Process for the production of microbial cellulose using waste textiles

The described process effectively converts cellulose to glucose from waste textiles using NaOH and urea pretreatment, addressing inefficiencies in current methods by enhancing enzymatic conversion and reducing energy use while preserving non-cellulosic fibers for recycling.

JP2024153571APending Publication Date: 2024-10-29SANKO TEKSTIL ISLETMELERI SANAYI VE TICARET AS
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2024064391
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-12
Filing Date
2024-04-12
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Current processes for producing microbial cellulose from waste textiles are inefficient due to partial degradation of non-cellulosic materials like polyester fibers, reduced enzymatic conversion of cellulose to glucose, high energy consumption, and the need for expensive chemical recovery of reagents.

Method used

A process involving pretreatment of waste textiles with an aqueous solution of NaOH and urea at controlled temperatures to minimize cellulose dissolution and enhance enzymatic conversion, followed by enzymatic saccharification to obtain glucose, which is then used to produce microbial cellulose.

Benefits of technology

The process achieves efficient conversion of cellulose to glucose with reduced energy consumption and cost, preserving non-cellulosic fibers for recycling, and producing high yields of microbial cellulose suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153571000001_ABST
    Figure 2024153571000001_ABST
Patent Text Reader

Abstract

To provide a process for producing microbial cellulose using waste textiles.SOLUTION: The invention relates to a production process of microbial cellulose using waste textile materials, such as 100% cotton or cotton / polyester / elastane waste mixed fiber textiles, the process comprising the steps of: providing the cellulose-containing waste textile material, in particular, preparing a certain amount of the waste textile material and pretreating the waste textile material with an aqueous solution comprising NaOH and urea at a temperature ranging from -25°C to +30°C; treating the pretreated fabric with a cellulase enzyme to convert cellulose into glucose, thereby obtaining a mixture containing glucose; preparing a culture medium comprising the glucose-containing mixture; inoculating the culture medium with a microorganism that produces microbial cellulose; and culturing the microbial cellulose-producing microorganism to obtain microbial cellulose.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a process for the production of microbial cellulose using waste textile materials. More particularly, the present invention relates to a process for the production of microbial cellulose starting from waste textile materials comprising cellulose fibres and optionally synthetic fibres. [Background technology]

[0002] Microbial cellulose is one of the best known and most studied bacterial biopolymers. It has the same chemical formula (C 6 H 10 O 5 ) n It is an organic compound produced as an extracellular polymer by certain types of microorganisms, such as bacteria. Microbial cellulose, e.g., bacterial cellulose, has the same molecular formula as plant cellulose, but differs from plant cellulose in its polymeric properties. In fact, microbial cellulose is generally more chemically pure (i.e., it does not contain hemicellulose or lignin) and has a higher water-holding capacity, higher tensile strength, higher degree of polymerization, and higher crystallinity than plant cellulose. Due to these unique properties, microbial cellulose has applications in several technical fields, such as the food industry, the medical field (e.g., wound dressings and vascular regeneration), and paper repair. Applications of microbial cellulose (e.g., bacterial cellulose) in the textile field are also known.

[0003] Recycling of used textiles, also known as "waste textiles", has become a major goal in the textile industry, and new efficient processes for recycling are being actively researched. One of the goals is to recycle the materials contained in waste textiles, for example the fibers contained in waste textiles, by converting them into raw materials suitable for use in different processes, such as the production process of microbial cellulose.

[0004] Processes for obtaining bacterial cellulose from waste textile materials are known in the art, in which fabrics containing yarns containing cotton fibers are pretreated with organic salts such as N-methylmorpholine-N-oxide (NMMO) or 1-alkyl-3-methylimidazolium ionic liquids prior to enzymatic hydrolysis.

[0005] For example, Patent Document 1 discloses a method for preparing bacterial cellulose from waste cotton cloth. The method according to Patent Document 1 includes a step of pretreating cotton cloth in an ionic liquid at 90°C to 130°C for 15 minutes to 10 hours. Next, cellulase enzyme is added to perform enzymatic hydrolysis to obtain an enzymatic decomposition liquid. This enzymatic decomposition liquid is used to prepare a culture medium for bacterial cellulose-producing bacteria.

[0006] Patent Document 2 discloses a method for preparing bacterial cellulose from waste polyester fabric, which includes the steps of adding a barium hydroxide solution and treating the fabric at a temperature of 120°C to 126°C for 90 to 100 minutes. After hydrolysis, sulfuric acid is added until no precipitate is formed, the pH value of the solution is adjusted to neutral, and the solution is centrifuged to obtain a supernatant, i.e., a polyester hydrolysate. This polyester hydrolysate is used as a carbon source for preparing a culture medium for bacteria that produce bacterial cellulose.

[0007] Currently available processes for obtaining microbial cellulose from waste textile materials have several drawbacks.

[0008] For example, currently available processes generally result in a reduced efficiency of enzymatic conversion to glucose, which the applicant has realized is due to the presence of dissolved cellulose in the liquid phase obtained after pretreatment and / or at least partial degradation of the cellulose fibers before the conversion of cellulose to glucose. For example, from "Enzymatic saccharification of dissolution pretreated waste cellulose fabric for bacterial cellulose production by Gluconacetobacter xylinus" by Friedrichs, et al., J. Appl. Phys. 2003, 143:1311-1329, it is known that cellulose is dissolved when the fabric is treated with ionic liquids. Treatment of cellulose-containing fabrics with ionic liquids (such as NMMO or 1-butyl-3-methylimidazolium chloride ([BMIM]Cl)) or strong acids (such as phosphoric acid and solutions thereof) dissolves most of the cellulose, necessitating a regeneration step to obtain the cellulose in solid form prior to treatment with cellulase enzymes. Thus, cellulose solutions are not suitable starting materials for the enzymatic conversion of cellulose to glucose. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] China Patent Application Publication No. 102080114 [Patent Document 2] China Patent Application Publication No. 111269953 [Non-patent literature]

[0010] [Non-Patent Document 1] CHIA-HUNG KUO et al., “JOURNAL OF CHEMICAL TECHNOLOGY AND BIOTECHNOLOGY”, Volume 85, No. 10, pp. 1346-1352 Summary of the Invention [Problem to be solved by the invention]

[0011] In addition to the above problems, currently available processes performed on waste textile products containing both cellulosic (e.g., cotton, lyocell, viscose) and non-cellulosic (e.g., synthetic, such as polyester) fibers result in at least partial degradation of the non-cellulosic materials, e.g., polyester fibers. Degradation of polyester fibers due to polymer hydrolysis can adversely affect the possibility of melting and reusing the polyester fibers to extrude new polyester fibers with the required mechanical properties.

[0012] On the other hand, it is necessary to realize a method to increase the rate of enzymatic conversion of the cellulose fibers in the fabric to glucose, thereby reducing the overall cost of the closed-loop recycling process that starts and ends with (recycled) cellulose fibers.

[0013] Additionally, currently available processes are energy intensive given the process conditions, and the reagents used in currently available processes (e.g., ionic liquids) require expensive chemical processes to recover and reuse. [Means for solving the problem]

[0014] The object of the present invention is to solve the above problems and provide a process for producing microbial cellulose that effectively uses waste fiber products. In particular, the object of the present invention is to provide a cellulose saccharification process that is efficient and easy to apply on an industrial scale.

[0015] Another object of the present invention is to provide a process for the production of microbial cellulose using waste textiles, suitable for carrying out on waste textiles containing both cellulose and non-cellulose synthetic fibers, particularly polyester fibers. The process should provide an end product consisting of or containing synthetic fibers, such as polyester fibers, substantially free of cotton and cellulose fibers. The process should also help to reduce or prevent depolymerization of polyester or other synthetic fibers present in textiles subjected to the treatment of the present invention.

[0016] Another object of the present invention is to provide a process for producing microbial cellulose using waste textile products, which can reduce energy consumption.

[0017] These objects are achieved according to the invention by the process according to claim 1, as well as by a process for enzymatic saccharification of cellulosic fabrics according to claim 2 and a process for recycling mixed textile products according to claim 19. Preferred embodiments of the invention are according to the dependent claims. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is a schematic diagram of one embodiment of the process of the present invention. [Diagram 2] 1 is a SEM image of an exemplary waste textile material before and after pretreatment with the process of the present invention. [Figure 3A] 1 is a microscopic image of an exemplary bacterial cellulose obtained by the process of the present invention. [Figure 3B] 3B shows microscopic images of bacterial cellulose at different magnifications of the microscopic image of FIG. 3A. [Figure 4A] 1 is a SEM image of 100% polyester fabric pretreated with an aqueous solution containing NaOH and urea at room temperature according to the present invention. [Figure 4B] 1 is a SEM image of a 100% polyester fabric pretreated according to the present invention with an aqueous solution containing NaOH and urea at a temperature of 50° C. [Figure 5A] 1 is a SEM image before pretreatment and enzyme treatment according to the process of the present invention. [Figure 5B] 1 is a SEM image of an exemplary waste textile material after pretreatment and enzymatic treatment according to the process of the present invention, particularly showing an exemplary waste textile material after pretreatment at 0° C. and treatment with cellulase according to an embodiment of the process of the present invention. [Figure 5C]1 is a SEM image of an exemplary waste textile material after pretreatment and enzymatic treatment according to the process of the present invention, particularly showing an exemplary waste textile material after pretreatment at room temperature and treatment with cellulase according to an embodiment of the process of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] As shown in FIG. 1, according to one embodiment, the present invention relates to a process for the production of microbial cellulose from waste textile materials containing cellulose in the form of cellulose fibers, the process comprising: a) preparing said waste textile material; b) pre-treating said waste textile material with an aqueous solution comprising a base, preferably NaOH, and an amide, preferably urea, at -25°C to +30°C to obtain a pre-treated textile material; c) treating the pretreated textile material with cellulase to convert the cellulose to glucose to obtain a mixture comprising a solid phase and a liquid phase; d) separating the liquid phase from the solid phase to obtain a liquid phase mixture comprising glucose; e) preparing a microbial culture containing a microbial cellulose-producing fungus using the liquid phase mixture containing glucose; and f) culturing the microbial culture to obtain microbial cellulose.

[0020] Advantageously, the present invention allows for the efficient production of microbial cellulose starting from waste textile materials, and also allows for the production of microbial cellulose starting from waste textile materials in an energy-saving and therefore cost-saving manner.

[0021] In a possible embodiment, the microbial cellulose obtained by the process of the present invention is used as the starting cellulose material in a viscose-like process that converts the microbial cellulose into regenerated cellulose fibers.

[0022] Apart from the cost-effectiveness of an affordable cellulose pretreatment solution, the presence of NaOH (or another base) and urea (or another amide, e.g. thiourea) realizes advantages such as improved cellulose properties that enhance the following steps of the microbial cellulose production process. More specifically, it has been found that the use of the above reagents at the specified temperatures, especially at room temperature, enhances the enzymatic degradation and increases the yield of glucose obtained after enzymatic saccharification. It has also been surprisingly found that a higher cellulose to glucose conversion yield is obtained if the textile product to be treated, i.e. fabric, is shredded (or generally subjected to a process to reduce its size) after undergoing a step of NaOH / urea pretreatment. The textile product is preferably dried before being shredded.

[0023] First, it is believed that the amount of cellulose dissolved during the pretreatment with NaOH and urea is so small that it does not impair or significantly reduce the enzymatic activity of cellulase in the following steps. Furthermore, since only a small amount of cellulose is dissolved during the pretreatment of the fabric with NaOH and urea, a regeneration step in which the cellulose is dissolved by adding water to the cellulose solution and then precipitated as a solid before shredding is not necessary, especially when the fabric area is large. A further reason is that the addition of urea captures free water, preventing interactions between cellulose chains through hydrogen bonds, and the treatment reduces the crystallinity of cellulose, resulting in negligible changes in the degree of polymerization of cellulose.

[0024] The present invention therefore further relates to a process for the enzymatic saccharification of waste textile materials comprising cellulose-containing cellulose fibres, the process comprising: a) preparing said waste textile material; b) pretreating the waste textile material with an aqueous solution containing NaOH and urea at -25°C to +30°C to obtain a pretreated textile material; c) treating the pretreated textile material with cellulase to convert the cellulose to glucose to obtain a mixture comprising a solid phase and a liquid phase; The pretreated textile material obtained in step b) is characterised in that, prior to step c), it is chopped into a plurality of pieces having a size suitable for enzymatic saccharification.

[0025] In fact, the pretreatment used in the process of the present invention reduces the amount of enzyme required for the enzymatic conversion of cellulose fibers to glucose, i.e. so low that it becomes economically viable to stop recovering the enzyme after the enzymatic reaction. This effect allows the glucose-containing solution to be used as a basis for the production of microbial cellulose without removing the cellulase enzyme. The cellulase enzyme is actually inactivated before the cellulose-producing bacteria are added to the glucose + enzyme solution, which serves as a source of nitrogen and carbon for biocellulose production.

[0026] In embodiments, the base is sodium hydroxide (NaOH), potassium hydroxide (KOH), calcium hydroxide (Ca(OH) 2 ), lithium hydroxide (LiOH), and sodium carbonate (Na 2 CO 3 ) is selected.

[0027] In an embodiment, the amide is selected from urea and thiourea. In a preferred embodiment of the pretreatment solution, the mass ratio of base / amide, i.e. NaOH / urea, is 1.0 / 1.0 to 1.0 / 2.0, preferably 1.0 / 1.5 to 1.0 / 2.0, more preferably 1.0 / 1.5 to 1.0 / 1.8, and the preferred mass ratio is about 1.0 / 1.7.

[0028] The pretreatment step is carried out at -25°C to +30°C with an aqueous solution containing a base (preferably NaOH) and an amide (preferably urea), resulting in energy savings. Suitable temperatures are -25°C to +25°C, preferably -10°C to +25°C, more preferably +10°C to +25°C, most preferably room temperature, i.e. 20°C ± 5°C. Indeed, the use of an aqueous solution containing NaOH and urea at the above temperatures, preferably +15°C to +25°C, results in a pretreated fabric in which the yarns of the fabric swell (but the fibers do not dissolve), creating spaces between the cellulose fibers and making the cellulase enzymes more accessible. At the same time, the degradation and dissolution levels of the cellulose fibers are minimized. A further advantage of the process of the invention is that in blended textile products, such as blended textile products, the method minimizes damage to the polyester portion of the blended textile product, i.e. the degradation of the polyester filaments or fibers is minimized, allowing the polyester material to be recovered and recycled.

