Electrode for non-aqueous electrolyte secondary battery

By using a polyborosiloxane and PVdF binders in the electrode active material layer, the rate characteristics of non-aqueous electrolyte secondary batteries are enhanced, addressing the insufficient performance of previous technologies.

JP2024154878AInactive Publication Date: 2024-10-31NISSAN MOTOR CO LTD +2
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023069083
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-20
Publication Date
2024-10-31
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing non-aqueous electrolyte secondary batteries do not exhibit sufficient rate characteristics when using a polymer with a siloxane bond for improving contact between the solid electrolyte and the electrode.

Method used

Incorporating two types of binders, including a polyborosiloxane binder with a specific chemical structure and a second binder such as PVdF, in the electrode active material layer to enhance ion transportability and reduce diffusion resistance.

Benefits of technology

The combination of binders significantly improves the rate characteristics of non-aqueous electrolyte secondary batteries, allowing for higher discharge rates and capacity extraction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024154878000001_ABST
    Figure 2024154878000001_ABST
Patent Text Reader

Abstract

To provide means for improving a rate characteristic in a non-aqueous electrolyte secondary battery.SOLUTION: In an electrode for a non-aqueous electrolyte secondary battery, formed by arranging an electrode active material layer containing an electrode active material and a binder onto a front surface of a collector, a first binder formed by polyborosiloxane having a predetermined structure in which a silicon atom and a boron atom are alternately bonded via an oxygen atom, and a second binder other than the polyborosiloxane are contained in the electrode active material layer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an electrode for a non-aqueous electrolyte secondary battery. [Background technology]

[0002] In recent years, the spread of various electric vehicles is expected to help solve environmental and energy problems. Secondary batteries have been developed as on-board power sources for driving motors, etc., which hold the key to the spread of these electric vehicles. As secondary batteries, non-aqueous electrolyte secondary batteries such as lithium-ion secondary batteries, which are expected to have high energy density and high output, have been attracting attention.

[0003] Here, Patent Document 1 discloses a technology in which a polymer having a siloxane bond (Si-O-Si) is used as a binder contained in an electrode active material layer in a secondary battery containing a solid electrolyte, in order to improve contact between the solid electrolyte and an electrode and to enhance ion transport properties. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Special Publication No. 2016-503564 Summary of the Invention [Problem to be solved by the invention]

[0005] However, as a result of investigations conducted by the present inventors, it was found that when the technology described in Patent Document 1 is applied to a non-aqueous electrolyte secondary battery, sufficient rate characteristics may not be exhibited.

[0006] Therefore, an object of the present invention is to provide a means for improving the rate characteristics of a non-aqueous electrolyte secondary battery. [Means for solving the problem]

[0007] The present inventors have conducted extensive research to solve the above problems, and in the process have found that the above problems can be solved by incorporating two or more binders, including a specific binder, into an electrode active material layer constituting a nonaqueous electrolyte secondary battery, thereby completing the present invention.

[0008] That is, according to one aspect of the present invention, there is provided an electrode for a non-aqueous electrolyte secondary battery, in which an electrode active material layer containing an electrode active material and a binder is disposed on a surface of a current collector. The binder contained in the electrode is represented by the following chemical formula 1:

[0009] [ka]

[0010] In the formula, R1 and R2 each independently represent a monovalent organic group, and at least one of R1 and R2 represents a monovalent aromatic group. and a repeating unit represented by the following chemical formula 2:

[0011] [ka]

[0012] In the formula, R3 represents a monovalent organic group. and a second binder other than the polyborosiloxane, the first binder having a structure in which the silicon atoms in the chemical formula 1 and the boron atoms in the chemical formula 2 are alternately bonded via oxygen atoms. Effect of the Invention

[0013] According to the present invention, the rate characteristics of a non-aqueous electrolyte secondary battery can be improved. [Brief description of the drawings]

[0014] [Figure 1]1 is a cross-sectional view showing a schematic diagram of a stacked (flat) non-bipolar (internal parallel connection) secondary battery according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] One embodiment of the present invention is an electrode for a non-aqueous electrolyte secondary battery, comprising an electrode active material layer containing an electrode active material and a binder disposed on a surface of a current collector, The binder is represented by the following chemical formula 1:

[0016] [ka]

[0017] In the formula, R1 and R2 each independently represent a monovalent organic group, and at least one of R1 and R2 represents a monovalent aromatic group. and a repeating unit represented by the following chemical formula 2:

[0018] [ka]

[0019] In the formula, R3 represents a monovalent organic group. and a second binder other than the polyborosiloxane, the first binder having a structure in which silicon atoms in Chemical Formula 1 and boron atoms in Chemical Formula 2 are alternately bonded via oxygen atoms, the first binder being made of polyborosiloxane and having a repeating unit represented by the formula:

[0020] A non-aqueous electrolyte secondary battery including the electrode for a non-aqueous electrolyte secondary battery according to the present embodiment has excellent rate characteristics.

[0021] Hereinafter, the above-mentioned embodiment of the present invention will be described with reference to the drawings, but the technical scope of the present invention should be determined based on the claims and is not limited to the following embodiments. The dimensional ratios in the drawings are exaggerated for the convenience of explanation and may differ from the actual ratios. In this specification, the range "X to Y" means "X or more and Y or less." Furthermore, unless otherwise specified, the operation and measurement of physical properties are performed under the conditions of room temperature (20 to 25°C) and relative humidity of 40 to 50% RH.

[0022] FIG. 1 is a cross-sectional view that illustrates a flat (laminated) non-bipolar (internal parallel connection) secondary battery (hereinafter also simply referred to as a "laminated secondary battery") according to one embodiment of the present invention.

[0023] As shown in Fig. 1, the stacked secondary battery 10a of this embodiment has a structure in which a substantially rectangular power generating element 21, in which a charge / discharge reaction actually proceeds, is sealed inside a laminate film 29. Here, the power generating element 21 has a configuration in which a positive electrode in which a positive electrode active material layer 13 is arranged on both sides of a positive electrode collector 11', an electrolyte layer 17 made of a separator containing an electrolytic solution, and a negative electrode in which a negative electrode active material layer 15 is arranged on both sides of a negative electrode collector 12 are laminated. Specifically, the positive electrode, the electrolyte layer, and the negative electrode are laminated in this order, with one positive electrode active material layer 13 and the adjacent negative electrode active material layer 15 facing each other with the electrolyte layer 17 interposed therebetween.

