Method for manufacturing lithium secondary battery, and lithium secondary battery manufactured thereby

A bimodal positive electrode material with boron and cobalt coatings for lithium composite transition metal oxides addresses irreversible capacity loss in lithium secondary batteries, enhancing efficiency and lifespan.

JP2024155978AActive Publication Date: 2024-10-31LG ENERGY SOLUTION LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024144226
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-11-27
Filing Date
2024-08-26
Publication Date
2024-10-31
Estimated Expiration
2041-10-22

AI Technical Summary

Technical Problem

Lithium secondary batteries face challenges with high irreversible capacity loss due to negative electrode materials like silicon, leading to reduced lithium consumption and decreased energy efficiency.

Method used

A bimodal positive electrode material is created by mixing small and large particle lithium composite transition metal oxides with boron and cobalt coatings, respectively, to form a bimodal particle size distribution, which compensates for irreversible capacity loss and enhances initial charge/discharge efficiency.

Benefits of technology

The method improves the output characteristics and high-temperature lifespan of lithium secondary batteries by reducing lithium consumption and minimizing resistance increases.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024155978000001_ABST
    Figure 2024155978000001_ABST
Patent Text Reader

Abstract

To provide a lithium secondary battery capable of ultimately reducing only a lithium consumption amount without reducing resistance and life properties by introducing a positive electrode material to mitigate the issues caused by a negative electrode material having a large irreversible capacity loss.SOLUTION: A method for manufacturing a lithium secondary battery comprises the following steps (1)-(5). (1) a step of mixing and heating a small particle lithium composite transition metal oxide having an average particle size (D50) of less than 7 μm with a boron-containing material to manufacture a first positive electrode active material; (2) a step of mixing and heating a large particle lithium composite transition metal oxide having an average particle size (D50) of 8 μm or more with a cobalt-containing material and a boron-containing material to manufacture a second positive electrode active material; (3) a step of mixing the first positive electrode active material with the second positive electrode active material to manufacture a positive electrode material having a bimodal particle size distribution; (4) a step of coating the positive electrode material onto a positive electrode current collector to manufacture a positive electrode; and (5) a step of assembling the positive electrode, a negative electrode containing a silicon-based negative electrode active material and a separation membrane.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of the filing date of Korean Patent Application No. 10-2020-0162322, filed with the Korean Intellectual Property Office on November 27, 2020, the entire contents of which are incorporated herein by reference.

[0002] The present invention relates to a method for manufacturing a lithium secondary battery and a lithium secondary battery manufactured thereby. [Background technology]

[0003] In recent years, with the rapid spread of electronic devices using batteries, such as mobile phones, notebook computers, and electric vehicles, the demand for secondary batteries that are small, lightweight, and have a relatively high capacity is rapidly increasing. In particular, lithium secondary batteries are lightweight and have high energy density, and are in the spotlight as a driving power source for portable devices. As a result, research and development efforts are being actively made to improve the performance of lithium secondary batteries.

[0004] Carbonaceous materials such as graphite are mainly used as the negative electrode material for lithium secondary batteries, but carbonaceous materials have a drawback in that it is difficult to increase the capacity of lithium secondary batteries because the capacity per unit mass is small. For this reason, materials that form intermetallic compounds with lithium, such as silicon, tin, and oxides of these materials, have been developed and used as non-carbonaceous negative electrode materials that exhibit higher capacity than carbonaceous materials, but these negative electrode materials have a problem in that they have a large irreversible capacity loss during initial charging and discharging.

[0005] To overcome this problem, methods have been proposed to overcome the irreversible capacity loss of the negative electrode by using a material as a positive electrode that can provide a lithium ion source or reservoir and is electrochemically active after the first cycle so as not to degrade the overall performance of the battery. Specifically, a lithium nickel-based oxide such as Li2NiO2 is used as a sacrificial positive electrode material or an overdischarge protection agent in the positive electrode.

[0006] However, most of the lithium nickel-based oxides are expensive and have problems in that they generate a large amount of lithium by-products, resulting in a large amount of gas generation. Therefore, an alternative method is required. Summary of the Invention [Problem to be solved by the invention]

[0007] The present invention provides a lithium secondary battery that can ultimately reduce the amount of lithium consumed without degrading the resistance and life characteristics by introducing a positive electrode material that compensates for the problem of a negative electrode material having a large irreversible capacity loss. [Means for solving the problem]

[0008] The present invention relates to (1) Average particle size (D 50 ) is mixed with a boron-containing raw material and heat-treated to produce a first positive electrode active material; (2) Average particle size (D 50 A step of mixing the large particle lithium composite transition metal oxide having a particle size of 8 μm or more with a cobalt-containing raw material and a boron-containing raw material and heat-treating the mixture to produce a second positive electrode active material; (3) mixing the first positive electrode active material and the second positive electrode active material to prepare a positive electrode material having a bimodal particle size distribution; (4) coating the positive electrode material onto a positive electrode current collector to produce a positive electrode; (5) assembling the positive electrode, a negative electrode including a silicon-based negative electrode active material, and a separator; The present invention provides a method for producing a lithium secondary battery, comprising:

[0009] The present invention also provides a lithium secondary battery comprising a positive electrode including a positive electrode material having a bimodal particle size distribution, a negative electrode including a silicon-based negative electrode active material, and a separator, The positive electrode material includes a first positive electrode active material and a second positive electrode active material, The first positive electrode active material has an average particle size (D 50) is less than 7 μm, and a boron-containing coating layer formed on the small-particle lithium composite transition metal oxide, The second positive electrode active material has an average particle size (D 50 and a coating layer containing cobalt and boron formed on the large-particle lithium composite transition metal oxide. Effect of the Invention

[0010] The method for manufacturing a lithium secondary battery according to the present invention makes it possible to manufacture a lithium secondary battery having improved output characteristics and high-temperature life by using a high-capacity silicon-based negative electrode active material while compensating for the problem of irreversible capacity loss by using a bimodal positive electrode material. [Brief description of the drawings]

[0011] [Figure 1] 1 is an EPMA analysis and SEM photograph of a cross section of a positive electrode prepared in Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention will now be described in more detail to aid in its understanding.

