Ethylene adsorption film, wound body, and method for producing ethylene adsorption film
The ethylene adsorption film with a base, anchor, and porous metal complex layer addresses the low adsorption capacity of conventional films by enhancing ethylene removal and adhesion, achieving high ethylene adsorption and reusable performance.
Patent Information
- Application Number
- JP2023069207
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-20
- Publication Date
- 2024-10-31
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional ethylene adsorption films exhibit insufficient ethylene adsorption capacity, necessitating improvements for better ethylene removal in applications like fruit and vegetable storage.
An ethylene adsorption film comprising a base layer, an anchor layer with a polar group-containing polymer or organic onium compound, and a porous metal complex layer, where the metal complex is formed by bonding metals like titanium, manganese, or copper with organic ligands such as 1,3,5-benzenedicarboxylic acid, enhancing the ethylene adsorption capacity and interlayer adhesion.
The film achieves excellent ethylene adsorption ability, with capacities exceeding 0.8 ppm/g/h, and demonstrates high interlayer adhesion, allowing for repeated use by desorbing ethylene at 100°C and maintaining visibility through appropriate light transmittance and haze levels.
Smart Images

Figure 2024154954000001_ABST
Abstract
Description
[Technical Field]
[0001] The present invention relates to an ethylene adsorption film, a roll, and a method for producing an ethylene adsorption film. [Background technology]
[0002] Ethylene is a gas produced by fruits and vegetables and is known as one of the plant hormones that promotes ripening and senescence of plant tissues. It is believed that the production of ethylene is a major cause of the loss of freshness of fruits and vegetables during storage and transportation after harvest. Therefore, to maintain the freshness of fruits and vegetables, it is important to remove or decompose ethylene and prevent it from coming into contact with harvested fruits.
[0003] Various methods for removing or decomposing ethylene have been investigated. For example, Patent Document 1 discloses a freshness-maintaining material composition that maintains the freshness of fresh produce such as fruits and vegetables by suppressing their deterioration, and that contains cyclodextrin. Furthermore, Patent Document 2 discloses a plastic functional film capable of adhering ethylene to its surface, which contains a substance with catalytic function that decomposes ethylene into carbon dioxide and water and enables them to be released from one side of the film to the other side.
[0004] Porous materials such as activated carbon, silica gel, zeolite, and porous metal complexes are sometimes used for deodorization and gas separation and purification, and the use of such materials for removing ethylene is also being considered. For example, Patent Document 3 discloses an adsorption sheet containing a porous metal complex having a porous structure formed by metal ions and organic ligands capable of binding to the metal ions, and organic fibers. Patent Document 4 also discloses an adsorption sheet containing [Cu(C 10 H8N4)] nPatent Document 5 discloses an ethylene gas adsorbent comprising a porous coordination polymer complex having a chemical structure with the basic structural unit of (I), and Patent Document 5 discloses an ethylene gas adsorbent comprising a porous metal complex or a metal-supported inorganic porous material. The adsorbent sheet disclosed in Patent Document 3 is a fiber sheet formed by a wet papermaking method, and the ethylene adsorbent disclosed in Patent Document 4 is a powder comprising a porous coordination polymer complex. In the ethylene gas adsorbent disclosed in Patent Document 5, the ethylene gas adsorbent is mixed and dispersed in a thermoplastic resin. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 2019-170368 [Patent Document 2] International Publication No. 2017 / 135433 [Patent Document 3] International Publication No. 2013 / 115033 [Patent Document 4] Japanese Patent Application Laid-Open No. 2004-322005 [Patent Document 5] Japanese Patent Publication No. 2022-001357 Summary of the Invention [Problem to be solved by the invention]
[0006] As described above, methods for removing ethylene by adsorbing ethylene onto porous metal complexes, etc. have been investigated. However, the ethylene adsorption capacity of conventional ethylene adsorption films is not sufficiently high, and further improvement is required.
[0007] Therefore, in order to solve the problems of the prior art, the present inventors have carried out investigations with the aim of providing an ethylene adsorption film that exhibits excellent ethylene adsorption capacity. [Means for solving the problem]
[0008] Examples of specific embodiments of the present invention are given below.
[0009] [1] An ethylene-adsorbed film comprising a substrate layer, an anchor layer containing a polar group-containing polymer or an organic onium compound, and a porous metal complex layer. [2] The porous metal complex layer is The ethylene adsorption film according to [1], which comprises a porous metal complex formed by bonding at least one metal selected from the group consisting of titanium, manganese, iron, cobalt, nickel, copper, zinc, silver, aluminum, zirconium, magnesium, calcium, vanadium, cadmium, and palladium to an organic ligand. [3] The ethylene-adsorbed film according to [2], wherein the organic ligand has at least one functional group selected from the group consisting of a carboxy group, a hydroxy group, an amino group, and a sulfonic acid group. [4] The ethylene-adsorbed film according to [2] or [3], wherein the organic ligand is at least one selected from the group consisting of 1,3,5-benzenetricarboxylic acid, 1,4-benzenedicarboxylic acid, and 2,5-dihydroxyterephthalic acid. [5] The ethylene adsorption film according to any one of [1] to [4], wherein the porous metal complex layer has a thickness of 0.1 to 10 μm. [6] The ethylene adsorption film according to any one of [1] to [5], wherein the arithmetic mean height Sa of the anchor layer is 0.1 to 20 μm. [7] The ethylene-adsorbed film according to any one of [1] to [6], wherein the anchor layer has a water contact angle of 50° or less. [8] The ethylene adsorption film according to any one of [1] to [7], wherein the polar group-containing polymer is at least one selected from the group consisting of polyvinyl alcohol, polyvinylpyrrolidone, polyethyleneimine, polyacrylic acid, sodium polyacrylate, poly(4-styrenesulfonic acid), poly(sodium 4-styrenesulfonate), and polyallylamine hydrochloride. [9] The ethylene adsorption film according to any one of [1] to [8], wherein the anchor layer comprises at least one kind of particles selected from organic particles and inorganic particles.
[10] The ethylene adsorption film according to [9], wherein the organic particles and the inorganic particles each have an average particle size of 0.1 to 20 μm.
[11] The ethylene adsorption film according to any one of [1] to
[10] , wherein the anchor layer consists of two or more layers.
[12] The ethylene-adsorbent film according to any one of [1] to
[11] , which is used for packaging fruits and vegetables.
[13] A rolled body obtained by rolling up the ethylene adsorption film according to any one of [1] to
[12] .
[14] A step of forming an anchor layer containing a polar group-containing polymer or an organic onium compound on a substrate layer; a step of applying a solution in which a metal hydroxide is dispersed onto the anchor layer, and converting the metal hydroxide into a porous metal complex to form a porous metal complex layer.
[15] The step of forming a porous metal complex layer includes:
[14] A method for producing an ethylene adsorption film, comprising the steps of: applying a solution in which a metal hydroxide is dispersed onto an anchor layer to form a coating film; and immersing the coating film in a solution containing an organic ligand to form a porous metal complex layer.
[16] The method for producing an ethylene adsorption film according to
[14] or
[15] , wherein the metal constituting the metal hydroxide is at least one selected from the group consisting of titanium, manganese, iron, cobalt, nickel, copper, zinc, silver, aluminum, zirconium, magnesium, calcium, vanadium, cadmium, and palladium.
