Composition using liquid-absorbing resin absorbing liquid organic compound, and applications for the same
A water-soluble polymer with acidic groups integrated into polysaccharides forms a physical gel, addressing the low absorption of liquid organic compounds by existing resins, enabling effective use in antibacterial and moisturizing sheets and food drip sheets.
Patent Information
- Application Number
- JP2023069496
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-20
- Publication Date
- 2024-10-31
AI Technical Summary
Existing water-absorbing resins, such as crosslinked polyacrylic acids, have low absorption properties for liquid organic compounds and mixtures containing both water and organic compounds.
A composition using a water-soluble polymer with acidic groups and/or their salts introduced into polysaccharides or partially decomposed polysaccharides, forming a physical gel that absorbs liquid organic compounds.
The composition effectively absorbs and retains liquid organic compounds, offering applications in antibacterial sheets, moisturizing sheets, and food drip sheets with enhanced absorption capabilities.
Smart Images

Figure 2024155083000001 
Figure 2024155083000002 
Figure 2024155083000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a novel use of a liquid-absorbent resin for absorbing a liquid organic compound. [Background technology]
[0002] Conventionally, water-absorbent resins, for example, crosslinked products of polyacrylic acid, have been used in paper diapers, sanitary napkins, etc. These water-absorbent resins absorb water, but have low water-absorbency for liquid organic compounds or mixtures of liquid organic compounds and water.
[0003] For example, as a liquid organic compound, an absorbent resin that absorbs alcohol has been studied. Patent Document 1 discloses a method for producing an alcohol absorbent resin, which is characterized in that a water-soluble polymerization initiator and an oil-soluble polymerization initiator are used as polymerization initiators when an aqueous solution containing an alcohol absorbent resin-forming monomer is copolymerized in an organic solvent by suspension polymerization or emulsion polymerization to produce an alcohol absorbent resin.
[0004] Patent Document 2 discloses a method for producing a highly alcohol-absorbent resin, which comprises polymerizing polymerizable monomers consisting of a cationic (meth)acrylic monomer having a tertiary amino group and / or a quaternary ammonium group and an anionic (meth)acrylic monomer having a sulfonic acid group, the molar ratio of which is in the range of 95:5 to 10:90, in an aqueous solution containing the polymerizable monomers at a concentration of 30% by weight or more up to a saturation concentration, in the presence of a crosslinking agent having two or more polymerizable ethylenically unsaturated bonds in one molecule, using a water-soluble or water-miscible radical polymerization initiator.
[0005] Patent Document 3 discloses a method for producing a highly alcohol-absorbent resin, which comprises polymerizing a polymerizable monomer containing 90 mol % or more of a cationic (meth)acrylic monomer having a tertiary amino group and / or a quaternary ammonium group in an aqueous solution containing the polymerizable monomer at a concentration of 30 wt % or more up to a saturated concentration, in the presence of a crosslinking agent having two or more polymerizable ethylenically unsaturated bonds in one molecule, using a water-soluble or water-miscible radical polymerization initiator. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Publication No. 151406 / 1983 [Patent Document 2] Japanese Patent Application Publication No. 2-215815 [Patent Document 3] Japanese Patent Application Publication No. 2-215816 Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a novel composition using a liquid-absorbent resin capable of absorbing a liquid organic compound, and uses thereof. [Means for solving the problem]
[0008] The composition of the present invention is a composition containing water, a liquid organic compound, and an absorbent resin, and is characterized in that the absorbent resin is made of a water-soluble polymer in which an acidic group and / or a salt thereof has been introduced into a polysaccharide or a partial hydrolysis product thereof. Effect of the Invention
[0009] According to the present invention, a novel composition using a liquid-absorbent resin that absorbs a liquid organic compound can be provided. The composition of the present invention can be suitably used as an antibacterial sheet, a moisture-retaining sheet, or a food drip sheet containing a liquid organic compound. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The composition of the present invention is a composition containing water, a liquid organic compound, and an absorbent resin, and is characterized in that the absorbent resin is made of a water-soluble polymer in which an acidic group and / or a salt thereof has been introduced into a polysaccharide or a partial hydrolysis product thereof.
[0011] The absorbent resin used in the present invention is preferably capable of absorbing water and liquid organic compounds. The absorbent resin is preferably made of a water-soluble polymer in which an acidic group and / or a salt thereof is introduced into a polysaccharide or a partial hydrolyzate thereof, and is preferably made of a water-soluble polymer in which an acidic group and / or a salt thereof is introduced into a starch or a partial hydrolyzate thereof.
[0012] The liquid-absorbent resin used in the present invention will now be described.
[0013] The liquid-absorbent resin used in the present invention is made from polysaccharides or their partial decomposition products as starting materials. The polysaccharides are polymeric compounds formed by the bonding of multiple monosaccharides, and preferably polymeric compounds formed by the bonding of 10 or more monosaccharides. Examples of the monosaccharides include xylose, ribosaccharide, glucose, galactose, fructose, and glucosamine.
[0014] Examples of the polysaccharides include acidic polysaccharides having an acidic group (e.g., a carboxyl group, a sulfate group, or a salt thereof), basic polysaccharides having a basic group, and electrically neutral neutral polysaccharides. Examples of the neutral polysaccharides include cellulose, tamarind seed gum, guar gum, locust bean gum, starch, pullulan, and the like. Examples of the acidic polysaccharides include carrageenan, pectin, gum arabic, xanthan gum, gellan gum, agar, tragacanth gum, and the like. Examples of the basic polysaccharides include chitosan, and the like.
[0015] In the present invention, it is preferable to use neutral polysaccharides from the viewpoint of introducing an acidic group and / or a salt thereof into the polysaccharide. Examples of the structure of neutral polysaccharides include cellulose, amylose, amylopectin, dextran, pullulan, inulin, galactan, mannan, xylan, arabinan, glucomannan, galactomannan, hydroxyethyl cellulose, and methyl cellulose.
[0016] Examples of polysaccharides include simple polysaccharides composed of one type of monosaccharide, complex polysaccharides composed of two or more types of monosaccharides, mucopolysaccharides containing amino sugars as constituent sugars, polyuronides containing uronic acid (D-glucuronic acid) as constituent sugars, etc. The liquid-absorbent resin used in the present invention preferably uses simple polysaccharides as the polysaccharide.
[0017] Examples of the simple polysaccharides include starch, dextrin, glycogen, cellulose, inulin, xylan, mannan, and galactan.
[0018] In the present invention, the polysaccharide to be used is preferably a simple polysaccharide that belongs to neutral polysaccharides, more preferably starch, dextrin, glycogen, cellulose, inulin, xylan, mannan, or galactan, and even more preferably starch or a partially hydrolyzed product thereof. Starch is a simple polysaccharide that contains amylose and amylopectin.
[0019] <Starch or its partial hydrolyzate> In the present invention, it is preferable to use starch or a partial starch hydrolyzate as the polysaccharide. By using starch, it is possible to obtain an absorbent resin that is safe for the human body, has excellent absorbency, and has a small environmental impact when disposed of. The raw material of the starch is not particularly limited, and examples thereof include tapioca starch, potato starch, corn starch such as waxy corn starch and high amylose starch, wheat starch, rice starch, and sweet potato starch. The partial starch hydrolyzate is a polymer in which a large number of α-glucose molecules are linked via glucosidic bonds, and some of the glucosidic bonds are decomposed, but the position where the decomposition occurs and the mode of decomposition are not limited. The method for producing the absorbent resin will be described later, and starch and a partial starch hydrolyzate may be used in combination to produce the absorbent resin.
[0020] When a partial starch hydrolysate is used, the weight-average molecular weight (Mw) of the partial starch hydrolysate is not particularly limited, but is preferably 7.5 million or less, more preferably 5 million or less, even more preferably 4.5 million or less, and even more preferably 4 million or less. The lower limit of the weight-average molecular weight of the partial starch hydrolysate is not particularly limited, but is preferably 50,000 or more, more preferably 100,000 or more, and even more preferably 200,000 or more. If the weight-average molecular weight is less than 50,000, the liquid absorption amount of the absorbent resin tends to decrease. When the viscosity of starch affects the operability in production, it is possible to use two or more types of starch and / or partial starch hydrolysate having different weight-average molecular weights, or other additives, etc., in combination depending on the application and cost. The method for measuring the weight-average molecular weight is not particularly limited, but for example, it can be determined by aqueous size exclusion chromatography based on a calibration curve of molecular weight and elution time prepared using pullulan with a known molecular weight.
[0021] The degree of dispersion (weight average molecular weight (Mw) / number average molecular weight (Mn)) of the partial starch hydrolyzate is not particularly limited, but is generally 5 or more, and if it is less than 5, the amount of liquid absorbed by the absorbent resin tends to decrease. The upper limit of the degree of dispersion is not particularly limited. The method for measuring the number average molecular weight is not particularly limited, but for example, it can be determined by aqueous size exclusion chromatography based on a calibration curve of molecular weight and elution time prepared using pullulan with a known molecular weight.
[0022] The weight-average molecular weight and dispersity of starch or its partial hydrolyzate are as described above, but when starch is used alone, starch derived from waxy corn, tapioca, corn, or potato is preferred, and starch derived from waxy corn, tapioca, or corn is more preferred. When a partial starch hydrolyzate is used alone, the weight-average molecular weight is preferably 50,000 to 7.5 million, more preferably 50,000 to 5 million, and even more preferably 100,000 to 4 million. The dispersity is preferably 5 or more, and more preferably 7 or more.
[0023] <Water-soluble polymer, acidic group> The term "water-soluble polymer" as used herein means a polysaccharide or a partial hydrolyzate thereof into which an acidic group and / or a salt thereof has been introduced. Specifically, examples include a polysaccharide or a partial hydrolyzate thereof into which only an acidic group has been introduced, a polysaccharide or a partial hydrolyzate thereof into which an acidic group and a salt thereof have been introduced, and a polysaccharide or a partial hydrolyzate thereof into which only a salt of an acidic group has been introduced. The water-soluble polymer of the present invention is preferably a polysaccharide or a partial hydrolyzate thereof into which an acidic group and a salt thereof have been introduced. The "introduction of an acidic group and / or a salt thereof" is preferably carried out by forming a salt of an acidic group in the polysaccharide or a partial hydrolyzate thereof and converting at least a part of the salt into a free acidic group by treating it with an acid, as described below.
[0024] Examples of the acidic group include acidic groups having a carboxy group, such as a carboxyalkyl group and a carboxyalkenyl group; acidic groups having a sulfo group, such as a sulfoalkyl group and a sulfoalkenyl group; and acidic groups having a phospho group, such as a phosphoalkyl group and a phosphoalkenyl group, and these acidic groups and / or salts thereof.
