Method of producing stretch-blow-molded article, resin composition and method of producing the same, and pellets and method of producing the same
By producing preforms from a melt-kneaded mixture of wax, styrene resin, and carbodiimide compound, the method addresses the issues of reduced impact strength and surface deformation in recycled polystyrene products, ensuring consistent quality and durability of toner bottles.
Patent Information
- Application Number
- JP2023070429
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-21
- Publication Date
- 2024-10-31
AI Technical Summary
The use of recycled polystyrene in stretch blow molding results in reduced impact strength and increased blow molding defects due to low molecular weight and varying stretchability, while chemical recycling is costly and environmentally impactful, and material recycling leads to surface deformation of toner particles in toner bottles, causing development defects in electrophotographic images.
A method involving the production of a preform from a melt-kneaded mixture of wax, styrene resin, and a carbodiimide compound, followed by stretch blow molding, to suppress wax migration and surface deformation in molded products, particularly toner bottles.
The method effectively prevents wax migration to the surface of molded products, reducing chemical attack and ensuring consistent product quality, thereby enhancing the performance and durability of recycled polystyrene-based toner bottles.
Smart Images

Figure 2024155586000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing a stretch blow molded article. The present disclosure also relates to a resin composition and a method for producing the same, and to pellets and a method for producing the same. [Background technology]
[0002] In electrophotographic image forming devices, toner bottles for supplying toner and the like need to be strong enough not to break even when dropped, so molded products made by injection stretch blow molding polystyrene such as high impact polystyrene (hereinafter sometimes referred to as "HIPS"), a styrene-based resin, in addition to polyethylene terephthalate, a polyester resin, are often used. For example, Patent Document 1 discloses a toner container made by blow molding using polystyrene resin.
[0003] In recent years, from the viewpoint of environmental protection, it has become common to collect thermoplastic resin products and their parts, regenerate them by temporarily changing their original shape, and then recycle them. Here, as described in paragraph
[0002] of Patent Document 2, chemical recycling and material recycling are known as methods for recycling thermoplastic resins such as polystyrene.
[0004] Chemical recycling requires multiple steps as disclosed in Patent Document 2, and since it requires decomposition equipment and purification treatment equipment, the recycling cost is high and the environmental load is also large. On the other hand, polystyrene obtained by material recycling (hereinafter also referred to as "material recycled polystyrene") is subjected to shear stress at high temperatures during regeneration processing, which causes the polymer chains of polystyrene to be partially cut, which reduces the molecular weight and makes the product more susceptible to problems such as a decrease in impact strength. In addition, when such partially depolymerized polystyrene is used, the low molecular weight and high molecular weight are mixed in large amounts, which causes variations in stretchability during stretch blow molding, making it more likely to cause blow molding defects.
[0005] Methods for compensating for the shortcomings of such material recycled products include the use of material recycled materials in which a larger amount of virgin material is mixed in with the plastic waste material to reduce the material recycled content, as described in paragraph
[0005] of Patent Document 3. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 6-067536 [Patent Document 2] JP 2009-001693 A [Patent Document 3] JP 2005-162847 A Summary of the Invention [Problem to be solved by the invention]
[0007] However, if the reuse rate is reduced by mixing more virgin material than plastic waste, the proportion of recycled material used will also decrease, and this needs to be improved in order to comply with a resource-circulating society. In addition, a process of washing bottles is generally carried out in material recycling. However, bottle washing may be performed multiple times using water, acid, alkali, etc., and a drying process is also required. Therefore, bottle washing can also increase the environmental burden. .
[0008] According to the inventors' investigations, material recycled polystyrene (hereinafter also referred to as "material recycled HIPS" or "MR-HIPS"), which is the result of material recycling of blown bottles as toner containers made of collected HIPS, may have a low molecular weight as described above. From the viewpoint of reducing the environmental load, the inventors simplified or omitted the cleaning of toner bottles to be recycled, obtained MR-HIPS from toner bottles with toner still attached inside, and used the MR-HIPS to manufacture toner bottles again. It was found that when toner was stored in the toner bottle obtained in this way, the surface of the toner particles was deformed at the contact points between the toner in the toner bottle and the inner surface of the toner bottle. Toner particles with deformed surfaces can cause development defects such as insufficient transfer during electrophotographic development (when the toner is transferred to the photosensitive drum), which can result in uneven density in electrophotographic images.
[0009] At least one aspect of the present disclosure is directed to a method for producing a stretch blow molded article, which can suppress migration of the wax to the surface of the blow molded article, on the premise that a wax-containing polystyrene is used as a raw material. Also, at least one aspect of the present disclosure is directed to providing a resin composition and a method for producing the same, which contribute to suppression of wax migration to the surface of the molded article, and pellets and a method for producing the same. [Means for solving the problem]
[0010] According to at least one aspect of the present disclosure, A method for producing a stretch blow molded product, comprising the steps of: A step of producing a preform from a melt-kneaded resin mixture containing at least wax, a styrene-based resin, and a carbodiimide compound; and Stretch blow molding the preform to produce a stretch blow molded article; A method for producing a stretch blow molded article is provided, comprising:
[0011] According to at least one embodiment of the present disclosure, there is provided a resin composition including a melt-kneaded mixture including a wax, a styrene-based resin, and a carbodiimide compound. According to at least one embodiment of the present disclosure, there is provided a pellet including a melt-kneaded mixture including a wax, a styrene-based resin, and a carbodiimide compound. Furthermore, according to at least one embodiment of the present disclosure, there is provided a method for producing a resin composition, the method including a step of obtaining a melt-kneaded product of a mixture containing a wax, a styrene-based resin, and a carbodiimide compound. Furthermore, according to at least one embodiment of the present disclosure, there is provided a method for producing pellets, the method including: obtaining a melt-kneaded product of a mixture containing a wax, a styrene-based resin, and a carbodiimide compound; and pelletizing the melt-kneaded product. Effect of the Invention
[0012] According to at least one aspect of the present disclosure, there is provided a method for producing a stretch blow molded article, which can suppress migration of the wax to the surface of the blow molded article, on the premise that a wax-containing polystyrene is used as a raw material. Also, according to at least one aspect of the present disclosure, there are provided a resin composition that contributes to suppression of migration of the wax to the surface of the molded article, a method for producing the same, and a pellet and a method for producing the same. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a schematic diagram of an image forming apparatus. [Diagram 2] FIG. 2 is a schematic diagram showing a method for molding a preform. [Diagram 3] FIG. 1 is a schematic diagram showing a blow molding method. [Figure 4] FIG. 1 is a schematic diagram of a one-stage blow molding process. [Diagram 5] FIG. 2 is a schematic diagram showing the process in which a wax component migrates to a surface. [Figure 6] FIG. 1 is a schematic diagram of a blow bottle. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] In the present disclosure, the expressions "XX to YY" and "XX to YY" expressing a numerical range mean a numerical range including the lower and upper limits, unless otherwise specified. When a numerical range is described in stages, any combination of the upper and lower limits of each numerical range is also disclosed.
