Aluminum alloy sheet for tab

The aluminum alloy plate with controlled Si, Fe, Cu, Mn, and Mg contents addresses the challenge of achieving high tab bending strength and toughness, enabling efficient recycling and reduced CO2 emissions by blending scrap materials.

JP2024153482AActive Publication Date: 2024-10-29UACJ CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023067404
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-10-29
Estimated Expiration
2043-04-17

AI Technical Summary

Technical Problem

Conventional aluminum alloy plates for tabs face challenges in achieving both high tab bending strength and toughness, particularly when recycling scrap materials from can bodies, leading to issues like increased risk of tab breakage and material failure during can opening.

Method used

An aluminum alloy plate composition with specific ranges of silicon (Si), iron (Fe), copper (Cu), manganese (Mn), and magnesium (Mg) contents, along with a thickness-tensile strength relationship, ensuring high tab bending strength and toughness while allowing for blending of scrap materials.

Benefits of technology

The alloy achieves both high tab bending strength and toughness, reducing the need for new metal usage and CO2 emissions by incorporating recycled 3104 aluminum alloy scraps, while maintaining formability and opening properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153482000007
    Figure 2024153482000007
  • Figure 2024153482000008
    Figure 2024153482000008
  • Figure 2024153482000009
    Figure 2024153482000009
Patent Text Reader

Abstract

To provide an aluminum alloy sheet for a tab having both high tab break strength and high toughness while blending a scrap raw material derived from a can material.SOLUTION: An aluminum alloy sheet for a can top has a composition comprising 0.10 mass% or more and 0.60 mass% or less of Si, 0.20 mass% or more and 0.70 mass% or less of Fe, 0.10 mass% or more and 0.40 mass% or less of Cu, 0.5 mass% or more and 1.2 mass% or less of Mn, 1.1 mass% or more and 4.0 mass% or less of Mg, and the balance of Al and inevitable impurities, where a sheet thickness t (mm) and a tensile strength σB_0° (MPa) in a 0° direction to a rolling direction satisfy the following formula (1). (2.7×t-0.45)×σB_0°≥67...(1).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an aluminum alloy sheet for a tab. [Background technology]

[0002] In recent years, with the rise in environmental awareness, there is a demand for aluminum alloy sheets with low CO2 emissions during the manufacturing process. In the aluminum manufacturing process, the compounding of new aluminum ingots in the casting process indirectly contributes greatly to CO2 emissions.

[0003] The production of primary aluminum ingots uses a large amount of electricity during the refining process, which leads to large amounts of CO2 emissions. Therefore, reducing the amount of primary aluminum ingots mixed and increasing the horizontal recycling rate will lead to a reduction in CO2 emissions in the production of aluminum alloy sheets.

[0004] It is generally said that CO2 emissions from remelting and casting aluminum scrap can be reduced to about one-thirtieth of that from producing new aluminum ingots. In particular, the production volume of aluminum alloy sheets for beverage cans used around the world is extremely large, and further improving the horizontal recycling rate of these sheets has great significance in reducing the environmental impact.

[0005] Among these, tabs, which are mainly made of 5182 aluminum alloy (AA5182 alloy), have lower upper limits of the composition standards for Si, Fe, Cu, Mn, etc. than can bodies made of 3104 aluminum alloy (AA3104 alloy), making it difficult to mix scrap derived from can materials that contain 3104 aluminum alloy.

[0006] For example, if can scrap (UBC: Used Beverage Can) generated in the city is mixed as is, the weight ratio of the can body to the can lid will result in a higher content of 3104 aluminum alloy components, which will easily exceed the upper limit of the content of 5182 aluminum alloy, making it necessary to dilute the components with virgin metal.

[0007] Therefore, compared to aluminum alloy sheets for can bodies, aluminum alloy sheets for tabs use more virgin metal and are adjusted to have the composition of 5182 aluminum alloy, and the recycling rate is low. Therefore, by changing the tab to an alloy whose composition is easily mixed with 3104 aluminum alloy, the usage rate of virgin metal for the tab can be significantly reduced.

[0008] Patent Documents 1 to 4 disclose aluminum alloy sheets for tabs having improved formability or openability. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Japanese Patent Application Publication No. 5-263175 [Patent Document 2] JP 2017-066458 A [Patent Document 3] JP 2017-166052 A [Patent Document 4] JP 2011-225977 A Summary of the Invention [Problem to be solved by the invention]

[0010] The problem with using an alloy for the tab with a composition similar to that of 3104 aluminum alloy is that it reduces the tab break strength and material toughness. Tab break strength is an index that indicates how difficult it is for the tab to break when the can is opened.

[0011] Generally, the greater the plate thickness and the greater the material strength, the greater the tab fracture strength. For this reason, high-strength 5182 aluminum alloy with a high Mg content is used for the tabs.

