive electrode tab and a laminate material having a negative electrode tab, and heat sealed under vacuum to obtain an all-solid-state battery for evaluation.
[0040] 6. Battery evaluation The obtained all-solid-state battery was sandwiched between two restraining plates, and these two restraining plates were clamped with a clamping tool at a restraining pressure of 5 MPa to fix the distance between these two restraining plates. The all-solid-state battery thus restrained was subjected to three sets of constant current charging and discharging at 1 / 10C and constant voltage charging and discharging to a final current of 1 / 100C in the voltage range from 0.45V to 3.25V. Thereafter, constant current charging at 1 / 10C to 3.25V and constant voltage charging to a final current of 1 / 100C were performed, and further, constant current discharging at 1 / 10C to 2.5V and constant voltage discharging to a final current of 1 / 100C were performed to adjust the SOC. The all-solid-state battery after the SOC adjustment was subjected to a constant current discharge of 3C for 10s, and the initial resistance value was calculated by dividing the difference between the voltage before discharge and the voltage at the end of discharge by the current value.
[0041] After measuring the initial resistance, 300 cycles of constant current charging and discharging at 2C were performed in the voltage range from 0.45V to 3.0V to obtain an all-solid-state battery after durability testing. After that, constant current charging at 1 / 10C up to 3.25V and constant voltage charging up to a cut-off current of 1 / 100C were performed, followed by constant current discharging at 1 / 10C up to 2.5V and constant voltage discharging up to a cut-off current of 1 / 100C to adjust the SOC after durability testing. The all-solid-state battery after durability testing was subjected to constant current discharging at 3C for 10s, and the resistance value after durability testing was calculated by dividing the difference between the voltage before discharge and the voltage at the end of discharge by the current value.
[0042] Based on the initial resistance value and the resistance value after durability measured as described above, the resistance increase rate was calculated from the following formula. Resistance increase rate (%) = Resistance after durability (Ω) / Initial resistance (Ω) x 100
[0043] 7. Evaluation Results The chemical composition of the solid electrolyte used in the positive electrode active material layer, the Young's modulus at 25° C., and the resistance increase rate of the evaluation battery are shown in Table 2. In Table 2, the resistance increase rate of the battery according to Example 3 is taken as the reference (100%), and the resistance increase rates of the batteries according to Examples 1 and 2 and Comparative Examples 1 to 3 are shown relative to each other.
[0044] [Table 2]
[0045] FIG. 2 shows the relationship between the Young's modulus of the solid electrolyte contained in the positive electrode active material layer of the evaluation battery and the resistance increase rate of the evaluation battery. From the results shown in Table 2 and FIG. 2, the following can be seen. First, from a comparison between Examples 1 to 3 and Comparative Examples 1 and 2, it can be seen that when the Young's modulus of the inorganic solid electrolyte contained in the positive electrode active material layer is 30 GPa or less, the resistance increase rate is significantly lower than when the Young's modulus exceeds 30 GPa. The positive electrode active material having an O2 type structure has a large volume change during charging and discharging, and it is considered that the contact between the inorganic solid electrolyte and the positive electrode active material is reduced by repeating contraction and expansion, and the resistance increases. Here, when the Young's modulus of the inorganic solid electrolyte is large, it is considered that the solid electrolyte does not easily follow the volume change of the positive electrode active material, and the voids in the positive electrode active material layer increase, which is considered to lead to an increase in resistance. On the other hand, when the Young's modulus of the inorganic solid electrolyte is small, it is considered that the inorganic solid electrolyte follows the volume change of the positive electrode active material, and the voids in the positive electrode active material layer are reduced. The results of the present Examples 1 to 3 show that when the Young's modulus of the inorganic solid electrolyte contained in the positive electrode active material layer is 30 GPa or less, even if the volume of the positive electrode active material changes, the inorganic solid electrolyte can easily deform, and the increase in voids in the positive electrode active material layer can be suppressed. In addition, in Comparative Example 3, an organic polymer electrolyte is used as the solid electrolyte contained in the positive electrode active material layer. In Comparative Example 3, the resistance increases significantly, even though the Young's modulus of the solid electrolyte contained in the positive electrode active material layer is small. It is considered that the organic polymer electrolyte breaks due to the volume change of the active material, and the ion conduction path is interrupted, resulting in an increase in resistance.
[0046] 8. Supplementary Information In the above examples, a positive electrode active material having an O2 type structure is exemplified as having a specific chemical composition, but the chemical composition of the positive electrode active material having an O2 type structure is not limited to this. In addition, in the above examples, an inorganic solid electrolyte contained in the positive electrode active material layer is exemplified as containing Li, P, S and a halogen element, but the chemical composition of the inorganic solid electrolyte contained in the positive electrode active material layer is not limited to this, and it is considered that the same effect is exhibited as long as the inorganic solid electrolyte has a Young's modulus of 30 GPa or less. In addition, in the above examples, an all-solid-state battery is exemplified as the battery for evaluation, but as long as the positive electrode active material having an O2 type structure and the inorganic solid electrolyte having a small Young's modulus are used in combination in the positive electrode active material layer, the other configurations are not limited. Even in a secondary battery containing a liquid in a part, it is considered that the same effect is exhibited as long as the positive electrode active material having an O2 type structure and the inorganic solid electrolyte having a small Young's modulus are used in combination in the positive electrode active material layer.
[0047] 9. Summary From the above results, it can be said that a secondary battery having the following configuration can reduce an increase in resistance when repeatedly charged and discharged. (1) The secondary battery has a positive electrode active material layer, a solid electrolyte layer, and a negative electrode active material layer. (2) The positive electrode active material layer contains a positive electrode active material having an O2 type structure. (3) The positive electrode active material layer contains an inorganic solid electrolyte having a Young's modulus of 30 GPa or less. [Explanation of symbols]
[0048] 10 Cathode active material layer 20 Solid electrolyte layer 30 Negative electrode active material layer 40 Positive electrode current collector 50 Negative electrode current collector 100 Secondary battery
Claims
1. A secondary battery having a positive electrode active material layer, a solid electrolyte layer, and a negative electrode active material layer, the positive electrode active material layer contains a positive electrode active material having an O2 type structure, The positive electrode active material layer contains an inorganic solid electrolyte having a Young's modulus of 30 GPa or less. Secondary battery.
2. 2. The secondary battery according to claim 1, The positive electrode active material contains, as constituent elements, at least one transition metal element selected from Mn, Ni, and Co, Li, and O. Secondary battery.
3. 3. The secondary battery according to claim 2, The positive electrode active material is Li a Na b Mn x-p Ni y-q Co z-r M p+q+r O 2 (wherein 0<a≦1.00, 0≦b≦0.20, x+y+z=1, and 0≦p+q+r≦0.15; and element M is at least one selected from B, Mg, Al, K, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, and W), Secondary battery.
4. 2. The secondary battery according to claim 1, The inorganic solid electrolyte contains at least Li, P, S and a halogen element as constituent elements; Secondary battery.
5. The secondary battery according to any one of claims 1 to 4, The Young's modulus of the inorganic solid electrolyte is 10 GPa or more and 30 GPa or less. Secondary battery.
Citation Information
Patent Citations
Method for producing positive electrode active material and method for manufacturing lithium ion battery
JP2021068555A
Method for producing positive electrode active material and method for manufacturing lithium ion battery
JP2021068556A
All-solid secondary battery
JP2021077643A
Negative electrode and all-solid-state secondary battery including the same
JP2021132031A
Electrode for all-solid battery and all-solid battery
JP2021144924A