Manufacturing method of cold forging article
The method improves cold forging by using wet blasting to roughen the surface and apply a lubricant with an extreme pressure additive, addressing lubricant peeling and environmental concerns, enhancing manufacturing efficiency and reducing environmental impact.
Patent Information
- Application Number
- JP2023070934
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-24
- Publication Date
- 2024-11-06
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure 2024156457000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a cold forged product. [Background technology]
[0002] Cold forging, which is used as a manufacturing method for various parts, has many advantages, such as the ability to mass-produce parts of the same shape, strength, short processing time, and material savings. Cold forging is a processing method in which a part or the whole of a forged material is compressed or struck using a tool such as a die without heating it. In such cold forging, a lubricating film is formed on the surface of the forged material to facilitate release from the tool and to prevent damage to the tool and the forged material itself due to heat and contact pressure generated during processing.
[0003] However, if the adhesion of the lubricating film to the surface of the workpiece to be forged is insufficient, the lubricating film is likely to peel off from the workpiece to be forged. The peeling of the lubricating film can cause the tool to seize on the workpiece to be forged during processing, leading to a decrease in yield and other factors that affect the manufacturability of cold forged products.
[0004] Under such circumstances, various attempts have been made to improve the adhesion between the forged member and the lubricating film, and for example, Patent Document 1 proposes a cold forging forming method in which a lubricating conversion coating treatment is applied to the surface of the forming material by a Bonder process or the like, and then a solid lubricating coating treatment is applied to the conversion coating by molybdenum disulfide or the like. However, the conversion coating treatment has a high environmental impact in terms of waste and energy consumption, etc., and a method for manufacturing cold forged products that has good manufacturability while reducing the environmental impact is desired. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 9-220633 Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention has been made in consideration of the above problems, and has as its main object to provide a method for manufacturing a cold forged product that has good manufacturability while reducing the environmental load. [Means for solving the problem]
[0007] A manufacturing method for a cold forged product according to an embodiment of the present disclosure includes a surface treatment step of performing a surface treatment of a forged member, an attachment step of attaching a lubricant to the surface of the forged member after the surface treatment step, and a forging step of cold forging the forged member using a tool after the attachment step, wherein the surface treatment step is a surface treatment by wet blasting, a forged member containing an iron (Fe) component is used as the forged member, and a lubricant containing a lubricating component and an extreme pressure additive is used as the lubricant.
[0008] The above summary of the invention does not list all of the necessary features of the present invention, and any subcombination of these features may also constitute an invention. Effect of the Invention
[0009] According to the present invention, it is possible to manufacture cold forged products with good manufacturability while reducing the environmental load. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 is a schematic diagram showing an example of a manufacturing method of a cold forged product according to the present invention. [Diagram 2] These are the results of XAFS measurements. [Diagram 3] These are the results of XAFS measurements. [Figure 4] These are the results of XAFS measurements. [Diagram 5] FIG. 1 is a schematic diagram of a ball threading test device. [Figure 6] This is the maximum load measurement result. [Figure 7] This is the measurement result of the remaining amount of phosphorus components. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Preferred embodiments for carrying out the present invention will be described below with reference to the drawings. Note that the following embodiments do not limit the inventions according to the claims, and all of the combinations of features described in the embodiments are not necessarily essential to the solution of the invention.
[0012] <<Manufacturing method for cold forged products>> The manufacturing method of the cold forged product according to the embodiment of the present invention (hereinafter, referred to as the manufacturing method of the embodiment) includes a surface treatment step, a bonding step, and a forging step. Each step will be described below by taking an example. Fig. 1 is a schematic diagram showing an example of the manufacturing method of the embodiment.
[0013] <Surface treatment process> The surface treatment step is a step of performing a surface treatment on the forged member 5. In a manufacturing method of one embodiment, in the surface treatment step, the surface of the forged member 5 is subjected to wet blasting.
[0014] (Forged parts) The forged member 5 used in the manufacturing method of one embodiment contains an iron (Fe) component. The forged member 5 may be made of only iron, a mixture of iron and other components, or an alloy of iron and other components. Examples of the forged member 5 include carbon steels such as S10C, S15C, S45C, S50C, and S60C, and chromium-molybdenum steels such as SCM435. As an example, the forged member 5 contains more than 50 mass% of iron.
[0015] There are no limitations on the shape and size of the forged member 5, and these may be appropriately determined depending on the tool 4 used in the forging process and the size of the cold forged product 1 to be produced. As an example, the shape of the forged member 5 is cylindrical (see FIG. 1(A)).