[0013] In this specification, the term "average particle size (D 50 The average particle size (D) is defined as the particle size corresponding to 50% of the cumulative volume in the particle size distribution curve. 50 ) can be measured, for example, by using a laser diffraction method. More specifically, the lithium composite transition metal oxide particles are dispersed in a dispersion medium, then introduced into a commercially available laser diffraction particle size measuring device (e.g., Microtrac MT 3000) and irradiated with ultrasonic waves of about 28 kHz at an output of 60 W, and the average particle size (D 50 ) can be calculated.

[0014] The method for producing a lithium secondary battery of the present invention includes the following steps (1) to (5). (1) Average particle size (D 50 ) mixing the small particle lithium composite transition metal oxide having a particle size of less than 7 μm with a boron-containing raw material and heat treating the mixture to prepare a first positive electrode active material; (2) Average particle size (D 50 (b) mixing the large particle lithium transition metal composite oxide having a particle size of 8 μm or more with a cobalt-containing raw material and a boron-containing raw material, and heat-treating the mixture to prepare a second positive electrode active material; (3) mixing the first positive electrode active material and the second positive electrode active material to prepare a positive electrode material having a bimodal particle size distribution; (4) coating the positive electrode material onto a positive electrode current collector to produce a positive electrode; and (5) Assembling the positive electrode, a negative electrode including a silicon-based negative electrode active material, and a separator.

[0015] To develop high-capacity cells, it is essential to use silicon-based negative electrode active materials with high capacity. However, silicon-based negative electrode active materials have a low initial charge / discharge efficiency of less than 85%, which poses the problem of a high rate of lithium ion loss due to irreversible reactions.

[0016] Furthermore, when a positive electrode active material with high initial charge / discharge efficiency is used, the charge capacity of the cell decreases, which is disadvantageous in achieving high energy.

[0017] Therefore, by using a low-efficiency positive electrode active material that can provide lithium to the silicon-based negative electrode active material during initial charge / discharge, the loss of lithium ions can be reduced and energy can be increased.

[0018] The method for manufacturing a lithium secondary battery according to the present invention provides a cathode material with improved output and reduced consumption of lithium ions due to low initial charge / discharge efficiency by applying a boron (B) and cobalt (Co) composite coating.

[0019] Boron coating forms a lithium boron oxide (LBO) phase on the surface of the positive electrode active material. This LBO phase has high ionic conductivity, which increases the capacity of the battery and reduces resistance, and its low electrical conductivity can suppress side reactions between the positive electrode surface and the electrolyte.

[0020] Cobalt coating forms cobalt oxide (Co3O4) on the surface of the positive electrode active material during low-temperature heat treatment, which can reduce discharge efficiency and increase initial resistance.

[0021] In the present invention, the composite coating of boron and cobalt can reduce the efficiency to match the silicon-based negative electrode active material without reducing the resistance, and can improve the output and lifespan compared to a coating of boron alone.

[0022] In particular, in a bimodal positive electrode active material consisting of small and large particles, cobalt coating is not applied to the small particles, which have a large specific surface area that significantly affects output performance, but is applied only to the large particles, which have a relatively small specific surface area, thereby minimizing the increase in initial resistance and the decrease in output caused by cobalt oxide.

[0023] Each step will now be described in detail.

[0024] <Production of cathode materials> In the step of producing the first positive electrode active material of the present invention, the average particle size (D 50 The small particle lithium transition metal composite oxide having a particle size of less than 7 μm is mixed with a boron-containing raw material and heat-treated.

[0025] The average particle diameter (D 50 ) may be 2 μm or more and less than 7 μm, preferably 3 μm to 6 μm.

[0026] The boron-containing raw materials include H3BO3, B2O3, B4C, BF3, (C3H7O)3B, (C6H5O)3B, [CH3(CH2)3O]3B, C 13 H 19 It may be one or more selected from O3, C6H5B(OH)2 and B2F4, preferably one or more selected from H3BO3 and B2O3, more preferably H3BO3. H3BO3 has a lower melting point and is more reactive with lithium ions than other boron-containing raw materials, and therefore plays a role in lowering the surrounding reaction temperature, specifically, the role of lowering the reaction temperature of plastic additives that aid grain growth and raw materials with high melting points. The same explanation applies to the boron-containing raw materials used in steps (1) and (2) of the present invention.