[0024] As a result, the positive electrode, the electrolyte layer, and the negative electrode form one unit cell layer 19. Therefore, the stacked secondary battery 10a shown in FIG. 1 can be said to have a configuration in which a plurality of unit cell layers 19 are stacked and electrically connected in parallel. The positive electrode current collectors of the outermost layers located on both outermost layers of the power generating element 21 each have the positive electrode active material layer 13 disposed on only one side, but active material layers may be provided on both sides. That is, instead of using a current collector dedicated to the outermost layer with an active material layer provided on only one side, a current collector having active material layers on both sides may be used as the current collector of the outermost layer as it is. Also, by reversing the arrangement of the positive electrode and the negative electrode from FIG. 1, the outermost negative electrode current collector may be located on both outermost layers of the power generating element 21, and the negative electrode active material layer may be disposed on one or both sides of the outermost negative electrode current collector.

[0025] A positive electrode current collector 25 and a negative electrode current collector 27 that are electrically connected to the electrodes (positive and negative electrodes) are attached to the positive electrode current collector 11' and the negative electrode current collector 12, respectively, and are structured to be sandwiched between the ends of the laminate film 29 and led out of the laminate film 29. The positive electrode current collector 25 and the negative electrode current collector 27 may be attached to the positive electrode current collector 11' and the negative electrode current collector 12 of the electrodes by ultrasonic welding, resistance welding, or the like, respectively, via a positive electrode terminal lead and a negative electrode terminal lead (not shown) as necessary.

[0026] 《Nonaqueous electrolyte secondary battery electrode》 The main components of the electrode for a non-aqueous electrolyte secondary battery according to the present embodiment will be described below. The electrode for a non-aqueous electrolyte secondary battery according to the present embodiment has an electrode active material layer that essentially contains a positive electrode active material and a binder.

[0027] [Current collector] The current collector has a function of mediating the movement of electrons from the positive electrode active material layer and the negative electrode active material layer described later. There are no particular limitations on the material constituting the current collector. For example, metals and conductive resins can be used as the material constituting the current collector.

[0028] Specifically, the metal may be aluminum, nickel, iron, stainless steel, titanium, copper, etc. In addition to these, a clad material of nickel and aluminum, a clad material of copper and aluminum, etc. may be used. Also, a foil in which a metal surface is coated with aluminum may be used. Among them, aluminum, stainless steel, copper, and nickel are preferable from the viewpoint of electronic conductivity, battery operating potential, adhesion of the negative electrode active material by sputtering to the current collector, etc. In addition, the latter conductive resin may be a resin in which a conductive filler is added to a non-conductive polymer material.

[0029] The current collector may be a single layer structure made of a single material, or may be a laminate structure made of a suitable combination of layers made of these materials. From the viewpoint of reducing the weight of the current collector, it is preferable that the current collector includes at least a conductive resin layer made of a resin having electrical conductivity. In addition, from the viewpoint of blocking the movement of lithium ions between the single cell layers, a metal layer may be provided on a part of the current collector.

[0030] [Electrode active material layer] The electrode active material layer is formed on the surface of an optional current collector, and essentially contains an electrode active material and a binder. The electrode active material layer may further contain other components such as a conductive assistant. When the electrode according to this embodiment is a positive electrode, the electrode active material is a positive electrode active material, and when the electrode according to this embodiment is a negative electrode, the electrode active material is a negative electrode active material. In this specification, unless otherwise specified, matters common to positive and negative electrodes are referred to as "electrode".

[0031] (Cathode active material) The positive electrode active material has a function of releasing ions such as lithium ions during charging and absorbing ions such as lithium ions during discharging. In this embodiment, the type of the positive electrode active material is not particularly limited, but it is preferable that the positive electrode active material is made of a space group of R3m because it has a higher capacity. The positive electrode active material belonging to the space group R3m has a predetermined layered structure (layered rock salt structure). Therefore, by using such a positive electrode active material, the battery capacity of the nonaqueous electrolyte secondary battery can be improved.

[0032] Examples of the positive electrode active material include layered rock salt active materials such as LiCoO2, LiMnO2, LiNiO2, LiVO2, and Li(Ni-Mn-Co)O2, LiMn2O4, and LiNi 0.5 Mn 1.5 Examples of metal oxides other than those mentioned above include spinel-type active materials such as LiFePO4 and LiMnPO4, olivine-type active materials such as Li2FeSiO4 and Li2MnSiO4, and Si-containing active materials such as Li4Ti5O 12 Among these, composite oxides containing lithium and nickel are preferably used, and more preferably Li(Ni-Mn-Co)O2 and those in which some of these transition metals have been replaced with other elements (hereinafter also simply referred to as "NMC composite oxides"). NMC composite oxides have a layered crystal structure in which lithium atomic layers and transition metal (Mn, Ni, and Co arranged in an orderly manner) atomic layers are alternately stacked with oxygen atomic layers interposed therebetween, and contain one Li atom per transition metal M atom, so that the amount of Li that can be extracted is twice that of spinel-based lithium manganese oxides, i.e., the supply capacity is doubled, and high capacity can be achieved.

[0033] As described above, the NMC composite oxide also includes composite oxides in which a part of the transition metal element is replaced by another metal element. In this case, the other elements include Ti, Zr, Nb, W, P, Al, Mg, V, Ca, Sr, Cr, Fe, B, Ga, In, Si, Mo, Y, Sn, V, Cu, Ag, Zn, etc., preferably Ti, Zr, Nb, W, P, Al, Mg, V, Ca, Sr, Cr, more preferably Ti, Zr, P, Al, Mg, Cr, and even more preferably Ti, Zr, Al, Mg, Cr from the viewpoint of improving cycle characteristics.

[0034] Since the NMC composite oxide has a high theoretical discharge capacity, it is preferable to use the NMC composite oxide represented by the general formula (1): Li a Ni b Mn c Co d M xO2 (wherein, in the formula, a, b, c, d, and x satisfy 0.98 ≦ a ≦ 1.2, 0.6 ≦ b ≦ 0.9, 0 < c ≦ 0.4, 0 < d ≦ 0.4, 0 ≦ x ≦ 0.3, and b + c + d + x = 1. M is at least one element selected from the group consisting of Ti, Zr, Nb, W, P, Al, Mg, V, Ca, Sr, and Cr). Here, a represents the atomic ratio of Li, b represents the atomic ratio of Ni, c represents the atomic ratio of Mn, d represents the atomic ratio of Co, and x represents the atomic ratio of M. Further, in the electrode for a non-aqueous electrolyte secondary battery according to this embodiment, the positive electrode active material is preferably an NMC composite oxide (high-nickel NMC composite oxide) that satisfies 0.8 ≦ b ≦ 0.9, 0 < c ≦ 0.2, 0 < d ≦ 0.2, and 0 ≦ x ≦ 0.2 in the general formula (1) described above).

