Image forming method and image forming system
By adjusting the silicon content and glass transition point of the aluminum substrate and toner in image forming systems, both low-temperature fixability and transferability are achieved, addressing the challenges faced by existing electrophotographic technologies.
Patent Information
- Application Number
- JP2023067717
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-18
- Publication Date
- 2024-10-30
AI Technical Summary
Existing image forming apparatuses using electrophotography face challenges in achieving both low-temperature fixability and transferability, as low-temperature fixing often deteriorates transferability.
Adjusting the silicon content of the aluminum substrate in the photoreceptor and the glass transition point of the electrostatic image developing toner to specific ranges, using a photoreceptor with an aluminum base, a toner containing a binder resin, and a developer carrier with a magnetic flux member, where the silicon content exceeds 0.6% by mass and the glass transition point is between 0 to 45°C.
This approach enables both low-temperature fixability and transferability by enhancing the resistance value of the metal part and reducing heat generation, while improving transferability through surface protrusions on the aluminum substrate, thereby maintaining image quality and efficiency.
Smart Images

Figure 2024154094000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an image forming method and an image forming system, and more particularly to an image forming method and an image forming system that can achieve both low-temperature fixability and transferability. [Background technology]
[0002] With the improvement of the performance of electrophotographic image forming apparatuses, it has become possible to obtain images of relatively high quality. As a result, electrophotographic image forming apparatuses have come to be widely used in fields such as light printing, where a relatively small number of prints are obtained. As a result, an even higher level of image quality is required for electrophotographic image forming apparatuses. In addition, electrophotographic image forming apparatuses are now being used for applications that were rare in the past. For example, electrophotographic image forming apparatuses are used for printing on coated paper, printing high coverage images, printing extremely high definition images or images with subtle tones, and large amounts of the same image are continuously printed. On the other hand, from the viewpoint of reducing the environmental load, low temperature fixing has been studied for reducing power consumption. For example, Patent Document 1 discloses that the molecular weight corresponding to the main peak top of the molecular weight distribution curve of the toner constituent components and the area ratio of the peak of the low molecular weight component amorphous material in the molecular weight distribution curve are controlled within a certain range. However, since the transferability deteriorates as the low-temperature fixing is promoted, it has become clear that it is difficult to achieve both low-temperature fixing and transferability at the same time. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2022-189247 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present invention has been made in consideration of the above problems and circumstances, and an object of the present invention is to provide an image forming method and an image forming system that can achieve both low-temperature fixability and transferability. [Means for solving the problem]
[0005] In order to solve the above problems, the present inventors have investigated the causes of the above problems, and have found that it is possible to achieve both low-temperature fixability and transferability by setting the silicon content of the aluminum substrate used in the photoreceptor and the glass transition point of the toner for developing electrostatic images within specific ranges. That is, the above-mentioned problems of the present invention are solved by the following means.
[0006] 1. An image forming method using a photoconductor using at least an aluminum substrate, a toner for developing an electrostatic image, the toner including toner particles containing at least a binder resin, and a developer carrier having a member for generating magnetic flux therein, The aluminum substrate contains silicon, The silicon content of the aluminum substrate is greater than 0.6% by mass; and The glass transition point (Tg) of the toner for developing electrostatic images is within a range of 0 to 45° C. 1. An image forming method comprising:
[0007] 2. The main component of the binder resin contained in the toner particles is polyester. 2. The image forming method according to claim 1,
[0008] 3. The silicon content of the aluminum substrate is more than 0.6% by mass and 20% by mass or less. 3. The image forming method according to claim 1 or 2,
[0009] 4. A photoconductor using at least an aluminum substrate; a means for developing the latent image formed on the photoreceptor with a toner for developing an electrostatic image; A means for transferring the toner image on the photoreceptor to a transfer medium; and an image forming system including the toner for developing an electrostatic image, The aluminum substrate contains silicon, The silicon content of the aluminum substrate is greater than 0.6% by mass; and The glass transition point (Tg) of the toner for developing electrostatic images is within a range of 0 to 45° C. 1. An image forming system comprising: Effect of the Invention
[0010] According to the above-mentioned means of the present invention, it is possible to provide an image forming method and an image forming system which are capable of achieving both low-temperature fixing property and transferability. Although the mechanism by which the effects of the present invention are manifested or the mechanism by which the effects of the present invention are acted upon has not been clearly understood, it is speculated as follows. Photoconductor element tubes are often made of JIS 3003 and 6063 type expanded aluminum materials. These are multi-element alloys that contain silicon (Si), but the Si content of the 3003 type is 0.6 mass% or less, while the Si content of the 6063 type is in the range of 0.4 to 0.8 mass%. Therefore, by making the Si content in the aluminum substrate exceed 0.6% by mass as in the present invention, Si crystals are precipitated, increasing the resistance of the metal part and suppressing heat generation, which allows the use of a toner with a lower glass transition point, enabling low-temperature fixing while maintaining transferability. Furthermore, in the case of an aluminum substrate containing silicon, protrusions are formed on the surface of the aluminum substrate due to crystal growth, unlike non-magnetic non-metallic substances, such as synthetic resins, rubbers, and ceramics. By forming the protrusions on the surface of the aluminum substrate, it is possible to impart an appropriate roughness to the surface of the photoreceptor, which in turn reduces the number of contact points between the toner and the photoreceptor, thereby improving transferability. As shown in Figure 1, the Al-Si alloy is a eutectic system with a eutectic point at 577°C with a Si content of 12.6%, and when the alloy is cooled in a liquid state (L), it undergoes eutectic solidification. The Si crystals that crystallize out as a eutectic do not form a solid solution with Al, and form protrusions due to crystal growth on the surface of the aluminum substrate.
[0011] For the above reasons, even if the glass transition point of the toner for developing electrostatic images is a low temperature of 0 to 45° C., the transferability is not deteriorated and both low-temperature fixability and transferability can be achieved by incorporating more than 0.6% by mass of silicon into the aluminum substrate of the photoreceptor. If the glass transition point is less than 0° C., the transferability deteriorates, and if the glass transition point is more than 45° C., the fixability deteriorates. [Brief description of the drawings]
[0012] [Figure 1] Phase diagram of the Al-Si system [Diagram 2] FIG. 1 is a diagram showing an example of a layer structure of a photoreceptor; [Diagram 3] Cross-sectional view of the developing roller viewed from the axial direction and perpendicular direction [Figure 4] Cross-sectional view of the developing roller in Figure 3 as seen from the axial direction [Diagram 5] Schematic diagram of hot air surface treatment device [Figure 6] FIG. 1 is a schematic diagram showing an example of an image forming apparatus according to the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The image forming method of the present invention is an image forming method using a photoreceptor using at least an aluminum substrate, a toner for developing electrostatic images, which includes toner particles containing at least a binder resin, and a developer carrier having a member for generating magnetic flux therein, characterized in that the aluminum substrate contains silicon, the silicon content of the aluminum substrate is more than 0.6 mass %, and the glass transition point (Tg) of the toner for developing electrostatic images is within the range of 0 to 45°C. This feature is a technical feature common to or corresponding to each of the following embodiments.
[0014] In an embodiment of the present invention, it is preferable that the main component of the binder resin contained in the toner particles is polyester, since it is easy to obtain a balance between low-temperature fixability and heat resistance. From the viewpoint of adhesion, polyester is a dehydration condensation reaction system, and is particularly compatible with paper. It also has a high internal cohesive force, so it has high folding fixability after fixing is complete. This allows for even lower temperature fixing. On the other hand, as mentioned above, by incorporating silicon into the aluminum substrate, protrusions are formed, which are advantageous for transfer in terms of adhesion to the toner. However, since the protrusions cause minute leaks, the toner particles can be polarized during transfer by incorporating a resin with high polarity such as polyester into the toner particles. As a result, minute leaks can be suppressed, and further improvement in transferability can be expected.
[0015] The silicon content of the aluminum substrate is preferably more than 0.6% by mass and not more than 20% by mass, in terms of improving transferability.
[0016] The image forming system of the present invention is an image forming system including at least a photoreceptor using an aluminum substrate, a means for developing a latent image formed on the photoreceptor with a toner for developing an electrostatic image, a means for transferring the toner image on the photoreceptor to a transfer recipient, and the toner for developing an electrostatic image, wherein the aluminum substrate contains silicon, the silicon content of the aluminum substrate is more than 0.6% by mass, and the glass transition point (Tg) of the toner for developing an electrostatic image is within the range of 0 to 45°C. This makes it possible to provide an image forming system that is capable of achieving both low-temperature fixing performance and transferability.
[0017] The present invention, its components, and embodiments and aspects for carrying out the present invention will be described below. In this application, the symbol "to" is used to mean that the numerical values before and after the symbol "to" are included as lower and upper limits.
[0018] [Outline of the image forming method of the present invention] The image forming method of the present invention is an image forming method using a photoreceptor using an aluminum substrate containing at least silicon, an electrostatic image developing toner including toner particles containing at least a binder resin, and a developer carrier having a member generating magnetic flux therein, characterized in that the silicon content of the aluminum substrate is more than 0.6 mass % and the glass transition point (Tg) of the electrostatic image developing toner is within the range of 0 to 45°C.
[0019] In the following description, the "electrophotographic photoreceptor" may also be simply referred to as the "photoreceptor." In addition, the “toner for developing electrostatic images” is also simply referred to as “toner.” The toner includes toner particles having toner base particles and an external additive disposed on the surface of the toner base particles. In this specification, "toner base particles" are those that constitute the base of "toner particles." The "toner base particles" according to the present invention contain at least a binder resin, and may contain other components such as a colorant, a release agent (wax), and a charge control agent, as necessary. The "toner base particles" are called "toner particles" when an external additive is added. And, "toner" refers to an aggregate of toner particles. Moreover, the term "developer carrier" refers to a developing roller.
[0020] <Silicon content of aluminum substrate> The aluminum substrate according to the present invention is a support for an electrophotographic photoreceptor, the main component of which is an aluminum alloy. The term "aluminum-based alloy" refers to an alloy in which the aluminum (Al) content is 50 mass % or more based on the total alloy. "Containing an aluminum-based alloy as a main component" means that the content of the aluminum-based alloy is 95 mass % or more based on the entire aluminum base.
[0021] Furthermore, the aluminum substrate according to the present invention contains silicon (Si). The silicon content is more than 0.6 mass% relative to the total mass of the entire aluminum substrate, and is preferably more than 0.6 mass% and not more than 20 mass%, more preferably in the range of 0.8 to 12.6 mass%, and even more preferably in the range of 1.0 to 5.0 mass%. When the silicon content in the aluminum substrate is 0.6% by mass or less, the resistance is low and there are few protrusions derived from silicon crystals, so that image defects are hardly generated. However, the number of protrusions is too small, so that the effect of excellent transferability due to the protrusions cannot be obtained. On the other hand, when the silicon content is 12.6% by mass or less, it is a eutectic system with a eutectic point at 12.6%, so that coarse crystals are not mixed in, and it is preferable from the viewpoint of preventing the occurrence of image defects.
[0022] The aluminum substrate may contain Fe, Cu, Mn, Mg, Ti, and the like in addition to Al and Si. It is preferable that Fe is 0.7 mass % or less, Cu is in the range of 0.05 to 0.2 mass %, Mn is 0.9 mass % or less, and Ti, Zn and Cr are 0.1 mass % or less, based on the total mass of the entire aluminum base.
[0023] <Toner glass transition temperature> The "glass transition point" is defined as the temperature at which the free volume of the molecules increases and micro-Brownian motion begins as the temperature of the resin components that make up the toner changes from low to high. The glass transition point (Tg) is also called the glass transition temperature.
[0024] In order to improve the low-temperature fixing ability of a toner, it is necessary to design it so that the glass transition point, which allows molecular motion at a lower temperature, is lower. It is also preferable to devise further measures to improve heat-resistant storage properties and suppress fusion of toner particles. For example, it is preferable to change the composition between the surface and the inside of the toner, to form a core-shell toner composition using a resin with a low glass transition point in the core and a resin with a high glass transition point in the shell. It is also preferable to harden only the surface by using a means for fixing inorganic fine particles as an external additive to the portion corresponding to the shell, thereby ensuring heat-resistant storage properties and resistance to fusion and aggregation.
[0025] The glass transition point of the toner according to the present invention is within a range of 0 to 45° C. The glass transition point is preferably within a range of 10 to 30° C. If the glass transition point is lower than 0° C., the toner becomes too soft, causing image defects, whereas if it is higher than 45° C., the low-temperature fixability of the toner deteriorates. The core resin constituting the toner according to the present invention must be designed to have a lower glass transition point, while the shell resin must be designed to have a higher glass transition point.
[0026] (Control Method) The glass transition point of the resin is controlled by changing the type of resin constituting the binder resin, the molecular weight of the resin, or, when a plurality of types of resins are used, the component ratio of each resin. Specifically, it is preferable to use a combination of an amorphous polyester and a crystalline polyester as the binder resin. When used in combination, it is preferable to contain the amorphous polyester in the range of 65 to 95 mass % and the crystalline polyester in the range of 5 to 35 mass % relative to the binder resin. Alternatively, only a styrene-(meth)acrylic copolymer resin may be used as the binder resin.
[0027] (Measurement method) The glass transition point can be determined from a differential scanning calorimetry (DSC) curve obtained by DSC. More specifically, it can be determined from the "extrapolated glass transition onset temperature" described in the method for determining the glass transition point in JIS K-7121-1987 "Method for measuring transition temperature of plastics." This measurement is carried out as follows. First, the substance to be measured is placed in a Shimadzu Corporation differential scanning calorimeter (apparatus name: DSC-50 type) equipped with an automatic tangent processing system, and liquid nitrogen is placed as the cooling medium. Next, the material is heated from 0°C to 150°C at a heating rate of 10°C / min (first heating process) to obtain the relationship between temperature (°C) and heat (mW). Next, the material is cooled to 0°C at a cooling rate of -10°C / min, and then heated again to 150°C at a heating rate of 10°C / min (second heating process) to collect data. The material was held at 0°C and 150°C for 10 minutes each. The melting temperature of the mixture of indium and zinc was used to correct the temperature of the detector of the measuring device, and the heat of melting of indium was used to correct the amount of heat. The sample was placed in an aluminum pan, and an empty aluminum pan for control was set. The glass transition point was determined as the temperature at the intersection of the baseline and the extended line of the rising edge in the endothermic part of the DSC curve obtained during the second heating process.
[0028] The photoconductor, developing roller and toner used in the image forming method of the present invention will be described below, and then the image forming system of the present invention will be described.
[0029] 1.Photoreceptor [Photoreceptor layer structure] The photoreceptor used in the image forming method of the present invention has a structure in which a photosensitive layer is laminated on a support, and the photoreceptor preferably has an intermediate layer between the support and the photosensitive layer.
[0030] The photosensitive layer may have a single layer structure containing a charge generating compound and a charge transporting compound, or may have a laminate structure of a charge generating layer containing a charge generating compound and a charge transporting layer containing a charge transporting compound. Furthermore, the photoreceptor according to the present invention preferably has a surface protective layer on the photosensitive layer. The layer structure of the photoreceptor can be, for example, as shown in the following (1) to (4).
[0031] (1) Support / Intermediate layer / Charge generating layer / Charge transport layer (2) Support / intermediate layer / single-layer photosensitive layer (3) Support / Intermediate layer / Charge generating layer / Charge transport layer / Surface protective layer (4) Support / intermediate layer / single-layer photosensitive layer / surface protective layer
[0032] Fig. 2 is a diagram showing an example of the layer structure of a photoreceptor. In the photoreceptor 1 shown in Fig. 2, an intermediate layer 102, a charge generating layer 103, a charge transport layer 104, and a surface protective layer 105 are laminated in this order on a support 101.
[0033] <Support> The support is the aluminum substrate according to the present invention as described above. Hereinafter, the aluminum substrate will also be simply referred to as the "support." The aluminum substrate contains Si. As described above, the Si content is more than 0.6 mass % relative to the total mass of the aluminum substrate.
[0034] The aluminum substrate is preferably a cylindrical substrate having a surface made of at least one of aluminum and an aluminum alloy. The surface of the aluminum substrate may be subjected to a hot water treatment, a blasting treatment, a cutting treatment, etc. The cross section of the cylindrical aluminum substrate does not include a cross section having two or more spaces.
[0035] The aluminum substrate is generally manufactured by hot extrusion and cold drawing, followed by cutting to a predetermined length and precision machining of the surface. The aluminum substrate preferably has a thickness within a range of 0.5 to 5.0 mm.
[0036] <Middle Class> The photoreceptor according to the present invention preferably has an intermediate layer between the support (aluminum substrate) and the photosensitive layer, which can provide the photoreceptor with a function of preventing charge leak spots that may occur due to crystals derived from alloy components.
[0037] The intermediate layer is, for example, a layer containing a binder resin (hereinafter, also referred to as "binder resin for intermediate layer") and, if necessary, conductive particles and metal oxide particles. Examples of binder resins for the intermediate layer include casein, polyvinyl alcohol, nitrocellulose, ethylene-acrylic acid copolymers, polyamide resins, polyurethane resins, gelatin, etc. Among these, alcohol-soluble polyamide resins are preferred.
