Polymer, coating material and assembly product

A polymer with benzene ring derivatives and lactide monomers addresses the low decomposition rates of biodegradable materials, ensuring effective marine waste disposal and durability by decomposing in light-irradiated conditions.

JP2024153595AActive Publication Date: 2024-10-29LARGAN MEDICAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2024066046
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-17
Filing Date
2024-04-16
Publication Date
2024-10-29
Estimated Expiration
2044-04-16

AI Technical Summary

Technical Problem

Biodegradable materials often have low decomposition rates and are limited by environmental conditions, leading to ineffective waste disposal and damage to marine ecosystems, with fragile molecular structures prone to decomposition in daily environments.

Method used

A polymer composed of benzene ring derivatives and lactide with caprolactone monomers, designed to decompose in a light-irradiated marine environment, with specific ratios and functional groups to enhance durability and decomposition rates.

Benefits of technology

The polymer achieves targeted decomposition in marine environments, reducing marine ecosystem damage and maintaining durability through controlled decomposition rates and molecular stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153595000001_ABST
    Figure 2024153595000001_ABST
Patent Text Reader

Abstract

To provide a degradable polymer.SOLUTION: A constituent monomer of a polymer includes a benzene ring derivative, lactide and caprolactone. The ratio of the benzene ring derivative in the polymer is smaller than the ratio of lactide in the polymer. The ratio of the benzene ring derivative in the polymer is smaller than the ratio of caprolactone in the polymer. Thereby, a product produced from the polymer can be decomposed in a light-irradiated marine environment, contributing to reducing the destruction of marine ecosystems by waste products.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to polymers and coating materials, and more particularly to polymers and coating materials that are adapted to assembled products and have degradability. [Background technology]

[0002] In recent years, with the rise in environmental awareness, there has been an increasing call for the use of environmentally friendly materials in everything from everyday items to electronic products. Common environmentally friendly materials include recyclable materials, regenerated materials and biodegradable materials. Biodegradable materials can reduce damage to the ecological environment and, due to their biodegradable nature, can also reduce the recycling costs of such products. Therefore, they are widely used in low-cost products that are used in large quantities in daily life, such as snack packaging bags, carrier bags and disposable containers. Summary of the Invention [Problem to be solved by the invention]

[0003] There are many products made of biodegradable materials, but most biodegradable materials have a low decomposition rate and their decomposition effect is limited by the environment, and they can usually only decompose in high temperature and high humidity environments, so if the waste is not properly treated and enters the ocean, it cannot be effectively decomposed and will ultimately destroy the marine ecosystem. In addition, because biodegradable materials have decomposable properties, their molecular structure is relatively fragile and they are easily decomposed or chemically reacted in the daily environment, which reduces their durability or may be damaged before they are made into products.

[0004] As can be seen from the above, research and development of biodegradable materials that are not limited by the environment and have high durability has become a very important goal. [Means for solving the problem]

[0005] The present disclosure provides a method for producing a product having degradable properties by designing a polymer having monomers of benzene ring derivatives, lactide and caprolactone, and the product produced from the polymer can be decomposed in a marine environment exposed to light, thereby contributing to reducing the damage to the marine ecosystem caused by waste products.

[0006] The polymer provided by the present disclosure is degradable, and the constituent monomers of the polymer include a benzene ring derivative, lactide, and caprolactone, and the proportion of the benzene ring derivative in the polymer is smaller than the proportion of lactide in the polymer, and the proportion of the benzene ring derivative in the polymer is smaller than the proportion of caprolactone in the polymer. The decomposition rate of the polymer in a marine environment exposed to light on the 28th day is called Drus28, and satisfies the condition of 13%≦Drus28.

[0007] The coating material provided by the present disclosure includes the polymer described in the preceding paragraph.

[0008] The assembled product provided by the present disclosure includes the coating material described in the preceding paragraph.

[0009] The polymer provided by the present disclosure is degradable, and the constituent monomers of the polymer include a benzene ring derivative, lactide and caprolactone, and the benzene ring derivative has at least one of a hydroxy group, a carbonyl group and an ether group. The wavelength at which the polymer has maximum absorbance is designated as WAmax, and satisfies the condition WAmax≦300 nm.

[0010] The coating material provided by the present disclosure includes the polymer described in the preceding paragraph.

[0011] The assembled product provided by the present disclosure includes the coating material described in the preceding paragraph. [Brief description of the drawings]

[0012] [Figure 1] FIG. 2 shows wavelength vs. absorbance diagrams for polymers according to a first embodiment and a second embodiment of the present disclosure. [Diagram 2] FIG. 2 shows a wavelength vs. transmittance diagram for polymers according to a first embodiment and a second embodiment of the present disclosure. [Diagram 3] FIG. 2 shows a graph showing the change in decomposition rate of a polymer according to a first embodiment of the present disclosure in a marine environment exposed to light and in a marine environment without light. [Figure 4] FIG. 2 shows a graph showing the change in decomposition rate of a polymer according to a second embodiment of the present disclosure in a marine environment exposed to light and in a marine environment without light. [Diagram 5] FIG. 2 shows a graph showing changes in biodegradation rates in a soil environment for polymers according to the first to third examples of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The polymer provided by the present disclosure has degradability, and the constituent monomers of the polymer include a benzene ring derivative, lactide, and caprolactone. Thus, the present disclosure designs a polymer with a benzene ring derivative, lactide, and caprolactone as monomers to manufacture a product with degradable properties, and the product manufactured from the polymer can be decomposed in a marine environment exposed to light, thereby contributing to the reduction of damage to the marine ecosystem caused by waste products.