[0035] From the viewpoint of high power output, the average particle diameter of the positive electrode active material is preferably 1 to 100 μm, more preferably 1 to 20 μm. In this specification, the average particle diameter of the particles shall be the median diameter (D50) measured by a particle size distribution measuring device using the laser diffraction / scattering method.

[0036] The content of the positive electrode active material in the positive electrode active material layer is not particularly limited, but for example, it is preferably in the range of 60 to 99% by mass, more preferably in the range of 80 to 98% by mass, based on 100% by mass of the total solid content of the active material layer.

[0037] (Negative electrode active material) The negative electrode active material has a function of releasing ions such as lithium ions during discharge and occluding ions such as lithium ions during charging. Examples of the negative electrode active material include carbon materials such as graphite (black lead), soft carbon, and hard carbon, lithium-transition metal composite oxides (for example, Li4Ti5O ), metal materials (tin, silicon), and silicon-containing alloy-based negative electrode materials (for example, Si 12 ), Sn 60 Ti 10 30 ​), lithium alloy negative electrode materials (e.g., lithium-tin alloy, lithium-silicon alloy, lithium-aluminum alloy, lithium-aluminum-manganese alloy, etc.), silicon oxide (SiO X ) and the like. In some cases, two or more kinds of negative electrode active materials may be used in combination. Preferably, from the viewpoint of capacity and output characteristics, silicon-containing alloy-based negative electrode materials, carbon materials, lithium-transition metal composite oxides, and lithium alloy-based negative electrode materials are preferably used as the negative electrode active materials. Among them, in this embodiment, from the viewpoint of particularly excellent effect of improving rate characteristics when the first binder is used, it is particularly preferable that the negative electrode active material contains at least graphite. Of course, negative electrode active materials other than the above may be used.

[0038] Average particle diameter of the negative electrode active material (D 50 ) is not particularly limited, but from the viewpoint of achieving high output, it is preferably 1 to 100 μm, and more preferably 1 to 20 μm.

[0039] The content of the negative electrode active material in the negative electrode active material layer is, for example, 60% by mass or more and less than 100% by mass, preferably 80% by mass or more and 99.5% by mass or less, more preferably more than 90% by mass or more and 99.0% by mass or less, and even more preferably 92% by mass or more and 98.5% by mass or less, based on 100% by mass of the total solid content of the active material layer. If the content of the negative electrode active material is within the above range, both the battery capacity and the output characteristics can be achieved.

[0040] (Binder) The binder has a function of maintaining the structure of the electrode active material layer by binding the members contained in the electrode active material layer to each other. The electrode according to this embodiment is characterized in that the electrode active material layer contains two different binders (a first binder and a second binder). In a non-aqueous electrolyte secondary battery using the electrode according to this embodiment, at least one of the positive electrode active material layer and the negative electrode active material layer may have the above-mentioned characteristic.

[0041] <First Binder> The first binder comprises a polyborosiloxane having a repeating unit represented by the following chemical formula 1 and a repeating unit represented by the following chemical formula 2, in which the silicon atoms in chemical formula 1 and the boron atoms in chemical formula 2 are alternately bonded via oxygen atoms.

[0042] [ka]

[0043] As described above, the polyborosiloxane as the first binder has a repeating unit represented by chemical formula 1 and a repeating unit represented by chemical formula 2, and has a structure in which the silicon atoms in chemical formula 1 and the boron atoms in chemical formula 2 are alternately bonded via oxygen atoms (also referred to simply as "alternate structure" in this specification). In other words, the polyborosiloxane can also be said to be a polymer having a repeating unit represented by the following chemical formula 3.

[0044] [ka]

[0045] In the above chemical formula, R1 and R2 each independently represent a monovalent organic group, and at least one of R1 and R2 represents a monovalent aromatic group. In the above chemical formula, R3 represents a monovalent organic group.

[0046] The type of the "monovalent organic group" is not particularly limited, and any known monovalent organic group can be used. Examples of the monovalent organic group include substituted or unsubstituted alkyl groups, substituted or unsubstituted alkenyl groups, substituted or unsubstituted alkynyl groups, substituted or unsubstituted aromatic groups (substituted or unsubstituted aryl groups, substituted or unsubstituted heteroaryl groups), and the like.

[0047] The alkyl group, alkenyl group and alkynyl group as the monovalent organic group may be linear, branched or cyclic, but preferably linear. The carbon number of the alkyl group is not particularly limited, but is preferably 1 to 20, more preferably 1 to 10, and even more preferably 1 to 4. The carbon numbers of the alkenyl group and alkynyl group are not particularly limited, but are preferably 2 to 20, more preferably 2 to 10, and even more preferably 2 to 4.

[0048] The aryl group as a monovalent organic group is a group derived from a hydrocarbon ring having aromaticity in part or as a whole. When the aryl group contains two or more hydrocarbon rings having aromaticity in part or as a whole, these rings may be bonded to each other by a single bond or condensed. The number of carbon atoms in the aryl group is not particularly limited, but is preferably 6 to 30. The number of carbon atoms in the aryl group is more preferably 6 to 12, and further preferably 6. In particular, the aryl group is preferably a monovalent group derived from an aromatic hydrocarbon ring having 6 or more ring atoms, and more preferably a monovalent group derived from an aromatic hydrocarbon ring having 6 to 16 ring atoms. Specific examples of these aromatic hydrocarbon rings include monocyclic groups such as a phenyl group, and condensed polycyclic hydrocarbon groups such as a biphenyl group, a phenanthryl group, a naphthyl group, an anthryl group, and a fluorenyl group.

[0049] The heteroaryl group as a monovalent organic group is a group derived from a heterocycle having aromaticity in part or as a whole. When the heteroaryl group contains two or more heterocycles having aromaticity in part or as a whole, these rings may be bonded to each other in part or as a whole by a single bond. When the heteroaryl group contains two or more heterocycles having aromaticity in part or as a whole, or other rings, these rings may be condensed with each other. In addition, when the heteroaryl group contains two or more heterocycles having aromaticity in part or as a whole, or other rings, one atom may also serve as a ring-forming atom of these rings. The heteroatom possessed by the heteroaryl group is not particularly limited, and examples thereof include one or more heteroatoms (e.g., nitrogen atom (N), oxygen atom (O), phosphorus atom (P), sulfur atom (S), silicon atom (Si), selenium atom (Se), germanium atom (Ge)) as ring-forming atoms. The number of carbon atoms in the heteroaryl group is preferably 3 to 30. The number of ring-forming atoms of the heteroaryl group is not particularly limited, but is preferably 5 to 30. The number of ring-forming atoms of the heteroaryl group is more preferably 5 to 14, and even more preferably 5 to 13. The number of heteroatoms of the heteroaryl group is not particularly limited, but is preferably 1 to 3. The number of heteroatoms of the heteroaryl group is more preferably 1 to 2, and even more preferably 1. In particular, the heteroaryl group is preferably a monovalent group derived from an aromatic heterocycle having 5 or more ring-forming atoms. In this specification, the term "aromatic group" is a general term for aryl groups and heteroaryl groups.

