Method for producing transparent rigid thermoplastic polyurethane

A thermoplastic polyurethane with a specific polyol composition and hard segment content is developed, addressing the balance of high hardness, modulus, and elongation, resulting in a transparent, non-brittle material with improved processing and reduced toxicity.

JP2024153852AActive Publication Date: 2024-10-29BASF SE
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024125210
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2016-12-23
Filing Date
2024-07-31
Publication Date
2024-10-29
Estimated Expiration
2037-12-22

AI Technical Summary

Technical Problem

Existing rigid thermoplastic polyurethanes face challenges in achieving a balance of high hardness, high modulus, and good elongation at break, often being brittle and difficult to process, with concerns over toxicity from certain components like bisphenol A.

Method used

A thermoplastic polyurethane is developed using a polyol composition with a molecular weight of 500 to 2000 g/mol and an aromatic polyester block, along with a hard segment content less than 75%, incorporating polyisocyanate and chain extenders to create a transparent, non-brittle material with high hardness and elasticity.

Benefits of technology

The solution results in a thermoplastic polyurethane with high hardness (over 75 Shore D), a modulus of elasticity greater than 2000 MPa, and an elongation at break of over 300%, while being transparent and processed through simple and inexpensive methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024153852000001
    Figure 2024153852000001
  • Figure 2024153852000002
    Figure 2024153852000002
Patent Text Reader

Abstract

To provide a thermoplastic polyurethane which is firstly transparent and has high hardness and a high elastic modulus and secondly has very good elongation at break and to provide a method for producing the same.SOLUTION: There is provided a transparent thermoplastic polyurethane which can be obtained or was obtained by converting (i) a polyisocyanate composition, (ii) at least one chain extender and (iii) at least one polyol composition, wherein the polyol composition includes at least one polyol (P1) having molecular weight Mw in the range of 500 to 2000 g / mol and at least one aromatic polyester block (B1) and a hard segment content is<75%, the chain extender used in (ii) is a diol having molecular weight of Mw<220 g / mol and the chain extender used in (ii) and the polyol (P1) present in the polyol composition are used in a molar ratio of 40:1 to 1:10.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoplastic polyurethane obtainable or obtained by converting a polyisocyanate composition, a chain extender and a polyol composition, wherein the polyol composition comprises a polyol (P1) having a molecular weight Mw in the range of 500-2000 g / mol and at least one aromatic polyester block (B1), and the hard segment content in the thermoplastic polyurethane is <75%. The present invention further relates to a process for producing a molding comprising such a thermoplastic polyurethane, and to a molding obtainable or obtained by the process of the present invention. [Background technology]

[0002] Thermoplastic polyurethanes for various applications are generally known from the prior art. By varying the feedstock, it is possible to obtain different aspects of the properties.

[0003] US5574092 discloses rigid thermoplastic polyurethanes having a Tg of at least 50° C., comprising hard segments based on diisocyanates and chain extender mixtures containing aromatic diols. According to the examples, very brittle materials are obtained, having elongations at break of less than 170%.

[0004] US5627254 describes the units of butanediol (BDO) and HO-(CH 2 CH 2 O) n Rigid thermoplastic polyurethanes have been disclosed that contain polyethylene glycol (PEG) units of the -H type, where n is an integer from 2 to 6. These materials have the disadvantage of being brittle and difficult to process.

[0005] WO2015 / 063062A1 relates to thermoplastic polyurethanes obtainable or obtained by reacting at least one aliphatic polyisocyanate, at least one chain extender and at least one polyol composition, the polyol composition comprising a polyol selected from the group consisting of polyetherols and at least one bisphenol derivative selected from the group consisting of bisphenol A derivatives with a molecular weight Mw>315 g / mol and bisphenol S derivatives with a molecular weight Mw>315 g / mol, where at least one of the OH groups of the bisphenol derivative is alkoxylated. The document also relates to a process for producing the thermoplastic polyurethanes and to a process for using the thermoplastic polyurethanes of the invention for the manufacture of extrusion products, films and mouldings. Such aliphatic TPUs have a hardness >70 Shore D but a low modulus and a completely insufficient elongation at break. A further disadvantage is the use of bisphenol A, which is of some concern from a toxicological point of view.

[0006] Typically, rigid thermoplastic polyurethanes have a hard segment content of 75% or more and are obtained by reacting isocyanates with chain extenders, such as hexane-1,6-diol or cyclohexane-1,4-dimethanol. These materials have high hardness and high dimensional stability, but are very brittle and have elongations at break of less than 200% or even less than 100%.

[0007] However, many applications require materials that not only have a high hardness, i.e. in particular a hardness >75 Shore D and a modulus >2000 MPa at room temperature, but also a good elongation at break of more than 300%. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] US5574092 [Patent Document 2] US5627254 [Patent Document 3] WO2015 / 063062A1 Summary of the Invention [Problem to be solved by the invention]

[0009] In progress from the prior art, it was an object of the present invention to provide a thermoplastic polyurethane which is, firstly, transparent, has a high hardness and a high modulus, and, secondly, has a very good elongation at break. A further object of the present invention was to provide a thermoplastic polyurethane which is, firstly, transparent, has a high hardness and a high modulus, and, secondly, has a very good elongation at break, and which can be produced in a simple and inexpensive manner, in a one-shot process. [Means for solving the problem]

[0010] This object is achieved according to the present invention by providing a composition comprising at least components (i) to (iii): (i) a polyisocyanate composition, (ii) at least one chain extender, and (iii) at least one polyol composition A thermoplastic polyurethane obtained or obtained by converting The polyol composition comprises at least one polyol (P1) having a molecular weight Mw in the range of 500 to 2000 g / mol and at least one aromatic polyester block (B1), The hard segment content in the thermoplastic polyurethane is <75%; This can be achieved with thermoplastic polyurethanes. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] According to the invention, the polyol (P1) has a molecular weight Mw in the range of 500 to 2000 g / mol. The polyol (P1) also has an aromatic polyester block (B1). This is understood to mean that in the context of the invention, the aromatic polyester block (B1) can be a polyester of an aromatic dicarboxylic acid and an aliphatic diol or a polymer of an aliphatic dicarboxylic acid and an aromatic diol. The aromatic polyester block (B1) in the context of the invention is preferably a polyester of an aromatic dicarboxylic acid and an aliphatic diol. Suitable aromatic dicarboxylic acids here are, for example, terephthalic acid, isophthalic acid or phthalic acid, preferably terephthalic acid. Thus, suitable polyols (P1) in the context of the invention are, for example, those having at least one polyethylene terephthalate block or at least one polybutylene terephthalate block, the number of repeat units in the aromatic system being at least 2 in series. The aromatic polyester block (B1) is preferably prepared in a separate step before further conversion to a polyol, in order to ensure sufficient block length of the repeat units of the aromatic system.

