Lithium supplement additive and manufacturing method therefor, electrochemical device, and electronic device

A core-shell structured lithium replenishment additive composed of specific metal oxides enhances the stability and capacity of lithium-ion batteries, addressing the instability and safety issues of existing additives.

JP2024155700AActive Publication Date: 2024-10-31ENVISION DYNAMICS TECH (JIANGSU) CO LTD +3

Patent Information

Application Number
JP2023208102
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-20
Filing Date
2023-12-08
Publication Date
2024-10-31
Estimated Expiration
2043-12-08

AI Technical Summary

Technical Problem

Existing lithium-ion battery additives like Li5FeO4, Li2NiO2, and Li6CoO4 are unstable in air, absorb moisture, and produce gases, posing safety hazards and reducing battery efficiency.

Method used

A lithium replenishment additive composed of components A and B, where A is Li6-xM1-yN1O4-z and B is Li1+(a/(2+a))M2O2, with M1 and M2 selected from specific metals, is used to enhance stability and theoretical capacity, formulated into a core-shell structure.

Benefits of technology

The additive improves energy density and cycle stability of lithium-ion batteries by stabilizing the cathode material and increasing theoretical capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155700000001
    Figure 2024155700000001
  • Figure 2024155700000002
    Figure 2024155700000002
  • Figure 2024155700000003
    Figure 2024155700000003
Patent Text Reader

Abstract

To provide a lithium supplement additive, its manufacturing method, an electrochemical device, and an electronic device.SOLUTION: A lithium supplement additive includes a component A and a component B. The general chemical formula of the component A is Li6-xM11-yN1yO4-z with 0≤x≤5.95, 0≤y≤1, 0≤z≤2 in the formula, M1 is selected from one or more of Fe, Ni, Co, Cu, Al, Mn, Ti, and Si, and N1 is selected from one or more of Ni, Co, Cu, Al, Mn, Ti, and Si. The general chemical formula of the component B is Li1+(a / (2+a))Mn2a / (2+a)M26 / (2+a)-2O2, 0.2≤a≤1, and at least a part of the component B is located on the surface of the component A. A positive electrode material including the lithium supplement additive of the invention has higher stability and high theoretical capacity, is used for a lithium ion battery, and improves energy density and cycle stability of the battery.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] In particular, the present invention relates to lithium replenishment additives and methods for their preparation, electrochemical devices, and electronic devices. [Background technology]

[0002] In lithium-ion batteries, the lower of the initial coulombic efficiencies of the positive and negative electrodes determines the initial efficiency of the entire battery. When the efficiencies of the positive and negative electrodes are equal, the utilization of the active lithium in the battery is highest. The initial efficiency of current commercial systems is limited by the low initial efficiency of the negative electrode. Thus, much of the active Li provided by the positive electrode is consumed, lowering the overall energy density of the battery.

[0003] Some currently widely studied lithium-ion auxiliary materials include Li5FeO4 (LFO), Li2NiO2 (LNO), and Li6CoO4 (LCO), all of which have very high theoretical capacity and very low reversibility (Coulombic efficiency <10%), making them ideal lithium supplement additives (i.e., cathode lithium supplement additives). However, LFO, LNO, and LCO are unstable in air and prone to absorbing moisture, which can generate residual alkali (Li2CO3, LiOH) that not only reduces their electrochemical activity but also causes the battery to gas and swell, potentially posing a safety hazard.

[0004] Based on the above studies, there is a need to provide a lithium supplementary additive that can be used as a positive electrode material to improve the energy density and cycle stability of the battery and achieve better stability and higher theoretical capacity. Summary of the Invention [Problem to be solved by the invention]

[0005] The technical problem solved by the present invention is to overcome the instability of existing lithium auxiliary additives in air, which leads to a decrease in electrochemical activity. The use of existing lithium auxiliary additives in lithium ion batteries generates gas in the battery, causing potential safety hazards. Therefore, a lithium supplementary additive and a method for producing the same, a positive electrode sheet, an electrochemical device and an electronic device are provided. The positive electrode material containing the lithium supplementary additive of the present invention has higher stability and theoretical capacity, and is used in lithium ion batteries to improve the energy density and cycle stability of the battery. [Means for solving the problem]

[0006] The present invention solves the above technical problems through the following technical solutions:

[0007] In a first aspect, the present invention provides a lithium supplemental additive comprising component A and component B. Component A has the general chemical formula Li 6-x M 1 1-y N 1 y O 4-z where 0≦x≦5.95, 0≦y≦1, 0≦z≦2, and M 1 is selected from one or more of Fe, Ni, Co, Cu, Al, Mn, Ti, and Si; 1 is selected from one or more of Fe, Ni, Co, Cu, Al, Mn, Ti, and Si. The general chemical formula of component B is Li 1+(a / (2+a)) Mn 2a / (2+a) M 2 6 / (2+a)-2 O2, 0.2≦a≦1, M 2 is selected from one or more of Fe, Ni, Co, Cu, Al, Mn, Ti, Si, Mg, Zr, Nb, La, Sr, and W, and at least a portion of component B is located on the surface of component A.

[0008] In a second aspect, the present invention also provides a method for the preparation of said lithium supplementary additive, comprising the steps of mixing and sintering precursors of components A and B to obtain said lithium supplementary additive.

[0009] In a third aspect, the present invention also provides an electrochemical device comprising a positive electrode sheet containing the lithium supplement additive, a negative electrode sheet, a separator, and an electrolyte.

