Method for producing optical laminate and optical laminate
By shearing the polarizing plate protective film with specific speed ratios between rotating blades, the method addresses adhesive layer sticking issues, enhancing the smoothness of cutting and reducing defects in optical laminates.
Patent Information
- Application Number
- JP2023071524
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-25
- Publication Date
- 2024-11-07
AI Technical Summary
Conventional methods for shearing films with resin and adhesive layers result in adhesive layer sticking to blades, leading to increased resistance and poor cutting, causing defects like chips and hangnails, which reduce the yield of optical laminates when bonded with polarizing plates.
The method involves shearing the polarizing plate protective film between rotating round blades with specific speed ratios (V1≧1.05V3 and V2≧1.05V3) to reduce rotational resistance and ensure smooth cutting, minimizing defects on the film surface and at the film-polarizing plate interface.
This approach reduces cutting defects in the polarizing plate protective film and improves the yield of optical laminates by ensuring smooth shearing and minimizing defects during the bonding process.
Smart Images

Figure 2024157266000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing an optical laminate and an optical laminate. [Background technology]
[0002] Conventionally, films have been sheared by a shear-cut method using upper and lower rotating circular blades, and the speed of the circular blades has been optimized to prevent poor cutting of the film.
[0003] For example, in JP 2005-28458 A (Patent Document 1), the speed of the lower circular blade that holds the film during shearing is set to be faster than the film transport speed, thereby preventing slack in the film during cutting, and the speed of the upper circular blade is set to be faster than the speed of the lower circular blade, thereby exerting an effect equivalent to that of a kitchen knife when cutting, thereby preventing poor cutting of the film. Specifically, the peripheral speed of the lower circular blade is set to about +1% of the film transport speed, and the peripheral speed of the upper circular blade is set to about +3% of the film transport speed. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2005-28458 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, it has been found that when a film including a resin layer and an adhesive layer is sheared by the conventional method, the adhesive layer of the film adheres to the upper and lower round blades, increasing the rotation resistance of the upper and lower round blades. In this case, it has been found that the film cannot be sheared smoothly, leading to poor cutting of the film and the risk of defects (such as chips and burrs) occurring on the cut surface of the film. Furthermore, it has been found that when this film is laminated to a polarizing plate to produce an optical laminate, defects (such as chips, glue chips, and cracks) occur at the interface between the film and the polarizing plate. Thus, there is a risk of a decrease in the yield of the optical laminate.
[0006] Therefore, an object of the present disclosure is to provide a manufacturing method for an optical laminate that can reduce cutting defects of a polarizing plate protective film and improve the yield of the optical laminate, and the optical laminate. [Means for solving the problem]
[0007] In order to solve the above problems, a method for producing an optical laminate according to one embodiment of the present disclosure includes: a first step of running a polarizing plate protective film including a resin layer and a pressure-sensitive adhesive layer laminated to each other between a first circular blade that is rotated and a second circular blade that is in contact with the first circular blade and rotates together with the first circular blade, thereby continuously shearing the widthwise end of the polarizing plate protective film with the second circular blade and the first circular blade; a second step of bonding the polarizing plate protective film with the edge portion sheared to a polarizing plate to form an optical laminate; Equipped with In the first step, the end of the polarizer protection film is sheared under a condition in which the relationship between the peripheral speed V1 of the first circular blade and the running speed V3 of the polarizer protection film satisfies V1≧1.05V3, and the relationship between the peripheral speed V2 of the second circular blade and the running speed V3 of the polarizer protection film satisfies V2≧1.05V3.
[0008] According to the above embodiment, the edge of the polarizing plate protective film is sheared in a state where V1≧1.05V3 and V2≧1.05V3 are satisfied, so that the speed difference between the peripheral speed V1 of the first circular blade and the running speed V3 of the polarizing plate protective film can be increased, and the speed difference between the peripheral speed of the second circular blade and the running speed of the polarizing plate protective film can be increased. This can reduce the rotational resistance applied to the first circular blade and the second circular blade due to the adhesive layer adhering to the first circular blade and the second circular blade when shearing the polarizing plate protective film. Therefore, the edge of the polarizing plate protective film can be smoothly sheared, reducing cutting defects of the polarizing plate protective film and reducing defects (such as cutting chips and burrs) that occur on the cut surface of the polarizing plate protective film.
[0009] Therefore, defects (such as chips, glue chips, and cracks) that occur at the interface between the polarizing plate protective film and the polarizing plate when the polarizing plate protective film and the polarizing plate are bonded together can be reduced, and the yield of the optical laminate can be improved.
[0010] Preferably, in one embodiment of the method for manufacturing an optical laminate, in the first step, the end of the polarizing plate protective film is sheared in a state in which the relationship between the peripheral speed V1 of the first circular blade and the running speed V3 of the polarizing plate protective film satisfies 1.2V3≧V1≧1.05V3.
[0011] According to the embodiment, the end of the polarizing plate protective film is sheared in a state where the relationship between the peripheral speed V1 of the first circular blade and the running speed V3 of the polarizing plate protective film satisfies V1≧1.05V3, thereby reducing cutting defects of the polarizing plate protective film and improving the yield of the optical laminate.
[0012] In addition, since the edge of the polarizing plate protective film is sheared in a state where the relationship between the peripheral speed V1 of the first circular blade and the running speed V3 of the polarizing plate protective film satisfies 1.2V3≧V1, the speed difference between the peripheral speed V1 of the first circular blade and the running speed V3 of the polarizing plate protective film can be prevented from becoming excessive, thereby reducing the occurrence of scratches on the polarizing plate protective film caused by the first circular blade sliding against the polarizing plate protective film.
