Multilayer film

A multilayer film with specific layer compositions and structures addresses the limitations of existing materials by providing superior thermal and dielectric properties, enhancing adhesion to copper, and suitability for advanced electronic applications.

JP2024154817AInactive Publication Date: 2024-10-31SHIN ETSU CHEMICAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023068914
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-20
Publication Date
2024-10-31
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing materials for printed wiring boards, such as modified polyphenylene ether resin and epoxy resin, fail to meet the requirements of low dielectric constant, low dielectric loss tangent, high heat resistance, and high adhesion to copper, especially in high-frequency applications.

Method used

A multilayer film composed of layers A, B, and C, where layers A and C contain cyclic imide compounds and a curing catalyst, and layer B contains modified polyphenylene ether and a curing catalyst, with specific organic groups and thicknesses to enhance adhesion and thermal properties.

Benefits of technology

The multilayer film achieves excellent heat resistance, low dielectric constant, low dielectric loss tangent, and high adhesion to copper, making it suitable for copper-clad laminates, printed wiring boards, flexible printed wiring boards, and semiconductor encapsulants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154817000001
    Figure 2024154817000001
  • Figure 2024154817000002
    Figure 2024154817000002
  • Figure 2024154817000003
    Figure 2024154817000003
Patent Text Reader

Abstract

To provide a multilayer film that yields a cured product with high adhesion to copper while having superior heat resistance as well as low dielectric constant and low dielectric loss tangent.SOLUTION: A multilayer film has layer A, layer B and layer C, represented by the following compositions. Layer A, layer B and layer C are laminated in the stated order. Layer A: a layer containing (a1) a cyclic imide compound and (a2) a curing catalyst. Layer B: a layer containing (b1) a modified polyphenylene ether and (b2) a curing catalyst. Layer C: a layer containing (c1) a cyclic imide compound and (c2) a curing catalyst.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a multilayer film, and in particular to a multilayer film used for copper-clad laminates, printed wiring boards, base films for flexible printed wiring boards, coverlay films, semiconductor encapsulants, and the like. [Background technology]

[0002] In recent years, the speed and capacity of signals used in electronic devices such as mobile phones, their base station equipment, servers, routers and other network infrastructure devices, and large computers have been increasing year by year. Accordingly, high frequencies such as the 20 GHz range are used for the printed wiring boards mounted on these electronic devices, and the properties required of printed wiring board materials are becoming increasingly higher, such as low dielectric constant, low dielectric loss tangent, low thermal expansion coefficient, high heat resistance, and low water absorption.

[0003] Materials that may satisfy these properties include modified polyphenylene ether resins and epoxy resins (Patent Documents 1 and 2). However, modified polyphenylene ether resins have low adhesive strength and do not fully satisfy the characteristics required for printed wiring board materials, and epoxy resins have high adhesive strength but high dielectric constants and dielectric loss tangents, making them unsuitable for use in high frequency bands.

[0004] As a method for solving these problems, a composite film having layers with different thicknesses or viscosities, one of which contains a polyimide compound and an inorganic filler and the other of which contains a multifunctional epoxy resin and a phenolic hydroxyl group-containing polyamide resin, has been proposed (Patent Documents 3-4). However, it has been found that even these composite films do not have sufficient heat resistance and adhesive strength. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2019-1965 A [Patent Document 2] JP 2018-28044 A [Patent Document 3] JP 2018-14388 A [Patent Document 4] JP 2018-12259 A Summary of the Invention [Problem to be solved by the invention]

[0006] Therefore, an object of the present invention is to provide a multilayer film that, when cured, has excellent heat resistance, a low dielectric constant, a low dielectric dissipation factor, and high adhesion to copper. [Means for solving the problem]

[0007] As a result of intensive research aimed at solving the above problems, the present inventors have found that the following multilayer film can achieve the above object, and have completed the present invention.

[0008] That is, the present invention provides the following multilayer film. [1] A multilayer film having layers A, B and C having the following composition, laminated in this order: A layer (a1): a cyclic imide compound represented by the following formula (1), (a2):Curing catalyst B layer (b1): Modified polyphenylene ether and (b2):Curing catalyst C layer (c1): a cyclic imide compound represented by the following formula (1), (c2):Curing catalyst [ka] (In formula (1), A independently represents a tetravalent organic group containing a cyclic structure. Q independently represents a divalent hydrocarbon group having 6 or more carbon atoms which does not contain an aromatic group which may contain a heteroatom. B independently represents an arylene group having 6 or more carbon atoms which may contain a heteroatom. X independently represents a hydrogen atom or a methyl group, n represents 0 to 200, and m represents 0 to 200.) [2] The multilayer film according to [1], wherein the resin composition constituting layer A and the resin composition constituting layer C are the same resin composition. [3] The multilayer film according to [1] or [2], wherein the organic group represented by A in the formula (1) is any one of tetravalent organic groups represented by the following structural formulas: [ka] (The bond not bonded to a substituent in the above structural formula is bonded to the carbonyl carbon that forms a cyclic imide structure in formula (1).) [4] The multilayer film according to any one of [1] to [3], wherein the divalent hydrocarbon group represented by Q in formula (1) is selected from the group consisting of divalent hydrocarbon groups represented by the following structural formulas and divalent hydrocarbon groups derived from a dimer acid skeleton: [ka] (R 1 Each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 20 carbon atoms. 1 and p 2 are each a number equal to or greater than 5 and may be the same or different, and p 3 and p 4 are each a number equal to or greater than 0 and may be the same or different, and p 5 and p 6 are each a number of 0 or more, and may be the same or different. The bond to which no substituent is bonded in the above structural formula is bonded to the nitrogen atom that forms a cyclic imide structure in formula (1). [5] The multilayer film according to any one of [1] to [4], wherein the arylene group represented by B in formula (1) is any one of arylene groups represented by the following structural formulas: [ka] (R 2 are each independently a hydrogen atom, a halogen atom, or an alkyl group having 1 to 6 carbon atoms; R 3 are each independently a hydrogen atom, a halogen atom, a methyl group, or a trifluoromethyl group, and Z is an oxygen atom, a sulfur atom, or a methylene group. The bond to which no substituent is bonded in the above structural formula is bonded to the nitrogen atom that forms a cyclic imide structure in formula (1). [6] The multilayer film according to any one of [1] to [5], wherein the cyclic imide compound of the component (a) is a cyclic imide compound represented by formula (1) in which m is 0. [7] The multilayer film according to any one of [1] to [6], wherein each of the layer A and the layer C has a thickness of 0.1 to 20 μm. [8] The multilayer film according to any one of [1] to [7], wherein the thickness of layer B is 20 to 100 μm. [9] The multilayer film according to any one of [1] to [8], wherein the minimum melt viscosity of layer A and layer C at 25 to 150° C. is 0.1 to 100 Pa·s.

[10] The multilayer film according to any one of [1] to [9], wherein the linear expansion coefficient of a cured product of layer B at 25 to 150° C. is 1 to 50 ppm / K. Effect of the Invention

[0009] The multilayer film of the present invention has excellent heat resistance, a low dielectric constant, a low dielectric loss tangent, and high adhesion to copper, and is therefore useful for applications such as copper-clad laminates, printed wiring boards, and base films for flexible printed wiring boards, coverlay films, and semiconductor encapsulants. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] <Multilayer film> The multilayer film of the present invention has a layer A, a layer B and a layer C represented by the following composition, with at least the layer A, the layer B and the layer C being arranged in this order, and preferably the layer A, the layer B and the layer C being arranged adjacent to one another in this order, and for example, the film may further have another layer such as a support or a protective film on the outermost layer side of the layer A or the layer C. A layer (a1): a layer containing a cyclic imide compound represented by the following formula (1) and (a2): a layer containing a curing catalyst B layer (b1): modified polyphenylene ether and (b2): layer containing a curing catalyst C layer (c1): a layer containing a cyclic imide compound represented by the following formula (1) and (c2): a layer containing a curing catalyst The A layer is formed from a resin composition containing (a1) and (a2), and in this specification, the resin composition may be referred to as the "resin composition constituting the A layer" or the "resin composition of the A layer". Similarly, the B layer is formed from a resin composition containing (b1) and (b2), and the resin composition may be referred to as the "resin composition constituting the B layer" or the "resin composition of the B layer", and the C layer is formed from a resin composition containing (c1) and (c2), and the resin composition may be referred to as the "resin composition constituting the C layer" or the "resin composition of the C layer". In the multilayer film of the present invention, the resin compositions constituting Layer A, Layer B and Layer C are each independently in an uncured state or in a semi-cured B-stage state.

[0011] [(a1) component, (c1) component] The component (a1) of Layer A and the component (c1) of Layer C are cyclic imide compounds represented by the following formula (1): The resin compositions constituting the outermost layers, Layer A and Layer C, contain the cyclic imide compound, and high adhesion to copper is achieved by reaction of the cyclic imide group of the cyclic imide compound. [ka] (In formula (1), A independently represents a tetravalent organic group containing a cyclic structure. Q independently represents a divalent hydrocarbon group having 6 or more carbon atoms which does not contain an aromatic group which may contain a heteroatom. B independently represents an arylene group having 6 or more carbon atoms which may contain a heteroatom. X independently represents a hydrogen atom or a methyl group, n represents 0 to 200, and m represents 0 to 200.)

[0012] The organic groups represented by A in formula (1) are independently tetravalent organic groups containing a cyclic structure, and are particularly preferably any of the tetravalent organic groups represented by the following structural formulas. [ka] (The bond not bonded to a substituent in the above structural formula is bonded to the carbonyl carbon that forms a cyclic imide structure in formula (1).)

[0013] Q in formula (1) is independently a divalent hydrocarbon group having 6 or more carbon atoms that does not contain an aromatic group which may contain a heteroatom, and is preferably a divalent hydrocarbon group represented by any of the following structural formulas or a divalent hydrocarbon group derived from a dimer acid skeleton: [ka] The bond not bonded to a substituent in the above structural formula is bonded to the nitrogen atom forming a cyclic imide structure in formula (1).

