Multilayer ceramic electronic component and manufacturing method thereof
The multilayer ceramic component design with thick cover parts mitigates peeling issues during firing, enhancing reliability and capacitance consistency by stabilizing the side margin portions.
Patent Information
- Application Number
- JP2024147555
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-10-31
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The side margin portions in multilayer ceramic capacitors tend to peel off during firing, leading to insulation defects due to moisture intrusion at the exposed internal electrodes, which affects the reliability and capacitance consistency.
A multilayer ceramic electronic component design where the cover parts have a thickness dimension that is at least 60% of the functional part's thickness, providing high rigidity to prevent mismatched shrinkage behaviors during firing, thereby securing the side margin portions.
Prevents peeling of the side margin portions, ensuring high reliability and consistent capacitance by minimizing insulation defects and variations in capacitance.
Smart Images

Figure 2024156044000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a multilayer ceramic electronic component to which a side margin portion is attached later, and a method for manufacturing the same. [Background technology]
[0002] There is a known technique for adding side margins during the manufacturing process of a multilayer ceramic capacitor (see, for example, Patent Document 1). This technique can suppress errors in the intersection area of the internal electrodes caused by misalignment in the patterning of the internal electrodes, thereby minimizing variations in the capacitance of the multilayer ceramic capacitor.
[0003] As an example, in the method of manufacturing a multilayer ceramic capacitor described in Patent Document 1, a laminate sheet in which ceramic sheets on which internal electrodes are printed are laminated is cut to produce a plurality of laminates whose cut surfaces expose the internal electrodes as side surfaces.Then, the ceramic sheet is punched out at the side surfaces of the laminates to form side margins on the side surfaces of the laminates. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2012-209539 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the technology of attaching the side margins to the side surfaces of the laminate, the side margins are likely to peel off from the side surfaces of the laminate when the laminate with the side margins is fired, which makes the multilayer ceramic capacitor susceptible to insulation failure due to moisture penetrating into the side surfaces of the laminate where the internal electrodes are exposed.
[0006] In view of the above circumstances, an object of the present invention is to provide a multilayer ceramic electronic component in which peeling at the side margins is unlikely to occur, and a method for manufacturing the same. [Means for solving the problem]
[0007] In order to achieve the above object, a multilayer ceramic electronic component according to one embodiment of the present invention includes a laminate and a side margin portion. The laminate has a functional part including a plurality of internal electrodes stacked in a first direction, and a pair of cover parts covering the functional part from both sides in the first direction, and when the dimension of the functional part in the first direction is t1 and the dimension of each of the pair of cover parts in the first direction is t2, the laminate satisfies the relationship (2×t2) / t1≧0.6. The side margin portion covers the laminate from a second direction perpendicular to the first direction.
[0008] In the laminate produced during firing in the manufacturing process of a multilayer ceramic electronic component, the shrinkage behavior of the functional section in which the internal electrodes are arranged differs from that of the cover section in which the internal electrodes are not arranged. Due to the mismatch in shrinkage behavior between the functional section and the cover section in the laminate produced during firing, the side margin section is likely to peel off from the side surface of the laminate. In this respect, in the above-mentioned configuration, the cover portion is formed thick and therefore has high rigidity. Therefore, in this configuration, the cover portion with high rigidity that sandwiches the functional portion prevents the functional portion from contracting in a manner different from that of the cover portion. As a result, in this configuration, the mismatch in contraction behavior between the functional portion and the cover portion in the laminated portion is mitigated. Therefore, in the multilayer ceramic electronic component having the above configuration, it is possible to prevent the side margins from peeling off from the side surfaces of the laminate, thereby suppressing the occurrence of insulation failures caused by moisture intrusion into the side surfaces of the laminate where the internal electrodes are exposed, thereby achieving high reliability.
[0009] In the multilayer ceramic electronic component, the thickness dimension in the first direction may be smaller than the smaller short-side dimension among the dimension in the second direction and the dimension in a third direction perpendicular to the first and second directions. The thickness dimension may be equal to or less than half of the short side dimension. The thickness dimension may be equal to or smaller than one-fourth of the short side dimension. In these low-profile multilayer ceramic electronic components, peeling is more likely to occur at the side margins, so the configuration of the present invention is particularly effective.
