Solid electrolyte, production method for solid electrolyte, and battery

A solid electrolyte with a lithium salt, carbonate solvent, and acrylic polymer binder addresses stability issues, enhancing ionic conductivity and stability against lithium metal for improved battery performance.

JP2024157069AInactive Publication Date: 2024-11-07LINTEC CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2021153978
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2021-09-22
Publication Date
2024-11-07
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing solid electrolytes using ionic liquid electrolytes and tetrafluoroethylene powder binders do not have sufficient stability against lithium metal under severe conditions, necessitating improvements in cycle discharge and charge performance.

Method used

A solid electrolyte comprising a lithium salt, carbonate solvent, metal oxide particles, and a binder containing an acrylic polymer is developed, with specific ratios and properties of components to enhance ionic conductivity and stability.

Benefits of technology

The electrolyte achieves high ionic conductivity and stability against lithium metal, facilitating film formation and preventing leakage, thereby improving battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157069000001
    Figure 2024157069000001
  • Figure 2024157069000002
    Figure 2024157069000002
Patent Text Reader

Abstract

To provide a solid electrolyte with high ion conductivity and high stability against lithium metal.SOLUTION: A solid electrolyte comprises an electrolytic solution containing a lithium salt and a carbonate solvent, metal oxide particles, and a binder containing an acrylic polymer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a solid electrolyte, a method for producing a solid electrolyte, and a battery. [Background technology]

[0002] Unlike liquid electrolytes, solid electrolytes are free from the risk of leakage and can form lightweight and flexible electrolyte membranes. Therefore, solid electrolytes are expected to be applied to secondary batteries using lithium ions, etc. For example, Patent Document 1 proposes a quasi-solid electrolyte that includes a metal oxide and an ion conductive material, and in which a specific ion conductive material is supported by metal oxide particles. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2017-059432 A Summary of the Invention [Problem to be solved by the invention]

[0004] The pseudo-solid electrolyte described in Patent Document 1 uses a mixture of either glymes or N,N-diethyl-N-methyl-N-(2-methoxyethyl)ammonium bis(trifluoromethanesulfonyl)imide as an ion-conducting material, and a lithium salt containing lithium bis(fluorosulfonyl)imide. This ion-conducting material is an ionic liquid-based electrolyte. In addition, the pseudo-solid electrolyte described in Patent Document 1 uses tetrafluoroethylene powder as a binder. However, in a more severe usage environment, a solid electrolyte using an ionic liquid-based electrolyte and a binder of tetrafluoroethylene powder does not have sufficient properties such as stability against lithium metal. For this reason, further improvement of the properties of the solid electrolyte, such as more stable cycle charge / discharge performance, is required.

[0005] An object of the present invention is to provide a solid electrolyte having high ionic conductivity and stability against lithium metal, a method for producing this solid electrolyte, and a battery including this solid electrolyte. [Means for solving the problem]

[0006] According to one aspect of the present invention, there is provided a solid electrolyte comprising an electrolytic solution containing a lithium salt and a carbonate-based solvent, metal oxide particles, and a binder containing an acrylic polymer.

[0007] In the solid electrolyte according to one embodiment of the present invention, the acrylic polymer contains a constitutional unit derived from an acrylic polymerizable compound, and the acrylic polymerizable compound has a reaction rate constant k p is 700 L·mol -1 ·s -1 It is preferable that the composition contains a monofunctional (meth)acrylate compound having the above structure.

[0008] In the solid electrolyte according to one aspect of the present invention, it is preferable that the acrylic polymerizable compound further contains a polyfunctional (meth)acrylate compound other than the monofunctional (meth)acrylate compound.

[0009] In the solid electrolyte according to one embodiment of the present invention, the polyfunctional (meth)acrylate compound is preferably at least one selected from the group consisting of 1,9-bis(acryloyloxy)nonane, trimethylolpropane triacrylate, pentaerythritol tetraacrylate, and dipentaerythritol hexaacrylate.

[0010] In the solid electrolyte according to one embodiment of the present invention, the structural unit derived from the acrylic polymerizable compound includes at least one selected from the group consisting of a structural unit derived from the monofunctional (meth)acrylate compound and a structural unit derived from the polyfunctional (meth)acrylate compound, and when the total of the structural units derived from the monofunctional (meth)acrylate compound and the structural units derived from the polyfunctional (meth)acrylate compound is taken as 100 mol %, it is preferable that the content of the structural units derived from the monofunctional (meth)acrylate compound is 90 mol % or more and 100 mol % or less, and the content of the structural units derived from the polyfunctional (meth)acrylate compound is 0 mol % or more and 10 mol % or less.

[0011] In the solid electrolyte according to one aspect of the present invention, when the total content of the electrolytic solution, the metal oxide particles, and the binder is taken as 100 mass%, it is preferable that the content of the electrolytic solution is 77 mass% or more and 90 mass% or less, the content of the metal oxide particles is 4 mass% or more and 16 mass% or less, and the content of the binder is 3 mass% or more and 10 mass% or less.

[0012] In the solid electrolyte according to one aspect of the present invention, the lithium salt is preferably at least one selected from the group consisting of lithium bis(fluorosulfonyl)imide and lithium borofluoride.

[0013] In the solid electrolyte according to one aspect of the present invention, the carbonate-based solvent is preferably at least one selected from the group consisting of dimethyl carbonate and propylene carbonate.

[0014] In the solid electrolyte according to one aspect of the present invention, the molar ratio of the lithium salt to the carbonate-based solvent (lithium salt / carbonate-based solvent) contained in the electrolytic solution is preferably 1 / 4 or more and 1 / 1 or less.

[0015] In the solid electrolyte according to one aspect of the present invention, the metal oxide particles are preferably silica particles.

[0016] In the solid electrolyte according to one embodiment of the present invention, the specific surface area of ​​the metal oxide particles measured by a BET method is 160 m 2 / g or more 700m 2 It is preferable that the molecular weight is not more than 1 / g.

[0017] According to one aspect of the present invention, there is provided a battery comprising the solid electrolyte according to the above aspect of the present invention.

[0018] According to one aspect of the present invention, there is provided a method for producing a solid electrolyte, the method comprising the steps of: mixing an electrolytic solution, metal oxide particles, an acrylic polymerizable compound, and a photopolymerization initiator to prepare a mixture; molding the mixture to obtain a molded product; and irradiating the molded product with ultraviolet light to obtain a solid electrolyte containing an acrylic polymer in which the acrylic polymerizable compound is cured, wherein the electrolytic solution contains a lithium salt and a carbonate-based solvent, and the solid electrolyte contains the electrolytic solution, the metal oxide particles, and a binder containing the acrylic polymer. Effect of the Invention

[0019] According to one aspect of the present invention, there are provided a solid electrolyte having high ionic conductivity and stability against lithium metal, a method for producing the solid electrolyte, and a battery including the solid electrolyte. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The present invention will be described below by taking an embodiment as an example, but the present invention is not limited to the content of the embodiment.