[0027] In the step (1), the boron-containing raw material may be mixed in an amount of 0.03% by weight to 0.25% by weight, preferably 0.05% by weight to 0.15% by weight, based on the total content of the small particle lithium composite transition metal oxide. When the content of the boron-containing raw material is 0.03% by weight or more based on the total content of the small particle lithium composite transition metal oxide, the LBO phase, which is a coating layer formed by the lithium by-products such as lithium hydroxide and lithium carbonate present on the surface of the positive electrode active material and boron, is sufficiently formed, and the effect of increasing capacity and decreasing resistance can be sufficiently realized, and the side reaction between the surface of the positive electrode active material and the electrolyte can be prevented. When the content of boron is 0.25% by weight or less, the phenomenon of increasing resistance due to the formation of boron oxide B2O3 can be prevented. Specifically, when the content of boron increases beyond the above range, the amount of boron becomes greater than the amount of lithium by-products that can react to form the LBO phase, and boron oxide B2O3 is formed in addition to LBO and acts as a resistor, which is undesirable in that the resistance may increase.

[0028] The heat treatment in step (1) may be performed at 250°C to 400°C, preferably 280°C to 350°C. When the heat treatment temperature in step (1) is 250°C or higher, it is preferable in that the temperature is sufficient for boron to react with lithium by-products on the surface of the positive electrode active material, and no unreacted boron source remains, while when the temperature is 400°C or lower, the LBO phase is sufficiently generated, which contributes to improving the capacity. When the heat treatment is performed at a temperature higher than this, it is not preferable in that the capacity may decrease because the temperature is higher than the optimal temperature for generating the LBO phase.

[0029] The heat treatment in step (1) may be carried out for 50 minutes to 500 minutes.

[0030] In the step of producing the second positive electrode active material of the present invention, the average particle size (D 50 The large particle lithium transition metal composite oxide having a particle size of 8 μm or more is mixed with a cobalt-containing raw material and a boron-containing raw material, and the mixture is heat-treated.

[0031] The average particle diameter (D 50 ) may be 8 μm or more and 20 μm or less, preferably 9 μm to 16 μm.

[0032] Cobalt coating is not applied to the small particle lithium composite transition metal oxide, which has a relatively small average particle size and therefore a large specific surface area, and thus has a significant effect on output performance. However, cobalt coating is applied to the large particle lithium composite transition metal oxide, which has a relatively small specific surface area, so that the initial charge / discharge efficiency of the positive electrode active material is reduced, but the effects of increased resistance and reduced output can be minimized.

[0033] The mixing in steps (1) and (2) may each be a dry mixing in which mixing is performed without using a solvent.

[0034] The cobalt-containing raw material may be one or more selected from Co3O4, Co(OH)2, Co2O3, Co3(PO4)2, CoF3, Co(OCOCH3)2·4H2O, Co(NO3)·6H2O, Co(SO4)2·7H2O and CoC2O4, preferably one or more selected from Co3O4 and Co(OH)2, more preferably Co(OH)2. Co(OH)2 has a lower melting point than other cobalt-containing raw materials, and therefore has the advantage that it can provide a sufficient cobalt coating effect even if it is heat-treated together with the boron-containing raw material at a temperature suitable for the boron-containing raw material, which has a lower reaction temperature than the cobalt-containing raw material.

[0035] In step (2) of the present invention, the boron-containing raw material and the cobalt-containing raw material are H3BO3 and Co(OH)2, respectively. This combination has the advantage that it can simultaneously achieve the effect of lowering the reaction temperature of the surrounding raw materials of H3BO3, and the coating effect of boron and cobalt at a low temperature due to the relatively low melting point of Co(OH)2.

[0036] In one embodiment of the present invention, the coating raw material components of the first and second positive electrode active materials may be different. More specifically, in the step of producing the first positive electrode active material, no other coating raw material may be mixed except the boron-containing raw material, and in the step of producing the second positive electrode active material, no other coating raw material may be mixed except the cobalt-containing raw material and the boron-containing raw material.

[0037] The heat treatment in step (2) may be performed at 250°C to 400°C, preferably 280°C to 350°C. When the heat treatment temperature in step (2) is 250°C or higher, it is preferable in that the temperature is sufficient to allow the boron and cobalt sources to react, and no unreacted boron and cobalt remain, whereas when the heat treatment temperature is 400°C or lower, the LBO phase is sufficiently generated, which contributes to improving the capacity. When the heat treatment is performed at a temperature higher than this, it is not preferable in that the capacity may decrease, since the temperature is higher than the optimum temperature for generating the LBO phase.

[0038] The heat treatment in step (2) may be carried out for 50 to 500 minutes.

[0039] In the step (2), the cobalt-containing raw material may be mixed in an amount of 0.1% by weight to 1.5% by weight, preferably 0.15% by weight to 1.3% by weight, based on the total content of the large particle lithium composite transition metal oxide. When the content of the cobalt-containing raw material is 0.1% by weight or more based on the total content of the large particle lithium composite transition metal oxide, it is preferable in that cobalt oxide is sufficiently formed to sufficiently play a role in reducing the efficiency of the positive electrode, and when it is 1.5% by weight or less, cobalt oxide is formed at an appropriate level on the surface of the positive electrode active material. When cobalt oxide is excessively formed on the surface of the positive electrode active material, it may cause a decrease in capacity and an increase in resistance.

