Gas adsorption sheet for secondary battery with cover film
The gas adsorption sheet for secondary batteries, with a heat-resistant base and inorganic porous particles, addresses handling and moisture issues of conventional adsorbents, ensuring effective gas adsorption and battery safety.
Patent Information
- Application Number
- JP2023068085
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-18
- Publication Date
- 2024-10-30
AI Technical Summary
Conventional gas adsorbents for non-aqueous secondary batteries, such as zeolite in granular or powdered form, suffer from poor handling properties, aggregation issues, and decreased performance due to moisture, making it difficult to apply them effectively in batteries.
A gas adsorption sheet for secondary batteries is developed, comprising a heat-resistant base material with a gas adsorption layer made of binder resin and inorganic porous particles, optionally with an intermediate layer and a cover film, which enhances handling and prevents moisture-induced deterioration.
The gas adsorption sheet provides excellent gas adsorption performance, easy application, and resistance to moisture, improving the safety and longevity of non-aqueous secondary batteries.
Smart Images

Figure 2024154314000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a gas adsorbent sheet with a cover film for use in a secondary battery. [Background technology]
[0002] Conventionally, non-aqueous secondary batteries, such as lithium ion batteries, have been widely used in various fields. In non-aqueous secondary batteries using a non-aqueous electrolyte, gases such as CO2 are easily generated by electrolysis of carbonate esters contained in the non-aqueous electrolyte, and the gas generation can cause deformation of the casing, an increase in internal resistance, a decrease in safety, and the like.
[0003] Various techniques have been studied to prevent the above-mentioned problems, and one of them is a gas adsorbent that is made of zeolite having fine pores and can adsorb gas by encapsulating it (Patent Document 1). This gas adsorbent can exhibit excellent gas adsorption performance and can significantly improve the safety of non-aqueous secondary batteries. In addition, by using the gas adsorbent, it is possible to omit the degassing step in the secondary battery manufacturing process.
[0004] However, the gas adsorbent is provided in a granular or powder form, which causes problems such as poor handling. In addition, since the gas adsorbent is in a granular or powder form, it is difficult to place the desired amount at the desired location due to aggregation or unnecessary dispersion. In addition, there is also a problem that the gas adsorption performance of the gas adsorbent is reduced due to the influence of moisture. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2015-162457 A Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made to solve the above-mentioned problems in the conventional technology, and an object of the present invention is to provide a gas adsorption sheet for secondary batteries that contains gas adsorption particles with excellent gas adsorption properties, and that allows the gas adsorption performance of the gas adsorption particles to be fully exhibited. [Means for solving the problem]
[0007] [1] A gas adsorption sheet for a secondary battery with a cover film according to an embodiment of the present invention comprises: a gas adsorption sheet for a secondary battery, the gas adsorption sheet including a heat-resistant substrate and a gas adsorption layer disposed on at least one side of the heat-resistant substrate; and a cover film disposed on the side of the gas adsorption layer opposite the heat-resistant substrate, the gas adsorption layer being made of a binder resin and an inorganic porous material having pores and including gas adsorption particles capable of adsorbing gas. [2] The gas adsorption sheet for a secondary battery with a cover film described in [1] above may further include an intermediate layer disposed between the heat-resistant substrate and the gas adsorption layer. [3] In the gas adsorption sheet for a secondary battery with a cover film according to the above [1] or [2], the gas adsorption particles may have a surface treated with silicone. [4] In the cover film-attached gas adsorption sheet for a secondary battery according to the above item [3], the silicone may have an ethoxysilane group or a methoxysilane group. [5] In the cover film-attached gas adsorption sheet for a secondary battery according to the above item [4], the silicone may be a silane coupling agent containing an epoxy group or an amino group. [6] In the gas adsorption sheet for a secondary battery with a cover film according to any one of [1] to [5] above, the binder resin may be an acrylic resin. [7] In the gas adsorption sheet for a secondary battery with a cover film described in [6] above, the binder resin may contain a structural unit derived from an alkyl (meth)acrylate, and the alkyl (meth)acrylate may have a linear or branched alkyl group having 4 to 12 carbon atoms. [8] In the gas adsorption sheet for a secondary battery with a cover film according to any one of [1] to [5] above, the binder resin may be butyl rubber, isoprene rubber, polyisobutylene rubber, ethylene propylene rubber or a silicone-based resin. [9] In the gas adsorption sheet for a secondary battery with a cover film according to any one of [1] to [8] above, the content of the gas adsorption particles may be 10 parts by weight to 90 parts by weight per 100 parts by weight of the gas adsorption sheet for a secondary battery.
[10] In the gas adsorption sheet for a secondary battery with a cover film described in any one of [1] to [9] above, the material constituting the heat-resistant substrate may be polyamideimide, polyetherimide, polyphenylene sulfide, polyethylene naphthalate, polyimide or polyether ether ketone.
[11] In the gas adsorption sheet for a secondary battery with a cover film according to any one of [1] to
[10] above, the cover film may comprise a substrate and a pressure-sensitive adhesive layer disposed on at least one side of the substrate.
[12] In the gas adsorption sheet for a secondary battery with a cover film described in
[11] above, the adhesive layer may be formed from an adhesive containing a base polymer, and the content of structural units derived from an organic acid monomer may be preferably 0.5 parts by weight or less per 100 parts by weight of the base polymer.
[13] In the gas adsorbing sheet for a secondary battery with a cover film according to any one of [1] to
[12] above, the cover film may be peelable. Effect of the Invention
[0008] According to the present invention, a gas adsorbent (gas adsorption sheet) with excellent handleability can be obtained by forming a sheet of gas adsorbent particles in combination with a heat-resistant substrate. In this gas adsorption sheet, the gas adsorption performance inherent to the gas adsorbent particles can be fully exhibited, and deterioration of the gas adsorption performance due to moisture can be prevented. [Brief description of the drawings]
[0009] [Figure 1] 1 is a schematic cross-sectional view of a gas adsorbent sheet for a secondary battery according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] A. Overall configuration of gas adsorption sheet for secondary batteries with cover film FIG. 1 is a schematic cross-sectional view of a gas adsorption sheet for a secondary battery with a cover film (hereinafter, also referred to as a gas adsorption sheet with a cover film) according to one embodiment of the present invention. The gas adsorption sheet with a cover film 100 includes a gas adsorption sheet for a secondary battery 110 including a heat-resistant substrate 10 and a gas adsorption layer 20 disposed on at least one side of the heat-resistant substrate 10, and a cover film 120 disposed on the opposite side of the gas adsorption layer 20 from the heat-resistant substrate 10. The gas adsorption layer includes a binder resin and gas adsorption particles. The gas adsorption particles are made of an inorganic porous material having pores. The gas adsorption particles exhibit high gas adsorption performance due to the inclusion action. Examples of gases adsorbed by the gas adsorption particles include CO, CO2, and the like. In one embodiment, the gas adsorption sheet 110 further includes an intermediate layer 30 between the heat-resistant substrate 10 and the gas adsorption layer 20. By forming the intermediate layer, it is possible to prevent the gas adsorption layer from falling off. In one embodiment, the cover film 120 includes a substrate 41 and an adhesive layer 51 disposed on at least one side of the substrate 41. The adhesive layer 51 can be laminated so as to face the gas adsorption layer 20. In this specification, the gas adsorption sheet for a secondary battery with a cover film is also simply referred to as a gas adsorption sheet with a cover film, and the gas adsorption sheet for a secondary battery is also simply referred to as a gas adsorption sheet. The gas adsorption sheet with a cover film and the gas adsorption sheet may include any other appropriate layer as long as the effects of the present invention can be obtained. For example, the gas adsorption sheet may include an adhesive layer disposed on one or both outer surfaces (not shown).
