Method for manufacturing glass preform
By controlling gas flow rates and using a burner with peripheral hood and gas injection, the method stabilizes flame decomposition and reduces hood deterioration, enhancing glass particle deposition efficiency and reducing gas usage and associated costs.
Patent Information
- Application Number
- JP2023068620
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-19
- Publication Date
- 2024-10-31
AI Technical Summary
The burner hood in glass manufacturing processes is susceptible to deterioration due to red heat, and the amount of combustion supporting gas used is not optimally controlled, leading to inefficiencies.
A method involving a burner with a hood on its periphery, where frit and fuel gases are injected centrally and auxiliaries are injected peripherally, with controlled flow rates to stabilize the flame and reduce hood deterioration, including a first and second deposition step with adjusted gas flow rates to manage glass particle deposition efficiently.
This method effectively suppresses hood deterioration and reduces the amount of combustion gas used, maintaining deposition efficiency while minimizing costs associated with chlorine treatment.
Smart Images

Figure 2024154668000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for manufacturing a glass base material. [Background technology]
[0002] Patent Document 1 discloses a burner used for producing a porous glass particle deposit body by the OVD method and the VAD method. The burner in Patent Document 1 has multiple tubes for injecting glass raw material, and multiple flame injection nozzles having a double tube structure for injecting fuel gas and combustion supporting gas.
[0003] Patent Document 2 discloses a method for manufacturing a glass base material in which the outer diameter of a portion where glass particles are deposited in each of a plurality of burners is monitored, and the amount of glass raw material supplied is adjusted so that the outer diameter becomes uniform in the longitudinal direction.
[0004] Patent Document 3 discloses a concentric multi-tube burner with a protrusion. The gas flow rate of the glass raw material gas injected from the center of the burner is 0.3 to 1.0 times the gas flow rate of the flame gas injected from the inside of the protrusion. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2004-331440 A [Patent Document 2] JP 2006-160551 A [Patent Document 3] International Publication No. 2017 / 188334 Summary of the Invention [Problem to be solved by the invention]
[0006] In order to stabilize the flame decomposition reaction, the burner may be provided with a hood that is provided on the outer periphery of the burner body and that protrudes downstream in the injection direction from the injection surface of the body. This hood is easily deteriorated by red heat due to the flame. In order to suppress deterioration of the hood due to red heat, it is preferable to inject a combustion supporting gas from the outer periphery of the emission surface. However, there is room for improvement in the amount of combustion supporting gas used in terms of oversupply.
[0007] An object of the present disclosure is to provide a method for manufacturing a glass base material that suppresses deterioration of a burner hood and reduces the amount of combustion supporting gas used. [Means for solving the problem]
[0008] A method for producing a glass base material, comprising: generating glass particles in a flame formed by a burner while reciprocating the burner relative to a target; and spraying and depositing the generated glass particles on the target, the method comprising the steps of: The burner is A main body portion, a hood provided on an outer periphery of the main body portion and protruding downstream in the injection direction from the injection surface of the main body portion; The main body portion is a raw material gas port provided at the center of the injection surface for injecting a glass raw material gas; a fuel gas port provided on an outer periphery of the raw material gas port and configured to inject a fuel gas; A plurality of first combustion improving gas ports are provided in the fuel gas port and inject a combustion improving gas; a second combustion improving gas port provided on the outer periphery of the fuel gas port and for injecting a combustion improving gas; a first deposition step of depositing the glass particles on the target by increasing a flow rate of the fuel gas injected from the fuel gas port and keeping a constant flow rate of the combustion supporting gas injected from the second combustion supporting gas port at a start of deposition of the glass particles on the target; The method includes a second deposition process in which, after the first deposition process, the flow rate of the fuel gas injected from the fuel gas port is increased and the flow rate of the combustion supporting gas injected from the second combustion supporting gas port is increased to deposit the glass particles. Effect of the Invention