[0038] The intermediate layer may contain various conductive particles or metal oxide particles for the purpose of adjusting the resistance.
[0039] Examples of the metal oxide particles that can be used include various metal oxide particles such as alumina, zinc oxide, titanium oxide, tin oxide, antimony oxide, indium oxide, bismuth oxide, zirconium oxide, etc. Composite metal oxide particles such as tin-doped indium oxide and antimony-doped tin oxide may also be used.
[0040] The number average primary particle size of the metal oxide particles is preferably from 10 to 300 nm, and more preferably from 20 to 100 nm.
[0041] The conductive particles or metal oxide particles may be used alone or in combination of two or more kinds. When two or more kinds are mixed, they may be in the form of a solid solution or fusion.
[0042] The content of the conductive particles or metal oxide particles is preferably within a range of 20 to 400 parts by mass, and more preferably within a range of 50 to 350 parts by mass, relative to 100 parts by mass of the binder resin.
[0043] The thickness of the intermediate layer is preferably within the range of 0.1 to 15 μm, and more preferably within the range of 0.3 to 10 μm.
[0044] <Photosensitive layer> The photosensitive layer may have a single layer structure containing a charge generating compound and a charge transporting compound, or may have a laminate structure of a charge generating layer containing a charge generating compound and a charge transporting layer containing a charge transporting compound.
[0045] (Charge generation layer) The charge generating layer is a layer containing a charge generating compound and a binder resin (hereinafter also referred to as "binder resin for charge generating layer").
[0046] "Charge-generating compound" refers to a compound that generates charge carriers, i.e., electrons or holes. Examples of the charge-generating compound include azo pigments such as Sudan Red and Diane Blue, quinone pigments such as pyrenequinone and anthanthrone, quinocyanine pigments, perylene pigments, indigo pigments such as indigo and thioindigo, polycyclic quinone pigments such as pyranthrone and diphthaloylpyrene, and phthalocyanine pigments, but are not limited thereto. Among these, polycyclic quinone pigments, titanyl phthalocyanine pigments, and gallium phthalocyanine are preferred. These charge-generating compounds may be used alone or in combination of two or more.
[0047] A known resin can be used as the charge generating layer binder resin. Examples of the known resin include polystyrene resin, polyethylene resin, polypropylene resin, acrylic resin, methacrylic resin, vinyl chloride resin, vinyl acetate resin, polyvinyl butyral resin, epoxy resin, polyurethane resin, phenol resin, polyester, alkyd resin, polycarbonate resin, silicone resin, melamine resin, and copolymer resins containing two or more of these resins (for example, vinyl chloride-vinyl acetate copolymer resin, vinyl chloride-vinyl acetate-maleic anhydride copolymer resin), poly-vinyl carbazole resin, etc., but are not limited thereto. Among these, polyvinyl butyral resin is preferred.
[0048] The content of the charge generating compound in the charge generating layer is preferably within a range of 1 to 600 parts by mass, more preferably within a range of 50 to 500 parts by mass, based on 100 parts by mass of the binder resin for the charge generating layer.
[0049] The thickness of the charge generating layer varies depending on the characteristics of the charge generating compound, the characteristics and content of the binder resin for the charge generating layer, etc., but is preferably within the range of 0.01 to 5 μm, and more preferably within the range of 0.05 to 3 μm.
[0050] (charge transport layer) The charge transport layer is a layer containing a charge transporting compound and a binder resin (hereinafter also referred to as "binder resin for charge transport layer").
[0051] The term "charge transporting compound" refers to a compound that exhibits the transport of charge carriers, i.e., electrons or holes. As the charge transporting compound, known charge transporting compounds can be used. As known charge transporting compounds, for example, carbazole derivatives, oxazole derivatives, oxadiazole derivatives, thiazole derivatives, thiadiazole derivatives, triazole derivatives, imidazole derivatives, imidazolone derivatives, imidazolidine derivatives, bisimidazolidine derivatives, styryl compounds, hydrazone compounds, pyrazoline compounds, oxazolone derivatives, benzimidazole derivatives, quinazoline derivatives, benzofuran derivatives, acridine derivatives, phenazine derivatives, aminostilbene derivatives, triarylamine derivatives, phenylenediamine derivatives, stilbene derivatives, benzidine derivatives, poly-N-vinylcarbazole, poly-1-vinylpyrene, poly-9-vinylanthracene, and triphenylamine derivatives can be mentioned. These may be used in combination of two or more kinds.
[0052] Preferred examples of the charge transporting compound used in a photoreceptor for short wave exposure such as a short wave laser are given below.
[0053] [ka]
[0054] Preferred examples of the charge transporting compound used in the photoreceptor for long wave exposure using a long wave laser or the like are given below.
[0055] [ka]
[0056] [ka]
[0057] As the charge transporting compound contained in the charge transport layer, the following compounds can also be suitably used.
[0058] [ka]
[0059] The charge transporting compound can be synthesized by a known synthesis method, for example, the synthesis methods described in JP-A-2010-26428 and JP-A-2010-91707.
[0060] The binder resin for the charge transport layer may be a known resin, such as polycarbonate resin, polyacrylate resin, polyester, polystyrene resin, styrene-acrylonitrile copolymer resin, polymethacrylic acid ester resin, and styrene-methacrylic acid ester copolymer resin, and is preferably polycarbonate resin.Furthermore, BPA, BPZ, dimethyl BPA, and BPA-dimethyl BPA copolymer are preferred in terms of crack resistance, abrasion resistance, and electrostatic property.
[0061] The content of the charge transporting compound in the charge transport layer is preferably 10 to 500 parts by mass, and more preferably 20 to 250 parts by mass, based on 100 parts by mass of the binder resin for the charge transport layer.
[0062] The charge transport layer may contain an antioxidant, an electronic conductive agent, a stabilizer, silicone oil, etc. As the antioxidant, those disclosed in JP-A-2000-305291 and as the electronic conductive agent, those disclosed in JP-A-50-137543 and JP-A-58-76483 are preferred.
[0063] The thickness of the charge transport layer differs depending on the characteristics of the charge transport compound, the characteristics of the binder resin, the mixing ratio, etc., but is preferably within the range of 5 to 40 μm, more preferably within the range of 10 to 30 μm.
[0064] (Photosensitive layer with single layer structure) The photosensitive layer having a single layer structure contains a charge generating compound and a charge transporting compound, and may contain other components that can be contained in the charge generating layer and the charge transporting layer.
[0065] When the photosensitive layer has a single layer structure, charge generation mainly occurs near the surface of the photosensitive layer. This makes it less susceptible to charge leak spots that may occur due to crystals derived from the alloy components of the support, and image defects are less likely to occur. In addition, when the photosensitive layer has a single layer structure, there is also the advantage that the photoconductor can be manufactured at low cost.
[0066] The thickness of the single-layer photosensitive layer varies depending on the characteristics of the charge generating compound, the characteristics of the charge transporting compound, the characteristics of the binder resin, the mixing ratio, etc., but is preferably within the range of 5 to 40 μm, and more preferably within the range of 10 to 30 μm.
[0067] <Surface protective layer> The surface protective layer is a layer containing a cured product of a composition for forming a surface protective layer. The photoreceptor of the present invention preferably has a surface protective layer, which can prevent an increase in surface roughness due to long-term use and suppress a decrease in cleaning properties.
[0068] The composition for forming a surface protective layer is a composition containing a polymerizable compound and a charge transporting compound, or a composition containing a charge transporting compound which is itself a polymerizable compound. The composition for forming a surface protective layer may contain a charge transporting compound which is itself a polymerizable compound, and another polymerizable compound.
[0069] The cured product of the composition is a cured product obtained by polymerizing the polymerizable compound in the composition to form a matrix.
[0070] "Charge transporting compound" refers to a compound that exhibits the transport of charge carriers, i.e., electrons or holes. As the charge transporting compound, known charge transporting compounds can be used, such as carbazole derivatives, oxazole derivatives, oxadiazole derivatives, thiazole derivatives, thiadiazole derivatives, triazole derivatives, imidazole derivatives, imidazolone derivatives, imidazolidine derivatives, bisimidazolidine derivatives, styryl compounds, hydrazone compounds, pyrazoline compounds, oxazolone derivatives, benzimidazole derivatives, quinazoline derivatives, benzofuran derivatives, acridine derivatives, phenazine derivatives, aminostilbene derivatives, triarylamine derivatives, phenylenediamine derivatives, stilbene derivatives, benzidine derivatives, poly-N-vinylcarbazole, poly-1-vinylpyrene, poly-9-vinylanthracene, and triphenylamine derivatives. These may be used in combination of two or more kinds.
[0071] The term "polymerizable compound" refers to a compound having a functional group capable of reacting by chain polymerization. The functional group capable of reacting by chain polymerization is preferably an acryloyloxy group (CH2=CHCOO-) or a methacryloyloxy group (CH2=C(CH3)COO-).
[0072] The composition for forming a surface protective layer preferably contains a polymerization initiator. The polymerization initiator is appropriately selected according to the type of polymerizable compound contained in the composition for forming the surface protective layer. The polymerization initiator may be a thermal polymerization initiator or a photopolymerization initiator, but is preferably a photopolymerization initiator. In particular, it is preferably a radical polymerization initiator.
[0073] The radical polymerization initiator is not particularly limited and may be any known one, and examples thereof include alkylphenone compounds and phosphine oxide compounds. Among these, compounds having an α-aminoalkylphenone structure or an acylphosphine oxide structure are preferred, and compounds having an acylphosphine oxide structure are more preferred. An example of a compound having an acylphosphine oxide structure is Omnirad819 (bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, manufactured by IGM Resins BV). The polymerization initiator may be used alone or in combination of two or more kinds. stomach.
[0074] The composition for forming a surface protective layer may further contain a solvent, inorganic fine particles, lubricating organic fine particles, an antioxidant, a stabilizer, silicone oil, and the like.
[0075] The thickness of the surface protective layer is preferably 0.2 to 10 μm, and more preferably 0.5 to 6 μm.
[0076] [Photoreceptor manufacturing method] The photoreceptor can be manufactured, for example, by successively forming each layer constituting the photoreceptor on the surface of the aluminum substrate according to the present invention. Each layer is formed by a process of forming a coating film made of a coating liquid containing a solid content (or its raw material components) constituting each layer and a solvent, and a process of curing the coating film. A specific method for manufacturing the photoreceptor will be described below using the manufacturing method for the photoreceptor 1 shown in FIG. 2 as an example.
[0077] The photoreceptor 1 can be manufactured, for example, through the following steps. Step (1): A step of forming an intermediate layer 102 by applying a coating liquid for forming an intermediate layer to the surface of a support (aluminum substrate) 101 and drying it. Step (2): A step of forming the charge generating layer 103 by applying a coating liquid for forming the charge generating layer on the surface of the intermediate layer 102 and drying it. Step (3): A step of forming the charge transport layer 104 by applying a coating liquid for forming the charge transport layer on the surface of the charge generation layer 103 and drying it. Step (4): A step of forming a surface protective layer 105 by applying a coating liquid for forming a surface protective layer on the surface of the charge transport layer 104 to form a coating film and curing the coating film.
[0078] <Step (1): Formation of intermediate layer> The intermediate layer 102 can be formed by applying a coating liquid for forming the intermediate layer to the surface of the support (aluminum substrate) 101 to form a coating film, and drying the coating film. The coating liquid for forming the intermediate layer can be prepared by dissolving a binder resin for the intermediate layer in a solvent and dispersing conductive particles therein.
[0079] As a means for dispersing the conductive particles, an ultrasonic disperser, a ball mill, a sand mill, a homomixer, or the like can be used.
[0080] Examples of the coating method of the coating liquid for forming the intermediate layer include known methods such as dip coating, spray coating, spinner coating, bead coating, blade coating, beam coating, and slide hopper methods (including circular slide hopper methods). The circular slide hopper method is a method used for coating the outer peripheral surface of a cylindrical or columnar article as the coating surface. The circular slide hopper method can be used as a method for coating the coating liquid for forming the intermediate layer on the outer peripheral surface of a drum-shaped support (aluminum substrate).
[0081] The method for drying the coating can be appropriately selected depending on the type of solvent and the thickness of the coating, but heat drying is preferred.
[0082] The solvent used in the step of forming the intermediate layer may be any solvent that can satisfactorily disperse the conductive particles or metal oxide particles and dissolve the binder resin for the intermediate layer. Specifically, the solvent is preferably an alcohol solvent having 1 to 4 carbon atoms, such as methanol, ethanol, n-propyl alcohol, isopropyl alcohol, n-butanol, t-butanol, sec-butanol, etc. By using these solvents, the solubility of the binder resin and the coating performance are excellent. Examples of co-solvents that can be used in combination with the above solvent to improve storage stability and particle dispersibility include benzyl alcohol, toluene, methylene chloride, cyclohexanone, and tetrahydrofuran.
[0083] The concentration of the binder resin for the intermediate layer in the coating liquid for forming the intermediate layer is appropriately selected according to the thickness of the intermediate layer and the production speed.
[0084] <Step (2): Formation of Charge Generation Layer> The charge generating layer 103 can be formed by applying a coating liquid for forming the charge generating layer to the surface of the intermediate layer 102 to form a coating film, and drying the coating film. The coating liquid for forming the charge generating layer can be prepared by dispersing a charge generating compound in a solution in which a binder resin for the charge generating layer is dissolved in a solvent.
[0085] As a means for dispersing the charge generating compound in the coating liquid for forming the charge generating layer, for example, an ultrasonic disperser, a ball mill, a sand mill, a homomixer, or the like can be used.
[0086] Examples of methods for applying the coating liquid for forming the charge generating layer include known methods such as dip coating, spray coating, spinner coating, bead coating, blade coating, beam coating, and slide hopper methods (including circular slide hopper methods).
[0087] The method for drying the coating can be appropriately selected depending on the type of solvent and the thickness of the coating, but heat drying is preferred.
[0088] Examples of solvents used in forming the charge generating layer include toluene, xylene, methylene chloride, 1,2-dichloroethane, methyl ethyl ketone, cyclohexane, ethyl acetate, t-butyl acetate, methanol, ethanol, propanol, butanol, methyl cellosolve, 4-methoxy-4-methyl-2-pentanone, ethyl cellosolve, tetrahydrofuran, 1-dioxane, 1,3-dioxolane, pyridine, and diethylamine.
[0089] <Step (3): Formation of Charge Transport Layer> The charge transport layer 104 can be formed by applying a coating liquid for forming the charge transport layer to the surface of the charge generating layer 103 to form a coating film, and drying the coating film. The coating liquid for forming the charge transport layer can be prepared by dissolving a binder resin for the charge transport layer and a charge transporting compound in a solvent.
[0090] Examples of methods for applying the coating liquid for forming the charge transport layer include known methods such as dip coating, spray coating, spinner coating, bead coating, blade coating, beam coating, and slide hopper methods (including circular slide hopper methods).
[0091] The method for drying the coating can be appropriately selected depending on the type of solvent and the thickness of the coating, but heat drying is preferred.
[0092] Examples of solvents used in forming the charge transport layer 104 include toluene, xylene, methylene chloride, 1,2-dichloroethane, methyl ethyl ketone, cyclohexanone, ethyl acetate, butyl acetate, methanol, ethanol, propanol, butanol, tetrahydrofuran, 1,4-dioxane, 1,3-dioxolane, pyridine, and diethylamine.
[0093] <Step (4): Formation of Surface Protection Layer> The surface protective layer 105 can be formed by applying a coating liquid for forming the surface protective layer onto the surface of the charge transport layer 104 to form a coating film, and then curing the coating film.
[0094] The coating liquid for forming the surface protective layer can typically be prepared by dissolving or dispersing the composition for forming the surface protective layer in a solvent. However, when the composition for forming the surface protective layer is a liquid composition having a viscosity that allows it to be applied to the surface of the charge transport layer, it is not necessary to use a solvent. In this case, the composition for forming the surface protective layer itself can be used as the coating liquid for forming the surface protective layer.
[0095] Examples of solvents used in forming the surface protective layer include methanol, ethanol, n-propyl alcohol, isopropyl alcohol, n-butanol, t-butanol, sec-butanol, benzyl alcohol, toluene, xylene, dichloromethane, methyl ethyl ketone, cyclohexane, ethyl acetate, butyl acetate, methyl cellosolve, ethyl cellosolve, tetrahydrofuran, 1,4-dioxane, 1,3-dioxolane, pyridine, and diethylamine.
[0096] Examples of methods for applying the coating liquid for forming the surface protective layer include known methods such as the slide hopper method (including the circular slide hopper method), dip coating method, spray coating method, spinner coating method, bead coating method, blade coating method, and beam coating method.
[0097] After the coating liquid for forming the surface protective layer is applied, the reactive components in the coating film are reacted to harden the coating film, thereby forming the surface protective layer 105.