[0029] In this process, the aqueous solution of NaOH and urea modifies the crystalline cellulose structure by converting the cellulose I structure to cellulose II structure, similar to the mercerization process that hydrolyzes the amorphous regions of cellulose. Advantageously, it has been observed that when the cellulose has II structure, cellulase enzymes are more effective at converting the cellulose to glucose compared to cellulose with I structure. Natural cotton cellulose is found to be mostly cellulose I structure. After pretreatment with NaOH / urea, the cellulose is mostly cellulose II structure. As mentioned above, the cellulose I structure is less easily converted to glucose by cellulase enzymes compared to the cellulose II structure. In fact, the cellulose I structure is more resistant to enzymatic hydrolysis. Cellulose I has a highly ordered structure, which makes it more difficult for cellulase enzymes to access and hydrolyze the cellulose chains. Cellulose II, on the other hand, has a more disordered structure, which makes it more accessible to cellulase enzymes and easier to hydrolyze. Without being bound to a particular scientific explanation, it has been observed that pretreatment with an aqueous solution of NaOH (or another base) and urea (or another amide) can be used to convert cellulose I to cellulose II, thereby increasing the accessibility of cellulose to cellulase enzymes and increasing the efficiency of cellulose hydrolysis while minimizing the amount of cellulose that dissolves, similar to what occurs in the mercaptanization process.

[0030] Furthermore, treatment with NaOH and urea promotes swelling and dissolution of the amorphous regions of cellulose, allowing for the extraction of impurities, and increases the surface area and reactivity of the fibers, making them ready for enzymatic pretreatment. In other words, the pretreatment process of the present invention increases the surface area of ​​the cellulose fibers in the treated textile, especially the yarn of the fabric, so that they can be contacted with cellulase enzymes, and thus the efficiency of the enzymatic conversion of cellulose to glucose is dramatically increased when the pretreated yarn or fabric is treated with cellulase. Also, the use of aqueous solutions at temperatures between -25°C and +30°C, preferably 0°C to room temperature, can reduce energy consumption and reduce overall costs, especially when the process is carried out at room temperature.

[0031] In other words, the process according to the invention makes it possible to obtain microbial cellulose from waste textile materials at a lower cost than known processes and without compromising the effectiveness of the process. Advantageously, the process according to the invention makes it possible to dramatically reduce the degradation and / or dissolution of cellulose fibers during the pretreatment step, resulting in an efficient conversion of cellulose to glucose. Advantageously, the process according to the invention does not include, i.e. does not require, a step of regenerating solid cellulose after pretreatment with an aqueous solution containing a base, preferably NaOH, and an amide, preferably urea.

[0032] Moreover, the process of the present invention is particularly suitable when the waste textile product contains both natural fibers (e.g. cotton fibers) and synthetic fibers (e.g. polyester fibers). Indeed, the use of an aqueous solution containing a base (preferably NaOH) and an amide (preferably urea) at temperatures between -25°C and +30°C, preferably at room temperature (20°C ± 5°C), results in a pretreated fabric with reduced degradation of polyester fibers (or another synthetic fiber), which can be recovered for recycling and reuse. Advantageously, the process of the present invention effectively and completely converts cellulose to glucose, making it possible to obtain high yields in the production of microbial cellulose, even when the starting textile material is a waste textile material containing cellulose and non-cellulose materials.

[0033] According to an embodiment, the waste textile material comprises cellulose in the form of cellulosic and non-cellulosic fibers.

[0034] In an embodiment, the cellulose fibers are virgin or recycled fibers selected from vegetable fibers, man-made cellulose fibers, recycled vegetable fibers, recycled man-made cellulose fibers, and mixtures thereof. According to an embodiment, the vegetable fibers can be selected from cotton fibers, hemp fibers, flax (linen) fibers, jute fibers, coconut fibers, sisal fibers, abaca fibers (Manila hemp fibers), kapok fibers, ramie fibers, kenaf fibers, agave fibers, henequen fibers, lotus fibers, nettle fibers, sugarcane bagasse fibers, pineapple leaf fibers, banana tree trunk fibers, rice straw fibers, and mixtures thereof. According to an embodiment, the man-made cellulose fibers can be selected from viscose fibers, lyocell fibers, modal fibers, acetate fibers, cupro fibers, carbamate fibers, and mixtures thereof. In an embodiment, the cellulose fibers are selected from cotton fibers, viscose fibers, and mixtures thereof.

[0035] In an embodiment, the non-cellulosic fibers are selected from synthetic fibers, biosynthetic fibers, recycled synthetic fibers, recycled biosynthetic fibers, and mixtures thereof.

[0036] According to an embodiment, the synthetic fibers are polyester fibers, polyamide fibers, elastane fibers, polypropylene (PP) fibers, acrylic fibers, polyurethane fibers, CO 2The polyester fibers are virgin or recycled fibers selected from the group consisting of polyester fibers, polyester-based fibers, and mixtures thereof. For example, the polyester fibers can be poly(ethylene terephthalate) (PET) fibers, polytrimethylene terephthalate (PTT) fibers, poly(butylene terephthalate) (PBT) fibers, polybutylene succinate (PBS) fibers, polybutylene adipate co-terephthalate (PBAT) fibers, polylactic acid (PLA) fibers, or polyhydroxyalkanoate (PHA) fibers. Recycled fibers can also be obtained by making fibers from recycled polymers. For example, recycled polyester fibers can be obtained from recycled polyester polymers obtained from waste textile products, such as cotton-polyester fabrics.

[0037] The biosynthetic fibers can be selected from fossil-derived fibers, bio-derived fibers, and mixtures thereof. The fossil-derived biosynthetic fibers can be selected from polylactic acid fibers (PLA) fibers, polyhydroxyalkanoic acid (PHA) fibers, polyurethane (PU) fibers, polytrimethylene terephthalate (PTT) fibers, polybutylene succinate (PBS) fibers, polybutylene adipate coterephthalate (PBAT) fibers, and mixtures thereof. According to an embodiment, the bio-derived biosynthetic fibers can be selected from bio-derived polylactic acid fibers (bio-PLA) fibers, bio-derived polyhydroxyalkanoic acid (bio-PHA) fibers, bio-derived polyurethane (bio-PU) fibers, bio-derived polytrimethylene terephthalate (bio-PTT) fibers, bio-derived polybutylene succinate (bio-PBS) fibers, bio-derived polybutylene adipate coterephthalate (bio-PBAT) fibers, and mixtures thereof. According to embodiments, the recycled synthetic fibers are selected from recycled polyethylene terephthalate (rPET) fibers, recycled polyamide (nylon) fibers, recycled elastane fibers, recycled polypropylene (PP) fibers, recycled acrylic fibers, recycled polyurethane (PU) fibers, recycled polytrimethylene terephthalate (PTT) fibers, polybutylene succinate (PBS) fibers, and mixtures thereof.

[0038] According to an embodiment, the waste textile material is selected from clothing, fabrics or yarns, and generally the process is carried out on fabrics and clothing. According to an embodiment, the waste textile material is clothing. For example, the fabric or clothing can be a cotton fabric or clothing (i.e. 100% cotton fabric or clothing) or can contain a combination of cotton and / or viscose fibers, possibly polyester fibers and / or elastane fibers. In an embodiment, the waste textile material is a waste textile material comprising viscose (or cotton, or both viscose and cotton), polyester, and elastane. According to an embodiment, the waste textile material is a blended textile material comprising polyester fibers or polyester filaments and cellulose fibers.

[0039] According to an embodiment, the waste textile material can be washed prior to the step of pretreating the waste textile material with an aqueous solution comprising NaOH and urea.

[0040] In an embodiment, non-textile elements optionally present in the waste textile material, such as label tags (e.g. made of leather or polyurethane), buttons, zippers (e.g. made of aluminum, brass or plastic), are removed, optionally after washing, before the step of pretreating the waste textile material with an aqueous solution comprising NaOH and urea. The removal of non-textile elements can be performed manually and / or automatically, using techniques and / or machines known per se in the art.

[0041] According to an embodiment, the process may further comprise a step of sorting the waste textile material before or after the step of pretreating the waste textile material with an aqueous solution containing NaOH and urea. Preferably, the process further comprises a step of sorting the waste textile material before the step of pretreating the waste textile material with an aqueous solution containing NaOH and urea. In an embodiment, the sorting is based on color, the type of dye present in the waste textile material (e.g., indigo, sulfur dye, or black reactive dye), the composition of the textile (e.g., fabric), the mass percentage of cellulose, the non-cellulose content, or a combination thereof. For example, near-infrared (NIR) sorting of textiles (e.g., fabrics and / or clothing) based on color and / or composition of the textile (e.g., fabrics and / or clothing) is known in the art.

[0042] According to an embodiment, the waste textile material contains dyes. If dyes are present, the method of the invention preferably comprises a step of removing at least a portion of the dyes from the waste textile material before the step of treating the textile with cellulase, preferably before the step of pretreating the waste textile with the aqueous solution comprising NaOH and urea. Advantageously, removing dyes from the waste textile material before the enzymatic step with cellulase results in a particularly efficient conversion of cellulose to glucose.

[0043] According to embodiments, the dyes can be removed using techniques known per se in the art. According to embodiments, the dyes can be removed from the waste textile material by a method selected from ozone washing, washing with a reducing solution, extraction of the dyes using, for example, a Soxhlet extractor, and combinations thereof.

[0044] According to an embodiment, the dyed waste textile material is washed with NaOH and sodium dithionite (Na 2 S 2 O 4Dyes can be removed from waste textile materials by treating them with a reducing solution containing sodium dithionite (NaOH). According to an embodiment, the concentration of NaOH in the reducing solution is 1 g / L to 60 g / L, preferably 10 g / L to 30 g / L, and more preferably 15 g / L to 22.5 g / L. The concentration of sodium dithionite (Na 2 S 2 O 4 The concentration of the fluoride is 1 g / L to 30 g / L, preferably 5 g / L to 15 g / L, and more preferably 7.5 g / L to 10 g / L.

[0045] According to an embodiment, the process preferably further comprises a step of reducing the size of the waste textile material after the step of pretreating the waste textile with the aqueous solution containing NaOH and urea. For example, the pretreated textile material can be cut or chopped, optionally after removing at least a part of the dye, before the step of treating the pretreated textile with cellulase. In this case, advantageously, the contact area between the pretreated textile material and the cellulase is increased. In an embodiment, the pretreated textile in step b) is chopped into a plurality of pieces having dimensions suitable for enzymatic saccharification before step c). For example, the fibers obtained in step b) are chopped into a plurality of pieces having an average dimension of 0.5 mm or less before step c). 2 (0.005cm 2 ) ~ 2500mm 2 (25cm 2 ), preferably 1 mm 2 (0.01cm 2 ) ~ 625mm 2 (6.25cm 2 ), more preferably 10 mm 2 (0.1cm 2 )~400mm 2 (4cm 2 ), for example, if the area is 100 mm 2 is shredded into multiple pieces.

[0046] Furthermore, by pretreating the waste textile material before shredding, the amount of cellulose dissolved in the pretreatment step is reduced. That is, the amount of cellulose dissolved during pretreatment with the aqueous solution containing NaOH and urea is reduced without endangering the enzymatic conversion of cellulose to glucose. Furthermore, if the waste textile material contains non-cellulosic fibers, such as polyester fibers, cutting or shredding the textile material after the pretreatment step can reduce the amount of non-cellulosic material (such as polyester) that may be lost due to cutting or shredding before the pretreatment step. Also, if the waste textile material contains non-cellulosic fibers, such as polyester fibers, cutting or shredding the textile material after the pretreatment step can reduce or avoid the adverse effects that the NaOH / urea solution may have on the non-cellulosic material (such as polyester). Advantageously, cutting or shredding the textile material before the pretreatment step with the aqueous solution containing NaOH and urea can recover more non-cellulosic material (e.g., polyester fibers) because some of the polyester particles are lost to the NaOH / urea solution when the textile material is cut or shredded after the pretreatment step.

[0047] Shredding can be done mechanically, as known in the art. In one embodiment, the waste textile product is transferred to an insulated container and liquid nitrogen is poured onto the waste textile product. The frozen waste textile product thus obtained is ground until pieces of 1 mm to 5 mm are obtained. An average size of 1 mm is preferred. The reduced size particles are then treated by the process steps of the invention, such as cellulase treatment. Advantageously, the size of the pretreated fabric can be quite large, for example about 180 cm in width and 4 to 6 m in length. Similarly, garments from which non-textile elements have been removed can be pretreated first and then shredded only after pretreatment with NaOH / urea.

[0048] As mentioned above, the process of pretreating waste textile materials with an aqueous solution containing NaOH and urea results in improved results in terms of time and efficiency of enzymatic conversion of textile cellulose to glucose by cellulase. Without being bound to a particular scientific explanation, it has been observed that the present invention, which pretreats waste textile materials with an aqueous solution containing NaOH and urea at room temperature between -25°C and +30°C, preferably +10°C and +25°C, more preferably +15°C and +25°C, swells the textile material and allows for effective conversion of cellulose to glucose using cellulase enzymes. In other words, it has been observed that the pretreatment of the present invention causes separation of the fibers of the textile (e.g., increasing the distance between the fibers), an effect also known as swelling, allowing cellulase enzymes to effectively access the cellulose chains, thereby effectively converting cellulose to glucose.

[0049] According to an embodiment, the aqueous solution containing NaOH and urea contains 1 w / v% to 15 w / v% (mass volume percent), preferably 2 w / v% to 10 w / v%, more preferably 3 w / v% to 9 w / v% NaOH. For example, the aqueous solution containing NaOH and urea may contain 6 w / v% to 8 w / v%, for example 7 w / v% NaOH.

[0050] According to an embodiment, the aqueous solution containing NaOH and urea contains 1 w / v% to 25 w / v%, preferably 3 w / v% to 20 w / v%, more preferably 5 w / v% to 15 w / v% urea. For example, the aqueous solution containing NaOH and urea may contain 11 w / v% to 13 w / v%, for example 12 w / v% urea.

[0051] According to an embodiment, in the step of pretreating the waste textile material with the aqueous solution containing NaOH and urea, the mass of the waste textile material is in the range of 1 w / v% to 20 w / v%, preferably 2 w / v% to 15 w / v%, more preferably 2.5 w / v% to 10 w / v% with respect to the volume of the aqueous solution containing NaOH and urea. For example, the mass of the waste textile material can be in the range of 3 w / v% to 7 w / v%, preferably 3.5 w / v% to 6.5 w / v%, more preferably 4 w / v% to 6 w / v%, for example 5 w / v%, with respect to the volume of the aqueous solution containing NaOH and urea.