[0016] In one embodiment of the manufacturing method, the surface of the forged member 5 is roughened in the surface treatment step (see FIG. 1(B)). In other words, fine irregularities are formed on the surface of the forged member 5 in the surface treatment step. In one embodiment of the manufacturing method, the surface area of the forged member 5 is increased by roughening, thereby improving adhesion with the lubricating film 3, which will be described later. Furthermore, by not carrying out a chemical conversion treatment, the environmental impact can be reduced.
[0017] In one embodiment of the manufacturing method, the active surface of the forged member 5 containing iron components can be exposed in the surface treatment step. In one embodiment of the manufacturing method, the lubricant 3 described below is applied to the exposed active surface of the forged member 5, thereby improving the adhesion between the forged member 5 and the lubricating film 3.
[0018] (Wet blasting) In a manufacturing method according to one embodiment, the surface of the forged member 5 is roughened and the active surface of the forged member 5 is exposed by wet blasting.
[0019] The wet blasting process (which may also be called wet blasting treatment) referred to in this specification is a processing method in which a slurry 6 is accelerated by compressed air and collided with the workpiece to roughen the surface of the workpiece while grinding it. An example of the slurry is a mixture of a liquid and abrasive grains (which may also be called an abrasive). An example of the liquid is water. An example of the slurry contains more than 50 mass % of water with respect to the total mass of the slurry. An example of the abrasive grains is stainless steel abrasive grains. The slurry may contain various additives such as a degreaser and a rust inhibitor. There is no limitation to the wet blasting process, and a conventionally known processing method may be appropriately selected and used.
[0020] As blasting processes other than wet blasting, dry blasting such as shot blasting, air blasting, and sand blasting are known, but the adhesion between the forged member 5 and the lubricating film 3 when dry blasting is performed is lower than when wet blasting is performed. The reason why wet blasting can achieve extremely good adhesion between the forged member 5 and the lubricating film 3 is presumed to be as follows.
[0021] In the wet blasting process, a slurry containing a liquid is used, so that the active surface of the forged member 5 is exposed, and the exposed active surface can be immediately covered with the liquid contained in the slurry. In other words, the liquid contained in the slurry can be used as a protective film (which may be called a liquid film) for the active surface of the forged member 5. Although the active surface of the forged member 5 tends to oxidize in the air and its activity gradually decreases, by protecting the exposed active surface with a protective film (liquid contained in the slurry), unintended oxidation of the active surface of the forged member 5 can be suppressed, and the activity of the active surface of the forged member 5 can be well maintained. The wet blasting process, which can maintain the activity of the active surface of the forged member 5, can improve the adhesion between the forged member 5 and the lubricating film 3 in the adhesion process.
[0022] In one example of a manufacturing method, the surface of the forged member 5 is treated by wet blasting, and the liquid covering the surface of the forged member 5 (the liquid contained in the slurry) is not removed until the adhesion step is performed.
[0023] <Attachment process> The adhesion step is a step of adhering the lubricant 3 to the forged member 5 after the surface treatment step (see FIG. 1(C)). The adhesion step is a step of forming a lubricant film 3 on the surface of the forged member 5. The lubricant film 3 in this specification means the lubricant 3 that has been dried after being adhered. Examples of a method for drying the lubricant 3 include natural drying, cold air drying, hot air drying, and light heating such as infrared rays. The lubricant 3 may also be dried by raising the temperature of the forged member 5 before or after the adhesion of the lubricant 3. For example, after the surface treatment step, hot water at about 90° C. is used to wash away the abrasive grains contained in the slurry, thereby removing the abrasive grains and raising the temperature of the forged member 5. The forged member 5 may also be heated by electromagnetic induction heating or the like.
[0024] There is no limitation on the method of applying the lubricant 3, and various application methods can be appropriately selected and used. Examples of application methods include spray application and dip coating. There is no limitation on the amount of the lubricant 3 applied. As an example, the amount of the lubricant 3 applied is 2 g / m2 in terms of the applied weight after drying. 2 That's all.
[0025] (Lubricant) The lubricant 3 used in the manufacturing method of one embodiment includes a lubricating component and an extreme pressure additive. As the lubricating component, a lubricating component conventionally known in the field of lubricants 3 can be appropriately selected and used. Examples of the lubricating component include water-based lubricants and lubricating oils. Examples of the water-based lubricant include inorganic metal salts, polymeric compounds, waxes, and solid lubricants, or mixtures thereof. Examples of the lubricating oil include mineral oils and synthetic oils. The lubricating component contained in the lubricant 3 may be one type or two or more types.