[0014] According to the polymer provided by the present disclosure, the ratio of the benzene ring derivative in the polymer is smaller than the ratio of lactide in the polymer, and the ratio of the benzene ring derivative in the polymer is smaller than the ratio of caprolactone in the polymer. By adjusting the ratio of the benzene ring derivative in the polymer to be smaller than the ratio of lactide and caprolactone in the polymer, the ratio of the benzene ring derivative in the polymer is small, that is, it has the effect of decomposing in a marine environment exposed to light, and can contribute to balancing the decomposition rate and durability of the polymer. The ratio of the benzene ring derivative, lactide and caprolactone in the polymer may be 1:2 to 7:2 to 5, and may be 1:2:2, 1:2:3, 1:3:3, 1:4:3, 1:4:4, 1:5:4, 1:5:5, 1:6:5 or 1:7:5, but the present disclosure is not limited to the above ratio.

[0015] According to the polymer provided by the present disclosure, the decomposition rate of the polymer in a marine environment exposed to light on the 28th day is defined as Drus28, and satisfies the condition of 13%≦Drus28. By satisfying the decomposition rate of the polymer in a marine environment exposed to light, it is possible to improve the decomposition effect in a marine environment exposed to light after disposal of a product made from the polymer, prevent the polymer product from remaining in the ocean, and further reduce damage to the marine ecosystem. It is also possible to satisfy the condition of 14%≦Drus28. It is also possible to satisfy the condition of 15%≦Drus28≦100%.

[0016] According to the polymer provided by the present disclosure, the benzene ring derivative has at least one of a hydroxy group, a carbonyl group, and an ether group. By designing the monomer of the polymer to be a benzene ring derivative having a hydroxy group, a carbonyl group, and an ether group, the functional group can participate in the photoreaction, increase the number of intramolecular or intermolecular bonds, and contribute to improving the photoreaction rate of the benzene ring derivative.

[0017] According to the polymer provided by the present disclosure, the wavelength at which the polymer has maximum absorbance is WAmax, and the condition WAmax≦300 nm is satisfied. As a result, the atmospheric layer can block light rays with wavelengths of 300 nm or less, so by limiting the wavelength at which the polymer has maximum absorbance to 300 nm or less, the polymer can be prevented from being consumed by chemical reaction due to irradiation with natural light, and this can contribute to improving the durability of the polymer. The condition WAmax≦400 nm may be satisfied. The condition WAmax≦350 nm may be satisfied. The condition 0 nm≦WAmax≦270 nm may be satisfied.

[0018] According to the polymer provided by the present disclosure, the benzene ring derivative may have light absorbing properties.Therefore, by designing the benzene ring derivative in the polymer to have the properties of a light absorber, electron transfer occurs in the polymer upon irradiation with light, which can contribute to reducing the difficulty of the polymer undergoing chemical reaction.

[0019] According to the polymer provided by the present disclosure, the average molecular weight of the polymer is Mw, and may satisfy the condition of 300 g / mole≦Mw. By satisfying the lower limit of the average molecular weight of the polymer, the polymer can be prevented from passing through the cell membrane, which contributes to improving biosecurity. The condition of Mw≦10000 g / mole may be satisfied. By limiting the upper limit of the average molecular weight of the polymer, the difficulty of cleaving the molecular bonds can be reduced, which contributes to reducing the difficulty of decomposing the polymer. The condition of 300 g / mole≦Mw≦10000 g / mole may be satisfied. The condition of 500 g / mole≦Mw may be satisfied. The condition of 1000 g / mole≦Mw≦10000 g / mole may be satisfied. The condition of 1200 g / mole≦Mw≦8000 g / mole may be satisfied. The condition of 1500 g / mole≦Mw≦6000 g / mole may be satisfied. In addition, the condition 2000 g / mole≦Mw≦4000 g / mole may be satisfied.

[0020] According to the polymer provided by the present disclosure, the decomposition temperature of the polymer is Pt, and the condition of 100°C≦Pt may be satisfied. By satisfying the decomposition temperature of the polymer, it is possible to contribute to the stable maintenance of the structure of the polymer at high temperatures. The condition of 120°C≦Pt may be satisfied. The condition of 150°C≦Pt≦1000°C may be satisfied. The condition of 180°C≦Pt≦800°C may be satisfied. The condition of 200°C≦Pt≦500°C may be satisfied.