[0052] According to an embodiment, the pretreatment of the waste textile material with the aqueous solution containing NaOH and urea is carried out at a temperature between -15°C and +25°C, preferably at room temperature, ie between +15°C and +25°C.

[0053] According to an embodiment, the step of pretreating the waste textile material with the aqueous solution containing NaOH and urea has a duration of 0.5 hours to 10 hours, preferably 1 hour to 8 hours, more preferably 2 hours to 7 hours. For example, the step of pretreating the waste textile material with the aqueous solution containing NaOH and urea can have a duration of 4 hours to 6 hours, for example 5 hours.

[0054] For example, the pretreatment of the waste textile material can be carried out at -15°C to +25°C, preferably at room temperature, for 1 hour to 8 hours, more preferably 2 hours to 7 hours, using an aqueous solution containing 3 w / v% to 9 w / v%, preferably 6 w / v% to 8 w / v% NaOH and 5 w / v% to 15 w / v%, preferably 11 w / v% to 13 w / v% urea. In one embodiment, a pretreatment solution containing about 7 w / v% NaOH, 12 w / v% urea is used at room temperature for 2 hours to achieve the required separation of fibers (e.g., separation by fiber swelling) of cotton / polyester blend fabric (5 w / v%).

[0055] According to an embodiment, the pretreated textile product obtained after the step of pretreatment with an aqueous solution containing NaOH and urea is washed. The washing can be carried out, for example, with a weak acid solution (for example, an acetic acid solution) or with water. The water can be, for example, tap water, distilled water, reverse osmosis water, or a mixture thereof. The washing is preferably carried out at 10°C to 30°C, preferably 15°C to 28°C, for example 25°C. According to an embodiment, after the washing step, the pH of the pretreated textile product after aqueous extraction is 6 to 8, preferably 6.5 to 7.5, for example 7. The pH of the pretreated textile product after aqueous extraction is measured according to the standard ISO 3071:2020.

[0056] According to an embodiment, after the step of pretreatment with an aqueous solution containing NaOH and urea, and after washing if necessary, the resulting textile product is dried. For example, drying is carried out in industrial dryers known per se in the art, such as rotary dryers or conveyor belt dryers, at temperatures between 50°C and 100°C, preferably between 70°C and 90°C, for example at 90°C. According to an embodiment, the textile product obtained after the step of pretreatment with an aqueous solution containing NaOH and urea, after washing if necessary and drying if necessary, is cut or chopped (for example into small pieces or fragments) in order to reduce the size of the pretreated textile material. For example, the textile product obtained after the step of pretreatment with an aqueous solution containing NaOH and urea, may be cut or chopped (for example into small pieces or fragments) in order to reduce the size of the pretreated textile material. 2 (0.005cm 2 )~2500mm 2 (25cm 2 ), preferably 1 mm 2 (0.01cm 2 )~625mm 2 (6.25cm 2 ), more preferably 10 mm 2 (0.1cm 2 )~400mm 2 (4cm 2 ), e.g. 100mm 2 (1cm 2 The material is cut or chopped into a number of pieces, each of which is about 1x1 cm.

[0057] According to an embodiment, after the step of pretreating the textile product with an aqueous solution containing NaOH (or another base) and urea (or another amide), the aqueous solution containing NaOH (or another base) and urea (or another amide) can be reused. According to an embodiment, the aqueous solution containing NaOH (or another base) and urea (or another amide) can be reused 1 to 20 times, preferably 5 to 15 times, more preferably 8 to 12 times, for example 10 times. In an embodiment, the concentrations of NaOH (or another base) and urea (or another amide) can be adjusted as necessary before reuse. For example, the NaOH concentration can be adjusted to a range of 1 w / v% to 15 w / v%, preferably 2 w / v% to 10 w / v%, more preferably 3 w / v% to 9 w / v%, as necessary. For example, the urea concentration can be adjusted to a range of 1 w / v% to 25 w / v%, preferably 3 w / v% to 20 w / v%, more preferably 5 w / v% to 15 w / v%, as necessary.

[0058] According to an embodiment, the step of pre-treating the waste textile material with the aqueous solution comprising NaOH and urea is carried out in a reaction chamber, and the aqueous solution comprising NaOH and urea is supplied to the waste textile material in the reaction chamber and circulated through the waste textile. Preferably, the waste textile is in a stationary, i.e. static state, and the solution comprising NaOH and urea is circulated through the waste textile to provide a pre-treated textile. Circulating the aqueous solution comprising NaOH and urea through the waste textile allows for particularly short pre-treatment times.

[0059] The term "circulated" in reference to the aqueous solution comprising NaOH (or another base) and urea (or another amide) is defined as a forced flow of the solution through the textile and through the reaction chamber in which the textile is held. This flow is preferably achieved by a pump that feeds the solution into the reaction chamber and passes it through the textile and the reaction chamber. The solution leaves the reaction chamber and then returns to the reaction chamber and circulates again through the textile and the reaction chamber. According to an embodiment, when washing the pretreated textile obtained after the step of pretreatment with the aqueous solution comprising NaOH and urea, the washing solution can also be circulated through the textile several times, as can the solution comprising NaOH and urea. In an embodiment, a plant carrying out the step of pretreatment of the waste textile material with the aqueous solution comprising NaOH and urea typically comprises a fluid circuit including an inlet and an outlet to the reaction chamber. Preferably, in this embodiment, the liquor ratio, i.e. the mass of fabric to the volume of the solution, is 5 w / v % with respect to the volume of the aqueous solution comprising NaOH and urea.

[0060] The term "quiescent" or "static" state is defined as a textile article contained in a reaction chamber and held there while an aqueous solution (or wash solution) comprising NaOH and urea is pumped through the textile article. The textile article fills the reaction chamber so as not to move with the solution, i.e., not to be displaced under the action of the solution flow. In an embodiment, the textile article is compressed in the reaction chamber.

[0061] According to one embodiment, the process of the invention further comprises a step of treating the textile material obtained by pretreatment with an aqueous solution comprising NaOH and urea with cellulase in order to convert the cellulose present in the textile to glucose.

[0062] According to an embodiment, the pretreated textile material is treated with a solution containing cellulase, i.e., a cellulase enzyme.

[0063] According to the embodiment, the mass of the pretreated textile material relative to the volume of the solution containing cellulase is 1 w / v% to 20 w / v%, preferably 2 w / v% to 15 w / v%, more preferably 2.5 w / v% to 10 w / v%. For example, 5 g of pretreated waste textile product can be treated with 100 mL of the solution containing cellulase. In this case, the mass of the pretreated textile material is 5 w / v% relative to the volume of the solution containing cellulase.

[0064] According to an embodiment, the cellulase is in an amount such that the enzymatic activity is 1 FPU (Filter Paper Unit) per gram of cellulose to 50 FPU per gram of cellulose, preferably 10 FPU per gram of cellulose to 30 FPU per gram of cellulose, more preferably 15 FPU per gram of cellulose to 25 FPU per gram of cellulose. The enzymatic activity of cellulase can be measured according to methods known per se in the art. For example, the enzymatic activity of cellulase can be measured according to Adney B. and Baker J., "Measurement of Cellulase Activity", National Renewable Energy Laboratory, 1996, or Selig M., Weiss N., and Ji Y., "Enzymatic Saccharification of Lignocellulosic Biomass", National Renewable Energy Laboratory, 2008. Cellulases suitable for use according to the present invention are known per se in the art. For example, suitable currently commercially available products may be used: Novozymes Cellic® CTec3 HS, AB Enzyme - Flashzyme Plus 200, Novozymes Cellic® CTec2, and Novozymes Cellusoft® AB Conc.

[0065] According to an embodiment, the enzymatic step of treating the pretreated textile material with cellulase is carried out at 30° C. to 70° C., preferably 40° C. to 60° C., more preferably 45° C. to 55° C. For example, the step of treating the pretreated textile material with cellulase can be carried out at 50° C.

[0066] According to an embodiment, the step of treating the pretreated textile material with cellulase is carried out for 10 minutes to 144 hours, preferably 30 minutes to 96 hours, more preferably 12 hours to 72 hours, even more preferably 18 hours to 48 hours, and even more preferably 20 hours to 36 hours. For example, the step of treating the pretreated textile material with cellulase can be carried out for 24 hours.

[0067] According to an embodiment, the step of treating the pretreated textile material with cellulase can be carried out with stirring at 5 rpm to 200 rpm (revolutions per minute), for example 50 rpm to 100 rpm. Preferably, the enzymatic step of treating the pretreated textile material with cellulase is carried out without stirring.

[0068] According to an embodiment, the step of treating the pretreated textile material with cellulase is carried out at a pH of 3.0 to 6.0, preferably at a pH of 4.0 to 5.0. For example, the step of treating the pretreated textile material with cellulase can be carried out at a pH of 5.0.

[0069] According to an embodiment, the pretreated textile material contains a dye, and at least a portion of the dye is removed from the pretreated textile material, in other words, in an embodiment, after the step of pretreating the waste textile material with an aqueous solution containing NaOH and urea, at least a portion of the dye can be removed before the step of treating the pretreated textile material with cellulase.

[0070] In a preferred embodiment, the pretreated textile material is undyed, in other words, in an embodiment, the step of treating the pretreated textile material with cellulase is carried out on an undyed pretreated textile material.

[0071] For example, the step of treating the pretreated textile material with cellulase can be carried out without stirring using an aqueous solution containing cellulase enzyme at 1 FPU (Filter Paper Unit) per gram of cellulose to 50 FPU per gram of cellulose, preferably 10 FPU per gram of cellulose to 30 FPU per gram of cellulose, and more preferably 15 FPU per gram of cellulose to 25 FPU per gram of cellulose, at 30°C to 70°C, preferably 40°C to 60°C, and more preferably 45°C to 55°C, for 10 minutes to 144 hours, preferably 30 minutes to 96 hours, more preferably 12 hours to 72 hours, even more preferably 18 hours to 48 hours, and even more preferably 20 hours to 36 hours.

[0072] According to an embodiment, at the end of the process of treating the pretreated textile material with cellulase, a mixture is obtained that includes a solid phase and a liquid phase. For example, the solid phase can include non-cellulosic fibers (e.g., polyester fibers) that were contained in the waste textile material, and, if necessary, insoluble dyes (e.g., indigo dyes and sulfur dyes), and, if necessary, undigested cellulose fibers and materials. For example, the liquid phase can include the cellulase solution used in the treatment of the pretreated textile material, glucose, and, if necessary, soluble dyes (e.g., reactive black dyes), if present.

[0073] According to one embodiment, the process of the invention comprises a step of separating the liquid phase from the solid phase to obtain a liquid mixture comprising glucose.

[0074] According to an embodiment, when the waste textile material comprises non-cellulosic fibers, the non-cellulosic fibers are recovered from the solid phase of the mixture comprising solid and liquid phases, for example after the separation step.

[0075] According to an embodiment, the separation of the liquid phase from the solid phase can be performed by gravity, preferably by waiting for the heavier substances (polyester, elastane) to settle to the bottom of the reactor before draining the supernatant liquid phase. Additionally or alternatively, the separation of the liquid phase from the solid phase can include a step of filtration or multi-stage filtration (also known as sequential cascade filtration), preferably through sieves with a pore size of 0.3 mm to 0.5 cm, preferably through centrifugation at a speed of 5000 rpm (revolutions per minute) to 50000 rpm, or a combination thereof. For example, in an embodiment, the mixture comprising the solid and liquid phases can be filtered, preferably using a sieve with a pore size of 0.3 mm. In an embodiment, the mixture comprising the solid and liquid phases, or the liquid phase, can be centrifuged, for example, at 9000 rpm for 30 minutes. The supernatant obtained after centrifugation can be collected as a liquid mixture comprising glucose. In other words, after a separation step, for example after separating the liquid phase from the solid phase (e.g. via filtration or multi-stage filtration, centrifugation, or using a combination thereof), the resulting liquid phase can be recovered as a liquid mixture comprising glucose. A suitable separator is a clarifier, in particular a clarifier for foodstuffs.

[0076] According to an embodiment, the cellulase enzyme can be recovered from the liquid phase, and preferably reused. The cellulase enzyme can be recovered using techniques known per se in the art, such as, for example, dialysis or ultrafiltration. According to an embodiment, the recovered cellulase enzyme can be reused 1 to 10 times, preferably 2 to 8 times, more preferably 2 to 5 times, for example 3 times. In an embodiment, the amount of cellulase can be adjusted as needed. For example, the amount of cellulase can be adjusted for reuse, as needed, so that the enzyme activity is 1 FPU (Filter Paper Unit) per gram of cellulose to 50 FPU per gram of cellulose, preferably 10 FPU per gram of cellulose to 30 FPU per gram of cellulose, more preferably 15 FPU per gram of cellulose to 25 FPU per gram of cellulose.

[0077] According to embodiments, the cellulase enzymes can be recovered and reused to treat the solid phase obtained after the separation step and / or to treat one or more additional pretreated waste textile materials.

[0078] According to an embodiment, the cellulase enzyme can be recovered and reused, for example, 1-10 times, preferably 2-8 times, more preferably 2-5 times, for example 3 times, to treat the solid phase obtained after the separation step. Reusing the cellulase enzyme to treat the solid phase obtained after the separation step allows digestion of cellulose fibers and materials that were not digested in the previous treatment or treatments with cellulase, thereby improving the conversion yield of cellulose to glucose. The enzymatic treatment of the solid phase further results in a mixture comprising a solid phase and a liquid phase as described above.

[0079] According to an embodiment, the cellulase enzyme can be recovered and reused, for example, 1 to 10 times, preferably 2 to 8 times, more preferably 2 to 5 times, for example 3 times, to treat one or more additional pretreated waste textile materials.

[0080] According to an embodiment, at least a portion of the dye can be removed and / or recovered from the solid phase or the liquid phase of the mixture comprising solid and liquid phases, preferably after the step of separating the liquid phase from the solid phase. For example, when the dye is removed and / or recovered from the liquid phase, the dye can be removed from the liquid phase by passing the liquid phase through an activated carbon column.

[0081] According to one embodiment, the process of the present invention comprises a step of preparing a microbial culture using the glucose-containing mixture, preferably obtained after the separation step, said microbial culture comprising a microbial cellulose-producing fungus.