[0015] The present inventors speculate that the reason why the surface of the toner contained in the toner bottle molded using MR-HIPS obtained from the toner bottle with toner still attached thereto is deformed is as follows. That is, it is believed that the wax contained in the toner is also mixed in the toner bottle. It is believed that at least a part of the mixed wax is present on the inner surface of the toner bottle. It is believed that the surface of the toner particles is deformed when the toner contained in the toner bottle comes into contact with the wax exposed on the inner surface of the toner bottle. The phenomenon of the deformation of the toner particle surface due to wax may be referred to as chemical attack hereinafter.
[0016] Material recycling In the process of obtaining stretch-blow molded products from raw materials containing polystyrene, the stretch-blow molded products may be kept at or above the glass transition temperature of polystyrene. Since the wax in the toner component has a low molecular weight (molecular weight of about 300 to 1500), the wax has low viscosity while the polystyrene is at or above its glass transition temperature. In addition, polystyrene is also in a state where molecular motion is easy while it is at or above its Tg. Therefore, it is thought that the wax easily migrates to the surface of the blow molded product (the surface in contact with the air).
[0017] Therefore, it is considered that a larger amount of wax exists on the surface of the stretch blow molded product molded from the raw material containing the recycled polystyrene from toner bottles, and as a result, the stretch blow molded product is considered to be more likely to cause chemical attack on the substance that comes into contact with the surface.
[0018] Therefore, the present inventors recognized that it is necessary to develop a technology for obtaining a stretch blow molded article in which wax is unlikely to migrate to the surface of the stretch blow molded article and which is unlikely to cause chemical attack on substances in contact with the surface, even if the stretch blow molded article is made from a raw material containing recycled polystyrene derived from toner bottles. Based on this recognition, the present inventors conducted extensive research and found that the following method for producing a stretch blow molded article is effective in obtaining a stretch blow molded article in which wax migration to the surface can be suppressed.
[0019] That is, the method includes a step of producing a preform from a molten mixture of a resin mixture containing at least wax, a styrene-based resin, and a carbodiimide compound, and a step of stretch-blow molding the preform to produce the stretch-blow molded article.
[0020] Hereinafter, an embodiment of the present disclosure will be described in detail with reference to the drawings. However, the scope of the present invention is not limited to the following embodiment. In the following description, "%" means "% by mass" unless otherwise specified.
[0021] (Preform) The stretch-blow molded product is produced by stretch-blow molding a preform. The preform is a resin blend containing at least wax, a styrene-based resin, and a carbodiimide compound. The preform is manufactured using a melt-kneaded resin composition containing the melt-kneaded resin composition. That is, the preform is composed of a resin composition containing the melt-kneaded resin composition. Therefore, the stretch-blow molded product according to the present disclosure obtained by stretch-blow molding the preform is also composed of the above-mentioned resin composition. The details of the manufacturing method of the preform will be described later.
[0022] Here, "melt kneading" includes applying a shear force to a resin mixture in a state where the resin mixture is heated and has fluidity. Specifically, for example, the resin mixture is heated to a temperature equal to or higher than the glass transition temperature of the styrene resin, and the styrene resin has fluidity, and at least a part of the wax is melted, or at least a part of the carbodiimide compound is melted, or at least a part of the wax and at least a part of the carbodiimide compound are melted. The "melt kneaded product" includes the product obtained by the above-mentioned "melt kneading".
[0023] The styrene resin preferably contains polystyrene. Examples of polystyrene include at least one selected from the group consisting of high impact polystyrene (HIPS) and styrene alloys. Examples of styrene alloys include polymer alloys whose main raw material is acrylonitrile styrene (AS) or general purpose polystyrene (GPPS), specifically, alloys of polypropylene and polystyrene (PP / PS) and alloys of polyphenylene ether and polystyrene (PPE / PS). The styrene resin preferably contains high impact polystyrene (HIPS).
[0024] A carbodiimide compound has at least one carbodiimide group represented by "-N=C=N-" in the molecule. Examples of the carbodiimide compound include carbodiimide and polycarbodiimide.
[0025] The stretch-blow molded product can be used as a toner bottle. When a stretch-blow molded product is molded using MR-HIPS obtained from a raw material to which toner has adhered, and toner is stored in the resulting stretch-blow molded product, the wax in the toner contained in the MR-HIPS tends to cause chemical attack on the surface of the stored toner. When wax is contained in the raw material of the preform, the wax 202 migrates to the surface of the stretch blow molded product during the molding process when the styrene resin 201 reaches or exceeds the glass transition temperature, as shown in Fig. 5. When the styrene resin reaches or exceeds the glass transition temperature, the thermal motion of the styrene resin becomes active, so that the low-viscosity wax easily migrates from the gaps in the styrene resin to the surface of the stretch blow molded product.
[0026] The inclusion of a carbodiimide compound in the resin mixture, which is the raw material of the preform, can suppress the migration of wax to the surface of the stretch blow molded product. One of the reasons for this is that when the resin mixture is used to manufacture a preform, in the process of melt-kneading the resin mixture, the resin mixture is subjected to a temperature necessary for plasticizing the styrene-based resin and a shear force. In the process, it is considered that the wax reacts with the carbodiimide compound, and the wax polymerizes. Therefore, the melt-kneaded product, which is the result of melt-kneading, or the resin composition containing the melt-kneaded product contains polymerized wax. Since the polymerized wax has low fluidity, it is considered that the migration of wax to the surface can be prevented in the melt-kneaded product or the molded product made of the resin composition.
[0027] As described above, the reaction between the wax in the resin mixture and the carbodiimide compound is believed to proceed due to heat and shear force applied to the mixture in the process of melt-kneading the resin mixture when producing a preform from the resin mixture. In particular, it is believed that the reaction between the wax and the carbodiimide compound proceeds more easily when the mixture is heated to a temperature equal to or higher than the glass transition temperature (90°C) of the styrene-based resin in the mixture. Due to the above-mentioned action, It is believed that migration of wax to the surface of the stretch blow molded article is suppressed, and chemical attack that occurs when the stretch blow molded article is used as a toner bottle is suppressed.
[0028] The styrene resin may be a material recycled styrene resin, or may be a virgin styrene resin that has not undergone molecular weight reduction. However, when the styrene resin is a material recycled polystyrene made from recycled toner bottles, the effects of the present disclosure are more pronounced. Therefore, the resin mixture preferably contains material recycled polystyrene, and more preferably contains material recycled high impact polystyrene (MR-HIPS).
