Carrier for electrophotographic image formation, two-component developer, image forming apparatus, process cartridge, and image forming method
By incorporating hydrophobized antimony-containing particles in the carrier coating layer, the carrier's durability and image stability are improved, addressing issues of adhesion and density fluctuations in electrophotographic image formation.
Patent Information
- Application Number
- JP2023069470
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-20
- Publication Date
- 2024-10-31
AI Technical Summary
Existing electrophotographic image forming carriers face challenges in maintaining durability and stability of image quality over time, particularly due to carrier adhesion and fluctuations in image density.
The use of antimony-containing particles subjected to hydrophobization treatment in the coating layer of the carrier, which improves dispersibility and reduces particle agglomeration, thereby stabilizing carrier resistance and preventing adhesion.
The solution enhances carrier durability and maintains consistent image density over a long period by reducing carrier adhesion and surface unevenness, ensuring high-quality image formation.
Smart Images

Figure 2024155069000010 
Figure 2024155069000011 
Figure 2024155069000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a carrier for electrophotographic image formation, a two-component developer, an image forming apparatus, a process cartridge, and an image forming method. [Background technology]
[0002] In recent years, electrophotographic image forming methods have come to require high image quality on a par with that of printed matter, and various improvements and developments have been made to meet this demand. Among these, the issue of high image quality stability over a long period of time has been an issue, and improvements have been made to toner, carrier, developing means, etc. High image quality stability can be achieved by lowering the resistance of the carrier, but as a side effect, carrier adhesion to solid printed areas becomes more likely to occur, and this is being addressed by adjusting the carrier and developing device.
[0003] Regarding carriers, a carrier that can ensure durability while maintaining image quality over time has been proposed, which is a carrier for electrostatic latent image developers that is composed of magnetic core particles and a resin layer covering the surface of the core particles, and contains conductive particles in the resin layer, the conductive particles being conductive particles formed by coating phosphorus-doped tin or tungsten-doped tin on a white inorganic pigment, and the ratio of phosphorus or tungsten doped to tin in the conductive material is 0.010 to 0.100 (see, for example, Patent Document 1).
[0004] Furthermore, in order to suppress an increase in fluidity even when the toner concentration in the developing means decreases, a carrier for developing electrostatic images has been proposed which includes, as carrier particles, single particles having a core material and a coating layer covering the core material, and associated particles in which two or more single particles are bound together via the coating layer, wherein the average particle size D1 of the single particles is smaller than the average particle size D2 of the associated particles, and the ratio of the particle number N2 of the associated particles to the sum of the particle number N1 of the single particles and the particle number N2 of the associated particles is 5% or more by number (see, for example, Patent Document 2). Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a carrier for electrophotographic image formation which is excellent in durability and capable of suppressing carrier adhesion and fluctuations in image density over a long period of time. [Means for solving the problem]
[0006] The above problems can be solved by the present invention having the configuration described below. 1. A carrier for electrophotographic image formation comprising core particles and a coating layer that coats the core particles, the coating layer containing antimony-containing particles that have been subjected to a hydrophobic treatment. Effect of the Invention
[0007] The present invention can provide a carrier for electrophotographic image formation which is excellent in durability and capable of suppressing fluctuations in image quality, such as carrier adhesion and image density, over a long period of time. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a schematic diagram showing an example of a cell for measuring volume resistivity. [Diagram 2] FIG. 2 is a schematic view showing an example of the process cartridge of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] In the prior art, various improvements to carriers for electrostatic latent image developers have been proposed, but they are still not fully satisfactory in terms of maintaining carrier adhesion and image density over a long period of time, and further improvements are desired.
[0010] As a result of extensive research, the present inventors have found that in a carrier for electrophotographic image formation comprising core particles and a coating layer covering the core particles, it is important to use antimony-containing particles that have been subjected to a hydrophobic treatment in the coating layer as conductive particles in order to suppress fluctuations in image quality, such as carrier adhesion and image density, over a long period of time.
[0011] The reason is as follows. By using antimony-containing particles, which have a high resistance adjustment capability to the carrier, as conductive particles, the resistance value of the carrier can be adjusted even if the amount of conductive particles used is reduced. Therefore, the amount of particles in the carrier coating layer can be reduced, the unevenness of the carrier surface is reduced, and wear of the coating layer due to collisions between carrier particles is suppressed. It is believed that this is why the carrier resistance is stable over a long period of time and carrier adhesion can be suppressed.
[0012] Furthermore, by subjecting the antimony-containing particles to hydrophobic treatment, the particles have better dispersibility and are less likely to aggregate in the coating layer than when the antimony-containing particles are not hydrophobic treated. As a result, the unevenness of the carrier surface is further reduced, and it is believed that wear of the coating layer due to collisions between carrier particles is suppressed.
[0013] In addition, antimony-containing particles have a bluish color, and when an electrophotographic image forming carrier using antimony-containing particles collides in a developing device, the antimony-containing particles break off and adhere to the toner, causing fluctuations in image density. Therefore, by using antimony-containing particles that have been subjected to hydrophobic treatment as in this case, the dispersibility of the particles is improved as described above, and the aggregation of the particles in the coating layer is suppressed, so that the particles are less likely to break off when the carrier collides, and as a result, it is believed that the image density is stabilized.
[0014] <Antimony-containing particles> Examples of antimony-containing particles include diantimony pentoxide particles, tin oxide particles doped with an antimony compound, and particles in which tin oxide particles doped with an antimony compound are provided on the surface of a substrate made of inorganic particles. As the antimony-containing particles, it is preferable to use tin oxide particles doped with antimony and particles in which tin oxide particles doped with an antimony compound are provided on the surface of a substrate made of inorganic particles. As the antimony compound, diantimony pentoxide is preferable.
[0015] When inorganic particles are surface-coated with tin oxide doped with an antimony compound, even if the antimony-containing particles crumble and break into fragments within the coating layer, they will not be detached from the coating layer, thereby preventing a decrease in the electrical resistance of the carrier for electrophotographic image formation.
[0016] The method of surface coating is not particularly limited and can be appropriately selected depending on the purpose. For example, a hydrochloric acid solution of stannic chloride and antimony trichloride, and a sodium hydroxide solution are added in parallel to a suspension of a substrate powder in which alumina is dispersed, and the pH is adjusted. Thereafter, the resulting suspension is washed by decantation, filtered, dried, fired, and pulverized, thereby allowing the surface to be coated.
[0017] Examples of the surface treatment agent that can be used include amino-based silane coupling agents, methacryloxy-based silane coupling agents, vinyl-based silane coupling agents, mercapto-based silane coupling agents, alkyl-based silane coupling agents, and styryl-based silane coupling agents.
[0018] The inorganic particles serving as the base are not particularly limited and can be appropriately selected depending on the purpose. Examples of the inorganic particles include fine metal particles such as gold, silver, copper, silica, and aluminum, titanium oxide, tin oxide, zinc oxide, zirconium oxide, indium oxide, antimony oxide, calcium oxide, ITO, silicone oxide, colloidal silica, aluminum oxide, yttrium oxide, cobalt oxide, copper oxide, iron oxide, manganese oxide, niobium oxide, vanadium oxide, selenium oxide, barium sulfate, magnesium oxide, magnesium hydroxide, silicon dioxide, boron nitride, silicon nitride, potassium titanate, hydrotalcite, tin oxide doped with antimony or tungsten, and indium oxide doped with tin.
[0019] Among these, aluminum oxide and titanium oxide are preferred, and aluminum oxide is more preferred since it can provide better charging stability and can further prevent carrier adhesion.
[0020] The content of the antimony-containing particles is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 20 parts by mass to 60 parts by mass, more preferably 30 parts by mass to 50 parts by mass, relative to 100 parts by mass of the coating layer. When the content is 20 parts by mass to 60 parts by mass, it is possible to suppress the detachment of the antimony-containing particles and the exposure of fine particles due to the scraping of the coating layer, thereby preventing carrier adhesion.
[0021] <Core particles> The core particles are not particularly limited as long as they are magnetic, and examples thereof include ferromagnetic metals such as iron and cobalt, iron oxides such as magnetite, hematite, and ferrite, various alloys and compounds, and resin particles in which these magnetic materials are dispersed in resin. Among these, Mn-based ferrite, Mn-Mg-based ferrite, and Mn-Mg-Sr ferrite are preferred from the viewpoint of environmental friendliness.