[0026] (Extreme Pressure Additives) Examples of the extreme pressure additive contained in the lubricant 3 include phosphorus-based, chlorine-based, sulfur-based, and organic molybdenum-based additives. Other extreme pressure additives may also be used. Examples of phosphorus-based extreme pressure additives include phosphate esters and zinc dialkyldithiophosphates. Examples of chlorine-based extreme pressure additives include chlorinated paraffin and methyl trichlorostearate. Examples of sulfur-based extreme pressure additives include sulfurized fatty esters, alkyl polysulfides, and sulfurized olefins. Examples of the organic molybdenum-based extreme pressure additives include molybdenum dialkyldithiophosphates and molybdenum dialkyldithiocarbamates. The lubricant 3 may contain one type of extreme pressure additive or two or more types of extreme pressure additive. There is no limitation on the content of the extreme pressure additive, and compared to the use of a lubricant 3 that does not contain an extreme pressure additive, the adhesion between the forged member 5 and the lubricating film 3 and the lubricity of the lubricating film 3 can be improved.
[0027] In one embodiment of the manufacturing method, in the surface treatment step, the surface of the forged member 5 is roughened by wet blasting to expose the active surface of the forged member 5. In addition, in the manufacturing method of one embodiment, the exposed active surface of the forged member 5 is protected by the wet blasting liquid, and oxidation of the active surface can be suppressed. In addition, in the manufacturing method of one embodiment, the adhesion between the forged member 5 and the lubricating film 3 and the lubricity of the lubricating film 3 can be improved by the action of the extreme pressure additive contained in the lubricant 3 and the active surface of the forged member 5 that is exposed in the surface treatment step and whose activity is maintained.
[0028] Although the detailed mechanism is not clear at present, in the manufacturing method of one embodiment, (i) the active surface of the forged member 5 containing iron is exposed by a surface treatment process, (ii) the exposed active surface of the forged member 5 can be protected by the wet blast liquid, and the activity of the active surface can be maintained, and (iii) a compound containing iron and a constituent element of the extreme pressure additive is generated by the reaction between the active surface of the forged member 5 whose activity is maintained and the extreme pressure additive contained in the lubricant 3, and this generated compound acts on the adhesion suppression effect, or the generated compound increases the affinity between the surface of the forged member 5 and the lubricating film 3, and it is presumed that the above effect is expressed. In particular, the manufacturing method of one embodiment in which the wet blasting process that can maintain the activity of the active surface is performed can generate a large amount of compounds containing iron and a constituent element of the extreme pressure additive, compared to the case of performing a blasting process other than the wet blasting process.
[0029] Hereinafter, the case where a phosphorus-based extreme pressure additive is used will be mainly described. Hereinafter, the terms iron phosphide and iron phosphate may be read as a reaction product between iron and a constituent element of the extreme pressure additive.
[0030] Examples of compounds generated when using a lubricant 3 containing a phosphorus-based extreme pressure additive include iron phosphate and iron phosphide. Among these compounds, it is presumed that iron phosphate contributes greatly to improving the adhesion between the forged member 5 and the lubricating film 3, and to improving the lubricity of the lubricating film 3. In the manufacturing method of one embodiment, it is presumed that a so-called tribofilm is formed by the generated iron phosphate.
[0031] In addition, in the manufacturing method of one embodiment, iron phosphate can be generated at a stage before the forging process, in other words, at the stage where the lubricating film 3 is formed in the adhesion process, and good adhesion and good lubricity between the forged member 5 and the lubricating film 3 can be achieved from the early stage of the forging process. In other words, iron phosphate can be generated even without conditions such as high surface pressure and high temperature. Note that if surface treatment by blasting is not performed, the active surface of the forged member 5 cannot be exposed, and a sufficient amount of iron phosphate cannot be generated at the stage where the lubricating film 3 is formed in the adhesion process.
[0032] <Forging process> The forging process is a process in which the forged member 5 is cold forged using a tool 4 after the adhering process (see Figs. 1(D) and (E)). Through this process, a cold forged product 1 can be manufactured (see Fig. 1(F)). The manufacturing method of one embodiment can suppress seizure between the tool 4 and the forged member 5 during the manufacture of the cold forged product 1. In addition, due to the good lubricity of the lubricating film 3 formed on the surface of the forged member 5, damage to the tool 4 and the forged member 5 can be suppressed. In the embodiment shown in the figure, the lubricating film 3 is present on the surface of the manufactured cold forged product 1, but a process of removing the lubricating film 3 may be included.