[0010] In a fourth aspect, the present invention also provides an electronic device comprising a positive electrode material containing the lithium supplementary additive or a lithium ion secondary battery containing the lithium supplementary additive.

[0011] In a fifth aspect, the present invention also provides a cathode material comprising an active material and a lithium supplement additive, the mass percentage of the lithium supplement additive in the cathode material being 0.5% to 31%. Effect of the Invention

[0012] The advantageous effects of the present invention are as follows: The positive electrode material containing the lithium supplement additive of the present invention has higher stability and higher theoretical capacity, and is used in lithium ion batteries to improve the energy density and cycle stability of the batteries.

[0013] The present invention will be further described below with reference to examples, but the present invention is not limited to the scope of the examples. In the following examples, experimental methods not specifically described are selected according to conventional methods and conditions or product instructions.

[0014] In the lithium supplemental additive of the first aspect of the present invention, preferably M 1 is Fe, Ni, Co, Cu, Al, Mn, Ti, or Si.

[0015] Preferably, N 1 is Fe, Ni, Co, Cu, Al, Mn, Ti, or Si.

[0016] Preferably, M 2 is Fe, Ni, Co, Cu, Al, Mn, Ti, Si, Mg, Zr, Nb, La, Sr, or W.

[0017] Preferably, the value of x is in the range 0≦x≦5, for example 0.4, 0.5, 0.8, 1, 2 or 4.

[0018] Preferably, the value of y is in the range 0≦y≦0.9, for example 0.2, 0.5, 0.6 or 0.8.

[0019] Preferably, the value of z is in the range 0≦z≦2, for example 0.4, 0.5, 0.8, 1 or 1.5.

[0020] Preferably, the value of a is in the range 0.22≦a≦1, for example 0.3, 0.5, 0.7 or 0.8.

[0021] Preferably, at least a portion of component B is coated on the surface of component A. Preferably, the mass ratio of component A to the total mass of "components A and B" is 89% to 99.1%, for example, 90%, 92%, 95%, 96%, 97%, 98%, or 99%.

[0022] Preferably, the lithium supplement additive has a core-shell structure. The average particle size of the core of the core-shell structure may be 0.5 μm to 15 μm. The average thickness of the shell of the core-shell structure may be 20 nm to 200 nm.

[0023] In some preferred embodiments of the present invention, the chemical formula of the lithium supplement additive is ALi 5+e Fe 1-e Co e O4 / (1-A)Li 1.33 MnO2 or ALi2Ni 1-f Cu f O2 / (1-A)Li 1.33 MnO2, where 0.8≦A<1; 0≦e≦1; 0≦f≦1.

[0024] A is for Li 5+e Fe 1-e Co e O4 / Li 1.33 Li in MnO2 5+e Fe 1-e Coe Mass fraction of O4 or Li2Ni 1-f Cu f O2 / Li 1.33 Li2Ni in MnO2 1-f Cu f The mass fraction of O2 is shown.

[0025] In some preferred embodiments of the invention, the range of values ​​for A is preferably 0.89≦A≦0.991, for example 0.9, 0.96, 0.97, 0.98 or 0.99.

[0026] In some preferred embodiments of the invention, the value of e is in the range of 0.2≦e≦1, for example, 0.5 or 0.4.

[0027] In some preferred embodiments of the invention, the value of f is in the range of 0.5≦f≦1, for example, 0.8.

[0028] In some preferred embodiments of the present invention, the general chemical formula of component A is Li 6-x M 1 1-y N 1 y O 4-z where 0≦x≦5.95, 0≦y≦1, 0≦z≦2, and M 1 is Fe, Ni, Co, Cu, Al, Mn, Ti, or Si, and N 1 is Fe, Ni, Co, Cu, Al, Mn, Ti, or Si, and the general chemical formula of component B is Li 1+(a / (2+a)) Mn 2a / (2+a) M 2 6 / (2+a)-2 O2, 0.2≦a≦1, M 2 is Fe, Ni, Co, Cu, Al, Mn, Ti, Si, Mg, Zr, Nb, La, Sr or W, and at least a portion of component B is coated on the surface of component A.

[0029] In some preferred embodiments of the present invention, the chemical formula of component A is Li2NiO2, Li2Ni 0.5 Cu 0.5 O2, Li2Ni0.8 Cu 0.2 O2, Li2Ni 0.4 Cu 0.6 O2, Li2Cu2O2, Li5FeO4, Li 5.5 Fe 0.5 Co 0.5 O4, Li 5.2 Fe 0.8 Co 0.2 O4, Li 5.6 Fe 0.4 Co 0.6 The chemical formula of component B is LiO4 or Li6CoO4. 1.33 Mn 0.67 O2, Li 1.26 Mn 0.63 Ni 0.11 O2, Li 1.2 Mn 0.6 Ni 0.2 O2 or Li 1.1 Mn 0.75 Ni 0.25 It's O2.

[0030] In some preferred embodiments of the present invention, the chemical formula of component A is Li2NiO2, Li2Ni 0.5 Cu 0.5 O2, Li2Ni 0.8 Cu 0.2 O2, Li2Ni 0.4 Cu 0.6 O2, Li2Cu2O2, Li5FeO4, Li 5.5 Fe 0.5 Co 0.5 O4, Li 5.2 Fe 0.8 Co 0.2 O4, Li 5.6 Fe 0.4 Co 0.6 The chemical formula of component B is LiO4 or Li6CoO4. 1.33 Mn 0.67 It's O2.