[0050] The alkyl group, alkenyl group, alkynyl group, aryl group and heteroaryl group as the monovalent organic group may each be a substituted group. The substituent is not particularly limited, and examples thereof include an alkyl group, an alkoxy group, an alkenyl group, an alkynyl group, a halogen atom, a hydroxyl group, a carboxyl group, a cyano group, an amino group, and a carbamoyl group. Note that the above-mentioned substituent does not substitute the same type of group. For example, the substituent that substitutes an alkyl group does not include an alkyl group.

[0051] Among them, in terms of the effect of the present invention being more excellent and the stability of the obtained polyborosiloxane being more excellent, it is preferable that both R1 and R2 are monovalent aromatic groups, and it is more preferable that both of them are monovalent aromatic hydrocarbon groups. In addition, R3 is preferably a monovalent aromatic group, and more preferably a monovalent aromatic hydrocarbon group. An example of a preferred chemical structure of polyborosiloxane is as follows.

[0052] [ka]

[0053] The polyborosiloxane as the first binder preferably contains the above-mentioned alternating structure (a structure having a repeating unit represented by chemical formula 1 and a repeating unit represented by chemical formula 2, in which the silicon atom in chemical formula 1 and the boron atom in chemical formula 2 are alternately bonded via an oxygen atom) as a main constituent unit. Here, the main constituent unit means that the total content of the repeating unit represented by chemical formula 1 and the repeating unit represented by chemical formula 2 in the alternating structure is 70 mol% or more, preferably 80 mol% or more, and more preferably 90 mol% or more, based on the total repeating units of the polyborosiloxane. There is no particular limit to the upper limit, and an example of the upper limit is 100 mol%. In addition, from the viewpoint of more significantly exhibiting the effects of the present invention, the molar ratio (Si / B) of silicon atoms to boron atoms contained in the polyborosiloxane as the first binder preferably satisfies 0.4≦Si / B≦0.6, and more preferably satisfies 0.45≦Si / B≦0.55.

[0054] Polyborosiloxane may contain a structure (repeating unit) other than the above alternating structure, for example, a structure in which repeating units represented by Chemical Formula 1 are continuously bonded. When two repeating units represented by Chemical Formula 1 are bonded, an oxygen atom of one repeating unit represented by Chemical Formula 1 is bonded to a silicon atom of the other repeating unit represented by Chemical Formula 1. The same applies to the repeating unit represented by Chemical Formula 2.

[0055] The number average molecular weight (Mn) of the polyborosiloxane as the first binder is not particularly limited, but from the viewpoint of handling, it is preferably 350 to 100,000, more preferably 5,000 to 50,000, and even more preferably 10,000 to 50,000. The dispersity (Mw / Mn) of the polyborosiloxane is not particularly limited, but from the viewpoint of handling, it is preferably 1.0 to 3.5, more preferably 1.1 to 3.0, and even more preferably 1.2 to 2.5. The shape of the polyborosiloxane is not particularly limited, but from the viewpoint of handling, it is preferably a linear polymer.

[0056] The number average molecular weight and dispersity are measured by gel permeation chromatography (GPC) under the following conditions: Equipment: Shimadzu LC-20AD Column: Tosoh TSK-GEL G3000H Column temperature: 35℃ Flow rate: 1.0 mL / min Eluent: Tetrahydrofuran Calibration curve: polystyrene.

[0057] Polyborosiloxane as the first binder can be prepared based on the description in JP 2015-168804 A, for example.

[0058] There are no particular limitations on the mass proportion of the first binder (polyborosiloxane) relative to the total amount (100 mass%) of binders contained in the electrode active material layer, but from the viewpoint of further improving the rate characteristics of the battery, it is preferably 10 to 70 mass%, more preferably 15 to 60 mass%, even more preferably 20 to 50 mass%, and particularly preferably 20 to 40 mass%.

[0059] The content of the first binder (polyborosiloxane) in the electrode active material layer is not particularly limited, but from the viewpoint of further improving the rate characteristics of the battery, it is preferably 1 to 3 mass %, more preferably 1 to 2 mass %.

[0060] <Second Binder> The second binder is a binder other than the above-mentioned polyborosiloxane. There is no particular restriction on the specific type of the second binder as long as it is other than polyborosiloxane. However, it is preferable that the second binder contains a polymer having a repeating unit (VdF unit) derived from vinylidene fluoride (VdF). By adopting such a configuration, it is possible to uniformly distribute the above-mentioned polymer as the second binder in the first binder (polyborosiloxane) while ensuring the binding property in the electrode active material layer.

[0061] When the second binder contains a polymer having a repeating unit derived from vinylidene fluoride (VdF), the polymer may be a VdF homopolymer (PVdF) consisting of only VdF units, or may have a repeating unit derived from VdF units and a monomer copolymerizable with VdF. In a preferred embodiment, the second binder contains PVdF. In this case, the content of VdF units in PVdF is preferably 70 mol % or more, more preferably 80 mol % or more, and even more preferably 90 mol % or more, based on the total repeating units of PVdF. The upper limit is not particularly limited, and may be 100 mol %.