[0025] A carboxyalkyl group is an alkyl group substituted with a carboxy group. The number of carbon atoms of the alkyl group substituted with a carboxy group is preferably 1 to 8, more preferably 1 to 5. The alkyl group may be either linear or branched. Specific examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an i-propyl group, an n-butyl group, an i-butyl group, an s-butyl group, a t-butyl group, an n-pentyl group, a 1-methyl-n-butyl group, a 2-methyl-n-butyl group, a 3-methyl-n-butyl group, a 1,1-dimethyl-n-propyl group, a 1,2-dimethyl-n-propyl group, a 2,2-dimethyl-n-propyl group, and a 1-ethyl-n-propyl group.
[0026] Specific examples of the carboxyalkyl group include a carboxymethyl group, a carboxyethyl group, a carboxypropyl group, a carboxybutyl group, and a carboxypentyl group.
[0027] A carboxyalkenyl group is an alkenyl group substituted with a carboxy group. The number of carbon atoms of the alkenyl group substituted with a carboxy group is preferably 2 to 8, more preferably 2 to 4. The alkenyl group may be either linear or branched. Specific examples of the alkenyl group include an ethenyl group, a 1-propenyl group, a 2-propenyl group, a 1-methyl-1-ethenyl group, a 1-butenyl group, a 2-butenyl group, a 3-butenyl group, a 2-methyl-1-propenyl group, a 2-methyl-2-propenyl group, a 1-ethylethenyl group, a 1-methyl-1-propenyl group, and a 1-methyl-2-propenyl group.
[0028] Specific examples of the carboxyalkenyl group include a carboxyethenyl group, a carboxypropenyl group, and a carboxybutenyl group.
[0029] The sulfoalkyl group is an alkyl group substituted with a sulfo group. Examples of the alkyl group substituted with a sulfo group include the alkyl groups mentioned in relation to the carboxyalkyl group. Specific examples of the sulfoalkyl group include a sulfomethyl group, a sulfoethyl group, and a sulfopropyl group.
[0030] The sulfoalkenyl group is an alkenyl group substituted with a sulfo group. The alkenyl group substituted with a sulfo group can be any of the alkenyl groups described above for the carboxyalkenyl group. Specific examples of the sulfoalkenyl group include a sulfoethenyl group and a sulfopropenyl group.
[0031] A phosphoalkyl group is an alkyl group substituted with a phospho group. The alkyl group substituted with a phospho group can be any of the alkyl groups mentioned for the carboxyalkyl group. Specific examples of the phosphoalkyl group include a phosphomethyl group, a phosphoethyl group, and a phosphopropyl group.
[0032] A phosphoalkenyl group is an alkenyl group substituted with a phospho group. The alkenyl group substituted with a phospho group can be any of the alkenyl groups described above for the carboxyalkenyl group. Specific examples of the phosphoalkenyl group include a phosphoethenyl group and a phosphopropenyl group.
[0033] Among the acidic groups, from the viewpoint of ease of introduction into polysaccharides or partial hydrolyzates thereof, acidic groups having a carboxy group or a sulfo group are preferred, carboxyalkyl groups, carboxyalkenyl groups and sulfoalkyl groups are more preferred, and carboxyalkyl groups having 1 to 5 carbon atoms are even more preferred.
[0034] The cation forming the salt of the acidic group is not particularly limited, but examples thereof include alkali metal ions such as lithium, sodium, potassium, etc., alkaline earth metal ions such as magnesium, calcium, etc. Among these, the cation forming the salt of the acidic group is preferably a sodium ion or a potassium ion.
[0035] In addition to the introduction of an acidic group and / or a salt thereof into the polysaccharide or its partial hydrolysis product, the water-soluble polymer may have a hydrogen atom of a hydroxyl group of a monosaccharide constituting the main chain substituted with a functional group other than an acidic group. Examples of the functional group other than an acidic group include hydrocarbon groups such as methyl and ethyl groups, and substituents having a hydroxyl group such as hydroxypropyl and hydroxyethyl groups. The position of the hydroxyl group substituted with a functional group other than an acidic group is not particularly limited, and for example, in the case of glucose, it may be any of the 1st, 2nd, 3rd, 4th, and 6th positions of the glucose unit, but the 2nd, 3rd, and 6th positions are preferred.
[0036] <Physical properties of water-soluble polymers> The molecular weight of the water-soluble polymer is not particularly limited, but the weight average molecular weight calculated as pullulan by aqueous size exclusion chromatography is preferably 100,000 or more, more preferably 1 million or more, even more preferably 5 million or more, preferably 50 million or less, more preferably 30 million or less, and even more preferably 25 million or less. If the weight average molecular weight is less than 100,000, the absorbent resin tends to have a low absorbency, and if it exceeds 30 million, the viscosity is high and the handling properties during production tend to be poor. The weight average molecular weight calculated as pullulan by aqueous size exclusion chromatography can be determined based on a calibration curve of molecular weight and elution time prepared by aqueous size exclusion chromatography using pullulan with a known molecular weight.
[0037] The water-soluble polymer preferably has a total acid value of 50 mgKOH / g or more, more preferably 60 mgKOH / g or more, even more preferably 100 mgKOH / g or more, preferably 350 mgKOH / g or less, more preferably 300 mgKOH / g or less, and even more preferably 250 mgKOH / g or less. As described below, the total acid value of the water-soluble polymer means the acid value measured in the state of free acid groups by converting the salt of an acidic group of the water-soluble polymer into a free acid group when the water-soluble polymer has the salt, and indicates the amount of all acidic groups that the water-soluble polymer has. If the total acid value is 50 mgKOH / g or more and 350 mgKOH / g or less, the liquid-absorbing performance of the aqueous solution containing a liquid organic compound such as a cosmetic product becomes even better in the liquid-absorbing resin after crosslinking the water-soluble polymer.
[0038] When an acidic group and / or its salt is reacted with a haloalkyl group having an acidic group to introduce it into a starch hydroxyl group to produce a water-soluble polymer, the amount of the acidic group and / or its salt introduced can also be expressed by the degree of etherification. The degree of etherification is preferably 0.1 to 2.0, more preferably 0.2 to 1.5. The degree of etherification can be determined by an ashing titration method or the like. In addition, the total acid value is detected by the introduction of an acidic group, and when the raw polysaccharide or the partial hydrolysis product of the polysaccharide does not contain an acidic group, the acidic group detected by the measurement of the total acid value is considered to be equal to that introduced by the etherification reaction. Therefore, when the raw polysaccharide or the partial hydrolysis product of the polysaccharide does not contain an acidic group, the degree of etherification may be calculated simply from the value of the total acid value. For example, when the acidic group is a carboxymethyl group and all of the acidic groups are neutralized as sodium salts, the degree of etherification can be calculated by the following formula: degree of etherification = (162 x total acid value) / (56100 - 80 x total acid value). The unit of the total acid number is mgKOH / g.
[0039] The water-soluble polymer preferably has an acidic group and a salt of the acidic group. The acidic group is preferably a salt of the acidic group that is converted into a free acidic group by treating a part of the salt of the acidic group with an acid. The cation forming the salt of the acidic group is not particularly limited, but may be, for example, an alkali metal ion such as lithium, sodium, or potassium, or an alkaline earth metal ion such as magnesium or calcium. Among these, the cation forming the salt of the acidic group is preferably a sodium ion or a potassium ion.
[0040] When the water-soluble polymer has an acidic group and a salt of the acidic group, the molar ratio of the acidic group / salt of the acidic group is preferably 0.02 or more, more preferably 0.03 or more, even more preferably 0.04 or more, and preferably 0.8 or less, more preferably 0.7 or less, and even more preferably 0.6 or less. If the molar ratio of the acidic group / salt of the acidic group is within the above range, the gel strength of the liquid-absorbent resin is favorable.
[0041] The free acid value of the water-soluble polymer is preferably 4 mgKOH / g or more, more preferably 7 mgKOH / g or more, more preferably 60 mgKOH / g or less, more preferably 50 mgKOH / g or less, and even more preferably 25 mgKOH / g or less. The free acid value of the water-soluble polymer means the acid value measured only for the free acid groups possessed by the water-soluble polymer, and does not include the acid groups forming salts. If the free acid value is 4 mgKOH / g or more and 60 mgKOH / g or less, the liquid absorbing performance of the absorbent resin becomes even better.
[0042] The dispersity (weight average molecular weight / number average molecular weight) of the water-soluble polymer is not particularly limited, but is preferably 5 to 110, and more preferably 7 to 70. If the dispersity is 5 or more and 110 or less, the liquid absorbing performance of the absorbent resin becomes better. The number average molecular weight of the water-soluble polymer can be determined based on a calibration curve of molecular weight and elution time prepared by aqueous size exclusion chromatography using pullulan with a known molecular weight.
[0043] <Cross-linked structure of liquid-absorbent resin> Generally, water-absorbent resins that have polyacrylic acid as the main structural unit have a network structure formed by covalent bonds, and form a chemical gel by absorbing water. In contrast, the liquid-absorbent resin used in the present invention is characterized by forming a physical gel by absorbing water. Since the crosslinking points of a physical gel disappear relatively easily due to thermal motion of molecular chains or changes in pH or ionic strength, and the physical gel can be converted into a sol with fluidity, it is easily decomposed by adding alkali or acid, heating, shaking, etc., which leads to a reduction in the environmental load when it is disposed of.
[0044] The formation of a physical gel can be confirmed by confirming the sol-gel transition caused by the disappearance of the crosslinking points. For example, when crosslinking is caused by ionic bonds and / or hydrogen bonds, it can be confirmed by fluidization after alkali or acid treatment. Specifically, when the absorbent resin is suspended in a 1% aqueous sodium hydroxide solution to a final concentration of 5% by weight, stirred for 60 minutes, and then sieved through a sieve with an opening of 500 μm, it can be determined that the physical gel formed by absorbing water has transitioned to a sol when the dry weight of the absorbent resin remaining on the sieve is less than 2% by weight of the dry weight of the absorbent resin contained in the aqueous solution.
[0045] More specifically, 0.5 g of the absorbent resin is suspended in 9.5 g of 1% sodium hydroxide aqueous solution and stirred for 60 minutes, then naturally filtered through a 30-mesh wire screen (500 μm mesh size) of about 50 mm × 50 mm square, and the mesh is washed with ion-exchanged water. After washing, the wire screen is dried for 2 hours in a 120 ° C. blower dryer. When the weight of the wire screen before filtration is Wm1 and the weight of the wire screen after filtration and drying is Wm2, it can be determined that the physical gel formed by absorbing water has transitioned to a sol when the 30-mesh pass residue calculated by the following formula is less than 2 wt%. The 500 μm mesh screen is a 30-mesh screen specified by JIS. 30 mesh pass residue (%) = (Wm2-Wm1) / 0.5 x 100 The 30 mesh pass residue is preferably less than 2% by weight, more preferably less than 1.5% by weight, even more preferably less than 1.0% by weight, and even more preferably less than 0.5% by weight.