[0009] According to the present disclosure, it is possible to provide a method for manufacturing a glass base material that suppresses deterioration of a burner hood and reduces the amount of combustion supporting gas used. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a schematic diagram showing a manufacturing apparatus used in the method for manufacturing a glass base material according to this embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing a burner of the production apparatus taken along line II-II in FIG. [Diagram 3] FIG. 3 is a graph showing the evaluation results of the fuel gas and the combustion supporting gas. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] (Description of one embodiment of the present disclosure) First, embodiments of the present disclosure will be listed and described. A method for producing a glass base material according to one embodiment of the present disclosure includes: (1) A method for producing a glass base material, comprising the steps of: generating glass particles in a flame formed by a burner while reciprocating the burner relative to a target; and spraying and depositing the generated glass particles on the target, the method comprising the steps of: The burner is A main body portion, a hood provided on an outer periphery of the main body portion and protruding downstream in the injection direction from the injection surface of the main body portion; The main body portion is a raw material gas port provided at the center of the injection surface for injecting a glass raw material gas; a fuel gas port provided on an outer periphery of the raw material gas port and configured to inject a fuel gas; A plurality of first combustion improving gas ports are provided in the fuel gas port and inject a combustion improving gas; a second combustion improving gas port provided on the outer periphery of the fuel gas port and for injecting a combustion improving gas; a first deposition step of depositing the glass particles on the target by increasing a flow rate of the fuel gas injected from the fuel gas port and keeping a constant flow rate of the combustion supporting gas injected from the second combustion supporting gas port at a start of deposition of the glass particles on the target; The method includes a second deposition process in which, after the first deposition process, the flow rate of the fuel gas injected from the fuel gas port is increased and the flow rate of the combustion supporting gas injected from the second combustion supporting gas port is increased to deposit the glass particles.
[0012] According to the present disclosure, the hood provided on the outer periphery of the main body and the second combustion supporting gas port provided on the outer periphery of the fuel gas port are adjacent to each other. Furthermore, in both the first deposition step and the second deposition step, the combustion supporting gas is injected from the second combustion supporting gas port adjacent to the hood. Therefore, the combustion supporting gas injected from the second combustion supporting gas port can suppress deterioration of the hood due to red heat.
[0013] Furthermore, in the first deposition step, the flow rate of the fuel gas is increased but the flow rate of the combustion supporting gas is constant. Then, in the second deposition step, the flow rate of the combustion supporting gas is increased. Therefore, compared to the case where the flow rate of the combustion supporting gas is increased from the start of deposition in the first deposition step in order to suppress deterioration of the hood due to red heat and then the flow rate of the combustion supporting gas is kept constant until the end of the second deposition step, it is possible to suppress deterioration of the hood while suppressing the amount of combustion supporting gas used.
[0014] (2) In the above (1), in the first deposition step, the injection speed of the combustion supporting gas injected from the second combustion supporting gas port may be 2 m / sec or more.
[0015] In the first accumulation step, the injection speed of the combustion supporting gas injected from the second combustion supporting gas port is 2 m / sec, so that deterioration of the hood due to red heat can be effectively suppressed.
[0016] (3) In the above (1) or (2), in the second deposition step, the flow rate of the combustion supporting gas injected from the second combustion supporting gas port may be 0.4 to 0.6 times the flow rate of the fuel gas.
[0017] In the second deposition step, if the flow rate of the combustion supporting gas injected from the second combustion supporting gas port is less than 0.4 times the flow rate of the fuel gas, the deposition amount (deposition efficiency) of the glass particles per unit time decreases, and the time required to deposit the glass particles on the target becomes longer. In addition, the flow rate of the combustion supporting gas required to suppress deterioration of the hood due to red heat is preferably larger because the temperature of the hood decreases, but if it is too large, the surface temperature of the glass particle deposit body may decrease and the glass particle deposit body may crack. The flow rate of the combustion supporting gas may be 0.6 times or less the flow rate of the fuel gas. If the flow rate of the combustion supporting gas injected from the second combustion supporting gas port exceeds 0.6 times the flow rate of the fuel gas, the combustion supporting gas will be used excessively. In the present disclosure, in the second deposition step, the flow rate of the combustion supporting gas injected from the second combustion supporting gas port is 0.4 times or more and 0.6 times or less the flow rate of the fuel gas. Therefore, while ensuring the deposition efficiency of the glass particles, it is possible to suppress deterioration of the hood due to red heat and to avoid excessive use of combustion supporting gas.