[0021] [Solid electrolyte] The solid electrolyte according to this embodiment will be described.

[0022] The solid electrolyte according to the present embodiment contains an electrolyte solution containing a lithium salt and a carbonate-based solvent, metal oxide particles, and a binder containing an acrylic polymer. According to the solid electrolyte according to the present embodiment, a solid electrolyte having high ionic conductivity and high stability against lithium metal is obtained. The reason for this is presumed to be as follows.

[0023] In the solid electrolyte according to the present embodiment, the thixotropy of the electrolyte solution (hereinafter, sometimes referred to as thixotropy) is improved by containing the electrolyte solution and metal oxide particles. This allows the electrolyte solution containing the metal oxide particles to be formed into a film. This film formation makes it possible to suppress leakage of the electrolyte solution while suppressing damage to the ionic conductivity of the electrolyte solution. Furthermore, the solid electrolyte according to the present embodiment includes an acrylic polymer, which allows the electrolyte solution to be formed into a film and improves stability against lithium metal. From the above, it is presumed that the solid electrolyte according to the present embodiment has high ionic conductivity and high stability against lithium metal (among these properties, the stability against lithium metal is particularly high).

[0024] <Electrolyte> The electrolyte solution according to this embodiment is obtained by containing a lithium salt and a carbonate-based solvent.

[0025] (Lithium salts) Specific examples of the lithium salt according to this embodiment include lithium hexafluorophosphate (LiPF6), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium 2-trifluoromethyl-4,5-dicyanoimidazolate (LiTDI), lithium 4,5-dicyano-1,2,3-triazolate (LiDCTA), lithium bis(pentafluoroethylsulfonyl)imide (LiBETI), lithium borofluoride (LiBF4), lithium bis(oxalato)borate (LiBOB), lithium nitrate (LiNO3), lithium chloride (LiCl), lithium bromide (LiBr), and lithium fluoride (LiF).

[0026] Among these, the lithium salt is preferably at least one selected from lithium bis(fluorosulfonyl)imide and lithium fluoroborate, in terms of obtaining a solid electrolyte with high ionic conductivity and stability against lithium metal. The lithium salt may be either lithium bis(fluorosulfonyl)imide (LiFSI) or lithium fluoroborate (LiBF4), or these two may be used together. In the solid electrolyte, the lithium salt may exist as a cation of lithium metal and a counter ion of the cation. By using these lithium salts, the stability against lithium metal is further improved.

[0027] (Carbonate solvent) Specific examples of the carbonate-based solvent according to the present embodiment include dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC). Among these, the carbonate-based solvent is preferably at least one selected from dimethyl carbonate and propylene carbonate, in terms of obtaining a solid electrolyte having high ion conductivity and high stability against lithium metal. The carbonate-based solvent may be one of dimethyl carbonate (DMC) and propylene carbonate (PC) alone, or these two may be used in combination. Here, the carbonate-based solvent in the present embodiment refers to a compound having a carbonate skeleton in its molecular structure.

[0028] (Molar ratio of lithium salt to carbonate solvent) In the electrolyte solution according to the present embodiment, the molar ratio of the lithium salt to the carbonate-based solvent (lithium salt / carbonate-based solvent) is preferably 1 / 4 or more and 1 / 1 or less. When this molar ratio is 1 / 4 or more, the stability to lithium metal is easily improved. On the other hand, when this molar ratio is 1 / 1 or less, the lithium salt is easily dissolved in the carbonate-based solvent. In terms of obtaining a solid electrolyte having high ionic conductivity and stability to lithium metal, this molar ratio may be 1 / 3 or more and 1 / 1 or less, or 1 / 2 or more and 1 / 1 or less.

[0029] Although the reason is unclear, the electrolyte according to the present embodiment is more stable to lithium metal when it is an electrolyte solution in which at least one lithium salt selected from lithium bis(fluorosulfonyl)imide and lithium borofluoride is combined with at least one carbonate-based solvent selected from dimethyl carbonate and propylene carbonate. In addition, when it is an electrolyte solution in which at least one lithium salt selected from lithium bis(fluorosulfonyl)imide and lithium borofluoride is combined with at least one carbonate-based solvent selected from dimethyl carbonate and propylene carbonate, the content of the lithium salt and the carbonate-based solvent is in the range of 1 / 4 to 1 / 1 in molar ratio, the stability to lithium metal is more excellent.

[0030] The content of the electrolytic solution in the solid electrolyte is preferably 75% by mass or more, more preferably 77% by mass or more, even more preferably 78% by mass or more, and even more preferably 79% by mass or more, based on the entire solid electrolyte, in order to obtain a solid electrolyte having high ionic conductivity and high stability against lithium metal. Also, in the same respect, the content of the electrolytic solution in the solid electrolyte is preferably 90% by mass or less, more preferably 89% by mass or less, and even more preferably 88% by mass or less, based on the entire solid electrolyte.

[0031] <Metal oxide particles> The solid electrolyte according to the present embodiment contains metal oxide particles. In the solid electrolyte according to the present embodiment, the electrolytic solution is supported on the metal oxide particles by containing the electrolytic solution and the metal oxide particles. Here, in the present embodiment, the supported state refers to a state in which the electrolytic solution is coated on at least a part of the surface of the metal oxide particles.

[0032] Metal oxide particles have a specific surface area of ​​160 m2 or more as measured by the BET method, which facilitates the formation of a solid electrolyte membrane. 2 / g or more 700m 2 The specific surface area (BET method) of the metal oxide particles is preferably 160 m 2 / g or more, the thixotropy is likely to be improved, and a film of an electrolyte solution containing metal oxide particles (i.e., a solid electrolyte) is likely to be formed. In addition, the specific surface area (BET method) is 700 m 2 When the specific surface area (BET method) of the metal oxide particles is less than 165 m / g, the metal oxide particles are easily mixed with the electrolytic solution, and a solid electrolyte membrane is easily formed. 2 / g or more is more preferable, and 170m 2 / g or more. 2 / g or less is more preferable, and 520m 2 / g or less is more preferable. Here, the BET method is a method in which gas molecules (usually nitrogen gas) are adsorbed on solid particles, and the specific surface area of ​​the solid particles is measured from the amount of adsorbed gas molecules. The specific surface area can be measured using various BET measuring devices.