[0062] In addition, when the above polymer has a repeating unit derived from a VdF unit and a monomer copolymerizable with VdF, the monomer copolymerizable with VdF may be a fluorinated monomer, a non-fluorinated monomer, etc., and is preferably a fluorinated monomer. Examples of the fluorinated monomer include vinyl fluoride, trifluoroethylene, chlorotrifluoroethylene (CTFE), fluoroalkyl vinyl ether, hexafluoropropylene (HFP), (perfluoroalkyl)ethylene, 2,3,3,3-tetrafluoropropene, trans-1,3,3,3-tetrafluoropropene, etc. Examples of the non-fluorinated monomer include ethylene and propylene. Among them, the monomer copolymerizable with VdF is preferably at least one fluorinated monomer selected from the group consisting of CTFE, fluoroalkyl vinyl ether, HFP, and 2,3,3,3-tetrafluoropropene, more preferably at least one fluorinated monomer selected from the group consisting of CTFE, HFP, and fluoroalkyl vinyl ether, and particularly preferably HFP. The polymer may further contain a repeating unit derived from a monomer other than the above. Here, the content of the monomer unit copolymerizable with VdF in the polymer is preferably 8.0 mol% or less, more preferably 7.0 mol% or less, still more preferably 6.0 mol% or less, even more preferably 5.0 mol% or less, particularly preferably 4.0 mol% or less, and particularly preferably 3.0 mol% or less, based on the total monomer units. In this specification, the composition of the polymer is, for example, 19 The ratio of the repeating unit derived from the monomer copolymerizable with VdF can be measured by F-NMR measurement. By setting the ratio of the repeating unit derived from the monomer copolymerizable with VdF within the above range, the swelling property and flexibility in the electrolyte can be improved. As a result, the ionic conductivity and electronic conductivity in the electrode active material layer are improved, and excellent output characteristics can be exhibited (especially, a large capacity can be extracted during discharge at a high discharge rate).

[0063] In addition, the polymer having a repeating unit (VdF unit) derived from vinylidene fluoride (VdF) as the second binder preferably has a linear structure. Since a polymer having a linear structure has high crystallinity, such a configuration can contribute to ensuring a diffusion path of lithium ions in the electrode active material layer. In this specification, "the polymer has a linear structure" means that the proportion of branched structural units in 100 mol % of the structural units of the polymer is 8 mol % or less.

[0064] The second binder may further include a binder other than the polymer having a repeating unit (VdF unit) derived from polyborosiloxane and vinylidene fluoride (VdF). However, from the viewpoint of further exerting the effects of the present invention, the content of the binder other than these (other binder) in the electrode active material layer containing the polymer having a repeating unit (VdF unit) derived from polyborosiloxane and vinylidene fluoride (VdF) is preferably 10 mass% or less, more preferably 5 mass% or less, even more preferably 3 mass% or less, particularly preferably 1 mass% or less, and most preferably 0 mass% (i.e., no other binder is included) with respect to the total amount of the binder. There is no particular limitation on the other binder, and known materials can be appropriately adopted.

[0065] There is no particular restriction on the mass ratio of the second binder relative to the total amount (100 mass%) of the binders contained in the electrode active material layer, but from the viewpoint of further improving the rate characteristics of the battery, it is preferably 30 to 90 mass%, more preferably 40 to 85 mass%, even more preferably 50 to 80 mass%, and particularly preferably 60 to 80 mass%.

[0066] There is no particular restriction on the content of the second binder in the electrode active material layer, but from the viewpoint of further improving the rate characteristics of the battery, it is preferably 1.5 to 4 mass %, more preferably 2 to 4 mass %, and even more preferably 3 to 4 mass %.

[0067] (Conductive assistant) The electrode active material layer preferably further contains a conductive assistant. The conductive assistant has a function of forming an electronic conduction path (conductive passage) in the positive electrode active material layer. When such an electronic conduction path is formed in the positive electrode active material layer, the internal resistance of the battery is reduced, and the output characteristics at a high rate can be improved. Examples of the conductive assistant include particulate carbon materials such as acetylene black, carbon black, channel black, thermal black, and Ketjen Black (registered trademark), and fibrous carbon materials such as carbon nanotubes (single-walled carbon nanotubes and multi-walled carbon nanotubes), carbon nanofibers, vapor-grown carbon fibers, electrospun carbon fibers, polyacrylonitrile-based carbon fibers, and pitch-based carbon fibers. Only one type of conductive assistant may be used alone, or two or more types may be used in combination.

[0068] The content of the conductive assistant contained in the electrode active material layer is preferably 2% by mass or less, more preferably 1% by mass or less, based on 100% by mass of the total solid content of the electrode active material layer. At such an upper limit, the aggregation of the conductive assistants is suppressed, so that an electron conduction path is well formed, and the output characteristics can be further improved. In addition, it is possible to further improve the energy density of the non-aqueous electrolyte secondary battery. The lower limit of the content of the conductive assistant is not particularly limited, but is preferably more than 0% by mass, and is preferably 0.1% by mass or more, preferably 0.2% by mass or more, and more preferably 0.3% by mass or more. At such a lower limit, there is a sufficient amount of conductive assistant to form an electron conduction path, and therefore the output characteristics can be further improved.

[0069] In the electrode for a non-aqueous electrolyte secondary battery according to the present embodiment, the thickness of the electrode active material layer is not particularly limited, and conventionally known knowledge about batteries can be appropriately referred to. For example, the thickness of the electrode active material layer is usually about 1 to 1000 μm, preferably 20 to 800 μm, more preferably 30 to 500 μm, and even more preferably 40 to 200 μm. The thicker the electrode active material layer is, the more electrode active material can be retained to exert sufficient capacity (energy density). On the other hand, the thinner the electrode active material layer is, the more output characteristics can be improved (especially, a large capacity can be extracted during discharge at a high discharge rate).

[0070] As described above, the electrode for a non-aqueous electrolyte secondary battery according to this embodiment is characterized in that the binder contained in the electrode active material layer contains a first binder and a second binder. By adopting such a configuration, the rate characteristics can be improved in a non-aqueous electrolyte secondary battery having the electrode according to this embodiment (especially, a large capacity can be extracted during discharge at a high discharge rate). Although the detailed mechanism by which the above effect is achieved is unknown, the present inventors speculate as follows. However, the technical scope of the present invention is not limited to the following mechanism in any way.

[0071] According to the study by the present inventors, it was found that the rate characteristics of a non-aqueous electrolyte secondary battery are significantly improved by using a first binder (polyborosiloxane) in combination with a second binder other than polyborosiloxane (for example, PVdF or PVdF-HFP) compared to the case of using them alone. Here, a large amount of boron atoms are uniformly distributed in the polymer molecules of the first binder (polyborosiloxane). Therefore, by using polyborosiloxane as the first binder, an anion trap effect due to the boron atoms in the polyborosiloxane is expressed, and a transport path of lithium ions in the electrode active material layer is suitably formed. As a result, it is considered that the diffusion resistance of lithium ions in the electrode active material layer is reduced, and a significant improvement in the rate characteristics is achieved.