[0012] According to the invention, the thermoplastic polyurethane can in particular be a compact thermoplastic polyurethane. Thus, in a further embodiment, the invention relates to a thermoplastic polyurethane as described above, in which the thermoplastic polyurethane is a compact thermoplastic polyurethane.

[0013] Thus, in a further embodiment, the present invention relates to a thermoplastic polyurethane as described above, in which the aromatic polyester block (B1) is a polyester of an aromatic dicarboxylic acid and an aliphatic diol. In yet a further embodiment, the present invention relates to a thermoplastic polyurethane as described above, in which the aromatic polyester block (B1) is a polyethylene terephthalate block or a polybutylene terephthalate block. In yet a further embodiment, the present invention relates to a thermoplastic polyurethane as described above, in which the aromatic polyester block (B1) is a polyethylene terephthalate block.

[0014] According to the present invention, the thermoplastic polyurethane has a hard segment content of <75%, where the hard segment content is the percentage of the thermoplastic polyurethane formed by the isocyanate and the chain extender. In the context of the present invention, the hard segment content is determined by the formula disclosed in WO2007 / 118827A1, where a value of 1.0 corresponds to 100%, and a hard segment content of <75% means that the hard segment content corresponds to a value of <0.75 according to the formula specified in WO2007 / 118827A1.

[0015] Surprisingly, by using a polyol (P1) having a molecular weight Mw in the range of 500 to 2000 g / mol and at least one aromatic polyester block (B1), transparent, hard and at the same time non-brittle thermoplastic polyurethanes with a hard segment content of <75% are obtained. Thus, the thermoplastic polyurethanes of the invention have a hardness of >75 Shore D, a modulus of elasticity at room temperature of >2000 MPa and an elongation at break of >300%.

[0016] In the context of the present invention, suitable polyols (P1) are particularly suitable based on aromatic polyesters, such as polybutylene terephthalate (PBT) or polyethylene terephthalate (PET). The polyols (P1) are preferably prepared by reacting aromatic polyesters with dicarboxylic acids and diols to obtain mixed aromatic / aliphatic polyester diols. For example, in the context of the present invention, it is possible to react aromatic polyesters in solid or liquid form with dicarboxylic acids and diols. According to the present invention, the aromatic polyesters used typically have a molecular weight greater than that of the blocks (B1) present in the polyol (P1).

[0017] The polyester polyols (P1) suitable according to the invention typically comprise from 20% to 70% by weight, preferably from 30% to 60% by weight, more preferably from 35% to 55% by weight, even more preferably from 40% to 50% by weight of aromatic polyester blocks (B1) (in each case based on the total polyester polyol (P1)). In a further embodiment, the invention therefore relates to a thermoplastic polyurethane as described above, in which the polyol (P1) comprises from 20% to 70% by weight of aromatic polyester blocks (B1), based on the total polyester polyol (P1).

[0018] According to the invention, the polyol (P1) has a molecular weight Mw in the range of 500 to 2000 g / mol, preferably in the range of 750 to 1500 g / mol, more preferably in the range of 900 to 1200 g / mol and most preferably in the range of 950 to 1050 g / mol. In a further embodiment, the invention therefore relates to a thermoplastic polyurethane as described above, in which the polyol (P1) has a molecular weight Mw in the range of 750 to 1500 g / mol.

[0019] The molecular weight (Mw) is calculated using the following formula, where z is the functionality of the polyester polyol and z=2: Mw=1000mg / g[(z·56.106g / mol) / (OHN[mg / g])]

[0020] In the preparation of the polyol (P1), it is preferred to use aromatic polyesters such as polybutylene terephthalate (PBT) or polyethylene terephthalate (PET). Polyethylene terephthalate is a thermoplastic polymer that can be produced by polycondensation. The quality of PET and its physical properties, such as toughness or durability, depend on the chain length. The old method of synthesis of PET is based on the transesterification of dimethyl terephthalate with ethylene glycol. Nowadays, PET is almost exclusively synthesized by direct esterification of terephthalic acid with ethylene glycol. Similarly, terephthalic acid can be reacted with butane-1,4-diol to obtain polybutylene terephthalate (PBT). Similar thermoplastic polymers are available under trade names such as CRASTIN® (DuPont), POCAN® (Lanxess), ULTRADUR® (BASF) or ENDURAN® and VESTODUR® (SABIC IP). The chemical and physical / technical properties of the thermoplastic polymer correspond approximately to those of PET.

[0021] According to the present invention, it is also possible to use aromatic polyesters such as polybutylene terephthalate (PBT) or polyethylene terephthalate (PET) obtained from recycling processes. For example, polyethylene terephthalate can be used in the form of flakes obtained from plastic recycling processes. This type of material typically has a molecular weight of about 12000 g / mol.

[0022] According to the invention, suitable polyols (P1) can also be obtained by transesterification using aromatic polyesters, such as polybutylene terephthalate or polyethylene terephthalate, having higher molecular weights with diols. Suitable reaction conditions are known per se to the person skilled in the art.

[0023] Furthermore, diols having 2 to 10 carbon atoms, such as ethanediol, propanediol, butanediol, pentanediol, hexanediol or di- or triethylene glycol, in particular butane-1,4-diol, or mixtures thereof, are used for the preparation of polyol (P1). Short polyether diols, such as PTHF 250 or PTHF 650, or short-chain polypropylene glycols, such as PPG 500, can also be used. The dicarboxylic acids used can be, for example, linear or branched diacids having 4 to 12 carbon atoms or mixtures thereof. Adipic acid, succinic acid, glutaric acid or sebacic acid or mixtures of said acids are preferably used. Adipic acid is particularly preferred in the context of the present invention. According to the present invention, it is also possible to use further polyester diols, such as butanediol adipate or ethylene adipate, as raw materials for the preparation of polyol (P1).

[0024] In the context of the present invention, it is essential to use at least one chain extender and a polyol composition as described above in the preparation of the thermoplastic polyurethane.