[0011] According to the present invention, a gas adsorption sheet that is easy to handle and can be applied to various applications can be obtained by dispersing gas adsorption particles in a binder resin, forming a gas adsorption layer composed of the gas adsorption particles and the binder resin, and forming the sheet. In addition, by providing a heat-resistant substrate, the effect of improving the handleability becomes more remarkable. Furthermore, by using a heat-resistant substrate as the substrate, it is possible to heat the gas adsorption sheet before use (for example, heating at 200°C for 24 hours). By heating before use, unnecessary substances attached to the gas adsorption particles can be removed, and the performance of the gas adsorption particles can be fully exhibited during use.
[0012] The gas adsorption sheet can be suitably used as a gas adsorbent for a non-aqueous secondary battery, for example. Specifically, it can be used in the form of an insulating sheet, insulating plate, insulating tape, etc., which is placed in a non-aqueous electrolyte. The gas adsorption sheet can adsorb CO and CO2 as well as moisture, hydrogen fluoride, etc., and the gas adsorption sheet can be applied to a battery to extend its life. In addition, by providing the gas adsorbent in the form of a sheet, it is possible to apply the gas adsorbent to a battery using existing battery manufacturing equipment. Furthermore, the gas adsorption sheet can be used to easily arrange a desired amount of gas adsorption particles in a desired position.
[0013] In the present invention, by disposing a cover film, it is possible to prevent deterioration of the gas adsorption layer due to moisture, for example, during storage. Even in a dry room (e.g., a dew point temperature of -50°C) and even in a gas adsorption sheet having a gas adsorption layer that is subject to moisture deterioration, the above-mentioned configuration makes it possible to prevent deterioration of the gas adsorption layer due to moisture (e.g., a decrease in gas absorbency).
[0014] The thickness of the gas adsorbent sheet with a cover film is preferably 15 μm to 1100 μm, more preferably 30 μm to 550 μm, and even more preferably 30 μm to 200 μm.
[0015] B. Gas adsorption sheet The gas adsorption sheet may have adhesiveness on one or both sides, or may be a gas adsorption sheet without adhesiveness. Examples of the gas adsorption sheet having adhesiveness include a gas adsorption layer having adhesiveness, and a gas adsorption sheet having an adhesive layer disposed on the outermost surface of the gas adsorption sheet.
[0016] When the gas adsorption sheet has adhesiveness, the adhesive strength of the gas adsorption sheet to a stainless steel plate at 25°C is preferably 0.1N / 20mm to 10N / 20mm, more preferably 0.5N / 20mm to 5N / 20mm. Within such range, the gas adsorption sheet can be suitable for battery applications. In this specification, the adhesive strength is an adhesive strength measured by a method conforming to JIS Z 0237:2000, and is measured by applying an adhesive tape to an adherend (SUS304BA) by rolling a 2 kg roller back and forth once, leaving the adhesive tape at 25°C for 30 minutes, and then peeling the adhesive tape at a peel angle of 180° and a peel speed (tensile speed) of 300mm / min.
[0017] The thickness of the gas adsorption sheet is preferably 10 μm to 1000 μm, more preferably 20 μm to 500 μm, further preferably 20 μm to 150 μm, and further preferably 20 μm to 130 μm. Within such a range, a gas adsorption sheet having excellent gas adsorption performance and handleability can be obtained.
[0018] B-1. Gas adsorption layer As described above, the gas adsorption layer contains a binder resin and gas adsorption particles dispersed in the binder resin. In the present invention, by adopting such a form, it is possible to form the gas adsorption layer by coating using a coating liquid containing the binder resin and the gas adsorption particles. As a result, a gas adsorption layer having excellent dispersibility of the gas adsorption particles can be formed, and a gas adsorption sheet having excellent gas adsorption performance can be obtained.
[0019] The thickness of the gas adsorption layer is preferably 5 μm to 150 μm, more preferably 5 μm to 120 μm, and further preferably 10 μm to 100 μm. Within such a range, the gas adsorption layer can fully exhibit the performance of the gas adsorption particles. In addition, a gas adsorption sheet with excellent handling properties can be obtained.
[0020] (Gas adsorption particles) The gas-adsorbing particles are made of an inorganic porous material having pores. In one embodiment, the gas-adsorbing particles are made of zeolite. The zeolite may be A-type zeolite, X-type zeolite, or LSX-type zeolite. The zeolite is preferably A-type zeolite in which the cationic portion of the zeolite is ion-exchanged with Li, or A-type zeolite in which the cation portion is ion-exchanged with Ca. The ratio of Si to Al (Si / Al) constituting the gas-adsorbing particles is preferably 1 to 5. If Si / Al is less than 1, the gas-adsorbing particles may be structurally unstable. If Si / Al is more than 5, the adsorption performance may be reduced.
[0021] The volume average particle diameter D50 (median diameter) of the gas adsorbed particles is preferably 50 μm or less, more preferably 20 μm or less. If the volume average particle diameter D50 is within this range, a gas adsorption layer with a large amount of gas adsorption can be formed. The volume average particle diameter D50 (median diameter) can be measured by a laser diffraction / scattering type particle size distribution measuring device.
[0022] The specific surface area of the gas adsorbing particles is preferably 100 m 2 / g~3000m 2 / g. Within this range, gas adsorption particles having excellent gas adsorption performance and mechanical strength can be obtained. Although gas adsorption particles having a large specific surface area are prone to aggregation, the present invention makes it possible to form a gas adsorption layer with good dispersibility of the gas adsorption particles.
[0023] The gas adsorption particles have pores. The size of the pores is preferably 3 Å to 10 Å. The pores are preferably present on the entire surface of the gas adsorption particles.
[0024] The CO2 adsorption amount of the gas adsorption particles is preferably 15 mL / g or more, more preferably 20 mL / g or more, and still more preferably 30 mL / g or more. The CO2 adsorption amount of the gas adsorption particles means the CO2 adsorption amount per 1 g of the gas adsorption particles. The method for measuring the CO2 adsorption amount is as follows. <Method for Measuring CO2 Adsorption Amount> The gas adsorption particles are immersed in an electrolyte for a lithium-ion battery (composition: lithium hexafluorophosphate (1 mol / l) ethylene carbonate solution / ethyl methyl carbonate = 3 / 7 (volume ratio)) so that the electrolyte is 80 ml / g per 1 g of the gas adsorption particles in a predetermined sealed glass container under an environment with a dew point of -40°C, and stored at 60°C for 24 hours. Thereafter, the CO2 concentration A in the glass container is measured by gas chromatography. Except for not adding the gas adsorption particles, in the same manner as above, that is, only the electrolyte for a lithium-ion battery is sealed in the glass container, stored at 60°C for 24 hours, and then the CO2 concentration B in the glass container is measured (concentration B = 0.43 v / v%), and the gas adsorption amount of the gas adsorption particles (the gas adsorption amount per 1 g of the gas adsorption particles (mL / g)) is evaluated from the difference between the CO2 concentration A and the CO2 concentration B.