[0014] In the above structural formula, R 1 R each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 20 carbon atoms. 1is preferably a hydrogen atom or a linear or branched alkyl group having 1 to 10 carbon atoms, and more preferably a hydrogen atom or a linear alkyl group having 1 to 10 carbon atoms. In the above structural formula, p 1 and p 2 are each a number of 5 or more, preferably a number of 5 to 12, more preferably a number of 6 to 10, and may be the same or different. In the above structural formula, p 3 and p 4 are each a number of 0 or more, preferably a number of 0 to 4, more preferably a number of 0 to 3, and may be the same or different. In the above structural formula, p 5 and p 6 are each a number of 0 or more, preferably a number of 0 to 4, more preferably a number of 0 to 2, and may be the same or different.

[0015] The divalent hydrocarbon group derived from the dimer acid skeleton is a group derived from dimer acid, a liquid fatty acid mainly composed of a dicarboxylic acid having 36 carbon atoms, which is produced by dimerization of unsaturated fatty acids having 18 carbon atoms, which are derived from natural products such as vegetable oils and fats. Dimer acids do not have a single skeleton, but have multiple structures, and there are several types of isomers. The dimer acid skeleton refers to a group derived from a dimer diamine having a structure in which the carboxyl group of such a dimer acid is substituted with a primary aminomethyl group. From the viewpoint of the heat resistance and reliability of the cured product, it is more preferable that the divalent hydrocarbon group derived from the dimer acid skeleton has a structure in which the carbon-carbon double bond in the hydrocarbon group derived from the dimer acid skeleton is reduced by a hydrogenation reaction. Generally, dimer acids may contain trimers (trimer acids) due to the use of natural products such as vegetable oils and fats as raw materials. However, it is preferable that the proportion of hydrocarbon groups derived from dimer acids among the hydrocarbon groups derived from dimer acids and trimer acids is high, for example, 95 mass% or more, because this tends to result in excellent dielectric properties, excellent moldability due to a tendency for the viscosity to decrease when heated, and reduced effects of moisture absorption. As described above, the dimer acid skeleton has a plurality of structures, and therefore, in this specification, the divalent hydrocarbon group derived from the dimer acid skeleton is referred to as the average structure, i.e., -C 36 H 70 It may be written as -.

[0016] In formula (1), B is independently an arylene group having 6 or more carbon atoms which may contain a heteroatom, and is preferably an arylene group represented by any of the following structural formulas. [ka] The bond not bonded to a substituent in the above structural formula is bonded to the nitrogen atom forming a cyclic imide structure in formula (1).

[0017] In the above formula, R 2 are each independently a hydrogen atom, a halogen atom or an alkyl group having 1 to 6 carbon atoms, and are preferably a hydrogen atom or a methyl group. In the above formula, R 3 are each independently a hydrogen atom, a halogen atom, a methyl group or a trifluoromethyl group, and are preferably a methyl group or a trifluoromethyl group. In the above formula, Z is an oxygen atom, a sulfur atom or a methylene group, and is preferably an oxygen atom.

[0018] In formula (1), X is a hydrogen atom or a methyl group.

[0019] In the formula (1), n ​​is an integer of 0 to 200, preferably 1 to 100, and more preferably 2 to 50. In the formula (1), m is an integer of 0 to 200, preferably 0 to 100, and more preferably 0 to 50.

[0020] In the above formula (1), when m=0, the cyclic imide compound of the component (a) is represented by the following formula (1′). [ka] (In formula (1'), A, Q, X, and n are the same as those in formula (1).)

[0021] The weight average molecular weight (Mw) of the cyclic imide compound represented by formula (1) is not particularly limited, but is preferably 2,000 to 1,000,000, more preferably 3,000 to 100,000, and even more preferably 3,500 to 50,000. If the weight average molecular weight (Mw) is within this range, the resin composition has sufficient strength and the terminal cyclic imide groups can be efficiently reacted.

[0022] The weight average molecular weight (Mw) referred to in this specification refers to the weight average molecular weight measured by GPC under the following conditions using polystyrene as the standard. [GPC measurement conditions] Developing solvent: Tetrahydrofuran Flow rate: 0.6mL / min Column: TSK Guardcolumn SuperH-L TSKgel SuperH4000(6.0mmI.D.×15cm×1) TSKgel SuperH3000(6.0mmI.D.×15cm×1) TSKgel SuperH2000(6.0mmI.D.×15cm×2) (All manufactured by Tosoh Corporation) Column temperature: 40℃ Sample injection volume: 20 μL (sample concentration: 0.5% by mass in tetrahydrofuran solution) Detector: Differential refractometer (RI)

[0023] The method for producing the cyclic imide compound represented by formula (1) (e.g., a maleimide compound, a citraconic imide compound, etc.) is not particularly limited. For example, the compound may be produced by reacting an amine compound with an excess of maleic anhydride or citraconic anhydride, or the compound may be produced by reacting an acid anhydride with a diamine to synthesize an amine-terminated compound, and then reacting the amine-terminated compound with an excess of maleic anhydride or citraconic anhydride.

[0024] Examples of the acid anhydride include pyromellitic anhydride, maleic anhydride, succinic anhydride, 4,4'-carbonyldiphthalic anhydride, 4,4'-diphthalic anhydride, 4,4'-sulfonyldiphthalic anhydride, 4,4'-oxydiphthalic anhydride, 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride, etc. These acid anhydrides may be used alone or in combination of two or more depending on the purpose, application, etc. From the viewpoint of the electrical properties of the cyclic imide compound, the acid anhydride is preferably pyromellitic anhydride, 4,4'-oxydiphthalic anhydride, or 4,4'-(4,4'-isopropylidenediphenoxy)diphthalic anhydride.

[0025] Examples of diamines include 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 4,4'-diamino-3,3'-dimethyldiphenylmethane, 4,4'-diamino-3,3'-diethyldiphenylmethane, 4,4'-diaminodiphenyl ether, 4,4'-diamino-3,3',5,5'-tetraethyldiphenylmethane, tetramethyl-1,3-bis(3-aminopropyl)disiloxane, and bis[4-(4-aminophenoxy)phenyl]sulfone. , 4,4'-diaminodiphenylmethane, 1,3-bis(4-aminophenoxy)benzene, 1,12-diaminododecane, 1,10-diaminodecane, dimer diamine, octyldiamine, 1,3-di(aminomethyl)cyclohexane, isophoronediamine, 2,4,4-trimethylhexane-1,6-diamine, 2-methylpentane-1,5-diamine, 3(4),8(9)-bis(aminomethyl)tricyclo[5.2.1.0(2,6)]decane, etc. These diamines may be used alone or in combination of two or more depending on the purpose, application, etc. From the viewpoint of the electrical properties of the cyclic imide compounds, the diamines are aromatic diamines such as 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 4,4'-diamino-3,3'-dimethyldiphenylmethane, 4,4'-diamino-3,3'-diethyldiphenylmethane, 4,4'-diaminodiphenylether, 4,4'-diamino-3,3',5,5'-tetraethyldiphenylmethane; tetramethyl-1,3-bis(3-aminopropyl)disilane; Aliphatic diamines such as hexane, 1,12-diaminododecane, 1,10-diaminodecane, dimer diamine, octyldiamine, 1,3-di(aminomethyl)cyclohexane, 1-amino-4-(aminomethyl)cyclohexane, 1,3-diaminoadamantane, isophoronediamine, 2,4,4-trimethylhexane-1,6-diamine, and 2-methylpentane-1,5-diamine are preferred, and dimer diamine and isophoronediamine are particularly preferred.

[0026] The cyclic imide compound represented by formula (1) may be a commercially available product. Examples of commercially available products include BMI-689, BMI-1400, BMI-1500, BMI-2500, BMI-3000, and BMI-6100 (all manufactured by Designer Molecules Inc.), SLK-6895, SLK-3000, SLK-2600, SLK-2700, and SLK-6100 (all manufactured by Shin-Etsu Chemical Co., Ltd.).

[0027] The cyclic imide equivalent of the cyclic imide group represented by formula (1) is preferably 0.001 to 0.5 mol / 100 g, more preferably 0.003 to 0.4 mol / 100 g, even more preferably 0.01 to 0.3 mol / 100 g, and even more preferably 0.02 to 0.2 mol / 100 g. This range is preferable because the cured product of the multilayer film has a low relative dielectric constant, a low dielectric tangent, and high adhesion.

[0028] [(a2) component, (c2) component] The resin compositions of the layers A and C contain a curing catalyst as the component (a2) and the component (c2). The curing catalyst is not particularly limited, but examples thereof include a thermal radical polymerization initiator and a thermal anionic polymerization initiator.