[0046] The absorbent resin is a crosslinked product of the water-soluble polymer described above. The crosslinking is composed of internal crosslinking and, optionally, surface crosslinking. However, it is preferable that the absorbent resin does not have an internal crosslinking structure via an ether bond or an ester bond. Furthermore, it is preferable that the absorbent resin does not have an internal crosslinking structure via a covalent bond. In addition to an ester bond and an ether bond, the covalent bond may be a carbon-carbon covalent bond or a double bond. Examples of the internal crosslinking structure constituting the absorbent resin include an ionic bond between an acidic group on the water-soluble polymer and a neutralized acidic group, an ionic bond with a compound having an opposite charge to the water-soluble polymer (a compound containing a basic group such as a cationic group or an amino group when the acidic group of the water-soluble polymer is a carboxylic acid), an ionic bond by a divalent alkali metal ion, a coordinate bond via a metal ion, and a hydrogen bond such as dimerization of a carboxylic acid when the acidic group is a carboxylic acid group. The method of forming a surface crosslinking will be described later.
[0047] The absorbent resin may optionally contain a constituent unit other than the water-soluble polymer. Examples of the constituent unit other than the water-soluble polymer include compounds having an opposite charge to the water-soluble polymer, such as a polymer having an amino group, such as chitosan, polyethyleneimine, vinylpyrrolidone-N,N-dimethylaminoethyl methacrylic acid copolymer, or a salt thereof, a polymer having a quaternary ammonium group, such as dimethylamine-epichlorohydrin copolymer, or polydiallyldimethylammonium chloride. When the absorbent resin contains a constituent unit other than the water-soluble polymer, the content of the constituent unit is preferably 90% by weight or less, more preferably 50% by weight or less, based on the total amount of the water-soluble polymer used as the main component.
[0048] <Physical properties of liquid-absorbent resin> The physical properties of the liquid-absorbent resin used in the present invention will be described below.
[0049] <Water absorption rate of ion-exchanged water without pressure> The absorbency of the absorbent resin used in the present invention without pressure is determined by measuring the absorbency of physiological saline or ion-exchanged water when no load is applied to the absorbent resin by the method described in the Examples. The absorbent resin used in the present invention, in a solid state, has an absorbency of ion-exchanged water without pressure of preferably 20 g / g or more, more preferably 50 g / g or more, and even more preferably 100 g / g or more, and preferably 1000 g / g or less, more preferably 800 g / g or less, and even more preferably 500 g / g or less.
[0050] <Saline absorption rate without pressure> The absorbent resin used in the present invention preferably has an absorption capacity for physiological saline without load of 10 g / g or more, more preferably 20 g / g or more, and preferably 70 g / g or less, more preferably 65 g / g or less.
[0051] The ratio (A / B) of the absorbency (A) of ion-exchanged water under no pressure to the absorbency (B) of physiological saline under no pressure of the absorbent resin used in the present invention is preferably 7 or less, more preferably 5 or less.
[0052] <Water retention rate of ion-exchanged water> The water retention rate of the absorbent resin used in the present invention can be determined by measuring the absorbency of physiological saline or ion-exchanged water when a load of 150 G is applied to the absorbent resin by the method described in the Examples. The absorbent resin used in the present invention, in a solid state, preferably has a water retention rate for ion-exchanged water of 15 g / g or more, more preferably 25 g / g or more, and even more preferably 50 g / g or more, and preferably 900 g / g or less, more preferably 700 g / g or less, and even more preferably 450 g / g or less.
[0053] <Water retention rate of saline solution> In addition, the absorbent resin used in the present invention preferably has a saline water retention capacity of 5 g / g or more, more preferably 10 g / g or more, even more preferably 15 g / g or more, and preferably 60 g / g or less.
[0054] <Absorption amount of 50% by mass isopropyl alcohol aqueous solution> The absorbent resin used in the present invention preferably has an absorption amount of 50% by mass of isopropyl alcohol aqueous solution of 20 g / g or more, more preferably has an absorption amount of 50 g / g or more, even more preferably has an absorption amount of 100 g / g or more, preferably has an absorption amount of 1000 g / g or less, more preferably has an absorption amount of 750 g / g or less, and even more preferably has an absorption amount of 500 g / g or less. If the absorption amount of the 50% by mass of isopropyl alcohol aqueous solution of the absorbent resin is within the above range, it can absorb various liquid organic compounds, and the function of the liquid organic compound contained in the composition of the present invention is easily exhibited.
[0055] <Water retention rate of 50% by mass isopropyl alcohol aqueous solution> The water retention rate of the 50% by mass isopropyl alcohol aqueous solution of the absorbent resin used in the present invention is preferably 15 g / g or more, more preferably 40 g / g or more, even more preferably 80 g / g or more, preferably 900 g / g or less, more preferably 600 g / g or less, and even more preferably 350 g / g or less. If the water retention rate of the 50% by mass isopropyl alcohol aqueous solution of the absorbent resin is within the above range, it can absorb various liquid organic compounds, and the function of the liquid organic compound contained in the composition of the present invention is easily exhibited.
[0056] <Method of manufacturing liquid-absorbent resin> The method for producing the liquid-absorbent resin used in the present invention is, for example, A first step of forming a salt of an acidic group in a polysaccharide or a partial hydrolyzate thereof; It is preferable to have a second step of treating at least a portion of the salt of the acidic group with an acid to convert it into an acidic group, thereby preparing a water-soluble polymer having an acidic group and / or a salt thereof introduced therein, and a third step of crosslinking the water-soluble polymer having an acidic group and / or a salt thereof introduced therein to prepare an absorbent resin.
[0057] When only the salt of the acidic group is introduced into the polysaccharide or its partial hydrolysis product, the second step of converting the salt of the acidic group into an acid can be omitted. In addition, in the second step, all or a part of the salt of the acidic group may be treated with an acid to convert it into a free acidic group, and then all or a part of the acidic group may be neutralized with an alkali to convert it into a salt. This step is useful when converting the cationic species of the salt of the acidic group into another cationic species. For example, when the salt of the acidic group is a sodium carboxylate, all or a part of the salt of the acidic group can be converted into a potassium salt by converting it into a free acidic group by acid treatment and then neutralizing it with potassium hydroxide. When only the acidic group is introduced into the polysaccharide or its partial hydrolysis product, it is preferable to convert all of the salt of the acidic group into a free acidic group in the second step by treating it with an acid.
[0058] Another method for producing the liquid-absorbent resin used in the present invention is, for example, A first step of forming an acidic group on a polysaccharide or a partial hydrolysis product thereof; It is preferable that the method comprises a second step of treating at least a portion of the acidic groups with an alkali to convert them into salts of the acidic groups, thereby preparing a water-soluble polymer having acidic groups and / or salts of the acidic groups introduced therein, and a third step of crosslinking the water-soluble polymer having acidic groups and / or salts thereof introduced therein to prepare an absorbent resin.
[0059] When only acidic groups are introduced into the polysaccharide or its partial hydrolyzate, the second step of converting the acidic groups into their salts can be omitted. When only salts of acidic groups are introduced into the polysaccharide or its partial hydrolyzate, it is preferable to convert all of the acidic groups into salts of the acidic groups in the second step by treating them with an alkali.
[0060] The step of forming a salt of an acidic group in a polysaccharide or a partial hydrolysis product thereof is preferably carried out by reacting the polysaccharide or a partial hydrolysis product thereof with an acidic group-containing compound or a precursor thereof under basic conditions.
[0061] Hereinafter, the method for producing the liquid-absorbent resin of the present invention will be described based on an embodiment in which starch or a partial hydrolyzate thereof is used as the polysaccharide or a partial hydrolyzate thereof.
[0062] The method for producing the absorbent resin used in the present invention preferably further includes a step of partially decomposing the polysaccharide. In the step of partially decomposing the starch, in many cases, the α-1,4-glucoside bond of the α-glucose molecule constituting the starch is decomposed, but the position and manner of decomposition are not limited. The decomposition method is not particularly limited, and includes methods of enzyme treatment, acid treatment, physical crushing, etc. These methods may be combined. The enzyme treatment may be performed after gelatinization of the starch, or may be performed simultaneously with gelatinization. As a method for performing the enzyme treatment after gelatinization of the starch, a method in which the starch is first suspended in water and heated to gelatinize it, and then an enzyme is added to perform an enzyme reaction is included. As a method for performing the enzyme treatment simultaneously with gelatinization of the starch, a method in which the starch is suspended in water, and the mixture to which the enzyme is added is heated within a temperature range in which the enzyme is not completely inactivated is included. Among these, it is preferable to perform the enzyme treatment while gelatinizing the starch by heating and kneading it at 70°C to 110°C.
[0063] When partial decomposition of starch is carried out by enzyme treatment, the enzyme to be used is not particularly limited as long as it can decompose starch, and may be either an exo-type enzyme or an endo-type enzyme. Specific examples of the enzyme include α-amylase, amylomaltase, cyclomaltodextrin glucanotransferase, 4-α-glucanotransferase, 4,6-α-glucanotransferase, neopullulanase, and amylopullulanase. These enzymes may be used in combination. The pH during the enzyme treatment is not particularly limited, but is preferably pH 5.0 to pH 7.0. The pH can be adjusted by adding hydrochloric acid, acetic acid, sodium hydroxide, potassium hydroxide, etc.
[0064] When the partial decomposition of starch is carried out by acid treatment, the acid to be used is not particularly limited as long as it can decompose starch, but specific examples include hydrochloric acid, sulfuric acid, oxalic acid, acetic acid, formic acid, trifluoroacetic acid, etc. The temperature during the acid treatment is preferably 150°C to 160°C.
[0065] When partial decomposition of starch is carried out by physical crushing, specific means include irradiation, shearing, grinding, high pressure treatment, ultrasonic waves, thermal decomposition, photolysis, and combinations thereof.
[0066] Starch or its partial hydrolyzates may be derivatives in which the hydrogen atoms of the hydroxyl groups of glucose units are replaced by functional groups (also called processed starch or chemically modified starch) or bleached starch. The position of the hydroxyl group where the hydrogen atom is replaced may be any of the 1st, 2nd, 3rd, 4th, and 6th positions of the glucose unit, but the 2nd, 3rd, and 6th positions are preferred. Examples of functional groups include hydrocarbon groups such as methyl and ethyl groups; substituents having a hydroxyl group such as hydroxypropyl and hydroxyethyl groups; and substituents having a carboxyl group such as carboxymethyl groups. Examples of derivatives of starch or its partial hydrolysis products include acetylated adipate crosslinked starch, acetylated phosphate crosslinked starch, acetylated oxidized starch, sodium octenyl succinate starch, starch acetate, oxidized starch, hydroxypropyl starch, hydroxypropyl phosphate crosslinked starch, phosphate monoesterified phosphate crosslinked starch, phosphorylated starch, phosphate crosslinked starch, cationic starch, urea phosphate esterified starch, etc., which are used in food and industrial applications and are known as processed starches. Methylethylated starch and hydroxypropylmethylated starch substituted with two or more functional groups can also be used. Among these, starch acetate, oxidized starch, hydroxypropyl starch, and sodium octenyl succinate starch are preferred because of the ease of controlling the properties of the liquid-absorbing resin.