[0025] In one embodiment, the gas adsorbent particles have a surface-treated surface. The surface treatment can be a treatment for adjusting the affinity between the gas adsorbent particles and the binder resin. By using gas adsorbent particles having a surface-treated surface, a gas adsorbent layer having excellent mechanical strength and difficult to fall off can be formed. The gas adsorbent sheet with cover film provided by laminating a cover film is particularly preferable in that damage to the gas adsorbent layer can be prevented when the cover film is peeled off during use of the gas adsorbent sheet. In addition, by using gas adsorbent particles having a surface-treated surface, a gas adsorbent sheet having excellent processability during cutting can be obtained. For example, damage to the gas adsorbent layer can be prevented when punching the gas adsorbent sheet with a blade such as a Thomson blade. The surface-treated surface may be the entire surface of the gas adsorbent particles, or may be a part of the surface. Examples of the surface treatment include a silane coupling agent treatment, an isocyanate compound treatment, a thiol compound treatment, an acid compound treatment, an alcohol compound treatment, and an epoxy compound treatment. In one embodiment, the surface treatment can be a coupling treatment. By using gas adsorbent particles that have been subjected to a coupling treatment, the effects of preventing detachment of the gas adsorbed layer and improving processability are remarkable.
[0026] In one embodiment, gas adsorption particles having a surface treated with silicone are used. In one embodiment, the silicone has an ethoxysilane group or a methoxysilane group. By using such a silicone, a gas adsorption layer having excellent mechanical strength and difficult to fall off can be formed. The silicone can be a silane coupling agent. Preferably, the silane coupling agent contains an epoxy group and / or an amino group. By using such a silane coupling agent, a gas adsorption layer having excellent mechanical strength and difficult to fall off can be formed. The gas adsorption particles, that is, the gas adsorption particles surface-treated with silicone (silane coupling agent), can be obtained by contacting the silane coupling agent with the gas adsorption particle surface to react an organic group (e.g., a hydroxyl group) present on the surface with a silanol group generated by hydrolysis of the silane coupling agent, or by binding an oligomer generated by condensation of the silanol groups to the gas adsorption particles.
[0027] Examples of the silane coupling agent include vinyltrimethoxysilane, vinyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, N-2-(aminoethyl)-3-amino N-propylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, N-phenyl-3-aminopropyltrimethoxysilane, N-(vinylbenzyl)-2-aminopropyltrimethoxysilane hydrochloride, tris-(trimethoxysilylpropyl)isocyanurate, 3-ureidopropyltrialkoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-isocyanatopropyltriethoxysilane, dithioltriazinepropyltriethoxysilane, and the like.
[0028] The content of the gas adsorbing particles is preferably 10 to 90 parts by weight, more preferably 30 to 80 parts by weight, and further preferably 40 to 70 parts by weight, relative to 100 parts by weight of the gas adsorbing sheet. Within such a range, a gas adsorbing sheet having excellent gas adsorption performance and excellent handleability can be obtained.
[0029] The content of the gas adsorbing particles is preferably 10 to 2000 parts by weight, more preferably 50 to 1500 parts by weight, further preferably 100 to 1000 parts by weight, and particularly preferably 280 to 1000 parts by weight, relative to 100 parts by weight of the binder resin constituting the gas adsorbing layer. If the content is within such a range, a gas adsorbing layer from which the gas adsorbing particles are difficult to desorb can be obtained. In addition, a gas adsorbing sheet having excellent gas adsorption performance, handling properties, and electrolyte resistance can be obtained.
[0030] (binder resin) As the binder resin, any suitable resin is used as long as the effect of the present invention can be obtained. Examples of the binder resin include acrylic resins; rubber-based resins such as butyl rubber, isoprene rubber, polyisobutylene rubber, and ethylene propylene rubber; silicone-based resins; urethane-based resins; epoxy-based resins; alkyd-based resins; polyester-based resins; melamine-based resins; polyamide-based resins; polyimide-based resins; ethylene-vinyl acetate copolymer resins; polyvinyl alcohol-based resins, and the like. In one embodiment, acrylic resins are preferably used. By using acrylic resins, a gas adsorption layer having excellent dispersibility of gas adsorption particles can be formed. In addition, by using acrylic resins, a gas adsorption layer that is difficult to desorb can be formed. In addition, a gas adsorption layer that can fully exhibit the gas adsorption performance of the gas adsorption particles can be formed. In another embodiment, butyl rubber, isoprene rubber, polyisobutylene rubber, ethylene propylene rubber, or silicone-based resins are used. By using these resins, a gas adsorption layer having excellent dispersibility of gas adsorption particles can be formed.
[0031] The binder resin is preferably gas permeable. By using a binder resin having gas permeability, a gas adsorption sheet suitable for battery applications can be obtained. Examples of resins having excellent gas permeability include rubber-based resins such as acrylic resins, butyl rubber, isoprene rubber, polyisobutylene rubber, and ethylene propylene rubber, silicone-based resins, urethane-based resins, epoxy-based resins, alkyd-based resins, polyester-based resins, melamine-based resins, polyamide-based resins, and polyimide-based resins. The CO2 permeability of the gas adsorption layer is preferably 1500 cm 3 / m 2 24hrs atm or higher, preferably 3000cm 3 / m 2 The CO2 permeation rate of the gas adsorption layer can be measured in an environment at 23°C according to JIS K 7126 (isobaric method).
[0032] The binder resin preferably has a high affinity for the non-aqueous electrolyte solution. For example, the binder resin may have an SP value of 8 cal / cm 3 ~15.4cal / cm 3 (Preferably 9cal / cm 3 ~13.2cal / cm 3 In addition, the binder resin preferably has high resistance to a non-aqueous electrolyte solution.
[0033] Examples of the acrylic resin include acrylic resins containing one or more kinds of constituent units derived from (meth)acrylic acid alkyl esters. The content of the constituent units derived from the (meth)acrylic acid alkyl esters is preferably 50 to 97 parts by weight, more preferably 70 to 94 parts by weight, based on 100 parts by weight of the acrylic resin.
[0034] Preferably, the (meth)acrylic acid alkyl ester has a linear or branched alkyl group having 1 to 24 carbon atoms (more preferably 3 to 20, and even more preferably 6 to 18).
[0035] In one embodiment, the (meth)acrylic acid alkyl ester preferably has a linear or branched alkyl group having 4 to 12 carbon atoms, and more preferably has a linear or branched alkyl group having 6 to 12 carbon atoms. If a gas adsorption layer is formed using an acrylic resin having such a (meth)acrylic acid alkyl ester as a main constituent unit, a gas adsorption sheet in which discoloration and swelling in an electrolytic solution are suppressed can be obtained. In addition, a gas adsorption layer that is difficult to desorb can be formed. In one embodiment, the content of the constituent unit derived from a linear or branched alkyl group having 4 to 12 carbon atoms in the acrylic resin is preferably 20 parts by weight to 100 parts by weight, more preferably 30 parts by weight to 100 parts by weight, still more preferably 50 parts by weight to 100 parts by weight, and particularly preferably 70 parts by weight to 100 parts by weight, relative to 100 parts by weight of the constituent unit derived from the (meth)acrylic acid alkyl ester.
[0036] Examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, and eicosyl (meth)acrylate.
[0037] In one embodiment, a (meth)acrylic acid alkyl ester having a branched alkyl group is used as the (meth)acrylic acid alkyl ester. By using a (meth)acrylic acid alkyl ester having a branched alkyl group, a gas adsorption layer that can fully exhibit the gas adsorption performance of the gas adsorption particles can be formed. A (meth)acrylic acid alkyl ester having a linear alkyl group and a (meth)acrylic acid alkyl ester having a branched alkyl group may be used in combination. In addition, a (meth)acrylic acid alkyl ester having a branched alkyl group may be used alone as the (meth)acrylic acid alkyl ester.