[0029] Examples of the thermal radical polymerization initiator include methyl ethyl ketone peroxide, methylcyclohexanone peroxide, methylacetoacetate peroxide, acetylacetone peroxide, 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane, 1,1-bis(t-hexylperoxy)cyclohexane, 1,1-bis(t-hexylperoxy)3,3,5-trimethylcyclohexane, 1,1-bis(t-butylperoxy)cyclohexane, 2,2-bis(4,4-di-t -butylperoxycyclohexyl)propane, 1,1-bis(t-butylperoxy)cyclododecane, n-butyl-4,4-bis(t-butylperoxy)valerate, 2,2-bis(t-butylperoxy)butane, 1,1-bis(t-butylperoxy)-2-methylcyclohexane, t-butyl hydroperoxide, p-menthane hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, t-hexyl hydroperoxide, dicumyl peroxide, 2,5-dimethyl 2,5-diethyl-2,5-bis(t-butylperoxy)hexane, α,α'-bis(t-butylperoxy)diisopropylbenzene, t-butylcumyl peroxide, di-t-butyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexyne-3, isobutyryl peroxide, 3,5,5-trimethylhexanoyl peroxide, octanoyl peroxide, lauroyl peroxide, cinnamic acid peroxide, m-toluoyl peroxide, benzoyl peroxide, diisopropyl Pyl peroxydicarbonate, bis(4-t-butylcyclohexyl) peroxydicarbonate, di-3-methoxybutyl peroxydicarbonate, di-2-ethylhexyl peroxydicarbonate, di-sec-butyl peroxydicarbonate, di(3-methyl-3-methoxybutyl) peroxydicarbonate, di(4-t-butylcyclohexyl) peroxydicarbonate, α,α'-bis(neodecanoylperoxy)diisopropylbenzene, cumyl peroxyneodecanoate, 1,1,3,3-Tetramethylbutylperoxyneodecanoate, 1-cyclohexyl-1-methylethylperoxyneodecanoate, t-hexylperoxyneodecanoate, t-butylperoxyneodecanoate, t-hexylperoxypivalate, t-butylperoxypivalate, 2,5-dimethyl-2,5-bis(2-ethylhexanoylperoxy)hexane, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, 1-cyclohexyl-1-methylethylperoxy-2-ethylhexanoate, t-hexylperoxy peroxy-2-ethylhexanoate, t-butylperoxy-2-ethylhexanoate, t-butylperoxyisobutyrate, t-butylperoxymaleic acid, t-butylperoxylaurate, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxyisopropyl monocarbonate, t-butylperoxy-2-ethylhexyl monocarbonate, 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane, t-butylperoxyacetate, t-hexylperoxybenzoate, t-butylperoxyethylhexanoate, Organic peroxides such as 2,2'-azobis(N-butyl-2-methylpropionamide), 2,2'-azobis(N-cyclohexyl-2-methylpropionamide), 2,2'-azobis[N-(2-methylpropyl)-2-methylpropionamide], 2,2'-azobis[N-(2-methylethyl)-2- ... 2,2'-azobis(N-hexyl-2-methylpropionamide), 2,2'-azobis(N-propyl-2-methylpropionamide), 2,2'-azobis(N-ethyl-2-methylpropionamide), 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 2,2'-azobis[N-(2-propenyl)-2-methylpropionamide], 2,2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide}, 2,Examples of the azo compounds include 2'-azobis[N-(2-propenyl)-2-methylpropionamide] and dimethyl-1,1'-azobis(1-cyclohexanecarboxylate).

[0030] Examples of the thermal anionic polymerization initiator include amine compounds such as triethylamine, triethylenediamine, 2-(dimethylaminomethyl)phenol, 1,8-diaza-bicyclo[5.4.0]undecene-7, tris(dimethylaminomethyl)phenol, and benzyldimethylamine; and isomers such as 2-methylimidazole, 2-ethylimidazole, 2-phenylimidazole, 2-ethyl-4-methylimidazole, 2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 2,4-diamino-6-[2-(2-methyl-1-imidazolyl)ethyl]-1,3,5-triazine, and 2-phenyl-4-hydroxy-5-methylimidazole. Midazole compounds; and organic phosphorus compounds such as triphenylphosphine, tributylphosphine, trioctylphosphine, tetrabutylphosphonium hexafluorophosphate, tetrabutylphosphonium tetraphenylborate, tetrabutylphosphonium acetate, tetraphenylphosphonium tetraphenylborate, tetraphenylphosphonium bromide, tetrabutylphosphonium bromide, tetrabutylphosphonium laurate, tetraphenylphosphonium hydrogen phthalate, bis(tetraphenylphosphonium) dihydrogen pyromellitate, and bis(tetrabutylphosphonium) dihydrogen pyromellitate.

[0031] Among these, thermal anionic polymerization initiators are preferred, and among these, 2-ethyl-4-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 2,4-diamino-6-[2-(2-methyl-1-imidazolyl)ethyl]-1,3,5-triazine, and 2-phenyl-4-hydroxy-5-methylimidazole are particularly preferred. These polymerization initiators may be used alone or in combination of two or more. The amount of the thermal radical polymerization initiator or thermal anionic polymerization initiator is not particularly limited, but is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, and even more preferably 0.3 to 3 parts by mass, relative to 100 parts by mass of the (a1) component and the (c1) component. Within this range, the resin composition can be sufficiently cured without adversely affecting the physical properties of the resin composition.

[0032] [Various resins] In addition to the components (a1), (a2), (c1) and (c2), the resin compositions of layers A and C may contain various resins other than thermoplastic resins such as polyester resin, polyethylene resin, cellulose resin, styrene resin, polyamide resin, polyimide resin and melamine resin, as well as various resins other than those exemplified as adhesion promoters described below, such as silicone resin, epoxy resin, silicone-epoxy resin and perfluoropolyether resin. In consideration of heat resistance and adhesion, epoxy resin is preferred as the various resins contained in the resin compositions of layers A and C. The content of the various resins is not particularly limited, but is preferably 1 to 20 mass % of the mass of the (a1) or (c1) component, more preferably 2 to 15 mass %, and even more preferably 2 to 10 mass %. This range is preferable because it is possible to increase the adhesive strength of the A layer and the C layer while maintaining a low relative dielectric constant and a low dielectric loss tangent.

[0033] The epoxy resin is not particularly limited, and examples thereof include known epoxy resins which are liquid or solid at room temperature, such as biphenol-type epoxy resins such as bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, 3,3',5,5'-tetramethyl-4,4'-biphenol-type epoxy resins and 4,4'-biphenol-type epoxy resins, biphenylaralkyl-type epoxy resins, phenol novolac-type epoxy resins, cresol novolac-type epoxy resins, bisphenol A novolac-type epoxy resins, naphthalene diol-type epoxy resins, trisphenylol methane-type epoxy resins, tetrakisphenylol ethane-type epoxy resins and phenol dicyclopentadiene novolac-type epoxy resins in which the aromatic rings are hydrogenated, and alicyclic epoxy resins.

[0034] When the A layer and the C layer contain an epoxy resin, it is preferable that the A layer and the C layer further contain a curing agent for the epoxy resin. Examples of such a curing agent include phenol novolac resin, various amine derivatives, acid anhydrides, and those in which an acid anhydride group is partially opened to generate a carboxylic acid. Among them, phenol novolac resin is preferable. In particular, it is preferable to mix the epoxy resin and the phenol novolac resin so that the ratio of the epoxy group of the epoxy resin to the phenolic hydroxyl group of the phenol novolac resin is 1:0.8 to 1.3.

[0035] Furthermore, in order to promote the reaction of the components (a1) and (c1) with the epoxy resin, and the reaction of the epoxy resin with the curing agent, imidazole derivatives, phosphine derivatives, amine derivatives, metal compounds such as organoaluminum compounds, and the like may be used as a reaction promoter (catalyst) in addition to the components (a2) and (c2).

[0036] [Insulating inorganic particles] The resin composition of the A layer and the C layer may contain insulating inorganic particles. The insulating inorganic particles are not particularly limited, but examples thereof include silica, calcium carbonate, potassium titanate, glass fiber, silica balloon, glass balloon, aluminum oxide, aluminum nitride, boron nitride, beryllium oxide, barium titanate, barium sulfate, zinc oxide, titanium oxide, magnesium oxide, antimony oxide, aluminum hydroxide, magnesium hydroxide, and the like, and preferably silica, aluminum oxide, aluminum nitride, boron nitride, and zinc oxide. By containing these insulating inorganic particles, the thermal expansion coefficient of the cured product of the resin composition of the A layer and the C layer can be reduced.

[0037] The particle size of the insulating inorganic particles is not particularly limited, but is preferably 0.05 to 10 μm, more preferably 0.1 to 8 μm, and even more preferably 0.2 to 5 μm, as a median diameter measured by a laser diffraction particle size distribution measuring device. Within this range, it is preferable because it is easy to disperse uniformly and there is no sedimentation over time. Furthermore, the particle size of the insulating inorganic particles is preferably 50% or less of the thickness of the A layer and the C layer. If the particle size is 50% or less of the thickness of the A layer and the C layer, it is preferable because it is easy to disperse the insulating inorganic particles uniformly and it is also easy to coat the A layer and the C layer evenly.

[0038] The content of the insulating inorganic particles is not particularly limited, but is preferably 5 to 80 mass % of the mass of the (a1) or (c1) component, more preferably 10 to 60 mass %, and even more preferably 15 to 50 mass %. Within this range, the thermal expansion coefficients of the A and C layers can be effectively reduced, and the resin composition of the A and C layers is preferably formed into a film and does not become brittle after being completely cured.

[0039] [Organic filler] The resin compositions of the A layer and the C layer may contain an organic filler. The organic filler is not particularly limited, but examples thereof include thermoplastic resin particles such as acrylic-butadiene copolymer, styrene-butadiene copolymer, acrylonitrile-butadiene-styrene copolymer (ABS resin), acrylic block copolymer, carbon fiber, cellulose fiber, silicone powder, acrylic powder, polytetrafluoroethylene powder, polyethylene powder, polypropylene powder, etc. These may be used alone or in combination of two or more.

[0040] The shape of the organic filler is not particularly limited, and examples thereof include spherical, fibrous, flake-like, needle-like, rod-like, and elliptical shapes. Among these, spherical, fibrous, flake-like, elliptical, and rod-like shapes are preferred, and spherical, fibrous, flake-like, and elliptical shapes are more preferred.

[0041] The primary particle size of the organic filler is not particularly limited, but is preferably 0.05 to 500 μm, more preferably 0.1 to 300 μm, and even more preferably 1 to 100 μm, as a median diameter measured by a laser diffraction particle size distribution measuring device. If it is within this range, it is preferable because it is easy to uniformly disperse the organic particles in the resin composition and the organic particles do not settle, separate, or become unevenly distributed over time.

[0042] The amount of the organic filler is not particularly limited, but is preferably 1 to 100 parts by mass, more preferably 5 to 80 parts by mass, and even more preferably 10 to 50 parts by mass, per 100 parts by mass of the (a1) component and the (c1) component. If the amount is within this range, it is possible to increase the strength of the cured products of the A layer and the C layer.

[0043] [Adhesion promoter] The resin compositions of the A layer and the C layer may contain an adhesion imparting agent as necessary to impart adhesiveness or tackiness (pressure-sensitive adhesiveness). Examples of adhesion imparting agents include acrylic resins, urethane resins, phenolic resins, terpene resins, silane coupling agents, etc. Among them, acrylic resins and silane coupling agents are preferred for imparting adhesiveness, and terpene resins are preferred for imparting tackiness (pressure-sensitive adhesiveness).