[0010] The positions of the ends of the internal electrodes in the second direction may be within a range of 0.5 μm in the second direction. This structure can reduce variations in performance due to misalignment of the internal electrodes. In particular, in the case of multilayer ceramic capacitors, errors in the crossing area of the internal electrodes are less likely to occur, so capacitance variations can be reduced.
[0011] A laminated ceramic electronic component according to one embodiment of the present invention has a functional section including a plurality of internal electrodes stacked in a first direction, and a pair of cover sections covering the functional section from both sides in the first direction, and after firing, an unsintered laminate is prepared which satisfies the relationship (2×t2) / t1≧0.6, where t1 is the dimension of the functional section in the first direction and t2 is the dimension of each of the pair of cover sections in the first direction. An unsintered side margin portion is formed to cover the unsintered laminate from the second direction, thereby producing an unsintered ceramic body. The green ceramic body is fired.
[0012] The green side margin portion may be formed by attaching a ceramic sheet to the green laminate. The green side margin portion may be formed by punching the ceramic sheet out of the green laminate. Effect of the Invention
[0013] As described above, according to the present invention, it is possible to provide a multilayer ceramic electronic component in which peeling is unlikely to occur at the side margins, and a method for manufacturing the same. [Brief description of the drawings]
[0014] [Figure 1] 1 is a perspective view of a multilayer ceramic capacitor according to an embodiment of the present invention; [Diagram 2] 2 is a cross-sectional view of the multilayer ceramic capacitor taken along line AA' in FIG. [Diagram 3] 2 is a cross-sectional view of the multilayer ceramic capacitor taken along line BB' in FIG. [Figure 4] 4 is a flowchart showing a method for manufacturing the multilayer ceramic capacitor. [Diagram 5] FIG. 2 is a plan view of a ceramic sheet prepared in a ceramic sheet preparing step of the manufacturing method. [Figure 6] FIG. 2 is a perspective view showing a lamination step of the manufacturing method. [Figure 7] FIG. 4 is a plan view showing a cutting step in the manufacturing method. [Figure 8] FIG. 2 is a perspective view of a laminate obtained in the cutting step. [Figure 9] FIG. 2 is a perspective view of an unfired ceramic body obtained in a side margin portion forming step of the above manufacturing method. [Figure 10] FIG. 4 is a partial cross-sectional view showing the side margin portion forming step. [Figure 11] 1A to 1C are cross-sectional views each showing a schematic diagram of a firing process for a ceramic body having a general configuration. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the drawings, an X-axis, a Y-axis, and a Z-axis are shown which are mutually orthogonal as appropriate. The Z-axis is an axis oriented in the vertical direction. The X-axis and the Y-axis are axes oriented in the horizontal direction and are orthogonal to the Z-axis. The X-axis, the Y-axis, and the Z-axis are common to all the drawings.
[0016] [Configuration of multilayer ceramic capacitor 10] 1 to 3 are views showing a multilayer ceramic capacitor 10 according to an embodiment of the present invention in a common position. Fig. 1 is a perspective view of the multilayer ceramic capacitor 10. Fig. 2 is a cross-sectional view of the multilayer ceramic capacitor 10 taken along line A-A' in Fig. 1. Fig. 3 is a cross-sectional view of the multilayer ceramic capacitor 10 taken along line B-B' in Fig. 1.
[0017] 1 and 2 show the longitudinal dimension L in the X-axis direction, the transverse dimension W in the Y-axis direction, and the thickness dimension T in the Z-axis direction of the multilayer ceramic capacitor 10. For the multilayer ceramic capacitor 10, the maximum dimension in the X-axis direction is the longitudinal dimension L, the maximum dimension in the Y-axis direction is the transverse dimension W, and the maximum dimension in the Z-axis direction is the thickness dimension T.