[0038] In one embodiment, the content of the structural unit derived from the (meth)acrylic acid alkyl ester having a branched alkyl group in the acrylic resin is preferably 20 parts by weight to 100 parts by weight, more preferably 30 parts by weight to 100 parts by weight, even more preferably 50 parts by weight to 100 parts by weight, and particularly preferably 70 parts by weight to 100 parts by weight, relative to 100 parts by weight of the structural unit derived from the (meth)acrylic acid alkyl ester (including methyl (meth)acrylate and ethyl (meth)acrylate) having a linear alkyl group and the (meth)acrylic acid alkyl ester having a branched alkyl group, 100 parts by weight in total. Within such a range, a gas adsorption sheet having particularly excellent electrolyte resistance can be obtained.
[0039] Examples of (meth)acrylic acid alkyl esters having a branched alkyl group include isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, isodecyl (meth)acrylate, stearyl (meth)acrylate, 2-ethylbutyl (meth)acrylate, 2-methylbutyl (meth)acrylate, etc. Among these, 2-ethylhexyl (meth)acrylate is preferred.
[0040] The acrylic resin may contain, as necessary, a structural unit derived from another monomer copolymerizable with the alkyl (meth)acrylate, for the purpose of modifying properties such as cohesive strength, heat resistance, and crosslinkability. Examples of such other monomers include carboxyl group-containing monomers such as (meth)acrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid; acid anhydride group-containing monomers such as maleic anhydride and itaconic anhydride; phosphoric acid group-containing monomers such as 2-hydroxyethyl acryloyl phosphate; sulfonic acid group-containing monomers such as styrene sulfonic acid, allyl sulfonic acid, 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acrylamidopropanesulfonic acid, sulfopropyl (meth)acrylate, and (meth)acryloyloxynaphthalenesulfonic acid; hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, hydroxyhexyl (meth)acrylate, hydroxyoctyl (meth)acrylate, hydroxydecyl (meth)acrylate, hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl methacrylate. hydroxyl group-containing monomers; (N-substituted) amide monomers such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N-butyl(meth)acrylamide, N-methylol(meth)acrylamide, and N-methylolpropane(meth)acrylamide; (meth)acrylic acid aminoalkyl monomers such as aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, and t-butylaminoethyl (meth)acrylate; methoxyethyl (meth)acrylate, (Meth)acrylate alkoxyalkyl monomers such as ethoxyethyl (meth)acrylate; maleimide monomers such as N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, and N-phenylmaleimide; itaconimide monomers such as N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-cyclohexylitaconimide, and N-laurylitaconimide;succinimide monomers such as N-(meth)acryloyloxymethylene succinimide, N-(meth)acryloyl-6-oxyhexamethylene succinimide, and N-(meth)acryloyl-8-oxyoctamethylene succinimide; vinyl monomers such as vinyl acetate, vinyl propionate, N-vinylpyrrolidone, methylvinylpyrrolidone, vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, vinylmorpholine, N-vinyl carboxylic acid amides, styrene, α-methylstyrene, and N-vinylcaprolactam; cyanoacrylate monomers such as acrylonitrile and methacrylonitrile; epoxy group-containing acrylic monomers such as glycidyl (meth)acrylate; polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, methoxyethylene glycol (meth)acrylate, and (meth)acrylate. Examples of the monomers include glycol-based acrylic ester monomers such as methoxy polypropylene glycol (meth)acrylate; acrylic ester monomers having heterocycles, halogen atoms, silicon atoms, etc., such as tetrahydrofurfuryl (meth)acrylate, fluorine (meth)acrylate, and silicone (meth)acrylate; polyfunctional monomers such as hexanediol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, epoxy acrylate, polyester acrylate, and urethane acrylate; olefin-based monomers such as isoprene, butadiene, and isobutylene; and vinyl ether-based monomers such as vinyl ether. These monomer components may be used alone or in combination of two or more.
[0041] The content of the structural units derived from the other monomers is preferably 20 parts by weight or less, more preferably 15 parts by weight or less, and even more preferably 1 to 10 parts by weight, relative to 100 parts by weight of the acrylic resin.
[0042] The weight average molecular weight of the acrylic resin is preferably 300,000 to 2,000,000, and more preferably 500,000 to 1,500,000. The weight average molecular weight can be measured by GPC (solvent: THF).
[0043] (Additives) The gas adsorption layer may contain any suitable additive as necessary, such as a crosslinking agent, a tackifier (e.g., a rosin-based tackifier, a terpene-based tackifier, a hydrocarbon-based tackifier, etc.), a plasticizer (e.g., a trimellitic acid ester-based plasticizer, a pyromellitic acid ester-based plasticizer), a pigment, a dye, an antioxidant, a conductive material, an antistatic agent, a light stabilizer, a release regulator, a softener, a surfactant, a flame retardant, an antioxidant, an ultraviolet absorbing agent, particles, etc.
[0044] B-2. Heat resistant base material In this specification, the heat-resistant substrate is a substrate that can withstand heating for 24 hours under an atmosphere of 150°C / pressure of -100 kPa to 0 kPa (preferably, 24 hours under an atmosphere of 200°C / pressure of -100 kPa to 0 kPa), specifically, a substrate that undergoes 5% or less dimensional change even when heated for 24 hours under an atmosphere of 150°C / pressure of -100 kPa (preferably, 24 hours under an atmosphere of 200°C / pressure of -100 kPa). In addition, when the heat-resistant substrate is formed from a resin, the heat-resistant substrate means a substrate made of a resin having a glass transition temperature of 80°C or higher (preferably, 100°C or higher, more preferably, 150°C or higher). The "glass transition temperature" means a temperature at which the loss tangent (tan δ) peaks are observed in the DMA method (tensile method) under the conditions of a heating rate of 5°C / min, a sample width of 5 mm, a chuck distance of 20 mm, and a frequency of 10 Hz.
[0045] As the material constituting the heat-resistant substrate, any appropriate material may be adopted as long as the effect of the present invention can be obtained. Preferably, the heat-resistant substrate is made of a resin. Examples of materials constituting the heat-resistant substrate include polyamideimide (PAI), polyetherimide (PEI), polyphenylene sulfide (PPS), polyethylene naphthalate (PEN), polyimide (PI), polyether ether ketone (PEEK), etc. These resins have excellent heat resistance and excellent electrolyte resistance.
[0046] The thickness of the heat-resistant substrate is preferably 5 μm to 500 μm, more preferably 10 μm to 300 μm, and further preferably 15 μm to 100 μm. Within such a range, a gas adsorbing sheet with particularly excellent handling properties can be obtained.
[0047] B-3.Middle layer The intermediate layer includes any appropriate resin. Examples of the resin forming the intermediate layer include acrylic resin, rubber resin, and silicone resin. Among them, acrylic resin can be preferably used. In addition, an active energy ray curable acrylic resin may be used as the adhesive. Examples of the resin constituting the intermediate layer include the binder resin. In one embodiment, the same resin as the binder resin constituting the gas adsorption layer is used as the resin constituting the intermediate layer. The intermediate layer does not include gas adsorption particles.
[0048] By forming the intermediate layer, it is possible to obtain a gas adsorbing sheet in which the gas adsorbing layer is less likely to desorb.
[0049] The thickness of the intermediate layer is preferably from 1 μm to 50 μm, more preferably from 2 μm to 30 μm, and further preferably from 2 μm to 20 μm.
[0050] The intermediate layer may contain any suitable additives as necessary, such as crosslinkers, tackifiers, plasticizers (e.g., trimellitic acid ester plasticizers, pyromellitic acid ester plasticizers), pigments, dyes, fillers, antioxidants, conductive agents, UV absorbers, light stabilizers, release regulators, softeners, surfactants, flame retardants, antioxidants, solvents, etc.