[0022] The core material is not particularly limited as long as it is a magnetic material, and examples of the core material include ferromagnetic metals such as iron and cobalt, iron oxides such as magnetite, hematite, and ferrite, various alloys and compounds, and resin particles in which these magnetic materials are dispersed in resin. Among these, Mn-based ferrite, Mn-Mg-based ferrite, and Mn-Mg-Sr ferrite are preferred from the viewpoint of environmental friendliness.
[0023] <Coating layer> The coating layer contains a resin, and preferably contains fine particles, and further contains other components as required.
[0024] -resin- The resin may be a silicone resin, an acrylic resin, or a combination of these. A silicone resin or a combination of a silicone resin and an acrylic resin is preferred.
[0025] Acrylic resin has strong adhesion and low brittleness, giving it excellent abrasion resistance, but on the other hand, its surface energy is high, so when combined with a toner that is prone to spent, problems such as a decrease in charge due to the accumulation of spent toner components can occur. In such cases, this problem can be solved by using silicone resin in combination, which has a low surface energy that makes it difficult for toner components to be spent, and which has the effect of making it difficult for spent components to accumulate, which would cause the coating layer to be scraped off.
[0026] However, since silicone resin has poor adhesion and high brittleness, it also has the drawback of poor abrasion resistance, so it is important to obtain a good balance between the properties of these two types of resin, which makes it possible to obtain a coating layer that is resistant to spent and has abrasion resistance. This provides a significant improvement. This is because silicone resin has low surface energy, so toner components are less likely to be spent, and the accumulation of spent components that would cause the coating layer to be scraped off is less likely to progress.
[0027] Silicone resin refers to all commonly known silicone resins, including straight silicone consisting only of organosiloxane bonds, and silicone resins modified with alkyd, polyester, epoxy, acrylic, urethane, etc.
[0028] As the silicone resin, commercially available products can be used, and examples of commercially available straight silicone resins include KR271, KR255, and KR152 manufactured by Shin-Etsu Chemical Co., Ltd., and SR2400, SR2406, and SR2410 manufactured by Toray Dow Corning Silicone Co., Ltd. In this case, it is possible to use the silicone resin alone, but it is also possible to use other components that undergo crosslinking reaction, charge amount adjusting components, etc. at the same time. Furthermore, examples of modified silicone resins include KR206 (alkyd modified), KR5208 (acrylic modified), ES1001N (epoxy modified), and KR305 (urethane modified) manufactured by Shin-Etsu Chemical Co., Ltd., and SR2115 (epoxy modified), SR2110 (alkyd modified), manufactured by Toray Dow Corning Silicone Co., Ltd.
[0029] The acrylic resin in this specification refers to all resins having an acrylic component, and is not particularly limited. In addition, it is possible to use the acrylic resin alone, but it is also possible to use at least one other component that undergoes a crosslinking reaction at the same time. Examples of the other components that undergo a crosslinking reaction here include, but are not limited to, amino resins and acid catalysts. The amino resins here refer to, but are not limited to, guanamine and melamine resins. In addition, the acid catalysts here can be any that have catalytic properties. For example, they can be those that have reactive groups such as a fully alkylated type, a methylol group type, an imino group type, and a methylol / imino group type, but are not limited to these.
[0030] Further, the coating layer more preferably contains a crosslinked product of an acrylic resin and an amino resin. This makes it possible to suppress fusion between the coating layers while maintaining an appropriate elasticity. The amino resin is not particularly limited, but is preferably a melamine resin or a benzoguanamine resin because it can improve the chargeability of the carrier. In addition, when it is necessary to appropriately control the chargeability of the carrier, the melamine resin and / or the benzoguanamine resin may be used in combination with other amino resins.
[0031] The acrylic resin that can be crosslinked with the amino resin preferably has a hydroxyl group and / or a carboxyl group, more preferably has a hydroxyl group. This can further improve the adhesion with the core particles and the conductive particles, and can also improve the dispersion stability of the conductive particles. In this case, the acrylic resin preferably has a hydroxyl value of 10 mgKOH / g or more, more preferably 20 mgKOH / g or more.
[0032] The resin may be an acrylic copolymer composed of the following monomer A component, monomer B component, and monomer C component. When such an acrylic copolymer is used, the coating layer is extremely strong and difficult to scrape off, and high durability can be achieved. Even if the coating layer is made thin, the core material is unlikely to become exposed during use.
[0033] [ka] [ka] [ka]
[0034] In the general formulas (1) to (3), R 1 , m, R 2 , R 3 , X, Y, and Z represent the following: R 1 represents a hydrogen atom or a methyl group. m represents an integer of 1 to 8. Therefore, (CH2) m represents an alkylene group having 1 to 8 carbon atoms, such as a methylene group, an ethylene group, a propylene group, or a butylene group. R 2 represents an alkyl group such as a methyl group, ethyl group, propyl group, isopropyl group, or butyl group having 1 to 4 carbon atoms. R 3 represents an alkyl group such as a methyl group, ethyl group, propyl group, isopropyl group, or butyl group having 1 to 8 carbon atoms, or an alkoxy group such as a methoxy group, ethoxy group, propoxy group, or butoxy group having 1 to 4 carbon atoms. X = 10 mol% to 40 mol%, Y = 10 mol% to 40 mol%, Z = 30 mol% to 80 mol%, and preferably 60 mol% < Y + Z < 90 mol%.
[0035] The monomer A component represented by the general formula (1) has an atomic group·tris(trimethylsiloxy)silane having a large number of methyl groups in the side chain. When the ratio of the monomer A component to the whole resin increases, the surface energy decreases, and the adhesion of toner resin components, wax components, etc. decreases. If the monomer A component is 10 mol% or more, a sufficient effect can be obtained, and a sharp increase in the adhesion of toner components can be prevented. Also, if it is 90 mol% or less, the monomer B component and the monomer C component described later will decrease, so that crosslinking does not proceed, toughness is insufficient, the adhesion between the core material and the coating layer decreases, and problems such as poor durability of the carrier coating can be prevented.
[0036] R 2 is an alkyl group having 1 to 4 carbon atoms. Examples of such a monomer A component include tris(trialkylsiloxy)silane compounds represented by the following formula. In the following formula, Me represents a methyl group, Et represents an ethyl group, and Pr represents a propyl group. CH2=CMe-COO-C3H6-Si(OSiMe3)3 CH2=CH-COO-C3H6-Si(OSiMe3)3 CH2=CMe-COO-C4H8-Si(OSiMe3)3 CH2=CMe-COO-C3H6-Si(OSiEt3)3 CH2=CH-COO-C3H6-Si(OSiEt3)3 CH2=CMe-COO-C4H8-Si(OSiEt3)3 CH2=CMe-COO-C3H6-Si(OSiPr3)3 CH2=CH-COO-C3H6-Si(OSiPr3)3 CH2=CMe-COO-C4H8-Si(OSiPr3)3
[0037] The monomer B component represented by the general formula (2) is a radically polymerizable bifunctional (R 3 is an alkyl group), or trifunctional (R 3 The monomer B is a silane compound (in the case of an alkoxy group), and if the monomer B component is 10 mol % or more, sufficient toughness can be obtained. On the other hand, if it is 90 mol % or less, the coating becomes hard and brittle, and the problem of the film being easily scraped off can be prevented. In addition, deterioration of environmental characteristics can be prevented. This is because if a large number of hydrolyzed crosslinking components remain as silanol groups, it is thought that this could worsen environmental characteristics (humidity dependency).
[0038] Examples of the monomer B component include 3-methacryloxypropyltrimethoxysilane, 3-acryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltriethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltri(isopropoxy)silane, 3-acryloxypropyltri(isopropoxy)silane, etc. These may be used alone or in combination of two or more.
[0039] The monomer C component represented by the general formula (3) imparts flexibility to the coating layer and improves adhesion between the core material and the coating layer. When the monomer C component is 30 mol % or more, sufficient adhesion can be obtained, and when it is 80 mol % or less, it is possible to prevent either the monomer A component or the monomer B component from becoming 10 mol % or less, and it is possible to achieve a balance between water repellency, hardness, and flexibility (film scraping) of the carrier coating.