[0029] The material recycled polystyrene may be obtained by using recycled raw materials having toner attached to the surface. The toner contains components such as wax. That is, the material recycled polystyrene may contain wax. The presence and quantification of imide bonds in the modified styrene resin can be performed, for example, by measurement using FT-IR.
[0030] <High impact polystyrene (HIPS)> As the high impact polystyrene (HIPS), for example, it is preferable to use a mixture of polystyrene with a rubber-like polymer or a rubber-like copolymer. As the rubber-like polymer or rubber-like copolymer, for example, at least one polymer selected from the group consisting of polybutadiene, styrene-butadiene copolymer, polyisoprene, butadiene-isoprene copolymer, natural rubber, and ethylene-propylene copolymer is preferably used. That is, the styrene-based resin may be a styrene-based resin composition containing at least one selected from the group consisting of a rubber-like polymer and a rubber-like copolymer in addition to polystyrene. The total content ratio of the rubber-like polymer and the rubber-like copolymer in the styrene-based resin is preferably less than 50 mass%. For example, "FP120" (trade name, manufactured by Toyo Styrene Co., Ltd.) can be used. It may also be a mixture with other resins.
[0031] The content of the styrene resin (e.g., HIPS) in the preform is not particularly limited, but is preferably 80% by mass or more, and more preferably 90% by mass or more, based on the mass of the preform. Also, it is preferably 99.9% by mass or less, and more preferably 99.5% by mass or less. For example, it is preferably in the range of 80 to 99.9% by mass or 90 to 99.5% by mass.
[0032] <Carbodiimide compound> A carbodiimide compound has at least one carbodiimide group in the molecule. Examples of the carbodiimide compound include carbodiimide and polycarbodiimide. Examples of the carbodiimide compound include carbodiimide, polycarbodiimide, etc. The carbodiimide and polycarbodiimide used for modification have at least one carbodiimide group represented by "-N=C=N-" in the molecule.
[0033] Polycarbodiimides can be produced, for example, by heating an organic isocyanate in the presence of a catalyst and subjecting it to a decarboxylation condensation reaction. Examples of the organic isocyanate include aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates. Specific examples of polycarbodiimides include aromatic polycarbodiimides such as poly(4,4'-diphenylmethanecarbodiimide), poly(p-phenylenecarbodiimide), poly(m-phenylenecarbodiimide), poly(diisopropylphenylcarbodiimide), and poly(triisopropylphenylcarbodiimide); and alicyclic polycarbodiimides such as poly(dicyclohexylmethanecarbodiimide). These polycarbodiimides may be used alone or in any combination of two or more.
[0034] Among these polycarbodiimides, aliphatic polycarbodiimides are preferred. For example, commercially available aliphatic polycarbodiimides such as "Carbodilite HMV-15CA", "Carbodilite LA-1" and "Carbodilite HMV-5CA-LC" (all trade names, manufactured by Nisshinbo Chemical Inc.) can be used.
[0035] As a method for producing a preform made of the resin composition according to the present disclosure, for example, there is a method in which a preform is obtained by melt-kneading a wax, a styrene-based resin, and a carbodiimide compound. In order to sufficiently react the wax with the carbodiimide compound, it is preferable to melt-knead a mixture containing at least the wax, the styrene resin, and the carbodiimide compound to obtain a melt-kneaded product of the mixture. It is believed that the reaction between the wax and the carbodiimide compound is more easily promoted by melt-kneading. Then, a preform is formed using the melt-kneaded product thus obtained, and the preform is stretch-blow molded to obtain a stretch-blow molded product.
[0036] Here, one of the non-limiting methods of obtaining a preform using the melt-kneaded product is, for example, to obtain a melt-kneaded product of a mixture containing at least a wax, a styrene-based resin, and a carbodiimide compound, and then pelletize the melt-kneaded product to obtain pellets containing the obtained melt-kneaded product. A method of obtaining a preform using the obtained pellets is exemplified. Another method is to not pelletize the melt-kneaded product, and to mold a preform following the melt-kneading step of the resin mixture.
[0037] Since polycarbodiimide has high reactivity, it is preferable to stabilize the physical properties of the modified styrene-based resin while controlling the amount of polycarbodiimide added. For example, polycarbodiimide may be diluted in advance with unmodified styrene-based resin and melt-kneaded at a temperature equal to or higher than the glass transition temperature of the styrene-based resin to prepare master batch pellets (second pellets). Then, it is preferable to melt-knead the obtained second pellets with pellets (first pellets) containing wax and unmodified styrene-based resin to form a preform, and further to obtain a stretch-blow molded product.
[0038] Specifically, for example, a first pellet containing wax and a styrene resin is prepared. The first pellet can be material recycled polystyrene, specifically, for example, MR-HIPS pellets containing wax obtained by melting and pelletizing crushed used HIPS toner bottles. Then, separate from the process of preparing the first pellets, the carbodiimide compound and another styrene-based resin B are mixed, melt-kneaded, extruded, and pelletized to form second pellets. The first pellets and the second pellets are injection-molded by the method described below to form a preform, and further a stretch-blow molded product is produced. The styrene-based resin B used to form the second pellets is not particularly limited, and may be the same styrene-based resin as the styrene-based resin contained in the first pellets, or may be a different styrene-based resin.
[0039] In preparing the master batch pellets, the dilution ratio when diluting the polycarbodiimide with the unmodified styrene resin is not particularly limited. For example, the polycarbodiimide is preferably diluted 5 to 15 times with the unmodified styrene resin, and more preferably 10 times. By setting the dilution ratio within the above range, the concentration of the carbodiimide compound in the second pellets can be set to an appropriate range. As a result, when the second pellets are melt-kneaded with the first pellets, the carbodiimide compound and the wax can be reacted more effectively.
[0040] The master batch pellets (second pellets) were then mixed with unmodified wax-containing spunbonded ... The unmodified styrene resin is mixed with pellets (first pellets) of the styrene resin and melt-kneaded at a temperature equal to or higher than the melting point of the styrene resin, so that the polycarbodiimide and the wax can react more uniformly. The first pellets and the second pellets may be uniformly stirred with a blender or the like, and the resulting pellet mixture may be fed into an injection molding machine and molded into a preform. By feeding the two types of pellets into the injection molding machine after mixing them uniformly, the polycarbodiimide and the unmodified styrene resin can react more uniformly during melt-kneading in the injection molding machine. As a result, a more homogeneous modified styrene resin can be obtained.