[0082] According to an embodiment, the step of preparing a microbial culture using a mixture containing glucose includes a step of concentrating the mixture containing glucose, if necessary, to increase the concentration of the glucose. Advantageously, concentrating the mixture containing glucose reduces the volume of the mixture, which facilitates handling and, if necessary, storage of the mixture. According to an embodiment, the concentrating step can be performed using a heat exchanger, a rotary evaporator, a vacuum evaporator, or a combination thereof. By treating the mixture containing glucose in a heat exchanger, for example, at 100° C. for 1 hour to 12 hours, the concentration of glucose in the mixture containing glucose can be increased, if necessary, depending on the volume of the mixture containing glucose to be concentrated and / or the final glucose concentration obtained.

[0083] According to an embodiment, the amount of glucose in a mixture containing glucose can be measured using the 3,5-dinitrosalicylic acid (DNS) method. The DNS method is a method known in the art. The DNS method is disclosed, for example, in Ghose, TK, 1987, "Measurement of cellulase activity", Pure & Applied Chemistry 59:257-268 and Miller GL, 1959, "Use of dinitrosalicylic acid reagent for the measurement of reducing sugars", Analytical Chemistry 31:426-428.

[0084] In an embodiment, the rate at which cellulose is converted to glucose is determined. Preferably, the rate at which cellulose is converted to glucose is calculated using the following formula: Cellulose conversion rate (%) = ((Glucose released by enzymatic hydrolysis (g / L) × reaction volume (L)) / (Substrate mass (g) × cellulose content (%)) × 0.9 × 100% Here, "glucose released from the enzyme solution" is determined using the DNS method. "Reaction volume" is the volume of the solution containing cellulase used to treat the pretreated textile. "Substrate mass" is the initial mass of the waste textile material. "Cellulose content" is the amount of cellulose in the waste textile material expressed as a percentage of the initial mass of the waste textile material, and "0.9" is the correction factor for the water molecules added during the hydrolysis of cellulose.

[0085] According to an embodiment, the step of preparing a microbial culture using the mixture containing glucose includes a step of adjusting the concentration of glucose in the mixture containing glucose to a concentration of 10 g / L to 30 g / L, preferably 15 g / L to 25 g / L. According to an embodiment, including the step of adjusting the concentration of glucose in the mixture containing glucose can be performed by concentrating the mixture containing glucose, by diluting the mixture containing glucose, or by a combination thereof. For example, after concentrating the mixture containing glucose and measuring the amount of glucose in the concentrated mixture containing glucose, it can be diluted to obtain a required concentration of glucose, for example, a concentration of glucose of 10 g / L to 30 g / L, preferably 15 g / L to 25 g / L. In an embodiment, the mixture containing glucose can be diluted to obtain a required concentration without concentrating it. In an embodiment, when cellulase is removed by dialysis from the liquid phase obtained after the separation step, the glucose concentration in the mixture containing glucose is reduced. In this case, the concentration of glucose in the mixture can be adjusted to obtain a required concentration of glucose, for example, a concentration of glucose of 10 g / L to 30 g / L, preferably 15 g / L to 25 g / L.

[0086] According to an embodiment, the mixture containing glucose is sterilized, preferably sterilized by autoclaving. In this case, advantageously, enzymes that may be present in the mixture are inactivated and can be used as an amino acid source for the microbial cellulose producer. In an embodiment, the cellulase enzyme is not removed from the liquid phase obtained after the separation step. In an embodiment, the concentration of the amino acids in the mixture can be adjusted as necessary. For example, the concentration of the amino acids in the mixture can be adjusted by adding peptone to the mixture. For example, if the enzyme is recovered and reused to treat additional pretreated textile products, additional nitrogen and carbon sources (such as peptone) can be added. In fact, the enzymatic treatment of each additional textile product increases the glucose in the mixture, resulting in a deficiency in the amount of amino acids in the mixture containing glucose. In an embodiment, if the enzyme is recovered and reused to treat additional pretreated textile products, the cellulase enzyme is not removed from the liquid phase obtained after the separation step performed after the enzymatic treatment of the last textile product. In embodiments, if the cellulase enzyme is recovered and reused in the treatment of the solid phase obtained after the separation step (i.e., a second enzymatic treatment performed on the solid phase obtained from the single starting waste textile material), additional nitrogen and carbon sources (such as peptone) may not be required. In embodiments, if the cellulase enzyme is recovered and reused in the treatment of the solid phase obtained after the separation step (i.e., a second enzymatic treatment performed on the solid phase obtained from the single starting waste textile material), the cellulase enzyme is not removed from the liquid phase obtained after the final separation step performed after the final enzymatic treatment.

[0087] According to one embodiment, the mixture containing glucose preferably has a glucose concentration of 10 g / L to 30 g / L, preferably 15 g / L to 25 g / L, for example 20 g / L, and can be used as a "waste textile glucose" (WTG) medium for the preparation of microbial cultures.

[0088] According to an embodiment, the step of preparing a microbial culture using a mixture comprising glucose comprises mixing the mixture comprising glucose with a starter microbial culture comprising a microbial cellulose producer.

[0089] According to an embodiment, the amount of the mixture containing glucose in the microbial culture is 99% by mass to 80% by mass, preferably 95% by mass to 85% by mass, of the mass of the microbial culture.

[0090] According to an embodiment, the amount of the starter microbial culture containing the microbial cellulose-producing bacteria in the microbial culture is 1% by mass to 20% by mass, preferably 5% by mass to 15% by mass, of the mass of the microbial culture.

[0091] As used herein, the term "starter microbial culture" refers to a culture of bacteria that is usually used in small amounts to inoculate a batch of media to ferment. A starter culture is usually the microbiological culture that actually does the fermentation and is added to the media to initiate the fermentation process.

[0092] According to an embodiment, the step of preparing a microbial culture using the mixture comprising glucose comprises adding at least one additive to the mixture comprising glucose, the additive being preferably selected from titanium(IV) bis(ammonium lactate) dihydroxide (TiBALDH), glycerol, ascorbic acid, ethephon (2-chloroethyl phosphate) and mixtures thereof.

[0093] Advantageously, the use of one or more additives increases the amount of microbial cellulose (eg, bacterial cellulose) obtained compared to the amount obtained without the use of an additive.

[0094] According to an embodiment, the additive is titanium(IV) bis(ammonium lactate) dihydroxide (TiBALDH), preferably at 0.0005 w / v% to 1 w / v%, more preferably at 0.0025 w / v% to 0.4 w / v%, even more preferably at 0.05 w / v% to 0.3 w / v%, for example 0.25 w / v%.

[0095] According to an embodiment, the additive is glycerol, preferably 0.1 w / v% to 10 w / v%, more preferably 0.5 w / v% to 2 w / v%, even more preferably 0.75 w / v% to 1.5 w / v%, for example 1 w / v%.

[0096] According to an embodiment, the additive is ascorbic acid, preferably at 0.05 w / v% to 10 w / v%, more preferably at 0.25 w / v% to 2 w / v%, even more preferably at 0.3 w / v% to 1 w / v%, for example 0.5 w / v%.

[0097] According to an embodiment, the additive is ethephon (2-chloroethyl phosphate), preferably at 0.001 mM to 10 mM, more preferably at 0.005 mM to 2 mM, even more preferably at 0.01 mM to 1 mM, for example 0.01 mM.

[0098] According to an embodiment, the additive is a mixture of glycerol and titanium(IV) bis(ammonium lactate) dihydroxide (TiBALDH), the glycerol being added to the mixture containing glucose preferably at 0.1 w / v% to 10 w / v%, more preferably at 0.5 w / v% to 2 w / v%, even more preferably at 1 w / v%, and the titanium(IV) bis(ammonium lactate) dihydroxide (TiBALDH) being added to the mixture containing glucose preferably at 0.0005 w / v% to 1 w / v%, more preferably at 0.0025 w / v% to 0.4 w / v%, even more preferably at 0.25 w / v%.

[0099] As used herein, the term "microorganism" refers to an organism that is too small to be seen by the naked eye. As used herein, the term "microorganism" includes both non-genetically modified (i.e., wild-type) and genetically modified microorganisms.

[0100] According to an embodiment, the microbial cellulose producer is selected from bacteria, algae, yeast, and mixtures thereof. According to an embodiment, the microbial cellulose producer may be a genetically modified microorganism. In a preferred embodiment, the microbial cellulose producer is a bacterium.

[0101] In embodiments, the microbial cellulose can be selected from microbial cellulose produced by bacteria (i.e., bacterial cellulose), microbial cellulose produced by algae, microbial cellulose produced by yeast, and mixtures thereof. According to embodiments, the microbial cellulose can be selected from microbial cellulose produced by bacteria (i.e., bacterial cellulose), microbial cellulose produced by algae, and mixtures thereof. Preferably, the microbial cellulose is bacterial cellulose.

[0102] According to an embodiment, the microbial cellulose producing bacteria is selected from Gluconacetobacter, Glyconacetobacter, Komagateibacter, Glyconacetibacter, Aerobacter, Glyconacetobacter, Acetobacter, Glyconacetobacter, Achromobacter, Glyconacter, Agrobacterium, Glyconacter, Azotobacter, Glyconacter, Salmonella, Glyconacter, Alcaligenes, Glyconacter, Pseudomonas, Glyconacter, Rhizobium, Glyconacter, Sarcina, Glyconacter, Glyconacter, Enterobacter, Escherichia, Glyconacter, Bacillus, Glyconacter, Klebsiella, Glyconacter, and mixtures thereof. According to a preferred embodiment, the microbial cellulose producing bacterium is selected from Gluconacetobacter hansenii, Gluconacetobacter xylinus, Komagateibacter xylinus, and mixtures thereof. According to a preferred embodiment, the bacterial cellulose producing bacterium is selected from Gluconacetobacter hansenii ATCC 53582, Gluconacetobacter xylinus ATCC 23770, Komagateibacter xylinus DSM46604, and mixtures thereof. For example, the bacterial cellulose producing bacterium can be Gluconacetobacter hansenii ATCC 53582 bacterium.

[0103] According to an embodiment, the microbial cellulose-producing algae is selected from brown algae, green algae, red algae, brown algae, ascomycetes, Chlorella, Nannochloropsis, Ulva, Cladophora, Valonia, and mixtures thereof. According to an embodiment, the microbial cellulose-producing algae is selected from Ascopyrum nodosum, Chlorella vulgaris, Nannochloropsis gaditana, Ulva prolifera, Ulva pertusa, Cladophora glomerata, Valonia ventricosa, and mixtures thereof. It is known in the art that heterotrophic and mixotrophic cultivation of algae under dark conditions requires glucose as a carbon source.

[0104] Cellulose-producing yeasts are known, for example, in “First report of biocellulose production by indigenous yeasts” Jasme, Nurshafqah et al. (2022) Pichia kudriavzevii USM-YBP2. Green Processing and Synthesis. Vol 11 issue 1.

[0105] According to one aspect, the process of the present invention comprises culturing a microbial culture to obtain microbial cellulose. In an embodiment, a bacterial culture is cultivated to obtain bacterial cellulose.

[0106] According to an embodiment, the culturing step is carried out at 15°C to 35°C, preferably 20°C to 30°C. For example, the culturing step can be carried out at 25°C to 30°C, for example 28°C.

[0107] According to an embodiment, the culture step can be performed for 1 to 30 days, preferably for 5 to 20 days, more preferably for 10 to 16 days. For example, the culture step can be performed for 13 to 15 days, for example, for 14 days.

[0108] In an embodiment, the starter culture medium may be Hestrin-Schramm (HS) medium and may have, for example, the following composition: glucose 20.0 g / L, peptone from soybean enzymatic digest 5.0 g / L, yeast extract 5.0 g / L, disodium hydrogen phosphate dihydrate 3.4 g / L, citric acid monohydrate 1.5 g / L, distilled water 1.0 L. In an embodiment, the mixture containing glucose prior to addition of the starter culture can have, for example, 20.0 g / L glucose derived from the enzymatic degradation of cellulose in waste textile material, 2.85 mL / L peptone derived from degraded cellulase enzymes, 10.5 g / L citric acid derived from the citrate buffer used in the cellulase enzyme treatment, and 1.0 L of used water derived from the mixture used in the cellulase enzyme treatment.

[0109] According to an embodiment, the mixture containing glucose and the starter culture can be mixed at a volume ratio of glucose:mixture containing starter culture of 99:1 to 80:20, preferably 95:5 to 85:15, for example 90:10.

[0110] The culture containing the microbial cellulose-producing fungus can be cultivated, for example, in one or more sterile containers. The container can be covered or uncovered. It is preferable that the container is covered. For example, the container can be provided with a cover that acts as a physical barrier (i.e., a barrier that is not permeable to air, e.g., a plastic lid) or a cover that acts as a partial physical barrier (e.g., a spunbond nonwoven layer with high air permeability, or a meltblown nonwoven layer with low air permeability).

[0111] The culture can be carried out for 1 to 30 days, preferably 5 to 20 days, more preferably 10 to 16 days, at 15° C. to 35° C., preferably 20° C. to 30° C. For example, the culture step can be carried out at 25° C. to 30° C., e.g., 28° C., for 13 to 15 days, e.g., 14 days.

[0112] According to embodiments, the resulting microbial cellulose (eg, bacterial cellulose) is washed and, if necessary, dried.

[0113] According to an embodiment, the cleaning is carried out with an aqueous solution containing a bleaching agent. In an embodiment, the bleaching agent is NaOCl, NaOH, H 2 O 2 , or mixtures thereof. In a preferred embodiment, the bleaching agent is NaOCl. According to an embodiment, the cleaning is performed with an aqueous solution containing 0.01 w / v% to 10 w / v%, preferably 0.1 w / v% to 0.05 w / v% NaOCl.

[0114] According to an embodiment, the mass ratio of microbial cellulose layer / washing liquid is 1 / 10, preferably 1 / 4.

[0115] According to an embodiment, washing is performed using an aqueous solution containing 0.01 w / v % to 10 w / v %, preferably 1 w / v % to 5 w / v %, NaOH.

[0116] According to an embodiment, the washing is performed with 0.01 w / v% to 10 w / v%, preferably 1 w / v% to 5 w / v% H 2 O 2 The reaction is carried out using an aqueous solution containing

[0117] According to an embodiment, the step of washing the microbial cellulose (e.g., bacterial cellulose) is carried out at 20°C to 80°C, preferably 25°C to 50°C, more preferably 25°C to 35°C. The step of washing the bacterial cellulose is carried out at 30±2°C. According to an embodiment, the step of washing the microbial cellulose is carried out on the microbial cellulose placed in a laundry bag. For example, the laundry bag can be made of a fabric having a mesh size of 50 micrometers to 100 micrometers, preferably 75 micrometers.