[0040] The acrylic compound (monomer) of the monomer C component is preferably, for example, an acrylic acid ester or a methacrylic acid ester, and specifically, methyl methacrylate, methyl acrylate, ethyl methacrylate, ethyl acrylate, butyl methacrylate, butyl acrylate, 2-(dimethylamino)ethyl methacrylate, 2-(dimethylamino)ethyl acrylate, 3-(dimethylamino)propyl methacrylate, 3-(dimethylamino)propyl acrylate, etc. may be mentioned. These may be used alone or in combination of two or more. Among these, alkyl methacrylate is preferable, and methyl methacrylate is more preferable.
[0041] In a preferred embodiment, the acrylic copolymer obtained by radically copolymerizing the above-mentioned monomer A component, the above-mentioned monomer B component, and the above-mentioned monomer C component is hydrolyzed to generate silanol groups, and condensed using a catalyst to obtain a crosslinked product, which is then coated on a core material and then heat-treated to form a coating layer. Examples of catalysts used in the condensation polymerization include titanium-based catalysts, tin-based catalysts, zirconium-based catalysts, and aluminum-based catalysts.
[0042] Among these, titanium catalysts are preferred. Titanium diisopropoxybis(ethylacetoacetate) is particularly preferred as the titanium catalyst. This is believed to be because it has a large effect of promoting the condensation reaction of silanol groups and the catalyst is not easily deactivated.
[0043] -Other ingredients- The other components are not particularly limited and can be appropriately selected depending on the purpose. Examples of the other components include a silane coupling agent and inorganic particles.
[0044] --Silane coupling agent-- The silane coupling agent is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include methyltrimethoxysilane, methyltriethoxysilane, vinyltriacetoxysilane, r-chloropropyltrimethoxysilane, hexamethyldisilazane, r-anilinopropyltrimethoxysilane, vinyltrimethoxysilane, octadecyldimethyl[3-(trimethoxysilyl)propyl]ammonium chloride, r-chloropropylmethyldimethoxysilane, methyltrichlorosilane, dimethyldichlorosilane, trimethylchlorosilane, allyltriethoxysilane, 3-aminopropylmethyldiethoxysilane, 3-aminopropyltrimethoxysilane, dimethyldiethoxysilane, 1,3-divinyltetramethyldisilazane, methacryloxyethyldimethyl(3-trimethoxysilylpropyl)ammonium chloride, etc. These may be used alone or in combination of two or more.
[0045] As the silane coupling agent, commercially available products can be used. Examples of the commercially available products include AY43-059, SR6020, SZ6023, SH6026, SZ6032, SZ6050, AY43-310M, SZ6030, SH6040, AY43-026, AY43-031, sh6062, Z-6911, sz6300, sz6075, sz6079, sz6083, sz6070, sz6072, Z-6721, AY43-004, and Z-6187. , AY43-021, AY43-043, AY43-040, AY43-047, Z-6265, AY43-204M, AY43-048, Z-6403, AY43-206M, AY43-206E, Z6341, AY43-210MC, AY43-083, AY43-101, AY43-013, AY43-158E, Z-6920, Z-6940 (manufactured by Toray Silicones), etc.
[0046] The content of the silane coupling agent is preferably 0.1% by mass or more and 10% by mass or less with respect to the resin. By having the content of the silane coupling agent be 0.1% by mass or more, the adhesion between the core particles or microparticles and the silicone resin does not decrease, and the coating layer does not fall off during long-term use. In addition, by having the content of the silane coupling agent be 10% by mass or less, toner filming does not occur during long-term use.
[0047] -Inorganic particles- When electrostatically charged particles are contained as inorganic particles in the coating layer in addition to the antimony-containing particles, the electrostatic charge imparting function of the particles can suppress the decrease in the charging ability of the carrier when the toner is balanced over a large image area, and the occurrence of abnormalities such as toner scattering and background scumming due to the decrease in electrostatic charge can be suppressed.
[0048] The electrically charged particles referred to here refer to particles having a relatively low ionization potential, and more specifically, refer to particles having an ionization potential lower than that of aluminum oxide particles (AA-03 manufactured by Sumitomo Chemical Co., Ltd.). Suitable inorganic particles include, for example, titanium oxide, tin oxide, zinc oxide, alumina, barium sulfate, magnesium oxide, magnesium hydroxide, hydrotalcite, etc. These may be used alone or in combination of two or more. Among these, barium sulfate and magnesium oxide are preferred from the viewpoint of maintaining electrostatic charge for a long period of time.
[0049] <Carrier manufacturing method> The carrier can be produced, for example, by dissolving the resin or the like in a solvent to prepare a coating solution, uniformly coating the coating solution on the surface of the core material by a known coating method, drying, and then baking. Examples of the coating method include a dipping method, a spraying method, and a brush coating method.
[0050] The solvent is not particularly limited and can be appropriately selected depending on the purpose. Examples of the solvent include toluene, xylene, methyl ethyl ketone, methyl isobutyl ketone, cellosolve, and butyl acetate.
[0051] The baking method is not particularly limited and can be appropriately selected depending on the purpose. For example, it may be an external heating method or an internal heating method.
[0052] The baking equipment is not particularly limited and can be appropriately selected depending on the purpose. Examples of the equipment include a fixed electric furnace, a fluidized electric furnace, a rotary electric furnace, a burner furnace, and an equipment equipped with a microwave.
[0053] The average thickness of the coating layer is preferably 0.50 μm or more and 1.10 μm or less, and more preferably 0.60 μm or more and 1.00 μm or less. Here, the average thickness of the coating layer can be calculated by image measurement, for example, on a cross-sectional SEM image.
[0054] <Carrier characteristics> The carrier of the present invention preferably has a volume resistivity of 10 (Log Ω·cm) to 14 (Log Ω·cm). If the volume resistivity is less than 10 (Log Ω·cm), carrier adhesion may occur in non-image areas, and if it exceeds 14 (Log Ω·cm), edge effects may reach an unacceptable level.
[0055] Here, the volume resistivity of the carrier can be measured using a cell shown in FIG. 1. Specifically, first, a cell consisting of a fluororesin container 2 containing electrodes 1a and 1b with a surface area of 2.5 cm×4 cm spaced apart from each other by a distance of 0.2 cm is filled with the carrier 3, and tapped 10 times at a drop height of 1 cm and a tapping speed of 30 times / min. Next, a direct current voltage of 1,000 V is applied between the electrodes 1a and 1b, and the resistance value r [Ω] after 30 seconds is measured using a high resistance meter 4329A (manufactured by Yokogawa Hewlett-Packard Co., Ltd.), and the volume resistivity [Ω·cm] can be calculated from the following formula (1).
number
[0056] (Two-component developer) The two-component developer of the present invention comprises the carrier and the toner of the present invention. The mixture ratio of the toner and carrier in the two-component developer is preferably 2.0 parts by mass to 12.0 parts by mass, more preferably 2.5 parts by mass to 10 parts by mass, per 100 parts by mass of the carrier.
[0057] <Toner> The toner contains a binder resin and a colorant, and may be either a monochrome toner or a color toner. The toner may also contain a release agent in order to be applied to an oil-less system in which oil for preventing toner adhesion is not applied to the fixing roller. Such toners are generally prone to filming, but the carrier of the present invention can suppress filming, so that the developer of the present invention can maintain good quality for a long period of time. Furthermore, color toners, particularly yellow toners, generally have a problem of color staining due to scraping of the carrier coating layer, but the developer of the present invention can suppress the occurrence of color staining.
[0058] The toner can be produced by a known method such as a pulverization method or a polymerization method. For example, when the toner is produced by a pulverization method, the toner materials are kneaded to obtain a molten mixture, which is then cooled, pulverized, and classified to produce toner base particles. Next, in order to further improve the transferability and durability, an external additive is added to the toner base particles to produce the toner.