[0044] The acrylic resin is not particularly limited, and examples thereof include lauryl acrylate, stearyl acrylate, isostearyl acrylate, phenoxyethyl acrylate, phenoxydiethylene glycol acrylate, tetrahydrofurfuryl acrylate, isobornyl acrylate, 2-acryloyloxyethyl phthalate, 2-acryloyloxyethyl acid phosphate, polyethylene glycol diacrylate, dimethylol tricyclodecane diacrylate, trimethylolpropane triacrylate, dipentaerythritol hexaacrylate, and the like. Examples of suitable methacrylates include tetrahydrofurfuryl methacrylate, dioxane glycol diacrylate, 9,9-bis[4-(2-hydroxyethoxy)phenyl]fluorene diacrylate, lauryl methacrylate, phenoxyethyl methacrylate, phenoxydiethylene glycol methacrylate, tetrahydrofurfuryl methacrylate, isobornyl methacrylate, 2-methacryloyloxyethyl phthalate, 2-methacryloyloxyethyl acid phosphate, polyethylene glycol dimethacrylate, and dimethylol tricyclodecane dimethacrylate.

[0045] The terpene resin is not particularly limited, and examples thereof include homopolymers of terpenes such as monoterpenes such as α-pinene, β-pinene, dipentene, and limonene, sesquiterpenes such as cedrene and farnesene, and diterpenes such as abietic acid, aromatic modified terpene resins which are copolymers of aromatic vinyl compounds such as styrene and α-methylstyrene with the above-mentioned terpenes, and terpene phenol resins which are copolymers of phenols such as phenol, cresol, hydroquinone, naphthol, and bisphenol A with the above-mentioned terpenes, etc. In addition, hydrogenated terpene resins obtained by hydrogenating these terpene resins can also be used.

[0046] The silane coupling agent is not particularly limited, and examples thereof include silane coupling agents such as n-propyltrimethoxysilane, n-propyltriethoxysilane, n-octyltrimethoxysilane, n-octyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, 2-[methoxy(polyethyleneoxy)propyl]-trimethoxysilane, methoxytri(ethyleneoxy)propyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-(methacryloyloxy)propyltrimethoxysilane, 3-isocyanatopropyltriethoxysilane, and 3-isocyanatopropyltrimethoxysilane.

[0047] The amount of the adhesion promoter is not particularly limited, but is preferably 0.1 to 20 parts by mass, more preferably 0.5 to 10 parts by mass, and even more preferably 1 to 5 parts by mass, per 100 parts by mass of the (a1) component and the (c1) component. Within this range, the adhesive strength or cohesive strength can be further improved without changing the mechanical properties of the A layer and the C layer.

[0048] [Antioxidants] The resin compositions of the A layer and the C layer may contain an antioxidant. The antioxidant is not particularly limited, but examples thereof include n-octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, n-octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)acetate, neododecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, dodecyl-β-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, ethyl ester, and the like. Octadecyl-α-(4-hydroxy-3,5-di-t-butylphenyl)isobutyrate, Octadecyl-α-(4-hydroxy-3,5-di-t-butylphenyl)isobutyrate, Octadecyl-α-(4-hydroxy-3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2-(n-octylthio)ethyl-3,5-di-t-butyl-4-hydroxyphenylacetate, 2-(n-octadecylthio)ethyl-3, 5-di-t-butyl-4-hydroxyphenyl acetate, 2-(n-octadecylthio)ethyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2-(2-stearoyloxyethylthio)ethyl-7-(3-methyl-5-t-butyl-4-hydroxyphenyl)heptanoate, 2-hydroxyethyl-7-(3-methyl-5-t-butyl-4-hydroxyphenyl)propionate, pentaethyl Phenolic antioxidants such as rhythritol tetrakis [3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]; sulfur-based antioxidants such as dilauryl-3,3'-thiodipropionate, dimyristyl-3,3'-thiodipropionate, distearyl-3,3'-thiodipropionate, ditridecyl-3,3'-thiodipropionate, and pentaerythrityl tetrakis (3-laurylthiopropionate);Examples of phosphorus-based antioxidants include tridecyl phosphite, triphenyl phosphite, tris(2,4-di-t-butylphenyl)phosphite, 2-ethylhexyl diphenyl phosphite, diphenyl tridecyl phosphite, 2,2-methylene bis(4,6-di-t-butylphenyl)octyl phosphite, distearyl pentaerythritol diphosphite, bis(2,6-di-t-butyl-4-methylphenyl)pentaerythritol diphosphite, and 2-[[2,4,8,10-tetrakis(1,1-dimethylethyl)dibenzo[d,f][1,3,2]dioxaphosphepin-6-yl]oxy]-N,N-bis[2-[[2,4,8,10-tetrakis(1,1-dimethylethyl)dibenzo[d,f][1,3,2]dioxaphosphepin-6-yl]oxy]-ethyl]ethanamine.

[0049] The amount of the antioxidant is not particularly limited, but is preferably 0.00001 to 5 parts by mass, more preferably 0.0001 to 4 parts by mass, and even more preferably 0.001 to 3 parts by mass, per 100 parts by mass of the (a1) component and the (c1) component. If it is within this range, oxidation can be prevented without changing the mechanical properties of the A layer and the C layer.

[0050] [Flame retardant] In order to impart flame retardancy, the resin compositions of the A layer and the C layer may contain a flame retardant as necessary. The flame retardant is not particularly limited, and examples thereof include phosphorus-based flame retardants, metal hydrates, halogen-based flame retardants, and guanidine-based flame retardants. Examples of phosphorus-based flame retardants include red phosphorus, ammonium phosphates such as monoammonium phosphate, diammonium phosphate, triammonium phosphate, and ammonium polyphosphate, inorganic nitrogen-containing phosphorus compounds such as guanidine phosphate and phosphoric acid amide, phosphoric acid, phosphine oxide, triphenyl phosphate, tricresyl phosphate, trixylenyl phosphate, cresyl diphenyl phosphate, cresyl di-2,6-xylenyl phosphate, resorcinol bis(diphenyl phosphate), 1,3-phenylene bis(di-2,6-xylenyl phosphate), bisphenol A-bis(diphenyl phosphate), 1,3-phenylene bis( Examples of suitable phosphazene compounds include phosphazene compounds such as diphenyl phosphate, divinyl phenylphosphonate, diallyl phenylphosphonate, bis(1-butenyl) phenylphosphonate, phenyl diphenylphosphinate, methyl diphenylphosphinate, bis(2-allylphenoxy)phosphazene, and dicresylphosphazene, as well as melamine phosphate, melamine pyrophosphate, melamine polyphosphate, melam polyphosphate, melem polyphosphate, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, and 10-(2,5-dihydroxyphenyl)-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide. Examples of suitable metal hydrates include aluminum hydroxide hydrate and magnesium hydroxide hydrate. Examples of halogen-based flame retardants include hexabromobenzene, pentabromotoluene, ethylene bis(pentabromophenyl), ethylene bistetrabromophthalimide, 1,2-dibromo-4-(1,2-dibromoethyl)cyclohexane, tetrabromocyclooctane, hexabromocyclododecane, bis(tribromophenoxy)ethane, brominated polyphenylene ether, brominated polystyrene, 2,4,6-tris(tribromophenoxy)-1,3,5-triazine, etc. Examples of guanidine-based flame retardants include guanidine sulfamate, guanidine phosphate, etc.

[0051] The amount of the flame retardant is not particularly limited, but is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 4 parts by mass, and even more preferably 0.1 to 3 parts by mass, per 100 parts by mass of the (a1) component and the (c1) component. Within this range, flame retardancy can be imparted without changing the mechanical properties of the A layer and the C layer.

[0052] The resin compositions constituting the layers A and C may be the same or different, but are preferably the same. If the resin compositions constituting the layers A and C are the same, this is preferred because the multilayer films will have higher adhesion when stacked together. In the resin composition constituting layer A, the (a1) component is preferably 50 to 99.9 mass %, more preferably 60 to 95 mass %, and even more preferably 70 to 90 mass %. In addition, in the resin composition constituting the C layer, the (c1) component is preferably 50 to 99.9 mass %, more preferably 60 to 95 mass %, and further preferably 70 to 90 mass %. In addition, it is preferable that the A layer and the C layer do not have a fiber base material such as E glass, low dielectric glass, quartz glass, S glass, or T glass, and are preferably composed of a resin composition constituting the A layer and a resin composition constituting the C layer, respectively.

[0053] In addition, the A and C layers used in the present invention preferably have a relative dielectric constant of 3.5 or less at 10 GHz when cured. Such a cured product can reduce transmission loss. Here, the relative dielectric constant refers to the value measured by completely curing the A and C layers alone at 180°C for 2 hours, cutting the cured product into a test piece of 30 mm length x 40 mm width and 100 μm thickness, and connecting a network analyzer (E5063-2D5 manufactured by Keysight Corporation) and a strip line (manufactured by Keycom Corporation).

[0054] In addition, the A layer and C layer used in the present invention preferably have a dielectric loss tangent of 0.003 or less at 10 GHz when cured. Such a cured product can reduce transmission loss. Here, the dielectric loss tangent refers to a value measured by completely curing the A layer and C layer alone at 180°C for 2 hours, cutting the cured product into a test piece of 30 mm length x 40 mm width and 100 μm thickness, as with the relative dielectric constant, and connecting a network analyzer (E5063-2D5 manufactured by Keysight Corporation) and a strip line (manufactured by Keycom Corporation).

[0055] The thickness of each of the A layer and the C layer is preferably 0.1 to 20 μm, more preferably 1 to 15 μm, and even more preferably 2 to 10 μm. If the thickness of the A layer and the C layer is within this range, it is preferable because it has a low linear expansion coefficient while maintaining a high adhesive strength. Furthermore, the thicknesses of the A layer and the C layer in the multilayer film of the present invention may be the same or different, so long as they are within the above range.

[0056] The minimum melt viscosity of each of the layers A and C at 25 to 150° C. is preferably 0.1 to 100 Pa s, more preferably 0.5 to 80 Pa s, and even more preferably 1 to 50 Pa s. If the minimum melt viscosity of the layers A and C is within this range, high adhesive strength can be maintained, and the unevenness of wiring can be easily filled during substrate fabrication. The minimum melt viscosity of layers A and C at 25 to 150°C refers to the melt viscosity value (minimum melt viscosity (Pa s)) at the temperature showing the minimum viscosity (minimum melt viscosity temperature (°C)) when the melt viscosity is measured using a dynamic viscoelasticity measuring device (Rheometer MR-300, manufactured by UPM) under conditions of a measurement frequency of 1.0 Hz, a probe diameter of 8.0 mm, a measurement temperature of 25°C to 150°C, and a heating rate of 5°C / min.