[0013] Preferably, in one embodiment of the method for manufacturing an optical laminate, in the first step, the end of the polarizing plate protective film is sheared while the peripheral speed V1 of the first circular blade and the peripheral speed V2 of the second circular blade are the same.
[0014] Here, the term "same" does not necessarily mean "completely same" but includes "substantially same." For example, when the absolute value of the difference in peripheral speed is 0.1 m / min or less, the peripheral speed is considered to be the same.
[0015] According to the embodiment, it is easy to control the peripheral speed V1 of the first circular blade and the peripheral speed V2 of the second circular blade.
[0016] Preferably, in one embodiment of the method for producing an optical laminate, the pressure-sensitive adhesive layer has a thickness of 10 μm or more and 40 μm or less.
[0017] According to the embodiment, when the thickness of the adhesive layer is 10 μm or more, the adhesive layer adheres to the first and second round blades, and the rotation resistance of the first and second round blades may be increased when the polarizing plate protective film is sheared. However, since V1≧1.05V3 is satisfied as described above, the cutting failure of the polarizing plate protective film is reduced, and the yield of the optical laminate can be improved. In addition, since the thickness of the adhesive layer is 40 μm or less, for example, when the polarizing plate protective film is finally peeled off from the optical laminate, the polarizing plate protective film can be easily peeled off from the optical laminate.
[0018] In one embodiment of the method for producing an optical laminate, the relationship between the width W1 of the polarizing plate protective film after shearing and the width W0 of the polarizing plate protective film before shearing preferably satisfies W0>W1≧0.95W0.
[0019] According to the embodiment, the relationship between the width W1 of the polarizing plate protective film after shearing and the width W0 of the polarizing plate protective film before shearing satisfies W0>W1≧0.95W0, so that the edge to be sheared has a narrow width. As described above, since V1≧1.05V3 is satisfied, the edge of the polarizing plate protective film can be smoothly sheared.
[0020] Preferably, in one embodiment of the method for manufacturing an optical laminate, in the first step, the sheared end and the polarizing plate protective film after shear are each transported downstream, and the angle between the transport direction of the sheared end and the transport direction of the polarizing plate protective film after shear is 0.1° or more and 1.4° or less, more preferably 0.3° or more and 0.7° or less.
[0021] According to the embodiment, the angle with respect to the conveying direction is 0.1° or more, so that the sheared end portion can be prevented from interfering with the second circular blade or the first circular blade, thereby preventing vibration of the polarizing plate protective film caused by the end portion coming into contact with the second circular blade or the first circular blade.
[0022] In addition, since the angle with respect to the conveying direction is 1.4° or less, it is possible to suppress the generation of a force that would tear the edge portion from the polarizing plate protective film to the outside in the width direction, thereby preventing the cut surface of the polarizing plate protective film from becoming rough.
[0023] Preferably, in one embodiment of the method for producing an optical laminate, In the optical laminate, the pressure-sensitive adhesive layer is in contact with the polarizing plate, The width direction dimension of the pressure-sensitive adhesive layer and the width direction dimension of the resin layer are the same, The width dimension of the pressure-sensitive adhesive layer and the width dimension of the resin layer are smaller than the width dimension of the polarizing plate.
[0024] Here, "same" does not necessarily mean "completely same" but includes "substantially same." For example, if the absolute value of the difference in dimensions is 0.5 mm or less, the item is considered to be "same."
[0025] According to the embodiment, the width dimension of the adhesive layer and the width dimension of the resin layer are the same, so that the end of the resin layer contacts the adhesive layer. This can suppress moisture absorption deformation of the end of the resin layer and suppress peeling of the resin layer from the adhesive layer due to moisture absorption deformation. Therefore, defects of the polarizing plate protective film can be reduced, and the yield of the optical laminate can be improved.
[0026] Preferably, in one embodiment of the optical laminate, A polarizing plate; a polarizing plate protective film laminated on the polarizing plate; Equipped with The polarizing plate protective film includes a resin layer and a pressure-sensitive adhesive layer laminated together, the pressure-sensitive adhesive layer is in contact with the polarizing plate, The width direction dimension of the pressure-sensitive adhesive layer and the width direction dimension of the resin layer are the same, The width dimension of the pressure-sensitive adhesive layer and the width dimension of the resin layer are smaller than the width dimension of the polarizing plate.
[0027] Here, "same" does not necessarily mean "completely same" but includes "substantially same." For example, if the absolute value of the difference in dimensions is 0.5 mm or less, the item is considered to be "same."
[0028] According to the embodiment, the width dimension of the adhesive layer and the width dimension of the resin layer are the same, so that the end of the resin layer contacts the adhesive layer. This can suppress moisture absorption deformation of the end of the resin layer and suppress peeling of the resin layer from the adhesive layer due to moisture absorption deformation. Therefore, defects of the polarizing plate protective film can be reduced, and the yield of the optical laminate can be improved. Effect of the Invention
[0029] According to the method for producing an optical laminate and the optical laminate according to one aspect of the present disclosure, cutting defects of a polarizing plate protective film can be reduced, thereby improving the yield of the optical laminate. [Brief description of the drawings]
[0030] [Figure 1]FIG. 2 is a schematic diagram showing an embodiment of an apparatus for producing an optical laminate. [Diagram 2] FIG. 2 is a schematic diagram showing a manufacturing apparatus for a polarizing plate protective film. [Diagram 3] FIG. 2 is a schematic plan view showing an end processing device. [Figure 4] FIG. 2 is a cross-sectional view showing a sheet-shaped polarizing plate protective film. [Diagram 5] FIG. 4 is a cross-sectional view of FIG. 3 . [Figure 6] FIG. 13 is a schematic diagram showing a cutting portion adjustment mechanism. [Figure 7] FIG. 4 is an explanatory diagram showing the positional relationship between a cutting end portion and a second circular blade. [Figure 8] FIG. 2 is a schematic diagram showing an optical laminate. [Figure 9] 1 is a graph showing the relationship between the peripheral speed of a first circular blade and the defect ratio of a polarizing plate protective film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0031] Hereinafter, an apparatus and method for producing an optical laminate according to one aspect of the present disclosure will be described in detail with reference to the embodiments shown in the drawings. Note that the drawings include some schematic views and may not reflect actual dimensions or proportions.