[0118] According to an embodiment, the step of washing the microbial cellulose (e.g., bacterial cellulose) can be performed while stirring at 5 rpm (revolutions per minute) to 250 rpm, preferably 50 rpm to 75 rpm. For example, the step of washing the microbial cellulose (e.g., bacterial cellulose) can be performed while stirring at 100 rpm.

[0119] Advantageously, the method of the invention allows obtaining microbial cellulose, in particular bacterial cellulose, with a low content of inorganic compounds.Advantageously, the content of inorganic substances in the microbial cellulose of the invention is less than 1% by weight, as measured by residues on ignition (ash content) at 525° C., according to ISO 1762:2019.

[0120] As mentioned above, one advantage of the process of the present invention is that it minimizes damage to the polyester portion of a blended textile product, such as a blended fabric, i.e., minimizes degradation of the polyester filaments or fibers in order to recover and recycle the polyester material.

[0121] The present invention therefore also relates to a process for recycling polyester fibres or blended fibre products comprising polyester filaments and cellulosic fibres, said process comprising the steps of: g) preparing a waste textile material; h) pretreating the waste textile material with an aqueous solution containing NaOH and urea at -25°C to +30°C to obtain a pretreated textile material; i) treating the pretreated textile material with cellulase to convert the cellulose to glucose to obtain a mixture comprising a liquid phase and a solid phase comprising polyester fibers or polyester filaments; j) separating the liquid phase from the solid phase to obtain a liquid mixture comprising glucose; and k) recovering the polyester fibers or polyester filaments from the solid phase.

[0122] All the features described herein with respect to the process for producing microbial cellulose from waste textile materials and the process for enzymatic saccharification of waste textile materials also apply to the above-mentioned method for recycling polyester fibers or blended fibers comprising polyester filaments and cellulose fibers.

[0123] FIG. 1 summarizes in schematic form an exemplary embodiment of the process of the present invention as follows:

[0124] The waste textile material is collected and washed to make it clean if necessary (block 1 in FIG. 1). The waste textile material comprises cellulose, e.g. natural cellulose fibers such as cotton fibers and / or regenerated cellulose fibers such as viscose fibers, and may optionally further comprise non-cellulosic fibers such as polyester and / or elastane. For example, the waste textile material may be selected from yarns, fabrics, garments, and combinations thereof.

[0125] After collection and washing of the waste textile material, if necessary, non-textile elements such as label tags (e.g. made of leather or polyurethane), buttons and zippers (e.g. commonly made of aluminium, brass or plastic) are removed from the waste textile material manually or automatically (using machines and equipment known per se in the art) (block 2 in Figure 1).

[0126] The waste textile material is then sorted, for example, based on color, the type of dye present in the waste textile material (e.g., indigo, sulfur dyes, or black reactive dyes), or the composition of the textile (e.g., fabric) (e.g., a 100% cotton textile can be separated from a fiber that contains both cotton and polyester fibers). For example, near-infrared (NIR) sorting of textiles (e.g., fabrics and / or clothing) based on color and / or composition of the textile (e.g., fabrics and / or clothing) is known in the art (Block 3 of FIG. 1).

[0127] If the waste textile material contains one or more dyes, e.g., the fabric is washed with NaOH and sodium dithionite (Na 2 S 2 O 4 It is preferred to remove the dye by treatment with a reducing solution of (block 4 in FIG. 1).

[0128] The waste textile material is pretreated with an aqueous solution containing NaOH and urea at a temperature ranging from -25°C to +30°C in order to swell the yarns and fibrillate the cellulose fibers (block 5). The pretreatment step can be carried out for different times depending on the temperature and concentration of the pretreatment solution. Typical treatment times are 1 hour to 8 hours, more preferably 2 hours to 5 hours. The treated textile material can be washed, for example, with a weak acid solution (e.g., acetic acid solution) or with water (block 5 in FIG. 1). The pretreated textile material is preferably dried after washing. The pretreated waste textile material is preferably shredded to reduce the size of the waste textile material and increase the surface area available for contact with the solution containing cellulase enzymes (block 5a in FIG. 1). The aqueous solution containing NaOH and urea can be reused, if necessary, for example up to 20 times in the pretreatment of further waste textile material, and the concentration of NaOH and / or urea can be adjusted for reuse, if necessary.

[0129] After the pretreatment and washing steps, the thus obtained textile material (preferably dried and chopped textile material) is contacted with a solution containing cellulase enzymes in order to convert the cellulose fibers of the textile material to glucose (Block 6). Preferably, the step of treating the pretreated textile material with cellulase is carried out without stirring at a pH range of 4.0-5.0. At the end of the enzymatic conversion of the cellulose fibers to glucose, a mixture is obtained comprising a solid phase and a liquid phase (Block 6 in FIG. 1).

[0130] The solid phase includes non-cellulosic fibers (e.g., polyester and / or elastane fibers), undigested cellulosic fibers, and insoluble dyes, if still present (such as indigo and sulfur dyes). The liquid phase typically includes the cellulase solution used to treat the pretreated textile material, glucose, and, if present, optional soluble dyes, such as reactive black dyes.

[0131] After the step of treating the pretreated textile material with cellulase, the resulting mixture is treated to separate the liquid phase from the solid phase (block 7 in FIG. 1). At the end of the separation step, a liquid mixture containing glucose is obtained (block 9 in FIG. 1). This liquid mixture contains the cellulase enzyme added in the previous step. In an embodiment, the cellulase enzyme is recovered and, if necessary, can be reused up to ten times in the treatment of the solid phase obtained after the separation step (not shown in FIG. 1). In an embodiment, the cellulase enzyme is recovered and can be reused in the treatment of one or more additional pretreated waste textile materials (not shown in FIG. 1). The cellulase enzyme can be recovered, for example, by dialysis. Advantageously, at the end of the enzyme treatment, the enzyme is not removed from the mixture. For example, materials such as non-cellulosic fibers (e.g. polyester and / or elastane fibers) and insoluble dyes (indigo dyes and sulfur dyes, if present) can be recovered from the solid phase (block 8 in FIG. 1). The polyester fibres or other synthetic fibres thus recovered can be recycled as starting material for making filaments and fibres for recycled yarns and fabrics (block 8a).

[0132] The resulting liquid mixture containing glucose and enzymes is then used for the preparation of a microbial culture for the production of biocellulose (i.e. bacterial cellulose) (block 12 in FIG. 1). For this purpose, the mixture is heat treated to inactivate the enzymes present therein. Preferably, the mixture containing glucose is sterilized, for example by heating at 121° C., for example in a reactor suitable for the production of microbial cellulose. If necessary, additives can also be added to the mixture containing glucose to sterilize it (block 10 in FIG. 1). If necessary, the concentration of glucose in the mixture can be adjusted.

[0133] Next, the microbial cellulose-producing bacteria are added as a starter culture to the liquid mixture containing glucose (block 11 in FIG. 1). The decomposed enzymes are no longer active and instead provide a source of nitrogen and carbon as nutrients for the microorganisms, for example in the form of amino acids or parts of amino acids. If necessary, the amino acid concentration in the mixture can be adjusted. For example, the amino acid concentration in the mixture can be adjusted by adding peptone to the mixture.

[0134] The culture containing the microbial cellulose-producing bacteria thus obtained is then cultivated to grow the microbial cellulose (block 13 in FIG. 1). At the end of the cultivation, the microbial cellulose is obtained, usually as a layer of microbial cellulose.

[0135] The microbial cellulose, e.g., the microbial cellulose layer, is collected from the one or more vessels, washed, and optionally dried (block 14 of FIG. 1). Washing can be performed using an aqueous solution containing a bleaching agent. The washed microbial cellulose is then optionally dried. In an embodiment, the microbial cellulose can be partially dried, preferably after washing. For example, partially drying the microbial cellulose results in microbial cellulose having a moisture content of 99% to 80% by weight, preferably 90% to 80% by weight, more preferably 85% by weight.

[0136] The microbial cellulose obtained in block 14 can be advantageously used as starting cellulose material in a process for preparing regenerated cellulose fibers. Suitable processes for the step of block 15 in Figure 1 are those used for viscose production. The regenerated cellulose fibers can then be used to produce yarns and fabrics in a complete circular cycle (block 15a).

[0137] The invention will now be further described with reference to the following non-limiting examples.

[0138] Example 1 - Production of bacterial cellulose starting from waste textile materials The process of the present invention has been carried out to produce bacterial cellulose from waste textile feedstock. waste textile materials Undyed blended waste fabric (fabric composition: 76% viscose, 23% polyester, 1% elastane) was used as the waste textile material. Pretreatment with aqueous solutions containing NaOH and urea To obtain an aqueous solution of NaOH and urea, 7 w / v% NaOH and 12 w / v% urea were dissolved in 40 L of distilled water and cooled to 0°C in an air-conditioned room. 2 kg of fabric was immersed in the cold aqueous solution of NaOH and urea and pretreated at 0°C for 5 hours. After 5 hours, the fabric was neutralized with tap water at 20°C until the pH was 7. Alternatively, the fabric can be neutralized with a weak acid (e.g. acetic acid) wash. The pretreated fabric was then dried at 120°C on a stenter machine. Treatment with cellulase enzymes The pretreated dough was shredded (approximately 1 cm x 1 cm), immersed in 40 L of citrate buffer (0.05 M, pH 5.0), and heated at 50°C in a bioreactor. 40 L of citrate buffer (0.05 M, pH 5.0) was prepared as follows: 420 g of citric acid monohydrate was weighed and dissolved in 35 L of distilled water. The mixture was stirred until the citric acid monohydrate was completely dissolved. The pH was adjusted to 5.0 with NaOH. Distilled water was added to a volume of 40 L. 114.28 mL of Novozyme Cellic® CTec3 HS cellulase (equivalent to 20 FPU enzyme per gram of cellulose) was added to the solution. After the enzyme was added to the solution, the solution was stirred at 100 rpm for 1 minute to ensure uniform dissolution of the enzyme. The dough was then incubated in the solution containing cellulase enzyme at 50°C for 24 hours without stirring. At the end of the process, a mixture is obtained that includes a solid phase (e.g., primarily non-cellulosic materials such as, but not limited to, polyester and elastane, partially degraded cellulosic materials such as partially degraded viscose) and a liquid phase that includes glucose. Separation of liquid phase from solid phase After cultivation, the mixture was filtered through a 0.3 mm sieve to separate the solid phase of the mixture from the liquid phase of the mixture. The filtered liquid phase was centrifuged at 9000 RPM for 30 minutes. After centrifugation, the supernatant was collected as a glucose-containing mixture (e.g., glucose-rich syrup). Preparation of microbial cultures If necessary, the mixture containing glucose can be concentrated, for example, with a rotary evaporator. For example, a 40 L mixture can be concentrated to a final volume of 10 L. The yield of the enzymatic reaction was measured using the mixture containing glucose without the concentration step. In this example, 38.8 g / L of glucose (measured in 40 L of the mixture containing glucose as above) was released from 2 kg of blended fabric containing 1.52 kg of viscose by DNS method. When the mixture is concentrated to a final volume of 10 L, the glucose concentration in the mixture increases to 155.2 g / L. In this example, the yield was 91.9% according to the NREL method, and was calculated as follows: Cellulose conversion rate (%) = ((glucose released by enzymatic hydrolysis (g / L) × reaction volume (L)) / (substrate weight (g) × cellulose content (%)) × 0.9 × 100% Cellulose conversion rate (%) = ((38.8 (g / L) x 40 (L)) / (2000 (g) x (76 / 100))) x 0.9 x 100% = 91.9% where 0.9 is a correction factor for water molecules added during the hydrolysis of cellulose. 40 L of the mixture containing glucose (38.8 g / L) was mixed with 37.6 L of distilled water to obtain a diluted mixture containing glucose with a glucose concentration of 20 g / L. 77.6 L of the diluted mixture containing glucose was autoclaved at 121° C. for 15 minutes. The resulting glucose-containing mixture is also known as "Waste Textile Glucose" (WTG) medium. The resulting glucose-containing mixture may have the following composition: 20.0 g / L glucose from the enzymatic conversion of cellulose in waste textile materials to glucose; Peptone derived from degraded cellulase enzymes 2.85mL / L; 10.5g / L citric acid from citrate buffer; Water derived from the mixture obtained after the step of treating with cellulase enzyme. Preparation of starter cultures of bacterial cellulose-producing bacteria Starter bacterial cultures were produced as follows: 8 L of Hestrin-Schramm (HS) medium was prepared by mixing the following components and autoclaving: Glucose 160g, Soybeans, peptone derived from enzyme digest 40g, Yeast extract 40g, Disodium hydrogen phosphate dihydrate 27.2 g, Citric acid monohydrate 12g, 8L water, Gluconacetobacter hanseii ATCC 53582 was inoculated into 0.8 L of autoclaved HS medium and cultured at 28°C for 2 days. 0.8 L of freshly prepared bacterial culture was mixed with 7.2 L of autoclaved HS medium, then incubated in a shaking incubator at 150 rpm for 2 days. 8 L of freshly prepared starter bacterial culture was obtained and ready for use. Mixture of glucose-containing mixture (WTG medium) and starter bacterial culture 77.6 L of dilution mixture (i.e., waste textile glucose medium) containing glucose (20 g glucose / L) was aseptically mixed with 8 L of freshly prepared starter bacterial culture. 4 L of the resulting fresh bacterial mixture was then distributed into 21 plastic containers (730 mm wide x 460 mm long x 193 mm high) and capped. Cultivation of bacterial cultures The covered plastic container was incubated in an air-conditioned room at 28°C for 14 days to obtain bacterial cellulose. Washing and drying of bacterial cellulose On average, 17±0.35 kg of wet dirty bacterial cellulose layer can be recovered from 85.6 L of bacterial culture. These bacterial cellulose layers were removed from the vessel and collected in the reactor. The bacterial cellulose layers were then washed with 100 L of hot water (80°C) containing 1% bleach for 3 h under stirring at 100 rpm. Here, the bleach contained 5 w / v% sodium hypochlorite (i.e., 100 L of hot water containing 0.05 w / v% sodium hypochlorite was used). Afterwards, 100 L of contaminated water was drained and another 100 L of clean hot water (80°C) was added and the solution was stirred at 100 rpm for 3 h. On average, 16±0.32 kg of wet clean bacterial cellulose layer can be obtained from 17±0.35 kg of wet dirty bacterial cellulose layer. These bacterial cellulose layers are dried at 28° C. for 12 hours to obtain dry bacterial cellulose. On average, 470±10 g of dry bacterial cellulose can be obtained from 16±0.32 kg of wet clean bacterial cellulose.