[0033] The metal oxide particles may be used alone, or two or more types of metal oxide particles having different specific surface areas may be used in combination. The type of metal oxide particles is not particularly limited, and examples thereof include silica particles, alumina particles, zirconia particles, ceria particles, magnesium silicate particles, calcium silicate particles, zinc oxide particles, antimony oxide particles, indium oxide particles, tin oxide particles, titanium oxide particles, iron oxide particles, magnesium oxide particles, aluminum hydroxide particles, magnesium hydroxide particles, potassium titanate particles, and barium titanate particles. The metal oxide particles may be used alone, or two or more types may be used in combination. Among these, the metal oxide particles are preferably at least one selected from silica particles, alumina particles, zirconia particles, magnesium oxide particles, and barium titanate particles in terms of improving thixotropy. The metal oxide particles are more preferably silica particles in terms of being lightweight and having a small particle diameter.

[0034] When silica particles are used as metal oxide particles, the silica particles may be wet silica particles or dry silica particles. Examples of wet silica particles include wet silica particles obtained by a precipitation method and a sol-gel method, which are obtained by a neutralization reaction between sodium silicate and a mineral acid. Examples of dry silica particles include combustion method silica particles (fumed silica particles) obtained by burning a silane compound, and deflagration method silica particles obtained by explosively burning metal silicon powder. When the silica particles are dry silica particles, the inclusion of moisture derived from the silica particles can be suppressed, and therefore the deterioration of the electrolyte is easily suppressed. For this reason, from the viewpoint of suppressing the deterioration of the electrolyte, the silica particles are preferably dry silica particles, and more preferably fumed silica particles.

[0035] The content of the metal oxide particles in the solid electrolyte is preferably 4% by mass or more, more preferably 5% by mass or more, and even more preferably 6% by mass or more, based on the entire solid electrolyte, in order to facilitate the formation of a film of the solid electrolyte. Also, from the same viewpoint, the content of the metal oxide particles in the solid electrolyte is preferably 16% by mass or less, more preferably 15% by mass or less, and even more preferably 14% by mass or less, based on the entire solid electrolyte.

[0036] <Binding agent> The solid electrolyte according to the present embodiment contains a binder containing an acrylic polymer (hereinafter, may be simply referred to as a binder). In the solid electrolyte according to the present embodiment, by containing an acrylic polymer as a binder, it is possible to form a film and the stability against lithium metal is improved.

[0037] (Acrylic polymer) In the solid electrolyte according to the present embodiment, the acrylic polymer contains a structural unit derived from an acrylic polymerizable compound. That is, the acrylic polymer is a resin polymerized using an acrylic polymerizable compound as a monomer, and contains a structural unit derived from the acrylic polymerizable compound in the main chain. Here, "derived from" means that the necessary structure is changed when the monomer is polymerized.

[0038] [Acrylic polymerizable compound] The acrylic polymerizable compound includes a (meth)acrylate compound. The acrylic polymerizable compound may include only a monofunctional (meth)acrylate compound, or may include both a monofunctional (meth)acrylate compound and a polyfunctional (meth)acrylate compound.

[0039] In this specification, "(meth)acrylic" is a notation used to represent both "acrylic" and "methacrylic", and the same applies to other similar terms. In this specification, the polyfunctional (meth)acrylate compound means a di- or higher functional (meth)acrylate compound.

[0040] ·Monofunctional (meth)acrylate compounds The solid electrolyte according to the present embodiment is an acrylic polymerizable compound having a reaction rate constant k p is 700 L·mol -1 ·s -1 In a similar manner, the acrylic polymerizable compound preferably contains a monofunctional (meth)acrylate compound having a reaction rate constant k p is 710 L mol -1 ·s -1 More preferably, it is 720 L·mol -1 ·s -1 The reaction rate constant k of the monofunctional (meth)acrylate compound contained in the acrylic polymerizable compound is more preferably equal to or greater than 1. p The upper limit is not particularly limited, and is, for example, 40,000 L·mol -1 ·s -1 May be less than 35000 L·mol -1 ·s -1 In this specification, the reaction rate constant k p is 700 L·mol -1 ·s -1 The monofunctional (meth)acrylate compound having the above reaction rate constant k may be referred to as component (A). p is 700 L·mol -1 ·s -1 It is believed that the use of the above monofunctional (meth)acrylate compound improves the reactivity of the monofunctional (meth)acrylate compound and increases the molecular weight, which makes it easier for the solid electrolyte to form a film.

[0041] Reaction rate constant k p is 700 L·mol -1 ·s -1 The monofunctional (meth)acrylate compound having the above reaction rate constant k is not particularly limited, and may be, for example, (meth)acrylic acid or alkyl (meth)acrylate. p is 700 L·mol -1 ·s -1The monofunctional (meth)acrylate compound having the above structure is preferably an alkyl (meth)acrylate having an alkyl group having 1 to 3 carbon atoms. Specific examples include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, and isopropyl (meth)acrylate. Among these, the monofunctional (meth)acrylate compound having the above structure is preferably an alkyl (meth)acrylate having an alkyl group having 1 to 3 carbon atoms. p is 700 L·mol -1 ·s -1 More preferably, the monofunctional (meth)acrylate compound having a reaction rate constant k p is 700 L·mol -1 ·s -1 By using the above monofunctional (meth)acrylate compound, a solid electrolyte having high ionic conductivity and stability against lithium metal can be more easily obtained.

[0042] · Polyfunctional (meth)acrylate compounds In the solid electrolyte according to the present embodiment, it is preferable that the acrylic polymerizable compound further contains a polyfunctional (meth)acrylate compound other than the monofunctional (meth)acrylate compound in order to facilitate the formation of a film of the solid electrolyte. When the acrylic polymerizable compound further contains a polyfunctional (meth)acrylate compound other than the monofunctional (meth)acrylate compound, a solid electrolyte having high ion conductivity and high stability against lithium metal is more easily obtained. In this specification, the polyfunctional (meth)acrylate compound may be referred to as component (B).

[0043] Multifunctional (meth)acrylate compounds have a reaction rate constant k p is 700 L L mol -1 ·s -1 There is no particular limitation as long as it is a bifunctional or higher functional (meth)acrylate compound other than the above monofunctional (meth)acrylate compound. The polyfunctional (meth)acrylate compound is preferably a polyfunctional (meth)acrylate compound having no reactive group other than an acryloyl group, from the viewpoint of obtaining a solid electrolyte having high ionic conductivity and stability against lithium metal, and from the viewpoint of facilitating the formation of a film of the solid electrolyte.