[0059] In this case, the device for kneading the toner materials is not particularly limited and can be appropriately selected depending on the purpose. Examples of the device include a batch-type two-roll mixer; a Banbury mixer; continuous twin-screw extruders such as a KTK type twin-screw extruder (manufactured by Kobe Steel, Ltd.), a TEM type twin-screw extruder (manufactured by Toshiba Machine Co., Ltd.), a twin-screw extruder (manufactured by KCK Corporation), a PCM type twin-screw extruder (manufactured by Ikegai Corporation), and a KEX type twin-screw extruder (manufactured by Kurimoto Iron Works, Ltd.); and continuous single-screw kneaders such as a Co-kneader (manufactured by Buss).
[0060] In addition, when the cooled molten kneaded product is pulverized, it can be roughly pulverized using a hammer mill, a rotoplex, etc., and then finely pulverized using a fine pulverizer using a jet stream, a mechanical fine pulverizer, etc. It is preferable to pulverize the product so that the volume average particle size is 3 μm or more and 15 μm or less.
[0061] Furthermore, when classifying the pulverized melt-kneaded product, an air classifier or the like can be used. It is preferable to classify the toner base particles so that the volume average particle size is 5 μm or more and 20 μm or less.
[0062] Furthermore, when an external additive is added to the toner base particles, the external additive is adhering to the surfaces of the toner base particles while being disintegrated by mixing and stirring using a mixer or the like.
[0063] -Binding resin- The binder resin is not particularly limited and can be appropriately selected depending on the purpose. Examples of the binder resin include homopolymers of styrene and its substitutes, such as polystyrene, poly-p-styrene, and polyvinyl toluene; styrene-p-chlorostyrene copolymers, styrene-propylene copolymers, styrene-vinyl toluene copolymers, styrene-methyl acrylate copolymers, styrene-ethyl acrylate copolymers, styrene-methacrylic acid copolymers, styrene-methyl methacrylate copolymers, styrene-ethyl methacrylate copolymers, styrene-butyl methacrylate copolymers, styrene-α-chloromethyl methacrylate copolymers, styrene-acrylonitrile copolymers, styrene-vinyl methyl ether copolymers, styrene-vinyl methyl ketone copolymers, styrene-butadiene copolymers, styrene-isoprene copolymers, and styrene-maleic acid ester copolymers; and polymethyl methacrylate, polybutyl methacrylate, polyvinyl chloride, polyvinyl acetate, polyethylene, polyester, polyurethane, epoxy resins, polyvinyl butyral, polyacrylic acid, rosin, modified rosin, terpene resins, phenolic resins, aliphatic or aromatic hydrocarbon resins, and aromatic petroleum resins. These may be used alone or in combination of two or more.
[0064] The binder resin for pressure fixing is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include polyolefins such as low molecular weight polyethylene and low molecular weight polypropylene; olefin copolymers such as ethylene-acrylic acid copolymer, ethylene-acrylic acid ester copolymer, styrene-methacrylic acid copolymer, ethylene-methacrylic acid ester copolymer, ethylene-vinyl chloride copolymer, ethylene-vinyl acetate copolymer, and ionomer resin; epoxy resin, polyester, styrene-butadiene copolymer, polyvinylpyrrolidone, methyl vinyl ether-maleic anhydride copolymer, maleic acid modified phenolic resin, and phenol modified terpene resin. These may be used alone or in combination of two or more.
[0065] -Coloring agent- The colorant (pigment or dye) is not particularly limited and can be appropriately selected depending on the purpose. Examples of the colorant include yellow pigments such as cadmium yellow, mineral fast yellow, nickel titanium yellow, navel yellow, naphthol yellow S, Hansa yellow G, Hansa yellow 10G, benzidine yellow GR, quinoline yellow lake, permanent yellow NCG, and tartrazine lake; orange pigments such as molybdenum orange, permanent orange GTR, pyrazolone orange, Balkan orange, indanthrene brilliant orange RK, benzidine orange G, and indanthrene brilliant orange GK; red iron oxide, cadmium red, permanent red 4R, lithol red, pyrazolone red, watching red calcium salt, and lake red. Red pigments such as tetrahydrofuran D, brilliant carmine 6B, eosin lake, rhodamine lake B, alizarin lake, brilliant carmine 3B, etc.; purple pigments such as fast violet B, methyl violet lake, etc.; blue pigments such as cobalt blue, alkali blue, Victoria blue lake, phthalocyanine blue, metal-free phthalocyanine blue, partially chlorinated phthalocyanine blue, fast sky blue, indanthrene blue BC, etc.; green pigments such as chrome green, chromium oxide, pigment green B, malachite green lake, etc.; black pigments such as azine-based pigments such as carbon black, oil furnace black, channel black, lamp black, acetylene black, aniline black, metal salt azo pigments, metal oxides, composite metal oxides, etc. These may be used alone or in combination of two or more.
[0066] -Release agent- The release agent is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include polyolefins such as polyethylene and polypropylene, fatty acid metal salts, fatty acid esters, paraffin wax, amide wax, polyhydric alcohol wax, silicone varnish, carnauba wax, ester wax, etc. These may be used alone or in combination of two or more kinds.
[0067] -Charge control agent-The toner may further contain a charge control agent. The charge control agent is not particularly limited and can be appropriately selected depending on the purpose. For example, 1 Nigrosine; azine dye having an alkyl group having 2 to 16 carbon atoms; CIBasic Yellow 2 (CI41000), CIBasic Yellow 3, CIBasic Red 1 (CI45160), CIBasic Red 9 (CI42500), CIBasic Violet 1 (CI42535), CIBasic Violet 3 (CI42555), CIBasic Violet 10 (CI45170), CIBasic Violet 14 (CI42510), CIBasic Blue 1 (CI42025), CIBasic Blue 3 (CI51005), CIBasic Blue 5 (CI42140), CIBasic Blue 7 (CI42595), CIBasic Blue 9 (CI52015), CIBasic Blue 24 (CI52030), CIBasic Examples of the basic dyes include Blue 25 (CI 52025), CI Basic Blue 26 (CI 44045), CI Basic Green 1 (CI 42040), and CI Basic Green 4 (CI 42000); lake pigments of these basic dyes; quaternary ammonium salts such as CI Solvent Black 8 (CI 26150), benzoylmethylhexadecylammonium chloride, and decyltrimethylchloride; dialkyltin compounds such as dibutyl and dioctyl; dialkyltin borate compounds; guanidine derivatives; polyamine resins such as vinyl polymers having amino groups and condensation polymers having amino groups; metal complex salts of monoazo dyes; salicylic acid; metal complexes of dialkylsalicylic acid, naphthoic acid, and dicarboxylic acids with Zn, Al, Co, Cr, Fe, and the like; sulfonated copper phthalocyanine pigments; organic boron salts; fluorine-containing quaternary ammonium salts; and calixarene compounds. These may be used alone or in combination of two or more. For color toners other than black, white metal salts of salicylic acid derivatives are preferred.
[0068] -External additives- The external additive is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include inorganic particles such as silica, titanium oxide, alumina, strontium titanate, silicon carbide, silicon nitride, and boron nitride; and resin particles such as polymethyl methacrylate particles and polystyrene particles having an average particle size of 0.05 μm to 1 μm obtained by a soap-free emulsion polymerization method. These may be used alone or in combination of two or more. Among these, silica whose surface has been hydrophobized is preferred.
[0069] Furthermore, it is more preferable to use two or more types of silica with different particle sizes in combination. Specifically, it is preferable to use silica with an average secondary particle size of 100 nm or more in combination with silica with an average secondary particle size of less than 100 nm. Large silica particles of 100 nm or more act as a spacer for the toner base particles, and can separate the highly adhesive toner base particles. By externally adding small silica particles of less than 100 nm to the toner base particles, it is possible to impart fluidity to the toner. As a result, a toner with high fluidity and in which each particle is separated is obtained, which contributes to high image quality. The secondary particle size can be measured, for example, using a Zetasizer Pro (manufactured by Spectris Inc.).
[0070] The total number of the large particle silica and the small particle silica is preferably 1.5 parts by mass or more and 55 parts by mass or less, and more preferably 25 parts by mass or more and 35 parts by mass or less, relative to 100 parts by mass of the toner base particles. By being 1.5 parts by mass or less, the fluidity of the toner is not reduced, and there is no risk of toner transfer defects occurring during the transfer process. On the other hand, by being 5 parts by mass or less, the silica does not adhere to the electrostatic latent image carrier, and there is no risk of abnormal images occurring.
