Aluminum alloy sheet for tab

The aluminum alloy plate addresses the challenge of blending scrap materials by optimizing Si, Fe, Mn, and Mg contents, achieving high tab bending strength and toughness, thus reducing new metal use and emissions.

JP2024153483AActive Publication Date: 2024-10-29UACJ CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023067405
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-10-29
Estimated Expiration
2043-04-17

AI Technical Summary

Technical Problem

Existing aluminum alloy plates for tabs face challenges in achieving both high tab bending strength and toughness, particularly when blending scrap materials derived from can stock, leading to potential can opening failures and increased material costs.

Method used

An aluminum alloy plate composition with specific ranges of silicon (Si), iron (Fe), manganese (Mn), and magnesium (Mg) contents, along with a plate thickness and tensile strength relationship, allowing for the blending of scrap materials while maintaining high tab bending strength and toughness.

Benefits of technology

The solution enables the use of a significant amount of 3104 aluminum alloy scrap, reducing new metal usage and CO2 emissions, while ensuring the alloy plate achieves sufficient tab bending strength and toughness without excessive thickness or cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153483000006
    Figure 2024153483000006
  • Figure 2024153483000007
    Figure 2024153483000007
  • Figure 2024153483000008
    Figure 2024153483000008
Patent Text Reader

Abstract

To provide an aluminum alloy sheet for a tab having both high tab break strength and high toughness while blending a scrap raw material derived from a can material.SOLUTION: An aluminum alloy sheet for a can top has a composition comprising 0.20 mass% or more and 0.60 mass% or less of Si, 0.30 mass% or more and 0.70 mass% or less of Fe, 0.11 mass% or more and 0.40 mass% or less of Cu, 0.7 mass% or more and 1.2 mass% or less of Mn, and 1.1 mass% or more and 3.0 mass% or less of Mg, where a sheet thickness t (mm) and a tensile strength σB_0° (MPa) in a 0° direction to a rolling direction satisfy the following formula (1), and a rate of a total area of Mg2Si particles having an area of 0.3 μm2 or more is 0.2% or less in an L-ST section. (2.7×t-0.45)×σB_0°≥67...(1).SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an aluminum alloy sheet for a tab. [Background technology]

[0002] In recent years, with the rise in environmental awareness, there is a demand for aluminum alloy sheets with low CO2 emissions during the manufacturing process. In the aluminum manufacturing process, the compounding of new aluminum ingots in the casting process indirectly contributes greatly to CO2 emissions.

[0003] The production of primary aluminum ingots uses a large amount of electricity during the refining process, which leads to large amounts of CO2 emissions. Therefore, reducing the amount of primary aluminum ingots mixed and increasing the horizontal recycling rate will lead to a reduction in CO2 emissions in the production of aluminum alloy sheets.

[0004] It is generally said that CO2 emissions from remelting and casting aluminum scrap can be reduced to about one-thirtieth of that from producing new aluminum ingots. In particular, the production volume of aluminum alloy sheets for beverage cans used around the world is extremely large, and further improving the horizontal recycling rate of these sheets has great significance in reducing the environmental impact.

[0005] Among these, tabs, which are mainly made of 5182 aluminum alloy (AA5182 alloy), have lower upper limits of the composition standards for Si, Fe, Cu, Mn, etc. than can bodies made of 3104 aluminum alloy (AA3104 alloy), making it difficult to mix scrap derived from can materials that contain 3104 aluminum alloy.

[0006] For example, if can scrap (UBC: Used Beverage Can) generated in the city is mixed as is, the weight ratio of the can body to the can lid will result in a higher content of 3104 aluminum alloy components, which will easily exceed the upper limit of the content of 5182 aluminum alloy, making it necessary to dilute the components with virgin metal.

[0007] Therefore, compared to aluminum alloy sheets for can bodies, aluminum alloy sheets for tabs use more virgin metal and are adjusted to have the composition of 5182 aluminum alloy, and the recycling rate is low. Therefore, by changing the tab to an alloy whose composition is easily mixed with 3104 aluminum alloy, the usage rate of virgin metal for the tab can be significantly reduced.

[0008] Patent Document 1 discloses an aluminum alloy sheet for tabs that has a composition relatively close to that of 3104 aluminum alloy, which has excellent recyclability. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Japanese Patent Application Publication No. 5-263175 Summary of the Invention [Problem to be solved by the invention]

[0010] The challenge of using an alloy for the tab with a composition similar to that of 3104 aluminum alloy is that it reduces the tab breaking strength and the toughness of the material. For example, in a mechanism that uses the leverage principle to pry open the score, such as a stay-on tab, there is a risk of the tab bending during can opening, resulting in a can opening defect.

[0011] The tab bending strength is the maximum load applied to the pulled part when a can is opened and the tab is bent due to a can opening failure, and is an index of the resistance to the tab bending. Therefore, a high tab bending strength is required to prevent can opening failure.

[0012] Generally, the greater the plate thickness and the greater the material strength, the greater the tab fracture strength. For this reason, high-strength 5182 aluminum alloy with a high Mg content is used for the tabs.

[0013] In contrast, if the conventional 3104 aluminum alloy is used for the tab, the tab break strength is significantly reduced, increasing the risk of can opening defects. Also, if the plate thickness is made too thick in order to increase the tab break strength, it will lead to an increase in the tab weight and tab cost.

[0014] In addition, the toughness of the material affects the formability of the tab. If the material has low toughness, forming cracks may occur, especially in the bent portion of the tab. However, aluminum alloy sheets for tabs that are relatively close to the composition of the conventional 3104 aluminum alloy do not satisfy either or both of the above two issues, i.e., tab breaking strength and toughness (formability).