[0021] According to the polymer provided by the present disclosure, the viscosity of the polymer is Vi, and may satisfy the condition Vi≦500 Pa·s. By limiting the viscosity of the polymer, it is possible to ensure that the polymer has good fluidity and contribute to improving the convenience of using the polymer. Note that the condition Vi≦300 Pa·s may be satisfied. Note that the condition Vi≦100 Pa·s may be satisfied. Note that the condition Vi≦50 Pa·s may be satisfied. Note that the condition 1 Pa·s≦Vi≦30 Pa·s may be satisfied.

[0022] According to the polymer provided by the present disclosure, the solubility of the polymer in water is Sw, and may satisfy the condition Sw≦5.00%. By limiting the solubility of the polymer in water, it is possible to prevent the polymer from being deactivated by moisture or water sprinkling, and contribute to improving the waterproofing of the polymer. It may satisfy the condition Sw≦3.00%. It may satisfy the condition Sw≦1.00%. It may satisfy the condition 0.00%≦Sw≦0.50%. It may satisfy the condition 0.10%≦Sw≦0.35%.

[0023] According to the polymer provided by the present disclosure, the decomposition rate of the polymer on the 28th day in a marine environment exposed to light is Drus28, and the decomposition rate of the polymer on the 28th day in a marine environment without light is Drs28, and the condition of 1%≦Drus28-Drs28 may be satisfied. By satisfying the difference in the decomposition rate between the marine environment exposed to light and the marine environment without light, it is possible to contribute to improving the additive effect of the decomposition of the polymer by light irradiation. The condition of 3%≦Drus28-Drs28 may be satisfied. The condition of 5%≦Drus28-Drs28≦100% may be satisfied.

[0024] According to the polymer provided by the present disclosure, the decomposition rate of the polymer on day 178 in a marine environment exposed to light is Drus178, and the decomposition rate of the polymer on day 178 in a marine environment without light is Drs178, and the condition of 5%≦Drus178-Drs178 may be satisfied. This satisfies the difference in long-term decomposition rate between a marine environment exposed to light and a marine environment without light, thereby contributing to improving the upper limit of the additive effect on the decomposition of the polymer by light irradiation. The condition of 10%≦Drus178-Drs178 may be satisfied. The condition of 15%≦Drus178-Drs178 may be satisfied. The condition of 20%≦Drus178-Drs178 may be satisfied. The condition of 25%≦Drus178-Drs178 may be satisfied. The condition of 30%≦Drus178-Drs178≦100% may be satisfied.

[0025] According to the polymer provided by the present disclosure, the polymer may be biodegradable, and the decomposition rate of the polymer in a soil environment on day 28 is defined as Dr28, and may satisfy the condition of 50%≦Dr28. Thus, by satisfying the decomposition rate of the polymer in a soil environment, it is possible to contribute to improving the decomposition effect of the polymer in a soil environment. The condition may be 60%≦Dr28. The condition may be 70%≦Dr28. The condition may be 80%≦Dr28. The condition may be 90%≦Dr28. The condition may be 95%≦Dr28≦100%.

[0026] According to the polymer provided by the present disclosure, the polymer may have biodegradability, and the time required for the polymer to reach 50% decomposition in a soil environment is defined as TDr50p, and may satisfy the condition TDr50p≦28 days. By satisfying the time required for the polymer to decompose in a soil environment, it is possible to contribute to improving the decomposition efficiency of the polymer in a soil environment. The condition TDr50p≦21 days may be satisfied. The condition 0 days≦TDr50p≦14 days may be satisfied. The condition 1 day≦TDr50p≦7 days may be satisfied. The condition 2 days≦TDr50p≦5 days may be satisfied.

[0027] According to the polymer provided by the present disclosure, the average transmittance of the polymer at wavelengths of 400 nm to 700 nm is T4070, and may satisfy the condition of 70.00%≦T4070. By satisfying the transmittance of the polymer in the visible light band, the influence of the polymer on the light transmittance can be avoided, and the range of application of the polymer can be expanded. The condition of 80.00%≦T4070 may be satisfied. The condition of 90.00%≦T4070 may be satisfied. The condition of 95.00%≦T4070≦100.00% may be satisfied.

[0028] According to the polymer provided by the present disclosure, the average transmittance of the polymer at wavelengths of 700 nm to 1000 nm is T70100, and may satisfy the condition of 70.00%≦T70100. By satisfying the transmittance of the polymer in the near-infrared light band, it is possible to avoid an effect on the transmission of near-infrared light through the polymer, and contribute to making the polymer into a near-infrared light-related product. It may also satisfy the condition of 80.00%≦T70100. It may also satisfy the condition of 90.00%≦T70100. It may also satisfy the condition of 95.00%≦T70100≦100.00%.