[0018] The multilayer ceramic capacitor 10 is configured as a low-profile type having a thin shape in the Z-axis direction. That is, in the multilayer ceramic capacitor 10, the longitudinal dimension L is greater than the lateral dimension W, and the thickness dimension T is smaller than the lateral dimension W. The low-profile multilayer ceramic capacitor 10 is particularly advantageous in applications where it is mounted on thin electronic components.
[0019] The multilayer ceramic capacitor 10 includes a ceramic body 11, a first external electrode 14, and a second external electrode 15. The ceramic body 11 is configured as a hexahedron having a pair of end faces facing each other in the X-axis direction, a pair of side faces facing each other in the Y-axis direction, and a pair of main faces facing each other in the Z-axis direction.
[0020] The external electrodes 14, 15 cover both end faces of the ceramic body 11 and face each other in the X-axis direction with the ceramic body 11 in between. The external electrodes 14, 15 extend from each end face of the ceramic body 11 to the main surface and side surfaces. As a result, the external electrodes 14, 15 have a U-shape in both a cross section parallel to the XZ plane and a cross section parallel to the XY plane.
[0021] The shape of the external electrodes 14, 15 is not limited to that shown in Fig. 1. For example, the external electrodes 14, 15 may extend from both end faces of the ceramic body 11 to only one of the main faces, and may have an L-shaped cross section parallel to the XZ plane. This allows the multilayer ceramic capacitor 10 to have a smaller thickness dimension T in the Z-axis direction.
[0022] The external electrodes 14, 15 are made of a good electrical conductor. Examples of the good electrical conductor that forms the external electrodes 14, 15 include metals or alloys containing, as a main component, copper (Cu), nickel (Ni), tin (Sn), palladium (Pd), platinum (Pt), silver (Ag), gold (Au), etc.
[0023] The ceramic body 11 is made of dielectric ceramics and has a laminate 16 and a side margin portion 17. The laminate 16 has a pair of side surfaces S facing each other in the Y-axis direction. The laminate 16 also has a pair of end faces that form part of the end faces of the ceramic body 11, and a pair of main surfaces that form part of the main surfaces of the ceramic body 11.
[0024] The laminate 16 has a configuration in which a plurality of sheet-like ceramic layers extending along the XY plane are laminated in the Z-axis direction. The laminate 16 has a capacitance forming portion 18 configured as a functional portion that forms capacitance, and a pair of cover portions 19 that cover the capacitance forming portion 18 from above and below in the Z-axis direction. The pair of cover portions 19 form a pair of main surfaces of the laminate 16.
[0025] The capacitance forming portion 18 is disposed between a plurality of ceramic layers, and has a plurality of sheet-like first and second internal electrodes 12, 13 extending along the XY plane. The internal electrodes 12, 13 are alternately disposed along the Z-axis direction. In other words, the mutually adjacent internal electrodes 12, 13 face each other in the Z-axis direction with the ceramic layer therebetween.
[0026] The first internal electrode 12 is extended to an end face covered by the first external electrode 14. On the other hand, the second internal electrode 13 is extended to an end face covered by the second external electrode 15. As a result, the first internal electrode 12 is connected only to the first external electrode 14, and the second internal electrode 13 is connected only to the second external electrode 15.
[0027] The internal electrodes 12, 13 are formed across the entire width of the capacitance forming portion 18 in the Y-axis direction, and are exposed on a pair of side surfaces S of the laminate 16. The side margin portions 17 cover the pair of side surfaces S of the laminate 16, respectively. This ensures insulation between the internal electrodes 12, 13 on both side surfaces S of the laminate 16.
[0028] With this configuration, in the multilayer ceramic capacitor 10, when a voltage is applied between the first external electrode 14 and the second external electrode 15, the voltage is applied to the multiple ceramic layers between the first internal electrode 12 and the second internal electrode 13. As a result, a charge corresponding to the voltage between the first external electrode 14 and the second external electrode 15 is stored in the multilayer ceramic capacitor 10.