[0057] [(b1) component] The modified polyphenylene ether of the component (b1) of layer B is not particularly limited, but is preferably one having functional groups at both ends as represented by the following formula (2). [ka] (In formula (2), L is a divalent organic group, R 4 are each independently an alkyl group having 1 to 6 carbon atoms or a hydrogen atom, and R 5 is a group selected from a hydroxy group, an epoxy group, a (meth)acrylic group, a vinyl group, and an amino group, s is a number from 1 to 100, and t is a number from 1 to 100.

[0058] In formula (2), L is a divalent organic group, preferably an alkylene group having 1 to 6 carbon atoms, or a group represented by the following formula (3) or (4).

[0059] [ka] (In formula (3), R 4 is the same as equation (2). [ka] (In formula (4), R 4 is the same as equation (2).

[0060] R in Equation (2) 4 are each independently an alkyl group having 1 to 6 carbon atoms or a hydrogen atom, and preferably a methyl group or a hydrogen atom.

[0061] R in Equation (2) 5 is a group selected from a hydroxy group, an epoxy group, a (meth)acrylic group, a vinyl group, and an amino group, and is preferably a (meth)acrylic group or a vinyl group.

[0062] In the formula (2), s is a number from 1 to 100, and preferably a number from 1 to 10.

[0063] In the formula (2), t is a number from 1 to 100, and preferably a number from 1 to 10.

[0064] The weight average molecular weight (Mw) of the modified polyphenylene ether of component (b1) is not particularly limited, but is preferably 500 to 5,000, more preferably 700 to 4,000, and even more preferably 1,000 to 3,000. If the weight average molecular weight (Mw) is within this range, the resin composition will have sufficient strength, and the functional groups introduced by modification can be efficiently reacted.

[0065] The method for producing the modified polyphenylene ether of component (b1) is not particularly limited, and may involve polymerizing a corresponding phenol compound by oxidative polymerization and then modifying the terminals, or heating a high-molecular-weight polyphenylene ether, a corresponding phenol compound, and a radical initiator in a solvent to cause a redistribution reaction, and then modifying the terminals.

[0066] The functional group equivalent of the modified polyphenylene ether of component (b1) is preferably 0.04 to 0.8 mol / 100 g, more preferably 0.05 to 0.3 mol / 100 g, and even more preferably 0.07 to 0.2 mol / 100 g, which is preferable because the functional groups react easily and the cured product of the multilayer film has a low relative dielectric constant, low dielectric tangent, and high heat resistance.

[0067] [(b2) component] The resin composition of the layer B contains a curing catalyst as the component (b2). The curing catalyst is not particularly limited, but examples thereof include a thermal radical polymerization initiator and a thermal anionic polymerization initiator.

[0068] Examples of the thermal radical polymerization initiator include methyl ethyl ketone peroxide, methylcyclohexanone peroxide, methylacetoacetate peroxide, acetylacetone peroxide, 1,1-bis(t-butylperoxy)3,3,5-trimethylcyclohexane, 1,1-bis(t-hexylperoxy)cyclohexane, 1,1-bis(t-hexylperoxy)3,3,5-trimethylcyclohexane, 1,1-bis(t-butylperoxy)cyclohexane, 2,2-bis(4,4-di-t -butylperoxycyclohexyl)propane, 1,1-bis(t-butylperoxy)cyclododecane, n-butyl-4,4-bis(t-butylperoxy)valerate, 2,2-bis(t-butylperoxy)butane, 1,1-bis(t-butylperoxy)-2-methylcyclohexane, t-butyl hydroperoxide, p-menthane hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, t-hexyl hydroperoxide, dicumyl peroxide, 2,5-dimethyl 2,5-diethyl-2,5-bis(t-butylperoxy)hexane, α,α'-bis(t-butylperoxy)diisopropylbenzene, t-butylcumyl peroxide, di-t-butyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexyne-3, isobutyryl peroxide, 3,5,5-trimethylhexanoyl peroxide, octanoyl peroxide, lauroyl peroxide, cinnamic acid peroxide, m-toluoyl peroxide, benzoyl peroxide, diisopropyl Pyl peroxydicarbonate, bis(4-t-butylcyclohexyl) peroxydicarbonate, di-3-methoxybutyl peroxydicarbonate, di-2-ethylhexyl peroxydicarbonate, di-sec-butyl peroxydicarbonate, di(3-methyl-3-methoxybutyl) peroxydicarbonate, di(4-t-butylcyclohexyl) peroxydicarbonate, α,α'-bis(neodecanoylperoxy)diisopropylbenzene, cumyl peroxyneodecanoate, 1,1,3,3-Tetramethylbutylperoxyneodecanoate, 1-cyclohexyl-1-methylethylperoxyneodecanoate, t-hexylperoxyneodecanoate, t-butylperoxyneodecanoate, t-hexylperoxypivalate, t-butylperoxypivalate, 2,5-dimethyl-2,5-bis(2-ethylhexanoylperoxy)hexane, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, 1-cyclohexyl-1-methylethylperoxy-2-ethylhexanoate, t-hexylperoxy peroxy-2-ethylhexanoate, t-butylperoxy-2-ethylhexanoate, t-butylperoxyisobutyrate, t-butylperoxymaleic acid, t-butylperoxylaurate, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxyisopropyl monocarbonate, t-butylperoxy-2-ethylhexyl monocarbonate, 2,5-dimethyl-2,5-bis(benzoylperoxy)hexane, t-butylperoxyacetate, t-hexylperoxybenzoate, t-butylperoxyethylhexanoate, Organic peroxides such as 2,2'-azobis(N-butyl-2-methylpropionamide), 2,2'-azobis(N-cyclohexyl-2-methylpropionamide), 2,2'-azobis[N-(2-methylpropyl)-2-methylpropionamide], 2,2'-azobis[N-(2-methylethyl)-2- ... 2,2'-azobis(N-hexyl-2-methylpropionamide), 2,2'-azobis(N-propyl-2-methylpropionamide), 2,2'-azobis(N-ethyl-2-methylpropionamide), 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 2,2'-azobis[N-(2-propenyl)-2-methylpropionamide], 2,2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide}, 2,Examples of the azo compounds include 2'-azobis[N-(2-propenyl)-2-methylpropionamide] and dimethyl-1,1'-azobis(1-cyclohexanecarboxylate).

[0069] Examples of the thermal anionic polymerization initiator include amine compounds such as triethylamine, triethylenediamine, 2-(dimethylaminomethyl)phenol, 1,8-diaza-bicyclo[5.4.0]undecene-7, tris(dimethylaminomethyl)phenol, and benzyldimethylamine; and isomers such as 2-methylimidazole, 2-ethylimidazole, 2-phenylimidazole, 2-ethyl-4-methylimidazole, 2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 2,4-diamino-6-[2-(2-methyl-1-imidazolyl)ethyl]-1,3,5-triazine, and 2-phenyl-4-hydroxy-5-methylimidazole. Midazole compounds; and organic phosphorus compounds such as triphenylphosphine, tributylphosphine, trioctylphosphine, tetrabutylphosphonium hexafluorophosphate, tetrabutylphosphonium tetraphenylborate, tetrabutylphosphonium acetate, tetraphenylphosphonium tetraphenylborate, tetraphenylphosphonium bromide, tetrabutylphosphonium bromide, tetrabutylphosphonium laurate, tetraphenylphosphonium hydrogen phthalate, bis(tetraphenylphosphonium) dihydrogen pyromellitate, and bis(tetrabutylphosphonium) dihydrogen pyromellitate.

[0070] Of these, thermal radical polymerization initiators are preferred, and among these, methyl ethyl ketone peroxide, dicumyl peroxide, t-butyl cumyl peroxide, di-t-butyl peroxide, lauroyl peroxide, and cinnamic acid peroxide are particularly preferred. These polymerization initiators may be used alone or in combination of two or more. The amount of the thermal radical polymerization initiator or thermal anionic polymerization initiator is not particularly limited, but is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, and even more preferably 0.3 to 3 parts by mass, relative to 100 parts by mass of component (b1). Within this range, the resin composition can be sufficiently cured without adversely affecting the physical properties of the resin composition.

[0071] [Various resins] In addition to the components (b1) and (b2), the resin composition of layer B may contain various resins such as thermoplastic resins such as acrylic resin, polyester resin, polyethylene resin, cellulose resin, styrene resin, butadiene-styrene block polymer resin, hydrogenated butadiene-styrene block polymer resin, polyamide resin, polyimide resin, and melamine resin, as well as silicone resin, epoxy resin, silicone-epoxy resin, phenol resin, perfluoropolyether resin, thermosetting butadiene-styrene block polymer resin, and thermosetting hydrogenated butadiene-styrene block polymer resin. In consideration of the low relative dielectric constant and low dielectric loss tangent properties, the various resins contained in the resin composition of layer B are preferably styrene resin, butadiene-styrene block polymer resin, hydrogenated butadiene-styrene block polymer, thermosetting butadiene-styrene block polymer resin, and thermosetting hydrogenated butadiene-styrene block polymer resin. The content of the various resins is not particularly limited, but is preferably 1 to 20 mass % of the mass of the (b1) component, more preferably 2 to 15 mass %, and even more preferably 2 to 10 mass %. Within this range, the flexibility of layer B can be increased while maintaining a low linear expansion coefficient, which is preferable.

[0072] Examples of styrene resins, butadiene-styrene block polymer resins, and hydrogenated butadiene-styrene block polymer resins include, but are not limited to, thermosetting butadiene-styrene block polymer resins and thermosetting hydrogenated butadiene-styrene block polymer resins such as "KIC-001", "KIC-002", "KIC-003", "KIC-004", "KIC-005", "FG1901", and "FG1924" manufactured by Kraton Corporation, and "Tuftech M1911", "Tuftech M1913", "Tuftech M1943", "Tuftech H1041", "Tuftech H1051", "Tuftech H1043", "Tuftech H1221", "Tuftech P1083", "Tuftech P2000", and "Tuftech MP10" manufactured by Asahi Kasei Corporation.