[0139] Example 2 - Exemplary room temperature chemical pretreatment and enzyme treatment of undyed blended waste fabric Undyed blended waste fabric (fabric composition: 76% viscose, 23% polyester, 1% elastane) was used as the waste textile material. 7 w / v % NaOH and 12 w / v % urea were dissolved in 1 L of distilled water. 50 g of fabric was pretreated for 2 h at room temperature (20–25 °C) by immersing in an aqueous solution of NaOH and urea (1 L). After 2 h, the fabric was neutralized to pH 7 with tap water at 20 °C. Alternatively, the fabric can be neutralized by washing with a weak acid (e.g., acetic acid). The pretreated fabric was then dried in an oven at 80 °C. The pretreated fabric was chopped (e.g., 1 cm x 1 cm), immersed in 1 L of citrate buffer (0.05 M, pH 5.0) and heated at 50°C in a bioreactor. 2.85 mL of Novozyme Cellic® CTec3 HS cellulase (equivalent to 20 FPU enzyme per gram of cellulose) was added to the solution. The enzyme was then added to the solution and the solution was stirred at 100 rpm for 1 min to dissolve the enzyme uniformly. The fabric was incubated in the solution containing cellulase enzyme at 50°C for 24 hours without stirring. At the end of the treatment, a mixture is obtained that contains a solid phase (mainly non-cellulosic materials such as polyester and elastane, and partially degraded cellulosic materials, e.g. partially degraded viscose) and a liquid phase containing glucose. After cultivation, the mixture was filtered through a 0.3 mm sieve to separate the solid phase of the mixture from the liquid phase of the mixture. The filtered liquid phase was centrifuged at 9000 RPM for 30 minutes. After centrifugation, the supernatant was collected as a glucose-containing mixture (e.g., glucose-rich syrup). The yield of the enzymatic reaction was measured. According to the DNS method, 36.2 g / L of glucose was released from 50 g of blended fabric containing 38 g of viscose. According to the NREL method, the yield was 85.7%, calculated as follows: Cellulose conversion rate (%) = ((36.2 (g / L) x 1 (L)) / (50 (g) x (76 / 100))) x 0.9 x 100% = 85.7% where 0.9 is a correction factor for water molecules added during the hydrolysis of cellulose. The mixture containing glucose (36.2 g / L) can be mixed with distilled water to obtain a diluted mixture containing glucose at a glucose concentration of 20 g / L, ie, waste textile glucose (WTG) medium.

[0140] Example 3 - Exemplary chemical pretreatment and enzyme treatment of undyed 100% cotton waste fabric Undyed waste fabric (fabric composition: 100% cotton) was used as the waste textile material. 7 w / v% NaOH and 12 w / v% urea were dissolved in 1 L of distilled water and cooled to 0°C in a refrigerator to obtain an aqueous solution of NaOH and urea. 50 g of fabric was immersed in the aqueous solution of NaOH and urea (1 L) and pretreated at 0°C for 5 h. After 5 h, the fabric was neutralized with tap water at 20°C to a pH of 7. Alternatively, the fabric can be neutralized by washing with a weak acid (e.g., acetic acid). The pretreated fabric was then dried in an oven at 80°C. The pretreated fabric was chopped (e.g., 1 cm x 1 cm), immersed in 1 L of citrate buffer (0.05 M, pH 5.0), and heated at 50°C in a bioreactor. 3.76 mL of Novozyme Cellic® CTec3 HS cellulase (equivalent to 20 FPU enzyme per gram of cellulose) was added to the solution. The enzyme was then added to the solution and the solution was stirred at 100 rpm for 1 minute to dissolve the enzyme uniformly. The fabric was incubated in the solution containing cellulase enzyme at 50°C for 96 hours without stirring. At the end of the treatment, a mixture is obtained that contains a solid phase (mainly partially degraded cellulosic material, e.g., partially degraded cotton) and a liquid phase containing glucose. The mixture containing the solid and liquid phases was centrifuged at 9000 RPM for 30 minutes. After centrifugation, the supernatant was collected as a glucose-containing mixture (e.g., glucose-rich syrup). The yield of the enzymatic reaction was measured. According to the DNS method, 50g of 100% cotton fabric releases 51.3gr / L of glucose. According to the NREL method, the yield was 92.34%, calculated as follows: Cellulose conversion rate (%) = ((51.3 (g / L) x 1 (L)) / (50 (g) x (100 / 100))) x 0.9 x 100% = 92.3% where 0.9 is a correction factor for water molecules added during the hydrolysis of cellulose. The mixture containing glucose (51.3 g / L) can be mixed with distilled water to obtain a diluted mixture containing glucose at a glucose concentration of 20 g / L, ie, waste textile glucose (WTG) medium.

[0141] Example 4 - Exemplary chemical pretreatment and enzyme treatment of undyed blended waste fabric

[0142] Undyed blended waste fabric (fabric composition: 76% viscose, 23% polyester, 1% elastane) was used as the waste textile material. 7 w / v% NaOH and 12 w / v% urea were dissolved in 1 L of distilled water and cooled to 0°C in a refrigerator to obtain an aqueous solution of NaOH and urea. 50 g of fabric was immersed in the cold aqueous solution of NaOH and urea (1 L) and pretreated at 0°C for 5 h. After 5 h, the fabric was neutralized with tap water at 20°C to a pH of 7. Alternatively, the fabric can be neutralized by washing with a weak acid (e.g., acetic acid). The pretreated fabric was then dried in an oven at 80°C. The pretreated fabric was chopped (e.g., 1 cm x 1 cm), immersed in 1 L of citrate buffer (0.05 M, pH 5.0), and heated at 50°C in a bioreactor. 2.85 mL of Novozyme Cellic® CTec3 HS cellulase (equivalent to 20 FPU enzyme per gram of cellulose) was added to the solution. The enzyme was then added to the solution and the solution was stirred at 100 rpm for 1 minute to dissolve the enzyme uniformly. The fabric was then incubated in the solution containing the cellulase enzyme at 50°C for 24 hours without stirring. At the end of the treatment, a mixture is obtained that contains a solid phase (mainly non-cellulosic materials such as polyester and elastane, and partially degraded cellulosic materials, e.g. partially degraded viscose) and a liquid phase containing glucose. After cultivation, the mixture was filtered through a 0.3 mm sieve to separate the solid phase of the mixture from the liquid phase of the mixture. The filtered liquid phase was centrifuged at 9000 RPM for 30 minutes. After centrifugation, the supernatant was collected as a glucose-containing mixture (e.g., glucose-rich syrup). The yield of the enzymatic reaction was measured. According to the DNS method, 38.4 g / L of glucose was released from 50 g of blended fabric containing 38 g of viscose. According to the NREL method, the yield was 90.9%, calculated as follows: Cellulose conversion rate (%) = ((38.4 (g / L) x 1 (L)) / (50 (g) x (76 / 100))) x 0.9 x 100% = 90.9% where 0.9 is a correction factor for water molecules added during the hydrolysis of cellulose. The mixture containing glucose (38.4 g / L) can be mixed with distilled water to obtain a diluted mixture containing glucose at a glucose concentration of 20 g / L, ie, waste textile glucose (WTG) medium.

[0143] Example 5 - Exemplary chemical pretreatment and enzyme treatment of indigo dyed blended waste fabric Indigo-dyed blended waste fabric (fabric composition: 99% cotton, 1% elastane, indigo dyed) was used as the waste textile material. 7 w / v % NaOH and 12 w / v % urea were dissolved in 1 L of distilled water and cooled to 0° C. in a refrigerator to obtain an aqueous solution of NaOH and urea. 60 g of fabric was pretreated for 5 h at 0 °C by soaking in a cold aqueous solution of NaOH and urea (1 L). After 5 h, the fabric was neutralized with tap water at 20 °C to a pH of 7. Alternatively, the fabric can be neutralized by washing with a weak acid (e.g., acetic acid). The pretreated fabric was then dried in an oven at 80 °C. The pretreated fabric was shredded (e.g., 1 cm x 1 cm), immersed in 1.2 L of citrate buffer (0.05 M, pH 5.0), and heated at 50°C in a bioreactor. 4.47 mL of Novozyme Cellic® CTec3 HS cellulase (equivalent to 20 FPU enzyme per gram of cellulose) was added to the solution. The enzyme was then added to the solution, and the solution was stirred at 100 rpm for 1 minute to dissolve the enzyme uniformly. The fabric was then incubated in the solution containing cellulase enzyme at 50°C for 24 hours without stirring. At the end of the treatment, a mixture is obtained that contains a solid phase (mainly partially degraded cellulosic materials such as cotton and non-cellulosic elastane) and a liquid phase containing glucose. After incubation, the mixture was filtered through a 0.3 mm sieve to separate the solid phase of the mixture from the liquid phase of the mixture. The filtered liquid phase was centrifuged at 9000 RPM for 30 minutes. After centrifugation, the supernatant was collected as a mixture containing glucose (e.g., glucose-rich syrup), and the precipitate containing indigo dye was collected. The glucose-containing mixture (i.e., waste textile glucose solution, i.e., glucose-rich syrup) can be mixed with distilled water to obtain a diluted glucose-containing mixture, i.e., waste textile glucose (WTG) medium, with a glucose concentration of 20 g / L.

[0144] Example 6 - Exemplary chemical pretreatment and enzyme treatment of blended waste fabric dyed with sulfur dyes A blended waste fabric dyed with sulfur dyes (fabric composition: 92.5% cotton, 5% polyester, 2.5% elastane, sulfur dyes) was used as the waste textile material. 7 w / v% NaOH and 10.5 w / v% urea were dissolved in 2 L of distilled water and cooled to 0°C in a refrigerator to obtain an aqueous solution of NaOH and urea. 100 g of fabric was immersed in the cold aqueous solution of NaOH and urea (2 L) and pretreated at 0°C for 5 h. After 5 h, the fabric was neutralized with tap water at 20°C to a pH of 7. Alternatively, the fabric can be neutralized by washing with a weak acid (e.g., acetic acid). The pretreated fabric was then dried in an oven at 80°C. The pretreated fabric was shredded (e.g., 1 cm x 1 cm), immersed in 2 L of citrate buffer (0.05 M, pH 5.0), and heated at 50°C in a bioreactor. 6.95 mL of Novozyme Cellic® CTec3 HS cellulase (equivalent to 20 FPU enzyme per gram of cellulose) was added to the solution. The enzyme was then added to the solution, and the solution was stirred at 100 rpm for 1 minute to dissolve the enzyme uniformly. The fabric was then incubated in the solution containing cellulase enzyme at 50°C for 24 hours without stirring. At the end of the treatment, a mixture is obtained that contains a solid phase (mainly non-cellulosic materials, including but not limited to polyester and elastane, and partially degraded cellulosic materials such as cotton) and a liquid phase containing glucose. After incubation, the mixture was filtered through a 0.3 mm sieve to separate the solid phase of the mixture from the liquid phase of the mixture. The filtered liquid phase was centrifuged at 9000 RPM for 30 minutes. After centrifugation, the supernatant was collected as a mixture containing glucose (e.g., glucose-rich syrup), and the precipitate containing the sulfur dye was collected. The glucose-containing mixture can be mixed with distilled water to obtain a diluted glucose-containing mixture with a glucose concentration of 20 g / L, ie, waste textile glucose (WTG) medium.

[0145] Example 7 - Exemplary chemical pretreatment and enzyme treatment of blended waste fabric dyed with black reactive dye The waste textile material used was a blended waste fabric dyed with a black reactive dye (fabric composition: 90% cotton, 6% polyester, 4% elastane, black reactive dye). 7 w / v% NaOH and 14.0 w / v% urea were dissolved in 2 L of distilled water and cooled to 0°C in a refrigerator to obtain an aqueous solution of NaOH and urea. 100 g of fabric was immersed in the cold aqueous solution of NaOH and urea (2 L) and pretreated at 0°C for 5 h. After 5 h, the fabric was neutralized with tap water at 20°C to a pH of 7. Alternatively, the fabric can be neutralized by washing with a weak acid (e.g., acetic acid). The pretreated fabric was then dried in an oven at 80°C. The pretreated fabric was shredded (e.g., 1 cm x 1 cm), immersed in 2 L of citrate buffer (0.05 M, pH 5.0), and heated at 50°C in a bioreactor. 6.77 mL of Novozyme Cellic® CTec3 HS cellulase (equivalent to 20 FPU enzyme per gram of cellulose) was added to the solution. The enzyme was then added to the solution, and the solution was stirred at 100 rpm for 1 minute to dissolve the enzyme uniformly. The fabric was then incubated in the solution containing cellulase enzyme at 50°C for 24 hours without stirring. At the end of the treatment, a mixture is obtained that contains a solid phase (mainly non-cellulosic materials, including but not limited to polyester and elastane, and partially degraded cellulosic materials such as cotton) and a liquid phase containing glucose. After incubation, the mixture was filtered through a 0.3 mm sieve to separate the solid phase of the mixture from the liquid phase of the mixture. The filtered liquid phase was centrifuged at 9000 RPM for 30 minutes. After centrifugation, the supernatant was collected as a mixture containing glucose (e.g., glucose-rich syrup) and further containing a black reactive dye. The dyes were removed from the liquid mixture by activated charcoal column chromatography. Specifically, to remove the dyes, the glucose-rich syrup was poured into the activated charcoal column at a flow rate of 2 mL / min. The 5 cm x 50 cm column contained 1 kg of activated charcoal beads with a diameter of 2.88 mm ± 0.26 mm. The mixture obtained after removal of the dye can be mixed with distilled water to obtain a dilute mixture containing glucose at a glucose concentration of 20 g / L, ie, waste textile glucose (WTG) medium.

[0146] Example 8 - Comparison of Hestrin-Schramm (HS) and Waste Textile Glucose (WTG) media The bacterial strain Gluconacetobacter hansenii ATCC 53582 was cultured in 500 mL of waste textile glucose (WTG) medium or Hestrin-Schramm (HS) medium in a sealed plastic box with a lid at an incubation temperature of 28°C–30°C for 14 days. After the cultivation was completed, the obtained wet bacterial cellulose was squeezed or compressed by a mechanical device to remove excess culture medium.The amount of the obtained wet bacterial cellulose was then measured. TIFF2024153571000002.tif35151 An approximately 20% increase in wet bacterial cellulose yield was observed using waste textile glucose medium compared to HS medium.