[0029] In the ceramic body 11, a dielectric ceramic with a high dielectric constant is used to increase the capacitance of each ceramic layer between the internal electrodes 12 and 13. An example of a dielectric ceramic with a high dielectric constant is a material with a perovskite structure containing barium (Ba) and titanium (Ti), such as barium titanate (BaTiO3).
[0030] The ceramic layer may be composed of compositions such as strontium titanate (SrTiO3), calcium titanate (CaTiO3), magnesium titanate (MgTiO3), calcium zirconate (CaZrO3), calcium zirconate titanate (Ca(Zr,Ti)O3), barium zirconate (BaZrO3), and titanium oxide (TiO2).
[0031] The internal electrodes 12 and 13 are made of a good electrical conductor. Typical examples of good electrical conductors that form the internal electrodes 12 and 13 include nickel (Ni), as well as metals or alloys mainly composed of copper (Cu), palladium (Pd), platinum (Pt), silver (Ag), gold (Au), etc.
[0032] Although details will be described later, in the multilayer ceramic capacitor 10, a side margin portion 17 is added to the side surface S of the laminate 16 at an unfired stage. Therefore, in the multilayer ceramic capacitor 10, the positions of the ends in the Y-axis direction of the multiple internal electrodes 12, 13 in the ceramic body 11 are within a range of 0.5 μm in the Y-axis direction.
[0033] As a result, in the multilayer ceramic capacitor 10, errors in the intersection area of the internal electrodes 12, 13 in the capacitance forming portion 18 are less likely to occur, so that variations in capacitance can be suppressed. Also, in the multilayer ceramic capacitor 10, by thinning the side margin portion 17, it is possible to achieve a reduction in size and an increase in capacitance.
[0034] 2 and 3 show the thickness dimension t1 in the Z-axis direction of the capacitance forming portion 18 and the thickness dimension t2 in the Z-axis direction of each cover portion 19 for the laminate 16. In the multilayer ceramic capacitor 10, the capacitance forming portions 18 and the cover portions 19 of the laminate 16 are configured to satisfy the relationship (2×t2) / t1≧0.6.
[0035] That is, in the multilayer ceramic capacitor 10, the cover portions 19 are formed thick so that the total dimension 2×t2 of the pair of cover portions 19 in the Z-axis direction is 60% or more of the dimension t1 of the capacitance forming portion 18. Note that it is preferable that the thickness dimension t2 of the pair of cover portions 19 is substantially the same, but they may be different from each other.
[0036] In this manner, in the laminate 16 of the multilayer ceramic capacitor 10, the capacitance forming portion 18 is sandwiched between the cover portion 19, which has a large thickness dimension t2 and high rigidity. Therefore, in the laminate 16 during firing, the capacitance forming portion 18 is unlikely to exhibit a shrinkage behavior different from that of the cover portion 19, and the stress applied to the side margin portion 17 from the side surface S is suppressed.
[0037] Therefore, in the multilayer ceramic capacitor 10, the side margin portion 17 is less likely to peel off from the side surface S of the laminate 16 during firing. As a result, in the multilayer ceramic capacitor 10, it is possible to suppress the occurrence of insulation defects between the internal electrodes 12, 13 caused by moisture penetrating into the side surface S of the laminate 16 where the internal electrodes 12, 13 are exposed.
[0038] [Method of manufacturing multilayer ceramic capacitor 10] Fig. 4 is a flowchart showing a method for manufacturing the multilayer ceramic capacitor 10 according to this embodiment. Figs. 5 to 10 are views showing the manufacturing process of the multilayer ceramic capacitor 10. The method for manufacturing the multilayer ceramic capacitor 10 will be described below along Fig. 4 with appropriate reference to Figs. 5 to 10.
[0039] (Step S01: Prepare ceramic sheet) In step S01, a first ceramic sheet 101 and a second ceramic sheet 102 for forming the capacitance forming portion 18, and a third ceramic sheet 103 for forming the cover portion 19 are prepared. The ceramic sheets 101, 102, and 103 are configured as unfired dielectric green sheets whose main component is dielectric ceramics.