[0018] (Details of one embodiment of the present disclosure) A specific example of a method for producing a glass base material according to an embodiment of the present disclosure will be described with reference to the drawings. It should be noted that the present disclosure is not limited to these examples, but is intended to include all modifications within the scope and meaning equivalent to the claims, as defined by the claims.
[0019] (Glass base material manufacturing equipment) First, a manufacturing apparatus used in the manufacturing method of the glass base material according to the present embodiment will be described with reference to Fig. 1. Fig. 1 is a schematic configuration diagram showing a manufacturing apparatus 1 of the glass base material. As shown in Fig. 1, the manufacturing apparatus 1 includes a reaction vessel 2, a traverse device 3, a support rod 4, a gas supply device 5, a plurality of burners 6, and a plurality of exhaust pipes 7.
[0020] The reaction vessel 2 is a vessel in which the glass particle deposit M is formed. The glass particle deposit M is formed before being made transparent as a glass base material. A traverse device 3 and a support rod 4 are provided above the reaction vessel 2. The upper part of the support rod 4 is supported by the traverse device 3. The support rod 4 is disposed by being inserted through a through hole formed in the upper wall of the reaction vessel 2. The target T is supported by the support rod 4 within the reaction vessel 2. The target T is columnar or cylindrical. The target T is, for example, a core glass rod for optical fiber mainly made of quartz glass.
[0021] The traverse device 3 is configured to rotate and vertically reciprocate the target T inside the reaction vessel 2 via a support rod 4. The traverse device 3 can control the rotation speed and vertical movement speed of the target T using a control unit (not shown). This causes the multiple burners 6 to reciprocate relative to the target T. Glass particles are sprayed from the multiple burners 6 onto the surface of the target T and deposited thereon, forming a glass particle deposit body M.
[0022] The gas supply device 5 is configured to supply glass raw material gas, fuel gas, and combustion supporting gas to each of the plurality of burners 6. The glass raw material gas is, for example, silicon tetrachloride (SiCl4) gas. The fuel gas is, for example, hydrogen (H2) gas. The combustion supporting gas is, for example, oxygen (O2) gas. In addition, the gas supply device 5 may supply, for example, nitrogen (N2) gas as a seal gas to each of the plurality of burners 6. The gas supply device 5 can control the flow rate per unit time (hereinafter simply referred to as "flow rate") and the flow velocity per unit time (hereinafter simply referred to as "flow velocity") of each gas by a control unit (not shown).
[0023] A plurality of burners 6 are attached to the side of the reaction vessel 2. In this embodiment, eight burners 6 are provided. Furthermore, a plurality of exhaust pipes 7 are attached to the other side of the reaction vessel 2 (a side at a position different from the position where the plurality of burners 6 are attached). Each of the plurality of exhaust pipes 7 is configured to exhaust glass particles that have not adhered to the glass particle deposit body M to the outside of the reaction vessel 2. In this embodiment, three exhaust pipes 7 are provided.
[0024] Each of the burners 6 is configured to inject a glass raw material gas, a fuel gas, and a combustion supporting gas toward the target T. The burners 6 may be configured to inject a seal gas in addition. In the flame formed by the fuel gas and the combustion supporting gas, the glass raw material gas undergoes a flame decomposition reaction, thereby generating glass particles. Each of the burners 6 is configured to spray the glass particles toward the target T.
