Manufacturing method negative electrode active material, and manufacturing method of lithium-ion battery

By pre-doping porous silicon clathrate with Li ions using a lithium-containing non-aqueous electrolyte and solvent removal, the method stabilizes the surface, addressing irreversible capacity and handling issues in silicon-based negative electrode active materials, enhancing lithium ion battery energy density.

JP2024155061AActive Publication Date: 2024-10-31TOYOTA JIDOSHA KK

Patent Information

Application Number
JP2023069455
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-20
Publication Date
2024-10-31
Estimated Expiration
2043-04-20

AI Technical Summary

Technical Problem

The irreversible capacity in lithium ion batteries limits their energy density, and pre-doping Li ions into silicon-based negative electrode active materials can lead to heat generation and handling issues.

Method used

A method involving porous silicon clathrate pre-doping with Li ions using a lithium-containing non-aqueous electrolyte, followed by solvent removal, to stabilize the surface with a lithium silicon oxide film, enhancing handling properties.

Benefits of technology

The method produces a stable, easily handled negative electrode active material for lithium ion batteries, improving energy density by minimizing irreversible capacity and handling challenges.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155061000001
    Figure 2024155061000001
Patent Text Reader

Abstract

To provide a manufacturing method of a negative electrode active material easy to handle, and a manufacturing method of a lithium-ion battery including the manufacture of such a negative electrode active material.SOLUTION: A disclosed method of manufacturing a negative electrode active material includes: causing porous silicon clathrate to contact with a lithium-containing non-aqueous electrolyte; and drying and removing a solvent of the lithium-containing non-aqueous electrolyte. A disclosed method of manufacturing a lithium-ion battery includes: preparing a negative electrode active material by using the disclosed method; and forming a negative electrode active material layer containing the negative electrode active material.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a method for manufacturing a negative electrode active material and a method for manufacturing a lithium ion battery.

Background Art

[0002] In recent years, battery development has been actively carried out. For example, in the automotive industry, the development of batteries used in electric vehicles or hybrid vehicles has been promoted. Further, silicon (Si) is known as a negative electrode active material used in batteries, particularly lithium ion batteries.

[0003] For example, Patent Document 1 discloses a silicon clathrate negative electrode active material having a silicon clathrate II-type crystal phase, having voids inside primary particles, and having a void volume of voids with a pore diameter of 100 nm or less of 0.05 cc / g or more and 0.15 cc / g or less. Patent Document 2 discloses a silicon clathrate negative electrode active material having a silicon clathrate II-type crystal phase and having a composition of Na x Si 136 (1.98 < x < 2.54).

Prior Art Documents

Patent Documents

[0004]

Patent Document 1

Patent Document 2

Summary of the Invention

Problems to be Solved by the Invention

[0005] Meanwhile, there is a demand for improving the energy density of lithium-ion batteries. One of the factors preventing the improvement of energy density is irreversible capacity. Irreversible capacity comes from the Li ions that are supplied from the positive electrode to the negative electrode during the first charge and cannot be used thereafter. The higher the capacity of the negative electrode active material, such as Si, the larger the irreversible capacity tends to be. The existence of irreversible capacity limits the effective charge / discharge capacity of the battery.

[0006] A method of supplying Li ions to Si in an amount equivalent to the irreversible capacity before the completion of the battery (called "pre-doping") has been considered. For example, Li ions can be supplied to Si by adhering Li metal (Li foil, etc.) to the surface of Si and leaving it. However, this method can cause the obtained negative electrode active material to generate heat and change in appearance, so there is a demand for improving the handleability of Si pre-doped with Li ions.