[0071] The color of the toner is not particularly limited and can be appropriately selected depending on the purpose, and can be at least one selected from black toner, cyan toner, magenta toner, and yellow toner. Each color toner can be obtained by appropriately selecting the type of colorant, but color toner is preferable.
[0072] (Process cartridge) The process cartridge of the present invention comprises an electrostatic latent image carrier, charging means for charging the surface of the electrostatic latent image carrier, developing means for developing the electrostatic latent image formed on the electrostatic latent image carrier using the developer of the present invention, and cleaning means for cleaning residual toner on the surface of the electrostatic latent image carrier, and may further comprise other means as necessary. The process cartridge can be detachably mounted in various electrophotographic image forming apparatuses, and is preferably detachably mounted in the image forming apparatus of the present invention described below.
[0073] (Image forming apparatus and image forming method) The image forming apparatus of the present invention comprises an electrostatic latent image carrier, a charging means for charging the electrostatic latent image carrier, an exposure means for forming an electrostatic latent image on the electrostatic latent image carrier, a developing means for developing the electrostatic latent image formed on the electrostatic latent image carrier with the developer of the present invention to form a toner image, a transfer means for transferring the toner image formed on the electrostatic latent image carrier to a recording medium, and a fixing means for fixing the toner image transferred to the recording medium, and may further comprise other means as necessary.
[0074] The image forming method of the present invention includes a charging step of charging an electrostatic latent image carrier, an exposure step of forming an electrostatic latent image on the electrostatic latent image carrier, a developing step of developing the electrostatic latent image formed on the electrostatic latent image carrier using the developer of the present invention to form a toner image, a transfer step of transferring the toner image formed on the electrostatic latent image carrier to a recording medium, and a fixing step of fixing the toner image transferred to the recording medium, and may further include other steps as necessary.
[0075] The electrostatic latent image carrier is not particularly limited in terms of its material, shape, structure, size, etc., and can be appropriately selected from known ones. A preferred shape is a drum shape, and examples of its material include inorganic photoconductors such as amorphous silicon and selenium, and organic photoconductors such as polysilane and phthalopolymethine.
[0076] Examples of the organic photoreceptor include a laminated type photoreceptor having a laminated structure in which a layer (charge generation layer) in which a charge generation material such as metal-free phthalocyanine or titanyl phthalocyanine is dispersed in a binder resin and a layer (charge transport layer) in which a charge transport material is dispersed in a binder resin are stacked on a support such as an aluminum drum, and a single-layer type photoreceptor having a single-layered photosensitive layer in which both a charge generation material and a charge transport material are dispersed in a binder resin on a support. In the single-layer type photoreceptor, a hole transport material and an electron transport material can also be added to the photosensitive layer as charge transport materials. An undercoat layer may be provided between the support and the multi-layer charge generating layer or the single-layer photosensitive layer.
[0077] <Charging process and charging means> The charging step can be carried out, for example, by applying a voltage to the surface of the electrostatic latent image bearing member using the charging means.
[0078] The charging means is not particularly limited and can be appropriately selected depending on the purpose. Examples of the charging means include a contact charger known per se having a conductive or semiconductive roller, brush, film, rubber blade, etc., and a non-contact charger utilizing corona discharge such as a corotron or scorotron.
[0079] The shape of the charging means may be any shape such as a roller, a magnetic brush, a fur brush, etc., and can be selected according to the specifications and shape of the electrophotographic device. When a magnetic brush is used, the magnetic brush uses various ferrite particles such as Zn-Cu ferrite as a charging member, and is composed of a non-magnetic conductive sleeve for supporting the magnetic brush and a magnet roller contained therein. When a brush is used, for example, the material of the fur brush is fur that has been treated to be conductive with carbon, copper sulfide, metal, or metal oxide, and this is wound or attached to a metal or other conductive core to form a charger.
[0080] The charging means is not limited to the contact type charger as described above, but it is preferable to use a contact type charger because this provides an image forming apparatus in which the amount of ozone generated from the charger is reduced.
[0081] <Exposure Step and Exposure Means> The exposure step can be carried out, for example, by exposing the surface of the electrostatic latent image bearing member imagewise using the exposure unit. The exposure means is not particularly limited as long as it can expose the surface of the electrostatic latent image carrier charged by the charging means in the form of an image to be formed, and can be appropriately selected depending on the purpose. Examples of the exposure means include various exposure devices such as a copying optical system, a rod lens array system, a laser optical system, and a liquid crystal shutter optical system. In the present invention, a light back system may be adopted in which exposure is performed imagewise from the back side of the electrostatic latent image bearing member.
[0082] <Developing step and developing means> The developing unit is a unit that develops the electrostatic latent image with the toner or the two-component developer to form a visible image. The visible image can be formed, for example, by developing the electrostatic latent image with the toner or the two-component developer of the present invention.
[0083] The developing means is not particularly limited as long as it can develop using the toner or the two-component developer, and can be appropriately selected depending on the purpose. However, it is preferable for the developing means to have at least a developing device that can accommodate the toner or the two-component developer and apply the toner or the two-component developer to the electrostatic latent image in a contact or non-contact manner, and a developing device equipped with a toner container is more preferable.
[0084] The developing means may be of a dry developing type or a wet developing type, and may be a monochrome developing device or a multi-color developing device. Suitable examples include a device having an agitator that frictionally agitates and charges the toner or the two-component developer, and a rotatable magnetic roller.
[0085] In the developing means, for example, the toner and the carrier are mixed and stirred, and the toner is charged by friction during this process and held in a standing state on the surface of the rotating magnet roller to form a magnetic brush. Since the magnet roller is disposed near the electrostatic latent image carrier (photoconductor), a part of the toner constituting the magnetic brush formed on the surface of the magnet roller moves to the surface of the electrostatic latent image carrier (photoconductor) by electrical attraction. As a result, the electrostatic latent image is developed by the toner, and a visible image of the toner is formed on the surface of the electrostatic latent image carrier (photoconductor).
[0086] The developer contained in the developing means is a developer containing the toner, and the developer may be a one-component developer or a two-component developer. The toner contained in the developer is the toner.
[0087] <Transfer process and transfer means> The transfer means is not particularly limited as long as it is a means for transferring the visible image onto a recording medium, and can be appropriately selected depending on the purpose. However, a means is preferred which uses an intermediate transfer body, primarily transfers the visible image onto the intermediate transfer body, and then secondarily transfers the visible image onto the recording medium. It is preferable that the toner used is a toner of two or more colors, preferably a full-color toner, and that the transfer means has a primary transfer means which transfers the visible image onto the intermediate transfer body to form a composite transfer image, and a secondary transfer means which transfers the composite transfer image onto the recording medium.
[0088] The transfer can be performed, for example, by charging the electrostatic latent image carrier (photoconductor) using a transfer charger, and can be performed by the transfer means. The transfer means preferably has a primary transfer means for transferring a visible image onto an intermediate transfer body to form a composite transfer image, and a secondary transfer means for transferring the composite transfer image onto a recording medium. The intermediate transfer body is not particularly limited and can be appropriately selected from known transfer bodies depending on the purpose. For example, a transfer belt is preferably used.
[0089] The transfer means (the primary transfer means, the secondary transfer means) preferably has at least a transfer device that peels and charges the visible image formed on the electrostatic latent image carrier (photoconductor) onto the recording medium. The number of transfer devices may be one or more. Examples of the transfer device include a corona transfer device that uses corona discharge, a transfer belt, a transfer roller, a pressure transfer roller, and an adhesive transfer device.
[0090] The recording medium is typically plain paper, but there are no particular limitations as long as it is capable of transferring the unfixed image after development, and can be selected appropriately according to the purpose. A PET base for overhead projectors can also be used.
[0091] <Fixing process and fixing means> The fixing means is a means for fixing the transferred image transferred to the recording medium using a fixing member, and may be a means for fixing each color of toner each time it is transferred to the recording medium, or may be a means for fixing each color of toner simultaneously at once in a stacked state. The fixing member is not particularly limited and can be appropriately selected depending on the purpose, but is preferably a known heating and pressing member, such as a combination of a heating roller and a pressure roller, or a combination of a heating roller, a pressure roller and an endless belt. The heating temperature in the heating and pressing member is usually preferably 80°C to 200°C.