[0029] According to the polymer provided by the present disclosure, the decomposition rate of the polymer on the 28th day in an aphotic marine environment is Drs28, and may satisfy the condition of 1%≦Drs28. Thus, by satisfying the decomposition rate of the polymer in an aphotic marine environment, it is possible to contribute to improving the decomposition effect of the polymer in an aphotic marine environment. The condition may be 3%≦Drs28. The condition may be 5%≦Drs28. The condition may be 8%≦Drs28. The condition may be 10%≦Drs28. The condition may be 12%≦Drs28≦100%.

[0030] According to the polymer provided by the present disclosure, the decomposition rate of the polymer on day 178 in an aphotic marine environment is Drs178, and may satisfy the condition of 5%≦Drs178. Thus, by satisfying the decomposition rate of the polymer on day 178 in an aphotic marine environment, it is possible to contribute to improving the long-term decomposition effect of the polymer in an aphotic marine environment. The condition of 10%≦Drs178 may be satisfied. The condition of 15%≦Drs178 may be satisfied. The condition of 20%≦Drs178 may be satisfied. The condition of 25%≦Drs178 may be satisfied. The condition of 30%≦Drs178≦100% may be satisfied.

[0031] According to the polymer provided by the present disclosure, the decomposition rate of the polymer in a marine environment irradiated with light on day 178 is Drus178, and may satisfy the condition of 30%≦Drus178. As a result, by satisfying the decomposition rate of the polymer in a marine environment irradiated with light on day 178, it is possible to contribute to improving the long-term decomposition effect of the polymer in a marine environment irradiated with light. The condition may be 40%≦Drus178. The condition may be 50%≦Drus178. The condition may be 60%≦Drus178. The condition may be 63%≦Drus178≦100%.

[0032] According to the polymer provided by the present disclosure, the decomposition rate of the polymer in a soil environment on day 35 is Dr35, and may satisfy the condition of 50%≦Dr35. As a result, by satisfying the decomposition rate of the polymer in a soil environment on day 35, it is possible to contribute to improving the short-term decomposition effect of the polymer in a soil environment. The condition of 60%≦Dr35 may be satisfied. The condition of 70%≦Dr35 may be satisfied. The condition of 80%≦Dr35 may be satisfied. The condition of 90%≦Dr35 may be satisfied. The condition of 95%≦Dr35≦100% may be satisfied.

[0033] According to the polymer provided by the present disclosure, the decomposition rate of the polymer in a soil environment on the 56th day is Dr56, and may satisfy the condition of 50%≦Dr56. As a result, by satisfying the decomposition rate of the polymer in a soil environment on the 56th day, it is possible to contribute to improving the medium-term decomposition effect of the polymer in a soil environment. It may satisfy the condition of 60%≦Dr56. It may satisfy the condition of 70%≦Dr56. It may satisfy the condition of 80%≦Dr56. It may satisfy the condition of 90%≦Dr56. It may satisfy the condition of 95%≦Dr56≦100%.

[0034] According to the polymer provided by the present disclosure, a catalyst may be added to the polymerization reaction of the polymer, and the catalyst may be stannous isooctanoate, stannous chloride, stannous sulfate, dibutyltin oxide or dibutyltin dilaurate.

[0035] According to the polymer provided by the present disclosure, having light absorbing properties refers to the monomer having or possessing the properties of a light absorber in the polymer. The monomer having light absorbing properties can chemically react after the polymer is irradiated with light, changing the strength or manner of intramolecular or intermolecular bonds, or changing its molecular form. The light absorber refers to a compound or substance that causes a chemical reaction when irradiated with light, and the chemical reaction that occurs when irradiated with light may be called a photoreaction, and the type of light that induces the photoreaction may be ultraviolet light or visible light. The monomer having light absorbing properties of the polymer of the present disclosure may be divided into ultraviolet light absorbing monomers that absorb ultraviolet light, visible light absorbing monomers that absorb visible light, and blue light absorbing monomers that absorb blue light. The benzene ring derivative may be 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone (IRGACURE 2959), 2-hydroxy-2-methyl-1-phenyl-1-propanone (HMPP), α-dimethoxy-α-phenylacetophenone (DMPA), 1-hydroxycyclohexyl phenyl ketone (HCPK) or other compounds having a benzene ring, but the present disclosure is not limited to the above compounds.

[0036] According to the polymers provided by the present disclosure, the average molecular weight of a polymer refers to the number average molecular weight of the whole polymer molecules at the time of testing, and the formula is as follows: Number average molecular weight = (Σ molecular weight) / total number of molecules.

[0037] According to the polymers provided by the present disclosure, the decomposition temperature of a polymer refers to the temperature at which the polymer begins to thermally decompose.

[0038] According to the polymers provided by the present disclosure, the viscosity of a polymer refers to the stickiness of the polymer and can represent the flowability of the polymer.

[0039] According to the polymers provided by the present disclosure, the solubility of the polymer in water refers to the solubility of the polymer when water is used as a solvent. During testing, a very small amount of the polymer is gradually added to water as a solute until the polymer cannot be dissolved.