[0032] <Embodiment> [Optical laminate manufacturing equipment] Fig. 1 is a schematic diagram showing an apparatus for manufacturing an optical laminate. Fig. 2 is a schematic diagram showing an apparatus for manufacturing a polarizing plate protective film. Fig. 3 is a schematic plan view showing an end processing apparatus. In this specification, "downward" refers to the downward direction in the vertical direction (gravity direction), and "upward" refers to the upward direction in the vertical direction (gravity direction).
[0033] 1, the optical laminate manufacturing apparatus 9 manufactures an optical laminate 17 including a polarizing plate protective film 15 and a polarizing plate 16. Specifically, the optical laminate manufacturing apparatus 9 includes a polarizing plate protective film manufacturing apparatus 1, a polarizing plate protective film feeding apparatus 5, a polarizing plate supplying apparatus 6, a bonding apparatus 7, and an optical laminate winding apparatus 8. The polarizing plate protective film manufacturing apparatus 1 includes a production apparatus 2, an edge processing apparatus 3, and a winding apparatus 4.
[0034] As shown in Figures 1, 2 and 3, a production device 2 produces a sheet-like polarizing plate protective film (hereinafter referred to as a sheet-like polarizing plate protective film 10) from a raw material. An edge processing device 3 cuts and recovers an edge 10a from the sheet-like polarizing plate protective film 10 produced by the production device 2. A winding device 4 winds up the polarizing plate protective film (hereinafter referred to as a polarizing plate protective film main body 12) whose edge has been recovered by the edge processing device 3 as a product. Here, the sheet-like polarizing plate protective film 10 is the polarizing plate protective film before the edge cutting process. The polarizing plate protective film main body 12 is the polarizing plate protective film after the edge cutting, and is hereafter treated as a product.
[0035] The end processing device 3 includes first, second and third transport sections 21, 22 and 23, a cutting section 31, a cutting section adjustment mechanism 60 and a recovery section 50. The first and second transport sections 21 and 22 transport the sheet-like polarizing plate protective film 10 along the transport direction A. The cutting section 31 cuts the end 10a of the sheet-like polarizing plate protective film 10 in the width direction B along the transport direction A of the sheet-like polarizing plate protective film 10. The width direction B is a direction perpendicular to the longitudinal direction (transport direction A) of the sheet-like polarizing plate protective film 10. The cutting section adjustment mechanism 60 adjusts the peripheral speed of the blade of the cutting section 31.
[0036] The third conveying section 23 is disposed downstream of the cutting section 31, and conveys downstream the cut end 11, which is the end 10a of the sheet-like polarizing plate protective film 10 cut by the cutting section 31. The cut end 11 is also called an edge material, and is unnecessary material cut to match the product width of the polarizing plate protective film. The collecting section 50 is disposed downstream of the third conveying section 23, and collects the cut end 11.
[0037] The polarizing plate protective film feeding device 5 feeds the polarizing plate protective film 15 taken up by the winding device 4. The polarizing plate supplying device 6 supplies a polarizing plate 16. The laminating device 7 laminates the polarizing plate protective film 15 and the polarizing plate 16 together to produce an optical laminate 17. The optical laminate winding device 8 winds up the optical laminate 17.
[0038] (Polarizing plate) A polarizing plate is a film that has the function of light absorption anisotropy, and generally includes a polarizing film in which a dichroic dye is uniaxially oriented. For example, to uniaxially align a dichroic dye, a polarizing film can be produced, which is a film that is uniaxially stretched in a state in which iodine or an organic dichroic dye is impregnated in a polymer such as a polyvinyl alcohol (PVA) resin. In other words, the polarizing function is expressed by anisotropic absorption of light by the dichroic dye encapsulated in the stretched polymer.
[0039] The polarizing plate includes a polarizing film and may have a protective film on one or both sides of the polarizing film.
[0040] (Polarizing film) A polarizing film, that is, a film obtained by uniaxially stretching a polymer such as a polyvinyl alcohol (PVA) resin film impregnated with iodine or an organic dichroic dye, can usually be produced through a process of uniaxially stretching a polyvinyl alcohol resin film, a process of dyeing the polyvinyl alcohol resin film with a dichroic dye such as iodine to adsorb the dichroic dye, a process of treating the polyvinyl alcohol resin film with the adsorbed dichroic dye with a crosslinking agent such as a boric acid-containing aqueous solution, and a process of washing with water after the treatment with the crosslinking agent such as a boric acid-containing aqueous solution. The polarizing film may contain a crosslinking agent.
[0041] The thickness of the polarizing film is usually 30 μm or less, preferably 18 μm or less, more preferably 15 μm or less, and further preferably 10 μm or less. The thickness is usually 1 μm or more, for example, 5 μm or more.