[0012] In contrast, if the conventional 3104 aluminum alloy is used for the tab, the tab breakage strength is significantly reduced, and the tab breaks when opening the can, which increases the risk of causing defects. Also, if the plate thickness is made too thick in order to increase the tab breakage strength, it will lead to an increase in the tab weight and cost.

[0013] The toughness of the material also affects the formability and opening ability of the tab. If the material has low toughness, forming cracks may occur, especially in the bent portion of the tab. Also, the base of the tab may tear when opening the tab, and the tab may separate when repeatedly opened.

[0014] However, conventional aluminum alloy sheets for tabs having recyclability do not satisfy either or both of the above two issues, that is, tab breaking strength and toughness (formability and openability).

[0015] An object of one aspect of the present disclosure is to provide an aluminum alloy sheet for tabs that can achieve both high tab breaking strength and high toughness while incorporating scrap raw material derived from can stock. [Means for solving the problem]

[0016] In one embodiment of the present disclosure, the silicon (Si) content is 0.10 mass% or more and 0.60 mass% or less, the iron (Fe) content is 0.20 mass% or more and 0.70 mass% or less, the copper (Cu) content is 0.10 mass% or more and 0.40 mass% or less, the manganese (Mn) content is 0.5 mass% or more and 1.2 mass% or less, the magnesium (Mg) content is 1.1 mass% or more and 4.0 mass% or less, the balance being aluminum (Al) and unavoidable impurities, and B_0° (MPa) satisfies the following formula (1):

[0017] (2.7×t-0.45)×σ B_0° ≧67 (1) According to this configuration, it is possible to obtain both high tab breaking strength and high toughness in the aluminum alloy sheet while blending scrap raw material derived from can material. That is, it is possible to blend a certain amount or more of 3104 aluminum alloy scrap for can body, and it is possible to reduce the usage rate of new ingots and reduce CO2 emissions. Furthermore, it is possible to obtain an aluminum alloy sheet for tabs that has both formability and openability. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is an explanatory diagram of the L-ST cross section. [Diagram 2] FIG. 2A is a schematic perspective view of the Erichsen Cup, and FIG. 2B is a schematic plan view of the Erichsen Cup. [Diagram 3] FIG. 3 is a graph showing an example of the measurement results of the sidewall height of the Erichsen Cup. [Figure 4] FIG. 4 is a graph showing the relationship between the value V and the tab bending strength in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, embodiments to which the present disclosure is applied will be described with reference to the drawings. [1. First embodiment] [1-1. Configuration] <Composition> The aluminum alloy sheet for tabs (hereinafter also simply referred to as "alloy sheet") of the present disclosure contains aluminum (Al), silicon (Si), iron (Fe), copper (Cu), manganese (Mn), and magnesium (Mg).

[0020] The lower limit of the Si content is 0.10 mass%, preferably 0.20 mass%. If the Si content is less than 0.10 mass%, the amount of Si precipitated in the processing heat of the hot rolling and the cold rolling after the solution treatment decreases, and the tensile strength of the alloy sheet may be insufficient.

[0021] In addition, the average value of the Si content standard of the 3104 aluminum alloy specified in JIS-H-4000:2014 is 0.30 mass%, and the average value of the Si content standard of the 5182 aluminum alloy specified in JIS-H-4000:2014 is 0.10 mass%. Therefore, by making the Si content 0.20 mass% or more, a large amount of 3104 aluminum alloy scrap can be blended.

[0022] The upper limit of the Si content is 0.60 mass%, and preferably 0.40 mass%. If the Si content exceeds 0.60 mass%, the number of Mg2Si particles increases, and the toughness of the alloy plate decreases.

[0023] The lower limit of the Fe content is 0.20% by mass, and preferably 0.30% by mass. The average Fe content standard of 3104 aluminum alloy is 0.40% by mass, and the average Fe content standard of 5182 aluminum alloy is 0.18% by mass. Therefore, by making the Fe content 0.20% by mass or more, a large amount of 3104 aluminum alloy scrap can be blended.

[0024] The upper limit of the Fe content is 0.70 mass%. If the Fe content exceeds 0.70 mass%, the amount of Al-Fe-Mn or Al-Fe-Mn-Si intermetallic compounds (i.e., second phase particles) increases. As a result, a crack propagation path is generated, and the toughness of the alloy plate decreases.

[0025] The lower limit of the Cu content is 0.10 mass%, preferably 0.11 mass%, and more preferably 0.20 mass%. If the Cu content is less than 0.10 mass%, the amount of Cu that increases the tensile strength by solid solution or precipitation is insufficient, and the tensile strength of the alloy sheet is reduced. Note that the tensile strength of the alloy sheet is significantly increased by precipitating Cu during the processing of hot rolling and cold rolling after solution treatment.