[0031] In some preferred embodiments of the present invention, component A has the formula LiNiO and component B has the formula Li 1.26 Mn 0.63 Ni 0.11 O2, Li 1.2 Mn 0.6Ni 0.2 O2 or Li 1.1 Mn 0.75 Ni 0.25 It's O2.

[0032] In the method for preparing the lithium supplementary additive of the second aspect of the present invention, preferably, the precursor of component A is first sintered to obtain component A, and then mixed with the precursor of component B.

[0033] The precursors of component A may be conventional precursors in the art that can be prepared to satisfy the above general chemical formula of component A, such as Li2O and NiO or Fe2O3 and LiOH. In general, the amount of each component of component A may be selected according to the corresponding stoichiometric amount depending on the resulting chemical formula of component A.

[0034] The temperature and time of the primary sintering may be conventional in the art. In general, the desired temperature and time of the primary sintering also vary depending on the type of component A precursor selected. For example, when the precursors of component A are Li2O and NiO, the temperature of the primary sintering is 600°C and the time of the primary sintering is 12 hours. When the precursors of component A are Fe2O3 and LiOH, the primary sintering is performed in two stages, the temperature of the first stage is 450°C and the time of the first stage is 12 hours, and the temperature of the second stage is 600°C and the time of the second stage is 24 hours.

[0035] Preferably, the precursor of component B may be a conventional precursor in the art, such as MnCO3 and Li2CO3, which can be prepared to satisfy the above general chemical formula of component B. In general, the amount of each component of component B may be selected according to the corresponding stoichiometric amount depending on the chemical formula of component B to be obtained.

[0036] Preferably, the sintering temperature and time may be conventional in the art. In general, the desired sintering temperature and time also vary depending on the type of component B precursor selected. For example, when the component B precursor is MnCO3 and Li2CO3, the sintering temperature is 500°C and the sintering time is 72 hours.

[0037] In the positive electrode sheet of the third embodiment, the mass ratio of the lithium supplementary additive to the total mass of the positive electrode sheet is preferably 0.5% to 31%, for example, 0.9%, 1%, 2%, 5%, 10%, 15%, 18%, 20%, 25%, 28% or 30%.

[0038] Preferably, the lithium iron phosphate is LiFePO4.

[0039] Preferably, the lithium manganese iron phosphate is LiMn 0.6 Fe 0.4 It is PO4.

[0040] Preferably, the nickel-cobalt-manganese ternary material is LiNi 0.9 Co 0.06 Mn 0.04 It's O2.

[0041] Preferably, the lithium cobalt oxide is LiCoO2.

[0042] Preferably, the lithium-rich manganese-based oxide is Li 1.1 Ni 0.4 Mn 0.6 It's O2.

[0043] Preferably, the lithium nickel manganese oxide is LiNi 1.5 Mn 0.5 He is O4.

[0044] In some preferred embodiments of the present invention, the active material is lithium iron phosphate, lithium manganese iron phosphate, nickel-cobalt-manganese ternary material, lithium cobalt oxide, lithium rich manganese oxide, or lithium nickel manganese oxide. The chemical formula of the lithium supplement additive is ALi 5+e Fe 1-e Co e O4 / (1-A)Li 1.33 MnO2 or ALi2Ni 1-f Cu f O2 / (1-A)Li 1.33Specifically, 0.8≦A<1, 0≦e≦1, 0≦f≦1, and A is Li 5+e Fe 1-e Co e O4 / Li 1.33 Li in MnO2 5+e Fe 1-e Co e Mass fraction of O4 or Li2Ni 1-f Cu f O2 / Li 1.33 Li2Ni in MnO2 1-f Cu f The mass fraction of O2 is shown.

[0045] In some preferred embodiments of the present invention, the active agent is LiMn 0.6 Fe 0.4 PO4, and the lithium supplement additive is Li2NiO2 / Li 1.33 Mn 0.67 O2, Li2Ni 0.5 Cu 0.5 O2 / Li 1.33 Mn 0.67 O2, Li2Ni 0.8 Cu 0.2 O2 / Li 1.33 Mn 0.67 O2, Li2Ni 0.4 Cu 0.6 O2 / Li 1.33 Mn 0.67 O2, Li2Cu2O2 / Li 1.33 Mn 0.67 O2, Li5FeO4 / Li 1.33 Mn 0.67 O2, Li 5.5 Fe 0.5 Co 0.5 O4 / Li 1.33 Mn 0.67 O2, Li 5.2 Fe 0.8 Co 0.2 O4 / Li 1.33 Mn 0.67 O2, Li 5.6 Fe 0.4 Co 0.6 O4 / Li 1.33 Mn 0.67 O2, Li6CoO4 / Li 1.33 Mn 0.67O2, Li2NiO2 / Li 1.26 Mn 0.63 Ni 0.11 O2, Li2NiO2 / Li 1.2 Mn 0.6 Ni 0.2 O2 or Li2NiO2 / Li 1.1 Mn 0.75 Ni 0.25 It's O2.

[0046] In some preferred embodiments of the present invention, the active agent is LiMn 0.6 Fe 0.4 PO4, LiFePO4, LiNi 0.9 Co 0.06 Mn 0.04 O2, Li 1.1 Ni 0.4 Mn 0.6 O2, LiCoO2 or LiNi 1.5 Mn 0.5 O4, and the lithium supplement additive is Li2NiO2 / Li 1.33 Mn 0.67 It's O2.