[0041] The amount of the carbodiimide compound is preferably 114 parts by mass or more, more preferably 227 parts by mass or more, relative to 100 parts by mass of the wax. Also, it is preferably 1141 parts by mass or less, more preferably 570 parts by mass or less. Specifically, the content of the carbodiimide compound in the polystyrene mixture used for molding the preform is preferably in the range of 114 to 1141 parts by mass, particularly preferably in the range of 227 to 570 parts by mass, relative to 100 parts by mass of the wax. By setting the amount of the carbodiimide compound to be added within the above range, the wax and the carbodiimide compound can be sufficiently reacted with each other, and bleeding of the wax onto the surface of the stretch-blow molded article can be more reliably suppressed.
[0042] As a method for reacting polycarbodiimide with wax, for example, a method of heating a mixture of polycarbodiimide or a master batch pellet containing polycarbodiimide and an unmodified styrene resin containing wax at a temperature equal to or higher than the glass transition temperature of the styrene resin using an extruder to melt-knead it can be mentioned. The temperature during melt-kneading is not particularly limited, but when HIPS is used as the styrene resin, it is preferably 200°C or higher, more preferably 210°C or higher.
[0043] The wax is not particularly limited, and for example, waxes that are generally used in toners can be used. For example, the following waxes can be mentioned. Examples of the wax include aliphatic hydrocarbon waxes such as low molecular weight polyethylene, low molecular weight polypropylene, polyolefin copolymers, polyolefin wax, microcrystalline wax, paraffin wax, and Fischer-Tropsch wax; oxides of aliphatic hydrocarbon waxes such as oxidized polyethylene wax; or block copolymers thereof; vegetable waxes such as candelilla wax, carnauba wax, Japan wax, and jojoba wax; animal waxes such as beeswax, lanolin, and spermaceti; mineral waxes such as ozokerite, ceresin, and petrolactam; waxes mainly composed of aliphatic esters such as montan acid ester wax and castor wax; and waxes in which aliphatic esters have been partially or completely deoxidized, such as deoxidized carnauba wax. Further, saturated straight-chain fatty acids such as palmitic acid, stearic acid, montanic acid, or long-chain alkyl carboxylic acids having even longer alkyl chains; unsaturated fatty acids such as brassidic acid, eleostearic acid, or valinaric acid; saturated alcohols such as stearyl alcohol, eicosyl alcohol, behenyl alcohol, carnaubyl alcohol, ceryl alcohol, melissyl alcohol, or alkyl alcohols having even longer alkyl chains; polyhydric alcohols such as sorbitol; aliphatic amides such as linoleic acid amide, oleic acid amide, or lauric acid amide; methylene bisstearic acid amide, ethylene biscapric acid amide, ethylene Saturated aliphatic bisamides such as ethylene bislauric acid amide and hexamethylene bisstearic acid amide; unsaturated fatty acid amides such as ethylene bisoleic acid amide, hexamethylene bisoleic acid amide, N,N'-dioleyl adipic acid amide and N,N'-dioleyl sebacic acid amide; aromatic bisamides such as m-xylene bisstearic acid amide and N,N'-distearyl isophthalic acid amide; fatty metal salts (commonly known as metallic soaps) such as calcium stearate, calcium laurate, zinc stearate and magnesium stearate; vinyl monomers such as styrene and acrylic acid in aliphatic hydrocarbon waxes. Examples of such waxes include waxes grafted with monomers; partial esters of fatty acids and polyhydric alcohols, such as behenic acid monoglyceride; and methyl ester compounds having hydroxyl groups obtained by hydrogenating vegetable oils. These waxes may be used alone or in any combination of two or more. It is considered preferable that the wax comprises an ester-based wax.
[0044] In addition, the waxes having a sharp molecular weight distribution obtained by subjecting them to a press sweating method, a solvent method, a recrystallization method, a vacuum distillation method, a supercritical gas extraction method, or a melt crystal precipitation method are preferably used, and those from which low molecular weight solid fatty acids, low molecular weight solid alcohols, low molecular weight solid compounds, and other impurities have been removed are also preferably used. Specific examples include Viscol (registered trademark) 330-P, 550-P, 660-P, and TS-200 (Sanyo Chemical Industries, Ltd.), Hiwax 400P, 200P, 100P, 410P, 420P, 320P, 220P, 210P, and 110P (Mitsui Chemicals, Inc.), Sasol H1, H2, C80, C105, and C77 (Schumann-Sasol), HNP-1, HNP-3, and HN P-9, HNP-10, HNP-11, HNP-12 (Nippon Seiro Co., Ltd.), Unilin (registered trademark) 350, 425, 550, 700, Unicid (registered trademark) 350, 425, 550, 700 (Toyo Petrolite Co., Ltd.), wood wax, beeswax, rice wax, candelilla wax, carnauba wax (available from Cerarica NODA Co., Ltd.), and the like.
[0045] The stretch blow molded product may contain a colorant as necessary. Examples of the colorant include carbon black. The content of the colorant in the stretch blow molded product is, for example, 0.01 to 0.20% by mass, or 0.02 to 0.10% by mass.
[0046] Next, one embodiment of a method for producing a stretch blow molded article by biaxial stretch blow molding using a preform will be described below. The method for producing a stretch blow molded product includes the following steps. (I) A step of producing a preform from a melt-kneaded resin mixture containing at least wax, a styrene-based resin, and a carbodiimide compound. (II) A process of stretch-blow molding the preform to produce a stretch-blow molded product.
[0047] (I) A step of producing a preform from a melt-kneaded resin mixture containing at least wax, a styrene-based resin, and a carbodiimide compound. An example of a method for producing a preform from a melt-kneaded resin mixture containing at least wax, a styrene-based resin, and a carbodiimide compound will be described. The preform is made of a resin composition including a melt-kneaded mixture of a resin mixture including at least a wax, a styrene-based resin, and a carbodiimide compound. That is, the method for producing the resin composition includes a step of obtaining a melt-kneaded mixture of a resin mixture including a wax, a styrene-based resin, and a polycarbodiimide compound.
[0048] The step of manufacturing the preform may include a step of preparing pellets of a melt-kneaded product of a resin mixture containing wax and a styrene-based resin. Also, for example, the step of crushing a toner containing wax and a toner bottle containing a styrene-based resin, melt-kneading them to form pellets. That is, the step of manufacturing the preform may include a step of crushing a recycled toner bottle with toner attached thereto, and obtaining a crushed product of the toner bottle.
[0049] For example, a resin mixture containing a wax, a styrene-based resin, and a carbodiimide compound may be melt-kneaded to form pellets. That is, a method for producing pellets may include a step of obtaining a melt-kneaded product of a resin mixture containing a wax, a styrene-based resin, and a carbodiimide compound, and a step of pelletizing the melt-kneaded product.