[0042] The uniaxial stretching of the polyvinyl alcohol-based resin film can be performed before, simultaneously with, or after dyeing with a dichroic dye. When the uniaxial stretching is performed after dyeing, the uniaxial stretching may be performed before or during the boric acid treatment. Of course, the uniaxial stretching can be performed in the multiple stages shown here. For the uniaxial stretching, a method of uniaxially stretching in the film transport direction between rolls having different peripheral speeds, a method of uniaxially stretching in the film transport direction using a heated roll, a method of stretching in the width direction using a tenter, etc. can be adopted. The uniaxial stretching may be performed by dry stretching in the air, or by wet stretching in a state in which the polyvinyl alcohol-based resin film is swollen using a solvent such as water. The stretching ratio is usually 3 to 8 times. In addition, an aqueous solution containing polyvinyl alcohol may be applied to the thermoplastic resin film, followed by drying treatment, and stretched together with the thermoplastic resin film by the above method.
[0043] The polyvinyl alcohol-based resin film can be dyed with a dichroic dye by, for example, immersing the polyvinyl alcohol-based resin film in an aqueous solution containing the dichroic dye. Specifically, iodine or a dichroic organic dye is used as the dichroic dye. The polarizing film obtained above can be further laminated with a protective film on one or both sides thereof to produce a polarizing plate.
[0044] (Protective film) The protective film has a function of protecting the surface of the polarizing film. The polarizing film and the protective film may be directly laminated to each other. Here, "directly laminated" includes an embodiment in which the protective film is laminated to the polarizing film by its self-adhesiveness, and an embodiment in which the protective film is laminated via a pressure-sensitive adhesive layer (adhesive layer or pressure-sensitive adhesive layer). The protective film may be subjected to a surface treatment (e.g., corona treatment, etc.) to improve adhesion to the polarizing film, and a thin layer such as a primer layer (also called an "easy adhesion layer") may be formed.
[0045] As the protective film, for example, a resin film excellent in transparency, mechanical strength, thermal stability, moisture barrier properties, isotropy, stretchability, etc. can be used. The resin film may be a thermoplastic resin film. Specific examples of resins constituting such a resin film include cellulose-based resins such as triacetyl cellulose; polyester-based resins such as polyethylene terephthalate and polyethylene naphthalate; polyethersulfone-based resins; polysulfone-based resins; polycarbonate-based resins; polyamide-based resins such as nylon and aromatic polyamide; polyimide-based resins; polyolefin-based resins such as polyethylene, polypropylene, and ethylene-propylene copolymers; cyclic polyolefin-based resins having cyclo- and norbornene structures (also called "norbornene-based resins"); (meth)acrylic resins such as polymethyl methacrylate; polyarylate-based resins; polystyrene-based resins; polyvinyl alcohol-based resins, and mixtures thereof. Polarizing element protective films made of such materials are easily available on the market. In addition, thermosetting resins or ultraviolet-curing resins such as (meth)acrylic, urethane, (meth)acrylic urethane, epoxy, and silicone resins can also be mentioned. In this specification, (meth)acrylic means either acrylic or methacrylic. The same applies to the expressions (meth)acrylate, (meth)acryloyl, etc.
[0046] The thickness of the protective film is preferably 0.1 μm or more and 60 μm or less, more preferably 0.5 μm or more and 40 μm or less, and further preferably 1 μm or more and 30 μm or less.
[0047] If necessary, the protective film may be subjected to surface treatment such as hard coat treatment, anti-reflection treatment, anti-sticking treatment, and anti-glare treatment.
[0048] A protective film can be produced by stretching the film containing the above thermoplastic resin.
[0049] (Polarizing plate protective film) The polarizing plate protective film is a protective film used in an optical laminate. The polarizing plate protective film and the polarizing plate are bonded together via an adhesive layer to form an optical laminate. Examples of the polarizing plate protective film include single-layer resin films such as cycloolefin resins, cellulose acetate resins, polyester resins such as polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate, polycarbonate resins, acrylic resins such as polymethyl methacrylate (PMMA), and olefin resins such as polypropylene. Furthermore, the single-layer resin film can have optical functions such as a function as a retardation resin film, a function as a brightness improvement resin film, a function as a reflection resin film, a function as a semi-transmission reflection resin film, a function as a diffusion resin film, and a function as an optical compensation resin film. The single-layer resin film may also be a laminated resin film in which optically functional resin films such as a retardation resin film, a brightness improvement resin film, a reflection resin film, a semi-transmission reflection resin film, a diffusion resin film, and an optical compensation resin film are laminated on the surface of the single-layer resin film. The thickness of the polarizing plate protective film used in the present invention is, for example, from 5 to 500 μm, and preferably from 10 to 300 μm.
[0050] Fig. 4 is a cross-sectional view of the sheet-shaped polarizing plate protective film 10. As shown in Fig. 4, the sheet-shaped polarizing plate protective film 10 includes a resin layer 101, an adhesive layer 102, and a peeling layer 103, which are laminated together. The resin layer 101 and the peeling layer 103 are made of, for example, the above-mentioned resin materials. The peeling layer 103 is peeled off from the adhesive layer 102 when the polarizing plate protective film and the polarizing plate are attached to each other. The resin layer 101 has a thickness of, for example, 10 µm or more and 300 µm or less. The peeling layer 103 has a thickness of, for example, 10 µm or more and 300 µm or less.
[0051] As the adhesive composition forming the adhesive layer 102, any conventionally known adhesive composition having excellent optical transparency can be used without any particular limitation, and for example, an adhesive composition having a base polymer such as an acrylic resin, a urethane resin, a silicone resin, or a polyvinyl ether resin can be used. In addition, an active energy ray curable adhesive composition, a heat curable adhesive composition, or the like may be used. Among these, an adhesive composition having an acrylic resin as a base polymer, which is excellent in transparency, adhesive strength, removability, weather resistance, heat resistance, and the like, is preferable. The pressure-sensitive adhesive composition may further contain a crosslinking agent, a silane compound, an antistatic agent, and the like.