[0047] In the manufacturing method of the positive electrode sheet of the fourth embodiment, the positive electrode current collector may preferably be a conventional positive electrode current collector in the art, typically an aluminum foil.

[0048] Preferably, the drying method may be any method conventional in the art.

[0049] Preferably, the drying temperature may be any temperature conventional in the art, for example 120°C.

[0050] Preferably, the drying time is that conventional in the art, for example 10 minutes.

[0051] Preferably, the slurry also typically includes a conductive agent, a solvent, and an adhesive.

[0052] Specifically, the conductive agent may be a conventional conductive agent in the art, such as conductive carbon black (Super P).

[0053] Specifically, the solvent may be a conventional solvent in the art, and is preferably N-methylpyrrolidone (NMP).

[0054] In particular, the adhesive may be a conventional adhesive in the art, such as polyvinylidene fluoride (PVDF).

[0055] Preferably, when the slurry contains an active material, a lithium supplementary additive, a conductive agent, and a binder, the mass ratio of the “positive electrode active material and the lithium supplementary additive”, the conductive agent, and the binder is (93-98):(1-4):(1-4), for example, 97:1.5:1.5.

[0056] In some preferred embodiments of the present invention, the method for preparing the positive electrode sheet includes coating a slurry containing the active material and the lithium supplement additive on at least one side of an aluminum foil, and drying at 120° C. for 10 minutes.

[0057] In the positive electrode material of the seventh embodiment, the value of A is preferably in the range of 0.89≦A≦0.991, for example, 0.9, 0.96, 0.97, 0.98 or 0.99.

[0058] Preferably, the value of e is in the range 0.2≦e≦1, for example 0.5 or 0.4.

[0059] Preferably, the value of f is in the range 0.5≦f≦1, for example 0.8.

[0060] Preferably, the mass proportion of the lithium supplement additive in the positive electrode material is 0.9% to 31%, for example 1%, 2%, 5%, 10%, 15%, 18%, 20%, 25%, 28% or 30%.

[0061] Preferably, the lithium iron phosphate is LiFePO4.

[0062] Preferably, the lithium manganese iron phosphate is LiMn 0.6 Fe 0.4 It is PO4.

[0063] Preferably, the nickel-cobalt-manganese ternary material is LiNi 0.9 Co 0.06 Mn 0.04 It's O2.

[0064] Preferably, the lithium cobalt oxide is LiCoO2.

[0065] Preferably, the lithium-rich manganese-based oxide is Li 1.1 Ni 0.4 Mn 0.6 It's O2.

[0066] Preferably, the lithium nickel manganese oxide is LiNi 1.5 Mn 0.5 He is O4.

[0067] In some preferred embodiments of the present invention, the active agent is LiMn 0.6 Fe 0.4 PO4, and the lithium supplement additive is Li2NiO2 / Li 1.33 Mn 0.67 O2, Li2Ni 0.5 Cu 0.5 O2 / Li 1.33 Mn 0.67 O2, Li2Ni 0.8 Cu 0.2 O2 / Li 1.33 Mn 0.67 O2, Li2Ni 0.4 Cu 0.6 O2 / Li 1.33 Mn 0.67 O2, Li2Cu2O2 / Li 1.33 Mn 0.67 O2, Li5FeO4 / Li 1.33 Mn 0.67 O2, Li 5.5 Fe 0.5Co 0.5 O4 / Li 1.33 Mn 0.67 O2, Li 5.2 Fe 0.8 Co 0.2 O4 / Li 1.33 Mn 0.67 O2, Li 5.6 Fe 0.4 Co 0.6 O4 / Li 1.33 Mn 0.67 O2, Li6CoO4 / Li 1.33 Mn 0.67 O2, Li2NiO2 / Li 1.26 Mn 0.63 Ni 0.11 O2, Li2NiO2 / Li 1.2 Mn 0.6 Ni 0.2 O2 or Li2NiO2 / Li 1.1 Mn 0.75 Ni 0.25 It's O2.

[0068] In some preferred embodiments of the present invention, the active agent is LiMn 0.6 Fe 0.4 PO4, LiFePO4, LiNi 0.9 Co 0.06 Mn 0.04 O2, Li 1.1 Ni 0.4 Mn 0.6 O2, LiCoO2 or LiNi 1.5 Mn 0.5 O4, and the lithium supplement additive is Li2NiO2 / Li 1.33 Mn 0.67 It's O2.

[0069] Based on common knowledge in the art, the above preferred conditions can be arbitrarily combined to obtain preferred examples of the present invention.

[0070] Example 1

[0071] The manufacturing process of the lithium supplementary additive in Example 1 was as follows: first, component A was prepared, then the precursor of component B was mixed with component A to generate component B on the surface of component A. Specifically, Li2O and NiO in a stoichiometric ratio were taken out, crushed, mixed, and then sintered at 600°C for 12 hours under N2 to obtain component A (Li2NiO2). Next, 0.9M Li2NiO2 was taken out, uniformly mixed with the precursor of component B (0.02M MnCO3, 0.02M Li2CO3), and sintered at 500°C for 72 hours to prepare the lithium supplementary additive (wherein component B was partially coated on the surface of component A, and the chemical formula of component B is Li2NiO2 / Li 1.33 Mn 0.67 (represented by O2).