[0025] Each of the burners 6 is cylindrical. Each of the burners 6 has a main body 61 and a hood 69. The hood 69 is provided on the outer periphery of the main body 61 and protrudes downstream in the injection direction of the glass raw material gas from the injection surface 62 of the main body 61. The length from the injection surface 62 to the tip of the hood 69 in the injection direction is, for example, 50 mm to 100 mm.
[0026] FIG. 2 is a cross-sectional view showing the burner 6 taken along line II-II in FIG. 2, the main body 61 has a multiple tube structure. The main body 61 has a raw material gas port 63, a fuel gas port 65, a plurality of first combustion supporting gas ports 66, and a second combustion supporting gas port 67. In addition, the main body 61 may have a seal gas port 64.
[0027] The raw material gas port 63 is provided in the center of the ejection surface 62. The raw material gas port 63 is configured to eject a glass raw material gas toward the target T.
[0028] The seal gas port 64 may be concentric with the raw material gas port 63 and provided between the raw material gas port 63 and the fuel gas port 65. The seal gas port 64 is configured to inject a seal gas so that the glass raw material gas injected from the raw material gas port 63 does not react with the fuel gas near the injection surface 62.
[0029] The fuel gas port 65 is provided on the outer periphery of the raw gas port 63. In the case where the main body 61 has the seal gas port 64, the fuel gas port 65 is provided on the outer periphery of the raw gas port 63 via the seal gas port 64. The fuel gas port 65 is provided concentrically with the raw gas port 63. The inner diameter of the fuel gas port 65 is larger than the inner diameter of the raw gas port 63. The fuel gas port 65 is configured to inject fuel gas toward the target T.
[0030] A plurality of first combustion supporting gas ports 66 are provided in the fuel gas port 65. Each of the plurality of first combustion supporting gas ports 66 is configured to inject a combustion supporting gas toward the target T. In this embodiment, eight first combustion supporting gas ports 66 are provided around the raw material gas port 63. The inner diameter of each of the first combustion supporting gas ports 66 is smaller than the inner diameter of the raw material gas port 63.
[0031] The second combustion supporting gas port 67 is provided on the outer periphery of the fuel gas port 65. The second combustion supporting gas port 67 is provided concentrically with the raw material gas port 63. The inner diameter of the second combustion supporting gas port 67 is larger than the inner diameter of the fuel gas port 65. The second combustion supporting gas port 67 is provided so as to inject a combustion supporting gas toward the target T.
[0032] In this embodiment, the second combustion improving gas port 67 is provided on the outermost side of the ejection surface 62. A hood 69 is provided on the outer periphery of the main body 61, and the second combustion improving gas port 67 and the hood 69 are adjacent to each other.
[0033] (Method of manufacturing glass base material) Next, a method for manufacturing the glass base material according to this embodiment will be described. The method for manufacturing the glass base material according to this embodiment is an outside vapor deposition (OVD) method. In the OVD method, at least one burner 6 is moved back and forth relative to the target T. Furthermore, glass particles are generated in a flame formed by the burner 6, and the generated glass particles are sprayed and deposited on the target T to form a glass particle deposit body M.
[0034] The method for producing a glass base material according to the present embodiment includes a first deposition step, a second deposition step, and a dehydration and sintering step.
[0035] The first and second deposition steps are both steps for depositing glass particles on a target T. In both the first and second deposition steps, each of the burners 6 injects a glass raw material gas, a fuel gas, and a combustion supporting gas. In each burner 6, the glass raw material gas undergoes a flame decomposition reaction in a flame formed by the fuel gas and the combustion supporting gas, and glass particles are generated. The generated glass particles are sprayed onto the target T. Furthermore, the burners 6 are reciprocated relative to the target T. In this embodiment, the traverse device 3 reciprocates the target T in the vertical direction while rotating it via the support rod 4. In this way, the glass particles are successively deposited in the radial direction of the target T, and a glass particle deposit body M is formed.