[0026] In addition, the average Cu content of the 3104 aluminum alloy is 0.15% by mass, and the average Cu content of the 5182 aluminum alloy is 0.075% by mass. Therefore, by making the Cu content 0.11% by mass or more, a large amount of 3104 aluminum alloy scrap can be blended.

[0027] The upper limit of the Cu content is 0.40 mass %. If the Cu content exceeds 0.40 mass %, the toughness of the alloy plate decreases.

[0028] The lower limit of the Mn content is 0.5 mass%, preferably 0.7 mass%, and more preferably 0.8 mass%. If the Mn content is less than 0.5 mass%, there is insufficient Mn that increases the tensile strength by solid solution or precipitation, and the tensile strength of the alloy sheet decreases.

[0029] In addition, the average value of the Mn content standard of the 3104 aluminum alloy is 1.1 mass%, and the average value of the Mn content standard of the 5182 aluminum alloy is 0.35 mass%. Therefore, by making the Mn content 0.7 mass% or more, a large amount of 3104 aluminum alloy scrap can be blended.

[0030] The upper limit of the Mn content is 1.2 mass%, and preferably 1.0 mass%. If the Mn content exceeds 1.2 mass%, the amount of Al-Fe-Mn or Al-Fe-Mn-Si intermetallic compounds (i.e., second phase particles) increases. As a result, a crack propagation path is generated, and the toughness of the alloy plate decreases.

[0031] The lower limit of the Mg content is 1.1 mass%. If the Mg content is less than 1.1 mass%, the amount of Mg that increases the tensile strength by solid solution or precipitation is insufficient, and the tensile strength of the alloy sheet decreases. Note that the tensile strength of the alloy sheet is significantly increased by precipitating Mg during hot rolling and cold rolling after solution treatment.

[0032] The upper limit of the Mg content is 4.0% by mass, and preferably 3.0% by mass. The average value of the Mg content standard of 3104 aluminum alloy is 1.05% by mass, and the average value of the Mg content standard of 5182 aluminum alloy is 4.5% by mass. Therefore, by making the Mg content 4.0% by mass or less, preferably 3.0% by mass or less, it is possible to reduce the amount of additional Mg-containing raw material while adding a large amount of 3104 aluminum alloy scrap.

[0033] The alloy plate may contain titanium (Ti). The upper limit of the Ti content is preferably 0.10 mass%. The ingot structure of the alloy plate is refined by containing Ti. If the Ti content exceeds 0.10 mass%, coarse crystals are generated during casting, and the toughness of the alloy plate is significantly reduced.

[0034] The alloy sheet may also contain zinc (Zn). The upper limit of the Zn content is preferably 0.25 mass %. If the Zn content exceeds 0.25 mass %, the corrosion resistance of the alloy sheet deteriorates.

[0035] Furthermore, the alloy plate may contain chromium (Cr). The upper limit of the Cr content is preferably 0.10 mass%. If the Cr content exceeds 0.10 mass%, coarse crystals are generated during casting, and the toughness of the alloy plate is significantly reduced.

[0036] The alloy plate may contain unavoidable impurities to the extent that the performance of the alloy plate is not significantly impaired. That is, the alloy plate contains Si, Fe, Cu, Mn, Mg, Ti, Zn, and Cr in the above-mentioned ranges, with the balance being aluminum and unavoidable impurities. The upper limit of the total amount of unavoidable impurities is preferably 0.15 mass%.

[0037] <Thickness, material strength and tab bending strength> In the alloy sheet of the present disclosure, the sheet thickness t (mm) and the tensile strength σ B_0° (MPa) satisfies the following formula (1). V = (2.7 × t - 0.45) × σ B_0° ≧67 (1)

[0038] Tensile strength σ in formula (1) B_0° is measured by the method specified in JIS-Z-2241: 2011. The plate thickness t is measured, for example, with a micro gauge.

[0039] Empirically, the value of the tab breaking strength of an aluminum alloy tab has a strong positive correlation with the value V (i.e., the left side of formula (1)). Therefore, when the value V is 67 or more, a tab with sufficient tab breaking strength can be formed.

[0040] In addition, the tensile strength σ B_0° It is preferable that the tab bending strength is 330 MPa or more. This makes it possible to form a tab having a sufficient tab bending strength without significantly increasing the plate thickness of the alloy plate.

[0041] The mechanical meaning of the relationship between the V value and the tab breaking strength can be explained as follows: When the tab is pulled up to open a can, if the resistance of the tab to the load applied to it is low, plastic deformation will begin due to localized material yielding before the score is opened normally. Tab breaking is a phenomenon in which the tab bends as this plastic deformation progresses.