[0007] An object of the present disclosure is to provide a method for producing a negative electrode active material that is easy to handle, and a method for producing a lithium ion battery that includes producing such a negative electrode active material. [Means for solving the problem]

[0008] The present inventors have found that the above problems can be solved by the following means. <Aspect 1> contacting the porous silicon clathrate with a lithium-containing non-aqueous electrolyte; and Drying and removing the solvent from the lithium-containing nonaqueous electrolyte solution. A method for producing a negative electrode active material. <Aspect 2> 2. The method of embodiment 1, wherein the solvent is an aprotic polar solvent. <Aspect 3> The method of embodiment 2, wherein the aprotic polar solvent is an ether. <Aspect 4> The method according to aspect 3, wherein the ether has a tetrahydrofuran skeleton. <Aspect 5> The method according to any one of aspects 1 to 4, wherein the negative electrode active material is for use as a negative electrode active material in a lithium ion battery. <Aspect 6> Producing a negative electrode active material by the method according to any one of aspects 1 to 5; and forming a negative electrode active material layer containing the negative electrode active material; A method for producing a lithium ion battery, comprising: Effect of the Invention

[0009] According to the present disclosure, it is possible to provide a method for producing a negative electrode active material that is easy to handle, and a method for producing a lithium ion battery that includes producing such a negative electrode active material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, embodiments of the present disclosure will be described in detail. Note that the present disclosure is not limited to the following embodiments, and various modifications can be made within the scope of the present disclosure.

[0011] <<Method for producing negative electrode active material>> The disclosed method for producing a negative electrode active material includes contacting a porous silicon clathrate with a lithium-containing non-aqueous electrolyte solution, and drying off the solvent from the lithium-containing non-aqueous electrolyte solution.

[0012] The present inventors have found that the handling of the negative electrode active material pre-doped with Li ions is improved by using porous silicon clathrate as Si and pre-doping the porous silicon clathrate with Li ions by liquid phase synthesis. The reason for this is presumed to be as follows, without intending to be bound by any theory. That is, when Li ions are pre-doped by liquid phase synthesis, Si and Li react to self-generate a surface coating of lithium silicon oxide that is stable in air. In addition, since the porous silicon clathrate has a larger surface area than normal Si, the stabilizing effect of the surface coating is large, which is thought to improve the handling.

[0013] <Contact process> The disclosed method of making an active negative electrode material includes contacting a porous silicon clathrate with a lithium-containing non-aqueous electrolyte.

[0014] An example of a method for contacting the porous silicon clathrate with the lithium-containing non-aqueous electrolyte solution is a method in which the porous silicon clathrate is added to the lithium-containing non-aqueous electrolyte solution and mixed, but the method is not limited to this.

[0015] (Porous silicon clathrate) In the method of the present disclosure, a porous silicon clathrate is used as Si. The porous silicon clathrate can be obtained, for example, by mixing Si and Li to obtain a lithium silicon alloy, and reacting the obtained lithium silicon alloy with ethanol.

[0016] (Lithium-containing non-aqueous electrolyte) The lithium-containing non-aqueous electrolyte in the method of the present disclosure may contain an aprotic polar solvent. The aprotic polar solvent is not ionized and does not react with Li ions, so it is preferable in that it can prevent the reduction of pre-doped Li ions.

[0017] As the aprotic polar solvent, carbonates, esters, ethers, nitriles, sulfones, lactones, etc. can be used. For example, ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), 1,2-dimethoxyethane, 1,2-diethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dioxane, 1,3-dioxolane, diethylene glycol, dimethyl ether, ethylene glycol, acetonitrile, propionitrile, nitromethane, N,N-dimethylformamide, dimethyl sulfoxide, sulfolane, γ-butyrolactone, etc. can be mentioned.

[0018] The lithium-containing non-aqueous electrolyte may contain a solvent other than the aprotic polar solvent. Such electrolyte may be exemplified by biphenyls. As an example of the biphenyls, 2-methylbiphenyl may be exemplified. By including biphenyls in the electrolyte, it is preferable that the overcharging of the battery is prevented.

[0019] The ratio of the aprotic polar solvent to the entire lithium-containing nonaqueous electrolyte solution may be 50% by volume or more, 60% by volume or more, 70% by volume or more, or 80% by volume or more.

[0020] <Drying process> The disclosed method for producing a negative electrode active material includes drying and removing the solvent from a lithium-containing nonaqueous electrolyte solution.

[0021] An example of a method for drying and removing the solvent of the lithium-containing nonaqueous electrolyte solution is a method for performing solid-liquid separation of Li ion-doped Si and the lithium-containing nonaqueous electrolyte solution, followed by drying, but is not limited thereto.