[0044] Specific examples of the polyfunctional (meth)acrylate compound include 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol diacrylate (1,9-bis(acryloyloxy)nonane), neopentyl glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, neopentyl glycol adipate di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, dicyclopentanyl di(meth)acrylate, dimethylol dicyclopentane di(meth)acrylate, and tricyclodecane dimethanol (meth)acrylate. difunctional (meth)acrylate compounds such as trimethylolpropane tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, and pentaerythritol tri(meth)acrylate; tetrafunctional (meth)acrylate compounds such as diglycerol tetra(meth)acrylate and pentaerythritol tetra(meth)acrylate; pentafunctional (meth)acrylate compounds such as dipentaerythritol penta(meth)acrylate; and hexafunctional (meth)acrylate compounds such as dipentaerythritol hexa(meth)acrylate.

[0045] Among these, from the viewpoints of obtaining a solid electrolyte having high ionic conductivity and stability against lithium metal, and of facilitating the formation of a film of the solid electrolyte, the polyfunctional (meth)acrylate compound is preferably at least one selected from the group consisting of 1,9-bis(acryloyloxy)nonane, trimethylolpropane triacrylate, pentaerythritol tetraacrylate, and dipentaerythritol hexaacrylate.

[0046] In the solid electrolyte according to the present embodiment, the structural unit derived from the acrylic polymerizable compound contained in the acrylic polymer preferably includes at least one selected from the group consisting of a structural unit derived from a monofunctional (meth)acrylate compound and a structural unit derived from a polyfunctional (meth)acrylate compound. The structural unit derived from the acrylic polymerizable compound more preferably includes a structural unit derived from a monofunctional (meth)acrylate compound. The structural unit derived from the acrylic polymerizable compound further preferably includes a structural unit derived from a monofunctional (meth)acrylate compound and a structural unit derived from a polyfunctional (meth)acrylate compound. In terms of facilitating the formation of a film of the solid electrolyte, the content of the structural unit derived from the monofunctional (meth)acrylate compound and the structural unit derived from the polyfunctional (meth)acrylate compound is preferably within the range shown below. In addition, when the content of the structural unit derived from the monofunctional (meth)acrylate compound and the structural unit derived from the polyfunctional (meth)acrylate compound is within the range shown below, a solid electrolyte having high ion conductivity and stability against lithium metal is more easily obtained.

[0047] When the total of the constitutional units derived from the monofunctional (meth)acrylate compound and the constitutional units derived from the polyfunctional (meth)acrylate compound is 100 mol%, the content of the constitutional units derived from the monofunctional (meth)acrylate compound is preferably 90 mol% or more, more preferably 91 mol% or more, and even more preferably 93 mol% or more. The content of the constitutional units derived from the monofunctional (meth)acrylate compound is preferably 100 mol% or less, more preferably 99 mol% or less, and even more preferably 97 mol% or less.

[0048] When the total of the constitutional units derived from the monofunctional (meth)acrylate compound and the constitutional units derived from the polyfunctional (meth)acrylate compound is 100 mol%, the content of the constitutional units derived from the polyfunctional (meth)acrylate compound is preferably 0 mol% or more, more preferably 1 mol% or more, and even more preferably 3 mol% or more. The content of the constitutional units derived from the polyfunctional (meth)acrylate compound is preferably 10 mol% or less, more preferably 9 mol% or less, and even more preferably 7 mol% or less.

[0049] The content of the acrylic polymer in the solid electrolyte is preferably 3% by mass or more, more preferably 4% by mass or more, and even more preferably 5% by mass or more, based on the entire solid electrolyte, in order to facilitate the formation of a film of the solid electrolyte. In addition, from the same viewpoint, the content of the metal oxide particles in the solid electrolyte is preferably 10% by mass or less, more preferably 9% by mass or less, and even more preferably 8% by mass or less, based on the entire solid electrolyte.

[0050] [Photopolymerization initiator] In the solid electrolyte according to the present embodiment, a photopolymerization initiator is preferably used to obtain an acrylic polymer. In the solid electrolyte according to the present embodiment, the acrylic polymer is obtained by polymerizing a binder composition containing an acrylic polymerizable compound and a photopolymerization initiator.

[0051] The photopolymerization initiator is not particularly limited, and may be a known compound used for the purpose of curing an acrylic polymerizable compound. The photopolymerization initiator is preferably a photopolymerization initiator that is sensitive to ultraviolet light. The photopolymerization initiator may be used alone or in combination of two or more kinds.

[0052] Specific examples of the photopolymerization initiator include α-ketol compounds such as 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl)ketone, α-hydroxy-α,α'-dimethylacetophenone, 2-methyl-2-hydroxypropiophenone, and 1-hydroxycyclohexylphenyl ketone; acetophenone compounds such as methoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxyacetophenone, and 2-methyl-1-[4-(methylthio)-phenyl]-2-morpholinopropane-1; benzoin ether compounds such as benzoin ethyl ether, benzoin isopropyl ether, and anisoin methyl ether; ketal compounds such as benzyl dimethyl ketal; and 2-naphthalenesulfonyl chloride. aromatic sulfonyl chloride compounds; photoactive oxime compounds such as 1-phenone-1,1-propanedione-2-(o-ethoxycarbonyl)oxime; benzophenone compounds such as benzophenone, benzoylbenzoic acid, and 3,3'-dimethyl-4-methoxybenzophenone; thioxanthone compounds such as thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2,4-diethylthioxanthone, and 2,4-diisopropylthioxanthone; camphorquinone; halogenated ketones; acylphosphinoxides; acylphosphonates; oligo[2-hydroxy-2-methyl-1-(4-(1-methylvinyl)phenyl)propanone], and the like.

[0053] The content of the binder in the solid electrolyte is preferably 3% by mass or more, more preferably 4% by mass or more, and even more preferably 5% by mass or more, based on the entire solid electrolyte, in order to facilitate the formation of a film of the solid electrolyte. Also, from the same viewpoint, the content of the binder in the solid electrolyte is preferably 10% by mass or less, more preferably 9% by mass or less, and even more preferably 8% by mass or less, based on the entire solid electrolyte.

[0054] The solid electrolyte according to the present embodiment contains an electrolyte solution containing the lithium salt according to the present embodiment and a carbonate-based solvent, metal oxide particles, and a binder containing an acrylic polymer. The solid electrolyte according to the present embodiment may contain other components as long as the object of the present invention is not impaired.