[0015] An object of one aspect of the present disclosure is to provide an aluminum alloy sheet for tabs that can achieve both high tab breaking strength and high toughness while incorporating scrap raw material derived from can stock. [Means for solving the problem]

[0016] In one embodiment of the present disclosure, the silicon (Si) content is 0.20 mass% or more and 0.60 mass% or less, the iron (Fe) content is 0.30 mass% or more and 0.70 mass% or less, the copper (Cu) content is 0.11 mass% or more and 0.40 mass% or less, the manganese (Mn) content is 0.7 mass% or more and 1.2 mass% or less, the magnesium (Mg) content is 1.1 mass% or more and 3.0 mass% or less, the balance being aluminum (Al) and unavoidable impurities, and B_0° (MPa) satisfies the following formula (1), and the area of ​​the L-ST cross section is 0.3 μm 2 The aluminum alloy sheet for tabs has a total area ratio of the above Mg2Si particles of 0.2% or less. (2.7×t-0.45)×σ B_0° ≧67 (1)

[0017] According to this configuration, it is possible to achieve both high tab breaking strength and high toughness in the aluminum alloy sheet while blending scrap raw material derived from can materials. That is, it is possible to blend a certain amount of 3104 aluminum alloy scrap for can bodies, thereby reducing the usage rate of new ingots and reducing CO2 emissions. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is a schematic diagram of a repeated bending test. [Diagram 2] FIG. 2 is an explanatory diagram of the L-ST cross section. [Diagram 3] FIG. 3 is a graph showing the relationship between the value V and the tab bending strength in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] Hereinafter, embodiments to which the present disclosure is applied will be described with reference to the drawings. [1. First embodiment] [1-1. Configuration] <Composition> The aluminum alloy sheet for tabs (hereinafter also simply referred to as "alloy sheet") of the present disclosure contains aluminum (Al), silicon (Si), iron (Fe), copper (Cu), manganese (Mn), and magnesium (Mg).

[0020] The lower limit of the Si content is 0.20 mass%, and preferably 0.27 mass%. If the Si content is less than 0.20 mass%, the amount of Si precipitated in the processing heat of the cold rolling after the hot rolling and the solution treatment decreases, and the tensile strength of the alloy sheet may be insufficient.

[0021] In addition, the average value of the Si content standard of the 3104 aluminum alloy specified in JIS-H-4000:2014 is 0.30 mass%, and the average value of the Si content standard of the 5182 aluminum alloy specified in JIS-H-4000:2014 is 0.10 mass%. Therefore, by making the Si content 0.27 mass% or more, a large amount of 3104 aluminum alloy scrap can be blended.

[0022] The upper limit of the Si content is 0.60 mass%, and preferably 0.39 mass%. If the Si content exceeds 0.60 mass%, the difference between the solidus temperature of Mg2Si and the solidus temperature of the Al matrix becomes small, making it difficult to dissolve more Mg2Si present in the ingot in the homogenization process. In addition, coarse Mg2Si is newly precipitated during hot rolling. As a result, the tensile strength and toughness are reduced.

[0023] Furthermore, by setting the Si content to 0.39 mass% or less, Mg2Si can be easily dissolved in the homogenization process, and the precipitation of coarse Mg2Si during hot rolling is suppressed, so that good tensile strength and toughness can be obtained without performing a heat treatment process after hot rolling.

[0024] The lower limit of the Fe content is 0.30% by mass, and preferably 0.35% by mass. The average Fe content standard of 3104 aluminum alloy is 0.40% by mass, and the average Fe content standard of 5182 aluminum alloy is 0.18% by mass. Therefore, by making the Fe content 0.30% by mass or more, a large amount of 3104 aluminum alloy scrap can be blended.

[0025] The upper limit of the Fe content is 0.70 mass%, and preferably 0.55 mass%. If the Fe content exceeds 0.70 mass%, the amount of abnormally coarse Al-Fe-Mn or Al-Fe-Mn-Si intermetallic compounds (i.e., giant compounds) increases. As a result, a crack propagation path is generated, and the toughness of the alloy plate decreases.

[0026] Furthermore, by setting the Fe content to 0.55 mass % or less, it is possible to suppress the crystallization of the coarse intermetallic compounds described above that occurs when a large amount of Mg is added, while compensating for the tensile strength and toughness of the alloy plate.

[0027] The lower limit of the Cu content is 0.11 mass%, preferably 0.17 mass%. If the Cu content is less than 0.11 mass%, the amount of Cu that increases the strength by solid solution or precipitation is insufficient, and the tensile strength of the alloy sheet is reduced. Note that the tensile strength of the alloy sheet is significantly increased by precipitating Cu during hot rolling and cold rolling after solution treatment.

[0028] In addition, the average Cu content of the 3104 aluminum alloy is 0.15% by mass, and the average Cu content of the 5182 aluminum alloy is 0.075% by mass. Therefore, by making the Cu content 0.11% by mass or more, a large amount of 3104 aluminum alloy scrap can be blended.

[0029] The upper limit of the Cu content is 0.40 mass%, preferably 0.25 mass%. If the Cu content exceeds 0.40 mass%, the amount of coarse precipitates increases, and the toughness of the alloy plate decreases. Furthermore, by making the Cu content 0.25 mass% or less, the tensile strength can be increased without significantly impairing the toughness of the alloy plate.

[0030] The lower limit of the Mn content is 0.7 mass%, and preferably 0.75 mass%. If the Mn content is less than 0.7 mass%, there will be insufficient Mn to increase strength by solid solution or precipitation, and the tensile strength of the alloy sheet will decrease.