[0072] The positive electrode material in the positive electrode sheet of Example 1 was LiMn 0.6 Fe 0.4 PO4 (component C, i.e., active material) and Li2NiO2 / Li 1.33 The positive electrode sheet positive electrode material further contained conductive carbon black (Super P) and polyvinylidene fluoride (PVDF). LiMnO2 (component A + component B, i.e., lithium supplement additive), where the proportion of component C in the total mass of "component A + component B + component C + Super P + PVDF" was 92.15%, and the mass proportion of "component A + component B" in the total mass of "component A + component B + component C" was 5%. 0.6 Fe 0.4 PO4 is Li2NiO2 / Li 1.33 It did not react with MnO2, but was merely physically mixed. The mass ratio of "Component A + Component B + Component C", Super P, and PVDF was 97:1.5:1.5.

[0073] The method for preparing the positive electrode sheet of Example 1 includes the following steps. First, the active material, Super P, and PVDF were mixed in the above ratio, and then N-methylpyrrolidone (NMP) was gradually added while stirring at high speed to prepare a positive electrode slurry having a certain viscosity. Next, the prepared slurry was uniformly applied onto an aluminum foil and dried for 10 minutes in a 120°C air drying oven. Finally, the dried electrode sheet was rolled and cut to prepare a positive electrode sheet.

[0074] The specific manufacturing process of the lithium supplement additive in Example 24 is to mix Fe2O3 and LiOH in a ratio of 1:10, then sinter at 450℃ under N2 for 12 hours, and cool to form. After grinding, the mixture is sintered at 600℃ under N2 for 24 hours to obtain LFO, i.e., component A (Li5FeO4), and then 0.9M Li5FeO4 is taken out and uniformly mixed with the precursor of component B (0.02M MnCO3, 0.02M Li2CO3) and sintered at 500℃ for 72 hours.

[0075] In Examples 2 to 6, the type of component C in the positive electrode material was changed (as shown in Table 2), and other experimental conditions were all the same as those in Example 1. Component C may be a conventional commercially available product.

[0076] In Examples 7 to 13, the mass ratio of "Component A + Component B" in the positive electrode material was changed (as shown in Table 2), but the other experimental conditions were all the same as in Example 1.

[0077] In Examples 14 to 19, all the experimental conditions were the same as in Example 1, except that the mass ratio of Component A to the total mass of "Component A + Component B" was changed (as shown in Table 2).

[0078] In Examples 20 to 28, the type of component A was changed (as shown in Table 1), but all other experimental conditions were the same as in Example 1. When component A is LixFeOy, the precursors of component A are Fe2O3 and LiOH, and the relative mass ratios of each precursor can be adjusted according to the final chemical formula of the designed component A. When component A is LixNiCuO, the precursors of component A are NiO, CuO, and Li2O, and the relative mass ratios of each precursor can be adjusted according to the final chemical formula of the designed component A.

[0079] In Examples 29 to 31, the type of component B was changed (as shown in Table 1), but all other experimental conditions were the same as in Example 1. The precursors of component B were Li2CO3, MnCO3, NiCO3, and CoCO3, and the relative mass ratio of each precursor could be adjusted according to the final chemical formula of the designed component B.

[0080] The lithium supplement additives (Component A+Component B) produced in Examples 1 to 31 had a core-shell structure. Specifically, the average particle size of the core was 0.5 μm to 15 μm, and the average thickness of the shell was 20 nm to 200 nm.

[0081] Example 2

[0082] LiFePO4 (component C)

[0083] Li2NiO2 / Li 1.33 MnO2 (component A + component B)

[0084] Specifically, the proportion of component C in the total mass of "component A + component B + component C + Super P + PVDF" was 92.15%. The mass proportion of "component A + component B" in the total mass of "component A + component B + component C" was 5%.

[0085] Cycle test voltage range: 2.5V~3.65V

[0086] Example 3

[0087] LiNi 0.9 Co0.06 Mn 0.04 O2 (component C)

[0088] Li2NiO2 / Li 1.33 MnO2 (component A+ component B)

[0089] Specifically, the proportion of component C in the total mass of "component A + component B + component C + Super P + PVDF" was 92.15%. The mass proportion of "component A + component B" in the total mass of "component A + component B + component C" was 5%.

[0090] Cycle test voltage range: 2.8V~4.2V

[0091] Example 4

[0092] LiNi 1.5 Mn 0.5 O4 (component C)

[0093] Li2NiO2 / Li 1.33 MnO2 (component A + component B)

[0094] Specifically, the proportion of component C in the total mass of "component A + component B + component C + Super P + PVDF" was 92.15%. The mass proportion of "component A + component B" in the total mass of "component A + component B + component C" was 5%.

[0095] Cycle test voltage range: 2.8V~4.45V

[0096] Example 5

[0097] LiCoO2 (component C)

[0098] Li2NiO2 / Li 1.33 MnO2 (component A+ component B)

[0099] Specifically, the proportion of component C in the total mass of "component A + component B + component C + Super P + PVDF" was 92.15%. The mass proportion of "component A + component B" in the total mass of "component A + component B + component C" was 5%.

[0100] Cycle test voltage range: 2.8V~4.7V

[0101] The main condition parameters included in the examples are as shown in Table 1 below. [Table 1] JPEG2024155700000002.jpg207166JPEG2024155700000003.jpg52166

[0102] Examples of Effects

[0103] (1) Rebound test of solid content and viscosity

[0104] Test subjects: positive electrode sheets produced in Examples 1 to 31 and Comparative Examples 1 to 8.