[0033] (tool) The tool 4 used in the manufacturing method of the embodiment is not limited, and may be determined in consideration of the shape of the cold forged product 1 to be manufactured. As the tool 4, a tool that is conventionally known in the field of cold forging can be appropriately selected and used. One example of the tool 4 is a die. The tool 4 in the form shown in FIG. 1 is a pair of upper and lower dies.
[0034] A manufacturing method of a cold forged product according to another embodiment of the present invention (hereinafter, referred to as the manufacturing method according to another embodiment) includes a surface treatment step and a forging step.
[0035] In the manufacturing method of the other embodiment, the forging step is performed in a state where the lubricant 3 containing the lubricating component and the extreme pressure additive is positioned between the tool 4 and the forged member 5. The manufacturing method of the one embodiment is different in that the lubricant 3 containing the lubricating component and the extreme pressure additive is attached to the forged member 5 after the surface treatment step, whereas the manufacturing method of the other embodiment is different in that the forging step is performed in a state where the lubricant 3 containing the lubricating component and the extreme pressure additive is positioned between the tool 4 and the forged member after the surface treatment step. Other than this difference, the configuration described in the manufacturing method of the one embodiment can be appropriately selected and used.
[0036] In one example forging process, a lubricant 3 containing a lubricating component and an extreme pressure additive is applied to a tool 4 side. As an example, the forging process is performed while pouring (supplying) a lubricant 3 containing a lubricating component and an extreme pressure additive between a tool 4 and a forged part 5, or after pouring the lubricant 3.
[0037] In the manufacturing method of the other embodiment, the exposed active surface of the forged part 5 can be brought into contact with the lubricant 3 containing a lubricating component and an extreme pressure additive during the forging process, and the cold forged product 1 can be produced with good manufacturing suitability, as in the manufacturing method of the embodiment described above.
[0038] <<How to apply lubricant>> The method for applying lubricant 3 according to one embodiment of the present invention (hereinafter, referred to as the application method of one embodiment) includes a surface treatment step and an application step.
[0039] The adhesion method of the embodiment is common to the manufacturing method of the cold forged product of the embodiment described above, except for the forging step. EXAMPLES
[0040] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to these examples in any way.
[0041] (Preparation of Samples 1 and 2) A carbon steel (S10C) cut to a diameter of 10 mm and a height of 15 mm was prepared as the forged component. This forged component was surface-treated under the conditions shown in Table 1 below, and then the surface-treated forged component was immersed in a lubricant containing a lubricating component and an extreme pressure additive (phosphorus-based) to attach it to the forged component. After the lubricant was applied, it was dried and a lubricating film was formed on the forged component to produce samples 1 and 2. Sample 1 was a sample that had been subjected to wet blasting as the surface treatment, and sample 2 was a sample that had been subjected to degreasing as the surface treatment.
[0042] [Table 1]
[0043] (Preparation of samples 3 and 4) For Sample 3 (Sample 4), a lubricating film was formed in the same manner as for Sample 1 (Sample 2), and then the forged component on which the lubricating film was formed was compressed with a hydraulic press using a top and bottom flat die at an average speed of 10 mm / s until the thickness reached 4 mm (compression rate 74%). Sample 3 was obtained by compressing Sample 1. Sample 4 was obtained by compressing Sample 2.
[0044] (XAFS measurement (X-ray absorption fine structure analysis)) XAFS measurements were performed on samples 1 to 4. Each sample was ultrasonically cleaned in an alkaline solution before XAFS measurements. XAFS measurements were performed at the Aichi Synchrotron Light Center BL6N1 using partial fluorescence yield and conversion electron yield methods. The measurement area was approximately 3 mm x 1 mm. Figures 2 and 4 (A) show the XAFS measurement results for samples 1 and 2, and Figures 3 and 4 (B) show the XAFS measurement results for samples 3 and 4. The horizontal axis in Figures 2 to 4 shows the absorbed energy, and the vertical axis shows the normalized amount of absorbed X-rays. For convenience of explanation, the phase is shifted vertically in Figures 2 and 3. Figures 2 and 3 also show the XAFS measurement results for the lubricating film, iron phosphate (FePO4), and iron phosphide (Fe2P and Fe3P).