[0031] In addition, the average value of the Mn content standard for 3104 aluminum alloy is 1.1 mass%, and the average value of the Mn content standard for 5182 aluminum alloy is 0.35 mass%. Therefore, by making the Mn content 0.75 mass% or more, it is possible to mix more 3104 aluminum alloy scrap than the conventional 5182 aluminum alloy.

[0032] The upper limit of the Mn content is 1.2 mass%, preferably 0.95 mass%. If the Mn content exceeds 1.2 mass%, the amount of abnormally coarse Al-Fe-Mn or Al-Fe-Mn-Si intermetallic compounds increases. As a result, crack propagation paths are formed, and the toughness of the alloy plate decreases.

[0033] The lower limit of the Mg content is 1.1 mass%, preferably 2.2 mass%. If the Mg content is less than 1.1 mass%, the amount of Mg that increases the strength by solid solution is insufficient, and the tensile strength of the alloy sheet is reduced. In addition, the tensile strength of the alloy sheet is significantly increased by precipitating Mg during the processing of hot rolling and cold rolling after the solution treatment.

[0034] The upper limit of the Mg content is 3.0% by mass, and preferably 2.8% by mass. The average value of the Mg content standard of 3104 aluminum alloy is 1.05% by mass, and the average value of the Mg content standard of 5182 aluminum alloy is 4.5% by mass. Therefore, by making the Mg content 3.0% by mass or less, preferably 2.8% by mass or less, it is possible to reduce the amount of additional Mg-containing raw material while mixing a large amount of 3104 aluminum alloy scrap.

[0035] The alloy plate may contain titanium (Ti). The upper limit of the Ti content is preferably 0.10 mass%. The ingot structure of the alloy plate is refined by including Ti. The alloy plate may also contain zinc (Zn). The upper limit of the Zn content is preferably 0.25 mass%. Furthermore, the alloy plate may contain chromium (Cr). The upper limit of the Cr content is preferably 0.10 mass%.

[0036] The alloy plate may contain unavoidable impurities to the extent that the performance of the alloy plate is not significantly impaired. That is, the alloy plate contains Si, Fe, Cu, Mn, Mg, Ti, Zn, and Cr in the above-mentioned ranges, with the balance being aluminum and unavoidable impurities. The upper limit of the total amount of unavoidable impurities is preferably 0.15 mass%.

[0037] <Thickness, material strength and tab bending strength> In the alloy sheet of the present disclosure, the sheet thickness t (mm) and the tensile strength σ B_0° (MPa) satisfies the following formula (1). V = (2.7 × t - 0.45) × σ B_0° ≧67 (1)

[0038] Empirically, the value of the tab bending strength of an aluminum alloy tab has a strong positive correlation with the value V (i.e., the left side of formula (1)) which is expressed by the material strength and plate thickness of the aluminum alloy plate. Therefore, when the value V is 67 or more, a tab with sufficient tab bending strength can be formed.

[0039] In addition, the tensile strength σ B_0° It is preferable that the tab bending strength is 330 MPa or more. This makes it possible to form a tab having a sufficient tab bending strength without significantly increasing the plate thickness of the alloy plate.

[0040] The mechanical meaning of the relationship between the V value and the tab breaking strength can be explained as follows: When the tab is pulled up to open a can, if the resistance of the tab to the load applied to it is low, plastic deformation will begin due to localized material yielding before the score is opened normally. Tab breaking is a phenomenon in which the tab bends as this plastic deformation progresses.

[0041] Considering the cross section parallel to the bending ridge at the position where the tab bends, the resistance to the bending moment applied to the cross section by the tab being pulled up is calculated by the section modulus, which is a value specific to the cross-sectional shape, and the 0.2% yield strength σ 0.2 The higher is the larger.

[0042] The section modulus in the above cross section increases with thickness if the tab has a fixed shape, such as the typical DRT type stay-on tab. Therefore, the ease with which the material yields and bending due to plastic deformation begins in a tab break is determined by the plate thickness and the material's 0.2% yield strength σ 0.2 This can be explained by the following.

[0043] In addition, since the tab breakage is a phenomenon that includes the progress of plastic deformation and the bending of the tab, it is necessary to take into account the work hardening of the material during plastic deformation. 0.2% yield strength σ 0.2Even if the strain rate is low and plastic deformation begins early, if the amount of work hardening during plastic deformation is large, the progress of plastic deformation is suppressed and the tab is less likely to bend.

[0044] Therefore, 0.2% yield strength σ 0.2 Instead of tensile strength, σ is used as an index of material strength including work hardening. B_0° is introduced, and the plate thickness t and tensile strength σ B_0° The tab breaking property of the aluminum alloy sheet can be evaluated by using the value V expressed by

[0045] Tensile strength σ in formula (1) B_0° is measured by the method specified in JIS-Z-2241: 2011. The plate thickness t is measured, for example, with a micro gauge.

[0046] The tab breaking strength of an aluminum alloy plate is measured, for example, by the following procedure. A shell formed from an aluminum alloy plate is subjected to conversion processing other than scoring, and a can lid is formed as an end without scores. A tab formed from an aluminum alloy plate is then attached to the can lid. The can lid is fixed to a jig, and the tab is pulled up. The maximum load applied to the pulled-up portion at this time is taken as the tab breaking strength.

[0047] Specifically, a typical DRT type stay-on-tab shaped tab mold is used to mold the tab. A φ204 Fullform (B64) shaped shell mold, for example, is used to mold the shell. A pop-tear tester from Reed Instruments, Ltd. is used to measure the tab breaking strength.