[0098] The coating film may be cured without being dried, but it is preferable to carry out the curing treatment after natural drying or heat drying.
[0099] Drying conditions can be appropriately selected depending on the type of solvent, the thickness of the coating film, etc. The drying temperature is preferably within the range of room temperature (25° C.) to 180° C., and particularly preferably within the range of 80 to 140° C. The drying time is preferably 1 to 200 minutes, and particularly preferably 5 to 100 minutes.
[0100] In the curing treatment for curing the coating film, for example, the coating film is irradiated with ultraviolet light to generate radicals, which cause a polymerization reaction of the polymerizable compound.
[0101] Any light source that generates ultraviolet light can be used without limitation as the ultraviolet light source, including, for example, a low pressure mercury lamp, a medium pressure mercury lamp, a high pressure mercury lamp, an ultra-high pressure mercury lamp, a carbon arc lamp, a metal halide lamp, a xenon lamp, and a flash (pulse) xenon lamp.
[0102] The irradiation conditions vary depending on the lamp. For example, the amount of ultraviolet light is usually 5 to 1000 dp. 500mJ / cm 2 within the range of 5 to 100 mJ / cm 2 The lamp power is preferably in the range of 0.1 to 5 kW, and particularly preferably in the range of 0.5 to 3 kW. The irradiation time for obtaining the necessary amount of ultraviolet irradiation is, for example, preferably 0.1 seconds to 10 minutes, and from the viewpoint of work efficiency, more preferably 0.1 seconds to 5 minutes.
[0103] In the step of forming the surface protective layer, drying can be appropriately carried out before, after, and during the irradiation of ultraviolet rays.
[0104] 2.Developing roller [Developing roller configuration] The developing roller according to the present invention includes a developing sleeve. The "developing sleeve" is a means having a function of carrying a moderately charged developer and supplying the developer to a photoconductor on which an electrostatic latent image is formed. The developing sleeve is a part of a developing roller included in a developing device provided in an electrophotographic image forming apparatus, for example, and the developing roller is composed of a developing sleeve, a flange, a shaft, and a member that generates a magnetic flux. Incidentally, since the above-mentioned "member generating magnetic flux" is generally used as a magnet roller, in the following description, the "member generating magnetic flux" will be simply referred to as a "magnet roller."
[0105] Fig. 3 is a cross-sectional view of the developing roller as viewed from a direction perpendicular to the axial direction, and Fig. 4 is a cross-sectional view of the developing roller as viewed from the axial direction of Fig. 3. In the drawings, reference numeral 10 denotes the developing roller.
[0106] The developing sleeve is rotatable and cylindrical, and serves to carry and transport the developer on its surface. As shown in FIG. 3, a substantially cylindrical developing sleeve 11 is provided, and a first flange 18 and a second flange 19 are fixedly attached to both ends of the developing sleeve 11.
[0107] The first flange 18 is formed with a shaft portion 18a that extends in a leftward protruding manner, and the first flange 18 is formed with a recess 18b in the approximate center of the right portion. A through hole is formed in the approximate center of the second flange 19 , and a shaft 16 is provided coaxially with the developing sleeve 11 in the center of the developing sleeve 11 . The left end of the shaft 16 is rotatably supported by the first flange 18 via a bearing 17 mounted in the recess 18b. The right end of the shaft 16 is rotatably supported by a second flange 19 via a bearing 17 mounted in the through hole, and extends rightward through the through hole.
[0108] A substantially cylindrical magnet roller 12 is fixed to a shaft 16 within the developing sleeve 11 in a non-contact manner with the inner peripheral surface of the developing sleeve 11 (see FIG. 4). The magnet roller 12 fixed to the shaft 16 is supported via a first flange 18 and a second flange 19 to be relatively rotatable relative to the developing sleeve 11 .
[0109] The magnet roller 12 has a general structure made of a resin magnet or a sintered magnet, with a plurality of magnetic poles formed in the circumferential direction on the outer periphery. For example, magnets may have south and north poles arranged alternately in the circumferential direction of the outer periphery, or magnets may have south and north poles arranged to form a predetermined magnetic pattern.
[0110] The developing sleeve according to the present invention preferably contains an aluminum alloy. The aluminum alloy is a conductive material with a relatively small electrical resistance, and when the developing sleeve is rotated relative to the magnet roller, the developing sleeve crosses the magnetic field lines generated by the magnet roller. This causes an electromagnetic induction effect, which generates an eddy current around the surface of the developing sleeve.
[0111] 3. Toner for developing electrostatic images [Toner base particles] The toner base particles constituting the electrostatic image developing toner according to the present invention contain at least a binder resin, and may contain a colorant, a release agent and other additives as required. The glass transition point (Tg) of the toner according to the present invention is within the range of 0 to 45° C. as described above.
[0112] In the present invention, the term "toner particles" refers to toner base particles to which an external additive has been added, and an aggregate of toner particles is called "toner". Generally, the toner base particles can be used as they are as toner particles, but in the present invention, the toner base particles to which an external additive has been added are used as toner particles. In the following description, when there is no need to particularly distinguish between toner base particles and toner particles, they are also simply referred to as "toner particles". Hereinafter, each of the constituent materials of the toner base particles according to the present invention will be described in detail.
[0113] <Binding resin> The toner base particles contain polyester as a binder resin, and it is particularly preferable that the main component of the binder resin is polyester. Here, the phrase "the main component of the binder resin is polyester" means that 50 mass % or more of the binder resin is polyester.
[0114] Polyester is a dehydration condensation reaction system that is particularly compatible with paper and has a high internal cohesion, which means that it has high folding fixability after fixing is complete, making it possible to fix at even lower temperatures. In addition, "fold fixability" refers to the property that indicates the ease with which the toner layer peels off at the fold line when, for example, a black band-like toner image is formed using toner on paper as a recording medium, the paper is then folded in half and then unfolded again. If the "folding fixability" is high, the above-mentioned destruction of the toner layer does not occur, and good fixability can be realized.
[0115] On the other hand, as mentioned above, by incorporating silicon into the aluminum substrate, protrusions are formed on the surface of the aluminum substrate, which is advantageous for transfer in terms of adhesion to the toner. However, since minute leaks also occur, the effect of the protrusions cannot be fully demonstrated. Therefore, by using a resin with high polarity such as polyester in the toner, it is possible to polarize the toner during transfer and suppress the above-mentioned minute leaks, which is expected to further improve transferability. From the above, it is preferable that the binder resin contains polyester in the range of 50 to 95% by mass from the viewpoint of improving low-temperature fixability and transferability.
[0116] The toner particles may contain a non-crystalline polyester and a crystalline polyester as a binder resin. Either crystalline or amorphous resin may be used, but it is the crystalline resin that provides the sharp melting property.
[0117] The term "crystalline" refers to a state in which a clear endothermic peak is present rather than a stepwise change in endothermic amount in differential scanning calorimetry (DSC), and specifically refers to a state in which the half-width of the endothermic peak is within 10°C when measured at a heating rate of 10 (°C / min). On the other hand, "amorphous" refers to a half-width exceeding 10°C, a stepwise change in endothermic heat, or no clear endothermic peak.
[0118] (amorphous polyester) The content of the amorphous polyester is preferably within a range of 50 to 88% by mass, and more preferably within a range of 60 to 80% by mass, based on the total amount of the binder resin. The amorphous polyester may be, for example, a condensation polymer of a polycarboxylic acid and a polyhydric alcohol. As the amorphous polyester, a commercially available product or a synthesized product may be used.
[0119] [Polycarboxylic acid] Examples of the polycarboxylic acid include aliphatic dicarboxylic acids, alicyclic dicarboxylic acids, aromatic dicarboxylic acids, their anhydrides, and their lower alkyl esters. Among these, the polycarboxylic acid is preferably, for example, an aromatic dicarboxylic acid.
[0120] Examples of the aliphatic dicarboxylic acid include oxalic acid, malonic acid, maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, succinic acid, alkenylsuccinic acid, adipic acid, and sebacic acid. The alicyclic dicarboxylic acid may, for example, be cyclohexanedicarboxylic acid. Examples of the aromatic dicarboxylic acid include terephthalic acid, isophthalic acid, phthalic acid, and naphthalenedicarboxylic acid.
[0121] The lower alkyl esters include, for example, those having 1 to 5 carbon atoms. The polyvalent carboxylic acid may be a trivalent or higher carboxylic acid having a crosslinked or branched structure in combination with a dicarboxylic acid. Examples of trivalent or higher carboxylic acids include trimellitic acid, pyromellitic acid, anhydrides thereof, and lower alkyl esters thereof. The lower alkyl esters include, for example, those having 1 to 5 carbon atoms. The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.
[0122] [Polyhydric alcohol] Examples of polyhydric alcohols include aliphatic diols, alicyclic diols, and aromatic diols. Among these, aromatic diols and alicyclic diols are preferred, and aromatic diols are more preferred.
[0123] Examples of the aliphatic diol include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butanediol, hexanediol, and neopentyl glycol. Examples of the alicyclic diol include cyclohexanediol, cyclohexanedimethanol, hydrogenated bisphenol A, and the like. Examples of the aromatic diol include an ethylene oxide adduct of bisphenol A and a propylene oxide adduct of bisphenol A.
[0124] As the polyhydric alcohol, a trihydric or higher polyhydric alcohol having a crosslinked or branched structure may be used in combination with the diol. Examples of trihydric or higher polyhydric alcohols include glycerin, trimethylolpropane, and pentaerythritol. The polyhydric alcohols may be used alone or in combination of two or more kinds.
[0125] [Glass transition temperature of amorphous polyester] The amorphous polyester is used either inside the toner or as a shell material on the surface of the toner.
[0126] When used inside the toner, the glass transition point (Tg) is preferably within the range of -5 to 40°C, and more preferably within the range of 0 to 30°C. When the amorphous polyester is used as a shell material, the glass transition point (Tg) is preferably within a range of 50 to 80°C, and more preferably within a range of 50 to 65°C. The glass transition point can be determined from a DSC curve obtained by differential scanning calorimetry (DSC). More specifically, it can be determined from the "extrapolated glass transition onset temperature" described in the method for determining the glass transition point in JIS K-7121-1987 "Method for measuring transition temperature of plastics."
[0127] 〔others〕 In this embodiment, two or more kinds of amorphous polyesters may be used in combination. In this case, the absolute value of the difference in SP value between the amorphous polyester exhibiting the largest SP value and the amorphous polyester exhibiting the smallest SP value is preferably 0.25 or less, more preferably within the range of 0.01 to 0.25, and even more preferably within the range of 0.10 to 0.25. When the absolute value of the difference in SP value is 0.25 or less, it becomes possible to adjust the compatibility between the crystalline polyester and the amorphous polyester within an appropriate range.
[0128] The amorphous polyester can be obtained by a known manufacturing method. Specifically, for example, the polymerization temperature is set within the range of 180 to 230° C., and the reaction system is reduced in pressure as necessary, and water and alcohol generated during condensation are removed during the reaction to obtain the polyvinyl chloride. If the raw material monomer is not soluble or compatible at the reaction temperature, a high boiling point solvent may be added as a dissolution aid to dissolve it. In this case, the polycondensation reaction is carried out while distilling off the solubilizing agent.
[0129] When a monomer having poor compatibility is present in the copolymerization reaction, it is advisable to condense the monomer having poor compatibility with the acid or alcohol to be polycondensed in advance, and then polycondense the monomer with the main component.
[0130] In the present embodiment, the SP value of the amorphous polyester can be adjusted by selecting the types of polyvalent carboxylic acid and polyhydric alcohol constituting the amorphous polyester so that the SP value of the amorphous polyester is a desired value.
[0131] (Crystalline polyester) The crystalline polyester is contained in an amount of preferably 5 to 35% by mass, and more preferably 10 to 30% by mass, based on the total amount of the binder resin. The crystalline polyester may be, for example, a polycondensate of a polycarboxylic acid and a polyhydric alcohol. As the crystalline polyester, a commercially available product or a synthesized product may be used. Here, the crystalline polyester is preferably a polycondensate using a polymerizable monomer having a linear aliphatic chain rather than a polymerizable monomer having an aromatic chain, since the crystalline polyester easily forms a crystalline structure.
[0132] [Polycarboxylic acid] Examples of the polycarboxylic acid include aliphatic dicarboxylic acids, aromatic dicarboxylic acids, anhydrides thereof, and lower alkyl esters thereof.
[0133] Examples of the aliphatic dicarboxylic acid include oxalic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid.
[0134] Examples of aromatic dicarboxylic acids include dibasic acids such as phthalic acid, isophthalic acid, terephthalic acid, and naphthalene-2,6-dicarboxylic acid. The lower alkyl esters include, for example, those having 1 to 5 carbon atoms.
[0135] The polyvalent carboxylic acid may be a trivalent or higher carboxylic acid having a crosslinked or branched structure in combination with a dicarboxylic acid. Examples of the trivalent carboxylic acid include aromatic carboxylic acids, their anhydrides, and their lower alkyl esters. Examples of aromatic carboxylic acids include 1,2,3-benzenetricarboxylic acid, 1,2,4-benzenetricarboxylic acid, and 1,2,4-naphthalenetricarboxylic acid.
[0136] The lower alkyl esters include, for example, those having 1 to 5 carbon atoms. As the polyvalent carboxylic acid, a dicarboxylic acid having a sulfonic acid group and a dicarboxylic acid having an ethylenic double bond may be used in combination with these dicarboxylic acids. The polyvalent carboxylic acids may be used alone or in combination of two or more kinds.
[0137] [Polyhydric alcohol] The polyhydric alcohol includes, for example, an aliphatic diol, and for example, a straight-chain aliphatic diol having a main chain carbon number in the range of 7 to 20 is preferable.
[0138] Examples of the aliphatic diol include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, and 1,14-eicosanedecanediol. Among these, 1,8-octanediol, 1,9-nonanediol and 1,10-decanediol are preferred.
[0139] The polyhydric alcohol may be used in combination with a diol and a trihydric or higher alcohol having a crosslinked or branched structure. Examples of trihydric or higher alcohols include glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol. The polyhydric alcohols may be used alone or in combination of two or more kinds. Here, the polyhydric alcohol has an aliphatic diol content of 80 mol % or more, preferably 90 mol % or more.
[0140] [Melting temperature of crystalline polyester] The melting temperature of the crystalline polyester is preferably within a range of 55 to 80°C, more preferably within a range of 55 to 78°C, and even more preferably within a range of 55 to 76°C. When the melting temperature of the crystalline polyester is 72° C. or higher, the heat storage property is further improved. If the melting temperature of the crystalline polyester is 80° C. or lower, the low-temperature fixing property is further improved. The melting temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC) based on the "melting peak temperature" described in the method for determining melting temperature in JIS K7121-1987 "Method for measuring transition temperature of plastics."
[0141] 〔others〕 The crystalline polyester can be obtained by a known manufacturing method, for example, in the same manner as the amorphous polyester. In the present embodiment, the SP value of the crystalline polyester can be adjusted by selecting the types of polyvalent carboxylic acid and polyhydric alcohol constituting the crystalline polyester so that the SP value of the crystalline polyester is a desired value.
[0142] (Other resins) In this embodiment, as the binder resin, resins other than the amorphous polyester and the crystalline polyester may be used. Other examples of binder resins include styrenes, (meth)acrylic acid esters, ethylenically unsaturated nitriles, Other examples of binder resins include vinyl resins made of homopolymers of monomers such as styrenes (e.g., styrene, parachlorostyrene, α-methylstyrene, etc.), vinyl ethers, vinyl ketones, olefins, etc., or copolymers of two or more of these monomers.
[0143] Examples of (meth)acrylic acid esters include methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, lauryl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, lauryl methacrylate, and 2-ethylhexyl methacrylate.
[0144] Examples of the ethylenically unsaturated nitriles include acrylonitrile and methacrylonitrile. Examples of the vinyl ethers include vinyl methyl ether and vinyl isobutyl ether. Examples of vinyl ketones include vinyl methyl ketone, vinyl ethyl ketone, and vinyl isopropenyl ketone. Examples of the olefins include ethylene, propylene, and butadiene.
[0145] Examples of the binder resin include non-vinyl resins such as epoxy resins, polyurethane resins, polyamide resins, cellulose resins, polyether resins, and modified rosin. Further, there may be mentioned a mixture of the above-mentioned resin with the vinyl resin, or a graft polymer obtained by polymerizing a vinyl monomer in the presence of the above-mentioned resin. These other binder resins may be used alone or in combination of two or more.
[0146] In this embodiment, a styrene-(meth)acrylic copolymer resin may be used as another binder resin. By using a styrene-(meth)acrylic copolymer resin as another binder resin, the fixing characteristics such as hot offset and the like and the heat storage properties are further improved. When a styrene-(meth)acrylic copolymer resin is used as the other binder resin, the proportion of the styrene-(meth)acrylic copolymer resin in the binder resin is preferably within a range of 5 to 25% by mass. The above range is more preferably within a range of 5 to 20% by mass, and further preferably within a range of 10 to 15% by mass. If the ratio of the styrene-(meth)acrylic copolymer resin in the binder resin is 5 or more, the fixing characteristics such as hot offset and the heat storage properties are further improved. If the proportion of the styrene-(meth)acrylic copolymer resin in the binder resin is 25% by mass or less, the low-temperature fixability is further improved.