[0025] According to the invention it is possible to use one chain extender but also a mixture of different chain extenders.

[0026] The chain extender used in the context of the present invention can be, for example, a compound with a hydroxyl or amino group, in particular with two hydroxyl or amino groups.However, according to the present invention, it is also possible to use a mixture of different compounds as chain extender.In that case, according to the present invention, the average functionality of the mixture is 2.

[0027] According to the invention, it is preferred to use compounds having hydroxyl groups, especially diols, as chain extenders. It is preferred to use aliphatic, araliphatic, aromatic and / or cycloaliphatic diols having a molecular weight of 50 g / mol to 220 g / mol. Alkanediols having 2 to 10 carbon atoms in the alkylene group are preferred, especially di-, tri-, tetra-, penta-, hexa-, hepta-, octa-, nona- and / or decaalkylene glycols. In the present invention, 1,2-ethylene glycol, propane-1,3-diol, butane-1,4-diol, hexane-1,6-diol are particularly preferred. It is also possible to use aromatic compounds such as hydroxyquinone (bis(2-hydroxyethyl)) ether.

[0028] According to the invention, it is also possible to use compounds which contain amino groups, such as diamines, as well as mixtures of diols and diamines.

[0029] As chain extenders, diols with a molecular weight Mw<220 g / mol are preferred. According to the invention, it is possible to use only one diol with a molecular weight Mw<220 g / mol for the preparation of transparent thermoplastic polyurethanes.

[0030] In a further embodiment, two or more diols are used as chain extenders. It is therefore also possible to use a mixture of chain extenders, where at least one diol has a molecular weight Mw<220 g / mol. When using two or more chain extenders, the second chain extender or any further chain extenders thereafter can have a molecular weight of ≧220 g / mol.

[0031] In a further embodiment, the chain extender is selected from the group consisting of butane-1,4-diol and hexane-1,6-diol.

[0032] In a further embodiment, the present invention therefore relates to a thermoplastic polyurethane as described above, wherein the chain extender used in (ii) is a diol having a molecular weight Mw<220 g / mol.

[0033] The chain extender, in particular the diol having a molecular weight Mw<220 g / mol, is preferably used in a molar ratio to the polyol (P1) in the range of 40:1 to 1:10. The chain extender and the polyol (P1) are preferably used in a molar ratio in the range of 20:1 to 1:9, more preferably in the range of 10:1 to 1:8, for example in the range of 5:1 to 1:5, or in the range of 4:1 to 1:4, more preferably in the range of 3:1 to 1:2.

[0034] In a further embodiment, the present invention therefore relates to a thermoplastic polyurethane as described above, wherein the chain extender used in (ii) and the polyol (P1) present in the polyol composition are used in a molar ratio of from 40:1 to 1:10.

[0035] According to the invention, the polyol composition can comprise a further polyol and said at least one polyol (P1).It is therefore also possible in the context of the present invention to use a polyol composition comprising at least one chain extender and said at least one polyol (P1) and at least one further polyol.

[0036] In another embodiment, the present invention provides a thermoplastic polyurethane as described above, wherein the polyol composition comprises a further polyol selected from the group consisting of polyetherols, polyesterols, polycaprolactone alcohols and hybrid polyols.

[0037] The high molecular weight compound having a hydrogen atom reactive with isocyanates used may be a commonly known polyol having a compound reactive with isocyanates.

[0038] Polyols are known in principle to the person skilled in the art and are described, for example, in "Kunststoffhandbuch [Plastics Handbook], Volume 7, Polyurethanes", Carl Hanser Verlag, 3rd Edition, 1993, Chapter 3.1. It is particularly preferred to use polyesterols or polyetherols as polyols. Polyester polyols are particularly preferred. It is likewise possible to use polycarbonates. Copolymers can also be used in the context of the present invention. The number-average molecular weight of the polyols which can be used according to the present invention is preferably 0.5×10 3 g / mol~8×10 3 g / mol, preferably 0.6×10 3 g / mol~5×10 3 g / mol, specifically 0.8×10 3 g / mol~3×10 3 g / mol.

[0039] These materials preferably have an average functionality with respect to isocyanates of 1.8 to 2.3, more preferably 1.9 to 2.2, especially 2.

[0040] The polyesterol used can be a polyesterol based on a diacid and a diol. The diol used is preferably a diol having 2 to 10 carbon atoms, such as ethanediol, propanediol, butanediol, pentanediol, hexanediol or di- or triethylene glycol, in particular butane-1,4-diol, or mixtures thereof. The diacid used can be any known diacid, such as linear or branched diacids having 4 to 12 carbon atoms, or mixtures thereof. It is preferred to use adipic acid as the diacid.

[0041] Suitable polyetherols according to the invention are polyethylene glycol, polypropylene glycol and polytetrahydrofuran.

[0042] In a particularly preferred embodiment, the polyol is polytetrahydrofuran (PTHF) having a molecular weight in the Mw range of 600 g / mol to 2500 g / mol.

[0043] As well as PTHF, various other polyethers are suitable in accordance with the invention, but polyesters, block copolymers and hybrid polyols such as poly(ester / amides) can also be used.

[0044] The polyols used preferably have an average functionality of 1.8 to 2.3, preferably 1.9 to 2.2, in particular 2. The polyols used according to the invention preferably have only primary hydroxyl groups.

[0045] According to the invention, the polyol can be used in pure form or in the form of a composition comprising said polyol and at least one solvent. Suitable solvents are known per se to those skilled in the art.

[0046] The additional polyol is preferably used in a molar ratio to the polyol (P1) ranging from 10:1 to 1:10. In a further preferred embodiment, the further polyol is used in a molar ratio to the polyol (P1) ranging from 9:1 to 1:9, more preferably in the range from 5:1 to 1:5.

[0047] According to the invention, at least one polyisocyanate is used. According to the invention, it is also possible to use a mixture of two or more polyisocyanates.

[0048] Suitable polyisocyanates in the context of the present invention are diisocyanates, in particular aliphatic or aromatic diisocyanates, more preferably aromatic diisocyanates.

[0049] In a further embodiment, the present invention therefore relates to a thermoplastic polyurethane as described above, wherein the polyisocyanate is an aliphatic or aromatic diisocyanate.

[0050] According to the present invention, the components are converted in such a ratio that the hard segment content in the thermoplastic polyurethane is <75%, preferably <70%, more preferably <50%, more preferably <40%. Therefore, the hard segment content in the thermoplastic polyurethane is preferably in the range of 10% to 75%, preferably in the range of 20% to 70%, more preferably in the range of 20% to 50%, more preferably in the range of 20% to 40%.