[0048] More specifically, a can lid with no score and a tab attached, which is formed using a special jig, is fixed to the jig. A load-applying jig is then attached to the tab-pulling portion, and the load-applying jig is fixed in place while applying a load in a direction perpendicular to the panel portion of the lid such that the tab does not undergo plastic deformation. In this state, the lid is rotated at a rotation speed of 30° / sec to pull up and bend the tab. The maximum load applied to the tab-pulling portion is read within a rotation angle range of up to 90°.

[0049] <Toughness> It is known that the formability of the tab is affected by the toughness of the aluminum alloy sheet.

[0050] (Number of repeated bending) A repeated bending test is one of the evaluation indices for the toughness of an aluminum alloy plate. If the plate thickness is the same, the more repeated bending times the aluminum alloy plate is subjected to, the more excellent the toughness of the aluminum alloy plate is.

[0051] The repeated bending test is carried out as follows. For example, as shown in Figure 1, a test piece cut into a rectangular shape with a width of 12.5 mm and a length of 200 mm is placed in a direction such that the bending ridge R is parallel to the rolling direction D of the alloy plate. Both ends of the test piece are fixed with chucks, and a tension of 200 N is applied.

[0052] In this state, the test piece is repeatedly bent by rotating the other chuck 90° left and right, using a jig with a bending radius of 2.0 mm positioned 150 mm in the longitudinal direction of the test piece as a fulcrum from the end of the test piece fixed to one of the immovable chucks, and the number of bends until the test piece breaks is measured.

[0053] The number of bending operations is counted as one each for bending 90° to either the left or right and returning to the original position. If the specimen breaks during bending, the angle Θ (0°-90°) is read and the number of repeated bending cycles N is calculated using the following formula (2). In formula (2), N0 is the total number of times the specimen is bent 90° to either the left or right and returned from the 90° bent position to the original 0° position before it breaks. N = N0 + Θ / 90 (2)

[0054] Repeated bending evaluation is more disadvantageous as the plate thickness increases, so it is necessary to correct for the standard plate thickness. Therefore, the normalized repeated bending times N was normalized by the following formula (3) using a plate thickness of 0.245 mm as the standard. s In addition, t t (mm) is the thickness of the test piece. N s= N × t t / 0.245 ···(3)

[0055] Standardized repeated bending number N of the aluminum alloy plate of the present disclosure s The number of rotations is preferably 11.7 or more, and more preferably 15.0 or more.

[0056] (second phase particles) Toughness is affected by strength and the distribution of second phase particles. In other words, the higher the strength and the higher the density of second phase particles with large area, the lower the toughness. In particular, when the Mg and Si contents are high, Mg2Si particles are easily formed. As a result, the Mg2Si particles become the starting point and propagation path of cracks, which affects the decrease in toughness.

[0057] In the aluminum alloy sheet of the present disclosure, the area is 0.3 μm in the central region of the sheet thickness of the L-ST cross section shown by the diagonal line in FIG. 2 The ratio of the total area of ​​the above Mg2Si particles is preferably 0.2% or less. In Fig. 2, L indicates the longitudinal direction, ST indicates the plate thickness direction, and LT indicates the width direction.

[0058] The area ratio of Mg2Si particles can be measured, for example, by the following method. First, the measurement sample is cut and the surface to be measured (i.e., the L-ST cross section) is mechanically polished to a mirror finish. Next, the polished surface (i.e., the L-ST cross section) is observed using a SEM (scanning electron microscope) to obtain 10 fields of view in the central region of the plate thickness. The accelerating voltage of the SEM is 15 kV, the magnification is 500 times, and the range of one field of view is 0.049 mm 2 The image is then taken and a COMPO (backscattered electron composition) image is obtained.

[0059] The captured COMPO image is analyzed using the image analysis software "ImageJ." Specifically, the most frequent brightness value of the image in 256 gradations is taken as the background brightness, and particles with brightness lower than the brightness of the most frequent value minus 30 are determined to be Mg2Si particles.

[0060] Among the determined Mg2Si particles, 0.3 μm 2The total area of ​​particles with an area of ​​0.3 μm or more was calculated and divided by the area of ​​10 fields of view (i.e., the total area photographed). 2 The ratio of the total area of ​​the above Mg2Si particles in the L-ST cross section is calculated.

[0061] <Strength anisotropy> It is known that materials with low cold rolling ratios (hereinafter abbreviated as cold rolling ratios) have high toughness. The higher the cold rolling ratio, the higher the 0.2% yield strength σ 0.2_90° 0.2% yield strength σ in the 0° direction 0.2_0° Therefore, the difference in 0.2% yield strength between the 0° direction and the 90° direction with respect to the rolling direction, that is, the strength anisotropy, can be associated with the cold rolling rate of the material.

[0062] The alloy sheet of the present disclosure has a 0.2% yield strength σ in the 0° direction relative to the rolling direction, which is calculated by the formula (4). 0.2_0° From the above, the 0.2% yield strength σ 0.2_90° It is preferable that the value D obtained by subtracting the above is −4 MPa or more. D=σ 0.2_0° -σ 0.2_90° (4)

[0063] 0.2% proof stress σ in formula (4) 0.2_0° ,σ 0.2_90° is measured using the method specified in JIS-Z-2241:2011.

[0064] 0.2% proof stress σ in the 0° direction to the rolling direction 0.2_0° From the above, the 0.2% yield strength σ 0.2_90° The material structure meaning of the strength anisotropy minus can be explained as follows.