[0052] [(Meth)acrylic resin] The (meth)acrylic resin contained in the pressure-sensitive adhesive composition is preferably a polymer (hereinafter also referred to as a "(meth)acrylic acid ester polymer") having as its main component (e.g., containing 50 parts by mass or more per 100 parts by mass of the structural unit of the (meth)acrylic resin) a structural unit derived from a (meth)acrylic acid alkyl ester represented by the following formula (I) (hereinafter also referred to as "structural unit (I)"): In this specification, the (meth)acrylic resin means either an acrylic resin or a methacrylic resin, and the "(meth)" in (meth)acrylate has the same meaning. Formula (I): TIFF2024157266000002.tif2368[where, R 10 represents a hydrogen atom or a methyl group, and R 20 represents an alkyl group having 1 to 20 carbon atoms, the alkyl group may have any of a linear, branched, or cyclic structure, and a hydrogen atom of the alkyl group may be replaced by an alkoxy group having 1 to 10 carbon atoms.]
[0053] Examples of the (meth)acrylic acid ester represented by formula (I) include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, i-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n- Examples of the alkyl acrylate containing an alkoxy group include 2-methoxyethyl (meth)acrylate and ethoxymethyl (meth)acrylate. Among them, it is preferable to include n-butyl (meth)acrylate or 2-ethylhexyl (meth)acrylate, n- and i-nonyl (meth)acrylate, n-decyl (meth)acrylate, i-decyl (meth)acrylate, n-dodecyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, stearyl (meth)acrylate, and t-butyl (meth)acrylate. Examples of the alkyl acrylate containing an alkoxy group include 2-methoxyethyl (meth)acrylate and ethoxymethyl (meth)acrylate. Among them, it is preferable to include n-butyl (meth)acrylate or 2-ethylhexyl (meth)acrylate, and it is particularly preferable to include n-butyl (meth)acrylate.
[0054] The (meth)acrylic acid ester polymer may contain a structural unit derived from a monomer other than the structural unit (I). The structural unit derived from the other monomer may be one type or two or more types. Examples of the other monomer that the (meth)acrylic acid ester polymer may contain include a monomer having a polar functional group, a monomer having an aromatic group, and an acrylamide monomer.
[0055] The monomer having a polar functional group may be a (meth)acrylate having a polar functional group, such as a hydroxy group, a carboxy group, an amino group substituted with an alkyl group having 1 to 6 carbon atoms or an unsubstituted amino group, or a heterocyclic group such as an epoxy group.
[0056] The content of the structural units derived from the monomer having a polar functional group in the (meth)acrylic acid ester polymer is preferably 10 parts by mass or less, more preferably 0.5 parts by mass or more and 10 parts by mass or less, even more preferably 0.5 parts by mass or more and 5 parts by mass or less, and particularly preferably 1 part by mass or more and 5 parts by mass or less, relative to 100 parts by mass of all structural units of the (meth)acrylic acid ester polymer.
[0057] Examples of monomers having an aromatic group include (meth)acrylic acid esters having one (meth)acryloyl group and one or more aromatic rings (e.g., benzene ring, naphthalene ring, etc.) in the molecule and having a phenyl group, a phenoxyethyl group, or a benzyl group. By including these structural units, it is possible to suppress the white spots on polarizing plates that occur in high temperature and high humidity environments.
[0058] The content of structural units derived from monomers having an aromatic group in the (meth)acrylic acid ester polymer is preferably 20 parts by mass or less, more preferably 4 parts by mass or more and 20 parts by mass or less, and even more preferably 4 parts by mass or more and 15 parts by mass or less, relative to 100 parts by mass of all structural units of the (meth)acrylic acid ester polymer.
[0059] Examples of the acrylamide monomer include N-(methoxymethyl)acrylamide, N-(ethoxymethyl)acrylamide, N-(propoxymethyl)acrylamide, N-(butoxymethyl)acrylamide, N-(2-methylpropoxymethyl)acrylamide, etc. By including these structural units, it is possible to suppress the bleeding out of additives such as antistatic agents, which will be described later.
[0060] Furthermore, structural units derived from monomers other than the structural unit (I) may include structural units derived from styrene-based monomers, structural units derived from vinyl-based monomers, structural units derived from monomers having multiple (meth)acryloyl groups in the molecule, and the like.
[0061] The weight average molecular weight (hereinafter, simply referred to as "Mw") of the (meth)acrylic resin (1) is preferably 500,000 to 2,500,000. When the weight average molecular weight is 500,000 or more, the durability of the first pressure-sensitive adhesive layer in a high-temperature and high-humidity environment can be improved. When the weight average molecular weight is 2,500,000 or less, the operability during application of a coating liquid containing the pressure-sensitive adhesive composition is improved. The molecular weight distribution (Mw / Mn), which is expressed as the ratio of the weight average molecular weight (Mw) to the number average molecular weight (hereinafter, simply referred to as "Mn"), is usually 2 to 10. In this specification, the "weight average molecular weight" and the "number average molecular weight" are polystyrene-equivalent values measured by gel permeation chromatography (GPC).
[0062] When the (meth)acrylic resin is dissolved in ethyl acetate to prepare a solution having a concentration of 20% by mass, the viscosity at 25° C. is preferably 20 Pa·s or less, and more preferably 0.1 to 15 Pa·s. When the viscosity of the (meth)acrylic resin at 25° C. is within the above range, it contributes to improved durability and reworkability of a polarizing plate including a pressure-sensitive adhesive layer formed from the resin. The viscosity can be measured by a Brookfield viscometer.
[0063] The glass transition temperature (Tg) of the (meth)acrylic resin is, for example, −60 to 20° C., preferably −50 to 15° C., more preferably −45 to 10° C., and further preferably −40 to 0° C. The glass transition temperature can be measured by a differential scanning calorimeter (DSC).