[0051] Furthermore, in the context of the present invention, the isocyanate components used may be pre-reacted prepolymers in which some OH components have reacted with isocyanates in a preceding reaction step. These prepolymers react with the remaining OH components in a further step, the actual polymer reaction, which then forms the thermoplastic polyurethane. The use of prepolymers makes it possible to use OH components that have secondary alcohol groups.

[0052] Aliphatic diisocyanates which can be used include conventional aliphatic and / or cycloaliphatic diisocyanates, such as tri-, tetra-, penta-, hexa-, hepta- and / or octamethylene diisocyanate, 2-methylpentamethylene 1,5-diisocyanate, 2-ethyltetramethylene-1,4-diisocyanate, hexamethylene-1,6-diisocyanate (HDI), pentamethylene-1,5-diisocyanate, butylene-1,4-diisocyanate, trimethylhexamethylene-1,6-diisocyanate, tetramethylhexamethylene-1,5-diisocyanate, tetramethylhexamethylene-1,4-diisocyanate, tetramethylhexamethylene-1,6-diisocyanate, tetramethylhexamethylene-1,5-diisocyanate, tetramethylhexamethylene-1,6 ... ,6-diisocyanate, 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (isophorone diisocyanate, IPDI), 1,4- and / or 1,3-bis(isocyanatomethyl)cyclohexane (HXDI), cyclohexane-1,4-diisocyanate, 1-methylcyclohexane 2,4- and / or 2,6-diisocyanate, methylenedicyclohexyl 4,4'-, 2,4'- and / or 2,2'-diisocyanate (H12MDI).

[0053] Preferred aliphatic polyisocyanates are hexamethylene 1,6-diisocyanate (HDI), 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane and methylenedicyclohexyl 4,4'-, 2,4'- and / or 2,2'-diisocyanate (H12MDI). Particularly preferred are methylenedicyclohexyl 4,4'-, 2,4'- and / or 2,2'-diisocyanate (H12MDI) and 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane or mixtures thereof.

[0054] In a further embodiment, the present invention therefore relates to a process as described above, wherein the polyisocyanate is selected from the group consisting of methylene dicyclohexyl 4,4'-, 2,4'- and / or 2,2'-diisocyanate (H12MDI), hexamethylene diisocyanate (HDI) and 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (IPDI) or mixtures thereof. Suitable aromatic diisocyanates are in particular diphenylmethane 2,2'-, 2,4'- and / or 4,4'-diisocyanate (MDI), naphthylene 1,5-diisocyanate (NDI), tolylene 2,4- and / or 2,6-diisocyanate (TDI), 3,3'-dimethyl-4,4'-diisocyanatodiphenyl (TODI), p-phenylene diisocyanate (PDI), diphenylethane 4,4'-diisocyanate (EDI), diphenylmethane diisocyanate, dimethyldiphenyl 3,3'-diisocyanate, diphenylethane 1,2-diisocyanate and / or phenylene diisocyanate.

[0055] Suitable aromatic diisocyanates are diphenylmethane 2,2'-, 2,4'- and / or 4,4'-diisocyanate (MDI) and mixtures thereof.

[0056] Suitable examples of more highly functional isocyanates are triisocyanates, such as triphenylmethane 4,4',4''-triisocyanate, and also the cyanurates of the abovementioned diisocyanates, and oligomers obtained by partial reaction of diisocyanates with water, such as the biurets of the abovementioned diisocyanates, and also oligomers obtained by controlled reaction of semi-blocked diisocyanates with polyols having on average more than two, preferably three or more, hydroxyl groups.

[0057] In a further embodiment, the present invention relates to the above process, wherein the polyisocyanate is an aliphatic diisocyanate.

[0058] According to the present invention, the polyisocyanate can be used in pure form or in the form of a composition comprising the polyisocyanate and at least one solvent. Suitable solvents are known to those skilled in the art. Suitable examples include non-reactive solvents such as ethyl acetate, methyl ethyl ketone, tetrahydrofuran and hydrocarbons.

[0059] According to the present invention, in the reaction of the at least one aliphatic polyisocyanate, the at least one chain extender, and the at least one polymer composition, it is possible to add further raw materials, such as catalysts or auxiliaries and additives.

[0060] Suitable auxiliaries and additives are known per se to those skilled in the art.Specific examples include, for example, surface-active substances, flame retardants, nucleating agents, oxidation stabilizers, antioxidants, lubricants and release aids, dyes and pigments, stabilizers (against hydrolysis, light, heat or discoloration), inorganic and / or organic fillers, reinforcing agents and plasticizers.Suitable auxiliaries and additives are described, for example, in Kunststoffhandbuch [Plastics Handbook], Volume VII, published by Vieweg and Hoechtlen, Carl Hanser Verlag, Munich 1966 (p.103-113).

[0061] Likewise, suitable catalysts are known in principle from the prior art.Suitable catalysts are, for example, organometallic compounds selected from the group consisting of organyls of tin, titanium, zirconium, hafnium, bismuth, zinc, aluminum and iron, such as tin organyl compounds, preferably tin dialkyls, such as tin(II) isooctanoate, tin dioctoate, dimethyltin, diethyltin, or tin organyl compounds of aliphatic carboxylic acids, preferably tin diacetate, tin dilaurate, dibutyltin diacetate, dibutyltin dilaurate, titanate esters, bismuth compounds, such as bismuth alkyl compounds, preferably bismuth neodecanoate or similar, or iron compounds, preferably iron(III) acetylacetonate.

[0062] In a preferred embodiment, the catalyst is selected from tin and bismuth compounds, more preferably tin or bismuth alkyl compounds, with tin(II) isooctanoate and bismuth neodecanoate being particularly suitable.

[0063] The catalyst is typically used in an amount of from 3 ppm to 2000 ppm, preferably from 10 ppm to 1000 ppm, more preferably from 20 ppm to 500 ppm, and most preferably from 30 ppm to 300 ppm.