[0036] The first deposition step is an initial step of depositing glass particles on the target T. The first deposition step includes the start of deposition of glass particles on the target T. In the first deposition step, the flow rate of the fuel gas injected from the fuel gas port 65 is increased, and the flow rate of the combustion supporting gas injected from the second combustion supporting gas port 67 is kept constant, so that the glass particles are deposited on the target T. Furthermore, in the first deposition step, the glass raw material gas is injected from the raw material gas port 63, and the combustion supporting gas is also injected from the first combustion supporting gas port 66. In the first deposition step, the flow rate per unit time of the raw material gas is kept constant, for example. In the first deposition step, the flow rate per unit time of the fuel gas is increased, for example, to 1.5 times the flow rate at the start of deposition. In the first deposition step, the flow rate per unit time of the combustion supporting gas injected from the first combustion supporting gas port 66 is kept constant, for example. In the first deposition step, the flow rate per unit time of the combustion supporting gas injected from the second combustion supporting gas port 67 is kept constant, for example. -5 m 3 / s (0°C, 1 atm equivalent value) to 84 x 10 -5 m 3 / s (0°C, 1 atmosphere equivalent value).
[0037] In the first deposition step, the injection speed of the combustion supporting gas injected from the second combustion supporting gas port 67 is 2 m / sec or more. In this embodiment, the gas supply device 5 controls the flow rate or flow speed of the combustion supporting gas so that the injection speed of the combustion supporting gas is 2 m / sec or more, and supplies the combustion supporting gas to each of the multiple burners 6.
[0038] The second deposition step is a step of further depositing glass particles on the target T after the first deposition step. In the second deposition step, the flow rate of the fuel gas injected from the fuel gas port 65 is increased, and the flow rate of the combustion supporting gas injected from the second combustion supporting gas port 67 is increased, so that the glass particles are further deposited on the target T. Furthermore, in the second deposition step, the glass raw material gas is injected from the raw material gas port 63, and the combustion supporting gas is also injected from the first combustion supporting gas port 66. In the second deposition step, the flow rate per unit time of the combustion supporting gas injected from the second combustion supporting gas port 67 is increased, for example, from the flow rate in the first deposition step to 1.3 times the flow rate in the first deposition step. The flow rate per unit time of the other gas in the second deposition step is the same as the flow rate per unit time of the other gas in the first deposition step.
[0039] In the second deposition step, the flow rate of the combustion supporting gas injected from the second combustion supporting gas port 67 is 0.4 to 0.6 times the flow rate of the fuel gas. In this embodiment, the gas supply device 5 can control the flow rates of the combustion supporting gas and the fuel gas by a control unit (not shown). In this manner, through the first and second deposition steps, a soot glass deposit body M is formed.
[0040] The dehydration and sintering step is a step in which the soot glass deposit M formed after the second deposition step is heated in a dehydration and sintering furnace to make it transparent and form a glass base material. For example, the soot glass deposit M is dehydrated by being heated in a mixed atmosphere of inert gas and chlorine gas in a dehydration and sintering furnace, and then sintered and made transparent by being further heated in a helium gas atmosphere. In this way, a transparent glass base material is formed.
[0041] As described above, in this embodiment, the hood 69 provided on the outer periphery of the main body 61 and the second combustion supporting gas port 67 provided on the outer periphery of the fuel gas port 65 are adjacent to each other. Furthermore, in both the first deposition step and the second deposition step, the combustion supporting gas is injected from the second combustion supporting gas port 67 adjacent to the hood 69. Therefore, the combustion supporting gas injected from the second combustion supporting gas port 67 can suppress deterioration of the hood 69 due to red heat.
[0042] In the first deposition step, the flow rate of the combustion supporting gas injected from the second combustion supporting gas port 67 is constant. Then, in the second deposition step, the flow rate of the combustion supporting gas is increased. Therefore, the amount of combustion supporting gas used can be reduced compared to the case where the flow rate of the combustion supporting gas is increased from the start of deposition in the first deposition step in order to suppress deterioration of the hood due to red heat, and then the flow rate of the combustion supporting gas is kept constant until the end of the second deposition step.