[0055] <Mass ratio of metal oxide, electrolyte, and binder> In terms of facilitating the formation of a membrane of the solid electrolyte, the solid electrolyte according to this embodiment preferably has the following contents when the total content of the electrolytic solution, the metal oxide particles, and the binder is taken as 100 mass %. In addition, in the total content of the electrolytic solution, the metal oxide particles, and the binder, if the contents of the electrolytic solution, the metal oxide particles, and the binder are within the following ranges, a solid electrolyte having high ionic conductivity and stability against lithium metal is more easily obtained. It is preferable that the content of the electrolyte is 77% by mass or more and 90% by mass or less, the content of the metal oxide particles is 4% by mass or more and 16% by mass or less, and the content of the binder is 3% by mass or more and 10% by mass or less. It is more preferable that the content of the electrolyte is 78% by mass or more and 89% by mass or less, the content of the metal oxide particles is 5% by mass or more and 15% by mass or less, and the content of the binder is 4% by mass or more and 9% by mass or less. It is more preferable that the content of the electrolyte is 79% by mass or more and 88% by mass or less, the content of the metal oxide particles is 6% by mass or more and 14% by mass or less, and the content of the binder is 5% by mass or more and 8% by mass or less.

[0056] [Method of manufacturing solid electrolyte] Next, a method for producing the solid electrolyte according to this embodiment will be described.

[0057] The method for producing a solid electrolyte according to this embodiment includes the following steps. A step of preparing a mixture by mixing an electrolyte solution, metal oxide particles, an acrylic polymerizable compound, and a photopolymerization initiator (step 1) A step of forming the mixture to obtain a formed product (step 2) A step of irradiating the molded product with ultraviolet light to obtain a solid electrolyte containing an acrylic polymer in which the acrylic polymerizable compound is cured (step 3). The electrolytic solution contains a lithium salt and a carbonate-based solvent, and the solid electrolyte contains an electrolytic solution, metal oxide particles, and a binder containing an acrylic polymer.

[0058] According to the method for producing a solid electrolyte of this embodiment, a solid electrolyte having high ion conductivity and high stability against lithium metal can be obtained. According to the method for producing a solid electrolyte of this embodiment, the moldability for obtaining a solid electrolyte is improved by using an acrylic polymerizable compound and a photopolymerization initiator as a binder composition for obtaining an acrylic polymer. The reason for the improvement in moldability is considered as follows. According to the method for producing a solid electrolyte of this embodiment, a solid electrolyte can be easily obtained without applying a strong shear force when mixing raw materials for obtaining a solid electrolyte. On the other hand, in order to obtain a solid electrolyte using a fluororesin such as tetrafluoroethylene powder as a binder, it is necessary to apply a strong shear force when mixing the tetrafluoroethylene powder. Therefore, according to the method for producing a solid electrolyte of this embodiment, the moldability is improved.

[0059] (Process 1) Step 1 is a step of mixing raw materials for obtaining a solid electrolyte to obtain a mixture. In step 1, first, as raw materials for obtaining a solid electrolyte, an electrolyte solution containing the above-mentioned lithium salt and a carbonate-based solvent, the above-mentioned metal oxide particles, and the above-mentioned acrylic polymerizable compound and photopolymerization initiator are prepared. Next, these raw materials are weighed in the desired amount. Then, the weighed raw materials are mixed to prepare a mixture. The mixture may be prepared by stirring the raw materials with a known stirring device or the like. In the method for producing a solid electrolyte according to this embodiment, the mixture is prepared without applying a strong shear force.

[0060] In step 1, when the metal oxide particles, the electrolyte, and the acrylic polymerizable compound and photopolymerization initiator as the binder composition are mixed, for example, it is preferable to mix them in the following ratio: When the total content of the metal oxide particles, the electrolyte, and the binder composition is 100 mass%, the mixing ratio of the metal oxide particles, the electrolyte, and the binder composition is, for example, preferably, 4 mass% to 16 mass%, the electrolyte 77 mass% to 90 mass%, and the binder composition 3 mass% to 10 mass%, based on mass.

[0061] In the binder composition, when the total content of the acrylic polymerizable compound and the photopolymerization initiator is taken as 100 mol %, the content of the acrylic polymerizable compound is preferably, for example, 90 mol % or more and 99.9 mol % or less, and the content of the photopolymerization initiator is preferably 0.1 mol % or more and 10 mol % or less.

[0062] (Process 2) Step 2 is a step of obtaining a molded product from the mixture prepared in step 1. In step 2, the mixture prepared in step 1 is molded to obtain a molded product. The molding of the mixture is not particularly limited, and may be molded, for example, by applying the mixture to the surface of a support to form a coating film. The mixture may also be molded, for example, by compression molding in a mold exhibiting releasability. The mold exhibiting releasability may be, for example, a release film having a surface treated with a release agent.

[0063] (Step 3) Step 3 is a step of obtaining a solid electrolyte from the molded product obtained in step 2. In step 3, the molded product obtained in step 2 is irradiated with ultraviolet light, whereby the acrylic polymerizable compound is cured to form an acrylic polymer. Then, a solid electrolyte containing the above-mentioned electrolytic solution, the above-mentioned metal oxide particles, and the cured acrylic polymer is obtained. The device for irradiating the molded product with ultraviolet light is not particularly limited, and may be any device that cures the acrylic polymerizable compound. For example, the device for irradiating ultraviolet light may be a device equipped with an ultraviolet LED lamp, a device equipped with a high-pressure mercury lamp, or a device equipped with a metal halide lamp.

[0064] The conditions for irradiating the molded body with ultraviolet (UV) rays are not particularly limited, and may be any conditions under which the acrylic polymerizable compound can be cured. The maximum illuminance and integrated light quantity when irradiating the ultraviolet rays may be, for example, as follows. The maximum illuminance is, for example, 5 mW / cm 2 or more, 10 mW / cm 2 or more, 50 mW / cm 2 The maximum illuminance may be 1000 mW / cm or more. 2 may be less than 700 mW / cm 2 may be less than 500 mW / cm 2 The integrated light amount may be, for example, 50 mJ / cm 2 or more, 100 mJ / cm 2 or more, 500 mJ / cm 2 The integrated light amount may be 5000 mJ / cm or more. 2 may be less than 3000 mJ / cm 2 or less than 2000 mJ / cm 2 It may be the following.

[0065] By carrying out the above steps 1, 2, and 3, the solid electrolyte according to this embodiment is obtained.

[0066] [battery] Next, the battery according to this embodiment will be described.

[0067] The battery according to the present embodiment includes the solid electrolyte according to the present embodiment. In the present embodiment, it is preferable that the solid electrolyte according to the present embodiment is included as a constituent material of the electrolyte layer of the battery. The battery is composed of an anode, a cathode, and an electrolyte layer disposed between the anode and the cathode. By adopting such a configuration, a battery excellent in each characteristic can be obtained. In addition, the battery is preferably a secondary battery, and more preferably a lithium ion secondary battery. The various members included in the lithium ion secondary battery according to the present embodiment are not particularly limited, and for example, materials generally used in batteries can be used.