[0051] C. Cover film In one embodiment, the cover film includes a substrate and a pressure-sensitive adhesive layer disposed on at least one side of the substrate.
[0052] In one embodiment, the cover film is arranged so as to be peelable. In one embodiment, the cover film is peelable from the gas adsorption sheet after being heated and dried at 110°C for 3 hours. The peelability of such a cover film can be controlled by adjusting the adhesive strength of the cover film, for example, by the composition of the adhesive layer.
[0053] The adhesive strength of the cover film to a stainless steel plate at 25° C. is preferably 0.05 N / 20 mm to 5 N / 20 mm, more preferably 0.1 N / 20 mm to 3 N / 20 mm, more preferably 0.15 N / 20 mm to 2 N / 20 mm, and even more preferably 0.15 N / 20 mm to 1 N / 20 mm.
[0054] The peel strength when peeling the cover film from the gas adsorption sheet after drying the gas adsorption sheet with cover film at 110°C under reduced pressure of -100 kPa for 3 hours is preferably 0.01 N / 50 mm to 5 N / 50 mm, more preferably 0.02 N / 50 mm to 3 N / 50 mm, and even more preferably 0.05 N / 50 mm to 2.5 N / 50 mm. Within such a range, the cover film can be peeled off while preventing damage to the gas absorbing layer. The peel strength can be measured by a method conforming to JIS Z 0237:2000. That is, the peel strength is measured by peeling the cover film of the gas adsorption sheet with cover film from the gas adsorption sheet under the conditions of a measurement temperature of 25°C, a peel angle of 180°, and a peel speed (tensile speed) of 300 mm / min.
[0055] C-1. Base material The substrate may be made of any suitable material. The substrate may be, for example, a resin film, paper, cloth, nonwoven fabric, metal foil, or a plastic laminate thereof, or a laminate of plastics. Among them, a resin film is most preferable from the viewpoint of handling and cost. The material constituting the resin film may be selected as necessary from the viewpoint of strength, heat resistance, and the like. Examples of the material include olefin-based resins having α-olefin as a monomer component, such as polyethylene (PE), polypropylene (PP), ethylene-propylene copolymer, and ethylene-vinyl acetate copolymer (EVA); polyesters such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), and polybutylene terephthalate (PBT); polyvinyl chloride (PVC); polyphenylene sulfide (PPS); amide-based resins such as polyamide (nylon) and fully aromatic polyamide (aramid); polyether ether ketone (PEEK), polyimide, polyetherimide, polystyrene, and acrylic resins. These materials may be used alone or in combination of two or more. The plastic film may be any of an unstretched film, a uniaxially oriented film, and a biaxially oriented film. These films may be laminated films consisting of two or more film layers, and from the viewpoint of handling, a film containing a lubricant such as inert particles may be appropriately added.
[0056] The thickness of the substrate is preferably 200 μm or less, more preferably 1 μm to 200 μm, even more preferably 5 μm to 100 μm, particularly preferably 10 μm to 100 μm, particularly preferably 20 μm to 100 μm, and most preferably 30 μm to 100 μm. Within such a range, a gas adsorbing sheet with a cover film can be obtained that is prevented from floating when formed into a roll and has excellent workability.
[0057] The moisture permeability of the substrate is preferably 500 g / m 2 - 24hr or less, preferably 100g / m 2The moisture permeability is determined in accordance with the moisture permeability test (cup method) of JIS Z 0208.
[0058] The substrate may be subjected to a surface treatment, such as corona treatment, chromate treatment, ozone exposure, flame exposure, high-voltage shock exposure, ionizing radiation treatment, or coating with a primer.
[0059] C-2. Adhesive layer The thickness of the pressure-sensitive adhesive layer is preferably 30 μm or less, more preferably 20 μm or less, and further preferably 10 μm or less. The lower limit of the thickness of the pressure-sensitive adhesive layer is, for example, 1 μm (preferably 0.5 μm).
[0060] The pressure-sensitive adhesive layer includes any suitable pressure-sensitive adhesive. Any suitable pressure-sensitive adhesive may be used as the pressure-sensitive adhesive as long as the effects of the present invention can be obtained. For example, a pressure-sensitive adhesive may be used as the pressure-sensitive adhesive.
[0061] Examples of pressure-sensitive adhesives include acrylic adhesives, rubber adhesives, vinyl alkyl ether adhesives, silicone adhesives, polyester adhesives, polyamide adhesives, urethane adhesives, and styrene-diene block copolymer adhesives. Among them, acrylic adhesives or rubber adhesives are preferred, and acrylic adhesives are more preferred. The above adhesives may be used alone or in combination of two or more. In one embodiment, from the viewpoint of ultraviolet absorption, an adhesive containing a base polymer having an aromatic ring and / or a double bond is used. From this viewpoint, an acrylic adhesive may be preferably used.
[0062] Examples of the acrylic adhesive include acrylic adhesives having an acrylic polymer (homopolymer or copolymer) as a base polymer, which uses one or more (meth)acrylic acid alkyl esters as monomer components. Specific examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, and (meth)acrylate. Examples of the (meth)acrylic acid C1-20 alkyl esters include nonyl acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, and eicosyl (meth)acrylate. Among these, (meth)acrylic acid alkyl esters having a linear or branched alkyl group having 4 to 18 carbon atoms can be preferably used.
[0063] The acrylic polymer may contain units corresponding to other monomer components copolymerizable with the alkyl (meth)acrylate, if necessary, for the purpose of modifying properties such as cohesive strength, heat resistance, and crosslinkability. Examples of such monomer components include carboxyl group-containing monomers such as acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid; acid anhydride monomers such as maleic anhydride and itanoic anhydride; hydroxyl group-containing monomers such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, hydroxyhexyl (meth)acrylate, hydroxyoctyl (meth)acrylate, hydroxydecyl (meth)acrylate, hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl methacrylate; sulfonic acid group-containing monomers such as styrene sulfonic acid, allyl sulfonic acid, 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acrylamidopropanesulfonic acid, sulfopropyl (meth)acrylate, and (meth)acryloyloxynaphthalenesulfonic acid; (N-substituted) amide monomers such as N,N-dimethyl(meth)acrylamide, N-butyl(meth)acrylamide, N-methylol(meth)acrylamide, and N-methylolpropane(meth)acrylamide; aminoalkyl(meth)acrylate monomers such as aminoethyl(meth)acrylate, N,N-dimethylaminoethyl(meth)acrylate, and t-butylaminoethyl(meth)acrylate; alkoxyalkyl(meth)acrylate monomers such as methoxyethyl(meth)acrylate and ethoxyethyl(meth)acrylate; maleimide monomers such as N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, and N-phenylmaleimide; itaconimide monomers such as N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-cyclohexylitaconimide, and N-laurylitaconimide;succinimide monomers such as N-(meth)acryloyloxymethylene succinimide, N-(meth)acryloyl-6-oxyhexamethylene succinimide, and N-(meth)acryloyl-8-oxyoctamethylene succinimide; vinyl monomers such as vinyl acetate, vinyl propionate, N-vinylpyrrolidone, methylvinylpyrrolidone, vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, vinylmorpholine, N-vinyl carboxylic acid amides, styrene, α-methylstyrene, and N-vinylcaprolactam; cyanoacrylate monomers such as acrylonitrile and methacrylonitrile; epoxy group-containing acrylic monomers such as glycidyl (meth)acrylate; polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, methoxyethylene glycol (meth)acrylate, and (meth)acrylate. Examples of the monomers include glycol-based acrylic ester monomers such as methoxy polypropylene glycol (meth)acrylate; acrylic ester monomers having heterocycles, halogen atoms, silicon atoms, etc., such as tetrahydrofurfuryl (meth)acrylate, fluorine (meth)acrylate, and silicone (meth)acrylate; polyfunctional monomers such as hexanediol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, epoxy acrylate, polyester acrylate, and urethane acrylate; olefin-based monomers such as isoprene, butadiene, and isobutylene; and vinyl ether-based monomers such as vinyl ether. These monomer components may be used alone or in combination of two or more.