[0064] In a further aspect, the present invention also provides a method for producing a pharmaceutical composition comprising the steps of: (a) (i) at least one polyisocyanate composition; (ii) at least one chain extender, and (iii) at least one polyol composition producing a thermoplastic polyurethane comprising the composition of Where: The polyol composition comprises at least one polyol (P1) having a molecular weight Mw in the range of 500 to 2000 g / mol and having at least one aromatic polyester block (B1), The hard segment content in the thermoplastic polyurethane is <75%; and (b) A process for producing a molded body (SC) from thermoplastic polyurethane The present invention relates to a method for producing a molded body (SC) comprising the steps of:

[0065] The method according to the present invention includes steps (a) and (b). First, in step (a), a thermoplastic polyurethane is prepared by reacting at least one polyisocyanate composition, at least one chain extender, and at least one polyol composition. According to the present invention, the polyol composition includes at least one polyol (P1) having a molecular weight Mw in the range of 500 to 2000 g / mol and having at least one aromatic polyester block (B1).

[0066] In step (b), a molded body (SC) is produced from the thermoplastic polyurethane obtained in step (a). In the context of the present invention, the molded body (SC) can also be, for example, a foil. In the context of the present invention, the molded body (SC) can be produced by any conventional method, for example by extrusion, injection molding or sintering methods or from a solution. In particular, the production of the molded body (SC) by injection molding is preferred in the context of the present invention.

[0067] In a further embodiment, the present invention therefore relates to a process as described above, wherein the shaped body (SC) is produced in step (b) by extrusion, injection moulding or sintering processes or from solution.

[0068] The process of step (a) can in principle be carried out under reaction conditions known per se.

[0069] In a preferred embodiment, the process of step (a) is carried out at a temperature above room temperature, more preferably in the range of 50°C to 200°C, more preferably in the range of 55°C to 150°C, especially in the range of 60°C to 120°C.

[0070] According to the invention, heating can be performed in any suitable manner known to the skilled artisan, preferably by electrical heating, heating via heated oil, heated polymer fluid or water, induction field, hot air or IR radiation.

[0071] The thermoplastic polyurethane obtained is processed according to the invention to obtain a molded body (SC). The process accordingly comprises steps (a) and (b). According to the invention, the method can comprise further steps, such as a heat treatment.

[0072] The process of the invention allows for the production of shaped bodies (SC) which are transparent, have a high hardness and at the same time are not brittle. In a further aspect, the invention also relates to shaped bodies obtainable or obtained by the process described above.

[0073] In principle, the molded body (SC) can be any molded body of any conceivable shape, such as extrusion products, such as films and other molded bodies.According to the present invention, the molded body can include consumer articles, such as toothbrushes, razors, housings for household goods, displays, computer or telephone parts, plugs, automobile interior parts, footwear parts, such as toe caps for safety shoes, and other consumer articles for use.

[0074] In a further embodiment, the present invention therefore relates to a molding as described above, wherein the molding is a consumer article, for example a consumer article for use as a toothbrush, a razor, a housing for a household item, a display, a computer or telephone part, a plug, an automobile interior part, a footwear part, for example a toe for a safety shoe, etc.

[0075] Further embodiments of the invention are evident from the claims and the examples. It is understood that the features of the subject matter / method / use according to the invention listed above and described below can be used not only in the combinations specified in each case, but also in other combinations without departing from the scope of the invention. For example, combinations of preferred features with particularly preferred features, or combinations of features not further characterized with particularly preferred features, etc. are implicitly included even if this combination is not explicitly mentioned.

[0076] Hereinafter, exemplary embodiments of the present invention will be described, but the present invention is not limited thereto. In particular, the present invention also encompasses embodiments resulting from the reference of dependent relationships and therefore combinations specified below. More specifically, in the following embodiments, when a certain range is described, for example, the expression "a method according to any of embodiments 1 to 4" should be understood as any combination of the embodiments within this range being explicitly disclosed to a person skilled in the art, and the expression should be considered to be synonymous with "a method according to any of embodiments 1, 2, 3, and 4."

[0077] 1. At least components (i) to (iii): (i) a polyisocyanate composition, (ii) at least one chain extender, and (iii) at least one polyol composition A thermoplastic polyurethane obtained or obtained by converting Where: The polyol composition comprises at least one polyol (P1) having a molecular weight Mw in the range of 500 to 2000 g / mol and at least one aromatic polyester block (B1), The hard segment content in the thermoplastic polyurethane is <75%; Thermoplastic polyurethane.

[0078] 2. The thermoplastic polyurethane according to embodiment 1, wherein the polyol (P1) comprises 20% to 70% by weight of aromatic polyester blocks (B1), based on the total polyester polyol (P1).

[0079] 3. The thermoplastic polyurethane according to embodiment 1 or 2, wherein the aromatic polyester block (B1) is a polyester of an aromatic dicarboxylic acid and an aliphatic diol.

[0080] 4. The thermoplastic polyurethane according to any one of embodiments 1 to 3, wherein the aromatic polyester block (B1) is a polyethylene terephthalate block or a polybutylene terephthalate block.

[0081] 5. The thermoplastic polyurethane according to any one of embodiments 1 to 4, wherein the aromatic polyester block (B1) is a polyethylene terephthalate block.

[0082] 6. The thermoplastic polyurethane according to any one of the preceding embodiments, wherein the polyol (P1) has a molecular weight Mw in the range of 750 to 1500 g / mol.

[0083] 7. The thermoplastic polyurethane according to any one of the preceding embodiments, wherein the polyol (P1) is obtained from an aromatic polyester having a molecular weight in the range of 10000 to 14000 g / mol.

[0084] 8. The thermoplastic polyurethane according to any one of the preceding embodiments, wherein the polyol (P1) is obtained by transesterification from an aromatic polyester having a molecular weight in the range of 10000 to 14000 g / mol.

[0085] 9. The thermoplastic polyurethane according to any one of the preceding embodiments, wherein the polyol (P1) is obtained by transesterification from a polyethylene terephthalate having a molecular weight in the range of 10000 to 14000 g / mol.

[0086] 10. Thermoplastic polyurethane according to any one of the preceding embodiments, wherein the chain extender used in (ii) is a diol having a molecular weight Mw<220 g / mol.

[0087] 11. Thermoplastic polyurethane according to any one of the preceding embodiments, wherein the chain extender used in (ii) and the polyol (P1) present in the polyol composition are used in a molar ratio of from 40:1 to 1:10.

[0088] 12. The thermoplastic polyurethane of any one of the preceding claims, wherein the polyol composition comprises an additional polyol selected from the group consisting of polyetherols, polyesterols, polycarbonate alcohols, and hybrid polyols.