[17] The method for producing an ethylene-adsorbed film according to
[15] or
[16] , wherein the organic ligand is at least one selected from the group consisting of 1,3,5-benzenetricarboxylic acid, 1,4-benzenedicarboxylic acid, and 2,5-dihydroxyterephthalic acid.
[18] The method for producing an ethylene adsorption film according to any one of
[14] to
[17] , wherein the polar group-containing polymer is at least one selected from the group consisting of polyvinyl alcohol, polyvinylpyrrolidone, polyethyleneimine, polyacrylic acid, sodium polyacrylate, poly(4-styrenesulfonic acid), poly(sodium 4-styrenesulfonate), and polyallylamine hydrochloride. [Effects of the Invention]
[0010] According to the present invention, an ethylene adsorption film exhibiting excellent ethylene adsorption capacity can be obtained. [Brief explanation of the drawings]
[0011] [Figure 1] FIG. 1 is a cross-sectional view illustrating the structure of the ethylene adsorption film of this embodiment. [Figure 2] FIG. 2 is a cross-sectional view illustrating the structure of the ethylene adsorption film of this embodiment. DETAILED DESCRIPTION OF THE INVENTION
[0012] The present invention will be described in detail below. The following description of the constituent elements may be based on representative embodiments or specific examples, but the present invention is not limited to such embodiments. In this specification, the expression "X to Y" (X and Y are arbitrary numbers) means "X or more and Y or less," unless otherwise specified, and also includes "preferably greater than X" or "preferably less than Y." Furthermore, the expression "X or more" (X is an arbitrary number) or "Y or less" (Y is an arbitrary number) also includes the meaning "preferably greater than X" or "preferably less than Y." In the following description, the terms "film" and "sheet" are not clearly distinguished from each other, and the term "film" includes the term "sheet," and the term "sheet" includes the term "film."
[0013] (Ethylene adsorption film) This embodiment relates to an ethylene adsorption film (hereinafter also referred to as the present ethylene adsorption film) comprising a substrate layer, an anchor layer containing a polar group-containing polymer or an organic onium compound, and a porous metal complex layer. As shown in Fig. 1, the present ethylene adsorption film 10 comprises a substrate layer 2, an anchor layer 4, and a porous metal complex layer 6, in this order. While other layers may be provided between the substrate layer 2, the anchor layer 4, and the porous metal complex layer 6 as needed, in this embodiment, it is preferable that the substrate layer 2 and the anchor layer 4 are directly laminated, and it is also preferable that the anchor layer 4 and the porous metal complex layer 6 are directly laminated.
[0014] The ethylene adsorption film of this embodiment, having the above-described configuration, can exhibit excellent ethylene adsorption capacity. Here, the ethylene adsorption capacity can be evaluated by calculating the ethylene adsorption amount using the following method. Specifically, first, the ethylene adsorption film is cut to a predetermined size (e.g., 5 cm x 9 cm), placed in a glass bottle, and sealed. Next, standard ethylene gas is injected into the glass bottle so that the ethylene gas concentration in the glass bottle becomes 100 ppm. Immediately, 1 mL of gas is sampled from the glass bottle, and the ethylene concentration is measured by gas chromatography. After one hour, 1 mL of gas is sampled again from the glass bottle, and the ethylene concentration is measured. The ethylene adsorption amount of the ethylene adsorption film is calculated from the difference. Furthermore, the same measurement is performed without the ethylene adsorption film to determine the amount of ethylene leaked from the glass bottle during the one hour period, and this amount is subtracted from the ethylene adsorption amount of the ethylene adsorption film. That is, the ethylene adsorption amount can be calculated using the following formula. Amount of ethylene adsorption (ppm / g / h) = Initial ethylene concentration (ppm) - Ethylene concentration after 1 hour in the glass bottle containing the ethylene adsorption film (ppm) - Amount of ethylene leaked from the glass bottle (ppm)
[0015] The ethylene adsorption amount (ppm / g / h) calculated by the above method is preferably 0.8 ppm / g / h or more, more preferably 0.9 ppm / g / h or more, even more preferably 1.0 ppm / g / h or more, still more preferably 1.5 ppm / g / h or more, even more preferably 2.0 ppm / g / h or more, still more preferably 2.5 ppm / g / h or more, and particularly preferably 3.0 ppm / g / h or more. The upper limit of the ethylene adsorption amount (ppm / g / h) calculated by the above method is not particularly limited and may be, for example, 100 ppm / g / h.
[0016] Porous metal complexes have a larger specific surface area than activated carbon or zeolite, and therefore exhibit excellent ethylene adsorption capacity. Previously, the use of powders of porous metal complexes as ethylene adsorbents has been investigated. However, when forming powdered ethylene adsorbents into sheets, the ethylene adsorbent and resin are typically mixed and then formed into a sheet. In this case, the ethylene adsorption sites are blocked by the resin, making it difficult to obtain a sheet with excellent ethylene adsorption capacity. Therefore, the present inventors conducted research aimed at producing an ethylene adsorption film having a porous metal complex layer with excellent ethylene adsorption capacity. The present inventors discovered that the configuration of this embodiment allows film formation without inhibiting the ethylene adsorption sites of the porous metal complex, resulting in a sheet with excellent ethylene adsorption capacity. Furthermore, in this embodiment, the provision of an anchor layer enables the porous metal complex layer to be thickened. The increased specific surface area and thicker porous metal complex layer allow for the production of an ethylene adsorption film with even better ethylene adsorption capacity.
[0017] In this embodiment, the size of the voids (adsorption sites) formed in the three-dimensional structure of the porous metal complex is suitable for ethylene, which is the substance to be adsorbed.
[0018] Furthermore, the ethylene adsorption film of this embodiment has the above-mentioned configuration, and therefore also has excellent interlayer adhesion. Specifically, in the ethylene adsorption film of this embodiment, a predetermined anchor layer is provided between the substrate layer and the porous metal complex layer, thereby enhancing interlayer adhesion. The interlayer adhesion can be evaluated by attaching an adhesive tape ("Cellotape (registered trademark)" manufactured by Nichiban Co., Ltd.) to the surface of the ethylene adsorption film facing the porous metal complex layer, and then peeling it off, and observing whether the adhesive tape remains adhesive.
[0019] Furthermore, the ethylene adsorption film of this embodiment can be reused repeatedly. For example, the porous metal complex layer that has adsorbed ethylene can be desorbed by heating it to about 100°C. The porous metal complex layer from which ethylene has been desorbed can then adsorb ethylene again, allowing for repeated use.
[0020] The total light transmittance of the present ethylene-adsorbed film is not particularly limited, but is preferably 70% or more, more preferably 75% or more, and even more preferably 80% or more. The upper limit of the total light transmittance of the present ethylene-adsorbed film is not particularly limited, and may be 100%. When the total light transmittance of the ethylene-adsorbed film is within the above range, the design properties of the ethylene-adsorbed film can be improved, and the visibility of the contents can also be improved. The total light transmittance of the present ethylene-adsorbed film is a value measured in accordance with JIS K 7136:2000.
[0021] The haze of the present ethylene adsorption film is not particularly limited, but is preferably 90% or less, more preferably 80% or less, and even more preferably 70% or less. The lower limit of the haze of the present ethylene adsorption film is not particularly limited, and may be 0%. When the haze of the ethylene adsorption film is within the above range, the design properties of the ethylene adsorption film can be improved, and the visibility of the contents can also be improved. The haze of the present ethylene adsorption film is a value measured in accordance with JIS K 7136:2000.