[0064] The (meth)acrylic resin may contain two or more kinds of (meth)acrylic acid ester polymers. Examples of such (meth)acrylic acid ester polymers include (meth)acrylic acid ester polymers having a relatively low molecular weight, such as those mainly composed of the structural unit (I) derived from the (meth)acrylic acid ester and having a weight average molecular weight in the range of 50,000 to 300,000.
[0065] The (meth)acrylic resin can be usually produced by a known polymerization method such as a solution polymerization method, a bulk polymerization method, a suspension polymerization method, or an emulsion polymerization method. In the production of the (meth)acrylic resin, the polymerization is usually carried out in the presence of a polymerization initiator. The amount of the polymerization initiator used is usually 0.001 to 5 parts by mass with respect to 100 parts by mass of the total of all the monomers constituting the (meth)acrylic resin. The (meth)acrylic resin can also be produced by a method of polymerization using active energy rays such as ultraviolet rays.
[0066] [Crosslinking agent] The pressure-sensitive adhesive composition preferably contains a crosslinking agent. Examples of the crosslinking agent include conventional crosslinking agents (e.g., isocyanate compounds, epoxy compounds, aziridine compounds, metal chelate compounds, peroxides, etc.), and from the viewpoints of the pot life of the pressure-sensitive adhesive composition, crosslinking speed, and durability of the polarizing plate, it is particularly preferable to use an isocyanate compound.
[0067] The isocyanate compound is a compound having at least two isocyanato groups (-NCO) in the molecule. Specific examples include tolylene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, diphenylmethane diisocyanate, hydrogenated diphenylmethane diisocyanate, naphthalene diisocyanate, and triphenylmethane triisocyanate. In addition, adducts obtained by reacting these isocyanate compounds with polyols such as glycerol and trimethylolpropane, and dimers and trimers of these isocyanate compounds are also included. Two or more types of isocyanate compounds may be combined.
[0068] The proportion of the crosslinking agent is, for example, 0.01 to 10 parts by mass, preferably 0.05 to 5 parts by mass, and more preferably 0.1 to 1 part by mass, relative to 100 parts by mass of the (meth)acrylic resin.
[0069] [Silane compounds] The pressure-sensitive adhesive composition may further contain a silane compound. Examples of the silane compound include vinyltrimethoxysilane, vinyltriethoxysilane, vinyltris(2-methoxyethoxy)silane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropylethoxydimethylsilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-chloropropylmethyldimethoxysilane, 3-chloropropyltrimethoxysilane, 3-methacryloyloxypropyltrimethoxysilane, and 3-mercaptopropyltrimethoxysilane. The silane compound may also contain an oligomer derived from the above silane compound.
[0070] The content of the silane compound in the pressure-sensitive adhesive composition is usually 0.01 to 10 parts by mass, and preferably 0.05 to 5 parts by mass, relative to 100 parts by mass of the (meth)acrylic resin. When the content of the silane compound is 0.01 part by mass or more, the adhesion between the pressure-sensitive adhesive layer and the adherend tends to be improved, and when the content is 10 parts by mass or less, bleeding out of the silane compound from the pressure-sensitive adhesive layer tends to be suppressed.
[0071] <Antistatic agent> The pressure-sensitive adhesive composition may further contain an antistatic agent. Examples of the antistatic agent include known ones, and ionic antistatic agents are preferred. Examples of the cationic component constituting the ionic antistatic agent include organic cations and inorganic cations. Examples of the organic cation include pyridinium cation, imidazolium cation, ammonium cation, sulfonium cation, phosphonium cation, etc. Examples of the inorganic cation include alkali metal cations such as lithium cation, potassium cation, sodium cation, and cesium cation, and alkaline earth metal cations such as magnesium cation and calcium cation. Examples of the anionic component constituting the ionic antistatic agent may include either inorganic anion or organic anion, but an anionic component containing a fluorine atom is preferred in terms of excellent antistatic performance. Examples of the anionic component containing a fluorine atom include hexafluorophosphate anion (PF6-), bis(trifluoromethanesulfonyl)imide anion [(CF3SO2)2N-], and bis(fluorosulfonyl)imide anion [(FSO2)2N-] anion. In view of excellent stability over time of the antistatic performance of the pressure-sensitive adhesive composition, an ionic antistatic agent that is solid at room temperature is preferred. The content of the antistatic agent is, for example, 0.01 to 20 parts by mass, preferably 0.1 to 10 parts by mass, and more preferably 1 to 7 parts by mass, relative to 100 parts by mass of the (meth)acrylic resin.
[0072] The adhesive composition may contain one or more additives such as an ultraviolet absorber, a solvent, a crosslinking catalyst, a tackifier resin, a plasticizer, etc. It is also useful to blend an ultraviolet curable compound into the adhesive composition, form an adhesive layer, and then irradiate the adhesive with ultraviolet light to cure the adhesive layer, thereby forming a harder adhesive layer. The thickness of the pressure-sensitive adhesive layer is usually 0.1 to 40 μm, preferably 3 to 40 μm, and more preferably 5 to 40 μm.