[0040] In step (2), the boron-containing raw material may be mixed in an amount of 0.03% by weight to 0.25% by weight, preferably 0.05% by weight to 0.15% by weight, based on the total content of the large-particle lithium composite transition metal oxide. When the content of the boron-containing raw material is 0.03% by weight or more based on the total content of the large-particle lithium composite transition metal oxide, the LBO phase, which is a coating layer formed by the lithium by-products such as lithium hydroxide and lithium carbonate present on the surface of the positive electrode active material and boron, is sufficiently formed, thereby fully realizing the effect of increasing capacity and reducing resistance, and side reactions between the surface of the positive electrode active material and the electrolyte can be prevented. When the content of boron is 0.25% by weight or less, the phenomenon of increasing resistance due to the formation of boron oxide B2O3 can be prevented. Specifically, when the content of boron is increased to a range exceeding the above range, the amount of boron becomes greater than the amount of lithium by-products capable of reacting to form the LBO phase, and boron oxide B2O3 is formed in addition to LBO and acts as a resistor, which is undesirable in that the resistance may increase.

[0041] In the present invention, the lithium composite transition metal oxide is represented by the following chemical formula 1.

[0042] [Chemical Formula 1] Li 1+x (Ni a Co b Mn c M d )O2 In Chemical Formula 1 above, M is one or more selected from W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo, x, a, b, c, and d are respectively 0 ≦ x ≦ 0.2, 0.70 ≦ a < 1, 0 < b ≦ 0.25, 0 < c ≦ 0.25, and 0 ≦ d ≦ 0.1.

[0043] Preferably, in Chemical Formula 1 above, M may be Al.

[0044] Also, a, b, c, and d may respectively preferably be 0.70 ≦ a ≦ 0.90, 0.05 ≦ b ≦ 0.25, 0.05 ≦ c ≦ 0.25, and 0 ≦ d ≦ 0.05, and more preferably 0.80 ≦ a ≦ 0.90, 0.05 ≦ b ≦ 0.15, 0.05 ≦ c ≦ 0.15, and 0 ≦ d ≦ 0.05.

[0045] That is, in the lithium composite transition metal oxide, the content of nickel (Ni) among the total content of transition metals may be 70 mol% or more, preferably 80 mol% or more.

[0046] The method for manufacturing a lithium secondary battery of the present invention includes the step (3) of mixing the first cathode active material and the second cathode active material. In step (3), the first cathode active material and the second cathode active material may be mixed at a weight ratio of 10:90 to 40:60, preferably 15:85 to 30:70, and may be present within the same content range in the manufactured cathode material.

[0047] <Manufacture of Cathode> In the step of manufacturing the positive electrode of the present invention, the positive electrode material is coated on a positive electrode current collector. This may be performed by a normal positive electrode manufacturing method, except for using the above-mentioned positive electrode material. Specifically, the positive electrode may be manufactured by applying a positive electrode slurry containing the above-mentioned positive electrode material and, optionally, a binder and a conductive material, onto a positive electrode current collector, followed by drying and rolling.

[0048] The positive electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity. For example, stainless steel; aluminum; nickel; titanium; baked carbon; or aluminum or stainless steel whose surface has been treated with carbon, nickel, titanium, silver, or the like can be used.

[0049] The solvent for the positive electrode slurry may be an organic solvent such as NMP (N-methyl-2-pyrrolidone), and may be used in an amount that provides a preferred viscosity when the positive electrode material and, optionally, a binder and a conductive material are included. For example, the positive electrode slurry may be contained so that the solid content concentration is 10% by weight to 90% by weight, preferably 40% by weight to 85% by weight.

[0050] The binder in the positive electrode slurry is a component that aids in bonding between the positive electrode material and the conductive material and to the current collector, and is usually added in an amount of 1% by weight to 30% by weight based on the total weight of the solid content in the positive electrode slurry. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene termonomer, styrene-butadiene rubber, fluororubber, and various copolymers thereof.

[0051] The conductive material in the positive electrode slurry is a substance that does not cause a chemical change in the battery and imparts conductivity, and may be added in an amount of 0.5% by weight to 20% by weight based on the total weight of the solid content in the positive electrode slurry.

[0052] Examples of conductive materials that can be used include carbon blacks such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; graphite powders such as natural graphite, artificial graphite, and graphite with highly developed crystal structures; conductive fibers such as carbon fibers and metal fibers; conductive powders such as carbon fluoride powder, aluminum powder, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.

[0053] The positive electrode material may be contained in an amount of 80% by weight to 99% by weight, specifically 90% by weight to 99% by weight, based on the total weight of the solid content in the positive electrode slurry. If the content of the positive electrode material is 80% by weight or less, the energy density may be reduced, and the capacity may be reduced.

[0054] <Production of negative electrodes> The negative electrode according to the present invention includes a silicon-based negative electrode active material, and may be prepared by coating a negative electrode current collector with a negative electrode slurry including a negative electrode active material, a binder, a conductive material, a solvent, and the like, followed by drying and rolling.

[0055] The negative electrode current collector generally has a thickness of 3 μm to 500 μm. Such a negative electrode current collector is not particularly limited as long as it does not cause a chemical change in the battery and has high conductivity. For example, copper, stainless steel, aluminum, nickel, titanium, fired carbon, those obtained by surface-treating the surface of copper or stainless steel with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. can be used. Also, similar to the positive electrode current collector, fine irregularities can be formed on the surface to strengthen the bonding force of the negative electrode active material, and it can be used in various forms such as films, sheets, foils, nets, porous bodies, foams, non-woven fabrics, etc.