[0065] After hot rolling or annealing, the material is in a recrystallized state, with a high concentration of isotropic cube orientation. From here, the plastic deformation caused by cold rolling transforms the cube orientation into a rolling texture with anisotropy in the rolling direction. Furthermore, the larger the cold rolling rate, the more the crystal grains are elongated in the rolling direction, so the diameter of the crystal grains in the 0° direction to the rolling direction becomes larger, while the change in the diameter of the crystal grains in the 90° direction to the rolling direction becomes smaller than in the 0° direction.

[0066] The structural changes caused by these rolling processes and the 0.2% yield strength σ 0.2 The relationship between these two can be expressed by the Hall-Petch equation as shown in Equation (5). In Equation (5), κ is the resistance to grain boundary sliding, and d is the grain size. σ 0.2 ∝κ×d -1 / 2 (5)

[0067] The resistance κ has different values ​​for tensile stress in the 0° or 90° direction to the rolling direction. This is because the rolling texture, which has anisotropy in the rolling direction, increases with increasing cold reduction ratio, and the resistance to grain boundary slippage changes depending on the tensile direction.

[0068] In addition, while the grains elongate and their diameter increases with increasing cold rolling in the 0° direction, the change in grain size with increasing cold rolling is relatively small in the 90° direction. The cumulative effect of these effects results in strength anisotropy with increasing cold rolling.

[0069] <Method of manufacturing aluminum alloy sheet> The aluminum alloy plate of the present disclosure can be produced, for example, as follows: First, an aluminum alloy having the composition of the aluminum alloy plate of the present disclosure is subjected to a semi-continuous casting method (i.e., DC casting) according to a conventional method to produce an ingot.

[0070] Next, the four sides of the ingot, excluding the front and rear ends, are chamfered. The ingot is then placed in a soaking furnace for homogenization. The temperature in the homogenization is preferably 530°C or higher and lower than the solidus temperature of the Al matrix.

[0071] If the homogenization temperature is 530°C or higher, the homogenization temperature is sufficiently higher than the solid solution temperature of Mg2Si, so that the amount of Mg2Si, which is a second phase particle crystallized or precipitated in the ingot, can be reduced. This improves both the tensile strength and toughness of the aluminum alloy sheet. Furthermore, by setting the homogenization temperature to 550°C or higher, the amount of Mg2Si can be extremely reduced.

[0072] On the other hand, when the temperature in the homogenization treatment is equal to or lower than the solidus temperature of the Al matrix, the aluminum alloy plate can be produced without local melting. The homogenization treatment temperature is preferably 10°C or more lower than the solidus temperature of the Al matrix. This allows the aluminum alloy plate to be produced stably without local melting.

[0073] The solution temperature of Mg2Si and the solidus temperature of the Al matrix are uniquely determined by the composition of the aluminum alloy. For example, these temperatures can be obtained by inputting the composition of the aluminum alloy into "JMatPro," a thermodynamic calculation software developed by Sente Software, and calculating the equilibrium phase diagram. The CALPHAD method is used to calculate the thermodynamic model.

[0074] The homogenization time is preferably, for example, 1 hour or more and 20 hours or less. When the homogenization time is 1 hour or more, the temperature of the entire slab becomes uniform, segregation of the ingot structure is easily eliminated, and Mg2Si particles are easily redissolved. The longer the homogenization time, the more the Mg2Si particles can be redissolved. However, when the homogenization time exceeds 20 hours, the effect of the homogenization treatment becomes saturated.

[0075] After the homogenization treatment, the ingot is subjected to hot rolling. The hot rolling process includes a rough rolling process and a finish rolling process. In the rough rolling process, the ingot is processed into a plate material having a thickness of about several tens of mm by reverse rolling. In the finish rolling process, the thickness of the plate material is reduced to about several mm by, for example, tandem rolling, and the plate material is wound into a coil to form a hot rolled coil.

[0076] If the total reduction rate of the finish rolling is high, the recrystallized structure will be formed after coiling, and the concentration of the isotropic cube orientation can be increased. If the coiling temperature of the finish rolling is high, the recrystallized structure will be formed after coiling, and the concentration of the cube orientation can be increased.

[0077] Also, an alloy plate with high tensile strength can be obtained by intermediate annealing (i.e., solution treatment) of the hot-rolled coil to re-dissolve Mg, etc. For example, the tensile strength of the alloy plate can be effectively increased by performing heat treatment (i.e., annealing) at a target actual temperature of 440°C or higher for 30 seconds or more using a continuous annealing furnace (CAL), followed by forced cooling by air cooling, etc.

[0078] Following hot rolling, the plate material is cold rolled. In cold rolling, the hot rolled coil is rolled until the product plate thickness is reached. Cold rolling may be either single rolling or tandem rolling. In single cold rolling, rolling is preferably performed in multiple passes, such as two or more passes.

[0079] In addition, intermediate annealing of the coil during cold rolling to redissolve Mg and other elements can increase the tensile strength of the material while lowering the final cold rolling rate to obtain an alloy sheet with suppressed anisotropy of the material. For example, heat treatment (i.e., annealing) is performed at a target solid temperature of 440°C or higher using a continuous annealing furnace, and then forced cooling is performed using air cooling or the like, thereby effectively increasing the tensile strength of the alloy sheet. Note that intermediate annealing of hot-rolled coils and coils during cold rolling is optional.

[0080] In addition, by setting the finishing temperature of cold rolling in intermediate passes other than the final pass to 120°C or higher, Si, Cu and Mg are finely precipitated and age hardened, so that the tensile strength of the alloy sheet can be increased. Furthermore, by setting the finishing temperature to 130°C or higher, the tensile strength of the alloy sheet can be further increased.