[0068] The present invention is not limited to the above-described embodiment, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. EXAMPLES

[0069] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The measurements and evaluations in the following examples and comparative examples were carried out by the methods shown below.

[0070] [Measurement of ionic conductivity of solid electrolytes] The solid electrolyte membrane was cut into a circle with a diameter of 6 mm, sandwiched between two stainless steel plates as electrodes, and the impedance between the stainless steel plates was measured. For the measurement, an AC impedance method was used in which an AC voltage (applied voltage of 10 mV) is applied between the electrodes to measure the resistance component, and the ionic conductivity was calculated from the real impedance intercept of the obtained Cole-Cole plot. A potentiostat / galvanostat (VMP-300, manufactured by Biologic) was used for the measurement. Ionic conductivity (σ A ) was calculated using the following formula (F1). σ A =L A / (R A ×S A ) · · · (F1) In formula (F1), σ A is the ionic conductivity (unit: S cm-1 ), R A is resistance (unit: Ω), S A is the cross-sectional area of ​​the solid electrolyte membrane at the time of measurement (unit: cm 2 ), L A indicates the distance between electrodes (unit: cm). The measurement temperature was 25°C. The ionic conductivity (σ A ) was calculated.

[0071] [Measurement of ionic conductivity of electrolyte] A circular mesh cloth with a diameter of 19 mm (α-UX SCREEN 150-035 / 380TW, manufactured by NBC Meshtec Co., Ltd.) was used as a separator. The separator was impregnated with an electrolyte prepared by mixing the lithium salt and carbonate-based solvent used in the examples or comparative examples in a prescribed manner, and sandwiched between two stainless steel plates with a diameter of 16 mm as electrodes, and the impedance between the stainless steel plates was measured. For the measurement, an AC impedance method was used in which an AC voltage (applied voltage of 10 mV) is applied between the electrodes to measure the resistance component, and the ionic conductivity was calculated from the real impedance intercept of the obtained Cole-Cole plot. For the measurement, a potentiostat / galvanostat (VMP-300 manufactured by Biologic Co., Ltd.) was used. Ionic conductivity (σ B ) was calculated using the following formula (F2). σ B =L B / (R B ×S B ) · · · (F2) In formula (F2), σ B is the ionic conductivity (unit: S cm -1 ), R B is resistance (unit: Ω), S B is the cross-sectional area of ​​the electrode (unit: cm 2 ), L B indicates the distance between electrodes (unit: cm). The measurement temperature was 25°C. The ionic conductivity (σ B ) was calculated.

[0072] [Stability evaluation for lithium metal (dissolution and precipitation test)] The solid electrolyte membrane was cut into a circle with a diameter of 19 mm, and sandwiched between two lithium metal electrodes to prepare a lithium symmetric cell. The lithium metal electrode had a diameter of 16 mm. The current density was 3 mA / cm at a temperature of 25°C. 2 The oxidation current was 3 mAh / cm 2 After that, the reduction current was increased to 3 mAh / cm 2 This series of operations was repeated 200 times, and the voltage change after 200 cycles was measured. This voltage measurement was used to investigate the dissolution and deposition behavior of lithium metal. It can be confirmed that the device is stable with respect to lithium metal when dissolution and deposition are repeated at a constant voltage without short circuits. The number of cycles in which the device operated at a potential within ±20mV of the voltage of the initial cycle was taken as the number of stable operation cycles, and the stability of each example with respect to lithium metal was compared.

[0073] [Example 1] Lithium bis(fluorosulfonyl)imide (LiFSI) was prepared as the lithium salt. Dimethyl carbonate (DMC) was prepared as the carbonate-based solvent. Fumed silica particles (AEROSIL® 380, Nippon Aerosil Co., Ltd., specific surface area by BET method: 350 m) were prepared as the metal oxide particles. 2 / g-410m 2 / g) was prepared. To obtain the acrylic polymer that constitutes the binder, methyl acrylate (component (A)) and 1,9-bis(acryloyloxy)nonane (component (B)) were prepared as acrylic polymerizable compounds, and 1-hydroxycyclohexyl phenyl ketone was prepared as a photopolymerization initiator. Here, methyl acrylate (component (A)) corresponds to a monofunctional (meth)acrylate compound, and the reaction rate constant k p is 720 L·mol -1 ·s -1 It was.

[0074] In Table 1, methyl acrylate is represented as "MA" and 1,9-bis(acryloyloxy)nonane is represented as "1,9-NDDA." In the following examples, the same components (A) and (B) are represented in Table 1 in the same manner.

[0075] Lithium bis(fluorosulfonyl)imide (LiFSI) and dimethyl carbonate (DMC) were weighed out to a molar ratio of 1 / 2 (=LiFSI / DMC) and thoroughly stirred to prepare an electrolyte. Methyl acrylate and 1,9-bis(acryloyloxy)nonane were weighed out to a molar ratio of 95 / 5 (=methyl acrylate / 1,9-bis(acryloyloxy)nonane) and then mixed to prepare an acrylic polymerizable compound mixture. Furthermore, the acrylic polymerizable compound mixture and 1-hydroxycyclohexylphenyl ketone as a photopolymerization initiator were mixed to a molar ratio of 97 / 3 (=acrylic polymerizable compound / photopolymerization initiator) to prepare a binder composition. Next, when the total of the fumed silica particles, the electrolyte, and the binder composition was taken as 100% by mass, the mixture was weighed out to be 15% by mass / 82% by mass / 3% by mass (=fumed silica particles / electrolyte solution / binder composition), and mixed thoroughly to obtain a mixture for forming a solid electrolyte membrane.

[0076] Thereafter, the mixture for forming the solid electrolyte membrane was compression molded on a release film (manufactured by Lintec Corporation, product name "PET38AL-5") to a thickness of 100 μm to obtain a molded product. This molded product was irradiated with ultraviolet (UV) rays [maximum illuminance: 180 mW / cm 2 , Accumulated light intensity: 1000mJ / cm 2and measuring with an illuminance actinometer manufactured by Eye Graphics (controller: EYE UV METER UVPF-A2, light receiver: EYE UV METER PD-365A2), and curing the binder composition to obtain a solid electrolyte membrane containing a binder containing an acrylic polymer. In the solid electrolyte membrane of Example 1, when the total content of the fumed silica particles, the electrolyte, and the binder containing an acrylic polymer is taken as 100 mass%, the respective contents of the fumed silica particles, the electrolyte, and the binder containing an acrylic polymer are as shown in Table 1.