[0042] Considering the cross section parallel to the bending ridge at the position where the tab bends, the resistance to the bending moment applied to the cross section by the tab being pulled up is calculated by the section modulus, which is a value specific to the cross-sectional shape, and the 0.2% yield strength σ 0.2 The higher the value, the larger the

[0043] The section modulus in the above cross section increases with thickness if the tab has a fixed shape, such as the typical DRT type stay-on tab. Therefore, the ease with which the material yields and bending due to plastic deformation begins in a tab break is determined by the plate thickness and the material's 0.2% yield strength σ 0.2 This can be explained by the following.

[0044] In addition, since the tab breakage is a phenomenon that includes the progress of plastic deformation and the bending of the tab, it is necessary to take into account the work hardening of the material during plastic deformation. 0.2% yield strength σ 0.2 Even if the strain rate is low and plastic deformation begins early, if the amount of work hardening during plastic deformation is large, the progress of plastic deformation is suppressed and the tab is less likely to bend.

[0045] Therefore, 0.2% yield strength σ 0.2 Instead of tensile strength, σ is used as an index of material strength including work hardening. B_0° is introduced, and the plate thickness t and tensile strength σ B_0° The tab breaking property of the aluminum alloy sheet can be evaluated by using the value V expressed by

[0046] The tab breaking strength of an aluminum alloy plate is measured, for example, by the following procedure. A shell formed from an aluminum alloy plate is subjected to conversion processing other than scoring, and a can lid is formed as an end without scores. A tab formed from an aluminum alloy plate is then attached to the can lid. The can lid is fixed to a jig, and the tab is pulled up. The maximum load applied to the pulled-up portion at this time is taken as the tab breaking strength.

[0047] Specifically, a typical DRT type stay-on-tab shaped tab mold is used to mold the tab. A φ204 Fullform (B64) shaped shell mold, for example, is used to mold the shell. A pop-tear tester from Reed Instruments, Ltd. is used to measure the tab breaking strength.

[0048] More specifically, a can lid with no score and a tab attached, which is formed using a special jig, is fixed to the jig. A load-applying jig is then attached to the tab-pulling portion, and the load-applying jig is fixed in place while applying a load in a direction perpendicular to the panel portion of the lid such that the tab does not undergo plastic deformation. In this state, the lid is rotated at a rotation speed of 30° / sec to pull up and bend the tab. The maximum load applied to the tab-pulling portion is read within a rotation angle range of up to 90°.

[0049] <Toughness> It is known that the formability and openability of the tab are affected by the toughness of the aluminum alloy plate.

[0050] (Number of repeated bending) A repeated bending test is one of the evaluation indices for the toughness of an aluminum alloy plate. If the plate thickness is the same, the more repeated bending times the aluminum alloy plate is subjected to, the more excellent the toughness of the aluminum alloy plate is.

[0051] The repeated bending test is carried out as follows. For example, a test piece cut into a rectangular shape with a width of 12.5 mm and a length of 200 mm is placed so that the bending ridgeline is parallel to the rolling direction of the alloy plate. Both ends of the test piece are fixed with chucks, and a tension of 200 N is applied.

[0052] In this state, the test piece is repeatedly bent by rotating the other chuck 90° left and right, using a jig with a bending radius of 2.0 mm positioned 150 mm in the longitudinal direction of the test piece as a fulcrum from the end of the test piece fixed to one of the immovable chucks, and the number of bends until the test piece breaks is measured.

[0053] The number of bending operations is counted as one each for bending 90° to either the left or right and returning to the original position. If the specimen breaks during bending, the angle Θ (0°-90°) is read and the number of repeated bending cycles N is calculated using the following formula (3). In formula (3), N0 is the total number of times the specimen is bent 90° to either the left or right and returned from the 90° bent position to the original 0° position before it breaks. N = N0 + Θ / 90 (3)

[0054] Repeated bending evaluation is more disadvantageous as the plate thickness increases, so it is necessary to correct for the standard plate thickness. Therefore, the normalized repeated bending times N was normalized by the following formula (3) using a plate thickness of 0.245 mm as the standard. s In addition, t t (mm) is the thickness of the test piece. N s = N × t t / 0.245 ···(3)

[0055] (second phase particles) Toughness is affected by tensile strength and distribution of second phase particles. In other words, the higher the tensile strength and the higher the density of second phase particles, the lower the toughness. In particular, when the Mg and Si contents are high, Mg2Si particles are more likely to form. As a result, the Mg2Si particles become the starting point and propagation path of cracks, which affects the decrease in toughness.

[0056] In the aluminum alloy sheet of the present disclosure, the area of ​​the L-ST cross section shown by the diagonal line in FIG. 2 The ratio of the total area of ​​the above Mg2Si particles is preferably 1.0% or less. In Fig. 1, L indicates the longitudinal direction, ST indicates the plate thickness direction, and LT indicates the width direction.