[0072] <<Method for manufacturing electrodes for non-aqueous electrolyte secondary batteries>> According to the present invention, a method for producing an electrode for a non-aqueous electrolyte secondary battery according to one embodiment of the present invention is also provided. This method is characterized in that it includes mixing an electrode active material and the first binder in an organic solvent to prepare a mixture, adding the second binder to the mixture and mixing to prepare an electrode active material slurry, and applying the electrode active material slurry to a surface of a current collector to form an electrode active material layer. According to this production method, an electrode for a non-aqueous electrolyte secondary battery according to one embodiment of the present invention is obtained. Furthermore, according to this production method, the rate characteristics of a battery using the obtained electrode are further improved compared to when the electrode active material, the first binder, and the second binder are added and mixed in a different order from the above. This is believed to be because the first binder can sufficiently cover the surface of the electrode active material in the absence of the second binder, and the above-mentioned anion trapping effect is more prominently exhibited.

[0073] In addition, in the manufacturing method according to the above embodiment, it is preferable to further include removing the organic solvent from the mixture by evaporation before adding the second binder. By adopting such a configuration, the rate characteristics of a battery using the obtained electrode are further improved. This is considered to be because the binding state of the components in the electrode active material layer is stabilized by once removing the organic solvent by evaporation, and this binding state is maintained even if the second binder is mixed thereafter.

[0074] The electrode for a non-aqueous electrolyte secondary battery according to this embodiment can improve the output characteristics of the non-aqueous electrolyte secondary battery by being applied to the non-aqueous electrolyte secondary battery. Therefore, according to another embodiment of the present invention, there is provided a non-aqueous electrolyte secondary battery including a power generating element including a positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer stacked in this order, and at least one of the positive electrode active material layer and the negative electrode active material layer is the electrode for a non-aqueous electrolyte secondary battery according to the embodiment of the present invention described above. The components of the non-aqueous electrolyte secondary battery other than the electrode will be briefly described below.

[0075] [Electrolyte layer] The electrolyte layer preferably has a configuration in which a separator is impregnated with an electrolytic solution (liquid electrolyte).

[0076] (electrolyte) The electrolyte functions as a carrier for lithium ions and has a form in which a lithium salt is dissolved in a non-aqueous solvent.

[0077] Examples of the non-aqueous solvent include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), ethyl methyl carbonate (EMC), methyl propionate (MP), methyl acetate (MA), methyl formate (MF), 4-methyldioxolane (4MeDOL), dioxolane (DOL), 2-methyltetrahydrofuran (2MeTHF), tetrahydrofuran (THF), dimethoxyethane (DME), propylene carbonate (PC), butylene carbonate (BC), dimethyl sulfoxide (DMSO), and γ-butyrolactone (GBL). Among them, the non-aqueous solvent is preferably a chain carbonate, more preferably at least one selected from the group consisting of diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC), from the viewpoint of further improving the rapid charging characteristics and the output characteristics.

[0078] Examples of the lithium salt include Li(FSO2)2N (lithium bis(fluorosulfonyl)imide; LiFSI), Li(C2F5SO2)2N, LiPF6, LiPO2F2, LiBF4, LiClO4, LiAsF6, and LiCF3SO3. Among them, the lithium salt preferably includes a fluorophosphate-based lithium salt such as LiPF6 or LiPO2F2 from the viewpoint of battery output and charge / discharge cycle characteristics. The concentration of the lithium salt in the electrolyte is preferably 0.1 to 3.0 mol / L, and more preferably 0.8 to 2.2 mol / L.

[0079] The electrolyte may further contain additives other than the above-mentioned components. Specific examples of such compounds include ethylene carbonate, vinylene carbonate, methylvinylene carbonate, dimethylvinylene carbonate, phenylvinylene carbonate, diphenylvinylene carbonate, ethylvinylene carbonate, diethylvinylene carbonate, vinylethylene carbonate, 1,2-divinylethylene carbonate, 1-methyl-1-vinylethylene carbonate, 1-methyl-2-vinylethylene carbonate, 1-ethyl-1-vinylethylene carbonate, 1-ethyl-2-vinylethylene carbonate, and 1-ethyl-2-vinylethylene carbonate. Examples of the additives include ethylene carbonate, vinyl vinylene carbonate, allyl ethylene carbonate, vinyloxymethyl ethylene carbonate, allyloxymethyl ethylene carbonate, acryloxymethyl ethylene carbonate, methacryloxymethyl ethylene carbonate, ethynyl ethylene carbonate, propargyl ethylene carbonate, ethynyloxymethyl ethylene carbonate, propargyl oxyethylene carbonate, methylene ethylene carbonate, and 1,1-dimethyl-2-methylene ethylene carbonate. These additives may be used alone or in combination of two or more. The amount of additive used in the electrolyte solution may be appropriately adjusted.

[0080] (Separator) The separator constituting the electrolyte layer has a function of retaining the electrolyte to ensure lithium ion conductivity between the positive electrode and the negative electrode, and a function of acting as a partition between the positive electrode and the negative electrode. Examples of the form of the separator include a porous sheet separator made of a polymer or fiber that absorbs and retains the electrolyte, a nonwoven fabric separator, and the like.

[0081] [Positive and negative current collectors] The material constituting the current collector plates (25, 27) is not particularly limited, and any known highly conductive material conventionally used as a current collector plate for a lithium ion secondary battery may be used. As the material constituting the current collector plates, for example, metal materials such as aluminum, copper, titanium, nickel, stainless steel (SUS), and alloys thereof are preferable. From the viewpoints of light weight, corrosion resistance, and high conductivity, aluminum and copper are more preferable, and aluminum is particularly preferable. The positive electrode current collector plate 25 and the negative electrode current collector plate 27 may be made of the same material or different materials.

[0082] [Positive and negative leads] Although not shown in the figures, the current collector 11 and the current collector plates (25, 27) may be electrically connected via a positive electrode lead and a negative electrode lead. As the constituent materials of the positive electrode and the negative electrode lead, materials used in known lithium ion secondary batteries may be similarly adopted. Note that the part removed from the exterior body is preferably covered with a heat-resistant insulating heat shrink tube or the like so as not to come into contact with peripheral devices or wiring, causing a current leak and affecting products (e.g., automobile parts, particularly electronic devices, etc.).

[0083] [Battery exterior] As the battery exterior body, a known metal can case can be used, and a bag-shaped case using a laminate film 29 containing aluminum, which can cover the power generating element as shown in FIG. 1, can be used. The laminate film can be, for example, a three-layer laminate film formed by laminating PP, aluminum, and nylon in this order, but is not limited thereto. A laminate film is preferable from the viewpoint of being excellent in high output and cooling performance and being suitable for use in batteries for large equipment such as EVs and HEVs. In addition, an aluminate laminate is more preferable as the exterior body because the collective pressure applied to the power generating element from the outside can be easily adjusted and the thickness of the electrolyte layer can be easily adjusted to the desired thickness.