[0040] According to the polymer provided by the present disclosure, the absorbance and transmittance of the polymer are obtained by performing an absorbance test once every 20 nm at wavelengths of 200 nm to 1000 nm using a spectrophotometer, and measuring the absorbance (OD). One side of the spectrophotometer has a light source and provides parallel light beams of various wavelengths. After the light beam passes through a test object, a detector on the other side detects the light beam intensity. The absorbance can be obtained by comparing the light beam intensity before and after passing through the test object, and the relationship between the absorbance and the transmittance is as follows: Absorbance=-log 10 (transmittance).

[0041] Because the polymer is liquid during measurement, the reflectance is very weak and can be ignored, and the sum of the absorbance and transmittance is 100%, so the absorbance and transmittance can be calculated from the absorbance. When testing the absorbance, the polymer concentration is 0.25% (weight percentage), and the dilution solvent is deionized water. The polymer transmits almost completely at some wavelengths, which causes a negative error in the absorbance. In this case, the absorbance is considered to be 0, and the transmittance is considered to be 100%.

[0042] According to the polymers provided by the present disclosure, the biodegradability of a polymer refers to the ability of the polymer to be gradually decomposed by microorganisms in a given environment.

[0043] According to the polymer provided by the present disclosure, the marine environment refers to immersing the specimen in a decomposition solution of simulated seawater. Specifically, the specimen and the decomposition solution are placed in a decomposition tank at a weight ratio of 1:6, and the decomposition tank is kept at 25±2°C and continuously observed for 180 days. The composition and steps of the decomposition solution are as follows:

[0044] I. Stock solution for mineral medium:

[0045] Solution (a): 8.50 g KH2PO4, 21.75 g K2HPO4, 33.40 g Na2HPO4 and 0.50 g NH4Cl were dissolved in deionized water to a total volume of 1 L and the pH value was adjusted to 7.4.

[0046] Solution (b): 27.50 g of CaCl2 or 36.40 g of CaCl2·2H2O were dissolved in deionized water to a total volume of 1 L.

[0047] Solution (c): 22.50 g of MgSO4·7H2O was dissolved in deionized water until the total volume reached 1 L.

[0048] Solution (d): 0.25 g of FeCl3·6H2O was dissolved in deionized water to a total volume of 1 L. For ease of storage, one drop of concentrated sulfuric acid or 0.4 g of ethylenediaminetetraacetic acid (EDTA) may be added to this solution.

[0049] II. Mineral medium: 10 mL of solution (a) was added to 800 mL of deionized water, then 1 mL each of solution (b), solution (c) and solution (d) were added in sequence, and the volume was supplemented to 1 L with deionized water.

[0050] III. Compost pretreatment - preparation of digested solution:

[0051] After removing large aggregates from the compost used in ASTM-D5338, the compost was washed with culture medium, centrifuged (1100g, 10min) and the supernatant was removed. This was repeated 3-5 times, dried in an oven at 70℃, and before use, redissolved in culture medium to 3g / L-5g / L, stirred for 2 minutes, left to stand for 20 minutes to allow the particles to settle, and then the supernatant was added to the culture medium, mixed with a decomposition solution with a concentration of 10mL / L, and the pH value was adjusted to 7.4±0.2.

[0052] During the test, fresh 0.1M KOH solution is mixed and dispensed into a 50mL PP tank, then placed in the decomposition tank, which is then placed at the bottom of a room temperature sealed box (25±2℃) measuring 88.4cm (length) x 70.2cm (width) x 76.4cm (height) for incubation, and the KOH solution absorbs the CO2 released during the decomposition of the test subject. The frequency of replacement of the KOH solution in the early stages of the test (1st to 30th days) is 6 times / week, and after one month, it is changed to 2 times / week until the 180th day, and the total test time may exceed 180 days.

[0053] The collected KOH solution is measured with a pH meter and compared with a control (0.1M KOH solution, placed in an incubator where no decomposition reaction is taking place), and then converted into hydrogen ion concentration. The hydrogen ion concentration is then converted into the weight of CO2 to estimate the decomposition rate. The conversion formula mentioned above is as follows: (1) Change in hydroxyl concentration = hydroxyl concentration of the control group - hydroxyl concentration of the experimental group = hydrogen ion concentration. (2) Change in weight of carbon dioxide (unit: mg) = concentration of hydrogen ions × 44 / 2 × 50 mL, where 44 is the molecular weight of carbon dioxide, 2 is the reaction equilibrium constant of carbon dioxide, and 50 mL is the volume of the aqueous solution. (3) Percentage of mineralization (decomposition) = weight change of carbon dioxide / theoretical amount of carbon dioxide required for complete decomposition by the subject × 100%.

[0054] According to the polymer provided by the present disclosure, the light irradiation environment and the no-light environment refer to whether or not the polymer is irradiated with light. The lamps used for the light irradiation are TL-K 40W / 10-R SLV from Shentell Corporation and TL 20W / 52 SLV / 25 from Philips Corporation, and the two types of lamps are installed at the top of the sealed box, and the wavelength of the light irradiation is about 350nm to 500nm.