[0057] The area ratio of Mg2Si particles can be measured, for example, by the following method. First, the measurement sample is cut and the surface to be measured (i.e., the L-ST cross section) is mechanically polished to a mirror finish. Next, the polished surface (i.e., the L-ST cross section) is observed using a SEM (scanning electron microscope) to obtain 10 fields of view in the central region of the plate thickness. The accelerating voltage of the SEM is 15 kV, the magnification is 500 times, and the range of one field of view is 0.049 mm 2 The image is then taken and a COMPO (backscattered electron composition) image is obtained.

[0058] The captured COMPO image is analyzed using the image analysis software "ImageJ." Specifically, the most frequent brightness value of the image in 256 gradations is taken as the background brightness, and particles with brightness lower than the brightness of the most frequent value minus 30 are determined to be Mg2Si particles.

[0059] Among the determined Mg2Si particles, 0.3 μm 2 The total area of ​​particles with an area of ​​0.3 μm or more was calculated and divided by the area of ​​10 fields of view (i.e., the total area photographed). 2 The ratio of the total area of ​​the above Mg2Si particles in the L-ST cross section is calculated.

[0060] (Ear rate) The number of repeated bending cycles also affects the texture, and the higher the concentration of cube orientation, the better. The concentration of cube orientation is reflected in the shape of the ears of the Erichsen cup E formed from an aluminum alloy sheet by the Erichsen test, as shown in Figures 2A and 2B.

[0061] Specifically, it is suggested that the greater the relative sidewall height H in the 0° / 180° direction with respect to the rolling direction RD with respect to the sidewall height H (i.e., ear height) in the 45° direction with respect to the rolling direction RD of the aluminum alloy sheet of Erichsen Cup E, the higher the degree of accumulation of cube orientation. That is, the aluminum alloy sheet of the present disclosure includes those having a relatively large degree of accumulation of cube orientation and a high sidewall height H in the 0° / 180° direction.

[0062] The relative sidewall height in the 0° / 180° direction to the sidewall height in the 45° direction can be evaluated using an index called earing balance. The procedure for measuring the earing balance is explained below.

[0063] The ear ratio is expressed by the left side of the following equation (4). (h 0p -h 45p ) / h v ×100≧-7.0 (4)

[0064] In formula (4), h 0p is the average value of the maximum sidewall heights in the first region A1 around 0° and the second region A2 around 180° with respect to the rolling direction. The first region A1 is, for example, in the range of 0°±11° with respect to the rolling direction. The second region A2 is, for example, in the range of 180°±11° with respect to the rolling direction.

[0065] h 45p is the average value of the maximum sidewall heights in the third region A3 around 45°, the fourth region A4 around 135°, the fifth region A5 around 225°, and the sixth region A6 around 315° with respect to the rolling direction.

[0066] The third region A3 is, for example, in the range of 45°±22° with respect to the rolling direction. The fourth region A4 is, for example, in the range of 135°±22° with respect to the rolling direction. The fifth region A5 is, for example, in the range of 225°±22° with respect to the rolling direction. The sixth region A6 is, for example, in the range of 315°±22° with respect to the rolling direction.

[0067] h v is the average value of the minimum side wall height in each of the seventh region A7 from 0° to 45°, the eighth region A8 from 45° to 135°, the ninth region A9 from 135° to 180°, the tenth region A10 from 180° to 225°, the eleventh region A11 from 225° to 315°, and the twelfth region A12 from 315° to 360° relative to the rolling direction.

[0068] Figure 3 is a graph showing an example of the measurement results of the sidewall height of an Erichsen cup. The angles shown in Figure 3 are angles with respect to the rolling direction. The distance from the center of the graph indicates the sidewall height.

[0069] In the figure, ad is the maximum value in the third region A3 to the sixth region A6, e and f are the maximum values ​​in the first region A1 and the second region A2, and gl is the minimum value in the seventh region A7 to the twelfth region A12.

[0070] The Erichsen Cup E is formed, for example, under the conditions of a blank diameter of 57 mm and a punch diameter of 33 mm. The sidewall height of the Erichsen Cup is measured, for example, using a Roncorder EC1550-H manufactured by Kosaka Laboratory Co., Ltd.

[0071] Specifically, a measurement probe is placed at the opening of the Erichsen cup with the rolling direction as the reference (0° / 180°), and the table on which the Erichsen cup is placed is rotated once to measure the opening height in the circumferential direction of 360°.

[0072] When formula (4) is satisfied, that is, when the earing ratio is -7.0% or more, the concentration of cube orientation increases, and as a result, the number of repeated bending cycles of the alloy sheet can be increased.