[0050] Also, a toner bottle to which a toner containing wax is attached may be pulverized, and a carbodiimide compound may be added to the pulverized product obtained and melt-kneaded to form pellets. The toner bottle contains a styrene-based resin. That is, the step of manufacturing a preform may include a step of melt-kneading raw materials containing at least wax, a styrene-based resin, and a carbodiimide compound to form pellets. Also, the step of manufacturing a preform may include a step of molding a preform from the pellets.
[0051] As described above, the carbodiimide compound may be diluted in advance with a small amount of unmodified styrene resin and melt-kneaded before use. For example, a first pellet containing wax and a styrene resin is prepared. Also, for example, a toner containing wax and a toner bottle containing a styrene resin may be crushed and melt-kneaded to prepare the first pellet. That is, the process of manufacturing a preform may include a process of crushing a recycled toner bottle to which toner is attached, melt-kneading the toner bottle, and preparing the first pellet.
[0052] Then, a second pellet containing a melt-kneaded mixture of the carbodiimide compound and the styrene-based resin B is formed separately from the step of forming the first pellet. The obtained first pellet and the second pellet are mixed, and the melt-kneaded mixture of the pellets is molded by a method described later to manufacture a preform. That is, the step of manufacturing a preform may include a step of melt-kneading the carbodiimide compound and the styrene-based resin B to form a second pellet. The step of manufacturing a preform may also include a step of mixing the first pellet and the second pellet. The step of manufacturing a preform includes a preform molding step of molding a pellet mixture of the first pellet and the second pellet into a preform.
[0053] The means for melt-kneading is not particularly limited, and known means such as a twin-screw extruder can be used. As the twin-screw extruder, for example, PC-46 (manufactured by Ikegai Corporation) can be used. The temperature during melt-kneading is not particularly limited, but is, for example, 200 to 300°C, preferably 240 to 280°C. By melt-kneading, the wax is easily fixed in the high molecular weight styrene-based resin. It is also considered that the reaction between the wax and the carbodiimide compound is more easily promoted.
[0054] The pellets obtained in the above steps are molded to manufacture a preform. As shown in FIG. 2, a test tube-shaped preform 104 is molded by injection molding. Specifically, a heating cylinder 105 heats the material fed into an injection molding machine 101 to a molten state, and an extrusion screw 207 injects the molten material into preform molds 102 and 103, and after cooling, the material is removed from the mold to obtain a preform 104. In the process of manufacturing a preform, it is preferable to manufacture the preform by injection molding. That is, the process of molding the preform preferably includes a process of injection molding a melt-kneaded product of pellets or a pellet mixture. In addition, the preform preferably has a test tube shape. By heating the raw material in the molding process of the preform, the wax is easily fixed in a styrene-based resin having a high molecular weight. In addition, it is considered that the reaction between the wax contained in the toner and the carbodiimide compound is further promoted.
[0055] (II) A process of stretch-blow molding the preform to produce a stretch-blow molded product. Next, a process for producing a stretch-blow molded product by stretch-blow molding a preform will be described. As shown in FIG. 3, a preform 104 is biaxially stretched and blown (biaxially stretched and molded). First, the preform 104 is placed in a heating furnace 107 and heated to a temperature at which it can be stretched. By heating the preform in the process for producing a blow molded product, the wax is easily fixed in the high molecular weight styrene resin. It is also believed that the reaction between the wax contained in the toner and the carbodiimide compound is further promoted.
[0056] The heated preform 104 is removed from the heating furnace 107 and placed in the mouth of a blow mold 108. The blow mold 108 has a cavity formed therein by combining a left mold 108-1 and a right mold 108-2. It is preferable to place the heated preform at the mouth of the blow mold in a short time (for example, within 10 seconds) so that the temperature of the preform does not drop before the start of the biaxial stretching step.
[0057] The heated preform placed in the blow mold 108 is stretched in the longitudinal direction of the preform using a stretch rod 109. This is called the first stretching. In the first stretching, it is preferable to flow gas so that the preform 104 does not come into contact with the stretch rod 109. The pressure of the gas at this time is called the first blow pressure.
[0058] After the first stretching, gas 110 is introduced from the preform mouth 106 to stretch the preform in the lateral direction (the circumferential direction, i.e., the direction intersecting the stretching rod 109). This is called the second stretching. The pressure of the gas at this time is called the secondary blow pressure. Examples of the gas introduced during the first and second stretching include air, nitrogen, carbon dioxide, and argon.
[0059] By carrying out these primary and secondary stretching steps, the preform 104 expands in each direction indicated by the arrows 301 and adheres to the inner wall of the blow mold 108, and is cooled and solidified in this state to produce the blow molded product 112. The molding step preferably includes a step of stretching the preform in the longitudinal direction of the preform using a stretching rod, and a step of injecting gas into the preform stretched in the longitudinal direction to stretch the preform in the circumferential direction.
[0060] Next, the left mold 108-1 and the right mold 108-2 of the blow mold 108 are separated. The blow molded article 112 is then removed from the blow mold 108 .
[0061] There are two types of injection stretch blow molding: one-stage and two-stage. The one-stage method uses the residual heat of the preform immediately after it is removed from the mold to stretch blow mold it as is, or after adjusting the temperature. The two-stage method cools the preform down to room temperature, and then stretch blow molds it again after adjusting the temperature. That is, the step of molding the pellets to produce a preform and the molding step of stretch-blow molding the preform to produce a stretch-blow molded article may be performed continuously while maintaining the temperature of the preform. Also, after the step of molding the pellets to produce a preform, the preform may be cooled to room temperature, and then the molding step of stretch-blow molding the preform to produce a stretch-blow molded article may be performed.
[0062] A schematic diagram of the one-stage method is shown in Fig. 4. In the one-stage method, after preform 104 is injection-molded from injection molding machine 101, cooling during injection molding is short, at 10 seconds or less, so that preform 104 does not fall below the glass transition temperature of the styrene-based resin. Then, the preform is immediately heated and kept at a blow molding temperature (for example, 90 to 120°C), and blow molded to produce blow-molded product 112. In the one-stage method, an apparatus in which an injection molding device and a blow molding device are integrated is used.
[0063] The two-stage method is a method in which, after injection molding the preform, it is cooled below the glass transition temperature of the styrene-based resin, removed, and then heated to the blow molding temperature (e.g., 90 to 120°C) in a separate blow molding device for blow molding. In the two-stage method, the injection molding device and the blow molding device are not integrated, but are independent devices.
[0064] The injection stretch blow molding method is appropriately selected depending on the components contained in the preform. The one-stage method is preferable in that it does not include a step of cooling the preform to below the glass transition temperature and therefore requires less energy for reheating compared to the two-stage method.