[0022] The total thickness of the ethylene adsorption film is preferably 10 μm or more, more preferably 15 μm or more, and even more preferably 20 μm or more. The total thickness of the ethylene adsorption film is preferably 3000 μm or less, more preferably 2000 μm or less, and even more preferably 1500 μm or less. By controlling the total thickness of the ethylene adsorption film within the above range, the ethylene adsorption capacity can be more effectively improved.
[0023] The present embodiment may also relate to a rolled body obtained by rolling up an ethylene adsorption film. Because the ethylene adsorption film has appropriate strength and flexibility, it can be stored or distributed in the form of a roll.
[0024] (Porous metal complex layer) The ethylene adsorption film has a porous metal complex layer. The porous metal complex layer is a layer containing a porous metal complex (Porous Coordination Polymer or Metal Organic Framework: MOF). The content of the porous metal complex in the porous metal complex layer is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, even more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more. The content of the porous metal complex in the porous metal complex layer may be 100% by mass, and the porous metal complex layer may be a layer made of the porous metal complex. In this embodiment, the porous metal complex has been successfully formed into a membrane, and therefore, as described above, a porous metal complex layer with a high content of the porous metal complex can be formed.
[0025] In porous metal complexes, the metal and organic ligands form a coordination network, resulting in a three-dimensional structure with a high specific surface area compared to activated carbon or zeolite. Furthermore, the self-organization of the metal and organic ligands in the porous metal complex forms a crystalline framework, which provides a high density of coordinatively unsaturated metal cations (adsorption sites), allowing for selective interaction with and adsorption of ethylene.
[0026] The metal (metal ion) contained in the porous metal complex is preferably at least one metal (metal ion) selected from metals belonging to groups 1 to 13 of the periodic table. The metal contained in the porous metal complex is preferably at least one selected from the group consisting of titanium, manganese, iron, cobalt, nickel, copper, zinc, silver, aluminum, zirconium, magnesium, calcium, vanadium, cadmium, and palladium, more preferably at least one selected from the group consisting of iron, copper, zinc, aluminum, and magnesium, and even more preferably at least one selected from the group consisting of copper and magnesium. The metal contained in the porous metal complex may be one type or two or more types.
[0027] The organic ligand constituting the porous metal complex is preferably an organic compound having two or more sites capable of forming a coordinate bond with the metal in the molecule, and is preferably an organic compound that forms a coordination network with the metal to form a porous structure having a plurality of pores capable of accommodating ethylene.
[0028] The organic ligand is preferably an anionic ligand. Here, the anionic ligand means a ligand whose coordinated site to the metal is anionic. Examples of the organic ligand include sulfonic acids such as trifluoromethanesulfonic acid and benzenesulfonic acid; formic acid, acetic acid, trifluoroacetic acid, propionic acid, butyric acid, isobutyric acid, valeric acid, caproic acid, enanthic acid, cyclohexanecarboxylic acid, caprylic acid, octylic acid, pelargonic acid, capric acid, lauric acid, myristic acid, pentadecylic acid, palmitic acid, margaric acid, stearic acid, tuberculostearic acid, arachidic acid, behenic acid, lignoceric acid, α-linolenic acid, eicosanoid acid, and the like. Aliphatic monocarboxylic acids such as sapentaenoic acid, docosahexaenoic acid, linoleic acid, and oleic acid; aromatic monocarboxylic acids such as benzoic acid, 2,5-dihydroxybenzoic acid, 3,7-dihydroxy-2-naphthoic acid, 2,6-dihydroxy-1-naphthoic acid, and 4,4'-dihydroxy-3-biphenylcarboxylic acid; heteroaromatic monocarboxylic acids such as nicotinic acid and isonicotinic acid; aliphatic dicarboxylic acids such as 1,4-cyclohexanedicarboxylic acid and fumarate; and 1,3-benzenedicarboxylic acid. aromatic dicarboxylic acids such as 1,4-benzenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, and 2,5-dihydroxyterephthalic acid; heteroaromatic dicarboxylic acids such as 2,5-thiophenedicarboxylic acid, 2,2'-dithiophenedicarboxylic acid, 2,3-pyrazinedicarboxylic acid, 2,5-pyridinedicarboxylic acid, and 3,5-pyridinedicarboxylic acid; 1,3,5-benzenetricarboxylic acid; Examples of the aromatic carboxylic acids include carboxylic acids, aromatic tricarboxylic acids such as 1,3,4-benzenetricarboxylic acid and biphenyl-3,4',5-tricarboxylic acid; aromatic tetracarboxylic acids such as 1,2,4,5-benzenetetracarboxylic acid, [1,1':4',1'']terphenyl-3,3'',5,5''-tetracarboxylic acid and 5,5'-(9,10-anthracenediyl)diisophthalate; and heterocyclic compounds such as imidazolate, 2-methylimidazolate and benzimidazolate.
[0029] Among these, the organic ligand preferably has at least one functional group selected from the group consisting of a carboxy group, a hydroxy group, an amino group, and a sulfonic acid group, and particularly preferably has a carboxy group. That is, the organic ligand is preferably at least one selected from the group consisting of an aliphatic monocarboxylic acid, an aromatic monocarboxylic acid, a heteroaromatic monocarboxylic acid, an aliphatic dicarboxylic acid, an aromatic dicarboxylic acid, a heteroaromatic dicarboxylic acid, an aromatic tricarboxylic acid, and an aromatic tetracarboxylic acid, more preferably at least one selected from the group consisting of an aromatic monocarboxylic acid, a heteroaromatic monocarboxylic acid, an aromatic dicarboxylic acid, a heteroaromatic dicarboxylic acid, an aromatic tricarboxylic acid, and an aromatic tetracarboxylic acid, and particularly preferably at least one selected from the group consisting of 1,3,5-benzenetricarboxylic acid, 1,4-benzenedicarboxylic acid, and 2,5-dihydroxyterephthalic acid. The organic ligand contained in the porous metal complex may be one type or two or more types.
[0030] The organic ligand preferably has a ring structure, and more preferably has a benzene ring. Organic ligands having a ring structure tend to have high molecular symmetry, and therefore are more likely to form the skeleton of a porous metal complex. Furthermore, when the organic ligand has a ring structure, the ring can be easily modified with a functional group, making it easier to impart various functionalities to the porous metal complex layer.
[0031] The organic ligands described above may further have a substituent. The substituent is not particularly limited, but examples thereof include alkyl groups (straight-chain or branched alkyl groups having 1 to 5 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, and pentyl), halogen atoms (fluorine, chlorine, bromine, and iodine), alkoxy groups (methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, and tert-butoxy), and amino groups. , monoalkylamino groups (such as a methylamino group), dialkylamino groups (such as a dimethylamino group), formyl groups, epoxy groups, acyloxy groups (such as an acetoxy group, an n-propanoyloxy group, an n-butanoyloxy group, a pivaloyloxy group, or a benzoyloxy group), alkoxycarbonyl groups (such as a methoxycarbonyl group, an ethoxycarbonyl group, or an n-butoxycarbonyl group), nitro groups, cyano groups, hydroxy groups, acetyl groups, and trifluoromethyl groups.