[0147] In this embodiment, (meth)acrylic means acrylic or methacrylic. The styrene-(meth)acrylic copolymer resin can be synthesized by various polymerization methods, for example, solution polymerization, precipitation polymerization, suspension polymerization, precipitation polymerization, bulk polymerization, and emulsion polymerization. The polymerization reaction can be carried out by known procedures such as batch, semi-continuous, and continuous.
[0148] A preferred combination of the binder resin according to the present invention is a combination of amorphous polyester and crystalline polyester. It is preferable that the binder resin contains 65 to 95% by mass of amorphous polyester and 5 to 35% by mass of crystalline polyester. Alternatively, only styrene-(meth)acrylic copolymer resin may be used as the binder resin.
[0149] <Coloring agent> The colorant may be, for example, a pigment or a dye. Examples of pigments include carbon black, chrome yellow, Hansa Yellow, benzidine yellow, threne yellow, quinoline yellow, pigment yellow, permanent orange GTR, pyrazolone orange, Balkan orange, watch young red, permanent red, brilliant carmine 3B, brilliant carmine 6B, DuPont oil red, pyrazolone red, lithol red, rhodamine B lake, lake red C, pigment red, rose bengal, aniline blue, ultramarine blue, chalco oil blue, methylene blue chloride, phthalocyanine blue, pigment blue, phthalocyanine green, and malachite green oxalate.
[0150] Examples of dyes include acridine-based, xanthene-based, azo-based, benzoquinone-based, azine-based, anthraquinone-based, thioindigo-based, dioxazine-based, thiazine-based, azomethine-based, indigo-based, phthalocyanine-based, aniline black-based, polymethine-based, triphenylmethane-based, diphenylmethane-based, and thiazole-based dyes.
[0151] The colorants may be used alone or in combination of two or more. The colorant may be surface-treated as necessary, or may be used in combination with a dispersant. In addition, a plurality of types of colorants may be used in combination. The content of the colorant is, for example, preferably within a range of 1 to 30% by mass, and more preferably within a range of 3 to 15% by mass, based on the total mass of the toner particles.
[0152] <Release agent> The release agent may be, for example, a hydrocarbon wax. Other examples include natural waxes, synthetic or mineral / petroleum-based waxes, and ester-based waxes, but are not limited to these. Examples of natural waxes include carnauba wax, rice wax, and candelilla wax. An example of the synthetic or mineral / petroleum wax is montan wax. Examples of the ester wax include fatty acid esters and montanic acid esters.
[0153] The melting temperature of the release agent is preferably within a range of 50 to 110°C, and more preferably within a range of 60 to 100°C. The melting temperature is determined from a DSC curve obtained by differential scanning calorimetry (DSC) based on the "melting peak temperature" described in the method for determining melting temperature in JIS K-7121-1987 "Method for measuring transition temperature of plastics."
[0154] The content of the release agent is, for example, preferably within a range of 1 to 20% by mass, and more preferably within a range of 5 to 15% by mass, based on the total mass of the toner particles.
[0155] <Other additives> Examples of other additives include well-known additives such as magnetic materials, charge control agents, and inorganic powders, and these additives are contained in the toner particles as internal additives.
[0156] (magnetic material) Magnetic materials include iron oxides such as magnetite, hematite, and ferrite, metals such as iron, cobalt, and nickel, and alloys of these metals with metals such as aluminum, cobalt, copper, lead, magnesium, tin, zinc, antimony, bismuth, calcium, manganese, titanium, tungsten, and vanadium, and mixtures thereof.
[0157] The shape of the magnetic material may be polyhedral, octahedral, hexahedral, spherical, needle-like, scale-like, etc., and those with less anisotropy such as polyhedral, octahedral, hexahedral, and spherical shapes are preferred in terms of increasing image density.
[0158] The magnetic material preferably has a number-average particle size within the range of 0.10 to 0.40 μm. Generally, the smaller the particle size of the magnetic material, the higher the coloring power, but the magnetic material is more likely to aggregate, so the above range is preferable from the viewpoint of the balance between coloring power and aggregation properties.
[0159] The number-average particle size of the magnetic material can be measured using a transmission electron microscope. Specifically, the toner particles to be observed are thoroughly dispersed in an epoxy resin, and then the resin is cured in an atmosphere at a temperature of 40° C. for two days to obtain a cured product. The obtained cured product is cut into a thin-section sample using a microtome, and the diameters of 100 magnetic particles in the field of view are measured using a transmission electron microscope (TEM) at a magnification of 10,000 or 40,000. Then, the number-average particle size is calculated based on the equivalent diameter of a circle equal to the projected area of the magnetic material. It is also possible to measure the particle size using an image analyzer.
[0160] The magnetic material used in the toner of the present invention can be produced, for example, by the following method. An aqueous solution containing ferrous hydroxide is prepared by adding an alkali such as sodium hydroxide in an amount equivalent to or greater than the amount of the iron component to an aqueous solution of a ferrous salt. While maintaining the pH of the prepared aqueous solution at 7 or higher, air is blown in and the aqueous solution is heated to 70°C or higher to carry out the oxidation reaction of ferrous hydroxide, thereby first producing seed crystals that will become the core of the magnetic iron oxide powder. Next, an aqueous solution containing about 1 equivalent of ferrous sulfate is added to the slurry liquid containing the seed crystals, based on the amount of the alkali previously added. While maintaining the pH of the liquid within the range of 5 to 10, the reaction of ferrous hydroxide is allowed to proceed while blowing in air, and magnetic iron oxide powder is grown around the seed crystals as cores. At this time, by selecting any pH, reaction temperature, and stirring conditions, it is possible to control the shape and magnetic properties of the magnetic material. As the oxidation reaction proceeds, the pH of the solution shifts to the acidic side, but it is preferable not to allow the pH of the solution to fall below 5. The magnetic material thus obtained is filtered, washed, and dried in a standard manner to obtain the desired magnetic material.
[0161] In the present invention, when the toner is produced in an aqueous medium, it is highly preferable to subject the surface of the magnetic material to a hydrophobic treatment. When performing surface treatment using a dry method, the washed, filtered and dried magnetic material is treated with a coupling agent. When the surface treatment is carried out by a wet method, the dried material is redispersed after the oxidation reaction is completed. Alternatively, after the oxidation reaction is completed, the iron oxide body obtained by washing and filtration is redispersed in another aqueous medium without drying, thereby carrying out the coupling treatment. In the present invention, either the dry method or the wet method can be appropriately selected.
[0162] The content of the magnetic material in the toner can be measured using a thermal analyzer, TGA7, manufactured by PerkinElmer, as follows. The toner is heated from room temperature to 900° C. at a temperature increase rate of 25° C. / min in a nitrogen atmosphere. The mass percent weight loss between 100°C and 750°C is taken as the amount of binder resin, and the remaining mass is taken as approximately the amount of magnetic material.
[0163] (Charge control agent) In order to stabilize the chargeability, it is preferable to use a charge control agent.
[0164] As such a charge control agent, any known charge control agent can be used alone or in combination.
[0165] Considering the suitability for color toners (the charge control agent itself is colorless or light-colored and does not interfere with the color tone of the toner), quaternary ammonium salt compounds are preferred for their positive chargeability.
[0166] Preferred examples of the negatively charged compounds include metal salts and metal complexes of salicylic acid or alkylsalicylic acid with chromium, zinc, aluminum, etc., metal salts and metal complexes of benzilic acid, amide compounds, phenol compounds, naphthol compounds, and phenolamide compounds.
[0167] Furthermore, the material may be a polymer that exhibits negative charging properties, such as a sulfonate, a carboxylate, or a halogen.
[0168] <Characteristics of toner particles, etc.> The toner particles may be toner particles having a single layer structure, or may be toner particles having a so-called core-shell structure composed of a core portion (core particle) and a coating layer (shell layer) that coats the core portion.
[0169] Here, the toner particles having a core-shell structure may be composed of a core portion containing, for example, a binder resin and, if necessary, other additives such as a colorant and a release agent, and a coating layer containing the binder resin.
[0170] Volume average particle size of toner particles (D 50 v) is preferably within the range of 2 to 10 μm, more preferably within the range of 4 to 8 μm. The various average particle sizes and particle size distribution indexes of the toner particles are measured using a Coulter Multisizer II (manufactured by Beckman Coulter, Inc.), and the electrolyte is measured using an ISOTON-II (manufactured by Beckman Coulter, Inc.).
[0171] For the measurement, 0.5 to 50 mg of the measurement sample is added to 2 mL of a 5% aqueous solution of a surfactant (preferably sodium alkylbenzene sulfonate) as a dispersant. This is added to 100 to 150 mL of electrolyte. The electrolyte with the sample suspended in it is dispersed for 1 minute using an ultrasonic disperser, and the particle size distribution of particles with a particle size in the range of 2 to 60 μm is measured using a Coulter Multisizer II with an aperture of 100 μm in diameter. The number of particles sampled is 50,000. Based on the particle size distribution measured, the cumulative distribution of volume and number is drawn for each divided particle size range (channel) from the small particle size side. The particle size at which the cumulative 16% occurs is called the volume particle size D 16 v, number particle size D 16 p, the particle size at which the cumulative 50% is reached is the volume average particle size D 50 v, cumulative number average particle diameter D 50 p, the particle size at which the cumulative 84% occurs is the volume particle size D 84 v, number particle size D 84 Define it as p. Using these, the volume average particle size distribution index (GSDv) is (D 84 v / D 16 v)1 / 2, the number average particle size distribution index (GSDp) is (D 84 p / D 16 p)1 / 2.
[0172] [External additives] The external additive may, for example, be inorganic particles. Examples of inorganic particles include SiO2, TiO2, Al2O3, CuO, ZnO, SnO2, CeO2, Fe2O3, MgO, BaO, CaO, K2O, Na2O, ZrO2, CaO·SiO2, K2O·(TiO2) n , Al2O3·2SiO2, CaCO3, MgCO3, BaSO4, MgSO 4、 In addition to the above, inorganic chlorides such as titanates can also be used.
[0173] The surfaces of the inorganic particles used as the external additive are preferably subjected to a hydrophobic treatment. The hydrophobic treatment is carried out, for example, by immersing the inorganic particles in a hydrophobic treatment agent. The hydrophobic treatment agent is not particularly limited, but examples thereof include silane coupling agents, silicone oil, titanate coupling agents, and aluminum coupling agents. These may be used alone or in combination of two or more. The amount of the hydrophobizing agent is usually within the range of 1 part by mass to 10 parts by mass with respect to 100 parts by mass of the inorganic particles.
[0174] Examples of the external additive include resin particles and cleaning lubricants. Examples of the resin particles include resin particles of polystyrene, polymethyl methacrylate (PMMA), melamine resin, and the like. Examples of cleaning lubricants include metal salts of higher fatty acids, such as zinc stearate, and particles of fluorine-based polymers.
[0175] The amount of the external additive added is preferably within a range of 0.01 to 5% by mass, and more preferably within a range of 0.01 to 2.0% by mass, based on the toner particles.
[0176] [Method of manufacturing toner for developing electrostatic images] Next, a method for producing the toner according to the present invention will be described.
[0177] The toner according to the exemplary embodiment is obtained by producing toner particles and then externally adding an external additive to the toner particles. The toner particles may be produced by either a dry production method (such as a kneading and pulverizing method) or a wet production method (such as an aggregation-coalescence method, a suspension polymerization method, a dissolution-suspension method, etc.). The "aggregation-coalescence method" is also called the "emulsion-association method." The method for producing the toner particles is not particularly limited, and any known method may be used. Some examples of the method for producing the toner particles are given below.
[0178] <Agglutination coalescence method> The aggregation and coalescence method includes, for example, three steps: (1) a resin particle dispersion preparation step, (2) an aggregated particle formation step, and (3) a fusion and coalescence step. Each step will be described in detail below. In the following description, a method for obtaining toner particles containing a colorant and a release agent will be described, but the colorant and the release agent are used as necessary. Of course, additives other than the colorant and the release agent may be used.
[0179] (1) Resin particle dispersion preparation process The resin particle dispersion preparation step is a step of preparing a resin particle dispersion in which resin particles that will become a binder resin are dispersed. Here, it is preferable to select a binder resin so that the glass transition temperature of the toner to be produced is in the range of 0 to 45°C. First, a resin particle dispersion in which resin particles serving as a binder resin are dispersed, a colorant particle dispersion in which colorant particles are dispersed, and a release agent particle dispersion in which release agent particles are dispersed are prepared. Here, the resin particle dispersion liquid is prepared, for example, by dispersing resin particles in a dispersion medium with the aid of a surfactant.
[0180] (dispersion medium) The dispersion medium used in the resin particle dispersion liquid is, for example, an aqueous medium. Examples of the aqueous medium include water such as distilled water and ion-exchanged water, alcohols, etc. These may be used alone or in combination of two or more kinds.
[0181] (Surfactant) Examples of the surfactant include anionic surfactants, cationic surfactants, and nonionic surfactants, with anionic surfactants and cationic surfactants being particularly preferred.
[0182] The nonionic surfactant may be used in combination with an anionic surfactant or a cationic surfactant. The surfactants may be used alone or in combination of two or more. Examples of the anionic surfactant include sulfate salts, sulfonate salts, phosphate salts, and soap salts. Examples of the cationic surfactant include amine salt types and quaternary ammonium salt types. Examples of nonionic surfactants include polyethylene glycol surfactants, alkylphenol ethylene oxide adduct surfactants, polyhydric alcohol surfactants, and the like.
[0183] (Distribution method) In the resin particle dispersion, the resin particles can be dispersed in a dispersion medium by a general dispersion method using, for example, a rotary shear type homogenizer, a ball mill having a media, a sand mill, a dyno mill, or the like. Depending on the type of resin particles, the resin particles may be dispersed in the resin particle dispersion liquid by using, for example, a phase inversion emulsification method.
[0184] The phase inversion emulsification method is the following method. The resin to be dispersed is dissolved in a hydrophobic organic solvent in which the resin is soluble, and a base is added to the organic continuous phase (O phase) to neutralize it. Thereafter, an aqueous medium (W phase) is added, causing the resin to undergo conversion (so-called phase inversion) from W / O to O / W, forming a discontinuous phase, and the resin is dispersed in particulate form in the aqueous medium.
[0185] The resin particle dispersion may be prepared by forming resin particles by a conventional emulsion polymerization method, and then aggregating and fusing the resin particles to form binder resin particles. Specifically, polymerizable monomers constituting the binder resin are introduced into an aqueous medium, dispersed therein, and then polymerized by a polymerization initiator to prepare a binder resin particle dispersion. The method of preparing a resin particle dispersion from a polymerizable monomer is called an emulsion polymerization method. The emulsion association method is a method of producing a toner using a dispersion obtained by the emulsion polymerization method or the like.
[0186] (Volume average particle size of resin particles) The volume average particle size of the resin particles dispersed in the resin particle dispersion is, for example, preferably within the range of 0.01 to 1 μm, more preferably within the range of 0.08 to 0.8 μm, and even more preferably within the range of 0.1 to 0.6 μm.
[0187] The volume average particle size of the resin particles can be measured by a laser diffraction particle size distribution measuring device. An example of a laser diffraction particle size distribution measuring device is the "LA-700" (manufactured by Horiba, Ltd.). Examples include: Using the particle size distribution obtained by measurement using the above-mentioned device, the cumulative distribution for the volume of each divided particle size range (channel) is subtracted from the small particle size side. The particle size that is cumulatively 50% of all particles is called the volume average particle size D 50 It is measured as v. The volume average particle diameters of particles in other dispersions are also measured in the same manner.
[0188] (Resin particle content) The content of the resin particles in the resin particle dispersion is, for example, preferably in the range of 5 to 50% by mass, and more preferably in the range of 10 to 40% by mass.
[0189] (Other preparation methods) In the same manner as the resin particle dispersion, for example, a colorant particle dispersion and a release agent particle dispersion are also prepared. In other words, the volume average particle size, dispersion medium, dispersion method, and particle content of the particles in the resin particle dispersion liquid are the same for the colorant particles dispersed in the colorant particle dispersion liquid and the release agent particles dispersed in the release agent particle dispersion liquid.
[0190] (2) Agglomerated particle formation process The aggregated particle forming step is a step of aggregating resin particles in a resin particle dispersion to form aggregated particles. The resin particle dispersion may be a mixture of other particle dispersions as required, and may be aggregated to form aggregated particles. Next, the colorant particle dispersion and the release agent particle dispersion are mixed together with the resin particle dispersion. Then, in the mixed dispersion, the resin particles, the colorant particles, and the release agent particles are hetero-aggregated to form aggregated particles containing the resin particles, the colorant particles, and the release agent particles and having a diameter close to that of the target toner particles.