[0067] When the starch or a partial hydrolyzate thereof is a derivative in which the hydrogen atom of the hydroxyl group of the glucose unit is substituted with an acidic group, it is preferable to further carry out a step of introducing an acidic group and / or a salt thereof.
[0068] In the step of introducing an acidic group and / or its salt, starch or a partial starch hydrolyzate is reacted with an acidic group-containing compound or its precursor. This reaction introduces an acidic group and / or its salt to the hydroxyl group of the starch or partial starch hydrolyzate. The acidic group-containing compound is not particularly limited as long as it can introduce the above-mentioned acidic group and / or its salt, and examples thereof include haloalkyl compounds having an acidic group, haloalkenyl compounds having an acidic group, acid anhydrides, and salts thereof. Examples of halogens constituting the haloalkyl compounds and haloalkenyl compounds include chlorine and bromine.
[0069] Specific examples of the acidic group-containing compound include monochloroacetic acid, monobromoacetic acid, 3-bromopropionic acid, 6-bromohexanoic acid, succinic anhydride, maleic anhydride, vinylsulfonic acid, phosphorus oxychloride, ethyl monochloroacetate, and sodium and potassium salts thereof. Specific examples of the salts include sodium monochloroacetate, potassium monochloroacetate, and sodium vinylsulfonate.
[0070] Examples of the precursor of the acidic group-containing compound include acrylonitrile, etc. As a method using acrylonitrile, for example, first, acrylonitrile is reacted with starch or a partial decomposition product thereof under basic conditions to introduce a cyanoethyl group, and the cyanoethyl group is converted to an amide group (Synthesis; 1989(12):949-950), and the obtained amide is then subjected to alkaline hydrolysis.
[0071] The outline of the reaction for producing a water-soluble polymer by reacting starch or a partial starch hydrolysate with monochloroacetic acid is shown in formula (I). [ka]
[0072] The outline of the reaction of starch or a partial starch hydrolysate with 3-bromopropionic acid to produce a water-soluble polymer is shown in formula (II). [ka]
[0073] The outline of the reaction of starch or a partial starch hydrolysate with 6-bromohexanoic acid to produce a water-soluble polymer is shown in formula (III). [ka]
[0074] The reaction scheme for producing a water-soluble polymer by reacting starch or a partial starch hydrolysate with succinic anhydride is shown in formula (IV). [ka]
[0075] The outline of the reaction for producing a water-soluble polymer by reacting starch or a partial starch hydrolysate with maleic anhydride is shown in formula (V). [ka]
[0076] The reaction scheme for producing a water-soluble polymer by reacting starch or a partial starch hydrolyzate with sodium vinyl sulfonate is shown in formula (VI). [ka]
[0077] Although the formulae (I) to (VI) show water-soluble polymers in which sodium salts of acidic groups have been introduced into all hydroxyl groups at the 6-position of glucose units, hydroxyl groups to which no acidic group has been introduced may remain. Also, acidic groups that have not been neutralized by salts may exist. The position at which the acidic group is introduced is not limited as long as it is a hydroxyl group present in starch or a partial starch hydrolyzate, and may be any of the 1-, 2-, 3-, 4-, and 6-position hydroxyl groups.
[0078] When a haloalkyl compound or a haloalkenyl compound is used as the acidic group-containing compound, it is preferable to use 1 to 1.5 molar equivalents of an alkaline agent per mole of the haloalkyl compound or haloalkenyl compound. Examples of the alkaline agent include sodium hydroxide, potassium hydroxide, lithium hydroxide, ammonia, sodium carbonate, and potassium carbonate. The acidic group introduced into starch or a partial hydrolyzate of starch preferably forms a salt with sodium, potassium, lithium, ammonia, etc. derived from the alkaline agent, and for this reason, it is preferable to use an amount of the alkaline agent that is necessary for both the reaction of the haloalkyl compound or the haloalkenyl compound with the starch or its partial hydrolyzate and the neutralization of the acidic group of the haloalkyl compound or the haloalkenyl compound. For example, when chloroacetic acid is used as the acidic group-containing compound, it is theoretically preferable to use 2 molar equivalents or more of the alkaline agent per mole of chloroacetic acid. When sodium chloroacetate is used, since the acidic group is neutralized in advance, it is preferable to use 1 molar equivalent or more of the alkaline agent per mole of sodium chloroacetate.
[0079] The amount of the acidic group-containing compound used can be set arbitrarily according to the desired total acid value (degree of etherification) of the water-soluble polymer. Usually, 0.5 to 5.0 molar equivalents are preferred, and 0.5 to 2 molar equivalents are more preferred, per mole of hydroxyl group of starch or partial starch hydrolysate. When reacting as an aqueous solution using a haloalkyl compound such as chloroacetic acid, the introduction reaction of the acidic group and the hydrolysis reaction of the haloalkyl compound compete with each other, so that the haloalkyl compound is required in excess of the theoretical amount. The amount of the haloalkyl compound used in the aqueous solution reaction is preferably set to 5 molar equivalents or less relative to the theoretical value.
[0080] The reaction temperature between starch or starch partial hydrolyzate and an acidic group-containing compound is not particularly limited, but is preferably 0°C to 120°C. The reaction time is not particularly limited, but is preferably 1 hour to 24 hours. The reaction may be carried out in water, or in a mixed solvent of water and alcohols such as methanol, ethanol, isopropanol, butanol, ethylene glycol, diethylene glycol, propylene glycol, and ethylene glycol monoethyl ether, and glycol ethers such as ethylene glycol dimethyl ether, or by dispersing the dried starch partial hydrolyzate powder in a hydrophilic solvent such as alcohols such as methanol, ethanol, isopropanol, and butanol, and glycol ethers such as ethylene glycol dimethyl ether. When a mixed solvent is used, the proportion of the solvent other than water in the mixed solvent is preferably 50% by volume or less. A reaction kettle, an extruder, or the like can be used as a reaction apparatus.
[0081] When a haloalkyl compound such as chloroacetic acid or a salt thereof is used as the acidic group-containing compound, the reaction temperature with starch or a partial starch hydrolyzate is not particularly limited, but is preferably 0°C to 100°C.
[0082] In particular, when chloroacetic acid or a salt thereof is used as the haloalkyl compound, the reaction is preferably carried out at 25°C to 90°C to prevent hydrolysis by water in the reaction solution. The reaction time is preferably the time until the raw material haloalkyl compound is consumed, and more preferably 1 hour to 12 hours for the stability of the haloalkyl compound and the efficiency of the process. The reaction may be carried out in water, or in a mixed solvent of water and alcohols such as methanol, ethanol, isopropanol, butanol, and glycol ethers such as ethylene glycol dimethyl ether, or by dispersing the powder of the dried starch partial hydrolyzate in a hydrophilic solvent such as alcohols such as methanol, ethanol, isopropanol, butanol, and glycol ethers such as ethylene glycol dimethyl ether. When a mixed solvent is used, the proportion of the solvent other than water is preferably 50% by volume or less in the mixed solvent. A reaction kettle, an extruder, or the like can be used as the reaction apparatus.
[0083] In addition, when an acid anhydride is used as the acid group-containing compound, the reaction proceeds simply by mixing the starch partial hydrolyzate with the acid anhydride and heating it, but in order to promote the reaction, a catalyst such as sodium carbonate, sodium hydroxide, tertiary amines such as triethylamine, imidazoles such as 2-methylimidazole, quaternary ammonium salts such as tetrabutylammonium bromide, or phosphonium salts such as tetrabutylphosphonium bromide may be used. The amount of these catalysts added is preferably 0.1 molar equivalents or less per mole of the acid group-containing compound. These catalysts may be used alone or in combination of two or more.
[0084] The reaction time is preferably the time until the raw material acid anhydride is consumed, and more preferably 1 to 12 hours. The end point of the reaction can be determined by acid value measurement or IR measurement. The reaction may be carried out in water, but in order to prevent hydrolysis or alcoholysis of the acid anhydride, the reaction solvent is preferably an aprotic solvent such as dimethylsulfoxide, dimethylformamide, dimethylacetamide, or N-methylpyrrolidone. When a mixed solvent is used, the ratio of the solvent other than water is preferably 50% by volume or more in the mixed solvent. When the reaction is carried out without a solvent, the acid anhydride can play the role of a solvent, so that the reaction temperature is preferably at or above the melting point of the acid anhydride. When a solvent is used in the reaction, the reaction temperature is preferably 50°C to 100°C, more preferably 70°C to 90°C. As the reaction apparatus, a reaction kettle, an extruder, or the like can be used.
[0085] It is preferable to neutralize a part of the salt of the acidic group added to the starch or the partial starch hydrolyzate. By neutralization, a part of the acidic groups that formed salts are converted to free acidic groups. For example, when monochloroacetic acid is used as the above-mentioned acidic group-containing compound and sodium hydroxide is used as the alkaline agent, a sodium salt of the carboxyl group is added to the starch or the partial starch hydrolyzate. By adding an acid to this, a part of the carboxyl group is converted to a free carboxylic acid.
[0086] The ratio of the salt of the acidic group converted to a free acidic group by neutralization (acid treatment) is, for example, preferably 2 mol % or more, more preferably 3 mol % or more, preferably 80 mol % or less, and even more preferably 70 mol % or less, based on 100 mol % of the salt of the acidic group. This is because, if the ratio of the salt of the acidic group converted to a free acidic group is within the above range, a liquid-absorbent resin having a preferable gel strength can be obtained.
[0087] The acid used for neutralization is not particularly limited, but when the acidic group is a carboxyl group, an acid having a pKa equal to or lower than that of the carboxyl group is preferred, and examples of such acids include hydrochloric acid, sulfuric acid, phosphoric acid, nitric acid, acetic acid, formic acid, and trichloroacetic acid. For neutralization of a sulfo group or a phospho group, a strong acid is preferably used, and a mineral acid such as hydrochloric acid or sulfuric acid, or a strongly acidic ion exchange resin is used. The neutralization can be carried out using a known device such as a reaction kettle or an extruder. After the addition of the acid, it is preferable to stir the mixture at 0°C to 50°C for 0.2 to 1 hour for the neutralization reaction. The neutralization reaction is preferably carried out under conditions of pH 6.8 to 7.2.