[0056] In the present invention, the silicon-based negative electrode active material is Si, S i O x (0 < x < 2) and Si - Y alloy (wherein Y is an element selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements, transition metals, rare earth elements, and combinations thereof, and is not Si), and is one or more selected therefrom, preferably Si or SiO.

[0057] Since the silicon-based negative electrode active material has a capacity nearly about 10 times higher than that of graphite, the mass loading (mg·cm -2 ) can be lowered to improve the rapid charging performance of the battery. However, there is a problem that the loss rate of lithium ions due to the irreversible reaction is high, but by applying the above-described positive electrode material, such a problem can be solved.

[0058] The anode of the present invention may further include a carbon-based anode active material in addition to the silicon-based anode active material. Any carbon-based anode active material commonly used in lithium ion secondary batteries may be used without particular limitation, and representative examples thereof include crystalline carbon, amorphous carbon, or both. Examples of the crystalline carbon include graphite such as amorphous, plate-like, flake-like, spherical, or fibrous natural graphite or artificial graphite, and examples of the amorphous carbon include soft carbon (low-temperature calcined carbon), hard carbon, mesophase pitch carbide, and calcined coke.

[0059] In the present invention, the silicon-based negative electrode active material may be contained in an amount of 1 wt % to 100 wt %, preferably 3 wt % to 10 wt %, based on the total weight of the negative electrode active material.

[0060] The negative electrode active material may be contained in an amount of 80% by weight to 99% by weight based on the total weight of the solid content in the negative electrode slurry.

[0061] The binder is a component that aids in bonding between the conductive material, the negative electrode active material, and the current collector, and may be added in an amount of 1% by weight to 30% by weight based on the total weight of the solid content in the negative electrode slurry. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer, styrene-butadiene rubber, fluororubber, and various copolymers thereof.

[0062] The conductive material is a component for further improving the conductivity of the negative electrode active material, and may be added in an amount of 1% by weight to 20% by weight based on the total weight of the solid content in the negative electrode slurry. Such a conductive material is not particularly limited as long as it does not cause a chemical change in the battery and has conductivity, and examples thereof include carbon black such as acetylene black, ketjen black, channel black, furnace black, lamp black, or thermal black; graphite powder such as natural graphite, artificial graphite, or graphite with a highly developed crystal structure; conductive fibers such as carbon fibers or metal fibers; conductive powders such as carbon fluoride powder, aluminum powder, or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive materials such as polyphenylene derivatives.

[0063] The solvent for the negative electrode slurry may include water or an organic solvent such as NMP or alcohol, and may be used in an amount that provides a preferred viscosity when the negative electrode active material, binder, conductive material, etc. are included. For example, the solvent may be included so that the concentration of solids in the slurry containing the negative electrode active material, binder, and conductive material is 50% by weight to 75% by weight, preferably 50% by weight to 65% by weight.

[0064] <Manufacturing lithium secondary batteries> The method for producing a lithium secondary battery of the present invention includes a step (5) of assembling the positive electrode, a negative electrode containing a silicon-based negative electrode active material, and a separator.

[0065] Specifically, in step (5), the positive and negative electrodes are stacked and dried in sequence with a separator interposed therebetween to produce a battery assembly, which is then inserted into a case, and an electrolyte is injected and sealed to produce a lithium secondary battery.

[0066] The separator separates the positive electrode and the negative electrode to provide a passage for lithium ions to move. Any separator that is generally used in lithium secondary batteries can be used without any particular restrictions, and is particularly preferred to have low resistance to the movement of electrolyte ions and excellent electrolyte humidification. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting glass fiber, polyethylene terephthalate fiber, etc., can also be used. In addition, a coated separator containing a ceramic component or a polymeric substance can be used to ensure heat resistance or mechanical strength, and can be selectively used as a single layer or multilayer structure.

[0067] Examples of the electrolyte include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries, but are not limited to these.

[0068] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0069] The organic solvent can be used without any particular limitation as long as it serves as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvent can be an ester solvent such as methyl acetate, ethyl acetate, γ-butyrolactone, or ε-caprolactone; an ether solvent such as dibutyl ether or tetrahydrofuran; a ketone solvent such as cyclohexanone; an aromatic hydrocarbon solvent such as benzene or fluorobenzene; dimethylcarbonate (DMC), diethylcarbonate (DEC), ethylmethylcarbonate (EMC), ethylene carbonate (EC), or propylene carbonate (propylene carbonate). Examples of the solvents that can be used include carbonate-based solvents such as ethylene carbonate (PC), alcohol-based solvents such as ethyl alcohol and isopropyl alcohol, nitriles such as R-CN (R is a C2-C20 straight-chain, branched or cyclic hydrocarbon group, which may contain a double bond aromatic ring or an ether bond), amides such as dimethylformamide, dioxolanes such as 1,3-dioxolane, and sulfolanes. Among these, carbonate-based solvents are preferred, and mixtures of cyclic carbonates (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that enhance the charge / discharge performance of the battery and low-viscosity chain carbonate compounds (e.g., ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate) are more preferred. In this case, when the cyclic carbonate and the chain carbonate are mixed at a volume ratio of about 1:1 to about 1:9, excellent electrolyte performance can be achieved.

[0070] The lithium salt can be used without any particular limitation as long as it is a compound capable of providing lithium ions used in lithium secondary batteries. Specifically, the lithium salt can be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, LiB(C2O4)2, or a combination thereof. The concentration of the lithium salt is preferably within the range of 0.1 to 2.0M. When the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, so that it can exhibit excellent electrolyte performance and lithium ions can move effectively.