[0092] <Other steps and other means> The other steps are not particularly limited and may be appropriately selected depending on the purpose. Examples of the other steps include a static elimination step, a cleaning step, a recycling step, and a control step. The other means are not particularly limited and can be appropriately selected depending on the purpose. Examples of the other means include a static elimination means, a cleaning means, a recycling means, and a control means.
[0093] -Static charge removal process and static charge removal means- The discharge means is not particularly limited as long as it is a means capable of applying a discharge bias to the electrostatic latent image bearing member, and may be appropriately selected depending on the purpose. For example, a discharge lamp may be used. -Cleaning process and cleaning means-
[0094] The cleaning means is not particularly limited as long as it is a means capable of removing the electrophotographic toner remaining on the electrostatic latent image carrier, and can be appropriately selected depending on the purpose. Examples of the cleaning means include a magnetic brush cleaner, an electrostatic brush cleaner, a magnetic roller cleaner, a blade cleaner, a brush cleaner, and a web cleaner.
[0095] -Recycling process and methods- The recycling means is not particularly limited and can be appropriately selected depending on the purpose. For example, known transport means can be used.
[0096] -Control process and control means- The control means is not particularly limited as long as it is a means capable of controlling the movement of each of the means, and can be appropriately selected depending on the purpose. For example, devices such as a sequencer and a computer can be mentioned.
[0097] An example of the process cartridge of the present invention is shown in Fig. 2. The process cartridge 10 in Fig. 2 integrally supports an electrostatic latent image carrier 11, a charging means 12 for charging the electrostatic latent image carrier 11, a developing means 13 for developing the electrostatic latent image formed on the electrostatic latent image carrier 11 with the developer of the present invention to form a toner image, and a cleaning means 14 for removing the toner remaining on the electrostatic latent image carrier 11 after the toner image formed on the electrostatic latent image carrier 11 is transferred to a recording medium, and the process cartridge 10 is detachable from the main body of an image forming apparatus such as a copier or printer.
[0098] Next, a method of forming an image using an image forming apparatus equipped with the process cartridge 10 will be described.
[0099] First, the electrostatic latent image carrier 11 is rotated at a predetermined peripheral speed, and the peripheral surface of the electrostatic latent image carrier 11 is uniformly charged to a predetermined positive or negative potential by the charging means 12. Next, exposure light is irradiated onto the peripheral surface of the electrostatic latent image carrier 11 from an exposure means (not shown) such as a slit exposure type exposure means or an exposure means for scanning and exposing with a laser beam, and an electrostatic latent image is formed sequentially. Furthermore, the electrostatic latent image formed on the peripheral surface of the electrostatic latent image carrier 11 is developed by the developing means 13 using the developer of the present invention, and a toner image is formed. Next, the toner image formed on the peripheral surface of the electrostatic latent image carrier 11 is transferred sequentially to a transfer paper fed from a paper feed section (not shown) between the electrostatic latent image carrier 11 and a transfer means (not shown) in synchronization with the rotation of the electrostatic latent image carrier 11. Furthermore, the recording medium onto which the toner image has been transferred is separated from the peripheral surface of the electrostatic latent image carrier 11 and introduced into a fixing means (not shown) where the toner image is fixed, and then printed out as a duplicate (copy) to the outside of the image forming apparatus. Meanwhile, the surface of the electrostatic latent image carrier 11 onto which the toner image has been transferred is cleaned by cleaning means 14 to remove residual toner, and then is discharged by discharging means (not shown) for repeated use in image formation. EXAMPLES
[0100] Examples of the present invention will be described below, but the present invention is not limited to these examples. In the following, "parts" means parts by mass, and "%" means % by mass.
[0101] (Production Example 1 of Core Particles) As raw materials, 21.5 kg of Fe2O3 (average particle size: 0.6 μm, SiO2 content: 0.02%), 10.4 kg of Mn3O4 (average particle size: 0.9 μm, SiO2 content: 0.01%), and 0.28 kg of SrCO3 (average particle size: 0.6 μm) were dispersed in 10.0 kg of pure water, and 120 g of carbon black as a reducing agent and 180 g of a polycarboxylate ammonium dispersant (Cerna D305, manufactured by Chukyo Yushi Co., Ltd.) as a dispersant were added to prepare a mixture.
[0102] This mixture was pulverized in a wet ball mill (media diameter: 2 mm) to obtain a mixed slurry. This mixed slurry was sprayed into hot air at about 130° C. using a spray dryer to obtain dried granules having particle sizes of 10 μm to 75 μm. The granulated material was placed in an electric furnace and heated to 1,400°C over 4.5 hours. Thereafter, firing was carried out by holding at 1,400°C for 8 hours. It was then cooled to room temperature over 10 hours. At this time, the oxygen concentration in the electric furnace was 5,000 ppm during firing and 1,200 ppm during cooling.
[0103] The obtained sintered material was degranulated using a hammer mill ("Hammer Crusher NH-34S", screen opening: 0.3 mm, manufactured by Sansho Industry Co., Ltd.) and classified using a vibrating sieve. The obtained sintered material was then subjected to an oxidation treatment (high resistance treatment) by holding it at 450°C for 1.5 hours in an air atmosphere, thereby obtaining [core particle C1].
[0104] (Conductive particle manufacturing example 1) An acid solution was prepared by dissolving 18.1 g of antimony trichloride (SbCl3) in 750 ml of 2.4 N hydrochloric acid prepared separately, and 1 / 5 of this acid solution and an aqueous ammonia solution were added in parallel over 1 hour to 2 liters of water heated to 70°C while maintaining the pH of the suspension at 7-8. Then, 4 / 5 of the remaining acid solution and an aqueous sodium hydroxide solution were added in parallel over 2 hours while maintaining the pH of the suspension at 7-8. After the addition was completed, the pH was adjusted to 6 with dilute hydrochloric acid, and the suspension was stirred and aged for 1 hour. The suspension was washed and filtered until the conductivity of the filtrate was 50 μS / cm or less. After drying at 110°C for 12 hours, it was fired in an electric furnace at 700°C. The obtained powder was pulverized, and the pulverized material was added with 4% by weight of vinyltriethoxysilane while stirring in a Henschel mixer heated to 70°C. The treated product was then subjected to a heat treatment at 100° C. for 1 hour to obtain [conductive particles P1].
[0105] (Conductive particle manufacturing example 2) An acid solution was prepared by dissolving 160.5g of stannic chloride (SnCl4·5H2O) and 18.1g of antimony trichloride (SbCl3) in 750ml of 2.4N hydrochloric acid. 1 / 5 of this acid solution and an aqueous ammonia solution were added in parallel over 1 hour to 2L of water kept at 70℃ while keeping the pH of the suspension at 7-8. Then, 4 / 5 of the remaining acid solution and an aqueous sodium hydroxide solution were added in parallel over 2 hours while keeping the pH of the suspension at 7-8. After the addition, the pH was adjusted to 6 with dilute hydrochloric acid, and the mixture was stirred and aged for 1 hour. The suspension was washed and filtered until the conductivity of the filtrate was 50μS / cm or less. After drying at 110℃ for 12 hours, it was fired in an electric furnace at 700℃. The obtained powder is pulverized, and the pulverized material is treated with 4% by weight of vinyltriethoxysilane while being stirred in a Henschel mixer heated to 70° C. The treated product is further heat-treated at 100° C. for 1 hour to obtain [conductive particle P2].
[0106] (Conductive particle manufacturing example 3) 300g of alumina (AKP-50, Sumitomo Chemical Co., Ltd.) calcined at 900℃ was dispersed in pure water using a homogenizer manufactured by Tokushu Kika Co., Ltd. to prepare a 2L aqueous suspension, which was then heated and maintained at 70℃. 160.5g of stannic chloride (SnCl4·5H2O) and 18.1g of antimony trichloride (SbCl3) were dissolved in 750mL of 2.4N hydrochloric acid to prepare an acid solution, and 1 / 5 of this acid solution and an aqueous ammonia solution were added in parallel over 1 hour while maintaining the pH of the suspension at 7-8. 4 / 5 of the remaining acid solution and an aqueous sodium hydroxide solution were added in parallel over 2 hours while maintaining the pH of the suspension at 7-8. After the addition was completed, the pH was adjusted to 6 with dilute hydrochloric acid, and the mixture was stirred and aged for 1 hour. The suspension was washed until the conductivity of the filtrate was 50μS / cm or less, and then filtered. After drying at 110°C for 12 hours, it was fired in an electric furnace at 700°C. The obtained powder was pulverized, and the pulverized material was added with 4% by weight of vinyltriethoxysilane while stirring in a Henschel mixer heated to 70°C. The treated product was further heat-treated at 100°C for 1 hour to obtain [Conductive Particle P3].