[0040] The ceramic sheets 101, 102, and 103 are formed into a sheet shape using, for example, a roll coater or a doctor blade. The thicknesses of the ceramic sheets 101 and 102 are adjusted according to the thickness of the ceramic layer in the capacitance forming portion 18 after firing. The thickness of the third ceramic sheet 103 can be adjusted as appropriate.
[0041] Fig. 5 is a plan view of the ceramic sheets 101, 102, and 103. At this stage, the ceramic sheets 101, 102, and 103 are configured as large sheets that have not been divided into individual pieces. Fig. 5 shows cutting lines Lx and Ly for dividing into individual multilayer ceramic capacitors 10. The cutting line Lx is parallel to the X-axis, and the cutting line Ly is parallel to the Y-axis.
[0042] 5, an unsintered first internal electrode 112 corresponding to the first internal electrode 12 is formed on the first ceramic sheet 101, and an unsintered second internal electrode 113 corresponding to the second internal electrode 13 is formed on the second ceramic sheet 102. No internal electrode is formed on the third ceramic sheet 103 corresponding to the cover portion 19.
[0043] The internal electrodes 112, 113 can be formed by applying any conductive paste to the ceramic sheets 101, 102. The method for applying the conductive paste can be selected from among known techniques. For example, the conductive paste can be applied by screen printing or gravure printing.
[0044] Gaps in the X-axis direction along the cutting lines Ly are formed in the internal electrodes 112, 113 for every other cutting line Ly. The gaps in the first internal electrode 112 and the gaps in the second internal electrode 113 are arranged alternately in the X-axis direction. In other words, the cutting lines Ly passing through the gaps in the first internal electrode 112 and the cutting lines Ly passing through the gaps in the second internal electrode 113 are arranged alternately.
[0045] (Step S02: Lamination) In step S02, the ceramic sheets 101, 102, and 103 prepared in step S01 are laminated as shown in Fig. 6 to produce a laminated sheet 104. In the laminated sheet 104, the first ceramic sheet 101 and the second ceramic sheet 102 corresponding to the capacitance forming portion 18 are laminated alternately in the Z-axis direction.
[0046] In the laminated sheet 104, a third ceramic sheet 103 corresponding to the cover portion 19 is laminated on the upper and lower surfaces in the Z-axis direction of the alternately laminated ceramic sheets 101 and 102. The number of laminated ceramic sheets 101, 102, and 103 can be determined depending on the configuration of the laminated ceramic capacitor 10.
[0047] In particular, the thickness dimension t1 of the capacitance forming portion 18 can be adjusted by the thickness of the ceramic sheets 101, 102 and the number of layers of the ceramic sheets 101, 102. Furthermore, the thickness dimension t2 of the pair of cover portions 19 can be adjusted by the thickness of the third ceramic sheet 103 and the number of layers of the third ceramic sheet 103.
[0048] The laminated sheet 104 is integrated by pressing the ceramic sheets 101, 102, and 103 together. For example, hydrostatic pressure or uniaxial pressure is preferably used for pressing the ceramic sheets 101, 102, and 103 together. This makes it possible to increase the density of the laminated sheet 104.
[0049] (Step S03: Disconnect) In step S03, the laminate sheet 104 obtained in step S02 is cut along cutting lines Lx and Ly to produce an unfired laminate 116. The laminate 116 corresponds to the fired laminate 16. For example, a press blade or a rotary blade can be used to cut the laminate sheet 104.
[0050] 7 is a plan view of the laminated sheet 104 after step S03. The laminated sheet 104 is cut along the cutting lines Lx and Ly while being held by an adhesive sheet F1 such as a foam release sheet. By cutting the laminated sheet 104 in this manner, a laminate 116 is obtained.
[0051] 8 is a perspective view of the unsintered laminate 116 obtained in step S03. An unsintered capacitance forming portion 118 and a cover portion 119 are formed in the laminate 116. In addition, in the laminate 116, the internal electrodes 112, 113 are exposed on the side surface S, which is the cut surface, and the ends of the internal electrodes 112, 113 in the Y-axis direction are aligned on the side surface S.