[0081] If no solution treatment is performed during cold rolling, the cold rolling rate (i.e., the total rolling reduction rate) is preferably 75% or more. If the cold rolling rate is 75% or more, the tensile strength of the alloy sheet can be increased. In addition, the lower the cold rolling rate, the more the cube orientation remains, so the cold rolling rate is preferably 92% or less.

[0082] When solution treatment is performed during cold rolling, the cold rolling rate (i.e. the total reduction rate after solution treatment) is preferably 45% or more. When the cold rolling rate is 45% or more, the tensile strength of the alloy sheet can be increased by lowering the cold rolling rate and resolving Mg and other elements by solution treatment. In addition, the lower the cold rolling rate, the more the cube orientation remains, so the cold rolling rate is preferably 80% or less.

[0083] The cold rolling rate R (%) is calculated by the following formula (6) using the sheet thickness t0 (mm) after hot rolling or after solution treatment and the product sheet thickness t1 (mm) after cold rolling. R = (t0-t1) / t0 × 100 (6)

[0084] The product plate thickness can be appropriately selected so as to obtain a desired tab bending strength. The product plate thickness is selected so as to satisfy the formula (1). As described above, according to the aluminum alloy plate of the present disclosure, it is possible to suppress an increase in plate thickness for maintaining a high tab bending strength.

[0085] The coil that has been cold-rolled to the product thickness may or may not be precoated in a painting line, etc. When precoating is performed, the surface of the cold-rolled coil is degreased, washed, and subjected to a chemical conversion treatment, and then a paint is applied, followed by a paint baking treatment.

[0086] Chemical solutions such as chromate-based and zirconium-based are used in chemical conversion treatment. Epoxy-based and polyester-based paints are used. These can be selected according to the application. In the paint baking process, the coil is heated to a peak metal temperature (PMT) of 220°C to 270°C for approximately 30 seconds or less. The lower the PMT, the more the material recovery is suppressed, and the higher the tensile strength of the alloy plate can be maintained.

[0087] [1-2. Effects] According to the embodiment described above in detail, the following effects can be obtained. (1a) It is possible to achieve both high tab breaking strength and high toughness in aluminum alloy sheets while blending scrap raw materials derived from can stock. In other words, it is possible to blend a certain amount of 3104 aluminum alloy scrap for can bodies, reduce the usage rate of new ingots, and reduce CO2 emissions.

[0088] 2. Other embodiments Although the embodiments of the present disclosure have been described above, it goes without saying that the present disclosure is not limited to the above-described embodiments and can take various forms.

[0089] (2a) In addition to the aluminum alloy sheet of the above embodiment, the present disclosure also includes various embodiments of a member constituted by this aluminum alloy sheet, a manufacturing method of this aluminum alloy sheet, and the like.

[0090] (2b) The function of one component in the above embodiments may be distributed among multiple components, or the functions of multiple components may be integrated into one component. In addition, a part of the configuration of the above embodiments may be omitted. In addition, at least a part of the configuration of the above embodiments may be added to or substituted for the configuration of another of the above embodiments. Note that all aspects included in the technical idea identified from the wording of the claims are embodiments of the present disclosure.

[0091] 3. Working Examples The following describes the tests conducted to confirm the effects of the present disclosure and the evaluation results thereof.

[0092] <Production of aluminum alloy sheets> As examples and comparative examples, aluminum alloy sheets S1 to S17 shown in Tables 1 and 2 were produced. Specific production procedures are described below.

[0093] First, an ingot containing 0.32% by mass of Si, 0.43% by mass of Fe, 0.22% by mass of Cu, 0.80% by mass of Mn, 2.6% by mass of Mg, with the remainder being aluminum and unavoidable impurities, was produced by semi-continuous casting. The ingot contained 0.10% by mass or less of Ti, 0.25% by mass or less of Zn, 0.10% by mass or less of Cr, and 0.15% by mass or less of unavoidable impurities.

[0094] Next, the four sides of the ingot, excluding the front and rear ends, were chamfered. The ingot was then placed in a furnace and subjected to homogenization treatment. The homogenization temperature is shown in Table 1. After the homogenization treatment, the ingot was removed from the furnace and immediately hot rolling was started to produce a rolled sheet.

[0095] Furthermore, for S1-S8, the rolled sheets after hot rolling were cold rolled until they had the sheet thickness shown in Table 1. After cold rolling, the rolled sheets were subjected to intermediate annealing. The temperature during intermediate annealing was as shown in Table 1, and the time was 30 seconds. After intermediate annealing, the rolled sheets were cooled to room temperature by air cooling. After cooling, the rolled sheets were cold rolled again. The target cold reduction ratio in cold rolling after intermediate annealing is as shown in Table 1.

[0096] For S9-S14, intermediate annealing was performed on the hot-rolled rolled sheets. The sheet thickness and temperature during intermediate annealing were as shown in Table 1, and the time was 30 seconds. After intermediate annealing, the rolled sheets were air-cooled to room temperature. After cooling, the rolled sheets were cold-rolled. The target cold reduction ratios in cold rolling are as shown in Table 1.

[0097] For S15-S17, the hot-rolled sheets were cold-rolled without annealing. The target cold rolling reduction ratios are shown in Table 1.

[0098] The product thickness after cold rolling in S1-S17 (i.e., t1 in equation (6)) was set to a range of approximately 0.330±0.05 mm.