[0105] Test method: The viscosity of the positive electrode slurry was adjusted to 5000±500 mPa·s, the actual solid content was tested, and the positive electrode slurry was placed in a 500 mL beaker for 12 hours and the viscosity was tested again.

[0106] Test results: As shown in Table 2 below.

[0107] The manufacturing method of the test battery in the examples (2) to (4) for the following effects is as follows. The prepared positive electrode sheet and graphite negative electrode sheet were mounted to prepare a 1 Ah soft-pack battery. After the liquid was injected, a chemical conversion treatment of 4.5 V was carried out (that is, the first charging process of the battery after the liquid was injected, which activates the active material in the battery and activates the lithium battery). Then, after the aging process, a new battery was obtained.

[0108] (2) Capacity test

[0109] Test method: A battery cell equipped with a positive electrode prepared in the example was charged at 25°C, 2.0V to 4.2V, and 0.33°C with a constant current and constant voltage (end current 0.05C), and then discharged at a constant current of 0.33C. The discharge capacity is the capacity.

[0110] Test results: As shown in Table 2 below.

[0111] (3) Cycle testing

[0112] Test method: A battery cell incorporating the positive electrode prepared in the example was charged and discharged 500 times at 45° C. and 1C in the range of 2.5 V to 4.2 V, and the capacity ratio at the 500th cycle to the 1st cycle was recorded as the capacity retention rate.

[0113] Test results: As shown in Table 2 below.

[0114] (4) Storage gas production test

[0115] Test method: A battery cell equipped with the positive electrode prepared in the example was fully charged and stored at 60℃ and 4.2V. The capacity difference between the 30th day and the 1st day was recorded, and this value was divided by the capacity on the 1st day to calculate the storage capacity increase rate.

[0116] Test results: As shown in Table 2 below. [Table 2] JPEG2024155700000005.jpg246166JPEG2024155700000006.jpg244166

[0117] The data in Tables 1-2 are analyzed to find the following. In Examples 7-13, only the mass ratio of "component A + component B" in the "total mass of component A + component B + component C" is changed compared to Example 1, and the other conditions are the same. Therefore, the gram capacity, cycle capacity retention rate at 45°C, and storage capacity increase rate at 60°C are affected to various degrees. Specifically, when the mass ratio of "component A + component B" in the "total mass of component A + component B + component C" is 5% or less, for example, 1% to 5%, the gram capacity and cycle capacity retention rate at 45°C also increased as the mass ratio increased, and the storage capacity increase rate at 60°C decreased. When the mass ratio of "component A + component B" in the "total mass of component A + component B + component C" is more than 5% and 35% or less, for example, 5% to 31%, the gram capacity and cycle capacity retention rate at 45°C decreased as the mass ratio increased, and the storage capacity increase rate at 60°C increased.

[0118] Compared with Example 1, Examples 14 to 19 only change the mass ratio of component A in the "total mass of component A + component B", and the other conditions are the same. Therefore, the gram capacity, cycle capacity retention rate at 45 ° C, and storage capacity increase rate at 60 ° C are affected to various degrees. Specifically, when the mass ratio of component A to the "total mass of component A + component B" is more than 89%, for example, 98% to 99.1%, as the mass ratio increases, the gram capacity and cycle capacity retention rate at 45 ° C basically do not change, and the storage capacity increase rate at 60 ° C increases. When the mass ratio of component A to the "total mass of component A + component B" is less than 98%, such as 89% to 97%, as the mass ratio decreases, the gram capacity and cycle capacity retention rate at 45 ° C slightly decrease, and the storage capacity increase rate at 60 ° C decreases.

[0119] Compared with Example 1, Examples 20 to 28 only changed the type of component A, and the other conditions were the same. The gram capacity, cycle capacity retention rate at 45°C, and storage capacity increase rate at 60°C were affected to various degrees. For example, in Example 23, when component A was Li2Cu2O2, the gram capacity was 134.8mAh / g, the cycle capacity retention rate at 45°C was 92.4%, and the storage capacity increase rate at 60°C was 4.6%. Compared with Examples 1, 20 to 22, and 24 to 28, Example 23 had the smallest storage capacity increase rate at 60°C.

[0120] Compared with Example 1, Examples 29 to 31 only changed the type of component B, and the other conditions were the same. The gram capacity, cycle capacity retention rate at 45°C, and storage capacity increase rate at 60°C were affected to various degrees. For example, in Example 1, component B was Li 1.33 Mn 0.67 In the case of O2, the gram capacity was (137.6 mAh / g), the cycle capacity retention rate at 45°C was (92.8%), and the storage capacity increase rate at 60°C was (5.3%), all of which were better than those of Examples 29 to 31.

[0121] Compared with Example 1, Li2NiO2 / Li 1.33 Mn 0.67 Although O2 was not included in Comparative Example 1, the gram capacity and cycle capacity retention rate at 45°C of Comparative Example 1 both decreased, and the storage capacity increase rate at 60°C increased.

[0122] Compared with Example 2, Li2NiO2 / Li 1.33 Mn 0.67 Although O2 was not included in Comparative Example 2, the gram capacity and cycle capacity retention rate at 45°C of Comparative Example 2 both decreased, and the storage capacity increase rate at 60°C increased.