[0064] In one embodiment, the content of structural units derived from organic acid monomers (e.g., (meth)acrylic acid group-containing monomers, carboxyl group-containing monomers) in the base polymer (e.g., acrylic polymer) is preferably 0.5 parts by weight or less, more preferably 0.3 parts by weight or less, relative to 100 parts by weight of the base polymer. Within this range, a cover film can be obtained that is less likely to destroy the gas adsorption layer of the gas adsorption sheet when peeled off from the gas adsorption sheet. In particular, when gas adsorption particles that have been surface-treated (preferably coupling treated) are used, such an effect is remarkable. In one embodiment, an acrylic polymer that does not contain structural units derived from organic acid monomers is used.
[0065] In one embodiment, the content of the nitrogen-containing monomer-derived constitutional unit in the base polymer (e.g., acrylic polymer) is preferably 20 parts by weight or less, more preferably 15 parts by weight or less, based on 100 parts by weight of the base polymer. Within such a range, a cover film can be obtained that is unlikely to destroy the gas adsorption layer of the gas adsorption sheet when the gas adsorption sheet is peeled off.
[0066] The pressure-sensitive adhesive may contain any suitable additives as necessary, such as crosslinkers, tackifiers (e.g., rosin-based tackifiers, terpene-based tackifiers, hydrocarbon-based tackifiers, etc.), plasticizers (e.g., trimellitic acid ester-based plasticizers, pyromellitic acid ester-based plasticizers), pigments, dyes, antioxidants, conductive materials, antistatic agents, light stabilizers, release regulators, softeners, surfactants, flame retardants, antioxidants, ultraviolet absorbing agents, particles, etc.
[0067] Examples of the crosslinking agent include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, melamine-based crosslinking agents, peroxide-based crosslinking agents, urea-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, carbodiimide-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, and amine-based crosslinking agents. Among these, isocyanate-based crosslinking agents and epoxy-based crosslinking agents are preferred. In one embodiment, from the viewpoint of ultraviolet absorption, a crosslinking agent having an aromatic ring and / or a double bond (e.g., an aromatic isocyanate-based crosslinking agent) is used.
[0068] Specific examples of the isocyanate-based crosslinking agent include lower aliphatic polyisocyanates such as butylene diisocyanate and hexamethylene diisocyanate; alicyclic isocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate and isophorone diisocyanate; aromatic isocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate and xylylene diisocyanate; and isocyanate adducts such as trimethylolpropane / tolylene diisocyanate trimer adduct (manufactured by Tosoh Corporation, product name "Coronate L"), trimethylolpropane / hexamethylene diisocyanate trimer adduct (manufactured by Tosoh Corporation, product name "Coronate HL"), and isocyanurate of hexamethylene diisocyanate (manufactured by Tosoh Corporation, product name "Coronate HX"). The content of the isocyanate-based crosslinking agent can be set to any appropriate amount depending on the desired adhesive strength, and is typically 0.1 to 20 parts by weight, and more preferably 0.5 to 10 parts by weight, per 100 parts by weight of the base polymer.
[0069] Examples of the epoxy crosslinking agent include N,N,N',N'-tetraglycidyl-m-xylylenediamine, diglycidylaniline, 1,3-bis(N,N-glycidylaminomethyl)cyclohexane (manufactured by Mitsubishi Gas Chemical Company, Inc., product name "Tetrad C"), 1,6-hexanediol diglycidyl ether (manufactured by Kyoeisha Chemical Company, Inc., product name "Epolite 1600"), neopentyl glycol diglycidyl ether (manufactured by Kyoeisha Chemical Company, Inc., product name "Epolite 1500NP"), ethylene glycol Licor diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., product name "Epolite 40E"), propylene glycol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., product name "Epolite 70P"), polyethylene glycol diglycidyl ether (manufactured by Nippon Oil & Fats Co., Ltd., product name "Epiol E-400"), polypropylene glycol diglycidyl ether (manufactured by Nippon Oil & Fats Co., Ltd., product name "Epiol P-200"), sorbitol polyglycidyl ether (manufactured by Nagase ChemteX Corporation, product name "Denacol" Examples of the epoxy crosslinking agent include glycerol polyglycidyl ether (manufactured by Nagase Chemtex Corporation, trade name "Denacol EX-611"), glycerol polyglycidyl ether (manufactured by Nagase Chemtex Corporation, trade name "Denacol EX-314"), pentaerythritol polyglycidyl ether, polyglycerol polyglycidyl ether (manufactured by Nagase Chemtex Corporation, trade name "Denacol EX-512"), sorbitan polyglycidyl ether, trimethylolpropane polyglycidyl ether, adipic acid diglycidyl ester, o-phthalic acid diglycidyl ester, triglycidyl-tris(2-hydroxyethyl)isocyanurate, resorcinol diglycidyl ether, bisphenol-S-diglycidyl ether, and epoxy resins having two or more epoxy groups in the molecule. The content of the epoxy crosslinking agent can be set to any appropriate amount depending on the desired adhesive strength, and is typically 0.01 to 10 parts by weight, more preferably 0.03 to 5 parts by weight, relative to 100 parts by weight of the base polymer.
[0070] Examples of the tackifier include rosin-based resins (e.g., rosin ester resins, etc.), terpene-based resins (e.g., terpene-phenol copolymers (terpene-modified phenolic resins), hydrogenated terpene resins, etc.), coumarone-indene resins, alicyclic saturated hydrocarbon-based resins, petroleum-based resins (e.g., hydrocarbon-based petroleum resins such as aliphatic / aromatic copolymer petroleum resins, aromatic petroleum resins, etc.), and phenol-based resins. In one embodiment, from the viewpoint of ultraviolet absorption, a crosslinking agent having an aromatic ring and / or a double bond (e.g., rosin-based resin) is used. The content of the tackifier can be set to any appropriate amount depending on the desired adhesive strength, and is typically 1 part by weight to 50 parts by weight, more preferably 10 parts by weight to 30 parts by weight, relative to 100 parts by weight of the base polymer.
[0071] D. Gas adsorption sheet manufacturing method The gas adsorption sheet can be manufactured by any suitable method. In one embodiment, the gas adsorption sheet is manufactured by coating (coating and drying) a gas adsorption layer forming composition containing the binder resin and gas adsorption particles on a heat-resistant substrate. By forming a gas adsorption layer by coating, a gas adsorption sheet having excellent dispersibility of the gas adsorption particles and excellent gas adsorption performance can be obtained. When the gas adsorption sheet has an intermediate layer, it can be manufactured by forming the gas adsorption layer after coating the intermediate layer forming composition on a heat-resistant substrate to form the intermediate layer.