[0071] In addition to the constituents of the electrolyte, the electrolyte may further contain one or more additives such as haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexamethylphosphoric triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing the decrease in the capacity of the battery, improving the discharge capacity of the battery, etc. Here, the additives may be contained in an amount of 0.1% by weight to 5% by weight based on the total weight of the electrolyte.

[0072] <Lithium secondary battery> The lithium secondary battery according to the present invention comprises: A lithium secondary battery comprising a positive electrode including a positive electrode material having a bimodal particle size distribution, a negative electrode including a silicon-based negative electrode active material, and a separator, The positive electrode material includes a first positive electrode active material and a second positive electrode active material, The first positive electrode active material has an average particle size (D 50) is less than 7 μm, and a boron-containing coating layer formed on the small-particle lithium composite transition metal oxide, The second positive electrode active material has an average particle size (D 50 ) is 8 μm or more, and a cobalt- and boron-containing coating layer formed on the large-particle lithium composite transition metal oxide.

[0073] The lithium secondary battery can be manufactured by the above-mentioned method for manufacturing a lithium secondary battery, and the description of the above-mentioned method for manufacturing a lithium secondary battery can be cited for each component.

[0074] In the lithium secondary battery of the present invention, the coating layers included in the first and second positive electrode active materials can be confirmed using an electron probe micro analyzer (EPMA).

[0075] In one embodiment of the present invention, the coating layer of the first positive electrode active material and the coating layer of the second positive electrode active material are different in constituent components. More specifically, the coating layer of the first positive electrode active material is made of boron, and the coating layer of the second positive electrode active material is made of cobalt and boron.

[0076] The lithium secondary battery according to the present invention can be applied to portable devices such as mobile phones, notebook computers, and digital cameras, and to electric vehicles such as hybrid electric vehicles (HEVs).

[0077] According to another embodiment of the present invention, there is provided a battery module including the lithium secondary battery as a unit cell, and a battery pack including the same.

[0078] The battery module or battery pack can be used as a power source for one or more medium- to large-sized devices, such as a power tool; an electric vehicle (Electric Vehicle, EV), a hybrid electric vehicle, and a plug-in hybrid electric vehicle (PHEV); or a power storage system.

[0079] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, the embodiments of the present invention will be described in detail so that those skilled in the art can easily carry out the present invention. EXAMPLES

[0080] [Examples and Comparative Examples: Production of Positive Electrode] Example 1. Li(Ni) 0.8 Co 0.1 Mn 0.1 )O2(D 50 A lithium composite transition metal oxide represented by the formula (I = 4 μm) and H3BO3 were dry-mixed in a weight ratio of 1:0.05. The mixture was heat-treated at 290°C for 200 minutes in an air atmosphere to prepare a first positive electrode active material having a boron-containing coating layer.

[0081] Separately, Li(Ni 0.8 Co 0.1 Mn 0.1 )O2(D 50 A lithium composite transition metal oxide represented by the formula (I = 13 μm), Co(OH)2, and H3BO3 were dry-mixed in a weight ratio of 1:0.4:0.05. The mixture was heat-treated at 290°C for 200 minutes in an air atmosphere to prepare a second positive electrode active material having a cobalt- and boron-containing coating layer.

[0082] The first and second positive active materials were mixed in a weight ratio of 15:85 to prepare a bimodal positive electrode material.

[0083] The positive electrode material, conductive material (carbon black), and binder (polyvinylidene fluoride, PVdF) were mixed in a weight ratio of 97.5:1.0:1.5 in N-methyl-2-pyrrolidone (NMP) solvent to prepare a positive electrode slurry (solid content: 50 wt%). The positive electrode slurry was applied to one side of an aluminum current collector, which was then dried at 130°C and rolled to prepare a positive electrode.

[0084] Figure 1 shows a cross section of the positive electrode analyzed with an electron probe micro analyzer (EPMA) and photographed with a scanning electron microscope (SEM). In Figure 1, the green part is the Co coating layer, and the peak shown directly above the photograph indicates the Co concentration. Figure 1 shows that the Co coating layer is formed only on the large particles.

[0085] Example 2. In the above Example 1, when preparing the second positive electrode active material, the content of Co(OH)2 was increased so that the weight ratio of the lithium composite transition metal oxide, Co(OH)2 and H3BO3 was 1:1.1:0.05. A positive electrode was prepared in the same manner as in Example 1.

[0086] Example 3. A positive electrode was manufactured in the same manner as in Example 1, except that, in the manufacture of the first positive electrode active material, the content of H3BO3 was increased so that the weight ratio of the lithium composite transition metal oxide and H3BO3 was 1:0.13, and, in the manufacture of the second positive electrode active material, the content of H3BO3 was increased so that the weight ratio of the lithium composite transition metal oxide, Co(OH)2 and H3BO3 was 1:0.4:0.13.

[0087] Comparative Example 1 A positive electrode was manufactured in the same manner as in Example 1, except that no coating layer was formed on either the first positive electrode active material or the second positive electrode active material.

[0088] Comparative Example 2 A positive electrode was manufactured in the same manner as in Example 1, except that in forming the coating layer of the second positive electrode active material, cobalt was not used and only boron coating was applied.