[0123] Compared with Example 3, Li2NiO2 / Li 1.33 Mn 0.67 Although O2 was not included in Comparative Example 3, the gram capacity and cycle capacity retention rate at 45°C of Comparative Example 3 both decreased, and the storage capacity increase rate at 60°C increased.

[0124] Compared with Example 4, Li2NiO2 / Li 1.33 Mn 0.67 Although O2 was not included in Comparative Example 4, the gram capacity and cycle capacity retention rate at 45°C in Comparative Example 4 both decreased, and the storage capacity increase rate at 60°C increased.

[0125] Compared with Example 5, Li2NiO2 / Li 1.33 Mn 0.67 Although O2 was not included in Comparative Example 5, the gram capacity and cycle capacity retention rate at 45°C of Comparative Example 5 both decreased, and the storage capacity increase rate at 60°C increased.

[0126] Compared with Example 6, Li2NiO2 / Li 1.33 Mn 0.67 Although O2 was not included in Comparative Example 6, the gram capacity and cycle capacity retention rate at 45°C of Comparative Example 6 both decreased, and the storage capacity increase rate at 60°C increased.

[0127] Compared with Examples 1 to 19, Comparative Example 7 did not contain "Component A + Component B", but the gram capacity and cycle capacity retention rate at 45°C of Comparative Example 7 both decreased, and the storage capacity increase rate at 60°C increased.

[0128] Compared with Example 24, Comparative Example 8 does not contain "Component A + Component B", but the gram capacity and cycle capacity retention rate at 45°C of Comparative Example 8 both decreased significantly, and the storage capacity increase rate at 60°C increased significantly.

[0129] By analyzing the above data, the inventors concluded that the reasons for the above experimental phenomenon are as follows: 1. Increasing the amount of lithium supplementary additive "component A + component B" relative to active material component C improves cycling and storage. However, the lithium supplementary additive "component A + component B" has poor electrical conductivity, and too much of it will adversely affect the electrical properties of the positive electrode material, leading to the deterioration of the positive electrode material.

[0130] 2. The main function of component B is to stabilize component A, and the secondary function is to supply lithium, while the main function of component A is to supply lithium. Increasing the amount of component B improves the stability of the lithium supplement additive "component A + component B", but if there is too much component B, the lithium supplement effect of the lithium supplement additive "component A + component B" will decrease.

[0131] 3. Different types of component A have different electrochemical properties.

[0132] Furthermore, the inventors have found through experiments that by adjusting the firing temperature, component B in the lithium supplementary additive can be more uniformly coated on the surface of component A. Specifically, the Mn source in the precursor of component B is first fired at a low temperature (e.g., 300°C to 500°C) to be coated on the surface of component A, and then fired at a high temperature (e.g., 600°C to 900°C) to react with the Li source in the precursor of component B, so that component B can better form a lithium supplementary additive in which component B is more uniformly coated on the surface of component A. [Industrial Applicability]

[0133] The positive electrode material containing the lithium supplement additive of the present invention has higher stability and higher theoretical capacity, and is used in lithium ion batteries to improve the energy density and cycle stability of the batteries.

[0134] The above describes in more detail the objectives, technical solutions and advantageous effects of the present invention through specific embodiments. It should be understood that the above description is only a specific embodiment of the present invention, and does not limit the present invention. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principle of the present invention shall be included within the scope of the present invention.

Claims

1. Contains component A and component B, The general chemical formula of component A is Li 6-x M 1 1-y N 1 y O 4-z where 0≦x≦5.95, 0≦y≦1, 0≦z≦2, and M 1 is selected from one or more of Fe, Ni, Co, Cu, Al, Mn, Ti, and Si; 1 is selected from one or more of Fe, Ni, Co, Cu, Al, Mn, Ti, Si; The general chemical formula of component B is Li 1+(a/(2+a)) Mn 2a/(2+a) M 2 6/(2+a)-2 O 2 , 0.2≦a≦1, and M 2 is selected from one or more of Fe, Ni, Co, Cu, Al, Mn, Ti, Si, Mg, Zr, Nb, La, Sr, W; At least a portion of said component B is located on the surface of said component A.

2. 2. The lithium supplement additive of claim 1, which satisfies one or more of the following conditions a to c: a. The M 1 is Fe, Ni, Co, Cu, Al, Mn, Ti, or Si. b. The N 1 is Fe, Ni, Co, Cu, Al, Mn, Ti, or Si. c. Said M 2 is Fe, Ni, Co, Cu, Al, Mn, Ti, Si, Mg, Zr, Nb, La, Sr, or W.

3. 2. The lithium supplement additive of claim 1, which satisfies one or more of the following conditions d to j: d) The value of x is in the range of 0≦x≦5. e) The value of y is in the range of 0≦y≦0.

9. f) The value of z is in the range of 0≦z≦2. g. The value of a is in the range of 0.22≦a≦1. h) At least a portion of the component B is coated on the surface of the component A. i. The mass ratio of component A to the total mass of “component A and component B” is 89% to 99.1%. j) The lithium supplement additive is a core-shell structure.