[0032] In this embodiment, the porous metal complex preferably contains at least one metal ion selected from the group consisting of iron, copper, zinc, aluminum, and magnesium, and at least one organic ligand selected from the group consisting of 1,3,5-benzenetricarboxylic acid, 1,4-benzenedicarboxylic acid, and 2,5-dihydroxyterephthalic acid. Examples of such porous metal complexes include HKUST-1 (Cu / 1,3,5-benzenetricarboxylic acid) and MOF-74 (Mg / 2,5-dihydroxyterephthalic acid).
[0033] The thickness of the porous metal complex layer is preferably 0.1 μm or more, more preferably 0.3 μm or more, even more preferably 0.5 μm or more, even more preferably 0.7 μm or more, and particularly preferably 1 μm or more. The thickness of the porous metal complex layer is preferably 10 μm or less, more preferably 7 μm or less, even more preferably 5 μm or less, and particularly preferably 3 μm or less.
[0034] Increasing the density of the porous metal complex layer increases the ethylene adsorption capacity, but in conventional techniques, it has been difficult to form a high-density porous metal complex layer on a substrate layer. Furthermore, when attempting to increase the density of the porous metal complex layer, the interlayer adhesion with the substrate layer and the strength of the porous metal complex layer itself tend to deteriorate, resulting in a trade-off between improved ethylene adsorption capacity and improved interlayer adhesion. However, in this embodiment, by forming a predetermined anchor layer on the substrate layer, the density of the porous metal complex layer has been successfully increased. Furthermore, in this embodiment, excellent interlayer adhesion is exhibited even when the density of the porous metal complex layer is increased.
[0035] In this embodiment, the porous metal complex layer may have a needle-shaped crystal structure (metal hydroxide nanostructure). That is, the ethylene adsorption film of this embodiment may include a substrate layer, an anchor layer, and a porous metal complex layer containing a needle-shaped crystal structure (metal hydroxide nanostructure). In this embodiment, the needle-shaped crystal structure (metal hydroxide nanostructure) is a precursor formed in the process of forming a porous metal complex layer by a method described below. At least a portion of the needle-shaped crystal structure (metal hydroxide nanostructure) is converted into a porous metal complex, but in this embodiment, some of the needle-shaped crystal structure (metal hydroxide nanostructure) formed in the manufacturing process may remain in the porous metal complex layer. When the porous metal complex layer contains a needle-shaped crystal structure (metal hydroxide nanostructure), the radius (cross-sectional radius) of the needle-shaped crystal structure (metal hydroxide nanostructure) is preferably, for example, 10 to 1000 nm, and the length is preferably 1 to 500 μm.
[0036] (Anchor layer) The ethylene adsorption film has an anchor layer containing a polar group-containing polymer or an organic onium compound. The content of the polar group-containing polymer or the organic onium compound in the anchor layer is preferably 20% by mass or more, more preferably 25% by mass or more, even more preferably 30% by mass or more, and even more preferably 35% by mass or more.
[0037] The polar group contained in the polar group-containing polymer is not particularly limited, and examples thereof include a carboxy group, a hydroxy group, an amino group, an isocyanate group, an imino group, a (meth)acrylate group, and a sulfonic acid group. Of these, the polar group-containing polymer is preferably a hydrophilic polymer. The polar group-containing polymer is preferably at least one selected from the group consisting of polyvinyl alcohol, polyvinylpyrrolidone, polyethyleneimine, polyacrylic acid, sodium polyacrylate, poly(4-styrenesulfonic acid), sodium poly(4-styrenesulfonate), and polyallylamine hydrochloride, and more preferably polyvinyl alcohol. Of these, polyvinyl alcohol that becomes insoluble in aqueous solvents upon reaction with a crosslinking agent is preferred. Examples of polyvinyl alcohol that becomes insoluble in aqueous solvents upon reaction with a crosslinking agent include polyvinyl alcohols modified with silanol groups, epoxy groups, acetoacetyl groups, amino groups, ammonium groups, sulfonic groups, carboxy groups, and the like.
[0038] The organic onium compound is an onium compound having at least one hydrocarbon group, and examples thereof include organic ammonium compounds and organic phosphonium compounds. Examples of the organic ammonium compound include quaternary ammonium halides having a hydrocarbon group and their salts, and examples of the organic phosphonium compound include quaternary phosphonium halides having a hydrocarbon group and their salts. Specific examples of the organic onium compound include polydiallyldimethylammonium and polydiallyldimethylammonium chloride.
[0039] The water contact angle of the surface of the anchor layer is preferably 50° or less, more preferably 45° or less, even more preferably 40° or less, even more preferably 35° or less, and particularly preferably 30° or less. The lower limit of the water contact angle of the surface of the anchor layer is not particularly limited, and it is sufficient as long as it is 0° or more. By setting the water contact angle of the anchor layer within the above range, the interlayer adhesion with the porous metal complex layer can be more effectively improved. Furthermore, the water contact angle of the surface of the anchor layer within the above range means that the anchor layer is hydrophilic. That is, the anchor layer preferably contains a hydrophilic polymer, and the polar group-containing polymer is preferably a hydrophilic polymer.
[0040] The arithmetic mean height Sa of the anchor layer is preferably 0.1 μm or more, more preferably 0.5 μm or more, even more preferably 1 μm or more, even more preferably 2 μm or more, still more preferably 3 μm or more, and particularly preferably 4 μm or more. The arithmetic mean height Sa of the anchor layer is preferably 20 μm or less, more preferably 15 μm or less, even more preferably 12 μm or less, even more preferably 10 μm or less, and particularly preferably 8 μm or less.
[0041] In this embodiment, the anchor layer preferably contains at least one type of particles selected from organic particles and inorganic particles, which makes it easier to control the arithmetic mean height Sa within a predetermined range.
[0042] In this embodiment, it is preferable to form a fine uneven structure in the anchor layer so as to achieve the above-mentioned arithmetic mean height Sa. The fine uneven structure is formed, for example, by incorporating at least one type of particle selected from organic particles and inorganic particles into the anchor layer. Forming such a fine uneven structure in the anchor layer can more effectively improve the interlayer adhesion between the porous metal complex layer and the anchor layer, and between the anchor layer and the base layer. Increasing the interlayer adhesion between the anchor layer and the porous metal complex layer facilitates thickening of the porous metal complex layer. Furthermore, forming such a fine uneven structure in the anchor layer can increase the specific surface area of the porous metal complex layer. By thickening the porous metal complex layer and / or increasing the specific surface area of the porous metal complex layer, the ethylene adsorption capacity of the porous metal complex layer can be more effectively improved.
[0043] The average particle diameter (average primary particle diameter) of the organic particles and inorganic particles is preferably 0.1 μm or more, more preferably 0.5 μm or more, even more preferably 1 μm or more, even more preferably 1.5 μm or more, and particularly preferably 2 μm or more. The average particle diameter of the organic particles and inorganic particles is preferably 20 μm or less, more preferably 15 μm or less, and even more preferably 10 μm or less. The average particle diameter (average primary particle diameter) of the organic particles and inorganic particles can be determined by measuring the diameters of 10 or more particles using a scanning electron microscope (SEM) and averaging the results. When the cross-sectional shape of the particles is not circular (e.g., elliptical), the average of the longest and shortest diameters is used as the diameter of each particle.