[0055] According to the polymer provided by the present disclosure, the soil environment refers to a test environment with ASTM-D5338 as the standard measurement method, and the decomposition rate of the soil environment is the test result obtained by the ASTM-D5338 method, which is the decomposition percentage calculated by weight. In detail, the subject and activated sludge (fertilizer) are mixed with each other in a weight ratio of 1:6, and the moisture content in the decomposition tank is maintained at about 50% with perlite, and the decomposition tank is placed at 58±2°C and continuously observed for 180 days. The main components of the fertilizer include livestock manure, soybean flour, bagasse, wood chips, wheat bran, and mushroom cultivation waste, and the components of perlite are as shown in Table 1 below. [Table 1]

[0056] During the test, fresh 0.1M KOH solution is mixed and dispensed into a 50mL PP tank, which is then placed in the decomposition tank and incubated in an incubator (58±2℃), allowing the KOH solution to absorb the CO2 released during the decomposition of the test subject. The frequency of replacement of the KOH solution in the early stages of the test (days 1-30) is 6 times / week, and after one month, it is changed to 2 times / week until day 180, and the total test time may exceed 180 days.

[0057] The collected KOH solution is measured with a pH meter and compared with a control (0.1M KOH solution, placed in an incubator where no decomposition reaction is taking place), and then converted into hydrogen ion concentration. The hydrogen ion concentration is then converted into the weight of CO2 to estimate the decomposition rate. The conversion formula mentioned above is as follows: (1) Change in hydroxyl concentration = hydroxyl concentration of the control group - hydroxyl concentration of the experimental group = hydrogen ion concentration. (2) Change in weight of carbon dioxide (unit: mg) = concentration of hydrogen ions × 44 / 2 × 50 mL, where 44 is the molecular weight of carbon dioxide, 2 is the reaction equilibrium constant of carbon dioxide, and 50 mL is the volume of the aqueous solution. (3) Percentage of mineralization (decomposition) = weight change of carbon dioxide / theoretical amount of carbon dioxide required for complete decomposition by the subject × 100%.

[0058] According to the polymers provided by the present disclosure, the degradation rate of the polymer on the nth day refers to the degradation rate of the polymer on the nth day in a soil environment, the degradation rate of the polymer on the nth day in a lightless marine environment, or the degradation rate of the polymer on the nth day in a light-exposed marine environment. The nth day may be the 7th day, 8th day, 9th day, 10th day, 14th day, 21st day, 24th day, 25th day, 26th day, 28th day, 29th day, 30th day, 31st day, 35th day, 42nd day, 49th day, 52nd day, 56th day, 59th day, 63rd day, 66th day, 70th day, 73rd day, 77th day, 80th day, 84th day, 87th day, 91st day, 94th day, 98th day, 101st day, 105th day, 140th day, 150th day, 154th day, 157th day, 175th day, 178th day, or 180th day, or may be the degradation rate on any day from 1st day to 180th day. For example, the Dr28 is the decomposition rate of the polymer in a soil environment on the 28th day, and may be defined separately according to the above rules, Dr21 represents the decomposition rate of the polymer in a soil environment on the 21st day, Drs14 represents the decomposition rate of the polymer in a light-free marine environment on the 14th day, and Drus42 represents the decomposition rate of the polymer in a light-irradiated marine environment on the 42nd day, and by analogy, the present disclosure is not limited to the above examples.

[0059] According to the polymers provided by the present disclosure, the polymers may be used in, but are not limited to, adhesive materials, repair materials, coating materials, wrapping materials, or packaging materials.

[0060] The coating material provided by the present disclosure includes the polymer. The coating material may include adhesive, viscose, gel, light curing adhesive, and oxidizing adhesive. The coating material may have viscosity or may be cured after light irradiation to form a film layer, and may adhere substances, elements, or objects that come into contact with the coating material by light irradiation. The coating material may be used in, but is not limited to, electronic products, packaging, clothing, containers, and various assembled products.

[0061] The present disclosure provides an assembly product comprising the coating material. The assembly product refers to a product that requires parts to be assembled, such as, but not limited to, mobile phones, smart bracelets, watches, cameras, laptops, desktop computer hosts, screens, mice, keyboards, home appliances, chairs, desks, batteries, bicycles, motorcycles, automobiles, containers, tableware, clothing, and packaging.

[0062] Based on the above embodiment, specific examples will be proposed and described in detail below with reference to the drawings.

[0063] <First Example>

[0064] The constituent monomers of the polymer of the first embodiment include a benzene ring derivative, lactide, and caprolactone, and the benzene ring derivative of the first embodiment is 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone.

[0065] In the first example polymer, the average molecular weight of the polymer is Mw, the decomposition temperature of the polymer is Pt, the viscosity of the polymer is Vi, and the solubility of the polymer in water is Sw, and the conditions that Mw=3700 g / mole, Pt=246° C., Vi=6.547 Pa s, and Sw=0.38% are satisfied.