4. The chemical formula of the lithium supplement additive is ALi 5+e Fe 1-e Co e O 4 / (1-A) Li 1.33 MnO 2 Or ALi 2 Ni 1-f Cu f O 2 / (1-A) Li 1.33 MnO 2 and In the formula, 0.8≦A<1; 0≦e≦1; 0≦f≦1. A is Li 5+e Fe 1-e Co e O 4 / Li 1.33 MnO 2 Li in 5+e Fe 1-e Co e O 4 Mass ratio of Li 2 Ni 1-f Cu f O 2 / Li 1.33 MnO 2 Li in 2 Ni 1-f Cu f O 2 2. The lithium supplement additive according to claim 1, wherein the weight percentage of

5. The general chemical formula of component A is Li 6-x M 1 1-y N 1 y O 4-z where 0≦x≦5.95, 0≦y≦1, 0≦z≦2, and M 1is Fe, Ni, Co, Cu, Al, Mn, Ti, or Si, and N 1 is Fe, Ni, Co, Cu, Al, Mn, Ti, or Si, and the general chemical formula of component B is Li 1+(a/(2+a)) Mn 2a/(2+a) M 2 6/(2+a)-2 O 2 , 0.2≦a≦1, and M 2 is Fe, Ni, Co, Cu, Al, Mn, Ti, Si, Mg, Zr, Nb, La, Sr or W, and at least a portion of B is coated on the surface of component A.

6. 2. The method of claim 1, comprising the step of mixing and sintering the precursors of components A and B to obtain the lithium supplementary additive.

7. An electrochemical device comprising a positive electrode sheet, a negative electrode sheet, a separator, and an electrolyte, the positive electrode sheet comprising a positive electrode current collector, a positive electrode active material layer disposed on at least one surface of the positive electrode current collector, and a lithium supplement additive; the positive electrode active material layer includes an active material, the active material including one or more of lithium iron phosphate, lithium manganese iron phosphate, nickel-cobalt-manganese ternary material, lithium-rich manganese oxide, and lithium nickel manganese oxide; The lithium iron phosphate and the lithium manganese iron phosphate each independently have the structural formula: Li a Mn m Fe 1-m-n M 3 n P.O. 4 In the formula, 0.9≦a≦1.10, 0≦m≦1.0, 0≦n≦0.02, 0.5≦m / (1−m−n)≦0.9, and M 3 The elements include one or more of Ti, Mg, Ni, Co, Al, V, Cr, Zr, Nb; The nickel-cobalt-manganese ternary material has the structural formula: Li 1+a [Ni x Co y Mn z N 2 1-x-y-z ]O 2-b A b , 0.7≦x<1, 0≦y<0.3, 0≦z<0.3, −0.2<a<0.2, 0≦b<0.1 are satisfied, wherein N 2 The elements include one or more of Sr, Y, Al, Ti, Mg, W, Mo, B, V, Se, Nb, Ru, Rh, Pd, Sb, Te, Ce, Ca, Zn, Ni, Co, Mn, Zr, and the A elements include one or more of F, N, Cl, S, P; The lithium cobalt oxide has the structural formula: Li a Co 1-b M 4 b O 2-b In the formula, M 4 the elements are selected from one or more of Na, Mg, Al, Ti, Zr, Y, Ha, Ni, Mn, V, Cr, La, Ce, 0.99≦a≦1.01, 0<b≦0.05; The lithium-rich manganese oxide has the structural formula: 2 MnO 3 (1-z)LiM 5 O 2 , 0≦z≦1, and M 5 is selected from one or more of Ni, Co, Mn; The lithium nickel manganese oxide has the structural formula: LiM 6 x+y Ni 0.5-x Mn 1.5-y O 4 In the formula, M 6 the elements are selected from one or more of Co, Al, Cr, Fe, Mg, Zr, and Ti, 0≦x<0.2, 0≦y<0.2; The lithium supplemental additive comprises component A and component B, The general chemical formula of component A is Li 6-x M 1 1-y N 1 y O 4-z where 0≦x≦5.95, 0≦y≦1, 0≦z≦2, and M 1is selected from one or more of Fe, Ni, Co, Cu, Al, Mn, Ti, and Si; 1 is selected from one or more of Fe, Ni, Co, Cu, Al, Mn, Ti, Si; The general chemical formula of component B is Li 1+(a/(2+a)) Mn 2a/(2+a) M 2 6/(2+a)-2 O 2 , 0.2≦a≦1, and M 2 is selected from one or more of Fe, Ni, Co, Cu, Al, Mn, Ti, Si, Mg, Zr, Nb, La, Sr, W; At least a portion of said component B is located on a surface of said component A.

8. The active material is lithium iron phosphate, lithium manganese iron phosphate, nickel-cobalt-manganese ternary material, lithium cobalt oxide, lithium-rich manganese oxide, or lithium nickel manganese oxide, and the lithium supplement additive has the chemical formula: ALi 5+e Fe 1-e Co e O 4 / (1-A) Li 1.33 MnO 2 , or ALi 2 Ni 1-f Cu f O 2 / (1-A) Li 1.33 MnO 2 and In the formula, 0.8≦A<1; 0≦e≦1; 0≦f≦1, and A is Li 5+e Fe 1-e Co e O 4 / Li 1.33 Li in MnO 5+e Fe 1-e Co e O 4 Mass ratio of Li 2 Ni 1-f Cu f O 2 / Li 1.33 MnO 2 Li in 2 Ni 1-f Cu f O 2 The electrochemical device according to claim 7 , wherein the mass proportion of

9. An electronic device comprising the electrochemical device of claim 7.

Citation Information

Patent Citations

  • Method for preparing surface-coated high-voltage positive electrode material of lithium ion battery

    CN103594696A