[0044] Examples of organic particles that the anchor layer may contain include fine particles made of resins, naturally occurring components, sugars, chemically synthesized components, etc. Examples of organic particles include fine particles of acrylic resins, polystyrene, polysiloxane, melamine resins, benzoguanamine resins, polytetrafluoroethylene, polycarbonate, polyamide, chitin, chitosan, dextrin, oligosaccharides, wheat starch, rice starch, corn starch, potato starch, dextrin, cyclodextrin, lactose, glucose, sugar, reduced maltose, sorbitol, erythritol, xylitol, lactitol, mannitol, lactic acid bacteria, and casein.
[0045] Examples of inorganic particles that can be contained in the anchor layer include fine particles made of metals, alloys, metal oxides, metal nitrides, glass, rock components, inorganic compounds, and components produced by chemical synthesis. Examples of inorganic particles include zeolite, light calcium carbonate, heavy calcium carbonate, magnesium carbonate, kaolin, talc, calcium sulfate, barium sulfate, titanium oxide, zinc oxide, zinc sulfide, zinc carbonate, satin white, carbon black, aluminum silicate, diatomaceous earth, calcium silicate, magnesium silicate, silica, aluminum hydroxide, alumina, alumina hydrate, aluminosilicate, boehmite, pseudo-boehmite, and iron oxide. Among these, the inorganic particles are preferably at least one selected from the group consisting of metals, alloys, metal oxides, and metal nitrides, more preferably metal oxides, and particularly preferably silica particles.
[0046] The above-mentioned particles may be used alone or in combination of two or more kinds. Also, organic particles and inorganic particles may be used in combination, or particles of the same kind but different particle diameters may be used in combination.
[0047] The thickness of the anchor layer is preferably 10 nm or more, more preferably 20 nm or more, and even more preferably 50 nm or more. The thickness of the anchor layer is preferably 1000 nm or less, more preferably 500 nm or less, and even more preferably 400 nm or less. As will be described later, when the anchor layer is a multilayer structure consisting of two or more layers, it is preferable that the thickness of each anchor layer is within the above range. The thickness of the anchor layer can be determined by observing the cross section with a scanning electron microscope (SEM), measuring the thickness at any five or more points, and averaging the measurements.
[0048] In this embodiment, the anchor layer may have a single-layer structure, or may have a multilayer structure consisting of two or more layers. For example, as shown in FIG. 2, the ethylene adsorption film of this embodiment may include two anchor layers. The ethylene adsorption film of FIG. 2 includes, in this order, a substrate layer 2, a first anchor layer 4', a second anchor layer 4, and a porous metal complex layer 6. In this case, the first anchor layer 4' is preferably provided to enhance adhesion between the substrate layer 2 and the second anchor layer 4, and the first anchor layer 4' preferably functions as an adhesive layer.
[0049] As shown in Figure 2, when two anchor layers are provided in the ethylene adsorption film, the first anchor layer preferably functions as an adhesive layer, and the second anchor layer preferably contains a polar group-containing polymer or an organic onium compound as described above. In this case, the first anchor layer preferably contains an adhesive resin. Examples of adhesive resins include polyolefins such as polyethylene, polyethyleneimine, polypropylene, and ethylene-propylene copolymers, polyesters, polyamides, ionomers, ethylene-vinyl acetate copolymers, acrylic resins such as acrylates and methacrylates, polyvinyl acetal, phenolic resins, modified epoxy resins, and copolymers or mixtures thereof. Among these, the adhesive resin is preferably at least one selected from the group consisting of polyethyleneimine, polyvinyl acetal, and modified epoxy resins.
[0050] The adhesive resin may be a thermoplastic elastomer, such as a styrene-based elastomer, an olefin-based elastomer, a urethane-based elastomer, a polyester-based elastomer, a nitrile-based elastomer, an amide-based elastomer, a polybutadiene-based elastomer, an acrylic-based elastomer, or a vinyl chloride-based thermoplastic elastomer.
[0051] The anchor layer may further contain a silane coupling agent, such as those having an epoxy group such as 3-glycidoxypropyltrimethoxysilane, those having an amino group such as 3-aminopropyltrimethoxysilane, those having a mercapto group such as 3-mercaptopropyltrimethoxysilane, and those having an isocyanate group such as 3-isocyanatepropyltriethoxysilane.
[0052] Furthermore, the anchor layer may contain various additives, such as antibacterial agents, antioxidants, ultraviolet absorbers, near-infrared absorbers, lubricants, and antistatic agents.
[0053] (base material layer) The ethylene-adsorbent film has a substrate layer. The type of substrate layer is not particularly limited, and examples thereof include a layer formed from a synthetic polymer, a woven fabric, a nonwoven fabric, metal foil, paper, cellophane, glass, and the like. The type of substrate layer is appropriately selected depending on the application of the ethylene-adsorbent film. For example, when the ethylene-adsorbent film is used as a packaging material for fruits and vegetables, the substrate layer preferably has a certain degree of flexibility, and a resin layer is preferably used. Furthermore, when the ethylene-adsorbent film is required to have light-blocking properties, it is possible to use a metal foil as the substrate layer.
[0054] When the substrate layer is a resin layer, examples of the resin constituting the resin layer include polyolefins (e.g., polyethylene, polypropylene), polyesters (e.g., polyethylene terephthalate, polybutylene terephthalate, polylactic acid), polyamides (e.g., nylon 6, nylon 66, nylon 610), polyvinyl chloride, polyvinylidene chloride, fluororesins, epoxy resins, acrylic resins, polyurethanes, silicone resins, phenolic resins, polyetherimides, polyimides, polyvinyl alcohol, polystyrene, cellulose-based resins, polycarbonates, etc. From the viewpoint of environmental conservation, it is also preferable to construct the substrate layer from a biodegradable resin or a biomass resin.
[0055] When the substrate layer is a resin layer, the resin layer may be a transparent resin layer, a semi-transparent resin layer, or an opaque resin layer. The resin layer may also be a foamable resin layer. Furthermore, the resin layer may be printed.
[0056] The substrate layer may be subjected to a surface treatment. Examples of the surface treatment include corona treatment, flame treatment, and plasma treatment. By subjecting the substrate layer to a surface treatment, the interlayer adhesion between the substrate layer and the anchor layer can be more effectively improved.
[0057] The thickness of the substrate layer is not particularly limited, but is preferably 5 μm or more, more preferably 10 μm or more. The thickness of the substrate layer is preferably 1000 μm or less, more preferably 900 μm or less, and even more preferably 800 μm or less. By setting the thickness of the substrate layer within the above range, the strength of the ethylene adsorption film can be increased and film formability can be improved. The substrate layer may have a single-layer structure or a multilayer structure having multiple layers. In the case of a multilayer structure, it is preferable that the thickness of each layer be within the above range.
[0058] The substrate layer may contain various additives. Examples of additives include antibacterial agents, antioxidants, ultraviolet absorbers, near-infrared absorbers, lubricants, antistatic agents, foaming agents, plasticizers, colorants, pH adjusters, opacifying agents, oils, flame retardants, near-infrared absorbers, and color correctors. The substrate layer may also contain zeolite or activated carbon as an ethylene adsorbent.
[0059] (arbitrary layer) The ethylene adsorption film may have other optional layers in addition to the porous metal complex layer, anchor layer, and substrate layer. Examples of such optional layers include a barrier layer for preventing the intrusion of water vapor, oxygen, light, etc. The barrier layer may be formed from a metal foil, a metal vapor-deposited film, an inorganic oxide vapor-deposited film, a carbon-containing inorganic oxide vapor-deposited film, or a film having any of these vapor-deposited films.