[0073] <Method of manufacturing aluminum alloy plate> The aluminum alloy plate of the present disclosure can be produced, for example, as follows: First, an aluminum alloy having the composition of the aluminum alloy plate of the present disclosure is subjected to a semi-continuous casting method (i.e., DC casting) according to a conventional method to produce an ingot.

[0074] Next, the surface of the ingot is chamfered. After that, the ingot is put into a soaking furnace and subjected to homogenization treatment. The temperature in the homogenization treatment is preferably, for example, 470° C. or more and 620° C. or less. The time for the homogenization treatment is preferably, for example, 1 hour or more and 20 hours or less.

[0075] When the homogenization temperature is 400°C or higher, segregation of the ingot structure is easily eliminated. Furthermore, when the homogenization temperature is 450°C or higher, Mg2Si particles are redissolved, and the tensile strength and toughness of the alloy plate can be improved. Furthermore, when the homogenization temperature is 490°C or higher, more preferably 550°C or higher, the redissolution of Mg2Si particles is promoted, and the tensile strength and toughness of the alloy plate can be further improved. On the other hand, when the homogenization temperature is 620°C or lower, local melting of the aluminum alloy is difficult to occur.

[0076] If the homogenization treatment time is 1 hour or more, the temperature of the entire slab becomes uniform, segregation in the ingot structure is easily eliminated, and Mg2Si particles are easily redissolved. The longer the homogenization treatment time, the more the Mg2Si particles can be redissolved. However, if the homogenization treatment time exceeds 20 hours, the effect of the homogenization treatment becomes saturated.

[0077] After the homogenization treatment, the ingot is subjected to hot rolling. The hot rolling process includes a rough rolling process and a finish rolling process. In the rough rolling process, the ingot is processed into a plate material having a thickness of about several tens of mm by reverse rolling. In the finish rolling process, the thickness of the plate material is reduced to about several mm by, for example, tandem rolling, and the plate material is wound into a coil to form a hot rolled coil.

[0078] If the total reduction rate of the finish rolling is high, the recrystallized structure will be formed after coiling, and the degree of accumulation of the cube orientation can be increased. If the coiling temperature of the finish rolling is high, the recrystallized structure will be formed after coiling, and the degree of accumulation of the cube orientation can be increased.

[0079] Also, high-strength alloy sheets can be obtained by solution treating hot-rolled coils and resolving Mg, etc. For example, heat treatment (i.e., annealing) is performed using a continuous annealing furnace at a target actual temperature of 440°C or higher for 30 seconds or more, and then forced cooling by air cooling or the like can be performed to effectively increase the tensile strength of the alloy sheet.

[0080] Following hot rolling, the plate material is cold rolled. In cold rolling, the hot rolled coil is rolled until the product plate thickness is reached. Cold rolling may be either single rolling or tandem rolling. In single cold rolling, rolling is preferably performed in multiple passes, such as two or more passes.

[0081] By setting the finishing temperature of cold rolling in the intermediate passes other than the final pass to 120°C or higher, Si, Cu and Mg are finely precipitated and age hardened, so that the tensile strength of the alloy sheet can be increased. Furthermore, by setting the finishing temperature to 130°C or higher, the tensile strength of the alloy sheet can be further increased.

[0082] The cold rolling reduction (i.e. the total reduction) is preferably 80% or more. When the cold rolling reduction is 80% or more, the tensile strength of the alloy sheet can be increased. The lower the cold rolling reduction, the more the cube orientation remains. The cold rolling reduction is preferably 92% or less.

[0083] The cold rolling reduction ratio R (%) is calculated by the following formula (5) using the plate thickness t0 (mm) of the hot rolled plate and the plate thickness t1 (mm) of the product after cold rolling. R = (t0-t1) / t0 × 100 (5)

[0084] In addition, as long as the effects of the aluminum alloy sheet of the present disclosure are exhibited, in the above-mentioned method for producing an aluminum alloy sheet, annealing may be performed, for example, before or after cold rolling or between passes.

[0085] The coil that has been cold-rolled to the product thickness may be precoated in a painting line, etc. When precoating is performed, the surface of the cold-rolled coil is degreased, washed, and subjected to a chemical conversion treatment, and further, a paint is applied, followed by a paint baking treatment.

[0086] Chemical solutions such as chromate-based and zirconium-based are used in chemical conversion treatment. Epoxy-based and polyester-based paints are used. These can be selected according to the application. In the paint baking process, the coil is heated to a peak metal temperature (PMT) of 220°C to 270°C for approximately 30 seconds or less. The lower the PMT, the more the material recovery is suppressed, and the higher the tensile strength of the alloy plate can be maintained.