[0191] Specifically, the aggregated particles are formed as follows.
[0192] For example, a flocculant is added to the mixed dispersion, the pH of the mixed dispersion is adjusted to be acidic, and a dispersion stabilizer is added as necessary. At this time, the pH is adjusted to within the range of 2 to 5. Thereafter, the mixture is heated to the glass transition temperature of the resin particles, and the particles dispersed in the mixture are aggregated to form aggregated particles. At this time, the glass transition point is within the range of (glass transition point of resin particles - 30°C) to (glass transition point - 10°C).
[0193] In the aggregated particle formation step, for example, the mixed dispersion may be stirred with a rotary shear homogenizer, the above-mentioned aggregating agent may be added at room temperature (e.g., 25°C), the pH of the mixed dispersion may be adjusted to an acidic state (e.g., a pH in the range of 2 to 5), and a dispersion stabilizer may be added as necessary, followed by the above-mentioned heating.
[0194] (Flocculant) The flocculating agent may be, for example, a surfactant having a polarity opposite to that of the surfactant used as the dispersant added to the mixed dispersion. Examples of the above surfactant include inorganic metal salts and divalent or higher metal complexes. In particular, when a metal complex is used as the flocculant, the amount of surfactant used is reduced and the charging characteristics are improved.
[0195] If necessary, an additive that forms a complex with the metal ion of the flocculant or a similar bond with the metal ion may be used. As this additive, a chelating agent is preferably used.
[0196] Examples of inorganic metal salts include metal salts such as calcium chloride, calcium nitrate, barium chloride, magnesium chloride, zinc chloride, aluminum chloride, and aluminum sulfate, as well as inorganic metal salt polymers such as polyaluminum chloride, polyaluminum hydroxide, and calcium polysulfide.
[0197] As the chelating agent, a water-soluble chelating agent may be used. Examples of the chelating agent include oxycarboxylic acids such as tartaric acid, citric acid, and gluconic acid, iminodiacetic acid (IDA), nitrilotriacetic acid (NTA), and ethylenediaminetetraacetic acid (EDTA). The amount of the chelating agent added is preferably within a range of 0.01 to 5.0 parts by mass, and more preferably 0.1 or more parts by mass and less than 3.0 parts by mass, per 100 parts by mass of the resin particles.
[0198] (3) Fusion / unification process The fusion / coalescence process is a process in which the aggregated particle dispersion liquid in which the aggregated particles are dispersed is heated to fuse and coalesce the aggregated particles to form toner particles.
[0199] After the aggregated particle forming step, the aggregated particle dispersion liquid in which the aggregated particles are dispersed is heated, for example, to a temperature equal to or higher than the glass transition point of the resin particles to fuse and coalesce the aggregated particles, thereby forming toner particles.
[0200] Through the above steps, toner particles are obtained. After obtaining an aggregated particle dispersion in which aggregated particles are dispersed, the toner particles may be produced through a step of forming second aggregated particles and a step of fusing and coalescing the second aggregated particles to form toner particles having a core / shell structure. The step of forming the second aggregated particles is a step of further mixing the aggregated particle dispersion liquid with the resin particle dispersion liquid in which resin particles are dispersed, and aggregating the aggregated particles so that the resin particles are further attached to the surfaces of the aggregated particles.
[0201] In addition, the process of fusing and coalescing the second aggregate particles to form toner particles having a core / shell structure is a process of fusing and coalescing the second aggregate particles by heating the second aggregate particle dispersion liquid in which the second aggregate particles are dispersed, thereby forming toner particles having a core / shell structure.
[0202] After the fusion and coalescence process, the toner particles formed in the solution are subjected to a known washing process, solid-liquid separation process and drying process to obtain dry toner particles. In the washing step, it is preferable to thoroughly carry out replacement washing with ion-exchanged water in terms of electrostatic charge. The solid-liquid separation step is not particularly limited, but from the viewpoint of productivity, it is preferable to carry out suction filtration, pressure filtration, or the like. The drying step is not particularly limited to a particular method, but from the viewpoint of productivity, freeze drying, flash jet drying, fluidized bed drying, vibration type fluidized bed drying, etc. are preferably used.
[0203] In the present embodiment, after the toner particles are prepared, the toner particles may be subjected to an annealing treatment under predetermined temperature and heating time conditions. The toner according to the present embodiment is produced, for example, by adding external additives to the obtained toner particles in a dry state and mixing them.
[0204] The mixing may be carried out, for example, by using a V blender, a Henschel mixer, a Loedige mixer or the like. Furthermore, if necessary, a vibration separator or an air separator may be used to remove coarse particles from the toner.
[0205] <Crushing method> When preparing a toner by the pulverization method, first, the binder resin, wax, charge control agent, etc. contained in the toner particles are thoroughly mixed in a mixer such as a Henschel mixer or a ball mill to obtain a mixture. Here, it is preferable to select the binder resin so that the glass transition point of the toner to be prepared is in the range of 0 to 45°C. The toner particles may be magnetic toner particles, and may contain a magnetic material in addition to a binder resin, a wax, and a charge control agent.
[0206] Next, the resulting mixture is melt-kneaded using a thermal kneader such as a twin-screw kneading extruder, a heating roll, a kneader, or an extruder, and then cooled and solidified, followed by pulverization and classification to obtain toner particles. The toner can be produced by adding and mixing an external additive to the obtained toner particles.
[0207] Examples of mixers include the following: Henschel Mixer (manufactured by Mitsui Mining Co., Ltd.), Super Mixer (manufactured by Kawata Co., Ltd.), Ribocone (manufactured by Okawara Manufacturing Co., Ltd.), Nauta Mixer, Turbulizer, Cyclomix (manufactured by Hosokawa Micron Corporation), Spiral Pin Mixer (manufactured by Pacific Machinery Co., Ltd.), and Loedige Mixer (manufactured by Matsubo Co., Ltd.).
[0208] Examples of kneading machines include the following: KRC kneader (Kurimoto Iron Works); Buss-Co kneader (Buss); TEM type extruder (Toshiba Machine); TEX twin-screw kneader (Japan Steel Works); PCM kneader (Ikegai Iron Works); three-roll mill, mixing roll mill, kneader (Inoue Seisakusho); Kneadex (Mitsui Mining); MS-type pressure kneader, Niderruder (Moriyama Seisakusho); Banbury mixer (Kobe Steel, Ltd.).
[0209] Examples of pulverizers include the following: Counter Jet Mill, Micron Jet, Innomizer (manufactured by Hosokawa Micron Corporation); IDS type mill, PJM jet pulverizer (manufactured by Nippon Pneumatic Mfg. Co., Ltd.); Cross Jet Mill (manufactured by Kurimoto Iron Works Co., Ltd.); Urmax (manufactured by Nisso Engineering Co., Ltd.); SK Jet-O-Mill (manufactured by Seishin Enterprise Co., Ltd.); Cryptron (manufactured by Kawasaki Heavy Industries, Ltd.); Turbo Mill (manufactured by Turbo Industrial Co., Ltd.); Super Rotor (manufactured by Nisshin Engineering Co., Ltd.).
[0210] Examples of classifiers include the following: Classeal, Micron Classifier, and Spedic Classifier (manufactured by Seishin Enterprise Co., Ltd.); Turbo Classifier (manufactured by Nisshin Engineering Co., Ltd.); Micron Separator, Turboplex (ATP), and TSP Separator (manufactured by Hosokawa Micron Corporation); Elbow Jet (manufactured by Nittetsu Mining Co., Ltd.), Dispersion Separator (manufactured by Nippon Pneumatic Mfg. Co., Ltd.); and YM Microcut (manufactured by Yaskawa Shoji Co., Ltd.).
[0211] As a mixing processing device for mixing the external additives, a known mixing processing device such as the above mixer can be used.
[0212] Furthermore, if the pulverized toner is designed to be soft, it is necessary to harden its surface separately; therefore, one technology is to use fine particles such as silica with a uniform particle size distribution of around 110 nm, such as "X24," to fix and coat the surface of the pulverized toner.
[0213] The toner base particles thus produced can then be further treated with an external additive for the purpose of adding a fluidizing agent.
[0214] (Hot air surface treatment) The classified toner particles may be subjected to a heat treatment (spheronization) step. The heat treatment (spheroidization) can be performed by the method shown in JP-A-59-125743 or JP-A-2022-96557. The apparatus shown in JP-A-59-125743 performs the process as follows. The classified particles are subjected to a heat treatment, for example, by a heat treatment (spheronization) device shown in FIG. 5, in an ejector 501, toner particles 503 supplied from a hopper 502 are mixed with compressed air 505 from a nozzle 504 in a mixing chamber 506, and this mixed dispersed airflow 507 is ejected from a diffuser section 508 into a heat treatment chamber 509. Hot air 511 heated by a heater 510 is first introduced into a hot air swirling chamber 512 to be made into a swirling current, and then blown into the ejected dispersed airflow 507, where it is thermally associated or mixed uniformly with the dispersed airflow 507. Cooling air 513 is introduced from the upper part of the side wall of heat treatment chamber 509. The toner that has been made spherical in heat treatment chamber 509 is cooled by the cooling air, passes through discharge outlet 514, and is collected by cyclone 515 and dust collector 516.
[0215] <Suspension polymerization method> The method for producing toner particles by the suspension polymerization method includes a dissolving step in which these additives are uniformly dissolved or dispersed to form a polymerizable monomer composition, a granulation step in which this polymerizable monomer composition is dispersed in an aqueous medium containing a dispersion stabilizer using an appropriate stirrer and granulated, a polymerization reaction step in which an aromatic solvent and a polymerization initiator are added as necessary to carry out a polymerization reaction, a cooling step in which the location and size of microdomains of the crystalline material are controlled, and a holding (annealing) step in which the degree of crystallinity of the crystalline material is controlled, thereby obtaining toner particles having a desired particle size.
[0216] <Toner surface modification> The toner produced by the above-mentioned method can also be obtained by, for example, adhering fine particles to the core surface. The adhesion of particles to the core surface is achieved, for example, by uniformly mixing the core material with inorganic particles, electrostatically attaching the inorganic particles to the surface of the core material to create an ordered mixture, and then applying a mechanical and thermal impact force to drive the inorganic particles into the core material and fix them there.
[0217] The inorganic fine particles are not completely embedded in the core material, but are fixed so that a part of them protrudes from the core material. Such devices for fixing inorganic fine particles are commercially available as surface modification devices or systems, and examples thereof include the following.
[0218] (1) Dry mechanochemical method: Mechanochemical (Okada Seiko Co., Ltd.), Mechanofusion System (Hosokawa Micron Co., Ltd.) (2) High-velocity airflow impact method: Hybridization System (Nara Machinery Works, Ltd.), Cryptron System (Kawasaki Heavy Industries, Ltd.) (3) Wet method: Dispercoat (Nisshin Flour Milling Co., Ltd.), Coatmizer (Freund Corporation) (4) Heat treatment method: Surfusing (Nippon Pneumatic Mfg. Co., Ltd.) (5) Others: Spray dryer (Okawahara Chemical Engineering Co., Ltd.)
[0219] [Developer] The electrostatic image developer according to the present invention contains at least the electrostatic image developing toner according to the present invention. The electrostatic image developer may be a one-component developer containing only the toner for developing electrostatic images, or may be a two-component developer in which the toner for developing electrostatic images is mixed with a carrier.
[0220] (Career) One of the main roles of the carrier in a two-component developer is to agitate and mix with the toner in the developer box and give the toner the desired charge. Another role of the carrier is to act as an electrode between the developer and the photoreceptor, and to carry the charged toner to the electrostatic latent image on the photoreceptor, thereby forming a toner image.
[0221] The carrier is held on a magnet roller by, for example, magnetic force, and after acting on the development, it returns to the development box, where it is stirred and mixed again with new toner, and is used repeatedly for a certain period of time. Therefore, in order to stably maintain desired image characteristics (image density, fog, white spots, gradation, resolution, etc.), it is naturally required that the characteristics of the carrier be stable during the period of use.
[0222] The carrier is not particularly limited, and may be any known carrier, such as a coated carrier in which the surface of a core material made of conductive particles or magnetic powder is coated with a coating resin, a magnetic powder dispersion type carrier in which magnetic powder is dispersed and mixed in a matrix resin, and a resin impregnated type carrier in which porous magnetic powder is impregnated with a resin. The magnetic powder dispersion type carrier and the resin impregnated type carrier may be a carrier in which the constituent particles of the carrier are used as a core material and are coated with a coating resin.
[0223] Examples of the conductive particles include particles of metals such as gold, silver, and copper, carbon black, titanium oxide, zinc oxide, tin oxide, barium sulfate, aluminum borate, and potassium titanate. Examples of the magnetic powder include magnetic metals such as iron, nickel, and cobalt, and magnetic oxides such as ferrite and magnetite.
[0224] Examples of the coating resin and matrix resin include polyethylene, polypropylene, polystyrene, polyvinyl acetate, polyvinyl alcohol, polyvinyl butyral, polyvinyl chloride, polyvinyl ether, polyvinyl ketone, vinyl chloride-vinyl acetate copolymer, styrene-acrylic acid copolymer, straight silicone resin containing an organosiloxane bond or a modified product thereof, fluororesin, polyester, polycarbonate, phenolic resin, and epoxy resin.
[0225] The coating resin and the matrix resin may contain other additives such as conductive materials. Here, the surface of the core material can be coated with the coating resin by a method such as coating with a coating layer forming solution prepared by dissolving the coating resin and, if necessary, various additives in a suitable solvent.
[0226] The solvent is not particularly limited, and may be selected taking into consideration the coating resin to be used, the suitability for application, and the like.
[0227] Specific resin coating methods include an immersion method in which the core material is immersed in a solution for forming a coating layer, a spray method in which the solution for forming a coating layer is sprayed onto the surface of the core material, a fluidized bed method in which the solution for forming a coating layer is sprayed onto the core material while it is suspended in flowing air, and a kneader coater method in which the core material of a carrier and the solution for forming a coating layer are mixed in a kneader coater and the solvent is removed.
[0228] In the two-component developer, the mixing ratio (mass ratio) of the toner and the carrier is preferably toner:carrier=1:100 to 30:100, and more preferably 3:100 to 20:100.
[0229] 4. Image forming system The "image forming system" of the present invention refers to an assembly that is composed of devices or apparatuses having predetermined functions as means elements required for each step of image formation, toner for developing electrostatic images, etc., and performs the function of image formation as a whole. Note that each means element may be disposed separately in different locations, or may be disposed together in a certain space as one device and integrated into a system device. The present invention is particularly an image forming system including a photoreceptor having a photosensitive layer formed on an aluminum substrate, means for developing a latent image formed on the photoreceptor with a toner for developing electrostatic images, means for transferring the toner image on the photoreceptor to a transfer recipient, and a toner for developing electrostatic images, characterized in that the aluminum substrate contains silicon, the silicon content of the aluminum substrate is more than 0.6 mass %, and the glass transition point (Tg) of the toner for developing electrostatic images is within the range of 0 to 45°C.
[0230] The image forming system of the present invention is a system that forms an image using the photoconductor, the developing means, the transfer means, and the cleaning means, and the toner for developing an electrostatic image. In the following, for the sake of explanation, the device portion having the photoconductor, the developing means, the transfer means, and the cleaning means is particularly referred to as the "electrophotographic image forming device". The image forming system of the present invention is not limited to each of the means constituting the electrophotographic image forming device, so long as it is a system of a form or mode in which an image is formed using a photoconductor, a developing means, a transfer means, and a cleaning means formed on a support mainly composed of aluminum having a silicon content within the specific range, and a toner for developing an electrostatic image that satisfies the specific shape coefficient and particle size conditions of the toner particles. In other words, the device used in the present invention may be a device that satisfies the above conditions, and is not particularly limited, and it is not necessarily required to make it an electrophotographic image forming device dedicated to the toner for developing an electrostatic image that satisfies the above specific conditions of the present invention.
[0231] The image forming system of the present invention is also preferably provided with a means for recording and storing the recording and copying information as electronic data, and a means for wirelessly transmitting the electronic data. For example, it is also preferable that the image forming system has a wireless interface for transmitting and receiving data to and from an information processing unit via wireless communication such as Bluetooth (registered trademark) or Wi-Fi (registered trademark). A typical electrophotographic image forming apparatus that can be used in the present invention will be described below. Note that the electrophotographic image forming apparatus is also simply called an "image forming apparatus."
[0232] The image forming apparatus includes the photoconductor, a developing unit, a transfer unit, and a cleaning unit. The image forming apparatus preferably includes a charging unit (first charging unit) and an exposure unit. The image forming apparatus may further include a second charging unit between the transfer unit and the cleaning unit.
[0233] 6 is a schematic diagram showing an example of an image forming apparatus according to the present invention. The image forming apparatus 100 is called a tandem type color image forming apparatus. The image forming apparatus 100 includes four process cartridges 10Y, 10M, 10C, and 10Bk, an intermediate transfer unit 7, a paper feed means 21, a fixing means 24, and the like. An original image reading device SC is disposed on the upper portion of the apparatus main body A of the image forming apparatus 100.