[0073] [Insulating inorganic particles] The resin composition of the B layer may contain insulating inorganic particles. There is no particular limitation on the insulating inorganic particles, but examples thereof include silica, calcium carbonate, potassium titanate, glass fiber, silica balloon, glass balloon, aluminum oxide, aluminum nitride, boron nitride, beryllium oxide, barium titanate, barium sulfate, zinc oxide, titanium oxide, magnesium oxide, antimony oxide, aluminum hydroxide, magnesium hydroxide, and the like, and preferably silica, aluminum oxide, aluminum nitride, boron nitride, and zinc oxide. By containing these insulating inorganic particles, the thermal expansion coefficient of the cured product of the resin composition of the B layer can be reduced.

[0074] The particle size of the insulating inorganic particles is not particularly limited, but is preferably 0.05 to 10 μm, more preferably 0.1 to 8 μm, and even more preferably 0.2 to 5 μm, as a median diameter measured by a laser diffraction particle size distribution measuring device. Within this range, it is preferable because it is easy to disperse the insulating inorganic particles uniformly and they do not settle over time. Furthermore, the particle size of the insulating inorganic particles is preferably 50% or less of the thickness of the B layer. If the particle size is 50% or less of the thickness of the B layer, it is preferable because it is easy to disperse the insulating inorganic particles uniformly and it is also easy to coat the B layer evenly.

[0075] The content of the insulating inorganic particles is not particularly limited, but is preferably 10 to 3,000 parts by mass, more preferably 20 to 2,500 parts by mass, and even more preferably 30 to 2,000 parts by mass, relative to 100 parts by mass of the (b1) component. Within this range, the thermal expansion coefficient of the B layer can be effectively reduced, and the resin composition of the B layer is preferably formed into a film and does not become brittle after being completely cured.

[0076] [Organic filler] The resin composition of layer B may contain an organic filler. The organic filler is not particularly limited, but examples thereof include thermoplastic resin particles such as acrylic-butadiene copolymer, styrene-butadiene copolymer, acrylonitrile-butadiene-styrene copolymer (ABS resin), acrylic block copolymer, carbon fiber, cellulose fiber, silicone powder, acrylic powder, polytetrafluoroethylene powder, polyethylene powder, polypropylene powder, etc. These may be used alone or in combination of two or more.

[0077] The shape of the organic filler is not particularly limited, and examples thereof include spherical, fibrous, flake-like, needle-like, rod-like, and elliptical shapes. Among these, spherical, fibrous, flake-like, elliptical, and rod-like shapes are preferred, and spherical, fibrous, flake-like, and elliptical shapes are more preferred. The primary particle size of the organic filler is not particularly limited, but is preferably 0.05 to 500 μm, more preferably 0.1 to 300 μm, and even more preferably 1 to 100 μm, as a median diameter measured by a laser diffraction particle size distribution measuring device. If it is within this range, it is preferable because it is easy to uniformly disperse the organic particles in the resin composition and the organic particles do not settle, separate, or become unevenly distributed over time.

[0078] The amount of the organic filler is not particularly limited, but is preferably 1 to 100 parts by mass, more preferably 5 to 80 parts by mass, and even more preferably 10 to 50 parts by mass, per 100 parts by mass of component (b1). If the amount is within this range, it is possible to increase the strength of the cured product of layer B.

[0079] [Antioxidants] The resin composition of layer B may contain an antioxidant. The antioxidant is not particularly limited, but examples thereof include n-octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, n-octadecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)acetate, neododecyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, dodecyl-β-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, ethyl Octadecyl-α-(4-hydroxy-3,5-di-t-butylphenyl)isobutyrate, Octadecyl-α-(4-hydroxy-3,5-di-t-butylphenyl)isobutyrate, Octadecyl-α-(4-hydroxy-3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2-(n-octylthio)ethyl-3,5-di-t-butyl-4-hydroxyphenylacetate, 2-(n-octadecylthio)ethyl-3, 5-di-t-butyl-4-hydroxyphenyl acetate, 2-(n-octadecylthio)ethyl-3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate, 2-(2-stearoyloxyethylthio)ethyl-7-(3-methyl-5-t-butyl-4-hydroxyphenyl)heptanoate, 2-hydroxyethyl-7-(3-methyl-5-t-butyl-4-hydroxyphenyl)propionate, pentaethyl Phenolic antioxidants such as rhythritol tetrakis [3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate]; sulfur-based antioxidants such as dilauryl-3,3'-thiodipropionate, dimyristyl-3,3'-thiodipropionate, distearyl-3,3'-thiodipropionate, ditridecyl-3,3'-thiodipropionate, and pentaerythrityl tetrakis (3-laurylthiopropionate);Examples of phosphorus-based antioxidants include tridecyl phosphite, triphenyl phosphite, tris(2,4-di-t-butylphenyl)phosphite, 2-ethylhexyl diphenyl phosphite, diphenyl tridecyl phosphite, 2,2-methylene bis(4,6-di-t-butylphenyl)octyl phosphite, distearyl pentaerythritol diphosphite, bis(2,6-di-t-butyl-4-methylphenyl)pentaerythritol diphosphite, and 2-[[2,4,8,10-tetrakis(1,1-dimethylethyl)dibenzo[d,f][1,3,2]dioxaphosphepin-6-yl]oxy]-N,N-bis[2-[[2,4,8,10-tetrakis(1,1-dimethylethyl)dibenzo[d,f][1,3,2]dioxaphosphepin-6-yl]oxy]-ethyl]ethanamine.

[0080] The amount of the antioxidant is not particularly limited, but is preferably 0.00001 to 5 parts by mass, more preferably 0.0001 to 4 parts by mass, and even more preferably 0.001 to 3 parts by mass, per 100 parts by mass of component (b1). If it is within this range, oxidation can be prevented without changing the mechanical properties of layer B.

[0081] [Flame retardant] In order to impart flame retardancy, the resin composition of layer B may contain a flame retardant as necessary. The flame retardant is not particularly limited, and examples thereof include phosphorus-based flame retardants, metal hydrates, halogen-based flame retardants, and guanidine-based flame retardants. Examples of phosphorus-based flame retardants include inorganic nitrogen-containing phosphorus compounds such as red phosphorus, ammonium phosphate such as monoammonium phosphate, diammonium phosphate, triammonium phosphate, and ammonium polyphosphate, guanidine phosphate, and phosphoric acid amide, phosphoric acid, phosphine oxide, triphenyl phosphate, tricresyl phosphate, trixylenyl phosphate, cresyl diphenyl phosphate, cresyl di-2,6-xylenyl phosphate, resorcinol bis(diphenyl phosphate), 1,3-phenylene bis(di-2,6-xylenyl phosphate), bisphenol A-bis(diphenyl phosphate), 1,3-phenylene bis( Examples of suitable phosphazene compounds include phosphazene compounds such as diphenyl phosphate, divinyl phenylphosphonate, diallyl phenylphosphonate, bis(1-butenyl) phenylphosphonate, phenyl diphenylphosphinate, methyl diphenylphosphinate, bis(2-allylphenoxy)phosphazene, and dicresylphosphazene, as well as melamine phosphate, melamine pyrophosphate, melamine polyphosphate, melam polyphosphate, melem polyphosphate, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, and 10-(2,5-dihydroxyphenyl)-9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide. Examples of suitable metal hydrates include aluminum hydroxide hydrate and magnesium hydroxide hydrate. Examples of halogen-based flame retardants include hexabromobenzene, pentabromotoluene, ethylene bis(pentabromophenyl), ethylene bistetrabromophthalimide, 1,2-dibromo-4-(1,2-dibromoethyl)cyclohexane, tetrabromocyclooctane, hexabromocyclododecane, bis(tribromophenoxy)ethane, brominated polyphenylene ether, brominated polystyrene, 2,4,6-tris(tribromophenoxy)-1,3,5-triazine, etc. Examples of guanidine-based flame retardants include guanidine sulfamate, guanidine phosphate, etc.

[0082] The amount of the flame retardant is not particularly limited, but is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 4 parts by mass, and even more preferably 0.1 to 3 parts by mass, per 100 parts by mass of component (b1). Within this range, flame retardancy can be imparted without changing the mechanical properties of layer B.

[0083] Of the resin composition constituting layer B (excluding insulating inorganic particles and organic filler), the (b1) component is preferably 50 to 99.9 mass %, more preferably 60 to 95 mass %, and even more preferably 70 to 90 mass %. Moreover, the layer B is preferably one that does not have a fiber base material such as E glass, low dielectric glass, quartz glass, S glass, or T glass, and is preferably made of a resin composition that constitutes the layer B.

[0084] In addition, the B layer used in the present invention preferably has a relative dielectric constant of 3.5 or less at 10 GHz when cured. Such a cured product can reduce transmission loss. Here, the relative dielectric constant refers to the value measured by completely curing the B layer alone at 180°C for 2 hours, cutting the cured product into a test piece of 30 mm length x 40 mm width and 100 μm thickness, and connecting a network analyzer (E5063-2D5 manufactured by Keysight Corporation) and a strip line (manufactured by Keycom Corporation).

[0085] In addition, the B layer used in the present invention preferably has a dielectric loss tangent of 0.002 or less at 10 GHz when cured. Such a cured product can reduce transmission loss. Here, the dielectric loss tangent refers to a value measured by completely curing the B layer alone at 180°C for 2 hours, cutting the cured product into a test piece of 30 mm length x 40 mm width and 100 μm thickness, as with the relative dielectric constant, and connecting a network analyzer (E5063-2D5 manufactured by Keysight Corporation) and a strip line (manufactured by Keycom Corporation).

[0086] The thickness of layer B is preferably 20 to 100 μm, more preferably 25 to 70 μm, and even more preferably 30 to 50 μm. If the thickness of layer B is within this range, it is preferable because the multilayer film has low linear expansion while maintaining heat resistance.