[0022] The method for solid-liquid separation may be, for example, suction filtration.

[0023] An example of a drying method is vacuum drying, etc. When vacuum drying is performed, the drying temperature may be 25° C. to 100° C., 35° C. to 90° C., or 45° C. to 80° C., and the drying time may be 0.5 hours or more, 1 hour or more, or 1.5 hours or more.

[0024] <Application> The negative electrode active material obtained by the method of the present disclosure can be used as a negative electrode active material for lithium ion batteries.

[0025] <<How lithium-ion batteries are manufactured>> The disclosed method of making a lithium ion battery includes making an active anode material and forming an active anode material layer that contains the active anode material.

[0026] For the method for producing the negative electrode active material, the above description regarding the method for producing the negative electrode active material of the present disclosure can be referred to.

[0027] The method for forming the negative electrode active material layer is not particularly limited, and a known method can be adopted. For example, a slurry containing the negative electrode active material can be applied to the negative electrode current collector and dried to obtain the negative electrode active material layer formed on the negative electrode current collector layer.

[0028] The method for forming the battery is not particularly limited, and a known method can be adopted. The method for manufacturing the battery in the present disclosure may include, in addition to producing the negative electrode active material and forming the negative electrode active material layer containing the negative electrode active material, arranging the negative electrode current collector layer, the negative electrode active material layer, the electrolyte layer, the positive electrode active material layer, and the positive electrode current collector layer in this order.

[0029] <Negative electrode current collector layer> Examples of materials for the negative electrode current collector include SUS, copper, nickel, and carbon.

[0030] <Negative electrode active material layer> The negative electrode active material layer contains at least a negative electrode active material.

[0031] (Negative electrode active material) For the negative electrode active material, reference can be made to the above description regarding the negative electrode active material of the present disclosure.

[0032] The ratio of the negative electrode active material in the negative electrode active material layer may be 20% by weight or more, 30% by weight or more, or 40% by weight or more. If the ratio of the negative electrode active material is too small, sufficient energy density may not be obtained. The ratio of the negative electrode active material may be 80% by weight or less, 70% by weight or less, or 60% by weight or less. If the ratio of the negative electrode active material is too high, the ionic conductivity and electronic conductivity in the negative electrode active material layer may be relatively reduced.

[0033] The negative electrode active material layer may contain at least one of an electrolyte, a conductive material, and a binder, as necessary.

[0034] (electrolyte) Examples of the solid electrolyte include inorganic solid electrolytes such as sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, and halide solid electrolytes, and organic polymer electrolytes such as polymer electrolytes.

[0035] Examples of the sulfide solid electrolyte include solid electrolytes containing Li, X (X is at least one of P, As, Sb, Si, Ge, Sn, B, Al, Ga, and In), and S. The sulfide solid electrolyte may further contain at least one of O and halogen. Examples of the halogen include F, Cl, Br, and I. The sulfide solid electrolyte may be glass (amorphous) or glass ceramics. Examples of the sulfide solid electrolyte include Li2S-P2S5, LiI-Li2S-P2S5, LiI-LiBr-Li2S-P2S5, Li2S-SiS2, Li2S-GeS2, and Li2S-P2S5-GeS2.

[0036] The electrolyte preferably contains a supporting salt and a solvent.

[0037] Examples of supporting salts (lithium salts) for electrolytes having lithium ion conductivity include inorganic lithium salts such as LiPF6, LiBF4, LiClO4, and LiAsF6, and organic lithium salts such as LiCF3SO3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(FSO2)2, and LiC(CF3SO2)3.

[0038] Examples of the solvent used in the electrolytic solution include cyclic esters (cyclic carbonates) such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC), and chain esters (chain carbonates) such as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC). The electrolytic solution preferably contains two or more kinds of solvents.

[0039] (Conductive material) Examples of the conductive material include carbon materials, metal particles, and conductive polymers.

[0040] Examples of carbon materials include particulate carbon materials such as acetylene black (AB) and ketjen black (KB), and fibrous carbon materials such as carbon fibers, carbon nanotubes (CNT), and carbon nanofibers (CNF).