[0089] 13. The thermoplastic polyurethane of any one of the preceding embodiments, wherein the polyisocyanate is an aliphatic or aromatic diisocyanate.

[0090] 14. The thermoplastic polyurethane according to any one of the preceding claims, wherein the hard segment content in the thermoplastic polyurethane is in the range of 10% to 75%.

[0091] 15. A method for producing a molded body (SC), comprising the steps of: (a) (i) at least one polyisocyanate composition; (ii) at least one chain extender, and (iii) at least one polyol composition producing a thermoplastic polyurethane comprising the composition of Where: The polyol composition comprises at least one polyol (P1) having a molecular weight Mw in the range of 500 to 2000 g / mol and having at least one aromatic polyester block (B1); The hard segment content in the thermoplastic polyurethane is <75%; (b) A process for producing a molded body (SC) from thermoplastic polyurethane A method comprising:

[0092] 16. The method according to embodiment 15, wherein the compact (SC) is produced in step (b) by extrusion, injection molding or sintering processes or from a solution.

[0093] 17. A shaped body obtainable or obtained by the method according to any one of embodiments 15 and 16.

[0094] 18. The molded article according to embodiment 17, wherein the molded article is a consumer article, such as a toothbrush, a razor, a housing for a household item, a display, a computer or telephone part, a plug, an automobile interior part, a footwear part, such as a toe for a safety shoe, and the like.

[0095] 19. At least components (i) to (iii): (i) a polyisocyanate composition, (ii) at least one chain extender, and (iii) at least one polyol composition A thermoplastic polyurethane obtained or obtained by converting Where: The polyol composition comprises at least one polyol (P1) having a molecular weight Mw in the range of 500 to 2000 g / mol and having at least one aromatic polyester block (B1); The hard segment content in the thermoplastic polyurethane is <75%; The polyol (P1) contains 20% by mass to 70% by mass of an aromatic polyester block (B1) based on the total polyester polyol (P1), Thermoplastic polyurethane, in which the aromatic polyester block (B1) is a polyethylene terephthalate block or a polybutylene terephthalate block.

[0096] 20. At least the following components (i) to (iii): (i) a polyisocyanate composition, (ii) at least one chain extender, and (iii) at least one polyol composition A thermoplastic polyurethane obtained or obtained by converting Where: The polyol composition comprises at least one polyol (P1) having a molecular weight Mw in the range of 500 to 2000 g / mol and having at least one aromatic polyester block (B1); The hard segment content in the thermoplastic polyurethane is in the range of 10% to 75%; A thermoplastic polyurethane, wherein the polyol (P1) contains 20% by mass to 70% by mass of an aromatic polyester block (B1) based on the total polyester polyol (P1), and the aromatic polyester block (B1) is a polyethylene terephthalate block.

[0097] 21. The thermoplastic polyurethane according to any one of embodiments 19 and 20, wherein the polyol (P1) has a molecular weight Mw in the range of 750 to 1500 g / mol.

[0098] 22. The thermoplastic polyurethane according to any one of embodiments 19 to 21, wherein the polyol (P1) is obtained from an aromatic polyester having a molecular weight in the range of 10000 to 14000 g / mol.

[0099] 23. The thermoplastic polyurethane according to any one of embodiments 19 to 22, wherein the polyol (P1) is obtained by transesterification from an aromatic polyester having a molecular weight in the range of 10 000 to 14 000 g / mol.

[0100] 24. Thermoplastic polyurethane according to any one of embodiments 19 to 23, wherein the polyol (P1) is obtained by transesterification from polyethylene terephthalate having a molecular weight in the range of 10000 to 14000 g / mol.

[0101] 25. The thermoplastic polyurethane according to any one of embodiments 19 to 24, wherein the chain extender used in (ii) is a diol having a molecular weight Mw<220 g / mol.

[0102] 26. Thermoplastic polyurethane according to any one of embodiments 19 to 25, wherein the chain extender used in (ii) and the polyol (P1) present in the polyol composition are used in a molar ratio of 40:1 to 1:10.

[0103] 27. The thermoplastic polyurethane of any one of embodiments 19-26, wherein the polyol composition comprises an additional polyol selected from the group consisting of polyetherols, polyesterols, polycarbonate alcohols, and hybrid polyols.

[0104] 28. The thermoplastic polyurethane of any one of embodiments 19-27, wherein the polyisocyanate is an aliphatic or aromatic diisocyanate.

[0105] 29. The thermoplastic polyurethane of any one of embodiments 19-28, wherein the polyisocyanate is an aromatic diisocyanate.

[0106] 30. A method for producing a molded body (SC), comprising the steps of: (a) (i) at least one polyisocyanate composition; (ii) at least one chain extender, and (iii) at least one polyol composition producing a thermoplastic polyurethane comprising the composition of Where: The polyol composition comprises at least one polyol (P1) having a molecular weight Mw in the range of 500 to 2000 g / mol and having at least one aromatic polyester block (B1); The hard segment content in the thermoplastic polyurethane is in the range of 10% to 75%; The polyol (P1) contains 20% by mass to 70% by mass of an aromatic polyester block (B1) based on the total polyester polyol (P1), and the aromatic polyester block (B1) is a polyethylene terephthalate block or a polyethylene terephthalate block; (b) A process for producing a molded body (SC) from thermoplastic polyurethane A method comprising:

[0107] 31. The method according to embodiment 30, wherein the aromatic polyester block (B1) is a polyethylene terephthalate block.

[0108] 32. The method according to any one of embodiments 30 and 31, wherein the polyol (P1) has a molecular weight Mw in the range of 1700 to 2300 g / mol.

[0109] 33. The method according to any one of embodiments 30 to 32, wherein the chain extender used in (ii) is a diol having a molecular weight Mw<220 g / mol.

[0110] 34. The method according to any one of embodiments 30 to 33, wherein the chain extender used in (ii) and the polyol (P1) present in the polyol composition are used in a molar ratio of from 40:1 to 1:10.

[0111] 35. The method according to any one of embodiments 30 to 34, wherein the molded body (SC) is produced in step (b) by extrusion, injection molding or sintering processes or from a solution.

[0112] 36. A molded article obtained or obtained by the method according to any one of embodiments 30 to 35.

[0113] 37. The molded article according to embodiment 36, wherein the molded article is a consumer article, such as a toothbrush, a razor, a housing for a household item, a display, a computer or telephone part, a plug, an automobile interior part, a footwear part, such as a toe for a safety shoe, and the like.