[0099] For S1-S14, S16, and S17, paint was applied to the sheet surface after cold rolling, and a paint baking treatment was performed for about 30 seconds. The practical temperature (PMT) during paint baking is shown in Table 1. For S15, neither paint application nor baking was performed. As a result, aluminum alloy sheets S1-S17 were obtained. Furthermore, the sheet thickness (i.e., product sheet thickness) of the aluminum alloy sheets S1-S17 measured by a microgauge is shown in Table 1.

[0100] [Table 1]

[0101] [Table 2]

[0102] <Evaluation of aluminum alloy sheets> (Tensile properties) Two No. 5 test pieces as specified in JIS-Z-2241:2011 were prepared from each of the S1-S17 aluminum alloy sheets by milling. The longitudinal directions of the two test pieces were aligned at angles of 0° and 90° to the rolling direction, respectively.

[0103] Tensile tests were conducted on these test pieces in accordance with JIS-Z-2241:2011 to measure the 0.2% proof stress and tensile strength. Tensile strength σ in the 0° direction to the rolling direction B_0° The measurement results of 0.2% yield strength σ 0.2_0° and 0.2% yield strength σ at 90° to the rolling direction 0.2_90° The measurement results are shown in Table 2.

[0104] In addition, from the measurement results of plate thickness and tensile strength, the value of formula (1) V = (2.7 × t - 0.45) × σ B_0°The calculation results are shown in Table 2.

[0105] (Toughness) In the aluminum alloy plates of S1-S17, the area is 0.3 μm by the measurement method described in the embodiment. 2 The ratio of the total area (area ratio) of the above Mg2Si particles in the L-ST cross section was calculated. The measurement results are shown in Table 2.

[0106] For the aluminum alloy sheets S1-S17, the normalized number of repeated bending cycles was calculated from the measurement method described in the embodiment and the formulas (2) and (3). The results are shown in Table 2.

[0107] (Strength Anisotropy) For the aluminum alloy sheets S1-S17, the strength anisotropy (i.e., value D) was calculated from the formula (4) explained in the embodiment. The results are shown in Table 2.

[0108] (scrap mixture ratio) Regarding the composition of the S1-S17 aluminum alloy plates, it was judged whether the possible blending ratio of 3104 aluminum alloy scrap was 50 mass% or more. The results are shown in Table 2.

[0109] In Table 2, aluminum alloy plates marked with "≧50" can contain 50 mass% or more of 3104 aluminum alloy. The possible content of 3104 aluminum alloy scrap is determined based on Table 3.

[0110] Table 3 shows the average values ​​of the component specifications for the 3104 and 5182 aluminum alloys, and the corresponding blend ratios. The first line of Table 3 shows the average values ​​of the component specifications for the 3104 aluminum alloy, and the second line shows the average values ​​of the component specifications for the 5182 aluminum alloy.

[0111] For example, when the blend ratio of 3104 aluminum alloy is 50 mass%, the average value of Si is 0.20 mass%, the average value of Fe is 0.29 mass%, the average value of Cu is 0.11 mass%, the average value of Mn is 0.7 mass%, and the average value of Mg is 2.8 mass%.

[0112] Therefore, when the ratio of each component of the aluminum alloy plate is equal to or greater than the above values ​​of Si, Fe, Cu, Mn, and Mg, the possible blending ratio of 3104 aluminum alloy plate is 50% by mass or more. As the blending ratio of 3104 aluminum alloy increases, the contents of Si, Fe, Cu, and Mn increase and the content of Mg decreases. The aluminum alloy plates of S1-S17 can blend 50% by mass or more of 3104 aluminum alloy scrap.

[0113] [Table 3]

[0114] (tab bending strength) In addition to the aluminum alloy plates S1 to S17, a number of aluminum alloy plates having different plate thicknesses and tensile strengths were prepared, and the tab bending strength of each was measured by the measurement method described in the embodiment.

[0115] The measurement results, the thickness t of the aluminum alloy plate, and the tensile strength σ in the 0° direction relative to the rolling direction B_0° And the value of equation (1) V = (2.7 × t - 0.45) × σ B_0° The relationship between these is shown in Table 4 and Figure 3. Table 5 shows the components of the aluminum alloy sheets used to measure the tab bending strength.

[0116] Figure 3 confirms that there is a high correlation between the value V and the tab breaking strength. Note that Figure 3 shows the results using a tab with a typical DRT type stay-on tab shape, but similar trends can be seen for tabs with other shapes.

[0117] [Table 4]

[0118] [Table 5]

[0119] As shown in Table 2, in any of the aluminum alloy sheets S1 to S17, the value V, which has a strong correlation with the tab breaking strength, was 67 or more, and it was confirmed that the sheet thickness and tensile strength were sufficient to obtain high tab breaking strength.

[0120] In addition, for all aluminum alloy sheets S1-S17, the tensile strength σ B_0° is 330 MPa or more, and high tab bending strength can be maintained while suppressing an excessive increase in plate thickness.

[0121] The aluminum alloy sheets S1-S11 and S15-S17, which have been subjected to higher homogenization temperatures, have shown higher tensile strength and normalized number of repeated bending cycles. For example, the aluminum alloy sheets S9-S11 have higher tensile strength and number of repeated bending cycles than the aluminum alloy sheets S12-S14, because the homogenization temperature is higher, even if the process and paint baking temperature are the same.

[0122] In addition, the lower the paint baking temperature (PMT), the higher the tensile strength of the alloy sheet. For example, when comparing S1 and S2, S5 and S6, S7 and S8, S9-S11, S12-S14, and S16 and S17, the lower the paint baking temperature, the higher the 0.2% proof stress σ 0.2_0° , 0.2% proof stress σ at 90° to the rolling direction 0.2_90° , and tensile strength σ in the 0° direction relative to the rolling direction B_90° showed high values.