[0088] In the step of introducing a salt of an acidic group or the subsequent neutralization reaction (acid treatment), a salt may be formed between a halogen derived from an acidic group-containing compound and a metal or ammonia derived from an alkaline agent, so it is preferable to perform desalting. As a desalting method, a method is exemplified in which a water-soluble polymer is dissolved in water to obtain an aqueous solution, which is dropped into a hydrophilic solvent such as methanol, ethanol, isopropanol, acetone, or acetonitrile, and the water-soluble polymer is reprecipitated and recovered by filtration, and then the water-soluble polymer recovered by filtration is dispersed again in aqueous methanol (water content of about 70 to 90%), stirred, and then washed by a process of recovering the water-soluble polymer particles by filtration. As a desalting method, a method is exemplified in which an aqueous solution of a hydrophilic polymer is treated with a filter having an ultrafiltration membrane. As a washing liquid for desalting, water or a mixture of water and a hydrophilic organic solvent such as methanol, ethanol, propanol, acetone, or acetonitrile can be used. It is preferable to perform desalting until the salt concentration in the water-soluble polymer becomes 1% or less.
[0089] In the step of forming an internal crosslinked structure, the water-soluble polymers are crosslinked with each other. The crosslinking can be formed without using a crosslinking agent, for example, by a method of heating and drying a water-soluble polymer in which some of the acidic groups are free acid groups under a water-containing condition. The temperature during the heating and drying is preferably 50°C to 150°C, more preferably 60°C to 130°C. The pressure during the heating and drying is not particularly limited, and can be performed at normal pressure, specifically, preferably 0.9 atm to 1.1 atm. The drying method is not particularly limited, and can be performed using a drum dryer, spray dryer, Nauta mixer, etc.
[0090] During the heat drying, the water-soluble polymer may contain a hydrophilic solvent in addition to water. Examples of the hydrophilic solvent include lower aliphatic alcohols such as methanol, ethanol, n-propanol, and isopropanol; ketones such as acetone; ethers such as dioxane, tetrahydrofuran, and methoxy(poly)ethylene glycol; and amides such as ε-caprolactam and N,N-dimethylformamide. The ratio of the hydrophilic solvent other than water in the total solvent is preferably adjusted according to the boiling point of the solvent. When the boiling point of the solvent is 100° C. or less, it is preferably 70% by volume or more, and when it exceeds 100° C., it is preferably 30% by volume or less. In addition, the water-soluble polymer at the start of the heat drying may be an aqueous solution or a powder containing a water-containing solvent having a water content of 1% by weight or more. When drying a powder containing a water-containing solvent, the wet ratio in the powder at the start of the drying is preferably 1% by mass to 85% by mass, more preferably 20% by mass to 80% by mass, and even more preferably 55% by mass to 75% by mass. The wet ratio here refers to the ratio of the total amount of water and hydrophilic solvent in the powder.
[0091] The water-soluble polymer is crosslinked by heating and drying to obtain a liquid-absorbent resin. The residual ratio of water and the hydrophilic solvent used in preparing the water-soluble polymer in the liquid-absorbent resin is preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less.
[0092] The obtained liquid-absorbent resin is preferably pulverized into particles, which improves processability.
[0093] In the production of the absorbent resin, surface cross-linking may be performed in addition to internal cross-linking. Surface cross-linking can improve the strength of the absorbent resin. Examples of cross-linking agents used for surface cross-linking include epoxy compounds, polyhydric alcohol compounds, polyamine compounds, polyisocyanate compounds, alkylene carbonate compounds, haloepoxy compounds, halohydrin compounds, polyvalent oxazoline compounds, carbodiimide compounds, silane coupling agents, and polyvalent metal compounds.
[0094] Examples of the epoxy compound include succinic acid glycidyl ester, sorbitol polyglycidyl ether, trimethylolpropane polyglycidyl ether, polyethylene glycol diglycidyl ether, glycerol polyglycidyl ether, diglycerol polyglycidyl ether, polyglycerol polyglycidyl ether, propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, and glycidol.
[0095] Examples of the polyhydric alcohol compound include ethylene glycol, diethylene glycol, propylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, 1,3-propanediol, dipropylene glycol, 2,2,4-trimethyl-1,3-pentanediol, polypropylene glycol, glycerin, polyglycerin, 2-butene-1,4-diol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,2-cyclohexanedimethanol, 1,2-cyclohexanediol, trimethylolpropane, diethanolamine, triethanolamine, polyoxypropylene, oxyethylene-oxypropylene block copolymer, pentaerythritol, and sorbitol.
[0096] Examples of the polyvalent amine compound include ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, polyethyleneimine, inorganic salts or organic salts (such as azithinium salts) of these polyvalent amine compounds, and the like.
[0097] Examples of the polyisocyanate compound include 2,4-tolylene diisocyanate and hexamethylene diisocyanate, and examples of the polyoxazoline compound include 1,2-ethylenebisoxazoline.
[0098] Examples of the alkylene carbonate compound include 1,3-dioxolan-2-one, 4-methyl-1,3-dioxolan-2-one, 4,5-dimethyl-1,3-dioxolan-2-one, 4,4-dimethyl-1,3-dioxolan-2-one, 4-ethyl-1,3-dioxolan-2-one, 4-hydroxymethyl-1,3-dioxolan-2-one, 1,3-dioxan-2-one, 4-methyl-1,3-dioxan-2-one, and 4,6-dimethyl-1,3-dioxan-2-one.
[0099] Examples of the haloepoxy compound include epichlorohydrin, epibromohydrin, α-methylepichlorohydrin, and polyamine adducts thereof (eg, Kaimen (registered trademark) manufactured by Hercules Corporation).
[0100] Other known crosslinking agents that can be used include aqueous carbodiimide compounds (e.g., Carbodilite manufactured by Nisshinbo Chemical Inc.), silane coupling agents such as γ-glycidoxypropyltrimethoxysilane and γ-aminopropyltriethoxysilane, and polyvalent metal compounds such as hydroxides and chlorides of zinc, calcium, magnesium, aluminum, iron, zirconium, etc.
[0101] Among these, epoxy compounds are preferred, and ethylene glycol diglycidyl ether, sorbitol polyglycidyl ether, and succinic acid glycidyl ester are more preferred.
[0102] The surface crosslinking can be formed by spraying a surface crosslinking agent onto the absorbent resin, mixing the resin by a known method using a cylindrical mixer, a V-shaped mixer, a ribbon mixer, a screw mixer, a double-arm mixer, a grinding kneader, etc. During the spraying and mixing, a surfactant can be added as necessary.
[0103] The absorbent resin can be decomposed by alkali treatment. During the alkali treatment, the absorbent resin is preferably kept at a pH of 9.0 or higher, more preferably at a pH of 10.0 or higher. The alkali treatment cleaves the crosslinked structure and glycoside bonds of the absorbent resin, decomposing it into a water-soluble polymer, thereby reducing the environmental load at the time of disposal.
[0104] The alkaline agent used in the alkaline treatment is not particularly limited, but examples thereof include sodium hydroxide, potassium hydroxide, lithium hydroxide, ammonia, sodium carbonate, potassium carbonate, etc. The temperature during the alkaline treatment is not particularly limited, but the treatment can be carried out under conditions of, for example, 5 to 50°C.
[0105] <Water, liquid organic compounds> The composition of the present invention contains, in addition to the liquid-absorbent resin, water and a liquid organic compound.
[0106] The liquid organic compound is preferably an alcoholic compound having a hydroxyl group.
[0107] Examples of the liquid organic compound include monohydric alcohols such as methanol, ethanol, n-propanol, isopropanol, butanol, pentyl alcohol, hexyl alcohol, heptyl alcohol, octyl alcohol, and decyl alcohol; dihydric alcohols such as ethylene glycol, propylene glycol, butanediol, 1,3-butylene glycol, pentanediol, hexanediol, heptanediol, octanediol, decanediol, diethylene glycol, and dipropylene glycol; trihydric alcohols such as glycerin and trimethylolpropane; and lactic acid.
[0108] In the composition of the present invention, water and a liquid organic compound are preferably absorbed in the absorbent resin, and more preferably, the liquid organic compound and water are absorbed in the absorbent resin as a mixed solvent. The absorbent resin used in the present invention is difficult to absorb only a large amount of a liquid organic compound. Therefore, for example, it is difficult to make the absorbent resin absorb water first and then absorb only a large amount of a liquid organic compound, or to make the absorbent resin absorb only a large amount of a liquid organic compound first and then absorb water.
[0109] The liquid organic compound is preferably a polar solvent, because it has high miscibility with water. The liquid organic compound is preferably one that is miscible with water at any ratio, but one that is not miscible with water at any ratio can also be used, and in this case, the solubility in water (25°C) is preferably 0.1 g / mL or more, more preferably 0.5 g / mL or more, and even more preferably 1 g / mL or more.
[0110] The content of the liquid organic compound in the mixed solvent of the liquid organic compound and water is preferably 10% by mass or more, preferably 40% by mass or more, more preferably 50% by mass or more, and is preferably 90% by mass or less, more preferably 80% by mass or less, even more preferably 70% by mass or less, and particularly preferably 60% by mass or less.
[0111] In the composition of the present invention, the amount of the liquid organic compound absorbed per 1 g of the liquid-absorbent resin is preferably 1 g or more, more preferably 3 g or more, even more preferably 5 g or more, and preferably 300 g or less, more preferably 250 g or less, and even more preferably 200 g or less. If the content of the liquid organic compound in the liquid-absorbent resin is within the above range, the function of the liquid organic compound contained in the composition of the present invention is easily exhibited.
[0112] <Uses of the composition of the present invention> The composition of the present invention can be used for cosmetics, hygiene products, medical products, civil engineering products, food preservation products, agricultural and horticultural products, and the like.
[0113] Since the composition of the present invention is capable of absorbing and retaining liquids containing proteins, it can be used in hygiene and medical applications to absorb and retain not only urine but also blood, menstrual blood, breast milk, and other fluids containing proteins. Specific hygiene products include paper diapers, sanitary products, incontinence pads, breast milk pads, masks for packs, portable toilets, pet toilets, cat litter, etc. Medical products include hemostatic sponges (medical pads), wound protection materials, wound healing materials, medical waste solidification agents, ice packs, carriers for drug delivery systems, artificial joints, and compresses.
[0114] Food preservation products include ice packs, cooling gels, water retention materials, condensation prevention sheets, drip absorbents, and freshness preserving agents.
[0115] Civil engineering products include waterproofing materials, waste liquid solidification agents, surplus soil solidification agents, and construction materials for preventing condensation.
[0116] Examples of agricultural and horticultural products include soil conditioners, soil water retention materials, seedling pots, seedbeds, hydroponic cultivation supports, fertilizer retention materials, and fertilizer sustained release agents.