[0114] The following examples are intended to illustrate the invention and are not intended to limit the subject matter in any way. EXAMPLES

[0115] The following raw materials were used:

[0116] Polyol 1: polyester polyol based on adipic acid, PET, butane-1,4-diol and diethylene glycol, OH number 111.2, functionality: 2 Polyol 2: polyester polyol based on adipic acid, PET, butane-1,4-diol and diethylene glycol, OH number 112.8, functionality: 2 Polyol 3: polyester polyol based on adipic acid, PET, butane-1,4-diol and propane-1,3-diol, OH number 112.1, functionality: 2 Polyol 4: polyester polyol based on adipic acid, succinic acid, glutaric acid, PET and diethylene glycol, OH number 75.6, functionality: 2 Polyol 5: polyester polyol based on adipic acid, succinic acid, glutaric acid, PET and diethylene glycol, OH number 110.6, functionality: 2 PET: polyethylene terephthalate in flake form, average molecular weight Mw 12000g / mol Isocyanate 1: Aromatic isocyanate (methylenediphenyl 4,4'-diisocyanate) Isocyanate 2: Aliphatic isocyanate (methylenedicyclohexyl 4,4'-diisocyanate) CE1: Butane-1,4-diol CE2: Hexane-1,6-diol Stabilizer 1: Polycarbodiimide-based hydrolysis stabilizer Catalyst 1: 50% tin(II) isooctanoate in diethylhexyl adipate

[0117] 2. Synthesis of polyester polyol containing PET blocks 2.1 Synthesis of polyol 1 A 4000 ml round bottom flask equipped with a PT100 thermocouple, nitrogen inlet, stirrer, column, column head, Anschutz-Thiele fittings and a heating mantle is initially charged with 880.84 g of adipic acid, 395.56 g of butane-1,4-diol and 465.79 g of diethylene glycol. This mixture is then heated to 120° C. until a homogeneous mixture is formed. 1000 g of polyethylene terephthalate (PET) is then added to the mixture in the form of PET flakes, followed by 10 ppm=2.5 g of TTB (tetra-n-butyl orthotitanate, 1% in toluene). The reaction mixture is first heated to 180° C. for about 1.5 hours and then further heated to 240° C., continuously removing the reaction water that is formed. Over the entire synthesis, the PET flakes are gradually decomposed and a clear mixture is formed. This is condensed until a product having an acid number <1.0 mg KOH / g is obtained.

[0118] The polymer obtained has the following characteristics:

[0119] Hydroxyl number: 111.2mgKOH / g Acid value: 0.45mgKOH / g Viscosity at 75℃: 757mPas

[0120] 2.2 Synthesis of polyol 2 A 4000 ml round bottom flask equipped with a PT100 thermocouple, nitrogen inlet, stirrer, column, column head, Anschutz-Thiele fittings and a heating mantle is initially charged with 705.39 g of adipic acid, 339.84 g of butane-1,4-diol and 400.18 g of diethylene glycol. This mixture is then heated to 120° C. until a homogeneous mixture is formed. 1250 g of polyethylene terephthalate (PET) is then added to the mixture in the form of PET flakes, followed by 10 ppm=2.5 g of TTB (tetra-n-butyl orthotitanate, 1% in toluene). The reaction mixture is first heated to 180° C. for about 1.5 hours and then further heated to 240° C., continuously removing the reaction water that is formed. Over the entire synthesis, the PET flakes are gradually decomposed and a clear mixture is formed. This is condensed until a product having an acid number <1.0 mg KOH / g is obtained.

[0121] The polymer obtained has the following characteristics:

[0122] Hydroxyl number: 112.8mgKOH / g Acid value: 0.55mgKOH / g Viscosity at 75℃: 1388mPas

[0123] 2.3 Synthesis of polyol 3 A 4000 ml round bottom flask equipped with a PT100 thermocouple, nitrogen inlet, stirrer, column, column head, Anschutz-Thiele fittings and a heating mantle is initially charged with 788.52 g of adipic acid, 309.27 g of propane-1,3-diol and 366.24 g of butane-1,4-diol. This mixture is then heated to 120° C. until a homogeneous mixture is formed. 1250 g of polyethylene terephthalate (PET) is then added to the mixture in the form of PET flakes, followed by 10 ppm=2.5 g of TTB (tetra-n-butyl orthotitanate, 1% in toluene). The reaction mixture is first heated to 180° C. for about 1.5 hours and then further heated to 240° C., continuously removing the reaction water that is formed. Over the entire synthesis, the PET flakes are gradually decomposed and a clear mixture is formed. This is condensed until a product having an acid number <1.0 mg KOH / g is obtained.

[0124] The polymer obtained has the following characteristics:

[0125] Hydroxyl number: 112.1mgKOH / g Acid value: 0.38mgKOH / g Viscosity at 75℃: 1803mPas

[0126] 2.4 Synthesis of polyol 4 A 3000 ml round bottom flask equipped with a thermometer, nitrogen inlet, stirrer and heating mantle is initially charged with 819.5 g of a dicarboxylic acid mixture (consisting of adipic acid, glutaric acid and succinic acid) and 925.9 g of diethylene glycol. This mixture is then heated to 120° C. until a homogeneous mixture is formed. 1000 g of polyethylene terephthalate (PET) in the form of PET flakes is then added to the mixture. The reaction mixture is further heated at 240° C. and the reaction water formed is continuously removed. Over the entire synthesis, the PET flakes are gradually decomposed and a transparent mixture is formed. This is condensed until a product having an acid value of <1.0 mg KOH / g is obtained.

[0127] The polymer obtained has the following characteristics:

[0128] Acid value: 110.6mgKOH / g Hydroxyl value: 0.6mgKOH / g Viscosity at 75℃: 660mPas

[0129] 2.5 Synthesis of polyol 5 A 3000 ml round bottom flask equipped with a thermometer, nitrogen inlet, stirrer and heating mantle is initially charged with 1040.9 g of a dicarboxylic acid mixture (consisting of adipic acid, glutaric acid and succinic acid) and 1016.2 g of diethylene glycol. This mixture is then heated to 120° C. until a homogeneous mixture is formed. 750 g of polyethylene terephthalate (PET) in the form of PET flakes is then added to the mixture. The reaction mixture is further heated at 240° C. and the reaction water formed is continuously removed. Over the entire synthesis, the PET flakes are gradually decomposed and a transparent mixture is formed. This is condensed until a product having an acid value of <1.0 mg KOH / g is obtained.