[0123] In the aluminum alloys S1-S11 and S15-S17 in which the homogenization temperature was 550°C or higher, the area ratio of Mg2Si particles was smaller than that in the other Examples, being 0.2% or less. Therefore, when comparing the aluminum alloy sheets S9-S11 and S12-S14, although the tensile strength in the 0° direction relative to the rolling direction of the aluminum alloy S9-S11 was higher than that of the aluminum alloy sheets S12-S14, the aluminum alloy sheets S9-S11 had a higher number of normalized repeated bending cycles than the aluminum alloy sheets S12-S14.

[0124] The number of repeated bending cycles also varies depending on the tensile strength. Comparing the aluminum alloy sheets S9 and S11, which have a relatively small area ratio of Mg2Si particles and the same cold-rolling rate, it can be seen that the aluminum alloy sheet S11, which has a relatively low tensile strength, has a higher normalized number of repeated bending cycles than the aluminum alloy sheet S9.

[0125] The normalized number of repeated bending cycles also differs depending on the anisotropy of the material structure. For example, when aluminum alloy sheets S1, S2, and S5, which have strength anisotropy of -4 MPa or more, are compared with aluminum alloy sheets S9-S11, which have strength anisotropy of less than -4 MPa, the tensile strengths of the sheets are relatively close to each other, but the number of repeated bending cycles of the sheets S1, S2, and S5 are much higher than that of the sheet S9-S11.

[0126] In addition, when comparing the aluminum alloy sheets S3, S4, and S6-S8, which have strength anisotropy of -4 MPa or more, with the aluminum alloy sheet S15-S17, which has strength anisotropy of less than -4 MPa, the tensile strengths are relatively close to each other, but the number of repeated bending cycles of S3, S4, and S6-S8 is much higher than that of S15-S17.

Claims

1. The silicon (Si) content is 0.20% by mass or more and 0.60% by mass or less, The iron (Fe) content is 0.30 mass% or more and 0.70 mass% or less, The copper (Cu) content is 0.11 mass% or more and 0.40 mass% or less, The manganese (Mn) content is 0.7% by mass or more and 1.2% by mass or less, The magnesium (Mg) content is 1.1% by mass or more and 3.0% by mass or less, The balance is aluminum (Al) and unavoidable impurities, Plate thickness t (mm) and tensile strength σ in the direction 0° to the rolling direction B_0° (MPa) satisfies the following formula (1), In the L-ST cross section, the area is 0.3 μm 2 More than Mg 2 An aluminum alloy sheet for tabs, in which the ratio of the total area of ​​Si particles is 0.2% or less. (2.7×t-0.45)×σ B_0° ≧67 ・・・(1)

2. The aluminum alloy sheet for tabs according to claim 1, A test piece cut into a rectangular shape having a width of 12.5 mm and a length of 200 mm to 300 mm was repeatedly bent in a direction in which the bending ridge line was parallel to the rolling direction, by bending the test piece by 90° and returning it to the 0° position. The number of repeated bending operations N until the test piece broke was calculated by dividing the number of repeated bending operations by the thickness t of the test piece. t (mm) and the normalized number of repeated bending cycles N normalized by the following formula (2) s is 11.7 times or more, The tensile strength σ B_0° The aluminum alloy sheet for tabs has a compressive strength of 330 MPa or more. N s =N×t t / 0.245 ・・・(2)

3. The aluminum alloy sheet for tabs according to claim 2, The normalized number of repeated bending times N s The aluminum alloy plate for tabs has a rolling resistance of 15.0 times or more.

4. The aluminum alloy sheet for a tab according to any one of claims 1 to 3, 0.2% proof stress σ in the 0° direction to the rolling direction 0.2_0° From the above, the 0.2% yield strength σ 0.2_90° The aluminum alloy sheet for tabs has a strength obtained by subtracting the above from the hardness, which is -4 MPa or more.

5. The aluminum alloy sheet for a tab according to any one of claims 1 to 3, The silicon (Si) content is 0.27% by mass or more and 0.39% by mass or less, The iron (Fe) content is 0.35 mass% or more and 0.55 mass% or less, The copper (Cu) content is 0.17% by mass or more and 0.25% by mass or less, The manganese (Mn) content is 0.75 mass% or more and 0.95 mass% or less, An aluminum alloy sheet for tabs, having a magnesium (Mg) content of 2.2 mass% or more and 2.8 mass% or less.

6. The aluminum alloy sheet for tabs according to claim 4, The silicon (Si) content is 0.27% by mass or more and 0.39% by mass or less, The iron (Fe) content is 0.35 mass% or more and 0.55 mass% or less, The copper (Cu) content is 0.17% by mass or more and 0.25% by mass or less, The manganese (Mn) content is 0.75 mass% or more and 0.95 mass% or less, An aluminum alloy sheet for tabs, having a magnesium (Mg) content of 2.2 mass% or more and 2.8 mass% or less.

Citation Information

Patent Citations

  • Aluminum two piece can body and its manufacture

    JP1992221036A

  • Aluminum alloy laminate for can cover adapted to recycling and manufacture thereof

    JP1997070925A

  • Continuous casting process for low earring aluminum alloy production

    JP2002514269A

  • Zirconium hydroxide powder and manufacturing method of zirconium hydroxide powder

    JP2023067405A

  • Can lid for food or drink

    WO2023095859A1