[0041] (binder) Examples of the binder include rubber-based binders and fluoride-based binders.

[0042] The thickness of the negative electrode active material layer is, for example, 0.1 μm or more and 1000 μm or less.

[0043] <Electrolyte layer> The electrolyte layer contains at least an electrolyte. For the electrolyte, reference can be made to the above description regarding the negative electrode active material layer of the present disclosure.

[0044] The thickness of the electrolyte layer is, for example, not less than 0.1 μm and not more than 1000 μm.

[0045] <Cathode active material layer> The positive electrode active material layer contains at least a positive electrode active material and may contain at least one of an electrolyte, a conductive material, and a binder, as necessary.

[0046] Examples of the positive electrode active material include oxide active materials. Examples of the oxide active material include LiCoO2, LiMnO2, LiNiO2, LiVO2, and LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, etc., rock salt layered active materials, LiMn2O4, Li4Ti5O 12 , Li(Ni 0.5 Mn 1.5 )O4 and the like; and olivine type active materials such as LiFePO4, LiMnPO4, LiNiPO4, and LiCoPO4.

[0047] A coating layer containing a Li-ion conductive oxide may be formed on the surface of the oxide active material. This is because it can suppress the reaction between the oxide active material and a solid electrolyte (especially a sulfide solid electrolyte). An example of the Li-ion conductive oxide is LiNbO3. The thickness of the coating layer is, for example, 1 nm or more and 30 nm or less.

[0048] Also, for example, Li2S can be used as the positive electrode active material.

[0049] The shape of the positive electrode active material may be, for example, particulate. The average particle size (D50) of the positive electrode active material is not particularly limited, but may be, for example, 10 nm or more, and may be 100 nm or more. On the other hand, the average particle size (D50) of the positive electrode active material is, for example, 50 μm or less, and may be 20 μm or less. The average particle size (D50) can be calculated, for example, from measurements using a laser diffraction particle size distribution meter or a scanning electron microscope (SEM).

[0050] For the electrolyte, conductive material, and binder used in the positive electrode active material layer, the above descriptions regarding the negative electrode active material of the present disclosure can be referred to.

[0051] The thickness of the positive electrode active material layer is, for example, 0.1 μm or more and 1000 μm or less.

[0052] <Positive electrode current collector layer> Examples of materials for the positive electrode current collector include SUS, aluminum, nickel, iron, titanium, and carbon.

[0053] The lithium ion battery produced by the method of the present disclosure may be a liquid battery containing an electrolytic solution as an electrolyte layer, or may be a solid battery having a solid electrolyte layer as an electrolyte layer. In the present disclosure, a "solid-state battery" means a battery using at least a solid electrolyte as an electrolyte, and therefore a solid-state battery may use a combination of a solid electrolyte and a liquid electrolyte as an electrolyte. The solid-state battery of the present disclosure may also be an all-solid-state battery, i.e., a battery using only a solid electrolyte as an electrolyte.

[0054] The lithium ion battery produced by the method of the present disclosure may be a primary battery or a secondary battery.

[0055] Examples of the shape of the lithium ion battery include a coin type, a laminate type, a cylindrical type, and a square type. EXAMPLES

[0056] Synthesis of negative electrode active material The negative electrode active materials of the respective examples were obtained as follows.

[0057] Synthesis of Porous Silicon Example 1 1g of silicon (Si) (Kojundo Kagaku, particle size 5μm) and 1g of lithium (Li) metal (Honjo Metals) were mixed in an agate mortar under an argon atmosphere to obtain a lithium silicon (LiSi) precursor. In a glass reactor under an argon atmosphere, 1.0g of LiSi precursor and 200ml of 1,3,5-trimethylbenzene (Nacalai Tesque) as a dispersion solvent were mixed using an ultrasonic homogenizer (SMT, UH-50) to obtain a mixed solution. This mixed solution was cooled to 0°C, and 200ml of ethanol (Nacalai Tesque) as a solvent for extracting Li was dripped into it, and the mixture was reacted for 2 hours to obtain a reaction solution. 100ml of acetic acid (Nacalai Tesque) was dripped into this reaction solution, and the mixture was reacted for 1 hour. Then, the solid reactant and the liquid were separated by suction filtration. Furthermore, this reactant was vacuum dried at 120°C for 2 hours to obtain porous silicon.