[0065] Next, a method for checking chemical attack on the toner contained in a toner bottle obtained by biaxial stretch blow molding will be described. Toner is placed in a toner bottle obtained by biaxial stretch blow molding. The toner bottle containing the toner is left in a usage environment. In the evaluation of chemical attack according to the present disclosure, the usage environment is set to 50°C for 72 hours, and the toner bottle is left in a test thermostatic chamber. The toner bottle exposed to the usage environment is removed, and only the toner adhering to the inner surface of the bottle is taken out from the toner contained in the toner bottle and observed under an electron microscope. In the present disclosure, the toner was discharged from the toner bottle with the opening of the bottle facing downward, and then the toner adhering to the inner surface of the bottle was attached to an adhesive tape, and only the toner adhering to the inner surface of the bottle was removed. When the deformation of the toner particle surface of the toner adhering to the inner surface of the bottle is observed with an electron microscope, the toner particles that have been subjected to chemical attack can be seen to have deformed areas on the contact surface with the toner bottle. The deformed areas on the contact surface with the toner bottle can be identified by the fact that they have less unevenness compared to the surrounding areas in the image observed with the electron microscope.
[0066] (Image forming device) An image forming apparatus using a toner storage bottle obtained by the manufacturing method of the present disclosure will be described below with reference to the drawings. Fig. 1 is a schematic diagram showing a four-color image forming apparatus using an electrophotographic method, and 80 in the figure indicates the main body of the image forming apparatus. The image forming apparatus 80 is configured as a so-called intermediate transfer tandem type image forming apparatus in which four color image forming units are arranged side by side on an intermediate transfer belt.
[0067] The image forming apparatus 80 forms an image as follows. First, the exposure device 50 (50y, 50m, 50c, 50bk) forms an electrostatic latent image on the photosensitive drum 17 (17y, 17m, 17c, 17bk) based on print data. Then, the developing device 21 (21y, 21m, 21c, 21bk) develops the formed electrostatic latent image to form a toner image.
[0068] The toner image is transferred onto an intermediate transfer body 62 by a primary transfer device 60 (60y, 60m, 60c, 60bk), and then transferred onto a sheet material S supplied from a paper feeder 63 in a secondary transfer section 64 (64a, 64b). Next, the toner image transferred onto the sheet material S is fixed onto the sheet material S by a fixing means 68, and then the sheet material S is discharged onto a paper discharge tray 70.
[0069] In the image forming apparatus 80, a toner image is formed by developing in the developing device 21 as described above. At this time, detachable toner bottles 3 (3Y, 3M, 3C, 3Bk) can be used to supply toner to the developing device 21. The toner bottles manufactured by the manufacturing method of the present disclosure are toner bottles used in this manner. EXAMPLES
[0070] The present disclosure will be described in detail below using examples and comparative examples. However, the present disclosure is not limited to these examples. In the following examples and comparative examples, "%" means "% by mass" unless otherwise specified.
[0071] <Toner bottle manufacturing> One-stage blow molding equipment (ASB-70DPH manufactured by Nissei ASB Machinery Co., Ltd.) ) was used to prepare a toner bottle 3 (total length 439.5 mm, diameter 101 mm) shown in Fig. 6. The blow stretching ratio was "vertical ratio x horizontal ratio = 6.7". The "longitudinal ratio" of the blow stretch ratio is a value calculated by dividing the "total length after stretching" by the "total length (before stretching) of the part (heated part) of the preform that reaches the stretching temperature." The "lateral ratio" of the blow stretch ratio is a value calculated by dividing the "diameter of the middle part after stretching" by the "diameter of the middle part of the preform (before stretching)".
[0072] First, the materials shown in Table 1 below were melt-kneaded and then pelletized to prepare a master batch with a carbon black concentration of 5 mass %. [Table 1]
[0073] Next, the master batch with a carbon black concentration of 5% by mass prepared above and HIPS were mixed in the ratio shown in Table 2 below, melt-kneaded, and then pelletized to obtain pellets of a resin mixture. [Table 2]
[0074] <Blow molding conditions> The pellets of the resin mixture were fed into an extrusion molding device of a one-stage blow molding machine (product name: ASB-70DPH; manufactured by Nissei ASB Machinery Co., Ltd.) and biaxial stretch blow molding was performed to mold a toner bottle. The one-stage blow molding machine can continuously perform a process of manufacturing a test tube-shaped preform by injection molding and a process of manufacturing a bottle-shaped molded product by biaxial stretch blow molding the preform. The screw diameter of the injection molding device in the molding machine was 54 mm.
[0075] First, a mold capable of molding a preform having an outer diameter of 30 mm, a wall thickness of 3.7 mm, and a length of 220 mm was prepared as a mold for molding a preform. Then, a preform was molded under the following molding conditions. Screw diameter: 54mm Screw position before filling the cavity with resin mixture: 95mm ·Injection speed Up to 5mm of screw advance: 50% of maximum speed Advance the screw another 20mm: 30% of maximum speed Until the screw advances another 35mm: 25% of maximum speed PV switching position: 35mm Injection pressure Up to PV switching: 12.0MPa After PV switching: 4.5MPa (holding pressure) - Pressure retention time after PV switching ·4.57 seconds ·Heating tube temperature: 230℃ ·Cooling time: 8.0 seconds Mold temperature: 18℃
[0076] After a cooling time of 8.0 seconds had elapsed, the preform was demolded and transported to the biaxial stretch blow station of the one-stage blow molding machine. The temperature of the preform during transportation was controlled as follows. Preform heating temperature 10% of the preform's total length from the top of the preform 190℃ 25% of the preform's total length from the top of the preform 210℃ 50% of the preform's total length from the top of the preform 210℃ 75% of the preform's total length from the top of the preform 190℃
[0077] Next, the preform adjusted to the above temperature was placed in a cylindrical mold adjusted to a temperature of 18°C and having a size corresponding to the size of the toner bottle, and was subjected to biaxial stretch blow molding to produce a blown bottle. The preform was heated during transportation to adjust its temperature, and the surface temperature of the central part of the preform immediately before being placed in the cylindrical mold was 110°C. First, the stretch bar, which was in the retreated position, was inserted into the preform through the opening of the preform and advanced until it contacted the top of the preform. Next, the air pressure driving the stretch bar was increased to 1.2 MPa to advance the stretch bar further. Next, 0.5 seconds after the start of further advancement of the stretch bar, primary air was introduced into the preform through the opening of the preform. The pressure of the primary air was set to 1.0 MPa. Next, 0.15 seconds after the introduction of the primary air, secondary air was introduced. The pressure of the secondary air was set to 2.9 MPa. Air was introduced into the preform for 7.0 seconds from the start of the introduction of the primary air. Next, the pressure inside the preform was returned to normal pressure over 2.5 seconds. In this way, a toner bottle was produced by blow molding. 200 toner bottles were prepared using the above method. Note that this toner bottle was made using virgin HIPS that had not been recycled. Using the above method, 200 toner bottles were produced using virgin HIPS.