[0089] Comparative Example 3. A positive electrode was manufactured in the same manner as in Example 1, except that no coating layer was formed on the first positive electrode active material, and only a cobalt coating was applied without using boron when forming a coating layer on the second positive electrode active material.

[0090] Comparative Example 4. A positive electrode was manufactured in the same manner as in Example 1, except that, when forming the coating layer of the first positive electrode active material, Co(OH)2 was added so that the weight ratio of the lithium composite transition metal oxide, Co(OH)2, and H3BO3 was 1:0.4:0.05 to form a cobalt- and boron-containing coating layer.

[0091] [Experimental Example] Experimental example 1: Confirmation of capacity and initial resistance An electrode assembly was prepared by interposing a 15 μm-thick polyethylene-based separator between each of the positive electrodes and lithium metal negative electrodes prepared in Examples 1 to 3 and Comparative Examples 1 to 4, and then the electrode assembly was placed inside a battery case, and an electrolyte was then injected into the case to prepare a lithium secondary battery. At this time, an electrolyte solution prepared by dissolving 1M LiPF6 in a mixed organic solvent in which ethylene carbonate (EC):ethyl methyl carbonate (EMC) was mixed in a volume ratio of 1:2 was injected as the electrolyte solution to prepare the lithium secondary battery, and the capacity and resistance at 0.1 C charge and discharge were measured.

[0092] Specifically, the lithium secondary batteries to which the positive electrodes of Examples 1 to 3 and Comparative Examples 1 to 4 were applied were charged at a constant current of 0.1 C at 25° C. up to 4.25 V with a 0.05 C cut-off. Then, the batteries were discharged at a constant current of 0.1 C up to 3.0 V to measure the initial charge / discharge capacity, and the initial resistance was measured by dividing the voltage drop during the initial 10 seconds of discharge by the current value, and is shown in Table 1 below.

[0093] [Table 1]

[0094] From Table 1, it can be seen that the batteries to which the positive electrodes of Examples 1 to 3 are applied have low initial resistance and initial charge / discharge efficiency in combination with a lithium metal negative electrode. This means that it is advantageous in that it can reduce the amount of lithium consumed when used with a silicon-based negative electrode active material with a high lithium ion loss rate. In contrast, the positive electrodes of Comparative Example 1, in which neither the small nor large particles are coated, and Comparative Example 2, in which both the small and large particles are coated with boron alone, have very high initial charge / discharge efficiency in combination with a lithium metal negative electrode, so it is expected that a large amount of lithium ions will be lost when used with a silicon-based negative electrode active material. On the other hand, in the case of the positive electrodes of Comparative Example 3, in which the small particles are not coated and only the large particles are coated with cobalt alone, and Comparative Example 4, in which both the small particles and the large particles are coated with boron and cobalt, the initial charge / discharge efficiency can be reduced, but the drawback of high initial resistance was confirmed.

[0095] Experimental example 2: Evaluation of output characteristics The room temperature output resistance of lithium secondary batteries including the positive electrodes of Examples 1 to 3 and Comparative Examples 1 to 4 and the silicon-based negative electrodes was measured.

[0096] Specifically, the negative electrode active material (composed of 3 wt% SiO and 97 wt% artificial graphite), binder (SBR-CMC) and conductive material (carbon black) were added to the solvent water in a weight ratio of 95:3.5:1.5 to prepare a negative electrode slurry (solid content: 60 wt%). The negative electrode slurry was applied to a copper (Cu) thin film as a negative electrode current collector with a thickness of 6 μm, dried and then roll pressed to prepare a negative electrode.

[0097] In each of the above Examples 1 to 3 and Comparative Examples 1 to 4, a polyethylene-based separator having a thickness of 15 μm was interposed between the positive electrode and the negative electrode to prepare an electrode assembly, which was then placed inside a battery case, and an electrolyte was then injected into the case to prepare a lithium secondary battery. At this time, the electrolyte was prepared by dissolving 1M LiPF6 in a mixed organic solvent in which ethylene carbonate (EC):ethyl methyl carbonate (EMC) was mixed in a volume ratio of 1:2, and the electrolyte was injected to prepare the lithium secondary battery.

[0098] Each of the lithium secondary batteries was charged at 0.5 C in CCCV mode at 25° C. until it reached 4.2 V, and then discharged at a constant current of 2.0 C for 30 seconds, and the output resistance was measured from the voltage drop over 30 seconds. The results are shown in Table 2 below.

[0099] [Table 2]

[0100] From the results in Table 2 above, it is apparent that the positive electrodes of Examples 1 to 3 have the effect of lowering the output resistance when combined with a negative electrode containing a Si-based negative electrode active material.

[0101] Experimental example 3: Evaluation of high temperature life characteristics The high-temperature life characteristics of lithium secondary batteries including the positive electrodes of Examples 1 to 3 and Comparative Examples 1 to 4 and silicon-based negative electrodes were measured.

[0102] Specifically, the negative electrode active material (composed of 3 wt% SiO and 97 wt% artificial graphite), binder (SBR-CMC) and conductive material (carbon black) were added to the solvent water in a weight ratio of 95:3.5:1.5 to prepare a negative electrode slurry (solid content: 60 wt%). The negative electrode slurry was applied to a copper (Cu) thin film as a negative electrode current collector with a thickness of 6 μm, dried and then roll pressed to prepare a negative electrode.