[0066] For the polymer of the first embodiment, the wavelength at which the polymer has maximum absorbance is WAmax, the average transmittance of the polymer at wavelengths of 400 nm to 700 nm is T4070, and the average transmittance of the polymer at wavelengths of 700 nm to 1000 nm is T70100, satisfying the conditions WAmax=280 nm, T4070=100.00%, and T70100=99.50%.

[0067] For the polymer of the first embodiment, the decomposition rate of the polymer on day 28 in a light-free marine environment is designated as Drs28, and the decomposition rate of the polymer on day 28 in a light-exposed marine environment is designated as Drus28, which satisfy the conditions Drs28 = 13%, Drus28 = 16%, and Drus28 - Drs28 = 3%.

[0068] For the polymer of the first embodiment, the decomposition rate of the polymer on day 178 in a marine environment without light is designated as Drs178, and the decomposition rate of the polymer on day 178 in a marine environment exposed to light is designated as Drus178, which satisfy the conditions Drs178 = 31%, Drus178 = 64%, and Drus178 - Drs178 = 33%.

[0069] For the polymer of the first embodiment, the decomposition rate of the polymer in a soil environment on the 28th day is Dr28, the decomposition rate of the polymer in a soil environment on the 35th day is Dr35, the decomposition rate of the polymer in a soil environment on the 56th day is Dr56, and the time required for the polymer to reach a 50% decomposition rate in the soil environment is TDr50p, which satisfies the conditions Dr28=100%, Dr35=99%, Dr56=98%, and TDr50p=3 days.

[0070] The chemical structure and properties of the first example polymer are listed in Table 2 below.

[0071] <Second Example>

[0072] The constituent monomers of the polymer of the second embodiment include a benzene ring derivative, lactide and caprolactone, and the benzene ring derivative of the second embodiment is 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone.

[0073] The chemical structure and properties of the polymer of the second embodiment are listed in Table 2 below. The definitions of other parameters in Table 2 of the second embodiment are all the same as those of the first embodiment, and are not repeated here.

[0074] <Third Example>

[0075] The constituent monomers of the polymer of the third embodiment include a benzene ring derivative, lactide and caprolactone, and the benzene ring derivative of the third embodiment is 2-hydroxy-4'-(2-hydroxyethoxy)-2-methylpropiophenone.

[0076] The chemical structure and properties of the polymer of the third embodiment are listed in Table 2 below. The definitions of other parameters in Table 2 of the third embodiment are all the same as those of the first embodiment, and are not repeated here. [Table 2]

[0077] 1 and 2, Fig. 1 shows the relationship between wavelength and absorbance of the polymers according to the first and second embodiments of the present disclosure, and Fig. 2 shows the relationship between wavelength and transmittance of the polymers according to the first and second embodiments of the present disclosure. The present disclosure measured the absorbance and transmittance of the polymers according to the first and second embodiments of the present disclosure at different wavelengths of light, and the measurement results are shown in Table 3 below. [Table 3]

[0078] As can be seen from Table 3, Figures 1 and 2, the wavelength of maximum absorbance of the polymer of the present disclosure may be less than 300 nm, which can prevent the polymer from being consumed by chemical reaction due to irradiation with natural light, and contribute to improving the durability of the polymer. In addition, the average transmittance of the polymer of the present disclosure at wavelengths of 400 nm to 700 nm may be greater than 70.00%, which can prevent the polymer from affecting the light transmittance, and contribute to expanding the application range of the polymer.

[0079] 3 and 4, Fig. 3 shows a graph of the change in the decomposition rate of the polymer of the first embodiment of the present disclosure in a marine environment exposed to light and in an achromatic marine environment, and Fig. 4 shows a graph of the change in the decomposition rate of the polymer of the second embodiment of the present disclosure in a marine environment exposed to light and in an achromatic marine environment. In the present disclosure, the decomposition rates of the polymers of the first embodiment and the second embodiment in a marine environment exposed to light and in an achromatic marine environment were measured, and the achromatic marine environment refers to the irradiation of the polymer with light including ultraviolet light (UV), and the achromatic marine environment refers to the absence of ultraviolet light irradiation. The measurement results are shown in Table 4 below. [Table 4]

[0080] As can be seen from Table 4, Figures 3 and 4 above, the difference in degradation rate of the polymer of the present disclosure between a light-irradiated marine environment and a lightless marine environment on day 28 may be greater than 1%, and the difference in degradation rate on day 178 may be greater than 5%, which contributes to the additive effect of light irradiation on the degradation of the polymer and further improves the upper limit of the additive effect.