[0073] The end 10a of the sheet-shaped polarizing plate protective film 10 is the end of the resin layer 101 in the width direction and the end of the peeling layer 103 in the width direction. The end of the resin layer 101 is a part that does not overlap with the adhesive layer 102 in a planar view. The end of the peeling layer 103 is a part that does not overlap with the adhesive layer 102 in a planar view. When the end 10a of the sheet-shaped polarizing plate protective film 10 is cut by the cutting part 31, the resin layer 101 is cut at the cutting line shown by the two-dot chain line, and the peeling layer 103 is cut at the cutting line shown by the two-dot chain line. As a result, the width dimension of the resin layer 101 and the width dimension of the adhesive layer 102 become the same, and the end face of the resin layer 101 and the end face of the adhesive layer 102 are located on the same plane. In addition, the width dimension of the peeling layer 103 and the width dimension of the adhesive layer 102 become the same, and the end face of the peeling layer 103 and the end face of the adhesive layer 102 are located on the same plane. Here, "same" does not necessarily mean "completely same" but includes "substantially same." For example, if the absolute value of the difference in dimensions is 0.5 mm or less, the item is considered to be "same."
[0074] In this manner, the end portion 10a of the sheet-like polarizing plate protective film 10 is cut to produce a polarizing plate protective film 15 (polarizing plate protective film main body 12). That is, in the polarizing plate protective film 15, the width dimension of the resin layer 101 is the same as the width dimension of the adhesive layer 102, and the width dimension of the peeling layer 103 is the same as the width dimension of the adhesive layer 102. Preferably, the relationship between the width W1 of the polarizing plate protective film (polarizing plate protective film main body 12) after cutting along the cut line shown by the two-dot chain line and the width W0 of the polarizing plate protective film (sheet-like polarizing plate protective film 10) before cutting satisfies W0>W1≧0.95W0.
[0075] (Production device 2) The preparation device 2 is not particularly limited as long as it is a device for preparing a single-layer or laminated polarizing plate protective film. For example, it may be a device for preparing a polarizing plate protective film by melt extrusion or solvent casting, a device for laminating a plurality of polarizing plate protective films with a pair of laminating rolls to prepare a laminated polarizing plate protective film, a device for stretching a polarizing plate protective film to prepare a stretched polarizing plate protective film, a rewinder device, or the like.
[0076] (Take-up device 4) The winding device 4 has a winding roller 40. The winding roller 40 winds the polarizing plate protection film body 12 around it and winds it up into a roll. The polarizing plate protection film body 12 wound up into a roll is then collected as a product.
[0077] (First and second conveying sections 21 and 22) The first conveying section 21 is disposed upstream of the second conveying section 22 in the conveying direction A. The first conveying section 21 has an upper first roller 21a and a lower second roller 21b. The first roller 21a and the second roller 21b are in contact with each other and hold the sheet-like polarizing plate protective film 10 therebetween, and are rotated in the direction of the arrow in FIG. 2 by a motor (not shown) to convey the sheet-like polarizing plate protective film 10 in the conveying direction A.
[0078] The second conveying section 22 has a first roller 22a on the upper side and a second roller 22b on the lower side, similar to the first conveying section 21. The first roller 22a and the second roller 22b rotate in the direction of the arrow in FIG. 2 by a motor (not shown) while sandwiching the polarizer protective film main body 12, thereby conveying the polarizer protective film main body 12 in the conveying direction A.
[0079] In addition, as long as the sheet-like polarizing plate protective film 10 can be transported in the transport direction A, either the first transport section 21 or the second transport section 22 may be provided.
[0080] (cutting section 31) Fig. 5 is a VV cross-sectional view of Fig. 3. As shown in Figs. 2, 3, and 5, the cutting section 31 is disposed between the first transport section 21 and the second transport section 22 in the transport direction A of the sheet-like polarizing plate protective film 10. The cutting section 31 is disposed on the inside of the edge of the sheet-like polarizing plate protective film 10 in the width direction B when viewed from the planar direction. In other words, the cutting section 31 is disposed at a position facing the end 10a of the sheet-like polarizing plate protective film 10.
[0081] The cutting section 31 has a first circular blade 311 and a second circular blade 312. The first circular blade 311 and the second circular blade 312 are in contact with each other to clamp the end 10a of the sheet-like polarizing plate protective film 10, and are rotated by a motor (not shown) to cut the end 10a of the sheet-like polarizing plate protective film 10 along the conveying direction A. The first circular blade 311 is disposed on the lower side in the vertical direction (gravity direction), and the second circular blade 312 is disposed on the upper side in the vertical direction (gravity direction). The first circular blade 311 may be disposed on the upper side, and the second circular blade 312 may be disposed on the lower side.
[0082] Specifically, the first circular blade 311 is rotated in the direction of the arrow in FIG. 2 by a motor (not shown). The second circular blade 312 comes into contact with the first circular blade 311 and rotates together with the first circular blade 311 in the direction of the arrow in FIG. 2. The second circular blade 312 may be rotated, for example, by a motor (not shown), or may be mechanically connected to the first circular blade 311 via a gear and rotate following the first circular blade 311. The sheet-like polarizing plate protective film 10 travels between the first circular blade 311 and the second circular blade 312, and the end portion 10a of the sheet-like polarizing plate protective film 10 is continuously sheared by the first circular blade 311 and the second circular blade 312.
[0083] The second circular blade 312 is formed in a disk shape and has a blade tip on the outer circumferential surface of the second circular blade 312. The first circular blade 311 is formed in a cylindrical shape and has two annular grooves 311a on the outer circumferential surface of the first circular blade 311. Each groove 311a is disposed opposite each of the two second circular blades 312. The blade tip at the bottom of the outer circumferential surface of the second circular blade 312 is disposed so as to enter the groove 311a of the first circular blade 311. The blade tip of the second circular blade 312 is in contact with the inner side surface of the groove 311a. Then, the blade tip of the second circular blade 312 shears the end 10a of the sheet-like polarizing plate protective film 10 while entering the groove 311a of the first circular blade 311.