[0087] The linear expansion coefficient of layer B at 25 to 150° C. is preferably 1 to 50 ppm / K, more preferably 3 to 45 ppm / K, and even more preferably 5 to 40 ppm / K. If the linear expansion coefficient of layer B is within this range, the multilayer film preferably has low linear expansion.

[0088] The multilayer film of the present invention has the above-mentioned A layer, B layer, and C layer arranged in this order, preferably the A layer, B layer, and C layer arranged adjacent to each other in this order, and may further have a support or protective film, etc. on the outermost layer side of the A layer or the C layer, as described above. Examples of the support include a PET film or an ETFE film whose surface has been subjected to a release treatment. Examples of the protective film include a polyethylene film, a polypropylene film, etc.

[0089] The total thickness of Layer A, Layer B and Layer C in the multilayer film of the present invention is preferably from 10 to 300 μm, more preferably from 20 to 200 μm, from the viewpoints of flexibility and handleability.

[0090] Furthermore, when the multilayer film of the present invention has a support or protective film, these are peeled off to obtain a multilayer film consisting of Layer A, Layer B, and Layer C, and the multilayer film is press-cured at 180°C for 1 hour. The cured product of the multilayer film preferably has a relative dielectric constant of 3.5 or less, more preferably 3.2 or less, even more preferably 3.0 or less, and particularly preferably 2.9 or less at a frequency of 10 GHz, and similarly the dielectric loss tangent is preferably 0.0030 or less, more preferably 0.0025 or less, even more preferably 0.0020 or less, and particularly preferably 0.0015 or less. Furthermore, the glass transition temperature of the cured product of the multilayer film obtained by press curing the multilayer film consisting of Layer A, Layer B, and Layer C at 180°C for 1 hour is preferably 160°C or higher, more preferably 170°C or higher, and even more preferably 180°C or higher. Furthermore, the linear expansion coefficient of the cured product of the multilayer film obtained by press curing a multilayer film consisting of Layer A, Layer B, and Layer C at 180°C for 1 hour is preferably 50 ppm / K or less, more preferably 45 ppm / K or less, and even more preferably 40 ppm / K or less. Furthermore, when a multilayer film consisting of Layer A, Layer B, and Layer C is sandwiched between a SUS plate and copper foil and heat-cured at 180°C for 1 hour, the peel strength is preferably 0.8 kN / m or more, more preferably 0.9 kN / m or more, and even more preferably 1.0 kN / m or more.

[0091] <Manufacturing method of multilayer film> The method for producing the multilayer film of the present invention is not particularly limited, but the film can be produced, for example, by coating and drying the resin compositions constituting each layer in order so that the A layer, B layer, and C layer are stacked on top of each other on a support such as a PET film, and laminating them. The resin composition constituting the A layer may be prepared by mixing the (a1) component, the (a2) component, other additives added as necessary, and an organic solvent (e.g., cyclopentanone, cyclopentanone, cyclohexanone, mesitylene, anisole, dibutyl ether, diphenyl ether, 1,4-dioxane, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, N-methylpyrrolidone, etc.) using, for example, a planetary mixer (manufactured by Inoue Seisakusho Co., Ltd.) or a mixer THINKY CONDITIONING MIXER (manufactured by Thinky Corporation). The A layer is formed by applying the resin composition constituting the A layer to a specified thickness on a PET film, heating it, and drying only the organic solvent. Similarly, for layer B, the resin composition constituting layer B is prepared by mixing component (b1), component (b2), other additives added as necessary, and an organic solvent, and the resin composition constituting layer B is applied onto layer A to a specified thickness, heated, and only the organic solvent is dried to form layer B. Similarly, the C layer is obtained by preparing a resin composition constituting the C layer by mixing the (c1) component, the (c2) component, other additives added as necessary, and an organic solvent, applying the resin composition constituting the C layer onto the B layer to a specified thickness, heating, and drying only the organic solvent.

[0092] <Use of multi-layer film> The multilayer film of the present invention has excellent heat resistance, a low dielectric constant, a low dielectric loss tangent, and high adhesion to copper, and is therefore suitable for use in copper-clad laminates produced by laminating the A layer and / or the C layer in contact with copper foil. A printed wiring board can also be produced by subjecting the copper-clad laminate having the multilayer film of the present invention to circuit formation processing and multilayer adhesion processing by known methods, such as drilling, metal plating, and etching of metal foil. Furthermore, since the multilayer film of the present invention has flexibility in addition to the above-mentioned properties, it can be suitably used as a base film and a coverlay film for flexible printed wiring boards, and is also useful for applications such as semiconductor encapsulation materials. EXAMPLES

[0093] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0094] The molecular weights shown in the following examples are weight average molecular weights (Mw) measured by gel permeation chromatography (GPC) using polystyrene as a standard substance. The measurement conditions are as follows: [GPC measurement conditions] Developing solvent: Tetrahydrofuran Flow rate: 0.6mL / min Column: TSK Guardcolumn SuperH-L TSKgel SuperH4000(6.0mmI.D.×15cm×1) TSKgel SuperH3000(6.0mmI.D.×15cm×1) TSKgel SuperH2000(6.0mmI.D.×15cm×2) (All manufactured by Tosoh Corporation) Column temperature: 40℃ Sample injection volume: 20 μL (sample concentration: 0.5% by mass in tetrahydrofuran solution) Detector: Differential refractometer (RI)

[0095] (a1) Cyclic imide compound (a1-1) Maleimide compound 200g (1.0mol) of 1,12-diaminododecane and 207g (0.95mol) of pyromellitic anhydride were added to 196g of N-methylpyrrolidone, and the mixture was stirred at 25°C for 3 hours, and then stirred at 150°C for another 3 hours. 196g (2.0mol) of maleic anhydride, 82g (1.0mol) of sodium acetate, and 204g (2.0mol) of acetic anhydride were added to the obtained solution, and the mixture was stirred at 80°C for 1 hour. 500g of toluene was then added, and the mixture was washed with water and dehydrated, and the solvent was distilled off under reduced pressure to obtain bismaleimide (a1-1) represented by the following formula. (Weight average molecular weight 3,500, maleimide equivalent 0.057mol / 100g) [ka] (n≒8 (average value))

[0096] (a1-2) Citraconimide compounds 523g (1.0mol) of dimer diamine and 211g (0.97mol) of pyromellitic anhydride were added to 263g of N-methylpyrrolidone, and the mixture was stirred at 25°C for 3 hours, and then further stirred at 150°C for 5 hours. 226g (2.0mol) of citraconic anhydride, 82g (1.0mol) of sodium acetate, and 204g (2.0mol) of acetic anhydride were added to the obtained solution, and the mixture was stirred at 80°C for 1 hour. Then, 500g of toluene was added, and the mixture was washed with water and dehydrated, and the solvent was distilled off under reduced pressure to obtain citraconic imide (a1-2) represented by the following formula. (Weight average molecular weight 10,000, maleimide equivalent 0.020mol / 100g) [ka] (n≒18 (average value))

[0097] (a1-3) Maleimide compounds Maleimide compound represented by the following formula (BMI-2500, manufactured by Designer Molecules Inc.) (weight average molecular weight 3,500, maleimide equivalent 0.057 mol / 100 g) [ka] (n1≒3 (average value), n2≒3 (average value))

[0098] (a1-4) Maleimide compounds Maleimide compound represented by the following formula (BMI-3000, manufactured by Designer Molecules Inc.) (weight average molecular weight 10,000, maleimide equivalent 0.020 mol / 100 g) [ka] (n≒18 (average value))

[0099] (a2) Curing catalyst (a2-1) 2-Ethyl-4-methylimidazole (trade name: "2E4MZ" (manufactured by Shikoku Chemical Industry Co., Ltd.) (a2-2) 2,4-diamino-6-[2-(2-methyl-1-imidazolyl)ethyl]-1,3,5-triazine (trade name: "2MZ-A" (manufactured by Shikoku Chemical Industry Co., Ltd.)

[0100] (b1) Modified polyphenylene ether (b1-1) Polyphenylene ether resin modified with methacrylic acid at both ends (product name: "SA-9000" (weight average molecular weight 3000, manufactured by SABIC Corporation)) (b1-2) Polyphenylene ether resin modified with vinyl at both ends (product name: "OPE-2St-1200" (weight average molecular weight 1200, manufactured by Mitsubishi Gas Chemical Co., Inc.))

[0101] (b2) Curing catalyst (b2-1) t-Butylcumyl peroxide (product name: "Perbutyl C" (NOF Corporation)) (b2-2) Dicumyl peroxide (product name: "Percumyl D" (manufactured by NOF Corp.)

[0102] (c1) Cyclic imide compounds (c1-1) Maleimide compounds Maleimide synthesized in (a1-1) above (weight average molecular weight 3,500, maleimide equivalent 0.057 mol / 100 g) [ka] (n≒8 (average value))

[0103] (c1-2) Citraconimide compounds Citraconimide synthesized in (a1-2) above (weight average molecular weight 10,000, maleimide equivalent 0.020 mol / 100 g) [ka] (n≒18 (average value))

[0104] (c1-3) Maleimide compounds Maleimide compound represented by the following formula (BMI-2500, manufactured by Designer Molecules Inc.) (weight average molecular weight 3,500, maleimide equivalent 0.057 mol / 100 g) [ka] (n1≒3 (average value), n2≒3 (average value))

[0105] (c1-4) Maleimide compounds Maleimide compound represented by the following formula (BMI-3000, manufactured by Designer Molecules Inc.) (weight average molecular weight 10,000, maleimide equivalent 0.020 mol / 100 g) [ka] (n≒18 (average value))

[0106] (c2) Curing catalyst (c2-1) 2-Ethyl-4-methylimidazole (trade name: "2E4MZ" (manufactured by Shikoku Chemical Industry Co., Ltd.) (c2-2) 2,4-diamino-6-[2-(2-methyl-1-imidazolyl)ethyl]-1,3,5-triazine (trade name: "2MZ-A" (manufactured by Shikoku Chemical Industry Co., Ltd.)

[0107] (d) Epoxy resin (d-1) Biphenyl aralkyl type epoxy resin (product name: "NC-3000" (manufactured by Nippon Kayaku Co., Ltd.))