[0087] [1-2. Effects] According to the embodiment described above in detail, the following effects can be obtained. (1a) It is possible to obtain both high tab breaking strength and high toughness in an aluminum alloy sheet while blending scrap raw materials derived from can stock. In other words, it is possible to blend a certain amount or more of 3104 aluminum alloy scrap for can bodies, which reduces the usage rate of new ingots and reduces CO2 emissions. Furthermore, it is possible to obtain an aluminum alloy sheet for tabs that has both formability and openability.

[0088] 2. Other embodiments Although the embodiments of the present disclosure have been described above, it goes without saying that the present disclosure is not limited to the above-described embodiments and can take various forms.

[0089] (2a) In addition to the aluminum alloy sheet of the above embodiment, the present disclosure also includes various embodiments of a member constituted by this aluminum alloy sheet, a manufacturing method of this aluminum alloy sheet, and the like.

[0090] (2b) The function of one component in the above embodiments may be distributed among multiple components, or the functions of multiple components may be integrated into one component. In addition, a part of the configuration of the above embodiments may be omitted. In addition, at least a part of the configuration of the above embodiments may be added to or substituted for the configuration of another of the above embodiments. Note that all aspects included in the technical idea identified from the wording of the claims are embodiments of the present disclosure.

[0091] 3. Working Examples The following describes the tests conducted to confirm the effects of the present disclosure and the evaluation results thereof.

[0092] <Production of aluminum alloy sheets> As examples and comparative examples, aluminum alloy sheets S1 to S21 shown in Tables 1 and 2 were produced. Specific production procedures are described below.

[0093] First, an ingot containing the components (% by mass) of Alloy Nos. 1-8 shown in Table 3, with the balance being aluminum and unavoidable impurities, was produced by semi-continuous casting. The ingot contained 0.10% by mass or less of Ti, 0.25% by mass or less of Zn, 0.10% by mass or less of Cr, and 0.15% by mass or less of unavoidable impurities.

[0094] Next, the four sides of the ingot, excluding the front and rear ends, were chamfered. The ingot was then placed in a furnace and subjected to homogenization treatment. The homogenization temperature is shown in Table 1. After the homogenization treatment, the ingot was removed from the furnace and immediately hot rolling was started to produce a rolled sheet.

[0095] The obtained rolled sheet was annealed. The annealing temperature was as shown in Table 1, and the annealing time was 30 seconds. After annealing, the rolled sheet was cooled to room temperature by air cooling. After cooling, the rolled sheet was subjected to cold rolling. The target total reduction in cold rolling was as shown in Table 1.

[0096] After cold rolling, paint was applied to the sheet surface and a paint baking treatment was performed for 30 seconds. The practical temperature (PMT) during paint baking is shown in Table 1. The aluminum alloy sheet of S1-S21 was obtained by baking the paint. The sheet thickness (i.e., product sheet thickness) of the aluminum alloy sheet of S1-S21 measured by a microgauge is also shown in Table 1.

[0097] [Table 1]

[0098] [Table 2]

[0099] [Table 3]

[0100] <Evaluation of aluminum alloy sheets> (Tensile properties) No. 5 test pieces as defined in JIS-Z-2241:2011 were prepared from the S1-S21 aluminum alloy sheets. The longitudinal direction of the test pieces was extended in a direction forming an angle of 0° with respect to the rolling direction.

[0101] A tensile test was performed on this test piece in accordance with JIS-Z-2241:2011, and the tensile strength σ B_0° The tensile strength σ B_0° The measurement results are shown in Table 2. In addition, from the measurement results of the plate thickness and tensile strength, the value of formula (1) V = (2.7 × t - 0.45) × σ B_0° The calculation results are shown in Table 2.

[0102] (Toughness) In the aluminum alloy plates of S1-S21, the area is 0.3 μm by the measurement method described in the embodiment. 2 The ratio of the total area (area ratio) of the above Mg2Si particles in the L-ST cross section was calculated. The measurement results are shown in Table 2.

[0103] For the aluminum alloy sheets S1-S21, the earing ratio was calculated from the measurement method described in the embodiment and the left side of formula (4). The results are shown in Table 2. In the table, "-" indicates that the measurement was not performed.

[0104] For the aluminum alloy sheets S1 to S21, the normalized number of repeated bending cycles was calculated from the measurement method described in the embodiment and the formulas (2) and (3). The results are shown in Table 2.

[0105] (scrap mixture ratio) Regarding the composition of the aluminum alloy plate of S1-S21, it was judged whether the possible mixing ratio of 3104 aluminum alloy scrap was 50 mass% or more. The results are shown in Table 2.

[0106] In Table 2, aluminum alloy plates marked with "≧50" can contain 50 mass% or more of 3104 aluminum alloy. The possible content of 3104 aluminum alloy scrap is determined based on Table 4.