[0052] (Step S04: Forming side margins) In step S04, unsintered side margin portions 117 are provided on both side surfaces S of the laminate 116 obtained in step S03. This results in the unsintered ceramic body 111 shown in Fig. 9. The side margin portions 117 can be formed, for example, by attaching ceramic sheets 117s to the side surfaces S of the laminate 116.
[0053] For example, a punching method can be used to attach the ceramic sheet 117s to the side surface S of the laminate 116. That is, by punching the ceramic sheet 117s at the side surface S of the laminate 116, the ceramic sheet 117s can be cut along the contour of the side surface S and adhered to the side surface S at the same time.
[0054] 10 is a cross-sectional view showing the process of a punching method for forming side margin portions 117. In the method shown in FIG. 10, ceramic sheets 117s are punched out simultaneously from the side surfaces S of multiple laminates 116, making it possible to form side margin portions 117 on the side surfaces S of multiple laminates 116 all at once.
[0055] 10A, multiple laminates 116 with one side surface S facing upward are arranged on an adhesive sheet F2 that holds the other side surface S. Next, the lower surface of the adhesive sheet F2 is held by a flat holding member H, and a ceramic sheet 117s is placed on the upward-facing side surface S of the multiple laminates 116.
[0056] Furthermore, a flat elastic member D made of an elastic body is placed opposite to the upper side of the ceramic sheet 117s covering the multiple laminates 116. Then, as shown in Fig. 10B, the elastic member D is moved downward until it comes into contact with the ceramic sheet 117s, and the elastic member D further presses the ceramic sheet 117s downward.
[0057] At this time, the elastic member D bites into the spaces between the multiple laminates 116, thereby pressing downward the areas of the ceramic sheet 117s that are not held by the side surfaces S of the laminates 116. As a result, the ceramic sheet 117s is cut along the contours of the side surfaces S of the respective laminates 116 by a shear force applied in the vertical direction.
[0058] 10C, the elastic member D is moved upward to separate the elastic member D from the ceramic sheet 117s. At this time, the ceramic sheet 117s remaining on the side surface S of each laminate 116 becomes the side margin portion 117. The ceramic sheet 117s remaining in the spaces between the multiple laminates 116 is removed.
[0059] Then, the multiple laminates 116 held on the adhesive sheet F2 are transferred to another adhesive sheet, thereby inverting the orientation of the multiple laminates 116 upside down. This allows the side margin portions 117 to be formed collectively on the other side surface S of the multiple laminates 116 by the same method as above.
[0060] The method of attaching the ceramic sheet 117s to the side surface S of the laminate 116 does not have to be the punching method. For example, the side margin portion 117 can also be formed by attaching the ceramic sheet 117s cut to fit the outline of the side surface S of the laminate 116 to both side surfaces S of the laminate 116.
[0061] Moreover, the ceramic sheet 117s does not have to be used to form the side margin portion 117, and for example, a ceramic slurry may be used. That is, the side margin portion 117 can also be formed by immersing the side surface S of the laminate 116 in a ceramic slurry and attaching the ceramic slurry to the side surface S of the laminate 116.
[0062] (Step S05: Firing) In step S05, the ceramic body 111 obtained in step S04 and shown in Fig. 9 is fired to produce the ceramic body 11 of the multilayer ceramic capacitor 10 shown in Figs. 1 to 3. That is, in step S05, the laminate 116 becomes the laminate 16, and the side margin portion 117 becomes the side margin portion 17.
[0063] The firing temperature in step S05 can be determined based on the sintering temperature of the ceramic body 111. For example, when a barium titanate (BaTiO3)-based material is used, the firing temperature can be about 1000 to 1300° C. Furthermore, the firing can be performed, for example, in a reducing atmosphere or a low oxygen partial pressure atmosphere.
[0064] In the laminate 116, the capacitance forming portion 118 in which the internal electrodes 112, 113 are arranged has a higher sinterability than the cover portion 119 in which the internal electrodes 112, 113 are not arranged. Therefore, in the laminate 116 during firing, the capacitance forming portion 118 starts to shrink earlier than the cover portion 119 and tends to shrink more than the cover portion 119.