[0147] Example 9 - Comparison of additives (TiBALDH, glycerol, ascorbic acid) The bacterial strain Gluconacetobacter hansenii ATCC 53582 was cultivated in 500 mL of waste fiber glucose medium in a plastic box with a sealed lid at an incubation temperature of 28°C–30°C for 14 days. Various experiments were performed to test the effect of the addition of different additives (TiBALDH, glycerol, ascorbic acid) at different concentrations on the production of bacterial cellulose. The amount of wet bacterial cellulose obtained at the end of the culture was measured. Comparisons of the changes (%) in the amount of wet bacterial cellulose in Tables 2, 3, 4, and 5 are based on the data in Table 1. TiBALDH The first additive tested was titanium(IV) bis(ammonium lactato) dihydroxide solution (TiBALDH), CAS number 65104-06-5. TIFF2024153571000003.tif51153 The results showed that the addition of 0.25% TiBALDH to the waste textile glucose medium resulted in the greatest increase in the amount of wet bacterial cellulose obtained (+55.30%). Glycerol The second additive tested was glycerol, CAS number 56-81-5. TIFF2024153571000004.tif34150 The results showed that the addition of 1% glycerol to the waste textile glucose medium resulted in the greatest increase in the amount of wet bacterial cellulose (+19.74%). Ascorbic Acid (Vitamin C) The third additive tested was ascorbic acid (vitamin C), CAS number 50-81-7. TIFF2024153571000005.tif51150 The results showed that the addition of 0.5% ascorbic acid to the waste textile glucose medium resulted in the greatest increase in the amount of wet bacterial cellulose (+9.25%). Additive combinations Various combinations of three additives, TiBALDH, glycerol, and ascorbic acid, were tested. TIFF2024153571000006.tif62151 According to the results obtained, the highest wet bacterial cellulose amount was achieved (58.04%) with the addition of 1% glycerol and 0.25% TiBALDH.

[0148] Example 10 - Comparison of waste textile materials before and after pretreatment with aqueous solutions containing NaOH and urea A blended waste fabric (fabric composition: 76% viscose, 23% polyester, 1% elastane) was treated in a solution of 7 w / v% NaOH and 12 w / v% urea at 0°C for 5 hours. Images of the fabric before and after treatment were taken and analyzed using a scanning electron microscope (SEM). As can be seen from Figure 2, the fabric after treatment is swollen, i.e., the fibers of the fabric after treatment are separated compared to the fibers of the fabric before treatment.

[0149] Example 11 - Effect of pretreatment with aqueous solutions containing NaOH and urea at room temperature and 50°C on polyester Two samples of 100% polyester fabric were treated with a solution of 7 w / v% NaOH and 12 w / v% urea at room temperature and 50 °C for 5 h, respectively. After treatment, images of the samples were taken and analyzed using a scanning electron microscope (SEM). As can be seen in Figure 4A, the pretreatment performed at room temperature did not damage the polyester fibers. Conversely, the pretreatment performed at 50 °C did damage the polyester fibers (Figure 4B).

[0150] Example 12 - Comparison of waste textile materials before and after pretreatment with aqueous solutions containing NaOH and urea (at 0°C and room temperature) and enzyme treatment A blended waste fabric sample (fabric composition: 76% viscose, 23% polyester, 1% elastane) was pretreated in a solution of 7 w / v% NaOH and 12 w / v% urea at 0° C. or room temperature for 5 hours and then treated with cellulase enzyme. Images of the samples were taken before and after treatment and analyzed using a scanning electron microscope (SEM). FIG. 5A shows an SEM image of the sample before pretreatment and enzyme treatment. FIG. 5B shows the sample material after pretreatment at 0° C. and treatment with cellulase. FIG. 5C shows the sample material after pretreatment at room temperature and treatment with cellulase. It can be seen that the process of the present invention does not damage the polyester fibers.

[0151] Example 13 - Characteristics of glucose obtained after cellulase treatment Blended waste fabric (fabric composition: 76% viscose, 23% polyester, 1% elastane) and 100% cotton waste fabric were pretreated with a solution of NaOH and urea and then treated with cellulase enzyme according to the process of the present invention. The glucose obtained after the cellulase enzyme treatment step was analyzed by Nuclear Magnetic Resonance (NMR) and the following results were obtained: Blended fabric: D 2 Glucose in O 1 H-NMR. α-glucose 40.7%, β-glucose 59.3%, 5.21 ppm (bs, H 1-α ), 4.63 ppm (d, J = 7.6 Hz, H 1-β ), 3.87 ppm (d, J = 12.0 Hz, H 6-β ), 3.81 ppm (d, J = 10.9 Hz, H 5-α and H 6-α ), 3.77-3.64 ppm (m, H 6-α and H 3-α and H 6-β ), 3.52 ppm (d, J = 8.0 Hz, H 2-α ), 3.46ppm(dd, J=18.2, 9.1Hz, H 3-β and H 5-β ), 3.38ppm(dd, J=15.3, 8.6Hz, H 4-α and H 4-β), 3.23 ppm (t, J = 8.1 Hz, H 2-β ) 100% cotton fabric: D 2 Glucose in O 1 H-NMR. α-glucose 43.3%, β-glucose 56.7% 5.23 ppm (d, J = 3.7 Hz, H 1-α ), 4.65 ppm (d, J = 7.9 Hz, H 1-β ), 3.90ppm(dd, J=12.3, 1.9Hz, H 6-β ), 3.87-3.81 ppm (m, H 5-α or H 6-α ), 3.76ppm(dd, J=12.5, 5.5Hz, H 6-α ), 3.75-3.69 ppm (m, H 3-α and H 6-β ), 3.53ppm (dd, J=9.8, 3.7Hz, H 2-α ), 3.50-3.45ppm(m,H 3-β and H 5-β ), 3.41ppm(dt, J=9.4, 6.1Hz, H 4-α and H 4-β ), 3.24ppm(dd, J=9.1, 8.1Hz, H 2-β )

[0152] Example 14 - Exemplary bacterial cellulose structures obtained by the process of the present invention Exemplary bacterial cellulose samples obtained by the process of the present invention were analyzed and characterized. The following results were obtained: Viscosity: 980ml / g (measured according to ISO 5351:2010) Molecular weight distribution: Mn=88047g / mol, Mw=510577g / mol, DI=5.8 (SEC analysis with 0.5w / v% LiCl / DMAc mobile phase) Cellulose content in bacterial cellulose >99% Hemicellulose content in bacterial cellulose <1%; arabinose 0.08 g / kg, galactose 0.03 g / kg, xylose 0.05 g / kg, mannose 0.4 g / kg, glucose 882 g / kg (SCAN-CM71:09) Ash content <0.5% (according to ISO 1762:2019) 3A and 3B show the structure of bacterial cellulose as observed by light microscopy at two magnifications: 150x in FIG. 3A and 75x in FIG. 3B. As can be seen in Figures 3A and 3B, the structure of bacterial cellulose is striped with a network of both thin and thick fibers.

[0153] Example 15 - Washing of bacterial cellulose Once the bacterial cellulose (BC) fermentation is finished, the BC layer is removed from the fermentation vessel and placed in a laundry bag closed with a resealable Velcro® fastener. The laundry bag is made of fabric with a mesh size of 50 micrometers to 100 micrometers, preferably 75 micrometers. The laundry bag is squeezed with a fabric wringer to remove excess bacterial solution. The laundry bag is then placed in a commercial washing machine to inactivate and remove the bacteria and whiten the BC layer. The washing protocol is as follows: Bacterial cellulose layer / water weight ratio: 1 / 10, preferably 1 / 4; Whitening agent: 1% bleach Temperature: 30℃ Time required: 30 minutes

[0154] Example 16 - Exemplary room temperature chemical pretreatment and enzyme treatment of undyed 100% cotton waste fabric Undyed waste fabric (fabric composition: 100% cotton) was used as the waste textile material. 7 w / v % NaOH and 12 w / v % urea were dissolved in 1 L of distilled water. 50 g of fabric was pretreated for 2 h at room temperature (20–25 °C) by immersing in an aqueous solution of NaOH and urea (1 L). After 2 h, the fabric was neutralized with tap water at 20 °C until the pH was 7. Alternatively, the fabric can be neutralized by washing with a weak acid (e.g., acetic acid). The pretreated fabric was then dried in an oven at 80 °C. The pretreated fabric was shredded (e.g., 1 cm x 1 cm), immersed in 1 L of citrate buffer (0.05 M, pH 5.0), and heated at 50°C in a bioreactor. 3.76 mL of Novozyme Cellic® CTec3 HS cellulase (equivalent to 20 FPU enzyme per gram of cellulose) was added to the solution. The enzyme was then added to the solution, and the solution was stirred at 100 rpm for 1 minute to dissolve the enzyme uniformly. The fabric was then incubated in the solution containing cellulase enzyme at 50°C for 24 hours without stirring. At the end of the treatment, a mixture is obtained that contains a solid phase (partially degraded cellulosic material, e.g., partially degraded cotton) and a liquid phase containing glucose. After incubation, the mixture was filtered through a 0.3 mm sieve to separate the solid phase of the mixture from the liquid phase of the mixture. The filtered liquid phase was centrifuged at 9000 RPM for 30 minutes. After centrifugation, the supernatant was collected as a mixture containing glucose (e.g., glucose-rich syrup). The yield of the enzyme reaction was measured. According to the DNS method, 45.62 g / L of glucose was released from 50 g of 100% cotton fabric. According to the NREL method, the yield was 82.12%, calculated as follows: Cellulose conversion rate (%) = ((45.62 (g / L) x 1 (L)) / (50 (g) x (100 / 100))) x 0.9 x 100% = 82.12% where 0.9 is a correction factor for water molecules added during the hydrolysis of cellulose. The mixture containing glucose (45.62 g / L) can be mixed with distilled water to obtain a diluted mixture containing glucose at a glucose concentration of 20 g / L, ie, waste textile glucose (WTG) medium.

[0155] Example 17 - Comparison of enzyme activity at different chemical pretreatment temperatures: -20°C, 0°C and room temperature An undyed waste textile fabric (fabric composition: 76% viscose, 23% polyester, 1% elastane) was used (similar to Examples 1 and 2). Pretreatment with NaOH and urea was carried out for 24 hours at -20°C. Then, the same process as in Example 1 was carried out. The cellulose conversion yield obtained from the enzyme treatment was 89.6%. According to Example 1, pretreatment with NaOH and urea was carried out for 5 hours at 0° C. The cellulose conversion yield obtained from the enzyme treatment was 91.9% (see also Example 1). According to Example 2, pretreatment with NaOH and urea was carried out for 2 hours at room temperature (20-25° C.). The cellulose conversion yield obtained from the enzymatic treatment was 87.5% (see also Example 2). Results: By performing the pretreatment steps with NaOH and urea at room temperature, a high conversion rate of cellulose to glucose can be obtained while significantly shortening the pretreatment time.

[0156] Example 18 - Exemplary chemical pretreatment and enzyme treatment of undyed 100% cotton waste fabric Undyed waste textile fabric (fabric composition: 100% cotton) was used as the waste textile material. The same process as in Example 3 was carried out using the enzyme AB Enzyme-Flashzyme Plus 200 instead of Novozymes Cellic® CTec3 HS. TIFF2024153571000007.tif45151 The cellulose conversion yield obtained from the enzyme treatment was 93.51% after 144 h.

[0157] Example 19 - Recycling of cellulase enzymes Undyed waste textile fabric (fabric composition: 100% cotton) was used as the waste textile material. 7 w / v% NaOH and 12 w / v% urea were dissolved in 1 L of distilled water and cooled to 0°C in a refrigerator to obtain an aqueous solution of NaOH and urea. 50 g of fabric was immersed in the aqueous solution of NaOH and urea (1 L) and pretreated at 0°C for 5 h. After 5 h, the fabric was neutralized with tap water at 20°C to a pH of 7. Alternatively, the fabric can be neutralized by washing with a weak acid (e.g., acetic acid). The pretreated fabric was then dried in an oven at 80°C. The pretreated fabric was shredded (e.g., 1 cm x 1 cm), immersed in 1 L of citrate buffer (0.05 M, pH 5.0), and heated at 50°C in a bioreactor. 3.76 mL of Novozyme Cellic® CTec3 HS cellulase (equivalent to 20 FPU enzyme per gram of cellulose) was added to the solution. The enzyme was then added to the solution and the solution was stirred at 100 rpm for 1 minute to dissolve the enzyme uniformly. The fabric was then incubated in the solution containing cellulase enzyme at 50°C for 24 hours without stirring. At the end of the treatment, a mixture is obtained that contains a solid phase (mainly partially degraded cellulosic material, e.g., partially degraded cotton) and a liquid phase containing glucose. The mixture containing the solid and liquid phases was centrifuged at 9000 RPM for 30 minutes. After centrifugation, the supernatant was collected as a glucose-containing mixture (e.g., glucose-rich syrup). After centrifugation, the enzyme was removed from the supernatant (i.e., the mixture containing glucose) by dialysis (Dialysis cassette: Thermo Scientific - Slide-A-Lyzer cassette (10 K MWCO)) as follows. 1 L of 0.05 M citric acid (pH 5) buffer was prepared and placed on ice. The dialysis cassette was placed in the buffer solution and stirred with a magnetic stirrer for 3 hours, and glucose produced by cellulose decomposition was removed from the mixture in the dialysis cassette by enzyme recycling. To prevent the enzyme from decomposing, dialysis was performed under low temperature conditions. To prevent the enzyme from passing through the dialysis cassette, a 10 kDa dialysis cassette was selected based on the approximate molecular weight of cellulase. After 3 hours, the solution from the dialysis cassette was used to contact the solid phase (mainly partially degraded cellulosic material, e.g., partially degraded cotton) obtained as described above for the continuous enzymatic degradation. After 24 h of incubation at 50°C without stirring (total time of enzymatic treatment: 48 h), the resulting mixture containing the solid phase and the liquid phase containing glucose was centrifuged. After centrifugation, the enzyme was removed from the supernatant and reused in contact with the solid phase obtained after centrifugation. The same process of enzyme treatment, separation of the liquid phase from the solid phase, recovery of the enzyme by dialysis, and reuse of the enzyme were carried out two more times (enzyme treatment for 72 and 96 hours). The cellulose to glucose conversion (yield %) after the second application of the enzyme solution (i.e., after a total of 48 hours of enzyme treatment) was 79.77%. After the fourth application of the enzyme solution (ie, after a total of 96 hours of enzyme treatment), the conversion rate (yield %) of cellulose to glucose was 99.18%.