[0234] The process cartridge 10Y, which forms a yellow image, has a first charging means 2Y, an exposure means 3Y, a developing means 4Y, a primary transfer roller 5Y, a second charging means 9Y, and a cleaning means 6Y, which are arranged in sequence around the drum-shaped photoreceptor 1Y in the direction of rotation of the photoreceptor 1Y.
[0235] The process cartridge 10M, which forms a magenta image, has a first charging means 2M, an exposure means 3M, a developing means 4M, a primary transfer roller 5M, a second charging means 9M and a cleaning means 6M, which are arranged in sequence around the drum-shaped photosensitive member 1M in the direction of rotation of the photosensitive member 1M.
[0236] The process cartridge 10C, which forms a cyan image, has a first charging means 2C, an exposure means 3C, a developing means 4C, a primary transfer roller 5C, a second charging means 9C and a cleaning means 6C, which are arranged in sequence around the drum-shaped photosensitive member 1C in the direction of rotation of the photosensitive member 1C.
[0237] The process cartridge 10Bk, which forms a black image, has a first charging means 2Bk, an exposure means 3Bk, a developing means 4Bk, a primary transfer roller 5Bk, a second charging means 9Bk and a cleaning means 6Bk, which are arranged in sequence around the drum-shaped photosensitive member 1Bk along the direction of rotation of the photosensitive member 1Bk.
[0238] As the photoreceptors 1Y, 1M, 1C, and 1Bk, the electrophotographic photoreceptor of the present invention described above is used.
[0239] The process cartridges 10Y, 10M, 10C, and 10Bk are configured similarly, except that the colors of the toner images formed on the photoconductors 1Y, 1M, 1C, and 1Bk are different. Therefore, the process cartridge 10Y will be described in detail as an example, and the description of the process cartridges 10M, 10C, and 10Bk will be omitted.
[0240] The process cartridge 10Y has a first charging means 2Y, an exposure means 3Y, a developing means 4Y, a primary transfer roller 5Y, a second charging means 9Y, and a cleaning means 6Y arranged around a photoconductor 1Y which is an image forming body, and forms a yellow (Y) toner image on the photoconductor 1Y. The process cartridge 10Y may be detachable from the image forming apparatus 100. In this embodiment, at least the photoconductor 1Y, the first charging means 2Y, the developing means 4Y, the second charging means 9Y, and the cleaning means 6Y of the process cartridge 10Y are integrally provided.
[0241] The first charging means 2Y is a means for applying a uniform potential to the photoconductor 1Y, and for example, a corona discharge type charger is used.
[0242] The exposure unit 3Y is a unit that performs exposure based on an image signal (yellow) on the photoconductor 1Y to which a uniform potential has been applied by the first charging unit 2Y, and forms an electrostatic latent image corresponding to the yellow image. As the exposure unit 3Y, for example, one composed of LEDs in which light emitting elements are arranged in an array in the axial direction of the photoconductor 1Y and an imaging element, or a laser optical system is used.
[0243] The developing means 4Y is, for example, a developing sleeve that has a magnet built in and rotates while holding the developer. and a voltage application device for applying a DC and / or AC bias voltage between the photoconductor 1Y and the developing sleeve.
[0244] The primary transfer roller 5Y is a means for transferring the toner image formed on the photoconductor 1Y to an endless belt-like intermediate transfer body 70. The primary transfer roller 5Y is disposed in contact with the intermediate transfer body 70.
[0245] The second charging means 9Y is a discharging means for charging (discharging) the surface of the photoreceptor 1Y after the toner image is transferred to the intermediate transfer body 70, and is provided as a pre-cleaning member. As the second charging means 9Y, for example, a corona discharge type charger is used.
[0246] The cleaning means 6Y is composed of a cleaning blade and a brush roller provided upstream of the cleaning blade.
[0247] The intermediate transfer unit 7 has an endless belt-like intermediate transfer body 70. The intermediate transfer body 70 is a semiconductive endless belt-like second image carrier that is wound around a plurality of rollers 71, 72, 73, and 74 and rotatably supported. In the intermediate transfer unit 7, a cleaning means 6b for removing toner from the intermediate transfer body 70 is disposed.
[0248] The process cartridges 10Y, 10M, 10C, and 10Bk and the intermediate transfer unit 7 constitute a housing 8. The housing 8 is configured so as to be capable of being pulled out from the apparatus main body A via support rails 82L and 82R.
[0249] The image forming apparatus 100 includes a secondary transfer roller 5b that transfers a color image formed on the intermediate transfer body 70 to a transfer material P. The paper feed unit 21 is a means for supplying the transfer material P to the secondary transfer roller 5b. The paper feed unit 21 includes a paper feed cassette 20 that stores the transfer material P, a plurality of intermediate rollers 22A, 22B, 22C, and 22D that transport the transfer material P to the secondary transfer roller 5b, and a registration roller 23.
[0250] The fixing means 24 is a means for fixing the color image transferred onto the transfer material P onto the transfer material P. An example of the fixing means 24 is a heat roller fixing type. For example, the fixing means 24 is composed of a heating roller having a heat source inside and a pressure roller that is provided in a state of being pressed against the heating roller so as to form a fixing nip portion. The image forming apparatus 100 has a paper discharge tray 26 for removing the transfer material P on which the image has been formed. The image forming apparatus 100 also includes a paper discharge roller 25 downstream of the fixing section 24 for transporting the transfer material P that has been subjected to the fixing process to the paper discharge tray 26.
[0251] In the above embodiment, the image forming apparatus 100 is a color laser printer, but is not limited to this. For example, the image forming apparatus may be a monochrome laser printer, a copier, a multifunction machine, etc. Furthermore, the exposure light source may be a light source other than a laser, such as an LED light source.
[0252] Using the above image forming apparatus, an image can be formed as follows. In the charging step (first charging step), the surfaces of the photoconductors 1Y, 1M, 1C, and 1Bk are discharged and negatively charged by the first charging means 2Y, 2M, 2C, and 2Bk.
[0253] In the exposure step, the surfaces of the photoconductors 1Y, 1M, 1C, and 1Bk are exposed to light by exposure means 3Y, 3M, 3C, and 3Bk based on image signals to form electrostatic latent images.
[0254] In the developing step, toner is applied to the surfaces of the photoconductors 1Y, 1M, 1C, and 1Bk by developing means 4Y, 4M, 4C, and 4Bk, respectively, to form toner images.
[0255] In the transfer process, the toner images of each color formed on the photoconductors 1Y, 1M, 1C, and 1Bk are sequentially transferred (primary transfer) onto the rotating intermediate transfer body 70 by the primary transfer rollers 5Y, 5M, 5C, and 5Bk. Then, a color image is formed on the intermediate transfer body 70.
[0256] In the second charging step, the surfaces of the photoconductors 1Y, 1M, 1C, and 1Bk are neutralized by the second charging means 9Y, 9M, 9C, and 9Bk.
[0257] In the cleaning process, the toner remaining on the surfaces of the photoconductors 1Y, 1M, 1C, and 1Bk is removed by cleaning means 6Y, 6M, 6C, and 6Bk. Then, in preparation for the next image forming process, the photoconductors 1Y, 1M, 1C, and 1Bk are negatively charged by charging means 2Y, 2M, 2C, and 2Bk.
[0258] Meanwhile, a transfer material P is fed from a paper feed cassette 20 by a paper feed means 21, and is transported to a secondary transfer roller 5b via a plurality of intermediate rollers 22A, 22B, 22C, 22D and a registration roller 23. Then, a color image is transferred (secondary transfer) onto the transfer material P by the secondary transfer roller 5b.
[0259] The transfer material P onto which the color image has been transferred in this manner is fixed by fixing means 24, and then is nipped by paper discharge rollers 25, discharged outside the apparatus, and placed on a paper discharge tray 26. In addition, after the transfer material P is separated from the intermediate transfer body 70, the remaining toner on the intermediate transfer body 70 is removed by cleaning means 6b. In this manner, an image can be formed on the transfer material P. EXAMPLES
[0260] The present invention will be specifically described below with reference to examples, but the present invention is not limited thereto. In the following examples, unless otherwise specified, the operations were performed at room temperature (25°C). Furthermore, unless otherwise specified, "%" and "parts" mean "% by mass" and "parts by mass", respectively.
[0261] <Preparation of photoreceptor 1> (1) Preparation of the photoreceptor substrate A support 1 (outer diameter φ 30 mm, length 360 mm) having the composition shown in Table I was prepared.
[0262] (2) Formation of the middle class The following materials were mixed and dispersed to prepare a coating solution for the intermediate layer. A sand mill was used as the dispersing machine, and dispersion was carried out in a batch manner for 10 hours. Polyamide resin 1.0 parts by weight Titanium oxide 1.1 parts by mass Ethanol 20 parts by weight The polyamide resin (resin binder) used was X1010 (manufactured by Daicel-Evonik Co., Ltd.). The titanium oxide (conductive particles) used was SMT500SAS (manufactured by Teika Co., Ltd.). The number average primary particle diameter of the titanium oxide was 0.035 μm. The coating solution was applied to the surface of the support by dip coating, and then dried in an oven at 110° C. for 20 minutes to form an intermediate layer having a thickness of 3 μm.
[0263] (3) Formation of the charge generating layer The following materials were mixed and dispersed using a circulation type ultrasonic homogenizer "RUS-600TCVP (manufactured by Nippon Seiki Seisakusho Co., Ltd.) to prepare a coating solution for the charge generating layer. The dispersion conditions were 19.5 kHz, 600 W, circulation flow rate 40 L / H, and 0.5 hours. Charge generating compound 24 parts by mass Polyvinyl butyral resin 12 parts by weight Mixed solvent 400 parts by weight The charge generating compounds used were titanyl phthalocyanine, which has clear peaks at 8.3°, 24.7°, 25.1°, and 26.5° in Cu-Kα characteristic X-ray diffraction spectrum measurement, and a mixed crystal of a 1:1 adduct of (2R,3R)-2,3-butanediol and unadducted titanyl phthalocyanine. The polyvinyl butyral resin used was S-LEC BL-1 (manufactured by Sekisui Chemical Co., Ltd., "S-LEC" is a registered trademark of the company). The mixed solvent used was 3-methyl-2-butanone:cyclohexanone = 4:1 (volume ratio). The coating liquid was applied to the surface of the intermediate layer by dip coating and then dried to form a charge generating layer having a thickness of 0.3 μm.
[0264] (4) Formation of the charge transport layer The following materials were mixed and dissolved to prepare a coating solution for the charge transport layer. Charge transporting compound (CTM-48) 75 parts by mass Polycarbonate 100 parts by weight Antioxidant 4 parts by weight The polycarbonate used was Z300 (Mitsubishi Gas Chemical Company, Inc., bisphenol Z-type polycarbonate). The antioxidant used was IRGANOX1010 (BASF, Inc., "IRGANOX" is a registered trademark of the company). The coating liquid was applied to the surface of the charge generating layer by dip coating, and then dried at 120° C. for 70 minutes to form a charge transport layer having a thickness of 24 μm.
[0265] <Preparation of photoreceptors 2 to 5> Photoreceptors 2 to 5 were prepared in the same manner as in the preparation of photoreceptor 1, except that the supports used were changed to supports 2 to 10, each having the composition shown in Table I below.
[0266] [Table 1]
[0267] <Preparation of Photoreceptor 6> In the preparation of the photoreceptor 1, a support 6 (outer diameter φ30 mm, length 360 mm) made of a titanium alloy (DAT5, manufactured by Daido Steel Co., Ltd.) having a higher resistance than an aluminum alloy was prepared as the support used. The rest of the support was prepared in the same manner as the photoreceptor 1.
[0268] <Toner Production> (Synthesis of amorphous polyester 1 (APEs-1)) Bisphenol A ethylene oxide adduct 30 parts by mass Bisphenol A propylene oxide adduct 270 parts by mass Terephthalic acid 60 parts by mass Fumaric acid 40 parts by mass Tetrapropenylsuccinic anhydride 40 parts by mass The monomer components were added to a reaction vessel equipped with a stirrer, a thermometer, a condenser, and a nitrogen gas inlet tube, and the inside of the reaction vessel was replaced with dry nitrogen gas. Then, tin dioctanoate was added in an amount of 0.3% based on the total amount of the monomer components. The temperature was raised to 235°C over 1 hour under a nitrogen gas stream, and the reaction was allowed to proceed for 3 hours. The pressure in the reaction vessel was reduced to 10.0 mmHg, and the reaction was allowed to proceed with stirring. When the desired molecular weight was reached, the reaction was terminated, and amorphous polyester 1 was obtained.
[0269] (Preparation of amorphous polyester dispersion 1) APEs-1 100 parts by mass Methyl ethyl ketone 60 parts by weight Isopropyl alcohol 10 parts by weight The above components were put into a reaction vessel equipped with a stirrer and dissolved at 60°C. After confirming dissolution, the reaction vessel was cooled to 35°C, and 3.5 parts of 10% aqueous ammonia solution was added. Then, 300 parts of ion-exchanged water was dropped into the reaction vessel over 3 hours to prepare a polyester dispersion. Then, methyl ethyl ketone and isopropyl alcohol were removed using an evaporator to obtain amorphous polyester dispersion 1.
[0270] (Synthesis of amorphous polyester 2 (APEs-2)) Amorphous polyester 2 was obtained in the same manner as in the synthesis of amorphous polyester 1, except that the following monomer components were added. Bisphenol A ethylene oxide adduct 210 parts by mass Bisphenol A propylene oxide adduct 230 parts by mass Terephthalic acid 30 parts by mass Fumaric acid 135 parts by mass Tetrapropenylsuccinic anhydride 40 parts by mass
[0271] (Preparation of amorphous polyester dispersion 2) Amorphous polyester dispersion 2 was prepared in the same manner as for amorphous polyester dispersion 1, except that the amorphous polyester used was APEs-2.
[0272] (Synthesis of amorphous polyester 3 (APEs-3)) Amorphous polyester 3 was obtained in the same manner as in the synthesis of amorphous polyester 1, except that the following monomer components were added. Ethylene glycol 106 parts by weight Dimethyl terephthalate 245 parts by mass 1,10-Decanedicarboxylic acid 105 parts by mass
[0273] (Preparation of amorphous polyester dispersion 3) Amorphous polyester dispersion 3 was prepared in the same manner as for amorphous polyester dispersion 1, except that the amorphous polyester used was APEs-3.
[0274] (Synthesis of amorphous polyester 4 (APEs-4)) Amorphous polyester 4 was obtained in the same manner as in the synthesis of amorphous polyester 1, except that the following monomer components were added. Bisphenol A ethylene oxide adduct 150 parts by mass Bisphenol A propylene oxide adduct 250 parts by mass Terephthalic acid 100 parts by mass Tetrapropenyl succinic anhydride 130 parts by mass Trimellitic acid 15 parts by mass
[0275] (Preparation of amorphous polyester dispersion 4) Amorphous polyester dispersion 4 was prepared in the same manner as for amorphous polyester dispersion 1, except that the amorphous polyester used was APEs-4.
[0276] (Synthesis of amorphous polyester 5 (APEs-5)) Amorphous polyester 5 was obtained in the same manner as in the synthesis of amorphous polyester 1, except that the following monomer components were added. Bisphenol A propylene oxide adduct 350 parts by mass Terephthalic acid 35 parts by mass Fumaric acid 90 parts by mass Tetrapropenylsuccinic anhydride 13 parts by mass
[0277] (Preparation of amorphous polyester dispersion 5) Amorphous polyester dispersion 5 was prepared in the same manner as for amorphous polyester dispersion 1, except that the amorphous polyester used was APEs-5.
[0278] (Synthesis of amorphous polyester 6 (APEs-6)) Fumaric acid 54.3 parts by mass Bisphenol A propylene oxide adduct (BPA-PO) 22.0 parts by mass Dipropanol 23.8 parts by mass Tin 2-ethylhexanoate (esterification catalyst) 0.5 parts by mass The above materials were weighed into a reaction vessel equipped with a condenser, stirrer, nitrogen inlet, and thermocouple. After the atmosphere in the reaction vessel was replaced with nitrogen gas, the temperature was gradually raised with stirring, and the reaction was carried out for 3 hours at a temperature of 140° C. with stirring. Next, the pressure in the reaction vessel was reduced to 8.3 kPa, and the temperature was raised to 200° C. with stirring, and the reaction was carried out for 4 hours. Thereafter, the pressure in the reaction vessel was reduced again to 5 kPa or less, and the reaction was carried out at 200° C. for 3 hours, thereby obtaining amorphous polyester 6.
[0279] (Preparation of amorphous polyester dispersion 6) Amorphous polyester dispersion 6 was prepared in the same manner as for amorphous polyester dispersion 1, except that the amorphous polyester used was APEs-6.