[0108] (e) Thermosetting butadiene-styrene block polymer resin (e-1) Thermosetting butadiene-styrene block polymer resin (product name "KIC-003" (Kraton Corporation))

[0109] (f) Insulating inorganic particles (f-1) Silica "SFP-130MC" (median diameter of primary particles: 0.6 μm) (manufactured by Denka Co., Ltd.)

[0110] [How to make multi-layer film] For Examples 1 to 9 and Comparative Examples 5 and 6, in addition to the formulation (parts by mass) shown in Table 1, 100 parts by mass of cyclopentanone was added to a total of 100 parts by mass of each component constituting each layer and mixed to prepare resin compositions for layers A, B, and C. The resin composition for layer A was applied onto a PET film and dried by heating at 120°C for 5 minutes to form layer A on the PET film. Subsequently, the resin composition for layer B was applied onto layer A and dried by heating at 120°C for 5 minutes to form layer B on layer A. Furthermore, the resin composition for layer C was applied onto layer B and dried by heating at 120°C for 5 minutes to form layer C on layer B, thereby producing a multilayer film having layers A, B, and C.

[0111] For Comparative Example 1, a resin composition was prepared in the same manner as above, and then layer A was applied onto a PET film and dried by heating at 120° C. for 5 minutes to prepare a film.

[0112] For Comparative Example 2 and Comparative Example 8, the resin compositions were prepared in the same manner as above, and then the resin composition for layer A was coated on a PET film and dried by heating at 120° C. for 5 minutes to form layer A on the PET film. Next, the resin composition for layer C was coated on layer A and dried by heating at 120° C. for 5 minutes to produce a multilayer film having layers A and C.

[0113] For Comparative Example 3 and Comparative Example 7, the resin compositions were prepared in the same manner as above, and then the resin composition for layer A was coated on a PET film and dried by heating at 120° C. for 5 minutes to form layer A on the PET film. Subsequently, the resin composition for layer B was coated on layer A and dried by heating at 120° C. for 5 minutes to produce a multilayer film having layers A and B.

[0114] For Comparative Example 4 and Comparative Example 9, the resin compositions were prepared in the same manner as above, and then the resin composition for layer B was applied onto a PET film and dried by heating at 120° C. for 5 minutes to form layer B on the PET film. Subsequently, the resin composition for layer C was applied onto layer B and dried by heating at 120° C. for 5 minutes to produce a multilayer film having layers B and C.

[0115] [Minimum melt viscosity] The resin compositions of layers A and C were coated into a film having a thickness of 100 μm, then cut into 10 mm squares and measured using a dynamic viscoelasticity measuring device (UPM, Rheometer MR-300). The measurement conditions were a measurement frequency of 1.0 Hz, a probe diameter of 8.0 mm, a measurement temperature of 25°C to 150°C, and a heating rate of 5°C / min. The temperature showing the minimum viscosity (minimum melt viscosity temperature (°C)) and the melt viscosity value at that time (minimum melt viscosity (Pa·s)) were read. The results are shown in Tables 1 and 2.

[0116] [Dielectric constant and dielectric loss tangent] The PET film was peeled off from the prepared multilayer film, and the multilayer film was sandwiched between a 30 mm x 40 mm x 100 μm thick mold frame and press cured at 180°C for 1 hour to prepare a test sample. A network analyzer (E5063-2D5, manufactured by Keysight Corporation) and a strip line (manufactured by Keycom Corporation) were connected to the prepared test sample to measure the relative dielectric constant and dielectric loss tangent at a frequency of 10 GHz. The results are shown in Tables 1 and 2.

[0117] [Tg] The storage modulus (MPa) of the test sample (cured product) prepared as described in the above [Dielectric constant and dielectric tangent] section was measured in the range of 0°C to 300°C using DMA Q800 (manufactured by TA Instruments Co., Ltd.), and the peak top temperature obtained from a graph plotting the Tan δ values ​​derived from the obtained storage modulus and loss modulus values ​​was taken as the glass transition temperature (Tg). The measurement conditions were a test sample (cured product) of 20 mm x 5 mm x 100 μm thickness, a heating rate of 5°C / min, multi-frequency mode, tensile mode, and amplitude of 15 μm. The results are shown in Tables 1 and 2.

[0118] [Linear expansion coefficient] The linear expansion coefficient of the test sample (cured product) prepared as described in the above [Dielectric constant and dielectric loss tangent] section was measured in the range of 0°C to 200°C using a TMA Q400 (manufactured by TA Instruments Co., Ltd.), and the linear expansion coefficient was measured from 25°C to 150°C. The measurement conditions were a test sample (cured product) of 20 mm x 3 mm x 100 μm thickness, a heating rate of 5°C / min, and a tensile mode. The results are shown in Tables 1 and 2.

[0119] [Peel Strength] Using a vacuum laminator V-130 (manufactured by Nikko Materials Co., Ltd.), the multilayer film prepared by the above method was laminated so that the opposite side of the PET film was in contact with a SUS plate, and laminated for 60 seconds at 80 ° C, vacuum degree 0.6 hPa, and pressure 0.3 MPa. After cooling to room temperature, the PET film was peeled off, and a copper foil with a thickness of 18 μm (product name: TQ-M4-VSP, manufactured by Mitsui Metals Co., Ltd.) was laminated again at 80 ° C, vacuum degree 0.6 hPa, and pressure 0.3 MPa for 60 seconds, and then heated at 180 ° C for 1 hour to harden. In accordance with the standard JIS-C-6481:1996 for testing copper-clad laminates for printed wiring boards, the force (peel strength) when peeling the copper foil from the resin film at a speed of 50 mm / min in a 90 ° direction with a width of 10 mm was obtained using a Tensilon tester (manufactured by Toyo Seiki Seisakusho Co., Ltd., product name: Strograph VE-1D). The results are shown in Tables 1 and 2.

[0120] [Table 1]

[0121] [Table 2]

[0122] In Examples 1 to 9, the cured products had a low relative dielectric constant, a low dielectric tangent, a high Tg, a low coefficient of linear expansion, and high peel strength. In Comparative Examples 1, 2 and 8, the absence of layer B resulted in a low Tg and a high linear expansion coefficient. In Comparative Examples 3 and 7, since the C layer was not present, the multilayer film did not adhere to the SUS substrate, resulting in low peel strength. In Comparative Examples 4 and 9, the absence of Layer A resulted in low adhesive strength between the multilayer film and the copper foil, and low peel strength. In Comparative Example 5, since the layer B did not contain modified polyphenylene ether, the Tg was low and the linear expansion coefficient was also high. In Comparative Example 6, since the A layer and the C layer did not contain a cyclic imide compound, the adhesive strength was low and the peel strength was low.

Claims

1. A multilayer film having layers A, B and C having the following composition, in which layers A, B and C are laminated in this order. A layer (a1): a cyclic imide compound represented by the following formula (1), and (a2): Layer containing a curing catalyst B layer (b1): Modified polyphenylene ether and (b2): Layer containing a curing catalyst C layer (c1): a cyclic imide compound represented by the following formula (1), and (c2): Layer containing a curing catalyst [Formula 1] (In formula (1), A independently represents a tetravalent organic group containing a cyclic structure. Q independently represents a divalent hydrocarbon group having 6 or more carbon atoms which does not contain an aromatic group which may contain a heteroatom. B independently represents an arylene group having 6 or more carbon atoms which may contain a heteroatom. X independently represents a hydrogen atom or a methyl group, n is 0 to 200, and m is 0 to 200.)

2. 2. The multilayer film according to claim 1, wherein the resin composition constituting the layer A and the resin composition constituting the layer C are the same resin composition.

3. 2. The multilayer film according to claim 1, wherein the organic group represented by A in formula (1) is any one of tetravalent organic groups represented by the following structural formulas: [chemical 2] (The bond not bonded to a substituent in the above structural formula is bonded to the carbonyl carbon that forms a cyclic imide structure in formula (1).)

4. 2. The multilayer film according to claim 1, wherein the divalent hydrocarbon group represented by Q in formula (1) is selected from the group consisting of divalent hydrocarbon groups represented by the following structural formulas and divalent hydrocarbon groups derived from a dimer acid skeleton: [C3] (R 1Each independently represents a hydrogen atom or a linear or branched alkyl group having 1 to 20 carbon atoms. 1 and p 2 are each a number of 5 or more, and may be the same or different; p 3 and p 4 are each a number of 0 or more and may be the same or different, p 5 and p 6 are each a number of 0 or more, and may be the same or different. The bond to which no substituent is bonded in the above structural formula is bonded to the nitrogen atom that forms the cyclic imide structure in formula (1).

5. 2. The multi-layer film according to claim 1, wherein the arylene group represented by B in formula (1) is any of the arylene groups represented by the following structural formulas: [C4] (R 2 are each independently a hydrogen atom, a halogen atom, or an alkyl group having 1 to 6 carbon atoms; R 3 are each independently a hydrogen atom, a halogen atom, a methyl group, or a trifluoromethyl group, and Z is an oxygen atom, a sulfur atom, or a methylene group. The bond to which no substituent is bonded in the above structural formula is bonded to the nitrogen atom that forms a cyclic imide structure in formula (1).

6. 2. The multi-layer film according to claim 1, wherein the cyclic imide compound of the component (a) is a cyclic imide compound represented by formula (1) in which m is 0.

7. 2. The multilayer film according to claim 1, wherein each of the layers A and C has a thickness of 0.1 to 20 μm.

8. 2. The multilayer film according to claim 1, wherein the thickness of layer B is 20 to 100 μm.

9. 2. The multilayer film according to claim 1, wherein the minimum melt viscosity of each of the layers A and C at 25 to 150° C. is 0.1 to 100 Pa·s.

10. 2. The multilayer film according to claim 1, wherein the linear expansion coefficient of the cured product of layer B at 25 to 150° C. is 1 to 50 ppm / K.

Citation Information

Patent Citations

  • Composite film for electronic apparatus using signal in high frequency band, printed wiring board and production method of the same

    JP2018012259A

  • Thermosetting resin composition, resin film for interlayer insulation, printed wiring board and method for manufacturing the same

    JP2018014388A

  • Resin composition

    JP2018028044A

  • Resin composition, prepreg, metal-clad laminate, and printed wiring board

    JP2019001965A