[0158] Example 20 - Effect of chopping on the amount of dissolved cellulose Undyed waste textile fabric (fabric composition: 76% viscose, 23% polyester, 1% elastane) was used as the waste textile material. A 2 g sample of fabric was pretreated by soaking it in an aqueous solution of NaOH and urea. After pretreatment, the fabric was neutralized with tap water at 20°C until the pH was 7. The pretreated fabric was then dried in an oven at 80°C. The weight of the resulting pretreated fabric was 1.86 g. 2 g of fabric was shredded. The shredded fabric was pretreated by soaking in an aqueous solution of NaOH and urea. After pretreatment, the fabric was neutralized to pH 7 with tap water at 20°C. The pretreated fabric was then dried in an oven at 80°C. The weight of the resulting pretreated shredded fabric was 1.48 g. As can be seen, when the fabric was not shredded before treatment, 0.14 g of cotton was lost during pretreatment, which corresponds to a cellulose loss of 7%. Conversely, when the fabric was shredded before treatment, 0.52 g of cotton was lost during pretreatment, which corresponds to a cellulose loss of 26%. Shredding the waste textile material after pretreatment provides more cellulose to the cellulase enzymes, resulting in more glucose at the end of the enzymatic conversion of cellulose to glucose.

[0159] Example 21 - Illustrative comparison of chemically pretreated and non-pretreated undyed blended waste fabric Undyed blended waste fabric (fabric composition: 76% viscose, 23% polyester, 1% elastane) was used as the waste textile material. Chemical pretreatment 7 w / v% NaOH and 12 w / v% urea were dissolved in 100 mL of distilled water and cooled to 0°C in a refrigerator to obtain an aqueous solution of NaOH and urea. 5 g of fabric was immersed in the cold aqueous solution of NaOH and urea and pretreated at 0°C for 5 hours. After 5 hours, the fabric was neutralized to pH 7 with tap water at 20°C. Alternatively, the fabric can be neutralized with a weak acid (e.g., acetic acid) wash. The pretreated fabric was then dried in an oven at 80°C. The pretreated fabric was shredded (e.g., 1 cm x 1 cm). Non-pretreated 5g of fabric was cut into shreds (e.g. 1cm x 1cm). Treatment with cellulase enzymes The pretreated and non-pretreated fabrics were immersed in 100 mL of citrate buffer (0.05 M, pH 5.0) and heated to 50° C. on an orbital shaker. 0.28 mL of Novozyme Cellic® CTec3 HS cellulase (equivalent to 20 FPU enzyme per gram of cellulose) was added to the solution. After the enzyme was added to the solution, the solution was stirred at 100 rpm for 1 min to allow the enzyme to dissolve uniformly. The fabrics were then incubated in the solution containing cellulase enzymes for 24 h at 50° C. without stirring. At the end of the treatment, two mixtures are obtained: a solid phase (mainly non-cellulosic materials such as polyester, elastane, and partially degraded cellulosic materials, e.g. partially degraded viscose) and a liquid phase containing glucose. After cultivation, the mixture was filtered through a 0.3 mm sieve to separate the solid phase of the mixture from the liquid phase of the mixture. The filtered liquid phase was centrifuged at 9000 RPM for 30 minutes. After centrifugation, the supernatant was collected as a mixture containing glucose (e.g., glucose-rich syrup). Enzyme reaction yield - Chemical pretreatment According to the DNS method, 38.4 g / L of glucose was released from 5 g of blended fabric containing 3.8 g of viscose. According to the NREL method, the yield was 90.9%, calculated as follows: Cellulose conversion rate (%) = ((37.7 (g / L) x 0.1 (L)) / (5 (g) x (76 / 100))) x 0.9 x 100% = 89.3% where 0.9 is a correction factor for water molecules added during the hydrolysis of cellulose. Non-pretreated According to the DNS method, 12.7 g / L of glucose was released from 5 g of blended fabric containing 3.8 g of viscose. According to the NREL method, the yield was 90.9%, calculated as follows: Cellulose conversion rate (%) = ((12.7 (g / L) x 0.1 (L)) / (5 (g) x (76 / 100))) x 0.9 x 100% = 30.1% where 0.9 is a correction factor for water molecules added during the hydrolysis of cellulose. As can be seen, by pretreating waste textile materials according to the present invention, the cellulose to glucose conversion yield can be increased from 30.1% to 89.3%.

[0160] The above examples demonstrate that the process of the present invention provides a method for recycling cotton and cellulose fibers, as well as a method for recycling polyester or other synthetic fibers from waste textiles, i.e., fabrics. The cellulose fibers are converted into glucose, which is used to produce microbial cellulose, which is then dissolved and converted into viscose or similar cellulose fibers, completing a complete recycling cycle of the original cellulose fibers.

[0161] Also, the degradation of polyester fibers in the pretreatment step with the claimed solutions containing both NaOH and urea in the claimed temperature range, in particular at room temperature (20°C ± 5°C), is significantly reduced compared to prior art treatments, so that the polyester recovered after enzymatic conversion of cellulose fibers is suitable for recycling and re-spinning into recycled polyester filaments.

[0162] Moreover, this process provides that the enzymes used for the enzymatic conversion of cellulose can consist of cellulase enzymes, and has the advantage that the glucose and the enzymes present in the glucose-containing solution can be inactivated by heat, so that the glucose-containing solution can be used directly in the subsequent step of culturing the cellulose-producing microorganisms, where the inactivated enzymes serve as a nutrient source for said microorganisms.

[0163] This process is particularly advantageous for recycling blended yarns of synthetic and cellulose fibers where the cellulose fibers are difficult to recycle intact, for example by mechanical processes that maintain the fibers in fibrous form. As an example, this process is useful when the cellulose fibers are cotton fibers that come from already recycled fabrics and yarns and therefore have a short average length, resulting in a recycled fiber length that is too short for use as yarn.

Claims

1. A process for producing microbial cellulose from waste textile material, the waste textile material comprising cellulose fibers comprising cellulose, the process for producing microbial cellulose comprising: a) preparing said waste textile material; b) pretreating said waste textile material with an aqueous solution containing NaOH and urea at -25°C to +30°C to obtain a pretreated textile material; c) treating the pretreated textile material with cellulase to convert the cellulose to glucose to obtain a mixture comprising a solid phase and a liquid phase; d) separating the liquid phase from the solid phase to obtain a liquid mixture comprising glucose; e) preparing the microbial culture comprising a microbial cellulose producing microorganism using the liquid mixture comprising glucose; f) culturing said microbial culture to obtain microbial cellulose.

2. An enzymatic saccharification process for waste textile materials that are composed of cellulose-containing cellulose fibers, the enzymatic saccharification process comprising the steps of: a) providing said waste textile material; b) pretreating said waste textile material with an aqueous solution containing NaOH and urea at -25°C to +30°C to obtain a pretreated textile material; c) treating the pretreated textile material with cellulase to convert the cellulose to glucose to obtain a mixture comprising a solid phase and a liquid phase; A process for enzymatic saccharification, characterized in that the pretreated textile material obtained in step b) is chopped into a plurality of pieces having a size suitable for enzymatic saccharification prior to step c).

3. 3. The process according to claim 1 or 2, characterized in that the waste textile material comprises cellulosic and non-cellulosic fibres and is selected from yarns, fabrics and products comprising said fabrics.

4. 4. The process according to claim 3, characterized in that the cellulose fibers are selected from cotton fibers, hemp fibers, flax (linen) fibers, jute fibers, viscose fibers, lyocell fibers, modal fibers, acetate fibers, cupra fibers, and mixtures thereof, preferably the fibers are recycled fibers, and the non-cellulose fibers are selected from polyester fibers, polyamide fibers, elastane fibers, polypropylene (PP) fibers, acrylic fibers, and mixtures thereof, preferably the fibers are recycled fibers.

5. 3. The process according to claim 1 or 2, characterized in that the amount of NaOH in the aqueous solution containing NaOH and urea is 1 w / v% to 15 w / v% (percentage by volume) preferably 2 w / v% to 10 w / v%, more preferably 3 w / v% to 9 w / v% and the amount of urea in the aqueous solution is 1 w / v% to 25 w / v%, preferably 3 w / v% to 20 w / v%, more preferably 5 w / v% to 15 w / v%.

6. 3. The process according to claim 1 or 2, characterized in that the mass ratio of NaOH to urea (NaOH / urea) is from 1.0 / 1.0 to 1.0 / 2.0, preferably from 1.0 / 1.5 to 1.0 / 2.0, more preferably from 1.0 / 1.5 to 1.0 / 1.

8.

7. 3. The process according to claim 1 or 2, characterized in that in the step of pretreating the waste textile material with the aqueous solution containing NaOH and urea, the mass of the waste textile material relative to the volume of the aqueous solution containing NaOH and urea is 1 w / v% to 20 w / v%, preferably 2 w / v% to 15 w / v%, more preferably 2.5 w / v% to 10 w / v%, most preferably 5 w / v%.

8. 3. The process according to claim 1 or 2, characterized in that the step of pre-treating the waste textile material with the aqueous solution comprising NaOH and urea is carried out at a temperature between -25°C and +30°C, preferably between -15°C and +25°C, more preferably between 4°C and +25°C, most preferably between +15°C and +25°C.

9. 3. The process according to claim 1 or 2, characterized in that the pretreatment step is carried out for a period of from 0.5 h to 10 h, preferably from 1 h to 8 h, more preferably from 2 h to 7 h.

10. 3. The process according to claim 1 or 2, characterized in that the cellulase has an enzymatic activity of from 1 FPU to 50 FPU per gram cellulose, preferably from 10 FPU to 30 FPU per gram cellulose, more preferably from 15 FPU to 25 FPU per gram cellulose, and optionally the cellulase is in the form of a solution containing cellulase enzyme.

11. 3. The process according to claim 1 or 2, characterized in that the waste textile material comprises a dye and at least a part of the dye is removed from the waste textile material before step c), preferably before step b), or from the solid phase or the liquid phase of the mixture comprising a solid phase and a liquid phase after step d).

12. 4. The process of claim 3, wherein the non-cellulosic fibers are recovered from the solid phase of the mixture comprising a solid phase and a liquid phase.

13. 2. The process according to claim 1, characterized in that the mixture containing glucose obtained in step d) is subjected to a heat treatment to inactivate the cellulase enzymes before being used in step e), whereby the inactivated enzymes serve as a nutrient source for the microorganisms.

14. 2. The process according to claim 1, characterized in that the concentration of glucose in the liquid mixture containing glucose is between 10 g / L and 30 g / L, preferably between 15 g / L and 25 g / L, and the amount of the liquid mixture containing glucose is between 99% and 80% by weight, preferably between 95% and 85% by weight of the mass of the microbial culture.

15. 2. The process according to claim 1, characterized in that the liquid mixture containing glucose is mixed with a starter microbial culture containing microbial cellulose-producing microorganisms, the amount of the starter microbial culture containing microbial cellulose-producing microorganisms being between 1% and 20% by weight, preferably between 5% and 15% by weight, of the mass of the microbial culture.

16. 2. The process according to claim 1, characterized in that the step of preparing a microbial culture using the liquid mixture containing glucose comprises adding at least one additive to the liquid mixture containing glucose, the additive being preferably selected from titanium (IV) bis(ammonium lactate) dihydroxide (TiBALDH), glycerol, ascorbic acid, ethephon (2-chloroethyl phosphate) and mixtures thereof.

17. 2. The process according to claim 1, characterized in that the microbial cellulose is washed and optionally dried, the washing being carried out with an aqueous solution containing a bleaching agent, preferably sodium hypochlorite (NaOCl), at 0.01% to 10% w / v, preferably 0.1% to 0.05% w / v.

18. 2. The process of claim 1, wherein the microbial cellulose is used to produce cellulose fibers.

19. 1. A process for recycling polyester fibers or blended textile products containing polyester filaments and cellulosic fibers, the process comprising: g) providing a waste textile material; h) pre-treating the waste textile material with an aqueous solution containing NaOH and urea at -25°C to +30°C to obtain a pre-treated textile material; i) treating the pretreated textile material with cellulase to convert the cellulose to glucose to obtain a mixture comprising a liquid phase and a solid phase comprising polyester fibers or polyester filaments; j) separating the liquid phase from the solid phase to obtain the liquid mixture comprising glucose; k) recovering the polyester fibers or polyester filaments from the solid phase.

20. 20. The process of claim 19, wherein the waste textile material comprises cellulosic and non-cellulosic fibers and is selected from yarns, fabrics and products comprising the fabrics.

21. 20. The process according to claim 19, characterized in that the amount of NaOH in the aqueous solution containing NaOH and urea is between 1% and 15% w / v, preferably between 2% and 10% w / v, more preferably between 3% and 9% w / v, and the amount of urea in the aqueous solution is between 1% and 25% w / v, preferably between 3% and 20% w / v, more preferably between 5% and 15% w / v.

22. 20. The process according to claim 19, characterized in that the mass ratio of NaOH to urea (NaOH / urea) is from 1.0 / 1.0 to 1.0 / 2.0, preferably from 1.0 / 1.5 to 1.0 / 2.0, more preferably from 1.0 / 1.5 to 1.0 / 1.

8.

23. 20. The process according to claim 19, characterized in that in the step of pretreating the waste textile material with the aqueous solution containing NaOH and urea, the mass of the waste textile material relative to the volume of the aqueous solution containing NaOH and urea is 1 w / v% to 20 w / v%, preferably 2 w / v% to 15 w / v%, more preferably 2.5 w / v% to 10 w / v%, most preferably 5 w / v%.

24. 20. The process according to claim 19, characterized in that the step of pre-treating the waste textile material with the aqueous solution comprising NaOH and urea is carried out at a temperature between -25°C and +30°C, preferably between -15°C and +25°C, more preferably between 4°C and +25°C, most preferably between +15°C and +25°C.

25. 20. The process according to claim 19, characterized in that the pretreatment step is carried out for a period of from 0.5 h to 10 h, preferably from 1 h to 8 h, more preferably from 2 h to 7 h.

26. 20. The process according to claim 19, characterized in that the waste textile material comprises a dye and at least a part of the dye is removed from the waste textile material before step i), preferably before step h), or from the solid phase or the liquid phase of the mixture comprising solid and liquid phases after step j).

Citation Information

Patent Citations

  • Method for preparing bacterial cellulose (BC) by waste cotton fabrics

    CN102080114A

  • Method for preparing bacterial cellulose from waste polyester fabrics

    CN111269953A