[0084] The nonaqueous electrolyte secondary battery according to the present embodiment can exhibit excellent output characteristics, and is therefore suitable for use as a power source for driving EVs and HEVs.

[0085] The following embodiments are also included within the scope of the present invention: an electrode for a nonaqueous electrolyte secondary battery as defined in claim 1 having the characteristics of claim 2; an electrode for a nonaqueous electrolyte secondary battery as defined in claim 1 or 2 having the characteristics of claim 3; an electrode for a nonaqueous electrolyte secondary battery as defined in any one of claims 1 to 3 having the characteristics of claim 4; an electrode for a nonaqueous electrolyte secondary battery as defined in any one of claims 1 to 4 having the characteristics of claim 5; an electrode for a nonaqueous electrolyte secondary battery as defined in claim 5 having the characteristics of claim 6; an electrode for a nonaqueous electrolyte secondary battery as defined in any one of claims 1 to 6 having the characteristics of claim 7; a nonaqueous electrolyte secondary battery as defined in claim 8, comprising the electrode for a nonaqueous electrolyte secondary battery as defined in any one of claims 1 to 7; and a method for producing an electrode for a nonaqueous electrolyte secondary battery as defined in claim 9 having the characteristics of claim 10. EXAMPLES

[0086] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples.

[0087] [Example 1] <Preparation of negative electrode> A powder composition consisting of 94 parts by mass of graphite (Gr, average particle size (D50) = 20 μm) as a negative electrode active material and 1 part by mass of acetylene black (AB, manufactured by Denka Co., Ltd., Denka Black (registered trademark); average particle size (primary particle size): 0.023 μm) as a conductive assistant was mixed at 2000 rpm for 1 minute using a planetary stirring type mixing and kneading device "Awatori Rentaro" (ARE-310, manufactured by Thinky Corporation). Next, an appropriate amount of N-methyl-2-pyrrolidone (NMP), a slurry viscosity adjusting solvent, was added to the above powder composition and mixed at 2000 rpm for 2 minutes using the same device. Thereafter, a mixture having the following chemical structure as a first binder:

[0088] [ka]

[0089] A solution of 1 part by mass of polyborosiloxane (PBS, number average molecular weight (Mn) = 42500, polydispersity index (PDI) (Mw / Mn) = 1.2, molar ratio of silicon atoms to boron atoms (Si / B) = 1.0) dissolved in NMP was added and mixed for 3 minutes at 2000 rpm using the same device. Thereafter, the obtained slurry was dried at 80 ° C for 10 minutes to remove the solvent. Next, a solution of 4 parts by mass of PVdF (Kureha Corporation, Kureha KF Polymer (registered trademark) W # 9700) having a linear structure as a second binder was further added as a second binder, and mixed for 4 minutes at 2000 rpm using the same device to prepare a negative electrode active material slurry. The negative electrode active material slurry was applied to a Cu foil (thickness 10 μm) placed on a smooth plate so that the negative electrode active material mass (area weight of the negative electrode active material) was 5 mg / cm. 2 The mixture was uniformly applied using a doctor blade and dried on a hot plate at 80° C. for 1 hour. The obtained laminate was then pressed using a roll press. It was then placed in a vacuum dryer and dried at 130° C. for 8 hours under vacuum conditions to produce the negative electrode of this example. The porosity of the negative electrode active material layer in the obtained negative electrode was 25% and the thickness was 31 μm.

[0090] <Production of lithium-ion secondary battery (coin cell)> The negative electrode and counter electrode Li prepared above were placed opposite each other, and two separators (polyolefin, thickness: 20 μm) were placed between them. Next, a laminate of the negative electrode, separator, and counter electrode (Li metal) was placed on the bottom side of a coin cell (CR2032, material: stainless steel (SUS316)). Furthermore, a gasket was attached to maintain insulation between the electrodes, an electrolyte was injected with a syringe, a spring and a spacer were laminated, and the upper side of the coin cell was overlapped and sealed by crimping to prepare a lithium ion secondary battery (coin cell) of this example. As the electrolyte, an electrolyte obtained by dissolving LiPF61 mol / L in a mixed solvent (volume ratio 3:7) of ethylene carbonate (EC) and diethyl carbonate (DEC) was used.

[0091] [Example 2] The negative electrode and lithium ion secondary battery (coin cell) of this example were produced in the same manner as in Example 1 described above, except that the amount of the first binder (polyborosiloxane) added was changed to 2 parts by mass and the amount of the second binder (PVdF) added was changed to 3 parts by mass.

[0092] [Example 3] The negative electrode and lithium ion secondary battery (coin cell) of this example were produced in the same manner as in Example 1 described above, except that the amount of the first binder (polyborosiloxane) added was changed to 3 parts by mass and the amount of the second binder (PVdF) added was changed to 2 parts by mass.

[0093] [Example 4] The negative electrode and lithium ion secondary battery (coin cell) of this example were produced in the same manner as in Example 3 described above, except that the NMP solution of the first binder (polyborosiloxane) and the NMP solution of the second binder (PVdF) were simultaneously added to the above powder composition and mixed for 4 minutes at 2000 rpm using a planetary stirring type mixer / kneader to produce a negative electrode active material slurry.

[0094] [Example 5] The negative electrode and lithium ion secondary battery (coin cell) of this example were produced in the same manner as in Example 3 described above, except that the negative electrode active material slurry was produced by reversing the order of addition of the NMP solution of the first binder (polyborosiloxane) and the NMP solution of the second binder (PVdF).

[0095] [Example 6] The negative electrode and the lithium ion secondary battery (coin cell) of this example were produced in the same manner as in Example 2 described above, except that polyvinylidene fluoride-hexafluoropropylene (PVdF-HFP(1)) (Kyner Flex 2851, manufactured by Arkema, proportion of the number of constituent units derived from hexafluoropropylene: 2.4 mol%) having a linear structure was used instead of PVdF as the second binder.

[0096] [Example 7] The negative electrode and the lithium ion secondary battery (coin cell) of this example were produced in the same manner as in Example 2 described above, except that polyvinylidene fluoride-hexafluoropropylene (PVdF-HFP(2)) (Kyner Flex 2501, manufactured by Arkema, proportion of the number of constituent units derived from hexafluoropropylene: 6.9 mol%) having a linear structure was used instead of PVdF as the second binder.