[0107] (Conductive particle manufacturing example 4) In the conductive particle production example 3, the final vinyltriethoxysilane addition treatment was not carried out to obtain [conductive particle P4].
[0108] (Conductive Particle Manufacturing Example 5) Conductive particles P5 were obtained in the same manner as in Conductive Particle Production Example 3, except that antimony trichloride was changed to 18.6 g of orthophosphoric acid.
[0109] (Conductive Particle Manufacturing Example 6) Conductive particles P6 were obtained in the same manner as in conductive particle production example 3, except that antimony trichloride was changed to 4.3 g of sodium tungstate. Table 1 shows the compositions and structures of [Conductive Particles P1] to [Conductive Particles P6].
[0110] [Table 1]
[0111] (Carrier manufacturing example 1) -Creating the carrier- The following composition was dispersed in a homomixer for 10 minutes to obtain a mixed coating layer forming solution of acrylic resin and silicone resin. 5,000 parts of [core particle C1] was used as the core material, and the following coating layer forming solution was applied to the core material surface to a film thickness of 0.30 μm using a Spira Coater (manufactured by Okada Seiko Co., Ltd.) at a coater temperature of 55°C and dried. The obtained carrier was left in an electric furnace at 200°C for 1 hour to be fired. After cooling, the ferrite powder bulk was crushed using a sieve with 63 μm openings to obtain [Carrier 1] with a volume resistivity of 13.2 [Log Ω·cm].
[0112] [composition] Silicone resin solution: 600 parts (20% solids, SR2410, manufactured by Dow Corning Toray Silicone Co., Ltd.) Titanium catalyst: 4 parts (60% solids, TC-750, Matsumoto Fine Chemical Co., Ltd.): Aminosilane: 3.2 parts (100% solids, SH6020, manufactured by Dow Corning Toray Silicone Co., Ltd.) ·Conductive particles P1: 36 parts Toluene: 1,000 parts
[0113] <Volume resistivity> Using the cell shown in Figure 1, a cell consisting of a fluororesin container 2 containing electrodes 1a and 1b with a surface area of 2.5 cm × 4 cm, spaced 0.2 cm apart, was filled with a carrier 3, and tapped 10 times at a drop height of 1 cm and a tapping speed of 30 times / min. A DC voltage of 1,000 V was applied between electrodes 1a and 1b. The resistance value r [Ω] after 30 seconds was measured using a high resistance meter 4329A (manufactured by Yokogawa Hewlett-Packard Co., Ltd.), and the volume resistivity [Ω cm] was calculated using the following formula (1).
[0114]
number
[0115] (Carrier manufacturing example 2) [Carrier 2] having a volume resistivity of 13.1 [Log Ω cm] was obtained in the same manner as in Carrier Production Example 1, except that in Carrier Production Example 1, [Conductive Particles P1] was changed to [Conductive Particles P2].
[0116] (Carrier Manufacturing Example 3) [Carrier 3] having a volume resistivity of 13.1 [Log Ω cm] was obtained in the same manner as in Carrier Production Example 1, except that in Carrier Production Example 1, [Conductive Particles P1] was changed to [Conductive Particles P3].
[0117] (Carrier Manufacturing Example 4) [Carrier 4] having a volume resistivity of 13.3 [Log Ω·cm] was obtained in the same manner as in Carrier Production Example 3, except that 36 parts of barium sulfate (BF-10, manufactured by Sakai Chemical Industry Co., Ltd.) was added. (Carrier Manufacturing Example 5) [Carrier 5] having a volume resistivity of 13.2 [Log Ω·cm] was obtained in the same manner as in Carrier Production Example 3, except that 36 parts of magnesium oxide (TATEHOMAG #500, manufactured by Tateho Chemical Industries Co., Ltd.) was added.
[0118] (Comparative Carrier Manufacturing Example 1) [Carrier 6] having a volume resistivity of 13.5 [Log Ω·cm] was obtained in the same manner as in Carrier Production Example 4, except that [Conductive Particles P3] in Carrier Production Example 4 was changed to [Conductive Particles P4].
[0119] (Comparative Carrier Manufacturing Example 2) [Carrier 7] having a volume resistivity of 13.5 [Log Ω cm] was obtained in the same manner as in Carrier Production Example 4, except that in Carrier Production Example 4, [Conductive Particles P3] was replaced with 54 parts of [Conductive Particles P5].
[0120] (Comparative Carrier Manufacturing Example 3) [Carrier 8] having a volume resistivity of 13.1 [Log Ω cm] was obtained in the same manner as in Carrier Production Example 4, except that in Carrier Production Example 4, [Conductive Particles P3] was replaced with 54 parts of [Conductive Particles P6]. The property values of the obtained [Carrier 1] to [Carrier 8] are shown in Table 2.
[0121] (Toner Production Example 1) <Preparation of Toner 1> -Synthesis of polyester resin A- In a reaction vessel equipped with a thermometer, a stirrer, a cooler, and a nitrogen inlet tube, 443 parts of a bisphenol A PO adduct (hydroxyl value: 320 mgKOH / g), 135 parts of diethylene glycol, 422 parts of terephthalic acid, and 2.5 parts of dibutyltin oxide were placed and reacted at 200°C until the acid value reached 10 mgKOH / g, yielding [Polyester Resin A]. The resulting [Polyester Resin A] had a glass transition temperature (Tg) of 63°C and a peak number average molecular weight of 6,000.
[0122] -Synthesis example of polyester resin B- In a reaction vessel equipped with a thermometer, a stirrer, a cooler, and a nitrogen inlet tube, 443 parts of a bisphenol A PO adduct (hydroxyl value: 320 mg KOH / g), 135 parts of diethylene glycol, 422 parts of terephthalic acid, and 2.5 parts of dibutyltin oxide were placed and reacted at 230°C until the acid value reached 7 mg KOH / g, yielding [Polyester Resin B]. The glass transition temperature (Tg) of the resulting [Polyester Resin B] was 65°C, and the peak number average molecular weight was 16,000.
[0123] -Production of toner base particles- The following toner constituent materials were mixed in a Henschel mixer (a Henschel 20B manufactured by Nippon Coke and Engineering Co., Ltd., at 1,500 rpm for 3 minutes), and then kneaded in a single-screw kneader (a small Buss-Co Kneader manufactured by Buss) under the following conditions (set temperatures: inlet 100°C, outlet 50°C, feed rate: 2 kg / hr) to obtain a [toner base].
[0124] [Toner base composition] Polyester resin A: 40 parts Polyester resin B: 60 parts Carnauba wax (WA-05, manufactured by Cerarica Noda Co., Ltd.): 1 part Carbon black (#44, manufactured by Mitsubishi Chemical Corporation): 15 parts Next, the toner base is kneaded, rolled and cooled, pulverized in a pulverizer, and then milled in an I-type mill (IDS-2 type manufactured by Japan Pneumatic Co., Ltd.) using a flat impact plate and air pressure of 6.8 atm / cm.2 The mixture was finely pulverized under a constant pressure of 0.5 kg / hr (feed rate: 0.5 kg / hr) and further classified using a classifier (132MP, manufactured by Alpine Co., Ltd.) to obtain [toner base particles 1].
[0125] -External additive treatment- Next, 0.5 parts of large particle silica (MSP-009, manufactured by Teika Corporation, secondary particle diameter 160 nm) and 1.0 part of small particle silica (MSP-015, manufactured by Teika Corporation, secondary particle diameter 40 nm) were added as external additives to 100 parts of [toner base particles 1], and mixed in a Henschel mixer to obtain toner particles. [Toner 1] was produced in this manner. The volume average particle diameter of [Toner 1] was 7.2 μm.