[0107] Table 4 shows the relationship between the blend ratio of 3104 aluminum alloy and 5182 aluminum alloy and the average value of the component specifications. The first line of Table 4 shows the average value of the component specifications of 3104 aluminum alloy, and the second line shows the average value of the component specifications of 5182 aluminum alloy.

[0108] For example, when the blend ratio of 3104 aluminum alloy is 50 mass%, the average value of Si is 0.20 mass%, the average value of Fe is 0.29 mass%, the average value of Cu is 0.11 mass%, the average value of Mn is 0.7 mass%, and the average value of Mg is 2.8 mass%.

[0109] Therefore, when the ratio of each component of the aluminum alloy plate is equal to or greater than the above values ​​of Si, Fe, Cu, Mn, and Mg, the possible blending ratio of the 3104 aluminum alloy plate is 50% by mass or more. As the blending ratio of the 3104 aluminum alloy increases, the contents of Si, Fe, Cu, and Mn increase, and the content of Mg decreases. The aluminum alloy plates of S1-S21 can be blended with 50% by mass or more of the 3104 aluminum alloy scrap.

[0110] [Table 4]

[0111] (tab bending strength) In addition to the aluminum alloy plates S1 to S21, a number of aluminum alloy plates having different plate thicknesses and tensile strengths were prepared, and the tab bending strength of each was measured by the measurement method described in the embodiment.

[0112] The measurement results, the thickness t of the aluminum alloy plate, and the tensile strength σ in the 0° direction relative to the rolling direction B_0° And the value of equation (1) V = (2.7 × t - 0.45) × σ B_0° The relationship between these is shown in Table 5 and Figure 4. Table 6 shows the components of the aluminum alloy sheets used to measure the tab bending strength.

[0113] It was confirmed from Figure 4 that there is a high correlation between the value V and the tab breaking strength. Note that Figure 4 shows the results using a tab with a typical DRT type stay-on tab shape, but similar trends can be seen for tabs with other shapes.

[0114] [Table 5]

[0115] [Table 6]

[0116] As shown in Table 2, in the aluminum alloy sheets of S11-S21, the value V, which has a strong correlation with the tab breaking strength, is 67 or more, and it was confirmed that the sheet thickness and tensile strength are capable of obtaining high tab breaking strength.

Claims

1. The silicon (Si) content is 0.10% by mass or more and 0.60% by mass or less, The iron (Fe) content is 0.20 mass% or more and 0.70 mass% or less, The copper (Cu) content is 0.10 mass% or more and 0.40 mass% or less, The manganese (Mn) content is 0.5% by mass or more and 1.2% by mass or less, The magnesium (Mg) content is 1.1% by mass or more and 4.0% by mass or less, The balance is aluminum (Al) and unavoidable impurities, Plate thickness t (mm) and tensile strength σ in the direction 0° to the rolling direction B_0° (MPa) satisfies the following formula (1). (2.7×t-0.45)×σ B_0° ≧67 ・・・(1)

2. The aluminum alloy sheet for tabs according to claim 1, In the L-ST cross section, the area is 0.3 μm 2 More than Mg 2 An aluminum alloy sheet for tabs, in which the ratio of the total area of ​​Si particles is 1.0% or less.

3. The aluminum alloy sheet for tabs according to claim 1 or 2, The average value h of the maximum sidewall height in the circumferential direction of the Erichsen cup formed by the Erichsen test in the region around 0° and the region around 180° with respect to the rolling direction 0p and the average value h of the maximum sidewall height in each of the regions around 45°, 135°, 225°, and 315° with respect to the rolling direction. 45p and the average value h of the minimum sidewall height in each of the regions of 0° to 45°, 45° to 135°, 135° to 180°, 180° to 225°, 225° to 315°, and 315° to 360° with respect to the rolling direction. v and an aluminum alloy sheet for a tab, which satisfies the following formula (2): (h 0p -h 45p ) / h v ×100≧-7.0 ・・・(2)

4. The aluminum alloy sheet for tabs according to claim 1 or 2, The silicon (Si) content is 0.20% by mass or more and 0.60% by mass or less, The iron (Fe) content is 0.30 mass% or more and 0.70 mass% or less, The copper (Cu) content is 0.11 mass% or more and 0.40 mass% or less, The manganese (Mn) content is 0.7% by mass or more and 1.2% by mass or less, An aluminum alloy sheet for tabs, having a magnesium (Mg) content of 1.1 mass% or more and 3.0 mass% or less.

Citation Information

Patent Citations

  • Aluminum two piece can body and its manufacture

    JP1992221036A

  • Aluminum alloy laminate for can cover adapted to recycling and manufacture thereof

    JP1997070925A

  • Continuous casting process for low earring aluminum alloy production

    JP2002514269A

  • Zirconium hydroxide powder and manufacturing method of zirconium hydroxide powder

    JP2023067405A

  • Can lid for food or drink