[0078] Example 1 <Production of recycled pellets> 200 unused toner cartridges (product name: Toner NPG-26; manufactured by Canon Inc.) filled with black toner were prepared. The black toner contained an ester-based wax. The wax content in the black toner was 6.9 parts by mass. The entire amount of black toner in each toner cartridge was transferred to the 200 toner bottles prepared above. Thereafter, the opening of the toner bottle was turned vertically downward to discharge the black toner therein. Even after this operation, a small amount of black toner was still attached to the inner wall of each toner bottle. At this time, the amount of black toner remaining in the toner bottle was 0.321% by mass, based on the mass of the toner bottle itself, on the average of 200 toner bottles. Note that the mass of the toner bottle itself here refers to the mass of the toner bottle and only the toner remaining inside it, after all supply parts and other items attached to the toner bottle have been removed.
[0079] Next, each of the toner bottles with toner adhering to the inner surface was crushed into pieces of about 5 to 10 mm square using a crusher to obtain crushed products (hereinafter also referred to as flake products). The flake products were melt-kneaded using a twin-screw extruder (Ikegai PC-46) at a temperature of 210°C, a screw rotation speed of 200 rpm, vent degassing of -0.08 MPa, and a discharge rate of 50 kg / h. The recycled pellets were designated as MR-HIPS (1-1).
[0080] <Making a blow bottle> A polycarbodiimide compound was added to MR-HIPS (1-1), and biaxial stretch blow molding was performed using the one-stage blow molding apparatus under the same blow molding conditions as described above. The polycarbodiimide compound was diluted and prepared in advance as a master batch pellet so that it could be easily mixed uniformly in a blender. Specifically, the polycarbodiimide compound and virgin HIPS were mixed in the ratio shown in Table 3, melt-kneaded, and then pelletized to prepare polycarbodiimide master batch pellets (second pellets). [Table 3]
[0081] Before feeding the material into the molding machine, 3.0% by mass of polycarbodiimide master batch pellets (second pellets) were added to MR-HIPS (1-1) (first pellets) and mixed uniformly with a blender. The polycarbodiimide master batch pellets were diluted at the ratio shown in Table 3, so the amount of polycarbodiimide added was effectively 0.3% by mass. The material stirred in the blender was put into the blow molding device and biaxial stretch blow molding was performed under the same blow molding conditions as described above. The obtained toner bottle was named toner bottle (1-1). Toner was placed in toner bottle (1-1) and left in an operating environment of 50°C for 72 hours. Thereafter, the toner adhering to the inner surface of the toner bottle was removed, and the surface of the toner particles was observed under an electron microscope. As a result, no deformation of the toner particle surface was confirmed, and it was confirmed that no chemical attack had occurred.
[0082] (Examples 2 and 3) Except for changing the compounding ratio of MR-HIPS (1-1) and polycarbodiimide master batch as shown in Table 1, the same procedure as in Example 1 was carried out to produce toner bottles (1-2) and (1-3). [Table 4] The toner bottles (1-1), (1-2), and (1-3) were crushed and melt-kneaded to form first pellets, which were then mixed with second pellets (master batch pellets) of a polycarbodiimide compound prepared in advance before being fed into a molding machine.
[0083] Example 4 <Production of recycled pellets> A polycarbodiimide compound (product name: Carbodilite HMV-15CA; manufactured by Nisshinbo Chemical Co., Ltd.) of 0.3% by mass was uniformly added to the flakes prepared in the same manner as in Example 1, and the mixture was melt-kneaded using a twin-screw extruder (manufactured by Ikegai Co., Ltd., PC-46) at a temperature of 230°C, a screw rotation speed of 200 rpm, vent degassing of -0.08 MPa, and a discharge rate of 50 kg / h. The polycarbodiimide used here was in powder form, not in master batch pellet form. The resulting recycled pellets were designated MR-HIPS (2-1).
[0084] <Making a blow bottle> The MR-HIPS (2-1) was placed in the one-stage blow molding apparatus and biaxial stretch blow molding was carried out under the same blow molding conditions as described above. Since polycarbodiimide was added during the extrusion process of the MR-HIPS (2-1), polycarbodiimide was not added when the material was placed in the blow molding machine, unlike in Examples 1 to 3. The obtained toner bottle was named toner bottle (2-1).
[0085] Toner was placed in a toner bottle (2-1) and left in the usage environment (50°C, 72 hours) to conduct an environmental test. After the test, the toner adhering to the inner surface of the toner bottle was observed using the above-mentioned method. As a result, no deformation of the toner particle surface was confirmed, and it was confirmed that no chemical attack had occurred.
[0086] (Examples 5 and 6) Pellets of MR-HIPS (2-2) and (2-3) were prepared in the same manner as for MR-HIPS (2-1) in Example 4, except that the blending ratio of polycarbodiimide was changed as shown in Table 5. [Table 5]
[0087] Each of the obtained pellets was subjected to biaxial stretch blow molding under the same conditions as in Example 4 to obtain toner bottles (2-2) and (2-3). Toner was placed in each bottle, and the toner was observed for deformation of the toner particle surface of the toner attached to the inner surface of the toner bottle after leaving it at 50°C for 72 hours. Toner bottle (2-2) was evaluated as Example 5, and toner bottle (2-3) was evaluated as Example 6. As a result, in Examples 5 and 6, no deformation of the toner particle surface was observed, and it was confirmed that no chemical attack occurred.
[0088] In Examples 4 to 6, no master batch pellets were prepared, and the carbodiimide compound was added when the pulverized toner bottles (flakes) to which the toner had adhered were melted and kneaded in an extruder to form pellets. In this method, it is believed that the wax and the carbodiimide compound were sufficiently kneaded in the extruder, and the reaction between the wax and the carbodiimide compound proceeded sufficiently. Therefore, migration of the wax to the inner surface of the toner bottle was sufficiently prevented, and the chemical reaction was prevented. The attack appears to have been contained. Table 6 shows the results of evaluation of chemical attack after molding of the toner bottles in Examples 4 to 6. [Table 6] As described above, polycarbodiimide was added to the toner bottles (2-1), (2-2) and (2-3) in the process of crushing the toner bottles, melt-kneading them and forming pellets.
[0089] Comparative Example 1 <Production of recycled pellets> The flakes prepared in the same manner as in Example 4 were melt-kneaded at a temperature of 230°C, a screw speed of 200 rpm, vent degassing at -0.08 MPa, and a discharge rate of 50 kg / h, and then pelletized. During melt-kneading, no polycarbodiimide compound was added. The obtained recycled pellets were named MR-HIPS (2-4).