[0103] In each of the above Examples 1 to 3 and Comparative Examples 1 to 4, a polyethylene-based separator having a thickness of 15 μm was interposed between the positive electrode and the negative electrode to prepare an electrode assembly, which was then placed inside a battery case, and an electrolyte was then injected into the case to prepare a lithium secondary battery. At this time, the electrolyte was prepared by dissolving 1M LiPF6 in a mixed organic solvent in which ethylene carbonate (EC):ethyl methyl carbonate (EMC) was mixed in a volume ratio of 1:2, and the electrolyte was injected to prepare the lithium secondary battery.

[0104] Each of the lithium secondary batteries was charged at 0.5 C in CCCV mode at 45° C. to 4.2 V, and discharged at a constant current of 0.5 C to 3.0 V, and then subjected to 200 charge-discharge cycles to measure the capacity retention rate and the resistance increase rate. The results are shown in Table 3.

[0105] [Table 3]

[0106] From the results in Table 3 above, it can be confirmed that, in combination with a negative electrode containing a Si-based active material, the positive electrodes of Examples 1 to 3 are more effective in increasing the capacity retention rate of the battery and reducing the resistance increase rate in a high-temperature environment than the positive electrodes of Comparative Examples 1 to 4.

[0107] To sum up the above experimental results, the lithium secondary battery according to one embodiment of the present invention is excellent in output characteristics and high-temperature life.

Claims

1. (1) Average particle size (D 50 mixing the small particle lithium composite transition metal oxide having a particle size of less than 7 μm with a boron-containing raw material and heat-treating the mixture to produce a first positive electrode active material; (2) Average particle size (D 50 a cobalt-containing raw material and a boron-containing raw material, and heat-treating the mixture to produce a second positive electrode active material; (3) mixing the first positive electrode active material and the second positive electrode active material to produce a positive electrode material having a bimodal particle size distribution.

2. The boron-containing source is H 3 B.O. 3 and B 2 O 3 The method for producing a positive electrode material for a lithium secondary battery according to claim 1, wherein the positive electrode material is one or more selected from the following:

3. The cobalt-containing raw material is Co 3 O 4 and Co(OH) 2 The method for producing a positive electrode material for a lithium secondary battery according to claim 1 or 2, wherein the positive electrode material is one or more selected from the following:

4. 4. The method for producing a positive electrode material for a lithium secondary battery according to claim 1, wherein in the step (1), the boron-containing raw material is mixed in an amount of 0.05 parts by weight to 0.13 parts by weight per 1 part by weight of the small particle lithium composite transition metal oxide.

5. 5. The method for producing a positive electrode material for a lithium secondary battery according to claim 1, wherein in the step (2), the cobalt-containing raw material is mixed in an amount of 0.4 parts by weight to 1.1 parts by weight per 1 part by weight of the large particle lithium composite transition metal oxide.

6. 6. The method for producing a positive electrode material for a lithium secondary battery according to claim 1, wherein in the step (2), the boron-containing raw material is mixed in an amount of 0.05 parts by weight to 0.13 parts by weight per 1 part by weight of the large particle lithium composite transition metal oxide.

7. The method for producing a positive electrode material for a lithium secondary battery according to any one of claims 1 to 6, wherein the heat treatment in step (1) is carried out at 250 ° C. to 400 ° C.

8. The method for producing a positive electrode material for a lithium secondary battery according to any one of claims 1 to 7, wherein the heat treatment in step (2) is carried out at 250 ° C. to 400 ° C.

9. 9. The method for producing a positive electrode material for a lithium secondary battery according to claim 1, wherein in the step (3), the first positive electrode active material and the second positive electrode active material are mixed in a weight ratio of 10:90 to 40:

60.

10. The method for producing a positive electrode material for a lithium secondary battery according to any one of claims 1 to 9, wherein the small particle and the large particle lithium composite transition metal oxide are each independently represented by the following chemical formula 1: [Chemical formula 1] Li 1+x (N a Co b Mn c M d )O 2 In the above Chemical Formula 1, M is at least one selected from W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; x, a, b, c and d are within the ranges of 0≦x≦0.2, 0.70≦a<1, 0<b≦0.25, 0<c≦0.25 and 0≦d≦0.1, respectively.

11. A cathode material having a bimodal particle size distribution, The positive electrode material includes a first positive electrode active material and a second positive electrode active material, The first positive electrode active material has an average particle size (D 50 and a boron-containing coating layer formed on the small-particle lithium composite transition metal oxide, The second positive electrode active material has an average particle size (D 50 and a coating layer containing cobalt and boron formed on the large-particle lithium composite transition metal oxide.

12. The positive electrode material for lithium secondary batteries according to claim 11, wherein the first positive electrode active material and the second positive electrode active material are mixed in a weight ratio of 10:90 to 40:

60.

13. The small particle and the large particle lithium composite transition metal oxide each independently have a nickel (Ni) content of 70 mol % or more of the total transition metal content. The positive electrode material for lithium secondary batteries according to claim 11 or 12.

Citation Information

Patent Citations

  • Y / La-doped Co / B co-coated nickel-cobalt-manganese ternary positive electrode material and preparation method thereof

    CN108550802A

  • High-voltage lithium cobalt oxide positive electrode active material and preparation method and application thereof

    CN111900359A

  • Composite positive electrode active material, positive electrode containing the same, and secondary battery

    JP2018505508A

  • Positive electrode active material for lithium secondary battery, method of manufacturing the same, and lithium secondary battery including the same