[0280] (Synthesis of amorphous polyester 7 (APEs-7)) The following raw material monomers for the vinyl polymerization segment (StAc segment) containing both reactive monomers and a radical polymerization initiator were placed in a dropping funnel. Styrene 80 parts by weight n-Butyl acrylate 20 parts by weight Acrylic acid 10 parts by mass Radical polymerization initiator (di-t-butyl peroxide) 16 parts by mass Furthermore, the raw material monomers for the amorphous polyester polymer segment (APEs segment) described below were placed in a four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, and were heated to 170° C. to dissolve. Bisphenol A propylene oxide dimer (BPA-PO) 228.6 parts by mass Bisphenol A ethylene oxide dimer (BPA-EO) 57.1 parts by mass Terephthalic acid 66.9 parts by mass Fumaric acid 47.4 parts by mass Next, the raw material monomers for the vinyl polymerization segment were added dropwise over 90 minutes while stirring, and the mixture was aged for 60 minutes, after which the unreacted raw material monomers for the vinyl polymerization segment were removed under reduced pressure (8 kPa). Thereafter, 0.4 parts by mass of Ti(On-Bu)4 was added as an esterification catalyst, the temperature was raised to 235°C, and the reaction was carried out at normal pressure (101.3 kPa) for 5 hours and then under reduced pressure (8 kPa) for 1 hour. Next, after cooling to 200° C., the reaction was carried out under reduced pressure (20 kPa) until the desired softening point was reached. Next, the solvent was removed to obtain amorphous polyester 7.
[0281] (Preparation of amorphous polyester dispersion 7) 100 parts by mass of the obtained amorphous polyester 7 was dissolved in 400 parts by mass of ethyl acetate (manufactured by Kanto Chemical Co., Ltd.), and further mixed with 638 parts by mass of a 0.26% by mass concentration sodium lauryl sulfate solution prepared in advance, and ultrasonically dispersed for 30 minutes at V-LEVEL 300 μA with stirring using an ultrasonic homogenizer "US-150T" (manufactured by Nippon Seiki Co., Ltd.). Thereafter, the mixture was heated to 40° C. and stirred under reduced pressure for 3 hours using a diaphragm vacuum pump “V-700” (manufactured by BUCHI) to completely remove ethyl acetate, thereby preparing amorphous polyester dispersion liquid 7.
[0282] (Synthesis of crystalline polyesters 1 (CPEs-1)) 1,10-Decanedicarboxylic acid 300 parts by mass Ethylene glycol 100 parts by mass The monomer components were charged into a reaction vessel equipped with a stirrer, a thermometer, a condenser, and a nitrogen gas inlet tube, and the atmosphere in the reaction vessel was replaced with dry nitrogen gas. Then, 0.3 parts by mass of tin dioctanoate was charged relative to 100 parts by mass of the monomer components. After stirring and reacting for 3 hours at 160°C under a nitrogen gas flow, the temperature was further increased to 180°C over 1.5 hours, and the pressure inside the reaction vessel was reduced to 3 kPa. The reaction was terminated when the desired molecular weight was reached, and crystalline polyester 1 was obtained.
[0283] (Preparation of Crystalline Polyester Dispersion 1) CPEs-1 100 parts by mass Methyl ethyl ketone 60 parts by weight Isopropyl alcohol 15 parts by weight The above components were placed in a reaction vessel equipped with a stirrer and dissolved at 65° C. After confirming dissolution, the reaction vessel was cooled to 60° C., and 5 parts by mass of a 10% aqueous ammonia solution was added. Next, 300 parts of ion-exchanged water was dropped into the reaction vessel over a period of 3 hours to prepare a polyester dispersion liquid. Next, methyl ethyl ketone and isopropyl alcohol were removed using an evaporator to obtain a crystalline polyester dispersion liquid 1.
[0284] (Synthesis of crystalline polyester 2 (CPEs-2)) Crystalline polyester 2 was obtained in the same manner as in the synthesis of crystalline polyester 1, except that the following monomer components were added. 1,10-Decanedicarboxylic acid 350 parts by mass 1,6-Hexanediol 170 parts by mass
[0285] (Preparation of Crystalline Polyester Dispersion 2) Crystalline polyester dispersion 2 was prepared in the same manner as for crystalline polyester dispersion 1, except that the crystalline polyester used was CPEs-2.
[0286] (Synthesis of crystalline polyester 3 (CPEs-3)) Crystalline polyester 3 was obtained in the same manner as in the synthesis of crystalline polyester 1, except that the following monomer components were added. 1,10-Decanedicarboxylic acid 350 parts by mass 1,9-nonanediol 240 parts by mass
[0287] (Preparation of Crystalline Polyester Dispersion 3) Crystalline polyester dispersion 3 was prepared in the same manner as for crystalline polyester dispersion 1, except that the crystalline polyester used was CPEs-3.
[0288] (Synthesis of crystalline polyester 4) The raw material monomers for the vinyl polymerization segment (styrene-acrylic polymerization segment, StAc segment) containing both reactive monomers and a radical polymerization initiator were placed in the dropping funnel. n-Butyl acrylate 12 parts by weight Acrylic acid 2 parts by mass Radical polymerization initiator (di-t-butyl peroxide) 7 parts by mass Furthermore, the raw material monomers for the crystalline polyester polymer segment (CPEs segment) described below were placed in a four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer, and a thermocouple, and were heated to 170° C. to dissolve. Ethylene glycol 106 parts by weight Dimethyl terephthalate 245 parts by mass 1,10-Decanedicarboxylic acid 105 parts by mass Next, the raw material monomers for the vinyl polymerization segment were added dropwise over 90 minutes under stirring, and the mixture was aged for 60 minutes. After that, the unreacted raw material monomers for the vinyl polymerization segment were removed under reduced pressure (8 kPa). The amount of the monomers removed was very small compared to the amount of the monomers for the vinyl polymerization segment. Thereafter, 0.8 parts by mass of Ti(On-Bu)4 was added as an esterification catalyst, the temperature was raised to 235°C, and the reaction was carried out at normal pressure (101.3 kPa) for 5 hours, and further at reduced pressure (8 kPa) for 1 hour. Next, after cooling to 200° C., the mixture was reacted for 1 hour under reduced pressure (20 kPa) to obtain Crystalline Polyester 4, which is a hybrid crystalline polyester.
[0289] (Preparation of Crystalline Polyester Dispersion 4) 30 parts by mass of the above crystalline polyester 4 was melted and transferred in the molten state to an emulsifying and dispersing machine "Cavitron CD1010" (manufactured by Eurotech Co., Ltd.) at a transfer rate of 100 parts by mass per minute. Simultaneously with the transfer of the molten crystalline polyester, dilute ammonia water having a concentration of 0.37% by mass, prepared by diluting 70 parts by mass of reagent ammonia water with ion-exchanged water in a separate aqueous solvent tank, was transferred to the emulsifying and dispersing machine "Cavitron CD1010" (manufactured by Eurotech Co., Ltd.) at a transfer rate of 0.1 liters per minute while being heated to 100°C by a heat exchanger. The emulsion dispersion machine was then operated at a rotor speed of 60Hz and a pressure of 5kg / cm 2 By operating under the above conditions, a crystalline polyester dispersion 4 was prepared.
[0290] (Preparation of styrene-acrylic copolymer resin dispersion 1) Styrene 126 parts by weight n-Butyl acrylate 14 parts by weight Dodecanethiol 2.1 parts by mass Isopropyl alcohol 0.88 parts by weight Anionic surfactant (Dowfax, manufactured by The Dow Chemical Company) 4 parts by weight Ion-exchanged water 59.2 parts by weight The above ingredients were placed in a container and emulsified using a homogenizer to prepare monomer emulsion A.
[0291] Meanwhile, the following components were charged into a polymerization reaction vessel, a reflux condenser was installed, and the mixture was slowly stirred while injecting nitrogen, and the polymerization flask was heated in a water bath to 75° C. and maintained at that temperature. 10 parts by mass of the monomer emulsion A was added dropwise to the vessel over a period of 10 minutes using a metering pump. Ion-exchanged water 133 parts by weight Anionic surfactant (Dowfax, manufactured by The Dow Chemical Company) 0.6 parts by mass Next, 1.05 parts of ammonium persulfate was dissolved in 10 parts of ion-exchanged water, and the solution was added dropwise to the polymerization flask over 10 minutes using a metering pump. Stirring was continued for 1 hour in this state. Further, the remaining monomer emulsion A was added dropwise over a period of 2 hours using a metering pump. After the addition was completed, stirring was continued for another 3 hours to obtain a styrene-acrylic copolymer resin dispersion 1 containing a styrene-acrylic copolymer resin (St / Ac1).
[0292] (Preparation of styrene-acrylic copolymer resin dispersion 2) (a) First-stage polymerization (preparation of dispersion of vinyl resin particles [d1]) A 5 L reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, and a nitrogen introduction device was charged with 8 parts by mass of sodium dodecyl sulfate and 3,000 parts by mass of ion-exchanged water. Then, while stirring at a speed of 230 rpm under a nitrogen stream, the internal temperature was raised to 80° C. After the temperature was raised, a solution in which 10 parts by mass of potassium persulfate was dissolved in 200 parts by mass of ion-exchanged water was added, and the liquid temperature was raised to 80° C. again, and the following mixed monomer liquid was added dropwise over 1 hour. n-Butyl acrylate 396 parts by weight Methacrylic acid 604 parts by mass After the dropwise addition, polymerization was carried out by heating and stirring at 80° C. for 2 hours to prepare a dispersion liquid of vinyl resin particles [d1].
[0293] (b) Second stage polymerization A solution of 7 parts by mass of sodium dodecyl sulfate dissolved in 3,000 parts by mass of ion-exchanged water was charged into a 5 L reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, and a nitrogen introducing device, and heated to 98° C. After heating, 300 parts by mass, calculated as solid content, of the dispersion of vinyl resin particles [d1] prepared by the above first-stage polymerization and a mixed solution of the following monomers, chain transfer agent, and release agent dissolved at 90° C. were added thereto. 2-Ethylhexyl acrylate 90.5 parts by mass Methacrylic acid 33.1 parts by mass n-Octyl mercaptan (chain transfer agent) 5.5 parts by mass Behenyl behenate (release agent, melting point 73°C) 130.0 parts by mass A mixing and dispersion process was carried out for 1 hour using a mechanical disperser CLEARMIX (manufactured by M-Technique Co., Ltd.) with a circulation path to prepare a dispersion containing emulsified particles (oil droplets). A polymerization initiator solution of 6 parts by mass of potassium persulfate dissolved in 200 parts by mass of ion-exchanged water was added to this dispersion. This system was heated and stirred at 78°C for 1 hour to polymerize, preparing a dispersion of vinyl resin particles [d2].
[0294] (c) Third stage polymerization 400 parts by mass of ion-exchanged water was further added to the dispersion of vinyl resin particles [d2] obtained by the second-stage polymerization and mixed thoroughly. Then, a solution of 6.0 parts by mass of potassium persulfate dissolved in 400 parts by mass of ion-exchanged water was added. Furthermore, a mixture of the following monomers and chain transfer agent was added dropwise over 1 hour at a temperature of 81°C. n-Butyl acrylate 143.2 parts by mass Methacrylic acid 200.5 parts by mass n-Octyl mercaptan (chain transfer agent) 8.0 parts by mass After the dropwise addition was completed, polymerization was carried out by heating and stirring for 2 hours, and then cooling to 28° C., whereby a styrene-acrylic copolymer resin dispersion 2 was obtained.
[0295] (Preparation of styrene-acrylic copolymer resin dispersion 3) (a) First stage polymerization An anionic surfactant solution in which 2.0 parts by mass of the anionic surfactant "sodium lauryl sulfate" was dissolved in 2900 parts by mass of ion-exchanged water was charged in a reaction vessel equipped with a stirrer, a temperature sensor, a temperature controller, a cooling tube, and a nitrogen introducing device. The internal temperature was raised to 80°C while stirring at a stirring speed of 230 rpm under a nitrogen stream. To this surfactant solution, 9.0 parts by mass of a polymerization initiator "potassium persulfate: KPS" was added, and the internal temperature was increased to 78° C. Thereafter, solution (1) having the following composition was added dropwise over a period of 3 hours. After the dropwise addition was completed, polymerization (first stage polymerization) was carried out by heating and stirring at 78° C. for 1 hour, to prepare a “dispersion of resin particles [a1]”. Composition of solution (1): Styrene 540 parts by weight n-Butyl acrylate 270 parts by weight Methacrylic acid 65 parts by mass n-Octyl mercaptan 17 parts by mass
[0296] (b) Second-stage polymerization: formation of the intermediate layer In a flask equipped with a stirrer, 55 parts by mass of paraffin wax (melting point: 73°C) as a release agent was added to a solution (2)) consisting of the following composition, and the solution was heated to 85°C to dissolve the mixture, thereby preparing a monomer solution [2]. Composition of solution (2): Styrene 94 parts by weight n-Butyl acrylate 60 parts by weight Methacrylic acid 11 parts by weight n-Octyl mercaptan 5 parts by mass Meanwhile, a surfactant solution in which 2 parts by mass of the anionic surfactant "sodium lauryl sulfate" was dissolved in 1,100 parts by mass of ion-exchanged water was heated to 90°C. 28 parts by mass of "dispersion of resin particles [a1]" was added to this surfactant solution, calculated as the solid content of the resin particles [a1]. After that, the monomer solution [2] was mixed and dispersed for 4 hours using a mechanical disperser "Clearmix" (manufactured by M Technique Co., Ltd.) with a circulation path, to prepare a dispersion containing emulsified particles with a dispersed particle diameter of 350 nm. To this dispersion, an aqueous initiator solution prepared by dissolving 2.5 parts by mass of a polymerization initiator "KPS" in 110 parts by mass of ion-exchanged water was added, and the system was heated and stirred at 90°C for 2 hours. In this way, polymerization (second-stage polymerization) was carried out to prepare a "dispersion of resin particles [a11]".
[0297] (c) Third-stage polymerization: formation of the outer layer To the above-mentioned "dispersion liquid of resin particles [a11]", an aqueous initiator solution prepared by dissolving 2.5 parts by mass of a polymerization initiator "KPS" in 110 parts by mass of ion-exchanged water was added, and a solution (3) having the following composition was added dropwise over a period of 1 hour under a temperature condition of 80°C. Composition of solution (3): Styrene 230 parts by weight n-Butyl acrylate 100 parts by mass n-Octyl mercaptan 5.2 parts by mass After the dropwise addition was completed, polymerization (third-stage polymerization) was carried out by heating and stirring for 3 hours, followed by cooling to 28° C. to prepare styrene-acrylic copolymer resin dispersion 3.
[0298] (Preparation of release agent dispersion) Hydrocarbon wax (manufactured by Nippon Seiro Co., Ltd., product name: FNP0090, melting temperature Tw = 90.2 ° C.) 270 parts by mass Anionic surfactant (Teika Power BN2060, manufactured by Teika Corporation, active ingredient amount: 60%) 13.5 parts by mass (as an active ingredient, 3.0% relative to the release agent) Ion-exchanged water 700 parts by weight The above components were mixed, and the release agent was dissolved in a pressure discharge homogenizer (Gaulin homogenizer, manufactured by Gaulin Co., Ltd.) at an internal liquid temperature of 120°C. After that, the mixture was dispersed at a dispersion pressure of 5 MPa for 120 minutes, then at 40 MPa for 360 minutes, and cooled to obtain a release agent dispersion. The volume average particle size D50v of the particles in this release agent dispersion was 220 nm. Ion-exchanged water was then added to adjust the solid content concentration to 20.0%.
[0299] (Preparation of Black Colorant Dispersion 1) Carbon black (REGAL330, manufactured by Cabot Japan Co., Ltd.) 200 parts by mass Anionic surfactant (Dai-ichi Kogyo Seiyaku Co., Ltd., Neogen SC) 33 parts by weight (60% active ingredient, 10% colorant) Ion-exchanged water 750 parts by weight The above components were placed in a stainless steel container that was large enough that the liquid level would be 1 / 3 of the container's height when all of the above components were placed in, and 280 parts of ion-exchanged water and an anionic surfactant were added to thoroughly dissolve the surfactant. Then, all of the pigment was placed in and stirred with a stirrer until there was no unwetted pigment. The remaining ion-exchanged water was then added, and the mixture was further stirred to thoroughly defoam it. After defoaming, the mixture was dispersed at 5,000 rpm for 10 minutes using a homogenizer (IKA Ultra Turrax T50), then stirred overnight with a stirrer for defoaming. After defoaming, the mixture was dispersed again at 6,000 rpm for 10 minutes using a homogenizer, then stirred overnight with a stirrer for defoaming. After degassing, the mixture was dispersed at a pressure of 240 MPa using a high-pressure impact disperser, Ultimizer (HJP30006, manufactured by Sugino Machine Co., Ltd.) The dispersion was performed for 25 passes, calculated based on the total amount charged and the processing capacity of the device. The obtained dispersion was left to stand for 72 hours to remove precipitates, and ion-exchanged water was added to adjust the solid concentration to 15%, to obtain black colorant dispersion 1. The volume average particle size D50v of the particles in this colorant dispersion was 110 nm.