[0117] Other uses include as an air freshener, disposable warmer, portable toilet, thickener for cosmetics, etc.
[0118] The composition of the present invention can be endowed with functions such as antibacterial properties, moisturizing properties, and fragrance by using a compound having antibacterial properties, moisturizing properties, and fragrance as the liquid organic compound.
[0119] Examples of antibacterial liquid organic compounds include methanol, ethanol, propanol, isopropanol, butanol, isobutanol, tertiary butanol, 1,3-butylene glycol, 1,2-pentanediol, 1,2-hexanediol, 1,2-octanediol, benzyl alcohol, phenylethanol, phenylpropanol, phenylbutanol, phenylpentanol, phenylhexanol, and phenoxyethanol.
[0120] Examples of liquid organic compounds having moisturizing properties include glycerin, diglycerin, triglycerin, polyglycerin, 3-methyl-1,3-butanediol (isopropylene glycol), 1,3-butylene glycol, isoprene glycol, polyethylene glycol, 1,2-pentanediol, 1,2-hexanediol, propylene glycol, dipropylene glycol, polypropylene glycol, ethylene glycol, diethylene glycol, triethylene glycol, pentaerythritol, and neopentyl glycol.
[0121] The composition of the present invention can be suitably used for cosmetic applications. Cosmetics contain the above-mentioned compounds to enhance antibacterial and moisturizing effects. The composition of the present invention can be absorbed with such compounds and water and then incorporated into the cosmetics.
[0122] When a cosmetic product containing the composition of the present invention is applied to the skin, the liquid organic compound having a high moisturizing effect can be retained, thereby enhancing the moisturizing effect.
[0123] Specific examples of the cosmetic product include emulsions, creams, lotions, packs, cleansers, makeup cosmetics, scalp and hair products, dispersions, ointments, liquids, aerosols, patches, poultices, liniments, oils, lipsticks, lipsticks, foundations, eyeliners, blushers, mascara, eye shadows, soaps (hand soaps, body soaps, facial cleansers), and the like.
[0124] The composition of the present invention can be used, for example, by coating on a support, laminating on a support, carrying on a support, or impregnating into a support.
[0125] Examples of the support include paper, fabrics such as woven or knitted fabrics, nonwoven fabrics, sheets, films, and porous bodies. The shape of the support is not particularly limited, but is preferably a sheet. Examples of the sheet-like support include paper, fabrics such as woven or knitted fabrics, nonwoven fabrics, sheets, films, and porous sheets.
[0126] Generally, the term "film" refers to a thin, flat product whose thickness is extremely small compared to its length and width, and whose maximum thickness is arbitrarily limited, and which is usually supplied in the form of a roll (Japanese Industrial Standard JIS K6900). For example, in terms of thickness, a product with a thickness of 100 μm or more is referred to as a sheet in the narrow sense, and a product with a thickness of less than 100 μm is referred to as a film. In the present invention, unless otherwise defined, "sheet" includes "film".
[0127] The thickness of the sheet-like support is not particularly limited and may be appropriately set depending on the application. For example, the thickness is preferably 0.1 mm or more, more preferably 1 mm or more, and is preferably 50 mm or less, more preferably 30 mm or less.
[0128] Examples of resins that may be used to make up the sheet or film include polyesters such as polyethylene terephthalate and polyethylene naphthalate; polycarbonate; poly(meth)acrylate; polystyrene; polyamide; polyacrylonitrile; polyolefins such as polypropylene, polyethylene, and polycycloolefin; polyphenylene sulfide; polyimide; polyvinyl chloride; polyvinylidene chloride; polyurethane, polyvinyl alcohol, and the like.
[0129] Examples of the paper support include crepe paper, absorbent paper, tissue paper, sanitary paper, etc., and include papers made mainly from plant fibers (e.g., pulp). Specifically, tissue is preferred, but is not limited thereto.
[0130] The fibers constituting the woven or knitted fabric may be either natural or synthetic. Examples of the natural fibers include plant fibers such as cotton and hemp, and animal fibers such as silk, wool, and other animal hair. Examples of the synthetic fibers include polyolefin fibers, polyester fibers, and polyamide fibers.
[0131] Examples of the nonwoven fabric include point-bonded nonwoven fabric, air-through nonwoven fabric, spunlace nonwoven fabric, and spunbonded nonwoven fabric. Examples of the fibers forming these nonwoven fabrics include hydrophilic fibers such as cellulose, rayon, and cotton; hydrophobic fibers such as polypropylene, polyethylene, polyester, polyamide, and nylon; and hydrophobic fibers whose surfaces have been hydrophilized with a surfactant.
[0132] Examples of the porous body include a porous sheet and a porous inorganic material.
[0133] The porous sheet is not particularly limited as long as it is a sheet having pores, and examples thereof include a sheet in which pores are formed continuously, a sheet in which pores are formed discontinuously, etc. Examples of the resin forming the porous sheet include polyesters such as polyethylene terephthalate and polyethylene naphthalate, polycarbonates, poly(meth)acrylates, polystyrenes, polyamides, polyacrylonitriles, polyolefins such as polypropylene, polyethylene, and polycycloolefins, polyphenylene sulfide, polyimides, polyvinyl chloride, polyvinylidene chloride, and polyurethanes.
[0134] Examples of methods for producing a porous sheet include a balloon foaming method, a chemical foaming method, a supercritical carbon dioxide injection molding method, a salt extraction method, and a solvent removal method. In the balloon foaming method, microballoons are contained in a resin composition, and the microballoons are expanded by heating to form a foam. In the chemical foaming method, a foaming agent (e.g., azodicarbonamide, azobisisobutyronitrile, N,N-dinitrosopentamethylenetetramine, p-toluenesulfonylhydrazine, p-oxybis(benzenesulfohydrazide)) or a foaming assistant is contained in the resin composition, and gas (carbon dioxide gas, nitrogen gas, etc.) is generated by a chemical reaction to form a foam. In the supercritical carbon dioxide injection molding, carbon dioxide in a supercritical state under high pressure is impregnated into the resin composition, and the resin composition is injected under normal pressure, and the carbon dioxide is vaporized to form a foam. In the salt extraction method, a readily soluble salt (boric acid, calcium chloride, etc.) is contained in the resin composition, and the salt is dissolved and extracted after molding to form pores. In the solvent removal method, a solvent is added to the resin composition, and after molding, the solvent is removed to form pores.
[0135] The porous sheet is preferably a foamed sheet. The foamed sheet is not particularly limited as long as it is a sheet formed by foaming a resin, and examples of the foamed sheet include a polyolefin foamed sheet, a polyethylene foamed sheet, and a polyurethane foamed sheet.
[0136] Examples of the porous inorganic material include inorganic materials such as diatomaceous earth, zeolite, and perlite. Diatomaceous earth is mud formed when the remains of diatoms, a type of plankton, accumulate on the bottom of the sea or lake and become fossilized. Diatomaceous earth is mainly composed of silica, and each particle has many fine pores. Perlite is a porous body formed by subjecting glassy volcanic rocks such as obsidian, pearlite, and rosinite to high heat treatment to evaporate the water contained in the volcanic rocks. Zeolite is a crystalline porous aluminosilicate.
[0137] The present invention includes a functional sheet in which the composition of the present invention is applied to, carried on, laminated on, or impregnated in a sheet-like support. The functional sheet of the present invention can be suitably used as, for example, an antibacterial sheet, a cosmetic pack, a drip sheet for food, etc.
[0138] For example, an antibacterial sheet in which a composition containing an absorbent resin that has absorbed an antibacterial liquid organic compound or the like is applied to, supported on, laminated on, or impregnated into a sheet support makes it easy to wipe off dirt due to the liquid organic compound absorbed by the absorbent resin, and can also impart antibacterial properties after wiping.
[0139] In a cosmetic pack in which a composition containing a liquid-absorbent resin that has absorbed water and a liquid organic compound having a moisturizing effect is applied to, supported on, laminated on, or impregnated into a sheet-like support, the moisturizing liquid organic compound and water absorbed by the liquid-absorbent resin enhance the moisturizing effect on the skin.
[0140] In a food drip sheet in which a composition containing an absorbent resin that has absorbed an antibacterial liquid organic compound and water is supported on a sheet support, the liquid organic compound absorbed by the absorbent resin has the effect of prolonging the shelf life of food. EXAMPLES
[0141] The present invention will be described below with reference to examples, but the present invention is not limited to the following examples. In the following, "parts" and "%" mean "parts by weight" and "% by weight", respectively, unless otherwise specified.
[0142] <Evaluation method> (1) Total acid number of water-soluble polymer Here, a method for measuring the total acid value of a water-soluble polymer having a carboxymethyl group as an acidic group is described. Approximately 0.3 g of the water-soluble polymer was precisely weighed in a 100 ml beaker and dissolved in 40 ml of ion-exchanged water. This aqueous solution was set in a potentiometric titration device (AT-610 manufactured by Kyoto Electronics Manufacturing Co., Ltd.) equipped with a glass electrode (C-171 manufactured by Kyoto Electronics Manufacturing Co., Ltd.). If the sample is all sodium salts, the potential at this stage is approximately 30 mV or less, so 1N hydrochloric acid is added until the potential reaches 320 mV or more, and all the carboxylic acid groups in the water-soluble polymer are made into a state of free acid (a state of excess hydrochloric acid). After confirming that the potential is 320 mV or more, neutralization titration is performed with a 0.1 N NaOH aqueous solution. In this titration, two inflection points are detected, the first inflection point being detected near 220 mV and the second inflection point being detected near 0 mV to -30 mV. The former is the neutralization point of excess hydrochloric acid in the sample, and the latter is the neutralization point of carboxylic acid in the water-soluble polymer. Therefore, the total acid number is calculated by the following formula 1. Total acid number (mgKOH / g) = [{(Vb-Va) x 0.1 x fa x 56.11} ÷ Sa] / (1-wr) (Equation 1) Here, Va is the volume (ml) of 0.1N NaOH consumed up to the first inflection point, Vb is the volume (ml) of 0.1N NaOH consumed up to the second inflection point, fa is the titer of 0.1N NaOH, Sa is the amount of sample taken, and wr is the wet ratio of the water-soluble polymer measured by the method described below.
[0143] (2) Degree of etherification of water-soluble polymer The total acid number is calculated using the above total acid number according to the following formula 2. Degree of etherification = (162 x TAV) ÷ (56100 - 80 x TAV) (Equation 2) Here, TAV is the total acid number of the water-soluble polymer (unit: mgKOH / g).