[0072] The gas adsorption layer forming composition may further contain any suitable additives in addition to the binder resin and the gas adsorption particles. Alternatively, the intermediate layer forming composition may further contain any suitable additives in addition to the resin. Examples of the additives include crosslinkers, tackifiers, plasticizers (e.g., trimellitic acid ester plasticizers, pyromellitic acid ester plasticizers), pigments, dyes, fillers, antioxidants, conductive agents, UV absorbers, light stabilizers, release regulators, softeners, surfactants, flame retardants, and antioxidants. Examples of the crosslinkers include isocyanate-based crosslinkers, epoxy-based crosslinkers, melamine-based crosslinkers, and peroxide-based crosslinkers, as well as urea-based crosslinkers, metal alkoxide-based crosslinkers, metal chelate-based crosslinkers, metal salt-based crosslinkers, carbodiimide-based crosslinkers, oxazoline-based crosslinkers, aziridine-based crosslinkers, and amine-based crosslinkers. Among these, isocyanate-based crosslinkers and epoxy-based crosslinkers are preferred. The gas adsorbing layer forming composition may also contain a solvent such as toluene or ethyl acetate.
[0073] Examples of methods for applying the gas adsorption layer forming composition and intermediate layer forming composition include coating methods such as air doctor coating, blade coating, knife coating, reverse coating, transfer roll coating, gravure roll coating, kiss coating, cast coating, spray coating, slot orifice coating, calendar coating, electrodeposition coating, dip coating, and die coating; and printing methods such as letterpress printing methods such as flexographic printing, intaglio printing methods such as direct gravure printing and offset gravure printing, lithographic printing methods such as offset printing, and stencil printing methods such as screen printing.
[0074] The gas adsorbing sheet with a cover film can be obtained by laminating the cover film on the gas adsorbing layer of the gas adsorbing sheet by any appropriate method. The cover film can be obtained by coating the pressure-sensitive adhesive on the substrate by any appropriate method. EXAMPLES
[0075] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The evaluation methods in the examples are as follows. In the examples, "parts" and "%" are by weight unless otherwise specified.
[0076] [Production Example 1] Production method of cover film A Monomers (2-ethylhexyl acrylate / ethyl acrylate / methyl methacrylate / hydroxyethyl acrylate=30 parts by weight / 70 parts by weight / 5 parts by weight / 4 parts by weight), 0.2 parts by weight of benzoyl peroxide as an initiator, and 244 parts by weight of toluene were charged into a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a cooler. Nitrogen gas was introduced while gently stirring, and a polymerization reaction was carried out for approximately 6 hours while maintaining the liquid temperature in the flask at around 60°C, thereby obtaining a resin composition A containing an acrylic copolymer A. To the resin composition A containing 100 parts by weight of the obtained acrylic copolymer A, 3 parts by weight of an isocyanate crosslinking agent (manufactured by Mitsui Chemicals, Inc., product name "Takenate D-101E") and ethyl acetate were added to prepare a 15% base adhesive A. The adhesive A was applied onto a 75 μm thick substrate (polyester film, manufactured by Toray Industries, Inc., product name "Lumirror S10") so that the adhesive layer would have a thickness of 10 μm after drying, to obtain a cover film A (substrate / adhesive layer A).
[0077] [Production Example 2] Production method of cover films B to Q Cover films B to Q were obtained in the same manner as in Production Example 1, except that the base material shown in Table 1 was used; the monomers shown in Table 1 were used as the material monomers for the acrylic copolymer instead of <2-ethylhexyl acrylate / ethyl acrylate / methyl methacrylate / hydroxyethyl acrylate = 30 parts by weight / 70 parts by weight / 5 parts by weight / 4 parts by weight>; the type and amount of crosslinking agent was as shown in Table 1; and the thickness of the adhesive layer was as shown in Table 1. Details of each component are as follows: (monomer) 2EHA: 2-ethylhexyl acrylate EA: Ethyl acrylate MMA: Methyl methacrylate HEA: Hydroxyethyl acrylate BA: Butyl acrylate 4HBA: 4-Hydroxybutyl acrylate AA: Acrylic acid NVP: N-vinylpyrrolidone (base material) Torayfan BO: Polypropylene film Lumirror S1N: Polyester film (Crosslinking agent) Tetrad C: Epoxy crosslinking agent, manufactured by Mitsubishi Gas Chemical Company, trade name "Tetrad C"
[0078] [Table 1]
[0079] [Example 1] A four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a cooler was charged with 100 parts by weight of gas-adsorbing particles (manufactured by Union Showa Co., Ltd., product name "Molecular Sieve 3AB Powder"), 4 parts by weight of a silane coupling agent (manufactured by Shin-Etsu Chemical Co., Ltd., product name "KBM-4803"), 150 parts by weight of tetrahydrofuran, and 1.3 parts by weight of distilled water. Nitrogen gas was introduced while gently stirring, and a coupling reaction was carried out for approximately 6 hours while maintaining the liquid temperature in the flask at around 60°C, to obtain surface-treated gas-adsorbing particles (1). A four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a cooler was charged with 2-ethylhexyl acrylate / acrylic acid (95 parts by weight / 5 parts by weight), 0.2 parts by weight of an initiator (benzoyl peroxide), and 120 parts by weight of ethyl acetate. Nitrogen gas was introduced while gently stirring, and the liquid temperature in the flask was kept at around 60°C. A polymerization reaction was carried out for approximately 6 hours to obtain a resin composition (1) containing an acrylic copolymer (1). To a resin composition (1) containing 100 parts by weight of an acrylic copolymer (1), 3 parts by weight of an isocyanate-based crosslinking agent (manufactured by Mitsui Chemicals, Inc., product name "Takenate D-101E") and ethyl acetate were added to prepare a composition (1) for forming an intermediate layer with a base of 18%. The obtained composition for forming an intermediate layer (1) was applied onto a heat-resistant substrate (polyimide film, manufactured by Toray DuPont Co., Ltd., product name "Kapton 100H", thickness: 25 μm) so that the thickness after drying would be 10 μm, thereby obtaining a heat-resistant substrate (1) with an intermediate layer. A 50% base composition for forming a gas adsorption layer (1) was prepared by adding 1 part by weight of an epoxy-based crosslinking agent (manufactured by Mitsubishi Gas Chemical Company, Inc., product name "Tetrad C"), ethyl acetate, and 900 parts by weight of the gas adsorption particles (1) to a resin composition (1) containing 100 parts by weight of an acrylic copolymer (1). The obtained gas adsorption layer forming composition (1) was applied onto a release treated film (manufactured by Fujiko Co., Ltd., product name "CA0", thickness: 75 μm) so as to have a thickness after drying of 80 μm, thereby obtaining a gas adsorption layer (1). The obtained gas adsorbing layer (1) was transferred onto the intermediate layer of the intermediate layer-forming composition (1) to obtain a gas adsorbing sheet (1). The above cover film A was laminated on the gas adsorption sheet (1) so that the gas adsorption layer (1) and the pressure-sensitive adhesive layer A faced each other, to obtain a gas adsorption sheet with a cover film.