[0300] (Preparation of Black Colorant Dispersion 2) 90 parts by mass of sodium dodecyl sulfate was dissolved in 1600 parts by mass of ion-exchanged water with stirring. While stirring this solution, 420 parts by mass of carbon black "Regal 330R" (manufactured by Cabot Corporation) was gradually added. Next, a dispersion treatment was performed using a stirring device "Clearmix" (manufactured by M Technique Co., Ltd.) to obtain black colorant dispersion 2. The volume average particle diameter D50v of the particles in this colorant dispersion was 110 nm.
[0301] <Preparation of toner base particles 1> Each dispersion was weighed out so as to obtain the following composition as the core of the toner base particle. The "parts by mass" in the following dispersions indicates the number of parts by mass of solids. The toner composition shown in Table II below indicates the respective contents (mass%) of APEs (amorphous polyester), CPEs (crystalline polyester) and St / Ac (styrene-acrylic resin) when the total mass of APEs (amorphous polyester), CPEs (crystalline polyester) and St / Ac (styrene-acrylic resin) is taken as 100 mass%. (First APEs) APEs-1 23 parts by mass (Second APEs) APEs-2 23 parts by mass CPEs-1 20 parts by mass St / Ac1 4 parts by mass Black colorant dispersion 1 6.5 parts by weight Release agent 1.5 parts by weight After each dispersion was poured into a round stainless steel flask, ion-exchanged water was added so that the solid content concentration was 12.5% by mass, and 6.3 parts by mass of a 10% aqueous solution of aluminum sulfate was further poured in. Next, the mixture was mixed and dispersed for 10 minutes at 5000 rpm using a homogenizer (Ultra Turrax T50, manufactured by IKA). After that, the contents in the flask were heated and stirred to 40°C, and thereafter, the temperature was raised at a rate of 0.5°C per minute, and the temperature was maintained when the particle size reached 6.1 μm. On the other hand, as the shell portion of the toner base particles, each dispersion liquid was weighed so as to have the following composition, and the mixed dispersion liquid was added and held for 60 minutes. APEs-5 10 parts by mass APEs-6 9 parts by mass Release agent 3 parts by weight Observation of the resulting contents with an optical microscope confirmed the formation of aggregated particles. 11 parts by mass of tetrasodium ethylenediaminetetraacetic acid (EDTA) (Chilest Co., Ltd., Chelest 40) was added. Then, an aqueous sodium hydroxide solution was added to adjust the pH to 8. Next, the temperature was raised to 82.5°C, and the pH was lowered by 0.05 every 10 minutes with nitric acid, and stirring was continued for 45 minutes. After cooling, the mixture was filtered, thoroughly washed with ion-exchanged water, and dried to obtain toner base particles 1.
[0302] <Preparation of toner base particles 2> Each dispersion was weighed out so as to obtain the following composition as the core portion of the toner base particle. (First APEs) APEs-3 47 parts by mass (Second APEs) None CPEs-1 22 parts by mass St / Ac1 None Black colorant dispersion 1 6.5 parts by weight Release agent 1.5 parts by weight On the other hand, toner base particles 2 were obtained in the same manner as toner base particles 1, except that the respective dispersion liquids were weighed out so as to obtain the following composition as the shell portion of the toner base particles. APEs-5 10 parts by mass APEs-6 10 parts by mass Release agent 3 parts by weight
[0303] <Preparation of toner base particles 3> Each dispersion was weighed out so as to obtain the following composition as the core portion of the toner base particle. (First APEs) APEs-4 26 parts by mass (Second APEs) APEs-5 26 parts by mass CPEs-2 19 parts by mass St / Ac1 None Black colorant dispersion 1 6.5 parts by weight Release agent 1.5 parts by weight On the other hand, toner base particles 3 were obtained in the same manner as toner base particles 1, except that the respective dispersion liquids were weighed so as to obtain the following composition as the shell portion of the toner base particles. APEs-5 9 parts by mass APEs-6 9 parts by mass Release agent 3 parts by weight
[0304] <Preparation of Toner Base Particles 7> Each dispersion was weighed out so as to obtain the following composition as the core portion of the toner base particle. (First APEs) APEs-3 47 parts by mass (Second APEs) None CPEs-1 22.5 parts by mass St / Ac1 None Black colorant dispersion 1 6.5 parts by weight Release agent 1.5 parts by weight On the other hand, toner base particle 7 was obtained in the same manner as toner base particle 1, except that each dispersion was weighed so as to obtain the following composition as the shell portion of the toner base particle. APEs-5 10 parts by mass APEs-6 10 parts by mass Release agent 3 parts by weight
[0305] <Preparation of toner base particles 8> Each dispersion was weighed out so as to obtain the following composition as the core portion of the toner base particle. (First APEs) APEs-4 26 parts by mass (Second APEs) APEs-5 26 parts by mass CPEs-2 16 parts by mass St / Ac1 None Black colorant dispersion 1 6.5 parts by weight Release agent 1.5 parts by weight On the other hand, toner base particle 8 was obtained in the same manner as toner base particle 1, except that each dispersion was weighed so as to obtain the following composition as the shell portion of the toner base particle. APEs-5 9 parts by mass APEs-6 9 parts by mass Release agent 3 parts by weight
[0306] <Preparation of Toner Base Particle 4> (Synthesis of amorphous polyester) Terephthalic acid 55.6 parts by mass Bisphenol A propylene oxide adduct (BPA-PO) 28.8 parts by mass Propanediol 15.5 parts by mass Tin 2-ethylhexanoate (esterification catalyst) 0.50 parts by mass The above materials were put into a reaction vessel equipped with a cooling tube, a stirrer, a nitrogen inlet tube, and a thermocouple. The atmosphere in the reaction vessel was then replaced with nitrogen gas, and the temperature was gradually raised while stirring. The above materials were reacted for 3 hours at a temperature of 140°C while stirring. Next, the pressure in the reaction vessel was reduced to 8.3 kPa, and the temperature was raised to 200° C. with stirring, and the reaction was carried out for 4 hours. Thereafter, the pressure in the reaction vessel was reduced again to 5 kPa or less, and the reaction was carried out at 200° C. for 3 hours, to obtain an amorphous polyester as a binder resin. Amorphous polyester 89 parts by weight Hydrocarbon wax (Fischer-Tropsch wax) 4.5 parts by weight Carbon black (REGAL330, manufactured by Cabot Japan Co., Ltd.) 6.5 parts by mass The above materials were mixed in a Henschel mixer (FM-75, manufactured by Mitsui Mining Co., Ltd.) at a rotation speed of 20 s. -1 The mixture was mixed with rotation for 5 minutes. The mixture was then kneaded in a twin-screw kneader (PCM-30, manufactured by Ikegai Corporation) set at a temperature of 150°C. The kneaded mixture was cooled and coarsely crushed to 1 mm or less using a hammer mill to obtain a coarsely crushed product. The coarsely crushed product was finely crushed using a mechanical crusher (T-250, manufactured by Turbo Kogyo Co., Ltd.). Furthermore, classification was performed using Faculty F-300 (manufactured by Hosokawa Micron Corporation). The operating conditions for Faculty F-300 were a classification rotor rotation speed of 130 s -1 It was decided. The classified particles were subjected to heat treatment using the surface treatment device shown in Figure 5. The operating conditions were feed rate = 3 kg / hr, hot air temperature = 150°C, hot air flow rate = 6 m 3 / min, cold air temperature = -5℃, cold air flow rate = 4m 3 / min, Blower air volume = 20m 3 / min, injection air flow rate = 1m 3 By carrying out the heat treatment, toner base particles 4 having an average particle size of 6.50 μm, an average shape factor of 0.945, and a fine powder content of 17% were obtained.
[0307] <Preparation of Toner Base Particles 5> The following materials and 2000 parts by mass of ion-exchanged water were placed in a reaction vessel equipped with a stirrer, a temperature sensor, and a cooling tube, and then a 5 mol / L aqueous sodium hydroxide solution was added to adjust the pH to 10 (25°C). Styrene-acrylic copolymer resin dispersion 2 285 parts by mass (solid content) Crystalline polyester dispersion 4 40 parts by weight (solid content) Dodecyl diphenyl ether disulfonic acid sodium salt (1% by mass (solid content equivalent) based on the total amount of vinyl resin and crystalline polyester) Then, 25.1 parts by mass (solid content equivalent) of the black colorant dispersion 2 was added. Next, an aqueous solution prepared by dissolving 60 parts by mass of magnesium chloride in 60 parts by mass of ion-exchanged water was added thereto at 30° C. over a period of 10 minutes with stirring. After that, the mixture was left for 3 minutes, and then the temperature was increased, and the system was heated to 80°C over 60 minutes. After reaching 80°C, the stirring speed was adjusted so that the particle size growth rate was 0.01 μm / min, while the particle size of the associated particles was measured using a Coulter Multisizer 3 (manufactured by Beckman Coulter, Inc.), and the particles were allowed to grow until the volume-based median diameter was 6.1 μm. Thereafter, 737 parts by mass (solid content equivalent) of amorphous polyester dispersion was added over 30 minutes, and when the supernatant of the reaction solution became transparent, an aqueous solution of 190 parts by mass of sodium chloride dissolved in 760 parts by mass of ion-exchanged water was added to stop particle growth. The temperature was then raised, and the mixture was heated and stirred at 80°C to promote particle fusion. The average circularity of the toner was measured (HPF detection number: 4000) using an average circularity measuring device for toner "FPIA-3000" (manufactured by Sysmex Corporation), and when the average circularity reached 0.970, the mixture was cooled to 30°C at a cooling rate of 2.5°C / min. Next, the toner cake was subjected to solid-liquid separation, and the dehydrated toner cake was washed by repeating the operation of redispersing the toner cake in ion-exchanged water and separating the solid and liquid three times. Thereafter, the toner cake was dried at 40° C. for 24 hours to obtain toner base particles 5.
[0308] <Preparation of Toner Base Particles 6> Into a reaction vessel equipped with a stirrer, a temperature sensor, and a cooling tube, 93.5 parts by mass in terms of solid content of styrene-acrylic copolymer resin dispersion 3, 6.5 parts by mass in terms of solid content of black colorant dispersion 2, and 700 parts by mass of ion-exchanged water were charged. Then, a 5 mol / L aqueous sodium hydroxide solution was added to adjust the pH to 10 at 25°C. Next, an aqueous solution prepared by dissolving 60 parts by mass of magnesium chloride in 60 parts by mass of ion-exchanged water was added thereto at 30° C. over a period of 10 minutes with stirring. After that, after leaving it for 3 minutes, the temperature was increased, and the system was heated to 80° C. over 60 minutes, and the particle growth reaction was continued while maintaining the temperature at 80° C. In this state, the particle size of the associated particles was measured using a Coulter Multisizer 3 (manufactured by Coulter Beckman Inc.), and when the volume-based median diameter (D50) reached 6.1 μm, an aqueous solution in which 190 parts by mass of sodium chloride was dissolved in 760 parts by mass of ion-exchanged water was added to stop the particle growth. The temperature was then raised and the particles were stirred at 90° C. to promote fusion of the particles. The particles were then cooled to 30° C. when the average circularity of the toner reached 0.945 (HPF detection count: 4,000 particles) using an average circularity measuring device "FPIA-2100" (Sysmex Corporation). The obtained toner base particle dispersion liquid 1 was subjected to solid-liquid separation using a centrifuge to form a wet cake of toner base particles. The wet cake was washed with ion-exchanged water at 35°C until the electrical conductivity of the filtrate from the centrifuge reached 5 μS / cm. The wet cake was then transferred to a "Flash Jet Dryer" (manufactured by Seishin Enterprise Co., Ltd.) and dried until the moisture content reached 0.5% by mass to produce toner base particles 6.
[0309] <Preparation of Toner 1> 100 parts by mass of toner base particles 1 and hydrophobic silica particles (BET: 200m) hydrophobized with hexamethyldisilazane 2 / g) 1.0 mass part, and titanium oxide fine particles surface-treated with isobutyltrimethoxysilane (BET: 80m 2 1.0 part by mass of 1 / g of strontium titanate and 0.5 parts by mass of strontium titanate 1 were mixed in a Henschel mixer (FM-75, manufactured by Mitsui Miike Chemical Engineering Co., Ltd.) at a rotation speed of 30 s. -1 The mixture was mixed at 10 minutes rotation time to obtain toner 1.
[0310] <Preparation of Toners 2 to 8> Toners 2 to 8 were prepared in the same manner as in the preparation of toner 1, except that toner base particle 1 was replaced with toner base particle 2 to 8, respectively.
[0311] <Glass transition temperature> For the obtained toners 1 to 8, the glass transition points were determined from the DSC curves obtained by differential scanning calorimetry (DSC) as described above.
[0312] [evaluation] (Transferability in high temperature and humidity environments) As the electrophotographic image forming apparatus for evaluation, a commercially available electrophotographic image forming apparatus "AccurioPress C4080" (manufactured by Konica Minolta, Inc.) was used. In a printing environment of high temperature and humidity (30℃, 80%RH), 20,000 copies of a 2% character chart were made. After that, the maximum image density was measured on A4-size wood-free paper (65g / m 2 A solid image was printed on the paper and the relative reflection density was measured using a densitometer "RD-918" (manufactured by Macbeth Co., Ltd.) based on the white paper density. A measured relative reflection density of 1.20 or more was deemed to be acceptable.
[0313] (Low temperature fixability) To evaluate the low-temperature fixing ability, the fixing device of each of the actual machines used in the actual printing was modified so that the fixing temperature was controlled to "normal temperature -30°C." In addition, Konica Minolta J paper was used as a recording medium, and a solid image (25 mm×25 mm) was formed and fixed. After printing 5,000 sheets, the image surface of the fixed image was folded in a valley and the degree of peeling of the image at the fold was observed. The width of the paper that appeared at the fold as a result of the image peeling was measured. A width of 1.0 mm or less was considered to be acceptable.
[0314] [Table 2]
[0315] [Table 3]
[0316] As shown by the above results, it is apparent that the image forming method of the present invention is superior in both transferability and low-temperature fixability to the image forming method of the comparative example. [Explanation of symbols]
[0317] 101 Support 102 Middle Class 102 Middle Class 103 Charge generating layer 104 Charge transport layer 105 Surface protective layer 10 Developing roller 11 Developing sleeve 12 Magnet Roller 16 Shaft 17 Bearings 18 First flange 18a Shaft 18b Recess 19 Second flange 501 Ejector 502 Hopper 503 Toner particles 504 Nozzle 505 Compressed Air 506 Mixing room 507 Mixed and dispersed airflow 508 Diffuser 509 Heat Treatment Room 510 Heater 511 Hot air 512 Hot air swirling room 513 Cooling air 514 Outlet 515 Cyclone 516 Dust collector 100 Image forming device 1, 1Y, 1M, 1C, 1Bk photoconductor 2Y, 2M, 2C, 2Bk 1st charging means 3Y, 3M, 3C, 3Bk exposure method 4Y, 4M, 4C, 4Bk developing means 5Y, 5M, 5C, 5Bk Primary transfer roller 5b Secondary transfer roller 6Y, 6M, 6C, 6Bk, 6b Cleaning means 7 Intermediate transfer unit 8. Cabinet 9Y, 9M, 9C, 9Bk Second charging means 10Y, 10M, 10C, 10Bk process cartridges 21 Paper feeding means 20 Paper feed cassette 22A, 22B, 22C, 22D Intermediate rollers 23 Resist Roller 24 Fixing Method 25 Paper ejection roller 26 Output tray 70 Intermediate transfer body 71, 72, 73, 74 Roller 82L, 82R Support rails P Transfer material
Claims
1. An image forming method using a photoconductor using at least an aluminum substrate, a toner for developing an electrostatic image, the toner including toner particles containing at least a binder resin, and a developer carrier having a member for generating magnetic flux therein, The aluminum substrate contains silicon, The silicon content of the aluminum substrate is greater than 0.6% by mass, and The glass transition point (Tg) of the electrostatic image developing toner is within the range of 0 to 45° C.
1. An image forming method comprising:
2. The main component of the binder resin contained in the toner particles is polyester.
2. The image forming method according to claim 1.
3. The silicon content of the aluminum substrate is more than 0.6 mass% and not more than 20 mass%.
3. The image forming method according to claim 1 or 2.
4. a photoreceptor using at least an aluminum substrate; a means for developing the latent image formed on the photoreceptor with a toner for developing an electrostatic image; A means for transferring the toner image on the photoreceptor to a transfer medium; and an image forming system including the toner for developing an electrostatic image, The aluminum substrate contains silicon, The silicon content of the aluminum substrate is greater than 0.6% by mass, and The glass transition point (Tg) of the electrostatic image developing toner is within the range of 0 to 45° C.
1. An image forming system comprising:
Citation Information
Patent Citations
Toner for electrostatic charge image development, method for manufacturing the same, and electrophotographic image forming method
JP2022189247A
Cited By
Crystalline-polyester-containing toner
WO2025070251A1