[0144] (3) Free acid value of water-soluble polymer The free acid value is defined as the acid value when the crosslinking of the water-soluble polymer is carried out by acid treatment. In the examples, since the crosslinked polymer is produced continuously after the acid treatment, direct quantification by titration is difficult, so the value calculated by the following calculation is defined as the free acid value. In the acid treatment, the acid has a lower pKa than the carboxylic acid of the water-soluble polymer, so the amount of acid added during the acid treatment is essentially equal to the free acid value. Therefore, the free acid value is calculated by the following formula 3. Free acid value (mgKOH / g) = (Vc × N × fb × 56.11) ÷ Sb (Equation 3) Here, Vc is the volume (ml) of the aqueous acid solution used in the acid treatment, N is the normality of the aqueous acid solution, fb is the titer of the aqueous acid solution, and Sb is the weight (pure content) of the water-soluble polymer charged in the acid treatment.
[0145] (4) Wetting rate of water-soluble polymer The wet ratio refers to the percentage of weight loss relative to the initial weight of a sample when the sample is dried at a drying temperature of 130°C using a halogen moisture meter. In this example, 0.5 to 1.0 g of the water-soluble polymer was set in a halogen moisture meter HC103 manufactured by Mettler Toledo K.K., and measurements were taken at a drying temperature of 130°C, a switch-off standard of 1 mg / 50 seconds, and in %MC mode (a mode that displays MC value = (initial sample weight - dry weight) ÷ initial sample weight × 100). The displayed MC value was taken as the wet ratio.
[0146] (5) Absorption capacity of absorbent resin without pressure (saline solution) 1.0 g of the measurement sample was placed in a tea bag (20 cm long, 10 cm wide) made of nylon net with a mesh size of 63 μm (JIS Z8801-1:2006), and immersed in 1,000 ml of physiological saline (salt concentration 0.9% by weight) without stirring for 3 hours, then hung for 10 minutes to drain. The weight (h1) including the tea bag was measured, and the water retention capacity was calculated using the following formula. The temperature of the physiological saline used and the measurement atmosphere was 25°C ± 2°C. FSC(g / g)=(h1)-(h2) Here, (h2) is the weight of the tea bag measured in the same manner as above without a measurement sample. Here, FSC is an abbreviation for Free Swell Capacity, which means the free swelling capacity, and indicates the water absorption capacity without pressure.
[0147] (6) Absorption capacity of absorbent resin without pressure (ion-exchanged water) 0.2 g of the measurement sample was placed in the tea bag, and the weight (h1') including the tea bag after immersion was measured in the same manner as for the water absorption capacity under no pressure (saline solution), except that ion-exchanged water was used instead of saline solution, and the water retention capacity was calculated using the following formula. Note that (h2') is the weight of the tea bag measured using the same procedure as above, but without the measurement sample. FSC(g / g)={(h1´)-(h2´)} / 0.2
[0148] (7) Water retention rate of absorbent resin (saline solution) After measuring the water absorption capacity without pressure as described above, the tea bag was placed in a centrifuge and centrifuged at 150G for 90 seconds to remove excess liquid components. The weight (h3) including the tea bag was measured and the water retention capacity was calculated using the following formula. CRC(g / g)=(h3)-(h4) Here, (h4) is the weight of the tea bag measured in the same manner as above, except that no measurement sample is used. CRC is an abbreviation for Centrifuge Retention Capacity, which means the centrifuge retention capacity and indicates the water retention rate.
[0149] (8) Water retention rate of absorbent resin (ion-exchanged water) After measuring the water absorption capacity without pressure as described above, the tea bag was placed in a centrifuge and centrifuged at 150G for 90 seconds to remove excess liquid. The weight including the tea bag (h3´) was measured and the water retention capacity was calculated using the following formula. CRC(g / g)={(h3´)-(h4´)} / 0.2 Note that (h4') is the weight of the tea bag measured in the same manner as above, but without a measurement sample.
[0150] (5) Absorption capacity of absorbent resin without pressure (mixed solvent) 0.2 g of the measurement sample was placed in a tea bag (20 cm long, 10 cm wide) made of nylon net with an opening of 63 μm (JIS Z8801-1:2006), and immersed in 1,000 ml of mixed solvent without stirring for 1 hour, then hung for 10 minutes to drain. The weight (h1) including the tea bag was measured, and the absorbency was calculated using the following formula. The mixed solvent used and the temperature of the measurement atmosphere were 25°C ± 2°C. FSC(g / g)=(h1)-(h2) Here, (h2) is the weight of the tea bag measured in the same manner as above without a measurement sample. Here, FSC is an abbreviation for Free Swell Capacity, which means the free swelling capacity, and indicates the water absorption capacity without pressure.
[0151] (9) Water retention rate of absorbent resin (mixed solvent) After measuring the water absorption capacity without pressure as described above, the tea bag was placed in a centrifuge and centrifuged at 150G for 90 seconds to remove excess liquid components. The weight (h3) including the tea bag was measured and the water retention was calculated using the following formula. CRC(g / g)=(h3)-(h4) Here, (h4) is the weight of the tea bag measured in the same manner as above, except that no measurement sample is used. CRC is an abbreviation for Centrifuge Retention Capacity, which means the centrifuge retention capacity and indicates the water retention rate.
[0152] <Production Example> (1) Materials used (1-1) Starch raw material Cornstarch Waxy Cornstarch Tapioca
[0153] (1-2) Hydrolase α-Amylase (Spitase® HK / R, Nagase Chemtex Corp.), 12,200 units / g amylomaltase: Thermus thermophilus was aerobically cultured, the collected cells were crushed, and the extract was centrifuged, and the supernatant was used as a crude enzyme solution. The crude enzyme solution was subjected to column chromatography in the usual manner, and the sample was purified to an electrophoretically homogeneous state and used as a purified enzyme solution.
[0154] The activity of amylomaltase was measured by the following method. A reaction solution containing 10% by weight maltotriose, 50 mM sodium acetate buffer (pH 6.0), and the enzyme was incubated at 60°C for 20 minutes. The reaction was then stopped by heating at 100°C for 10 minutes. The amount of glucose in the reaction solution was measured by the glucose oxidase method. The unit amount of amylomaltase was defined as 1 unit of amylomaltase activity that produces 1 μmol of glucose per minute.
[0155] (2) Production of partial starch hydrolysates Partial starch hydrolysates were produced by the following method. The weight-average molecular weight of the obtained partial starch hydrolysates was determined by aqueous size exclusion chromatography based on a calibration curve of molecular weight and elution time prepared using pullulan with a known molecular weight. The weight-average molecular weight and dispersity of the partial starch hydrolysates are shown in Table 1.
[0156] (Production Example 1) Partially hydrolyzed starch derived from tapioca starch Tapioca starch was suspended in city water to a concentration of 40% by weight, and then 1N aqueous sodium hydroxide solution was added to adjust the pH to 6.0 to obtain starch milk. Amylomaltase crude enzyme solution was added to this starch milk so that the amount was 8.0 units per gram of starch solids, and the mixture was stirred at room temperature for 30 minutes, and then reacted at 80°C for 6 hours while stirring to prepare liquefied starch. The weight-average molecular weight of the resulting starch partial hydrolyzate was 2.82 million, and the degree of dispersion was 9.82.
[0157] (Production Example 2) Partially hydrolyzed starch derived from tapioca starch Tapioca starch was suspended in city water to a concentration of 45% by weight, and then 1N aqueous sodium hydroxide solution was added to adjust the pH to 6.0 to obtain starch milk. Amylomaltase crude enzyme solution was added to this starch milk so that the amount was 8.0 units per gram of starch solids, and the mixture was stirred at room temperature for 30 minutes, and then reacted at 80°C for 6 hours while stirring to prepare liquefied starch. The weight-average molecular weight of the resulting partial starch hydrolyzate was 2.23 million, and the degree of dispersion was 7.63.
[0158] (3) Production of Water-Soluble Polymer (Production Example 3) 100g of a 40% by weight aqueous solution of the starch partial hydrolysate produced in Production Example 1 (0.74 mol of hydroxyl groups of the starch partial hydrolysate) was charged into a 500 ml separable flask equipped with a stirrer, a thermometer, and a cooling tube. Next, 30.3g of a 48.8% aqueous solution of sodium hydroxide (0.37 mol, 0.50 molar equivalents per mole of hydroxyl groups of the starch partial hydrolysate) was charged, and the solution was stirred at 60°C or less until it became completely homogeneous. After confirming that the solution became homogeneous, an aqueous solution of 18.0g of monochloroacetic acid (0.19 mol, 0.3 molar equivalents per mole of hydroxyl groups of the starch partial hydrolysate) dissolved in 50g of ion-exchanged water was added dropwise at 50-60°C over 30 minutes. After charging the aqueous solution of monochloroacetic acid, the temperature was adjusted to 45-50°C, and the mixture was stirred for 12 hours. The end point of the reaction was determined by sampling the reaction solution, measuring the chloride ion content in the reaction solution by potentiometric titration using a 0.01N silver nitrate aqueous solution, and determining that the chloride ion content reached 98% or more of the calculated value of 3.4% when all the monochloroacetic acid had reacted. In this production example, the chloride content was 3.4%.
[0159] After the reaction was completed, the reaction solution was diluted with 600 g of ion-exchanged water. The diluted reaction solution was cooled to room temperature and added to 5000 ml of methanol over about 30 minutes to precipitate and reprecipitate the water-soluble polymer. After all the reaction solution was added, the mixture was stirred for 30 minutes, and the water-soluble polymer dispersed in the methanol was subjected to solid-liquid separation by vacuum filtration.
[0160] Next, in order to remove the sodium chloride contained in the water-soluble polymer, the recovered water-soluble polymer was redispersed in 850 ml of aqueous methanol (methanol / water 80 / 20 (volume ratio)), stirred at room temperature for 30 minutes, washed, and then subjected to solid-liquid separation by vacuum filtration, and the water-soluble polymer was recovered again. The chlorine content of the recovered water-soluble polymer was measured by potentiometric titration using a 0.01N silver nitrate aqueous solution, and the washing process was repeated until the chlorine content was less than 1%. The total acid value of the obtained water-soluble polymer was 137 mg KOH / g, the degree of etherification calculated from the total acid value was 0.47, the weight average molecular weight was 10.28 million, and the degree of dispersion was 12.3.