[0060] The ethylene-adsorbent film may also include a printed layer as an optional layer. The printed layer may be provided as the outermost layer of the substrate layer or between the substrate layer and the anchor layer. The printed layer may display a pattern such as letters or a design. The printed layer may contain, for example, a urethane-based, acrylic-based, nitrocellulose-based, rubber-based, or vinyl chloride-based ink binder resin, and various additives such as pigments, plasticizers, desiccants, and stabilizers. The printed layer may be formed by, for example, known printing methods such as offset printing, gravure printing, and silk screen printing, or known coating methods such as roll coating, knife-edge coating, and gravure coating.
[0061] (Method of manufacturing ethylene adsorption film) This embodiment relates to a method for producing an ethylene adsorption film, which includes the steps of forming an anchor layer containing a polar group-containing polymer or an organic onium compound on a substrate layer, and applying a solution of a metal hydroxide dispersed on the anchor layer to convert the metal hydroxide into a porous metal complex to form a porous metal complex layer. Thus, in this embodiment, the porous metal complex layer is preferably a layer formed by converting a metal hydroxide into a porous metal complex.
[0062] The step of forming an anchor layer containing a polar group-containing polymer or an organic onium compound on a substrate layer preferably includes a step of applying an anchor layer-forming composition to the substrate layer. The anchor layer-forming composition preferably contains a polar group-containing polymer or an organic onium compound and a solvent to enhance coatability. The anchor layer-forming composition can be applied by any known coating method, including, for example, dip coating, dipping, roll coating, gravure coating, reverse coating, air knife coating, comma coating, die coating, screen printing, spray coating, and gravure offset.
[0063] A drying step is preferably carried out after the step of applying the anchor layer-forming composition onto the base layer. Drying methods that can be used include, for example, hot air drying, heat roll drying, high-frequency irradiation, infrared irradiation, and UV irradiation. When a heat drying method is employed in the drying step, the heating temperature is not particularly limited, but it is preferable to dry at, for example, 60 to 140°C.
[0064] Before the step of applying the anchor layer-forming composition onto the substrate layer, a step of surface-treating the substrate layer may be performed. Examples of surface treatment methods include corona treatment, flame treatment, and plasma treatment. By performing a surface treatment on the substrate layer, the interlayer adhesion between the substrate layer and the anchor layer can be more effectively improved.
[0065] After the anchor layer is formed on the substrate layer, a step of coating the anchor layer with a solution of dispersed metal hydroxide and converting the metal hydroxide into a porous metal complex to form a porous metal complex layer is preferably carried out. In this step, the anchor layer is first coated with a solution of dispersed metal hydroxide to form a coating film of metal hydroxide on the anchor layer. The metal constituting the metal hydroxide is preferably at least one selected from the group consisting of titanium, manganese, iron, cobalt, nickel, copper, zinc, silver, aluminum, zirconium, magnesium, calcium, vanadium, cadmium, and palladium.
[0066] The solution in which the metal hydroxide is dispersed preferably contains a solvent. The solvent may be an organic solvent, water, or a mixture thereof. Specifically, methanol, ethanol, propanol, diethyl ether, dimethoxyethane, tetrahydrofuran, hexane, cyclohexane, heptane, benzene, toluene, methylene chloride, chloroform, acetone, ethyl acetate, acetonitrile, N,N-dimethylformamide, water, or a mixture thereof.
[0067] The step of forming the porous metal complex layer preferably includes the steps of applying a solution in which a metal hydroxide is dispersed onto an anchor layer to form a coating film, and immersing the coating film in a solution containing an organic ligand to form the porous metal complex layer. The coating film containing metal hydroxide is a film containing metal hydroxide nanostructures (metal hydroxide nanobelts), and by immersing such a coating film in a solution containing an organic ligand, the metal hydroxide nanostructures (metal hydroxide nanobelts) are converted into a porous metal complex layer.
[0068] Examples of the organic ligand include the organic ligands described above. The solution containing the organic ligand preferably contains a solvent. The solvent may be any of the solvents described above. The solution containing the organic ligand may be water, alcohol, or a solvent containing these. Such solvents have low toxicity, and therefore the burden on the environment can be reduced.
[0069] From the viewpoint of facilitating the formation of a porous metal complex, the concentration of the organic ligand in the solution containing the organic ligand is preferably 0.01% by mass or more, more preferably 0.02% by mass or more, and even more preferably 0.05% by mass or more. On the other hand, from the viewpoint of the solubility of the organic ligand and the formation of a porous metal complex uniformly throughout the membrane, the concentration of the organic ligand in the solution containing the organic ligand is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 1% by mass or less.
[0070] When a coating containing copper hydroxide nanostructures is immersed in a solution containing 1,3,5-benzenetricarboxylic acid (HBTC) as an organic ligand, the following reaction occurs, forming a porous metal complex (Cu(BTC)). 3Cu(OH)2+2H3BTC→Cu3(BTC)2+6H2O When the porous metal complex (Cu3(BTC)2) is formed, Cu ions are eluted from the copper hydroxide nanostructure and form coordinate bonds with the ligands to form the porous metal complex. In this embodiment, the porous metal complex layer is formed on the anchor layer, and it is thought that the high surface free energy of the anchor layer allows the formed porous metal complex to be well adsorbed to the anchor layer.
[0071] The time for immersing the coating film containing a metal hydroxide in the solution containing an organic ligand is, for example, preferably 1 minute or more, more preferably 5 minutes or more, and even more preferably 10 minutes or more. The immersion time is preferably 100 hours or less. The immersion temperature is not particularly limited, and is preferably, for example, 10 to 50°C. In this embodiment, the immersion treatment can be carried out at a general temperature, such as room temperature.
[0072] In the method for producing an ethylene adsorption film of this embodiment, the step of immersing the coating film containing a metal hydroxide in a solution containing an organic ligand may be performed multiple times. That is, the method for producing an ethylene adsorption film of this embodiment may include the steps of forming an anchor layer containing a polar group-containing polymer or an organic onium compound on a substrate layer, applying a solution in which a metal hydroxide is dispersed on the anchor layer and converting the metal hydroxide into a porous metal complex to form a porous metal complex layer, and applying a solution in which a metal hydroxide is further dispersed on the formed porous metal complex layer and converting the metal hydroxide into a porous metal complex to form a porous metal complex layer. By performing the step of immersing the coating film containing a metal hydroxide in a solution containing an organic ligand multiple times, it is possible to increase the thickness of the porous metal complex layer.
[0073] In addition, in the method for producing an ethylene adsorption film of this embodiment, instead of the step of immersing the coating film containing a metal hydroxide in the solution containing an organic ligand, a step of applying a solution containing an organic ligand to the coating film containing a metal hydroxide may be provided.
[0074] (Application) The ethylene-adsorbent film of this embodiment exhibits excellent ethylene adsorption capacity and can therefore be used, for example, for packaging fruits and vegetables. By using the ethylene-adsorbent film of this embodiment for packaging fruits and vegetables, the progress of ripening and aging of fruits and vegetables due to the action of ethylene produced in the fruits and vegetables can be suppressed. For this reason, the ethylene-adsorbent film of this embodiment can also be called a freshness-keeping film.
[0075] When the ethylene-adsorbent film of the present embodiment is used for packaging fruits and vegetables, its shape is not particularly limited, and may be, for example, a sheet, a bag, or a box.