[0081] Referring to Fig. 5, Fig. 5 shows a change in biodegradation rate in soil environment of the polymers according to the first to third examples of the present disclosure. In the present disclosure, the decomposition rates in soil environment of the polymers according to the first to third examples were measured, and the measurement results are shown in Table 5 below. [Table 5]

[0082] As can be seen from Table 5 and Figure 5 above, the decomposition rate of the polymer of the present disclosure in soil environment on day 28 can be greater than 50%, which contributes to improving the decomposition effect of the polymer in soil environment. In addition, the time for the polymer of the present disclosure to reach 50% decomposition rate in soil environment can be shorter than 28 days, which contributes to improving the decomposition efficiency of the polymer in soil environment.

[0083] The present disclosure has been disclosed as above by the embodiments, but the embodiments do not limit the present disclosure, and those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present disclosure. Therefore, the scope of protection of the present disclosure is based on the contents specified in the following claims.

Claims

1. A degradable polymer containing a benzene ring derivative, lactide and caprolactone as constituent monomers, a ratio of the benzene ring derivative in the polymer is smaller than a ratio of the lactide in the polymer, and a ratio of the benzene ring derivative in the polymer is smaller than a ratio of the caprolactone in the polymer, The decomposition rate of the polymer after 28 days in a marine environment exposed to light is designated Drus28. 13%≦Drus28 A polymer that satisfies the above conditions.

2. The polymer of claim 1 , wherein the benzene ring derivative has light absorbing properties.

3. The polymer of claim 2 , wherein the benzene ring derivative has at least one of a hydroxy group, a carbonyl group, and an ether group.

4. The average molecular weight of the polymer is designated Mw; 300g / mole≦Mw The polymer according to claim 1, which satisfies the following conditions:

5. The average molecular weight of the polymer is designated Mw; Mw≦10000g / mole The polymer according to claim 1, which satisfies the following conditions:

6. The decomposition temperature of the polymer is Pt; 100°C≦Pt The polymer according to claim 1, which satisfies the following conditions:

7. The viscosity of the polymer is designated Vi; Vi≦500Pa・s The polymer according to claim 6, which satisfies the following conditions:

8. The solubility of the polymer in water is represented by Sw, Sw≦5.00% The polymer according to claim 1, which satisfies the following conditions:

9. The degradation rate of the polymer in the irradiated marine environment after 28 days is designated as Drus28, and the degradation rate of the polymer in the aphotic marine environment after 28 days is designated as Drs28; 1%≦Drs28-Drs28 The polymer according to claim 1, which satisfies the following conditions:

10. The degradation rate of the polymer in the irradiated marine environment after 178 days is designated as Drus178, and the degradation rate of the polymer in the aphotic marine environment after 178 days is designated as Drs178; 5%≦Drus178-Drs178 The polymer according to claim 9, which satisfies the following conditions:

11. The polymer is biodegradable, and the decomposition rate of the polymer in a soil environment after 28 days is designated Dr28; 50%≦Dr28 The polymer according to claim 1, which satisfies the following conditions:

12. The polymer is biodegradable, and the time it takes for the polymer to reach 50% decomposition in a soil environment is designated TDr50p; TDr50p≦28 days The polymer according to claim 1, which satisfies the following conditions:

13. A coating material comprising the polymer of claim 1.

14. 14. An assembled product comprising the coating material of claim 13.

15. A degradable polymer containing a benzene ring derivative, lactide and caprolactone as constituent monomers, the benzene ring derivative has at least one of a hydroxy group, a carbonyl group, and an ether group; The wavelength at which the polymer has maximum absorbance is designated WAmax; WAmax≦300 nm A polymer that satisfies the above conditions.

16. The polymer of claim 15, wherein the benzene ring derivative has light absorbing properties.

17. The average molecular weight of the polymer is designated Mw; 300g / mole≦Mw≦10000g / mole The polymer according to claim 15, which satisfies the following condition.

18. The solubility of the polymer in water is represented by Sw, Sw≦5.00% The polymer according to claim 15, which satisfies the following conditions:

19. The polymer has an average transmittance of T4070 at wavelengths of 400 nm to 700 nm, 70.00%≦T4070 The polymer according to claim 15, which satisfies the following conditions:

20. The polymer is biodegradable, and the decomposition rate of the polymer in a soil environment after 28 days is designated Dr28; 50%≦Dr28 The polymer according to claim 15, which satisfies the following conditions:

21. The polymer is biodegradable, and the time it takes for the polymer to reach 50% decomposition in a soil environment is designated TDr50p; TDr50p≦28 days The polymer according to claim 15, which satisfies the following conditions:

22. A coating material comprising the polymer of claim 15.

23. 23. An assembly comprising the coating material of claim 22.

Citation Information

Patent Citations

  • Polycaprolactone-inlay block-polylactide copolymer preparation method

    CN106496531A

  • Alternating (aba)▲downn▼ polylactide block copolymer

    JP1996506849A

  • Biodegradable Copolymers Attached to Segments with Multiple Functional Groups

    JP2004526043A

  • Method for producing photodegradable polymeric compound

    JP2007131710A

  • Biodegradability block copolymer and production method of the same, and compact

    JP2014047317A