[0058] Synthesis of Porous Silicon Clathrate 0.5 g of the obtained porous silicon and 0.5 g of sodium hydride (Wako Pure Chemical Industries, Ltd.) were mixed in an agate mortar under an argon atmosphere, placed in a tantalum crucible (Nilaco), and sealed in a stainless steel 304 airtight container. The airtight container was placed in an electric furnace and fired at 500°C for 40 hours to obtain a sodium silicon (NaSi) precursor. Under an argon atmosphere, the NaSi precursor was transferred to a stainless steel 304 vacuum container and vacuum fired at 400°C for 40 hours to obtain a porous silicon clathrate.

[0059] The porous silicon clathrate was doped with Li ions in the liquid phase by the following procedure. First, in a glass reactor under an argon atmosphere, 200 ml of 2-methyltetrahydrofuran (Tokyo Chemical Industry Co., Ltd.), 50 ml of 2-methylbiphenyl (Tokyo Chemical Industry Co., Ltd.), and 1 g of Li metal (Honjo Metals) were mixed to obtain a Li ion-doped solution. 1 g of the porous silicon clathrate was added to the Li ion-doped solution and stirred for 40 hours. Then, the solid reactant and the Li ion-doped solution were separated by suction filtration. Furthermore, the reactant was vacuum-dried at 60° C. for 2 hours to obtain the negative electrode active material of Example 1.

[0060] Comparative Example 1 The Si raw material in Example 1 (high purity chemical, particle size 5 μm) was used as the negative electrode active material in Comparative Example 1.

[0061] Comparative Example 2 In the doping of Li ions, the porous silicon clathrate was doped with Li ions in a solid phase by the following procedure: 1 g of porous silicon clathrate and 1 g of Li metal (Honjo Metals) were mixed in an agate mortar under an argon atmosphere to obtain a negative electrode active material of Comparative Example 2.

[0062] "evaluation" Handling test The negative electrode active material of each example was exposed to the air atmosphere to evaluate the handleability of the negative electrode active material. Regarding the handleability, those that did not generate heat or change in appearance when exposed to the air were marked with ◯, and those that generated heat or changed in appearance were marked with ×.

[0063] "result" The results are shown in Table 1.

[0064] [Table 1]

[0065] As shown in Table 1, the negative electrode active material of Example 1 in which the Si used was a porous silicon clathrate and Li ions were doped in a liquid phase was easy to handle.

Claims

1. contacting the porous silicon clathrate with a lithium-containing non-aqueous electrolyte; and Drying and removing the solvent from the lithium-containing nonaqueous electrolyte solution; A method for producing a negative electrode active material.

2. The method of claim 1 , wherein the solvent is a polar aprotic solvent.

3. The method of claim 2 , wherein the aprotic polar solvent is an ether.

4. The method according to claim 3 , wherein the ether has a tetrahydrofuran skeleton.

5. 10. The method of claim 1, wherein the negative electrode active material is for use as a negative electrode active material in a lithium ion battery.

6. Producing a negative electrode active material by the method according to any one of claims 1 to 5; and forming a negative electrode active material layer containing the negative electrode active material; A method for producing a lithium ion battery, comprising:

Citation Information

Patent Citations

  • Active material, negative electrode layer, battery and these manufacturing methods

    JP2021158003A

  • Method for manufacturing active material

    JP2021192365A

  • Porous silicon material, electricity storage device, and method for producing porous silicon material

    JP2022106635A

  • Method for manufacturing negative electrode active material

    JP2023043948A

  • Anode active substance and battery

    WO2023002756A1

Cited By

  • Method of manufacturing solid-state battery, and anode active material layer

    JP2024155024A

  • Method for manufacturing a solid-state battery, and negative electrode active material layer

    JP7856041B2