[0045] As shown in Figure 3, the spectra of samples 3 and 4 also show peaks different from the lubricating film and pre-edges that are not found in the lubricating film. This indicates that the peaks are not due to the lubricating film remaining on the surfaces of samples 3 and 4, but rather that compounds different from the lubricating film are present. Comparing with the standard samples of iron phosphide and iron phosphate, it can be seen that the compounds on the sample surfaces are a mixture of them. In samples 3 and 4, it is believed that compounds were formed by reactions due to the heat generated during compression deformation and the appearance of active surfaces due to the expansion of the surface area. At this time, a higher iron phosphate peak is expressed in sample 3, which was subjected to wet blasting as a surface treatment. From this, it can be inferred that the mixture ratio of the two compounds changes, and that the amount of iron phosphate that is effective for lubrication increases due to wet blasting.
[0046] As shown in Figure 2, a spectrum containing a mixture of iron phosphide and iron phosphate was observed in Samples 1 and 2, which were not compressed, but Sample 2 (degreased) had a significantly lower iron phosphate peak than the compressed Sample 4 (degreased). On the other hand, Sample 1 showed a spectrum similar to that of Sample 3, which was compressed, and it can be inferred that the lubricated surface exposed by the surface treatment can improve the adhesion between the forged component and the lubricating film, and form iron phosphate, which is effective for lubrication, even under conditions such as high surface pressure or high temperature.
[0047] In order to confirm the superiority of wet blasting over dry blasting, the following tests were conducted.
[0048] (Lubricity evaluation) The ball threading test apparatus shown in Figure 5 was prepared. The base material of the cylindrical specimen in Fig. 5 was S10C, and the inner wall surface was subjected to wet blasting or dry blasting, and then a lubricant was applied to the inner wall surface. The abrasive grains used in the wet blasting and dry blasting processes were stainless steel abrasive grains (polygonal shape, grain size 140 μm). The wet blasting process was performed at a projection pressure of 0.35 MPa. The slurry used in the wet blasting process was mixed with abrasive grains and water in a ratio (volume ratio) of 15:85. The dry blasting was also performed under the condition of a projection pressure of 0.35 MPa. The lubricant contains a phosphorus-based extreme pressure additive, and the lubricant adhesion weight is 7 g / m 2 (After drying). The inner diameter of the cylindrical test piece is φ14.5 mm. The balls used were SKH51 (hardened and tempered) and had a ball diameter of 17.46 mm. The wet blasting or dry blasting and the application of the lubricant were carried out on the base material of the cylindrical test piece in a state where it was divided into two halves, and after the application of the lubricant, the two halves were integrated to form the cylindrical test piece.
[0049] The ball was pushed into the cylindrical test piece with a punch, and the maximum load was measured with a load cell. The average speed at which the ball was pushed through was 370 mm s -1 It is. The maximum load is an index showing the lubricity of the lubricating film, and a smaller maximum load indicates better lubricity of the lubricating film. FIG. 6 is a graph of maximum load for cylindrical specimens subjected to wet blasting and dry blasting. As shown in Figure 6, the maximum load was smaller for the wet blasted sample than for the dry blasted sample, confirming the superior lubrication properties of the wet blasted sample.
[0050] (Adhesion evaluation) Figure 7 is a graph showing the results of energy dispersive X-ray analysis (EDX) of the distribution of remaining phosphorus (P) components on the ball-rubbed surface of a cylindrical test piece. The amount of detected phosphorus (P) is an index of the remaining amount of lubricating film, and a larger amount of detected phosphorus (P) indicates a larger amount of remaining lubricating film, and a larger amount of remaining lubricating film indicates better adhesion between the forged member and the lubricating film. The amount of P detected decreases with increasing distance from the tip of the test piece because the lubricant film is stretched and thinned during ball rubbing. As shown in Figure 7, the amount of phosphorus (P) detected was greater in the wet blasted sample than in the dry blasted sample, confirming the superiority of wet blasted adhesion between the forged component and the lubricant film. [Explanation of symbols]
[0051] 1. Cold forged products 3. Lubricant (lubricating film) 4...Tools 5...Forged member 6. Slurry
Claims
[Claim 1] A method for manufacturing a cold forged product, a surface treatment step for performing surface treatment on the forged component; a lubricant application step for applying a lubricant to the surface of the forged member after the surface treatment step; A forging step of cold forging the forged member using a tool after the adhering step, The surface treatment step is a surface treatment by wet blasting, A forged member containing an iron (Fe) component is used as the forged member, A lubricant containing a lubricating component and an extreme pressure additive is used as the lubricant. A manufacturing method for cold forged products.
Citation Information
Patent Citations
Cold-forge forming method and cold-forge forming apparatus of bevel gear
JP1997220633A
Cited By
Method for manufacturing cold forged products
JP2026144017A
Method for manufacturing cold forged products
JP7953683B2