[0161] (4) Production of Water-Soluble Polymer (Production Example 4) 100g of 45% by weight aqueous solution of the starch partial hydrolysate produced in Production Example 2 (0.83 mol of hydroxyl groups of the starch partial hydrolysate) was charged into a 500 ml separable flask equipped with a stirrer, a thermometer, and a cooling tube. Next, 34.0g of 48.8% aqueous sodium hydroxide solution (0.42 mol, 0.50 molar equivalents per mole of hydroxyl groups of the starch partial hydrolysate) was charged, and the solution was stirred at 60°C or less until it became completely homogeneous. After confirming that the solution became homogeneous, an aqueous solution of 19.8g of monochloroacetic acid (0.21 mol, 0.3 molar equivalents per mole of hydroxyl groups of the starch partial hydrolysate) dissolved in 50g of ion-exchanged water was added dropwise at 50-60°C over 30 minutes. After charging the aqueous solution of monochloroacetic acid, the temperature was adjusted to 45-50°C, and the mixture was stirred for 12 hours. The end point of the reaction was determined by sampling the reaction solution, measuring the chloride ion content in the reaction solution by potentiometric titration using a 0.01N silver nitrate aqueous solution, and determining that the chloride ion content reached 98% or more of the calculated value of 3.7% when all the monochloroacetic acid had reacted. In this production example, the chloride content was 3.7%.
[0162] After the reaction was completed, the reaction solution was diluted with 600 g of ion-exchanged water. The diluted reaction solution was cooled to room temperature and added to 5000 ml of methanol over about 30 minutes to precipitate and reprecipitate the water-soluble polymer. After all the reaction solution was added, the mixture was stirred for 30 minutes, and the water-soluble polymer dispersed in the methanol was subjected to solid-liquid separation by vacuum filtration.
[0163] Next, in order to remove the sodium chloride contained in the water-soluble polymer, the recovered water-soluble polymer was redispersed in 850 ml of aqueous methanol (methanol / water 80 / 20 (volume ratio)), stirred at room temperature for 30 minutes, washed, and then subjected to solid-liquid separation by vacuum filtration, and the water-soluble polymer was recovered again. The chlorine content of the recovered water-soluble polymer was measured by potentiometric titration using a 0.01N silver nitrate aqueous solution, and the washing process was repeated until the chlorine content was less than 1%. The total acid value of the obtained water-soluble polymer was 147 mg KOH / g, the degree of etherification calculated from the total acid value was 0.54, the weight average molecular weight was 10.41 million, and the degree of dispersion was 12.1.
[0164] (5) Production of absorbent resin (Production Example 5) 350g of the water-soluble polymer obtained in Production Example 3 (wet product of hydrous methanol, wet ratio 65%) was put into a 3000ml beaker, and 1500ml of hydrous methanol of methanol / water = 80 / 20 (volume ratio) was added to disperse the water-soluble polymer. 24ml of 1N hydrochloric acid solution was measured with a measuring cylinder and gradually added while stirring with a magnetic stirrer. After adding hydrochloric acid, the mixture was stirred for 5 minutes, and then subjected to reduced pressure suction filtration to recover the water-soluble polymer that was partially neutralized to free acid. The recovered water-soluble polymer was a wet crystal containing hydrous alcohol. The wet crystal was transferred to a tray, put into a blower dryer set at 70 ° C, and dried for 20 hours to perform a crosslinking treatment. The solid obtained after the treatment was crushed in a mortar and sieved using sieves with openings of 150 μm and 850 μm, and absorbent resin particles with a particle size of 150 to 850 μm were recovered.
[0165] (6) Production of absorbent resin (Production Example 6) 350g of the water-soluble polymer obtained in Production Example 3 (wet product of hydrous methanol, wet ratio 65%) was put into a 3000ml beaker, and 1500ml of hydrous methanol of methanol / water = 80 / 20 (volume ratio) was further added to disperse the water-soluble polymer. 120ml of 1N hydrochloric acid aqueous solution was measured with a measuring cylinder and gradually added while stirring with a magnetic stirrer. After adding hydrochloric acid, the mixture was stirred for 1 hour, and then subjected to reduced pressure suction filtration to recover the water-soluble polymer that was partially neutralized to free acid. The recovered water-soluble polymer was a wet crystal containing hydrous alcohol. The wet crystal was transferred to a tray, put into a blower dryer set at 100 ° C, and dried for 7 hours to perform a crosslinking treatment. The solid obtained after the treatment was crushed in a mortar and sieved using sieves with openings of 150 μm and 850 μm, and absorbent resin particles with a particle size of 150 to 850 μm were recovered.
[0166] (7) Production of absorbent resin (Production Example 7) The same operation as in Production Example 5 was carried out except that the water-soluble polymer was changed to 350 g of the water-soluble polymer obtained in Production Example 4 (wet product with water-containing methanol, wet ratio 63%) and the amount of 1N hydrochloric acid solution was changed to 26 ml, and water-absorbent resin particles were recovered.
[0167] (8) Production of absorbent resin (Production Example 8) The same operation as in Production Example 6 was carried out except that the water-soluble polymer was changed to 350 g of the water-soluble polymer obtained in Production Example 4 (wet product with water-containing methanol, wet ratio 63%) and the amount of 1N hydrochloric acid solution was changed to 128 ml, and water-absorbent resin particles were recovered.
[0168] (Comparative Manufacturing Example 1) Production of water-absorbent resin made of sodium polyacrylate 155 parts by mass (2.15 mol parts) of acrylic acid, 0.62 parts by mass (0.0024 mol parts) of pentaerythritol triallyl ether as an internal crosslinking agent, and 340.27 parts by mass of deionized water were stirred and mixed while being kept at 1°C. Nitrogen was introduced into this mixture to reduce the amount of dissolved oxygen to 0.1 ppm or less, and then 0.31 parts by mass of a 1% by mass aqueous hydrogen peroxide solution, 1.16 parts by mass of a 1% by mass aqueous ascorbic acid solution, and 2.325 parts by mass of a 0.5% by mass aqueous 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)-propionamide] solution were added and mixed to initiate polymerization. After the temperature of the mixture reached 85°C, the mixture was polymerized at 85±2°C for about 10 hours to obtain a hydrogel. Next, 502.27 parts by mass of this hydrous gel was chopped with a mincer (manufactured by ROYAL, "12VR-400K"), while 128.42 parts by mass of 48.5% by mass aqueous sodium hydroxide solution was added and mixed, and further 3 parts by mass of 1% by mass aqueous solution of ethylene glycol diglycidyl ether was added and mixed to obtain a chopped gel. The chopped gel was further dried in a ventilated band dryer {200°C, wind speed 5m / sec} to obtain a dried body. The dried body was pulverized with a juicer mixer (manufactured by Oster, "OSTERIZERBLENDER"), and then adjusted to a particle size of 150μm to 710μm using sieves with openings of 150μm and 710μm to obtain dried body particles.
[0169] The physical properties of the obtained liquid-absorbent resins 1 to 4 are shown in Table 1.
[0170] [Table 1]
[0171] <Absorption test of mixed solvent of liquid organic compound and water> A mixed solvent with water was prepared using isopropyl alcohol (IPA) having antibacterial properties as a liquid organic compound. A mixed solvent with water was also prepared using glycerin having moisture retention properties as a liquid organic compound. Table 1 shows the mixture ratio (mass ratio) of the liquid organic compound and water. The water absorption rate and water retention rate of the mixed solvent were measured for the absorbent resins 1 to 4 obtained above and the water-absorbing resin made of sodium polyacrylate (Comparative Production Example 1). The results are also shown in Table 2.
[0172] [Table 2]
[0173] From the results in Table 2, it is evident that the absorbent resin used in the present invention has a high absorption capacity for the mixed solvent of a liquid organic compound and water.
[0174] <Functional sheet 1> An antibacterial aqueous solution (1) was prepared by dissolving 50% by mass of isopropanol in water. 3 g of a water-absorbent material containing 40% by mass of pulp and 60% by mass of powder of absorbent resin No. 1 was covered with tissue paper to prepare an absorbent body. The obtained absorbent body was covered with a top sheet (air-through nonwoven fabric (basis weight 25 g / m 2 100mm x 100mm)) and back sheet (air-through nonwoven fabric (weight 25g / m 2 An absorbent article was prepared by sandwiching the absorbent article between a sheet of paper measuring 100 mm x 100 mm (100 mm x 100 mm). 70 g of the diluted solution of the drug-containing aqueous solution (1) was sprayed onto the absorbent article, and the diluted solution was dried for 5 minutes in a dryer (set temperature 45° C.) to obtain a functional sheet 1 having antibacterial properties.
[0175] The liquid-absorbent resin in the functional sheet 1 contains isopropanol, which imparts antibacterial properties. For example, by wiping the top of a table with the functional sheet 1, the table can be made antibacterial.
[0176] <Functional sheet 2> A moisturizing aqueous solution (2) consisting of a glycerin-urea aqueous solution was prepared by dissolving 20% by weight of glycerin and 20% by weight of urea in water. 3 g of a water-absorbent material containing 40% by weight of pulp and 60% by weight of powder of absorbent resin No. 1 was covered with tissue paper to prepare an absorbent body. The obtained absorbent body was covered with a top sheet (air-through nonwoven fabric (basis weight 25 g / m 2 100mm x 100mm)) and back sheet (air-through nonwoven fabric (weight 25g / m 2 An absorbent article was prepared by sandwiching the absorbent article between a sheet of paper (100 mm×100 mm) and a sheet of paper (100 mm×100 mm). 90 g of the diluted solution of the drug-containing aqueous solution (2) was sprayed onto the absorbent article, and the diluted solution was dried for 5 minutes in a dryer (set temperature 45° C.) to obtain a functional sheet 2 having moisture retention.
[0177] The liquid-absorbent resin in the functional sheet 2 contains glycerin, which provides moisture retention. For example, by attaching the functional sheet 2 to the skin, the skin can be moisturized and prevented from drying out.
Claims
1. A composition containing water, a liquid organic compound, and an absorbent resin, characterized in that the absorbent resin is made of a water-soluble polymer in which an acidic group and / or a salt thereof has been introduced into a polysaccharide or a partial hydrolysis product thereof.
2. The composition according to claim 1 , wherein the water-soluble polymer has an acidic group and a salt of the acidic group.
3. The composition of claim 1 , wherein the acidic group is a carboxyalkyl group.
4. 2. The composition according to claim 1, wherein the liquid-absorbent resin is formed by crosslinking the water-soluble polymer.
5. 2. The composition according to claim 1, wherein the liquid organic compound is a compound having antibacterial properties, moisturizing properties, or aromatic properties, and is absorbed in a liquid-absorbent resin.
6. 2. The composition according to claim 1, wherein 1 g to 300 g of the liquid organic compound is absorbed per 1 g of the liquid-absorbent resin.
7. The composition according to claim 1 , wherein the liquid organic compound is an alcoholic compound.
8. The composition according to claim 1, wherein the solubility of the liquid organic compound in water is 0.1 g / mL or more.
9. A functional sheet comprising a sheet-like support coated, supported, laminated or impregnated with the composition according to claim 5.
Citation Information
Patent Citations
Production of alcohol absorbing resin
JP1987151406A
Preparation of highly alcohol-absorbing resin
JP1990215815A
Preparation of highly alcohol-absorbing resin
JP1990215816A