[0076] Furthermore, the ethylene adsorption film of the present embodiment may be a film-like ethylene adsorbent instead of a packaging material. For example, by enclosing a film-like ethylene adsorbent together with fruits and vegetables inside a package, ethylene can be adsorbed and removed.
[0077] Incidentally, this embodiment may relate to an ethylene adsorption method or an ethylene removal method using this ethylene adsorption film. Further, this embodiment may relate to the use of this ethylene adsorption film for removing ethylene.
Examples
[0078] The features of the present invention will be described more specifically below by giving examples and comparative examples. The materials, amounts used, ratios, treatment details, treatment procedures, etc. shown in the following examples can be appropriately changed as long as they do not depart from the gist of the present invention. Therefore, the scope of the present invention should not be construed as being limited by the specific examples shown below.
[0079] <Thickness of MOF layer> The cross-section of the porous metal complex layer was observed with a scanning electron microscope (SEM), and the thicknesses at any five or more points were measured, and the average value thereof was obtained.
[0080] <Water contact angle> The water contact angle of the anchor layer surface was measured using a contact angle meter (Drop Master 500 manufactured by Kyowa Chemical Industry Co., Ltd.). The measurement was performed under an environment of 23°C and a relative humidity of 50%. The volume of the water droplet was 10 μL, the measurement was started 1 second after the water droplet was dropped, and the measured value 1 second after the start of the measurement was taken as the water contact angle.
[0081] <Surface roughness Sa> The arithmetic mean height Sa (ISO 25178) of the anchor layer surface was measured using an atomic force microscope ("SPI4000" manufactured by Hitachi High-Technologies Corporation). In Comparative Examples 1 and 2, since the anchor layer was not provided, the arithmetic mean height Sa of the base material layer surface was measured.
[0082] <Total light transmittance · haze> In accordance with JIS K 7136:2000, the total light transmittance and haze of the ethylene adsorption film were measured using a haze meter "HM-150" manufactured by Murakami Color Research Laboratory.
[0083] <Peel test> An adhesive tape (Nichiban Co., Ltd.'s "Cellotape (registered trademark)") was applied to the porous metal complex layer (MOF layer) surface of the ethylene adsorption film, and the adhesiveness of the adhesive tape after peeling was confirmed and evaluated according to the following criteria. A: The adhesiveness is maintained after peeling, i.e., the MOF layer is not attached to the adhesive tape. B: The adhesiveness is reduced after peeling, i.e., the MOF layer is attached to the adhesive tape.
[0084] <Amount of ethylene adsorbed> The ethylene adsorption film was cut into a 5 cm x 9 cm rectangle and placed in a 500 mL glass bottle and sealed. Standard ethylene gas was then injected into the bottle so that the ethylene gas concentration in the bottle was 100 ppm. Immediately, 1 mL of gas was sampled from the bottle and the ethylene concentration was measured using a gas chromatograph (Shimadzu Corporation, GC-2014). After 1 hour, 1 mL of gas was sampled again from the glass bottle and the ethylene concentration was measured. The amount of ethylene adsorbed by the ethylene adsorption film was calculated from the difference. The amount of ethylene leaked from the glass bottle within 1 hour was also determined by performing the same measurement without the ethylene adsorption film, and this was subtracted from the amount of ethylene adsorbed by the ethylene adsorption film.
[0085] Example 1 <Preparation of Polar Group-Containing Polymer Solution (B-1)> 0.15 g of acetoacetyl group-modified PVA (Z-100, manufactured by Mitsubishi Chemical Corporation), 0.23 g of silica particles (Mizupearl K500L, average particle size 4.6 μm, manufactured by Mizusawa Industrial Chemicals Co., Ltd.), and 0.01 g of a crosslinker (Safelink SPM-01, manufactured by Mitsubishi Chemical Corporation) were dissolved in water to a concentration of 4% by mass.
[0086] <Preparation of copper hydroxide dispersion solution (copper hydroxide nanobelt solution)> 0.202 g of CuSO4·5H2O (manufactured by Fujifilm Wako Pure Chemical Corporation) was dissolved in 20 mL of H2O. 6 mL of 28% aqueous ammonia solution (manufactured by Fujifilm Wako Pure Chemical Corporation) was added to the solution, and the mixture was stirred for 5 minutes. Then, 1.2 mL of 12 M NaOH aqueous solution was added. After stirring at room temperature for 1 hour, the solution was allowed to stand at 40 °C for 30 minutes to obtain a solid product. The solid product was washed with ion-exchanged water and ethanol (manufactured by Fujifilm Wako Pure Chemical Corporation), and then dispersed in 10 mL of ethanol to obtain a copper hydroxide nanobelt solution.
[0087] <Preparation of H3BTC Solution> 0.1 g of 1,3,5-benzenetricarboxylic acid (H3BTC) (manufactured by Fujifilm Wako Pure Chemical Corporation) was dissolved in a mixed solution (100 mL) of ethanol and water prepared at a volume ratio of 5:2.
[0088] <Preparation of Ethylene Adsorption Film> As the base layer, a polycarbonate sheet (FE-2000, manufactured by Mitsubishi Gas Chemical Company) was used. The surface of this polycarbonate sheet was corona-treated under the output condition: 100 W·min / m 2 Then, a coating solution obtained by diluting polyethyleneimine with ethanol to 2.5% by mass was bar-coated on the corona-treated surface and heated for drying (the first anchor layer). Next, a polar group-containing polymer solution (B-1) was bar-coated on the first anchor layer and heated for drying (the second anchor layer). Next, a copper hydroxide dispersion solution (copper hydroxide nanobelt solution) was bar-coated on the second anchor layer and dried at room temperature to form a copper hydroxide nanobelt layer. The obtained laminate was immersed in the H3BTC solution for 2 hours to convert the copper hydroxide nanobelt layer into a porous metal complex layer (MOF layer). In this way, an ethylene adsorption film was obtained.
[0089] (Example 2) An ethylene adsorption film was obtained in the same manner as in Example 1, except that the formation process of the porous metal complex layer (MOF layer) was repeated three times.
[0090] (Example 3) <Preparation of Polar Group-Containing Polymer Solution (B-2)> 0.15 g of acetoacetyl group-modified PVA (Z-100, manufactured by Mitsubishi Chemical Corporation), 0.23 g of silica particles (Sylysia 730, manufactured by Fuji Silysia Chemical Ltd., average particle size 4.0 μm), and 0.01 g of a crosslinker (Safelink SPM-01, manufactured by Mitsubishi Chemical Corporation) were dissolved in water to a concentration of 4% by mass.
[0091] <Preparation of ethylene adsorption film> An ethylene-adsorbed film was obtained in the same manner as in Example 1, except that the polar group-containing polymer solution (B-2) was used for bar coating instead of the polar group-containing polymer solution (B-1) in Example 1.
[0092] Example 4 An ethylene-adsorbed film was obtained in the same manner as in Example 3, except that the step of forming a porous metal complex layer (MOF layer) was repeated three times.
[0093] Example 5 <Preparation of Polar Group-Containing Polymer Solution (B-3)> <Preparation of Polar Group-Containing Polymer Solution (B-2)> 0.15 g of acetoacetyl group-modified PVA (Z-100, manufactured by Mitsubishi Chemical Corporation) and 0.01 g of a crosslinking agent (Safelink SPM-01, manufactured by Mitsubishi Chemical Corporation) were dissolved in water to a concentration of 4% by mass.