[0090] <Making a blow bottle> The MR-HIPS (2-4) was placed in the one-stage blow molding apparatus and subjected to biaxial stretch blow molding under the same blow molding conditions as described above. The resulting toner bottle was named toner bottle (2-4). The toner was placed in a toner bottle (2-4) and left in the usage environment (50°C, 72 hours) to conduct an environmental test. After the test, the toner adhering to the inner surface of the toner bottle was observed by the above-mentioned method, and it was confirmed that the surface of the toner particles had been deformed and that chemical attacks had occurred. [Table 7]
[0091] The present disclosure relates to the following methods and compositions: (Method 1) A method for producing a stretch blow molded product, comprising the steps of: A step of producing a preform from a melt-kneaded resin mixture containing at least wax, a styrene-based resin, and a carbodiimide compound; and Stretch blow molding the preform to produce a stretch blow molded article; A method for producing a stretch blow molded product, comprising the steps of: (Method 2) 2. Production of a stretch blow molded article according to method 1, wherein the content of the carbodiimide compound in the resin mixture is 114 to 1141 parts by mass per 100 parts by mass of the wax. method. (Method 3) The method for producing a stretch blow molded article according to Method 1 or 2, wherein the styrene-based resin comprises at least one selected from the group consisting of high-impact polystyrene and a styrene-based alloy. (Method 4) The method for producing a stretch blow molded article according to any one of Methods 1 to 3, wherein the wax is an ester-based wax. (Method 5) The method for producing a stretch blow molded article according to any one of Methods 1 to 4, wherein the resin mixture contains material recycled polystyrene. (Method 6) The method for producing a stretch blow molded article according to Method 5, wherein the material recycled polystyrene contains the wax. (Method 7) The method for producing a stretch blow molded article according to any one of Methods 1 to 6, wherein the stretch blow molded article is a toner bottle. (Method 8) The preform has a test tube shape; The step of producing the stretch blow molded article comprises: stretching the preform in a longitudinal direction of the preform using a stretching rod; A step of injecting a gas into the preform stretched in the longitudinal direction to stretch the preform in the circumferential direction; The method for producing a stretch blow molded article according to any one of Methods 1 to 7, comprising the steps of: (Method 9) The step of manufacturing the preform comprises: preparing pellets of the melt-kneaded resin mixture; forming a preform from the pellets; The method for producing a stretch blow molded article according to any one of Methods 1 to 8, comprising the steps of: (Method 10) 10. The method of producing a stretch blow molded article according to Method 9, wherein the step of molding the preform comprises a step of injection molding the pellets. (Method 11) The step of manufacturing the preform comprises: preparing a first pellet containing the wax and the styrene-based resin; forming a second pellet containing a melt-kneaded mixture of the carbodiimide compound and the styrene-based resin B; A step of injection molding a melt-kneaded mixture of the first pellets and the second pellets; The method for producing a stretch blow molded article according to any one of Methods 1 to 8, comprising the steps of: (Configuration 1) A resin composition comprising a melt-kneaded mixture containing a wax, a styrene-based resin and a carbodiimide compound. (Configuration 2) A pellet comprising a melt-kneaded mixture containing a wax, a styrene-based resin and a carbodiimide compound. (Method 12) A method for producing a resin composition, comprising the step of obtaining a melt-kneaded product of a mixture containing a wax, a styrene-based resin, and a carbodiimide compound. (Method 13) obtaining a melt-kneaded mixture containing a wax, a styrene-based resin, and a carbodiimide compound; A step of pelletizing the melt-kneaded product; A method for producing pellets, comprising: [Explanation of symbols]
[0092] 3: toner bottle, 21: developing device, 80: image forming device, 60: primary transfer device, 62: intermediate transfer body, 63: paper feeder, 64: secondary transfer section, 68: fixing means, 70: paper discharge tray, 101: injection molding machine, 102: preform mold, 103: preform mold, 104: preform, 105: heating cylinder, 106: preform mouth, 107: heating furnace, 108: blow mold, 109: stretch rod, 110: gas, 112: blow molded product, 201: styrene resin, 202: wax, 207: extrusion screw
Claims
1. A method for producing a stretch blow molded product, comprising the steps of: A step of producing a preform from a melt-kneaded resin mixture containing at least wax, a styrene-based resin, and a carbodiimide compound; and Stretch blow molding the preform to produce a stretch blow molded article; A method for producing a stretch blow molded product, comprising the steps of:
2. The method for producing a stretch blow molded product according to claim 1, wherein the content of the carbodiimide compound in the resin mixture is 114 to 1141 parts by mass per 100 parts by mass of the wax.
3. The method for producing a stretch blow molded article according to claim 1, wherein the styrene-based resin comprises at least one selected from the group consisting of high impact polystyrene and a styrene-based alloy.
4. The method for producing a stretch blow molded article according to claim 1 , wherein the wax is an ester-based wax.
5. The method for producing a stretch blow molded article according to claim 1 , wherein the resin mixture contains material recycled polystyrene.
6. The method for producing a stretch blow molded article according to claim 5 , wherein the material recycled polystyrene contains the wax.
7. The method for producing a stretch blow molded article according to claim 1 , wherein the stretch blow molded article is a toner bottle.
8. The preform has a test tube shape; The step of producing the stretch blow molded article comprises: stretching the preform in a longitudinal direction of the preform using a stretching bar; A step of injecting a gas into the preform stretched in the longitudinal direction to stretch the preform in the circumferential direction; The method for producing the stretch blow molded article according to claim 1, comprising:
9. The step of manufacturing the preform comprises: preparing pellets of the melt-kneaded resin mixture; forming a preform from the pellets; The method for producing the stretch blow molded article according to claim 1, comprising:
10. The method of claim 9, wherein the step of molding the preform comprises injection molding the pellets.
11. The step of manufacturing the preform comprises: preparing a first pellet containing the wax and the styrene-based resin; forming a second pellet containing a melt-kneaded mixture of the carbodiimide compound and the styrene-based resin B; A step of injection molding a melt-kneaded mixture of the first pellets and the second pellets; The method for producing the stretch blow molded article according to claim 1, comprising:
12. A resin composition comprising a melt-kneaded mixture containing a wax, a styrene-based resin and a carbodiimide compound.
13. A pellet comprising a melt-kneaded mixture containing a wax, a styrene-based resin and a carbodiimide compound.
14. A method for producing a resin composition, comprising the step of obtaining a melt-kneaded product of a mixture containing a wax, a styrene-based resin, and a carbodiimide compound.
15. obtaining a melt-kneaded mixture containing a wax, a styrene-based resin, and a carbodiimide compound; A step of pelletizing the melt-kneaded product; A method for producing pellets, comprising:
Citation Information
Patent Citations
Toner container
JP1994067536A
Styrene-based resin composition
JP2005162847A
Plastic-molded article comprising regenerated plastic and elastic polymer