[0130] The polymer obtained has the following characteristics:

[0131] Acid value: 75.6mgKOH / g Hydroxyl value: 0.7mgKOH / g Viscosity at 75℃: 840mPas

[0132] 3. Method 3.1 Determination of viscosity: Unless otherwise stated, the viscosity of the polyols was measured at 75° C. using a Rheotec RC 20 rotational viscometer using a CC 25 DIN spindle (spindle diameter: 12.5 mm; measuring cylinder inner diameter: 13.56 mm) according to DIN EN ISO 3219 (edition 01.10.1994) at a shear rate of 50 (1 / s).

[0133] 3.2 Hydroxyl number determination: Hydroxyl number is determined by the phthalic anhydride method DIN 53240 (edition 01.12.1971) and reported in mg KOH / g.

[0134] 3.3 Determination of Acid Number: The acid number is determined according to DIN EN 1241 (edition 01.05.1998) and is reported in mg KOH / g.

[0135] 4.General manufacturing example The polyol was first placed in a vessel at 60-80°C and mixed with the ingredients listed in Table 1 under vigorous stirring. The reaction mixture was heated to above 80°C and then poured onto a heated Teflon coated table. The resulting cast slab was heat treated at 80°C for 15 hours and then pelletized and processed by injection molding.

[0136] [Table 1]

[0137] 5. Mechanical properties The measurements summarized in Table 2 were established from the injection molded sheets of Examples 1-5.

[0138] For the resulting polyurethane, the following properties were determined by the methods listed below.

[0139] Hardness: DIN ISO 7619-1 Tensile strength and elongation at break: DIN 53504 Tear propagation resistance: DIN ISO 34-1, B(b) Elastic modulus: DIN EN ISO 527 Abrasion measurements: DIN ISO 4649

[0140] [Table 2]

[0141] In the presence of PET polyol, it is possible to reduce the hard segment content (isocyanate and chain extender) and nevertheless achieve high values ​​of >75 Shore D and elongation at break of >300% at the same time. The materials obtained according to examples 1 to 5 are all transparent. The examples demonstrate that particularly good properties can be achieved with a PET content in the range of 40% to 50% and an average molecular weight Mw of the polyol of about 1000 g / mol.

[0142] References US5574092 US5627254 WO2015 / 063062 A1 WO2007 / 118827 A1 Kunststoffhandbuch, Volume 7, “Polyurethane”, Carl Hanser Verlag, 3rd edition, 1993, Chapter 3.1 Kunststoffhandbuch, Volume 7, Carl Hanser Verlag, 1st edition, 1966, pp. 103-113

Claims

1. At least the following components (i) to (iii): (i) a polyisocyanate composition, (ii) at least one chain extender, and (iii) at least one polyol composition A thermoplastic polyurethane obtained or obtained by converting The polyol composition comprises at least one polyol (P1) having a molecular weight Mw in the range of 500 to 2000 g / mol and having at least one aromatic polyester block (B1), The hard segment content in the thermoplastic polyurethane is <75%. A thermoplastic polyurethane characterized by:

2. 2. The thermoplastic polyurethane of claim 1, wherein the polyol (P1) comprises from 20% to 70% by weight of aromatic polyester blocks (B1), based on the total polyester polyol (P1).

3. 3. The thermoplastic polyurethane according to claim 1, wherein the aromatic polyester block (B1) is a polyester of an aromatic dicarboxylic acid and an aliphatic diol.

4. The thermoplastic polyurethane according to any one of claims 1 to 3, wherein the aromatic polyester block (B1) is a polyethylene terephthalate block or a polybutylene terephthalate block.

5. The thermoplastic polyurethane according to any one of claims 1 to 4, wherein the aromatic polyester block (B1) is a polyethylene terephthalate block.

6. The thermoplastic polyurethane according to any one of the preceding claims, wherein the polyol (P1) has a molecular weight Mw in the range from 750 to 1500 g / mol.

7. A thermoplastic polyurethane according to any one of claims 1 to 6, wherein the chain extender used in (ii) is a diol having a molecular weight Mw<220 g / mol.

8. 8. Thermoplastic polyurethane according to claim 1 , wherein the chain extender used in (ii) and the polyol (P1) present in the polyol composition are used in a molar ratio of from 40:1 to 1:

10.

9. 9. The thermoplastic polyurethane of any one of claims 1 to 8, wherein the polyol composition comprises a further polyol selected from the group consisting of polyetherols, polyesterols, polycarbonate alcohols and hybrid polyols.

10. The thermoplastic polyurethane of any one of claims 1 to 9, wherein the polyisocyanate is an aliphatic or aromatic diisocyanate.

11. The thermoplastic polyurethane according to any one of claims 1 to 10, wherein the hard segment content in the thermoplastic polyurethane is in the range of 10% to 75%.

12. A method for producing a molded body (SC), comprising the steps of: (a) (i) at least one polyisocyanate composition; (ii) at least one chain extender, and (iii) at least one polyol composition 1. A process for producing a thermoplastic polyurethane comprising the composition of The polyol composition comprises at least one polyol (P1) having a molecular weight Mw in the range of 500 to 2000 g / mol and having at least one aromatic polyester block (B1), The hard segment content in the thermoplastic polyurethane is <75%; (b) A step of producing a molded body (SC) from thermoplastic polyurethane The method according to claim 1, further comprising:

13. 13. The method according to claim 12, wherein the shaped body (SC) is produced in step (b) by extrusion, injection moulding or sintering processes or from solution.

14. A moulded body obtainable or obtained by the method according to any one of claims 12 and 13.

15. The molded article according to claim 14, wherein the molded article is a consumer article, for example, a consumer article for applications such as toothbrushes, razors, housings for household appliances, displays, computer or telephone parts, plugs, automotive interior parts, footwear parts, such as toes for safety shoes.

Citation Information

Patent Citations

  • Viscoelastic resin for damping material

    JP1988048321A

  • Polyurethane resin

    JP1997040738A

  • Thermoplastic polyurethanes containing units derived from an aromatic diol

    US5574092A

  • Rigid thermoplastic polyurethane comprising units of butane diol and a polyethylene glycol

    US5627254A

  • Methods for producing transparent, thermoplastic polyurethane having high mechanical strength and hardness

    WO2015063062A1