[0080] [Examples 2 to 19, Comparative Examples 1 to 3] A gas adsorbent sheet with a cover film was obtained in the same manner as in Example 1, except that the type and amount of coupling agent used when preparing the gas adsorbent particles were as shown in Table 2; the thickness of the intermediate layer was as shown in Table 2; the type and amount of crosslinking agent added to the gas adsorbing layer was as shown in Table 2; and a cover film as shown in Table 2 was used. In the comparative examples, a pressure-sensitive adhesive sheet was obtained without laminating a cover film, and the pressure-sensitive adhesive sheet was subjected to the following evaluation. Furthermore, in the comparative example 1, a heat-resistant substrate (polyimide film, manufactured by Toray DuPont Co., Ltd., product name "Kapton 100H", thickness: 25 μm) was used instead of the heat-resistant substrate with an intermediate layer, and the gas adsorption layer-forming composition was applied to the heat-resistant substrate to obtain a gas adsorption sheet. Details of each component are as follows: (Coupling Agent) KBM903: Shin-Etsu Chemical Co., Ltd., product name "KBM903" KBM3033: Shin-Etsu Chemical Co., Ltd., product name "KBM3033" KBM13: Shin-Etsu Chemical Co., Ltd., product name "KBM13" KBM403: Shin-Etsu Chemical Co., Ltd., product name "KBM403"
[0081] [Table 2]
[0082] <Evaluation> The gas adsorbent sheets with cover films obtained in the Examples and Comparative Examples were subjected to the following evaluations. The results are shown in Table 2. (1) Cover film peel strength The gas adsorption sheet with the cover film was dried at 110° C. for 3 hours under a reduced pressure of −100 kPa, and then the cover film was peeled off from the gas adsorption sheet with the cover film, and the peel strength was measured. Test speed: 300mm / min Peel angle: 180 degrees Measurement temperature: 25℃
[0083] (2) Cover film removability (removability after drying) The fracture mode in the above evaluation (1) was evaluated. ○: Can be peeled off at the interface between the cover film and gas adsorption layer △: The surface of the gas adsorption layer is transferred to the cover film side. ×: The entire gas adsorption layer is transferred to the cover film side.
[0084] (3) Gas adsorption layer strength The gas adsorption sheet with the cover film was dried at 110°C for 3 hours under a reduced pressure of -100 kPa, and then the cover film was peeled off from the gas adsorption sheet with the cover film. No. 31B manufactured by Nitto Denko Corporation was attached to the exposed surface of the gas adsorption layer, and the peel strength was measured and recorded as the gas adsorption layer strength. Bonding conditions: Bonded in a 25°C environment using a 2 kg roller, going back and forth once. Test speed: 300mm / min Peel angle: 180 degrees Measurement temperature: 25℃
[0085] (4) Gas adsorption layer adhesion The failure mode in the above evaluation (3) was evaluated. ○: Cohesive failure mode of gas adsorption layer ×: Anchorage destruction mode of gas adsorption layer
[0086] (5) Heat resistance of cover film The gas adsorption sheet with the cover film was dried at 110° C. for 3 hours under a reduced pressure of −100 kPa, and the condition of the cover film was then evaluated. ○: No exposure of the gas adsorption layer due to lifting, peeling, or shrinkage ×: Any of the following occurs: floating, peeling, or exposure of the gas adsorption layer due to shrinkage.
[0087] (6) Processability The gas adsorption sheet with the cover film was punched using a Thomson blade (size 5 mm x 20 mm, blade thickness 0.7 mm, R: 0.2), and the condition of the gas adsorption sheet was evaluated after punching. ○: No chipping of the gas adsorption layer △: No chipping of the gas adsorption layer, but lifting and peeling of the cover film. ×: The gas adsorption layer is chipped.
[0088] (7) Moisture resistance The gas adsorption sheet with cover film was dried for 3 hours at 110°C under reduced pressure of -100 kPa in a dry room with a dew point temperature of -50°C and a room temperature of 23°C, and then stored in the dry room to measure the change in moisture content due to moisture absorption. 〇: Moisture content maintained below 1% for more than 8 hours in a dry room. ×: Moisture content cannot be maintained at 1% or less for 8 hours in a dry room. Moisture content measurement method (Karl Fischer method) Moisture content meter: Hiranuma AQ-2100
[0089] (8) Adhesive strength of cover film The obtained cover film was attached to a SUS304BA plate, and the peel strength when peeled off was measured, and this was taken as the adhesive strength of the cover film. Bonding conditions: Bonded in a 25°C environment using a 2 kg roller, going back and forth once. Test speed: 300mm / min Peel angle: 180 degrees Measurement temperature: 25℃
[0090] (9) Handling The defects occurring when winding a gas adsorption sheet with a cover film onto a 3-inch core made of ABS resin are evaluated. 〇: No problem ×: The gas adsorption layer was chipped during transportation, or the cover film was lifted after winding. [Industrial Applicability]
[0091] The gas adsorbent sheet of the present invention can be suitably used as a gas adsorbent for non-aqueous secondary batteries. [Explanation of symbols]
[0092] 10 Heat-resistant base material 20 Gas adsorption layer 30 Middle Class 100 Gas adsorption sheet with cover film
Claims
1. a gas adsorption sheet for a secondary battery, comprising a heat-resistant substrate and a gas adsorption layer disposed on at least one side of the heat-resistant substrate; a cover film disposed on the gas adsorption layer opposite the heat-resistant substrate; The gas adsorption layer includes a binder resin and gas adsorption particles that are made of an inorganic porous material having pores and can adsorb a gas. Gas adsorption sheet for secondary batteries with cover film.
2. 2. The gas adsorbing sheet for a secondary battery with a cover film according to claim 1, further comprising an intermediate layer disposed between said heat-resistant substrate and said gas adsorbing layer.
3. 2. The gas adsorbing sheet for a secondary battery with a cover film according to claim 1, wherein said gas adsorbing particles have a surface treated with silicone.
4. 4. The gas adsorbing sheet for a secondary battery with a cover film according to claim 3, wherein said silicone has an ethoxysilane group or a methoxysilane group.
5. 5. The gas adsorption sheet for a secondary battery with a cover film according to claim 4, wherein the silicone is a silane coupling agent containing an epoxy group or an amino group.
6. 2. The gas adsorbing sheet for a secondary battery with a cover film according to claim 1, wherein the binder resin is an acrylic resin.
7. the binder resin contains a structural unit derived from an alkyl (meth)acrylate ester, 7. The gas adsorption sheet for a secondary battery with a cover film according to claim 6, wherein the (meth)acrylic acid alkyl ester has a linear or branched alkyl group having 4 to 12 carbon atoms.
8. 2. The gas adsorption sheet for a secondary battery with a cover film according to claim 1, wherein the binder resin is butyl rubber, isoprene rubber, polyisobutylene rubber, ethylene propylene rubber or a silicone-based resin.
9. 2. The gas adsorption sheet for a secondary battery with a cover film according to claim 1, wherein the content of said gas adsorption particles is 10 to 90 parts by weight per 100 parts by weight of the gas adsorption sheet for a secondary battery.
10. 2. The gas adsorption sheet for a secondary battery with a cover film according to claim 1, wherein the material constituting said heat-resistant substrate is polyamideimide, polyetherimide, polyphenylene sulfide, polyethylene naphthalate, polyimide or polyether ether ketone.
11. 2. The gas adsorbing sheet for a secondary battery with a cover film according to claim 1, wherein the cover film comprises a substrate and an adhesive layer disposed on at least one side of the substrate.
12. the pressure-sensitive adhesive layer is formed from a pressure-sensitive adhesive containing a base polymer, The content of the structural unit derived from the organic acid monomer is preferably 0.5 parts by weight or less based on 100 parts by weight of the base polymer. The gas adsorbing sheet for a secondary battery with a cover film according to claim 11.
13. 12. The gas adsorbing sheet for a secondary battery with a cover film according to claim 11, wherein the cover film is peelable.
Citation Information
Patent Citations
Material capable of absorbing carbon monoxide and carbon dioxide, power storage device arranged by use thereof, and method for producing material capable of absorbing carbon monoxide and carbon dioxide
JP2015162457A