[0126] (Developer Production Examples 1 to 5 and Comparative Developer Production Examples 1 to 3) -Preparation of developers 1 to 8- To 93 parts each of [Carrier 1] to [Carrier 8] obtained in the carrier production example, 7.0 parts of [Toner 1] obtained in the toner production example was added, and the mixture was stirred in a ball mill for 20 minutes to produce two-component developers [Developer 1] to [Developer 8].
[0127] <Developer characteristics> Using each of the obtained two-component developers, image evaluation was performed in an environment of 23°C temperature and 55% relative humidity using a digital color copier / printer multifunction machine (Ricoh Pro C901, manufactured by Ricoh Co., Ltd.) Specifically, first, using [Developer 1] to [Developer 8] of the examples and comparative examples, printing was performed up to 1 million sheets at an image area ratio of 2%, and various evaluations were performed.
[0128] <<Image density>> After 1 million prints, the center of a 30mm x 30mm solid area (Note 1) was measured at five points using an X-Rite 938 spectrophotometer under the above development conditions, and the average values of L*, a*, and b* were calculated. The color difference ΔE was calculated from these and the L*, a*, and b* of the reference colors, and the color stain evaluation was performed as follows. Note 1: Development potential 400V equivalent point = (exposed area potential - development bias DC) = -100V - (-500V) The color difference ΔE in the L*a*b* color space is defined by the following equation (2).
number
[0129] [Evaluation Criteria] ◎ (Very good): 0 or more to less than 0.2 ○ (Good): 0.2 or more to less than 0.5 △ (usable): 0.5 or more to less than 1.0 × (defective): 1.0 or more
[0130] <<Solid carrier adhesion>> Carrier adhesion can cause scratches on the photoconductor and fixing roller, resulting in a decrease in image quality. Even if carrier adhesion occurs on the photoconductor, only a portion of the carrier is transferred to the paper, so it was evaluated using the following method. The number of carrier particles adhering to a solid image (30 mm x 30 mm) under the development conditions (charging potential (Vd): -600 V, potential after exposure of the image area (solid original): -100 V, development bias: DC -500 V) was counted on the photoconductor to evaluate carrier adhesion (solid area).
[0131] [Evaluation Criteria] ◎: Very good (no carrier adhesion) ◯: Good (there is some carrier adhesion, but it does not affect the image) △: Usable (there is carrier adhesion, which affects the image, but is at an acceptable level) ×: Unusable (carrier adhesion is present, affecting the image to an unacceptable level)
[0132] The results after 1 million sheets are shown in Table 3.
[0133] [Table 2]
[0134] [Table 3]
[0135] For example, aspects of the present invention are as follows. (1) A carrier for electrophotographic image formation comprising core particles and a coating layer covering the core particles, the coating layer containing antimony-containing particles which have been subjected to a hydrophobic treatment. (2) The carrier for electrophotographic imaging according to the above (1), wherein the hydrophobization treatment is a treatment in which the antimony-containing particles are coated with a silane coupling agent. (3) The carrier for forming an electrophotographic image according to (1) or (2) above, wherein the antimony-containing particles are diantimony pentoxide particles. (4) The carrier for electrophotographic imaging according to (1) or (2) above, wherein the antimony-containing particles are tin oxide particles doped with an antimony compound. (5) The carrier for forming an electrophotographic image according to (1) or (2) above, wherein the antimony compound is diantimony pentoxide. (6) The carrier for electrophotographic imaging according to (1) or (2) above, wherein the antimony-containing particles are particles in which tin oxide particles doped with an antimony compound are provided on the surface of a substrate made of inorganic particles. (7) The carrier for forming an electrophotographic image according to any one of (1) to (6) above, wherein the coating layer further contains inorganic particles. (8) The carrier for forming an electrophotographic image according to (7) above, wherein the inorganic particles are barium sulfate or magnesium oxide. (9) A two-component developer comprising the carrier for electrophotographic imaging according to any one of (1) to (6) above and a toner. (10) An image forming apparatus comprising: an electrostatic latent image carrier; a charging means for charging the electrostatic latent image carrier; an exposure means for forming an electrostatic latent image on the electrostatic latent image carrier; a developing means for developing the electrostatic latent image formed on the electrostatic latent image carrier using the two-component developer described in (9) above to form a toner image; a transfer means for transferring the toner image formed on the electrostatic latent image carrier to a recording medium; and a fixing means for fixing the toner image transferred to the recording medium. (11) A process cartridge comprising: an electrostatic latent image carrier; a charging member for charging the surface of the electrostatic latent image carrier; a developing unit for developing an electrostatic latent image formed on the electrostatic latent image carrier using the two-component developer described in (9) above; and a cleaning member for cleaning the electrostatic latent image carrier. (12) An image forming method comprising the steps of: charging an electrostatic latent image carrier; forming an electrostatic latent image on the electrostatic latent image carrier; developing the electrostatic latent image formed on the electrostatic latent image carrier using the two-component developer described in (9) above to form a toner image; transferring the toner image formed on the electrostatic latent image carrier to a recording medium; and fixing the toner image transferred to the recording medium. [Explanation of symbols]
[0136] 1a electrode 1b electrode 2. Fluororesin containers 3. Career 10 Process cartridge 11 Electrostatic latent image carrier 12 Charging means 13 Developing means 14 Cleaning methods [Prior art documents] [Patent documents]
[0137] [Patent Document 1] JP 2014-029464 A [Patent Document 2] JP 2009-103787 A
Claims
1. 1. A carrier for electrophotographic image formation comprising core particles and a coating layer that coats the core particles, the coating layer containing antimony-containing particles that have been subjected to a hydrophobic treatment.
2. 2. The carrier for electrophotographic imaging according to claim 1, wherein the hydrophobic treatment is a treatment in which the antimony-containing particles are coated with a silane coupling agent.
3. 3. The electrophotographic imaging carrier of claim 1, wherein said antimony-containing particles are diantimony pentoxide particles.
4. 3. The electrophotographic imaging carrier of claim 1, wherein the antimony-containing particles are tin oxide particles doped with an antimony compound.
5. 5. The electrophotographic imaging carrier of claim 4, wherein said antimony compound is diantimony pentoxide.
6. 3. The carrier for electrophotographic imaging according to claim 1, wherein said antimony-containing particles are particles in which tin oxide particles doped with an antimony compound are provided on the surface of a substrate made of inorganic particles.
7. 3. The carrier for forming an electrophotographic image according to claim 1, further comprising inorganic particles in the coating layer.
8. 8. The electrophotographic imaging carrier of claim 7, wherein said inorganic particles are barium sulfate or magnesium oxide.
9. A two-component developer comprising the carrier for electrophotographic imaging according to claim 1 and a toner.
10. 10. An image forming apparatus comprising: an electrostatic latent image carrier; charging means for charging the electrostatic latent image carrier; exposure means for forming an electrostatic latent image on the electrostatic latent image carrier; developing means for developing the electrostatic latent image formed on the electrostatic latent image carrier with the two-component developer according to claim 9 to form a toner image; transfer means for transferring the toner image formed on the electrostatic latent image carrier to a recording medium; and fixing means for fixing the toner image transferred to the recording medium.
11. 10. A process cartridge comprising: an electrostatic latent image carrier; a charging member for charging a surface of the electrostatic latent image carrier; a developing section for developing an electrostatic latent image formed on the electrostatic latent image carrier by using the two-component developer according to claim 9; and a cleaning member for cleaning the electrostatic latent image carrier.
12. 10. An image forming method comprising: a charging step of charging an electrostatic latent image carrier; a step of forming an electrostatic latent image on the electrostatic latent image carrier; a step of developing the electrostatic latent image formed on the electrostatic latent image carrier using the two-component developer according to claim 9 to form a toner image; a step of transferring the toner image formed on the electrostatic latent image carrier to a recording medium; and a step of fixing the toner image transferred to the recording medium.
Citation Information
Patent Citations
Electrostatic charge image developing carrier, electrostatic charge image developer, electrostatic charge image developer cartridge, process cartridge, image forming apparatus and image forming method
JP2009103787A
Carrier for two-component developer, electrostatic latent image developer using the same, color toner developer, developer to be supplied, image forming method, process cartridge with electrostatic latent image developer, and image forming device
JP2014029464A