[0094] <Preparation of ethylene adsorption film> An ethylene-adsorbed film was obtained in the same manner as in Example 1, except that the polar group-containing polymer solution (B-3) was used for bar coating instead of the polar group-containing polymer solution (B-1) in Example 1.
[0095] (Comparative Example 1) A polycarbonate sheet (FE-2000 manufactured by Mitsubishi Gas Chemical Company, Inc.) was used as the substrate layer. The surface of this polycarbonate sheet was heated at an output of 100 W min / m. 2It was corona-treated and a copper hydroxide dispersion solution (copper hydroxide nanobelt solution) was bar-coated on the surface subjected to the corona treatment, followed by drying at room temperature to form a copper hydroxide nanobelt layer. The obtained laminate was immersed in an H3BTC solution for 2 hours to convert the copper hydroxide nanobelt layer into a porous metal complex layer (MOF layer).
[0096] (Comparative Example 2) (Synthesis of HKUST-1 powder) 10 mL of water and 1 g of H3BTC were added to 25 mL of an ethanol dispersion of copper hydroxide nanobelts, and the mixture was stirred at room temperature for 14 hours. Subsequently, the solid product was collected by a centrifuge. At that time, the solid product was washed with ethanol.
[0097] (Preparation of porous metal complex-resin mixture) 0.45 g of PMMA (manufactured by Mitsubishi Chemical Corporation, BR-80) was dissolved in 9 g of PGM, and 0.45 g of HKUST-1 powder was mixed to prepare a porous metal complex-resin mixture.
[0098] (Preparation of ethylene adsorption film) As a base material layer, a polycarbonate sheet (FE-2000 manufactured by Mitsubishi Gas Chemical Company) was used. The surface of this polycarbonate sheet was corona-treated under the output condition: 100 W·min / m 2 and a porous metal complex-resin mixture was bar-coated on the surface subjected to the corona treatment, followed by heating and drying (porous metal complex-resin mixed layer (A-2)).
[0099] (Comparative Example 3) (Preparation of ethylene adsorption film) As a base material layer, a polycarbonate sheet (FE-2000 manufactured by Mitsubishi Gas Chemical Company) was used. The surface of this polycarbonate sheet was corona-treated under the output condition: 100 W·min / m 2The surface was subjected to a corona treatment with ethanol, and a coating liquid prepared by diluting polyethyleneimine with ethanol to 2.5% by mass was bar-coated onto the corona-treated surface and dried by heating (first anchor layer). Next, a polar group-containing polymer solution (B-2) was bar-coated onto the first anchor layer and dried by heating (second anchor layer). The porous metal complex-resin mixed solution obtained in Comparative Example 2 was bar-coated onto the second anchor layer and dried by heating (porous metal complex-resin mixed layer (A-2)).
[0100] [Table 1]
[0101] Compared with the comparative examples, the examples exhibited superior ethylene adsorption capacity and superior interlayer adhesion. [Explanation of symbols]
[0102] 2 Base material layer 4 Anchor layer (second anchor layer) 4' Anchor layer (first anchor layer) 6. Porous metal complex layer 10 Ethylene adsorption film
Claims
1. An ethylene-adsorbed film comprising a substrate layer, an anchor layer containing a polar group-containing polymer or an organic onium compound, and a porous metal complex layer.
2. The porous metal complex layer is 2. The ethylene adsorption film according to claim 1, comprising a porous metal complex comprising at least one metal selected from the group consisting of titanium, manganese, iron, cobalt, nickel, copper, zinc, silver, aluminum, zirconium, magnesium, calcium, vanadium, cadmium, and palladium bound to an organic ligand.
3. 3. The ethylene-adsorbed film according to claim 2, wherein the organic ligand has at least one functional group selected from the group consisting of a carboxy group, a hydroxy group, an amino group, and a sulfonic acid group.
4. 3. The ethylene-adsorbed film according to claim 2, wherein the organic ligand is at least one selected from the group consisting of 1,3,5-benzenetricarboxylic acid, 1,4-benzenedicarboxylic acid, and 2,5-dihydroxyterephthalic acid.
5. The ethylene adsorption film according to claim 1, wherein the porous metal complex layer has a thickness of 0.1 to 10 μm.
6. 2. The ethylene adsorption film according to claim 1, wherein the arithmetic mean height Sa of the anchor layer is 0.1 to 20 μm.
7. The ethylene adsorption film according to claim 1 , wherein the anchor layer has a water contact angle of 50° or less.
8. The ethylene adsorption film according to claim 1, wherein the polar group-containing polymer is at least one selected from the group consisting of polyvinyl alcohol, polyvinylpyrrolidone, polyethyleneimine, polyacrylic acid, sodium polyacrylate, poly(4-styrenesulfonic acid), poly(sodium 4-styrenesulfonate), and polyallylamine hydrochloride.
9. The ethylene adsorption film according to claim 1 , wherein the anchor layer comprises at least one selected from organic particles and inorganic particles.
10. The ethylene adsorption film according to claim 9, wherein the organic particles and the inorganic particles each have an average particle size of 0.1 to 20 μm.
11. The ethylene adsorption film according to claim 1 , wherein the anchor layer comprises two or more layers.
12. The ethylene-adsorbed film according to claim 1, which is used for packaging fruits and vegetables.
13. A roll obtained by rolling up the ethylene adsorption film according to any one of claims 1 to 12.
14. forming an anchor layer containing a polar group-containing polymer or an organic onium compound on a substrate layer; applying a solution having a metal hydroxide dispersed therein onto the anchor layer, and converting the metal hydroxide into a porous metal complex to form a porous metal complex layer.
15. The step of forming a porous metal complex layer includes: The method for producing an ethylene adsorption film according to claim 14, comprising the steps of: applying a solution in which a metal hydroxide is dispersed onto the anchor layer to form a coating film; and immersing the coating film in a solution containing an organic ligand to form a porous metal complex layer.
16. The method for producing an ethylene adsorption film according to claim 14, wherein the metal constituting the metal hydroxide is at least one selected from the group consisting of titanium, manganese, iron, cobalt, nickel, copper, zinc, silver, aluminum, zirconium, magnesium, calcium, vanadium, cadmium, and palladium.
17. The method for producing an ethylene-adsorbed film according to claim 15, wherein the organic ligand is at least one selected from the group consisting of 1,3,5-benzenetricarboxylic acid, 1,4-benzenedicarboxylic acid, and 2,5-dihydroxyterephthalic acid.
18. The method for producing an ethylene adsorption film according to claim 14, wherein the polar group-containing polymer is at least one selected from the group consisting of polyvinyl alcohol, polyvinylpyrrolidone, polyethyleneimine, polyacrylic acid, sodium polyacrylate, poly(4-styrenesulfonic acid), poly(sodium 4-styrenesulfonate) and polyallylamine hydrochloride.
Citation Information
Patent Citations
Ethylene gas adsorbent, production method therefor, and freshness-maintaining method for fresh goods using the adsorbent
JP2004322005A
Composition of freshness maintenance material, freshness maintenance material having composition, material for packaging or the like, coating material, coating device of coating material, and manufacturing method of material for packaging or the like
JP2019170368A
Ethylene gas adsorbent
JP2022001357A
Adsorption sheet and adsorption element used for same
WO2013115033A1
Functional film, functional container, and method for retaining freshness
WO2017135433A1
Cited By
Metal-organic framework for ethylene gas adsorption and its manufacturing method
KR102976363B1