[0077] [Example 2] A solid electrolyte membrane was produced in the same manner as in Example 1, except that the fumed silica particles, the electrolyte solution, and the binder composition were weighed out to be 4% by mass / 87% by mass / 9% by mass (=fumed silica particles / electrolyte solution / binder composition) when the total of the fumed silica particles, the electrolyte solution, and the binder composition was taken as 100% by mass, and mixed thoroughly.

[0078] [Example 3] A solid electrolyte membrane was produced in the same manner as in Example 1, except that the fumed silica particles, the electrolyte solution, and the binder composition were weighed out to be 5% by mass / 90% by mass / 5% by mass (=fumed silica particles / electrolyte solution / binder composition) when the total of the fumed silica particles, the electrolyte solution, and the binder composition was taken as 100% by mass, and mixed thoroughly.

[0079] [Example 4] A solid electrolyte membrane was produced in the same manner as in Example 1, except that the fumed silica particles, the electrolyte solution, and the binder composition were weighed out to be 6% by mass / 86% by mass / 8% by mass (=fumed silica particles / electrolyte solution / binder composition) when the total of the fumed silica particles, the electrolyte solution, and the binder composition was taken as 100% by mass, and mixed thoroughly.

[0080] [Example 5] A solid electrolyte membrane was produced in the same manner as in Example 1, except that the fumed silica particles, the electrolyte solution, and the binder composition were weighed out to be 9 mass % / 81 mass % / 10 mass % (=fumed silica particles / electrolyte solution / binder composition) when the total of the fumed silica particles, the electrolyte solution, and the binder composition was taken as 100 mass %, and mixed thoroughly.

[0081] [Example 6] A solid electrolyte membrane was produced in the same manner as in Example 1, except that the fumed silica particles, the electrolyte solution, and the binder composition were weighed out to be 11 mass % / 84 mass % / 5 mass % (=fumed silica particles / electrolyte solution / binder composition) when the total of the fumed silica particles, the electrolyte solution, and the binder composition was taken as 100 mass %, and mixed thoroughly.

[0082] [Example 7] A solid electrolyte membrane was produced in the same manner as in Example 1, except that the fumed silica particles, the electrolyte solution, and the binder composition were weighed out to be 13 mass % / 78 mass % / 9 mass % (=fumed silica particles / electrolyte solution / binder composition) when the total of the fumed silica particles, the electrolyte solution, and the binder composition was taken as 100 mass %, and mixed thoroughly.

[0083] In the solid electrolyte membranes of Examples 2 to 7, when the total content of the fumed silica particles, the electrolyte, and the binder containing an acrylic polymer is taken as 100 mass %, the respective contents of the fumed silica particles, the electrolyte, and the binder containing an acrylic polymer are as shown in Table 1.

[0084] [Example 8] As acrylic polymerizable compounds for obtaining the acrylic polymer constituting the binder, methyl acrylate (component (A)) and trimethylolpropane triacrylate (component (B)) were prepared, and as a photopolymerization initiator, 1-hydroxycyclohexyl phenyl ketone was prepared. In Table 1, trimethylolpropane triacrylate is abbreviated as "TMPTA."

[0085] A solid electrolyte membrane was produced in the same manner as in Example 1, except that methyl acrylate and trimethylolpropane triacrylate were weighed and mixed so as to have a molar ratio of 95 / 5 (=methyl acrylate / trimethylolpropane triacrylate).

[0086] [Example 9] As acrylic polymerizable compounds for obtaining the acrylic polymer constituting the binder, methyl acrylate (component (A)) and pentaerythritol tetraacrylate (component (B)) were prepared, and 1-hydroxycyclohexyl phenyl ketone was prepared as a photopolymerization initiator. In Table 1, pentaerythritol tetraacrylate is abbreviated as "PETA."

[0087] A solid electrolyte membrane was produced in the same manner as in Example 1, except that methyl acrylate and pentaerythritol tetraacrylate were weighed and mixed so as to have a molar ratio of 95 / 5 (=methyl acrylate / pentaerythritol tetraacrylate).

[0088] [Example 10] As acrylic polymerizable compounds to obtain the acrylic polymer that constitutes the binder, methyl acrylate (component (A)) and dipentaerythritol hexaacrylate (component (B)) were prepared, and 1-hydroxycyclohexyl phenyl ketone was prepared as a photopolymerization initiator. In Table 1, dipentaerythritol hexaacrylate is abbreviated as "DPHA."

[0089] A solid electrolyte membrane was produced in the same manner as in Example 1, except that methyl acrylate and dipentaerythritol hexaacrylate were weighed and mixed so as to have a molar ratio of 95 / 5 (=methyl acrylate / dipentaerythritol hexaacrylate).

[0090] [Example 11] Lithium borofluoride (LiBF4) was prepared as the lithium salt. A solid electrolyte membrane was produced in the same manner as in Example 1, except that lithium borofluoride (LiBF4) and dimethyl carbonate (DMC) were weighed out to have a molar ratio of 1 / 2 (=LiBF4 / DMC) and thoroughly stirred to prepare an electrolyte solution.

[0091] [Example 12] As a carbonate-based solvent, propylene carbonate (PC) was prepared. A solid electrolyte membrane was prepared in the same manner as in Example 1, except that lithium bis(fluorosulfonyl)imide (LiFSI) and propylene carbonate (PC) were weighed out as the lithium salts so as to have a molar ratio of 1 / 2 (=LiFSI / PC).

[0092] [Example 13] A solid electrolyte membrane was produced in the same manner as in Example 1, except that lithium bis(fluorosulfonyl)imide (LiFSI) and dimethyl carbonate (DMC) were weighed out to have a molar ratio of 1 / 3 (=LiFSI / DMC).

[0093] [Comparative Example 1] Lithium bis(fluorosulfonyl)imide (LiFSI) was prepared as the lithium salt. Tetraethylene glycol dimethyl ether (G4) was prepared as the solvent. Fumed silica particles (AEROSIL (registered trademark) 380, Nippon Aerosil Co., Ltd., specific surface area by BET method 350 m) were prepared as the metal oxide particles. 2 / g-410m 2 As a binder, polytetrafluoroethylene (PTFE) was prepared.