[0065] However, since the capacitance forming portion 118 is sandwiched between the highly rigid cover portion 119, the timing and amount of shrinkage are regulated by the cover portion 119. That is, in the laminate 116 during firing, the cover portion 119 prevents the capacitance forming portion 118 from shrinking in a manner different from that of the cover portion 119.
[0066] Therefore, in the laminate 116 during firing, the capacitance forming portion 118 and the cover portion 119 shrink in a similar manner, that is, a mismatch in shrinkage behavior is unlikely to occur between the capacitance forming portion 118 and the cover portion 119. This suppresses the stress applied to the side margin portion 117 from the side surface S of the laminate 116.
[0067] Therefore, during firing, the laminate 116 can be prevented from peeling off the side surface S of the laminate 116. As a result, in the multilayer ceramic capacitor 10, gaps are less likely to occur between the laminate 16 and the side margin 17 even after firing, and high moisture resistance is achieved.
[0068] 11 is a cross-sectional view showing a typical firing process of a ceramic body 111a. In a laminate 116a of the ceramic body 111a, a thickness dimension t1 of the capacitance forming portion 118a is large and a thickness dimension t2 of the cover portion 119a is small, which is advantageous for increasing capacity and reducing size.
[0069] That is, in the ceramic body 111a, the proportion of the cover portion 119a in the laminate 116a is smaller than the proportion of the cover portion 119 in the laminate 116 according to this embodiment. Therefore, the rigidity of the cover portion 119a of the ceramic body 111a is lower than the rigidity of the cover portion 119 of the ceramic body 111 according to this embodiment.
[0070] Therefore, in ceramic body 111a, the shrinkage behavior of capacitance forming portion 118a is not easily restricted by cover portion 119a. Therefore, in laminate 116a during firing, shrinkage of capacitance forming portion 118a begins earlier than that of cover portion 119a, and shrinks more than cover portion 119a.
[0071] 11, in the side margin portion 117a, both ends in the Z axis direction are restricted from the inside in the Y axis direction by the cover portion 119a, while only the center portion in the Z axis direction is pulled inward in the Y axis direction by the capacitance forming portion 118a. This makes it easier for the side margin portion 117a to peel off from the side surface S of the laminate 116a.
[0072] Similarly, in the laminate 116a during firing, the capacitance forming portion 118a shrinks more in the Z-axis direction than the side margin portion 117a, which makes it easier for the cover portion 119a to peel off from the capacitance forming portion 118a. In contrast, in the multilayer ceramic capacitor 10 according to this embodiment, peeling of the side margin portion 117a and the cover portion 119a is less likely to occur.
[0073] Peeling of the side margin portion 117 during firing is more likely to occur in a multilayer ceramic capacitor 10 having a smaller thickness dimension T, i.e., a smaller dimension in the Z-axis direction of the side surface S of the laminate 116. For this reason, the configuration of the present invention is more effective for a multilayer ceramic capacitor 10 having a smaller thickness dimension T.
[0074] That is, according to the present invention, it becomes possible to apply a technique for post-attaching the side margin portion 117 to a lower-height multilayer ceramic capacitor 10. Specifically, the present invention is more effective in a configuration in which the thickness dimension T is equal to or less than half the short side dimension W, and is more effective in a configuration in which the thickness dimension T is equal to or less than a quarter of the short side dimension W.
[0075] Furthermore, in the laminate 116 during firing, the amount of shrinkage of the capacitance forming portion 118 along the XY plane is kept small, thereby reducing the amount of change in the intersection area of the internal electrodes 112, 113. As a result, in the multilayer ceramic capacitor 10, errors in the intersection area of the internal electrodes 12, 13 are even less likely to occur, making it possible to more effectively suppress variations in capacitance.
[0076] (Step S06: Forming external electrodes) In step S06, external electrodes 14, 15 are formed on both ends in the X-axis direction of the ceramic body 11 obtained in step S05, thereby completing the multilayer ceramic capacitor 10 shown in Figures 1 to 3. The method for forming the external electrodes 14, 15 in step S06 can be arbitrarily selected from known methods.