[0043] Furthermore, by suppressing the amount of combustion supporting gas used in the first accumulation step, the flow rate of the combustion supporting gas supplied to the reaction vessel 2 is also reduced. As a result, the amount of chlorine generated by the flame decomposition reaction of the glass raw material gas is relatively reduced. Chlorine generally accumulates in the exhaust pipe 7, and its treatment is costly, but since the amount of chlorine is reduced, the cost of such chlorine treatment can also be reduced.
[0044] In this embodiment, the injection speed of the combustion supporting gas in the first deposition step is 2 m / sec or more, which makes it possible to suppress deterioration of the hood 69 due to red heat.
[0045] In the second deposition step, if the flow rate of the combustion supporting gas injected from the second combustion supporting gas port 67 is less than 0.4 times the flow rate of the fuel gas, the deposition amount (deposition efficiency) of the glass particles per unit time decreases, and the time required to deposit the glass particles on the target T becomes longer. In addition, the flow rate of the combustion supporting gas required to suppress the deterioration of the hood 69 due to red heat is preferably larger because the temperature of the hood decreases, but if it is too large, the surface temperature of the glass particle deposit body may decrease and the glass particle deposit body may crack. The flow rate of the combustion supporting gas may be 0.6 times or less than the flow rate of the fuel gas. If the flow rate of the combustion supporting gas exceeds 0.6 times the flow rate of the fuel gas, the combustion supporting gas will be used excessively. In this embodiment, in the second deposition step, the flow rate of the combustion supporting gas injected from the second combustion supporting gas port 67 is 0.4 times or more and 0.6 times or less than the flow rate of the fuel gas. Therefore, while ensuring the deposition efficiency of the glass particles, it is possible to suppress the deterioration of the hood 69 due to red heat and avoid excessive use of the combustion supporting gas.
[0046] (Evaluation experiment) The fuel gas and the combustion supporting gas were evaluated when glass particles were deposited on a target T using the manufacturing apparatus 1 shown in Figure 1. In the evaluation experiment, the fuel gas was hydrogen (H2) gas, and the combustion supporting gas was oxygen (O2) gas.
[0047] FIG. 3 is a graph showing the evaluation results of the fuel gas and the combustion supporting gas. The horizontal axis of FIG. 3 is the deposition time for depositing the glass particles on the target T. The deposition time shown in FIG. 3 includes the first deposition process and the second deposition process. The combustion supporting gas shown in FIG. 3 does not include the combustion supporting gas injected from the first combustion supporting gas port 66, but only the combustion supporting gas injected from the second combustion supporting gas port 67. It should be noted that immediately after the start of deposition, each gas is temporarily injected in large amounts to form a flame in the burner 6. However, since the effect is not large from the viewpoint of depositing the glass particles on the target T, the temporary increase in the flow rate of each gas immediately after the start of deposition is not taken into consideration. The vertical axis of FIG. 3 shows the flow rate of each gas when the flow rate of the fuel gas is normalized.
[0048] As shown in FIG. 3, in the first deposition step, the flow rate of the fuel gas injected from the fuel gas port 65 increases. At this time, the injection speed of the combustion supporting gas is 2 m / sec or more. In addition, the flow rate of the combustion supporting gas injected from the second combustion supporting gas port 67 is constant. The flow rate of the combustion supporting gas is, for example, 50×10 -5 m 3 / s (0°C, 1 atm equivalent value) to 84 x 10 -5 m 3 / s (0℃, 1 atmosphere equivalent value).
[0049] It was confirmed that the temperature of the hood 69 at the position farthest from the injection surface 62 of the burner 6 did not exceed 750° C. during the first deposition step. From the above, it was confirmed that the manufacturing method of this embodiment can suppress deterioration of the hood 69 due to red heat during the first deposition step.