[0094] Lithium bis(fluorosulfonyl)imide (LiFSI) and tetraethylene glycol dimethyl ether (G4) were weighed out to a molar ratio of 1 / 1 (=LiFSI / G4) and thoroughly stirred to prepare an electrolyte solution. Next, the electrolyte solution and fumed silica particles were weighed out to a mass ratio of 80 / 20 (=electrolyte solution / fumed silica particles) and thoroughly mixed. Furthermore, 5 parts by mass of polytetrafluoroethylene (PTFE) were added to a total of 100 parts by mass of the electrolyte solution and the fumed silica particles, and thoroughly mixed using an agate mortar. Then, this mixture was compression molded on a fluororesin mold to obtain a solid electrolyte membrane. In the solid electrolyte membrane of Comparative Example 1, when the total content of the fumed silica particles, the electrolyte solution, and the binder was taken as 100% by mass, the respective contents of the fumed silica particles, the electrolyte solution, and the binder were as shown in Table 1.

[0095] [Comparative Example 2] Dimethyl carbonate (DMC) was prepared as a carbonate solvent. A solid electrolyte membrane was produced in the same manner as in Comparative Example 1, except that lithium bis(fluorosulfonyl)imide (LiFSI) and dimethyl carbonate (DMC) were weighed out to have a molar ratio of 1 / 2 (=LiFSI / DMC) and thoroughly stirred to prepare an electrolyte solution.

[0096] [Comparative Example 3] As the lithium salt, lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) was prepared. A solid electrolyte membrane was produced in the same manner as in Comparative Example 1, except that lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and dimethyl carbonate (DMC) were weighed out to have a molar ratio of 1 / 2 (=LiTFSI / DMC) and thoroughly stirred to prepare an electrolyte solution.

[0097] [Comparative Example 4] As a carbonate solvent, diethyl carbonate (DEC) was prepared. A solid electrolyte membrane was prepared in the same manner as in Comparative Example 1, except that lithium bis(fluorosulfonyl)imide (LiFSI) and diethyl carbonate (DEC) were weighed out to have a molar ratio of 1 / 2 (=LiFSI / DEC) and the electrolyte solution was prepared by thoroughly stirring.

[0098] [Evaluation of solid electrolytes] The above-mentioned dissolution / precipitation test and ionic conductivity measurement were performed on the solid electrolyte membranes obtained in Examples 1 to 13 and Comparative Examples 1 to 4. In addition, the above-mentioned ionic conductivity measurement was performed on the electrolyte solutions used in each Example and Comparative Example.

[0099] The composition of the solid electrolyte membrane of each example is shown in Table 1, and the results of the dissolution / precipitation test, ion conductivity measurement, and lithium ion transport number measurement are shown in Table 2. In Table 1, Li salt refers to lithium salt, and solvent refers to carbonate-based solvent.

[0100] [Table 1]

[0101] [Table 2]

[0102] As a result of the dissolution and deposition test, it can be seen that in each of the examples, the battery operated stably for 200 cycles or more. In contrast, the battery in the comparative example operated for less than 200 cycles. In the comparative example, the voltage increased with the progress of cycles, and the battery did not operate stably.

[0103] From the above, it was found that the solid electrolyte membranes obtained in the Examples had higher ionic conductivity and higher stability to lithium metal than the solid electrolyte membranes obtained in the Comparative Examples, confirming that the solid electrolyte of the present invention is excellent in these properties.

Claims

1. an electrolyte solution including a lithium salt and a carbonate-based solvent; Metal oxide particles; A binder including an acrylic polymer; Contains solid electrolyte.

2. The solid electrolyte according to claim 1, the acrylic polymer contains a structural unit derived from an acrylic polymerizable compound, The acrylic polymerizable compound has a reaction rate constant k p is 700 L / mol -1 ・s -1 The monofunctional (meth)acrylate compound is solid electrolyte.

3. The solid electrolyte according to claim 2, The acrylic polymerizable compound further includes a polyfunctional (meth)acrylate compound other than the monofunctional (meth)acrylate compound. solid electrolyte.

4. The solid electrolyte according to claim 3, The polyfunctional (meth)acrylate compound is at least one selected from the group consisting of 1,9-bis(acryloyloxy)nonane, trimethylolpropane triacrylate, pentaerythritol tetraacrylate, and dipentaerythritol hexaacrylate. solid electrolyte.

5. The solid electrolyte according to claim 3 or 4, the structural unit derived from the acrylic polymerizable compound includes at least one selected from the group consisting of a structural unit derived from the monofunctional (meth)acrylate compound and a structural unit derived from the polyfunctional (meth)acrylate compound, When the total of the structural units derived from the monofunctional (meth)acrylate compound and the structural units derived from the polyfunctional (meth)acrylate compound is 100 mol %, The content of the structural unit derived from the monofunctional (meth)acrylate compound is 90 mol % or more and 100 mol % or less, The content of the structural unit derived from the polyfunctional (meth)acrylate compound is 0 mol% or more and 10 mol% or less. solid electrolyte.

6. The solid electrolyte according to any one of claims 1 to 5, When the total content of the electrolytic solution, the metal oxide particles, and the binder is 100 mass%, The content of the electrolyte is 77% by mass or more and 90% by mass or less, The content of the metal oxide particles is 4% by mass or more and 16% by mass or less, The content of the binder is 3% by mass or more and 10% by mass or less. solid electrolyte.

7. The solid electrolyte according to any one of claims 1 to 6, The lithium salt is at least one selected from the group consisting of lithium bis(fluorosulfonyl)imide and lithium borofluoride. solid electrolyte.

8. The solid electrolyte according to any one of claims 1 to 7, The carbonate-based solvent is at least one selected from the group consisting of dimethyl carbonate and propylene carbonate. solid electrolyte.

9. The solid electrolyte according to any one of claims 1 to 8, The molar ratio of the lithium salt to the carbonate-based solvent contained in the electrolytic solution (lithium salt / carbonate-based solvent) is 1 / 4 or more and 1 / 1 or less. solid electrolyte.

10. The solid electrolyte according to any one of claims 1 to 9, The metal oxide particles are silica particles. solid electrolyte.

11. The solid electrolyte according to any one of claims 1 to 10, The specific surface area of ​​the metal oxide particles measured by the BET method is 160 m 2 / g or more 700m 2 / g or less, solid electrolyte.

12. The solid electrolyte according to any one of claims 1 to 11 is provided. battery.

13. A step of preparing a mixture by mixing an electrolytic solution, metal oxide particles, an acrylic polymerizable compound, and a photopolymerization initiator; shaping the mixture to obtain a shaped product; a step of irradiating the molded product with ultraviolet light to obtain a solid electrolyte containing an acrylic polymer in which the acrylic polymerizable compound is cured; Equipped with the electrolyte solution contains a lithium salt and a carbonate-based solvent; The solid electrolyte contains the electrolytic solution, the metal oxide particles, and a binder containing the acrylic polymer. A method for producing a solid electrolyte.

Citation Information

Patent Citations

  • Pseudo solid electrolyte, and all-solid lithium secondary battery arranged by use thereof