[0097] [Comparative Example 1] A negative electrode and a lithium ion secondary battery (coin cell) of this comparative example were produced in the same manner as in Example 1 described above, except that the NMP solution of the first binder was not added and the amounts of graphite and the second binder (PVdF) added were changed to 89 parts by mass and 10 parts by mass, respectively.

[0098] [Comparative Example 2] Except for not adding the NMP solution of the second binder and changing the amount of the first binder (polyborosiloxane) to 5 parts by mass, an attempt was made to fabricate a negative electrode and a lithium ion secondary battery (coin cell) of this comparative example by the same method as in Example 1. However, it was not possible to form a negative electrode active material layer.

[0099] [Comparative Example 3] An attempt was made to fabricate a negative electrode and a lithium ion secondary battery (coin cell) of this comparative example by the same method as in Example 1, except that the NMP solution of the second binder was not added and the amounts of graphite and the first binder (polyborosiloxane) added were changed to 91 parts by mass and 8 parts by mass, respectively. However, it was not possible to form a negative electrode active material layer.

[0100] [Comparative Example 4] The negative electrode and lithium ion secondary battery (coin cell) of this comparative example were produced in the same manner as in Example 1 described above, except that the NMP solution of the second binder was not added and the amounts of graphite and the first binder (polyborosiloxane) added were changed to 89 parts by mass and 10 parts by mass, respectively.

[0101] [Comparative Example 5] A negative electrode and a lithium ion secondary battery (coin cell) of this comparative example were produced in the same manner as in Example 1 described above, except that the NMP solution of the first binder was not added and the amount of the second binder (PVdF) added was changed to 5 parts by mass.

[0102] [Evaluation of rate characteristics] The evaluation of the rate characteristics was carried out by placing the lithium ion secondary battery (coin cell) prepared above in a thermostatic chamber (manufactured by Espec Corporation) set at 25°C. Specifically, charging and discharging were repeated three times at a rate of 0.1C, with 1C=360mAh / g. At this time, discharging was carried out in CC-CV mode with the cell voltage in the range of 0.01 to 2.0V, and charging was carried out in CC mode. At this time, the rest time between charging and discharging was 8 hours. After that, the battery was discharged at 0.1C to 0.01V in CC-CV mode, and then charged at 3C to a cell voltage of 2.0V in CC mode. The percentage of the charge capacity (effective capacity) at 3C relative to the charge capacity (reference capacity) at 0.1C obtained at this time was calculated as the effective capacity ratio [%]. The results are shown in Table 1 below.

[0103] [Table 1]

[0104] From the results shown in Table 1, it can be seen that the rate characteristics can be improved according to the electrode for non-aqueous electrolyte secondary batteries according to the present invention (Examples 1 to 7) in which the first binder (polyborosiloxane) and the second binder (PVdF or PVdF-HFP) are used in combination. In contrast, it can be seen that in Comparative Examples 1 to 5 in which at least one of the first binder and the second binder is not used, it is not possible to form a negative electrode active material layer or to achieve sufficient rate characteristics. In addition, from a comparison between Comparative Example 1 and Comparative Example 4 and the Examples, it can also be seen that according to the present invention, the rate characteristics can be improved even with a smaller amount of binder (i.e., while increasing the energy density of the battery).

[0105] Furthermore, a comparison of Examples 3, 5, and 6 shows that the rate characteristics can be further improved by first obtaining a mixture containing an electrode active material and a first binder in an organic solvent, and then adding a second binder to the mixture to obtain an anode active material slurry and using the resulting mixture to form an electrode active material layer. [Explanation of symbols]

[0106] 10a laminated secondary battery, 11a: outermost current collector on the positive electrode side; 11b: an outermost current collector on the negative electrode side; 11' Positive electrode current collector 12 Negative electrode current collector 13 positive electrode active material layer, 15 negative electrode active material layer, 17 electrolyte layer, 19 cell layer, 21 Power generation elements, 25 Positive current collector (positive tab), 27 negative electrode current collector (negative electrode tab), 29 Laminating film.

Claims

1. An electrode for a non-aqueous electrolyte secondary battery, comprising an electrode active material layer containing an electrode active material and a binder disposed on a surface of a current collector, The binder is represented by the following chemical formula 1: 【Chemistry 1】 In the formula, R 1 and R 2 each independently represents a monovalent organic group; R 1 and R 2 At least one of represents a monovalent aromatic group; and a repeating unit represented by the following chemical formula 2: 【Chemistry 2】 In the formula, R 3 represents a monovalent organic group, and a second binder other than the polyborosiloxane, the first binder having a structure in which silicon atoms in Chemical Formula 1 and boron atoms in Chemical Formula 2 are alternately bonded via oxygen atoms, the first binder being composed of a polyborosiloxane having a repeating unit represented by the formula:

2. 2. The electrode for a non-aqueous electrolyte secondary battery in accordance with claim 1, wherein a molar ratio (Si / B) of silicon atoms to boron atoms contained in said polyborosiloxane satisfies 0.4≦Si / B≦0.

6.

3. 3. The electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein the content of the first binder in the electrode active material layer is 1 to 3 mass %.

4. 3. The electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein a mass ratio of said first binder to a total amount (100 mass%) of said binder is 10 to 70 mass%.

5. 3. The electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein the second binder contains a polymer having a repeating unit derived from vinylidene fluoride (VdF).

6. 6. The electrode for a non-aqueous electrolyte secondary battery according to claim 5, wherein the polymer has a linear structure.

7. 3. The electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein the negative electrode contains at least graphite as the electrode active material.

8. 3. A non-aqueous electrolyte secondary battery comprising: a power generating element including a positive electrode active material layer, an electrolyte layer, and a negative electrode active material layer laminated in this order; and at least one of the positive electrode active material layer and the negative electrode active material layer being the electrode for a non-aqueous electrolyte secondary battery according to claim 1 or 2.

9. A method for producing an electrode for a non-aqueous electrolyte secondary battery according to claim 1, comprising the steps of: mixing the electrode active material and the first binder in an organic solvent to prepare a mixture; adding the second binder to the mixture and mixing to prepare an electrode active material slurry; applying the electrode active material slurry to a surface of the current collector to form the electrode active material layer; The method for producing an electrode for a non-aqueous electrolyte secondary battery includes the steps of:

10. 10. The method for producing an electrode for a non-aqueous electrolyte secondary battery according to claim 9, further comprising removing the organic solvent from the mixture by evaporation before adding the second binder.

Citation Information

Patent Citations

  • Solid material- / gel electrolyte storage battery having a binder made of an inorganic-organic hybrid polymer and method for producing the same

    JP2016503564A