[0050] Furthermore, in the first deposition step, the flow rate of the combustion supporting gas is constant. Then, in the second deposition step, the flow rate of the combustion supporting gas is increased. Therefore, it was confirmed that the amount of the combustion supporting gas used can be reduced compared to the case where the flow rate of the combustion supporting gas is increased from the start of deposition in the first deposition step in order to suppress deterioration of the hood due to red heat, and the flow rate of the combustion supporting gas is then kept constant until the end of the second deposition step.
[0051] In the second deposition process, the flow rate of the fuel gas injected from the fuel gas port 65 increases. At this time, the injection speed of the combustion supporting gas is 2 m / sec or more. The flow rate of the combustion supporting gas injected from the second combustion supporting gas port 67 also increases. FIG. 3 shows a flow rate that is 0.4 times the flow rate of the fuel gas and a flow rate that is 0.6 times the flow rate of the fuel gas with dashed lines, indicating that the flow rate of the combustion supporting gas during the second deposition process is 0.4 to 0.6 times the flow rate of the fuel gas.
[0052] It was confirmed that the temperature of the hood 69 at the position farthest from the injection surface 62 of the burner 6 did not exceed 750° C. even during the second deposition process. From the above, it was confirmed that even if the flow rate of the combustion supporting gas is 0.4 to 0.6 times the flow rate of the fuel gas during the second deposition process, the manufacturing method of this embodiment can suppress deterioration of the hood 69 due to red heat.
[0053] Although the present disclosure has been described in detail and with reference to specific embodiments, it is clear to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present disclosure. Furthermore, the number, position, shape, etc. of the components described above are not limited to the above embodiments, and can be changed to the number, position, shape, etc. that are suitable for implementing the present disclosure. [Explanation of symbols]
[0054] 1 Manufacturing equipment 2 Reaction vessel 3 Traverse device 4 Support rod 5 Gas supply equipment 6 Burner 7. Exhaust pipe 61 Main body 62 Injection surface 63 Raw gas port 64 Seal gas port 65 Fuel gas port 66 First auxiliary combustion gas port 67 Second auxiliary combustion gas port 69 Food
Claims
1. A method for producing a glass base material, comprising: generating glass particles in a flame formed by a burner while reciprocating a burner relative to a target; and spraying and depositing the generated glass particles on the target, the method comprising the steps of: The burner is A main body portion, a hood provided on an outer periphery of the main body portion and protruding downstream in the injection direction from the injection surface of the main body portion; The main body portion is a raw material gas port provided at the center of the injection surface for injecting a glass raw material gas; a fuel gas port provided on an outer periphery of the raw material gas port and configured to inject a fuel gas; A plurality of first combustion improving gas ports are provided in the fuel gas port and inject a combustion improving gas; a second combustion improving gas port provided on the outer periphery of the fuel gas port and for injecting a combustion improving gas; a first deposition step of depositing the glass particles on the target by increasing a flow rate of the fuel gas injected from the fuel gas port and keeping a constant flow rate of the combustion supporting gas injected from the second combustion supporting gas port at a start of deposition of the glass particles on the target; a second deposition step of depositing the glass particles by increasing a flow rate of the fuel gas injected from the fuel gas port and increasing a flow rate of the combustion supporting gas injected from the second combustion supporting gas port after the first deposition step.
2. 2. The method for producing a glass base material according to claim 1, wherein in the first depositing step, the combustion assisting gas is injected from the second combustion assisting gas port at a jet speed of 2 m / sec or more.
3. 3. The method for producing a glass base material according to claim 1, wherein in the second deposition step, a flow rate of the combustion supporting gas injected from the second combustion supporting gas port is 0.4 to 0.6 times a flow rate of the fuel gas.
Citation Information
Patent Citations
Manufacturing method of porous glass particulate-deposited body and burner for glass synthesis used for the same
JP2004331440A
Glass preform and method of manufacturing glass
JP2006160551A
Method of synthesizing glass microparticles
WO2017188334A1