[0077] [Examples and Comparative Examples] As examples and comparative examples of the multilayer ceramic capacitor 10, 1000 samples each were produced for configurations 1 to 12 with variously different dimensions L, W, T, t1, and t2. In each sample of configurations 1 to 12, the dimensions L, W, T, t1, and t2 were as shown in Table 1, and all dimensions except for the dimensions L, W, T, t1, and t2 were common.
[0078] A moisture resistance test was conducted on samples of each of the configurations 1 to 12. In the moisture resistance test, each sample was kept at a temperature of 45°C, a humidity of 95%, and a rated voltage of 10 V was applied for 1000 hours. Samples with an electrical resistance value of less than 10 MΩ after the moisture resistance test were determined to have a failure due to poor insulation.
[0079] Table 1 shows the number of samples that failed out of 1000 samples as the evaluation result of the moisture resistance test for each of configurations 1 to 12. Table 1 also shows the value of (2×t2) / t1 calculated from the thickness dimension t1 of the capacitance forming portion 18 and the thickness dimension t2 of the cover portion 19 for each of configurations 1 to 12.
[0080] [Table 1]
[0081] As shown in Table 1, in the structures 2, 3, 4, 6, 7, 8, 10, 11, and 12 according to the embodiments in which (2×t2) / t1 is 0.6 or more, no failures occurred in any samples. On the other hand, in the structures 1, 5, and 9 according to the comparative examples in which (2×t2) / t1 is less than 0.6, failures were confirmed in multiple samples.
[0082] [Other embodiments] Although the embodiment of the present invention has been described above, the present invention is not limited to the above-mentioned embodiment, and various modifications can be made thereto.
[0083] For example, in the multilayer ceramic capacitor 10, the external electrodes 14, 15 may be provided at both ends in the short dimension W direction instead of at both ends in the long dimension L direction. In this case, in the laminate 16, the internal electrodes 12, 13 are drawn out to the side surfaces covered by the external electrodes 14, 15, and side margin portions 17 are provided on the end faces where the internal electrodes 12, 13 are exposed.
[0084] Furthermore, the multilayer ceramic capacitor 10 to which the present invention can be applied is not limited to a low-profile configuration in which the thickness dimension T is smaller than the short side dimension W. Even in a multilayer ceramic capacitor 10 in which the thickness dimension T is equal to or larger than the short side dimension W, the effect of the present invention in which peeling of the side margin portion 17 is less likely to occur can be obtained.
[0085] Furthermore, the present invention is applicable not only to multilayer ceramic capacitors but also to all multilayer ceramic electronic components having functional parts in which a plurality of internal electrodes are laminated. Examples of multilayer ceramic electronic components to which the present invention can be applied include, in addition to multilayer ceramic capacitors, chip varistors, chip thermistors, and multilayer inductors. [Explanation of symbols]
[0086] 10...Multilayer ceramic capacitor 11…Ceramic body 12,13…Internal electrode 14,15...External electrode 16...Laminate 17…Side margin 18...Capacity forming part 19…Cover part
Claims
[Claim 1] a laminate including a functional section including a plurality of internal electrodes stacked in a first direction, and a pair of cover sections covering the functional section from both sides in the first direction, the laminate satisfying a relationship of (2×t2) / t1≧0.6, where t1 is a dimension of the functional section in the first direction, and t2 is a dimension of each of the pair of cover sections in the first direction; a side margin portion covering the laminate from a second direction perpendicular to the first direction; A multilayer ceramic electronic component comprising:
Citation Information
Patent Citations
Manufacturing method of laminated ceramic electronic component
JP2012209539A
Multilayer ceramic electronic component and method of manufacturing the same
JP2013157593A
Multilayer ceramic capacitor and manufacturing method thereof
JP2017112163A
Method for manufacturing multilayer ceramic electronic component
JP2019016688A
Multilayer ceramic capacitor
JP2019024077A