[0084] The cutting unit 31 is disposed opposite each of both ends 10a of the sheet-like polarizing plate protective film 10 to cut each of the ends 10a, but may be disposed only at one of the ends 10a to cut only one of the ends 10a. The cutting unit 31 may be installed so as to be movable along the width direction B of the sheet-like polarizing plate protective film 10, so that the position can be adjusted according to the product width of the polarizing plate protective film.
[0085] (Cutting section adjustment mechanism 60) Fig. 6 is a schematic diagram showing the cutting unit adjustment mechanism 60. As shown in Fig. 6, the cutting unit adjustment mechanism 60 adjusts the peripheral speed of the second circular blade 312 and the first circular blade 311 of the cutting unit 31. The cutting unit adjustment mechanism 60 has a first speed sensor 61, a second speed sensor 62, a third speed sensor 63, and a control device 65.
[0086] The first speed sensor 61 detects the peripheral speed of the first circular blade 311. The second speed sensor 62 detects the peripheral speed of the second circular blade 312. The third speed sensor 63 calculates the running speed of the sheet-like polarizing plate protective film 10 from the rotation speed of the second conveyor section 22. The first to third speed sensors 61 to 63 are, for example, non-contact sensors such as rotary encoders.
[0087] The first speed sensor 61 may calculate the circumferential speed of the first circular blade 311 from the rotation speed of the first circular blade 311. The second speed sensor 62 may calculate the circumferential speed of the second circular blade 312 from the rotation speed of the second circular blade 312. The third speed sensor 63 may directly detect the running speed of the sheet-like polarizing plate protective film 10.
[0088] The control device 65 controls the circumferential speeds of the first circular blade 311 and the second circular blade 312 based on the circumferential speed and the traveling speed detected by the first to third speed sensors 61 to 63. The control device 65 controls, for example, the motors that drive the first circular blade 311 and the second circular blade 312, respectively.
[0089] The control device 65 controls the peripheral speed V1 of the first circular blade 311 and the running speed V3 of the sheet-type polarizing plate protective film 10 so that the relationship between them satisfies V1≧1.05V3. Preferably, the control device 65 controls them so that the relationship satisfies 1.2V3≧V1≧1.05V3.
[0090] The control device 65 controls the peripheral speed V2 of the second circular blade 312 and the running speed V3 of the sheet-shaped polarizing plate protective film 10 so that the relationship between them satisfies V2≧1.05V3. Preferably, the control device 65 controls them so that the relationship satisfies 1.2V3≧V2≧1.05V3.
[0091] According to the above configuration, the end 10a of the sheet-like polarizing plate protective film 10 is sheared in a state where V1 ≧ 1.05V3 and V2 ≧ 1.05V3 are satisfied, so that it is possible to increase the speed difference between the peripheral speed V1 of the first circular blade 311 and the running speed V3 of the sheet-like polarizing plate protective film 10, and to increase the speed difference between the peripheral speed V2 of the second circular blade 312 and the running speed V3 of the sheet-like polarizing plate protective film 10. This makes it possible to reduce the rotational resistance applied to the first circular blade 311 and the second circular blade 312 due to the adhesive layer 102 adhering to the first circular blade 311 and the second circular blade 312 when the sheet-like polarizing plate protective film 10 is sheared. Therefore, the end 10a of the sheet-shaped polarizing plate protective film 10 can be smoothly sheared, reducing cutting defects of the sheet-shaped polarizing plate protective film 10 (polarizing plate protective film main body 12) and reducing defects (such as cutting chips and splinters) that occur on the cut surface of the sheet-shaped polarizing plate protective film 10 (polarizing plate protective film main body 12).
[0092] This makes it possible to reduce defects (such as chips, glue chips, and cracks) that occur at the interface between the polarizing plate protective film 15 (polarizing plate protective film main body 12) and the polarizing plate 16 when the polarizing plate protective film 15 and the polarizing plate 16 are bonded together, thereby improving the yield of the optical laminate 17.
[0093] In addition, since the end portion 10a of the sheet-like polarizing plate protective film 10 is sheared in a state where 1.2V3≧V1 is satisfied, it is possible to prevent an excessive speed difference between the peripheral speed V1 of the first circular blade 311 and the running speed V3 of the sheet-like polarizing plate protective film 10. This makes it possible to reduce the occurrence of scratches on the polarizing plate protective film 15 (polarizing plate protective film main body 12) caused by the first circular blade 311 sliding against the sheet-like polarizing plate protective film 10.
[0094] In addition, since the end portion 10a of the sheet-like polarizing plate protective film 10 is sheared in a state where 1.2V3≧V2 is satisfied, it is possible to prevent an excessive speed difference between the peripheral speed V2 of the second circular blade 312 and the running speed V3 of the sheet-like polarizing plate protective film 10. This makes it possible to reduce the occurrence of scratches on the polarizing plate protective film 15 (polarizing plate protective film main body 12) caused by the second circular blade 312 sliding against the sheet-like polarizing plate protective film 10.
[0095] (Third conveying section 23) As shown in FIG. 2, the third conveying section 23 is disposed downstream of the cutting section 31 and conveys the cut end 11 cut by the cutting section 31 downstream. The first conveying section 23 has a first roller 23a and a second roller 23b. The first roller 23a and the second roller 23b contact each other to hold the cut end 11 therebetween and are rotated by a motor (not shown) to convey the cut end 11 downstream. A support roller 25 is disposed between the cutting section 31 and the third conveying section 23. The support roller 25 supports the cut end 11.
[0096] Fig. 7 is an explanatory diagram showing the positional relationship between the cut end 11 and the second circular blade 312. As shown in Fig. 3 and Fig. 7, the cut end 11 and the cut polarizing plate protective film (polarizing plate protective film main body 12) are each transported downstream, and the angle between the transport direction of the cut end 11 and the transport direction of the polarizing plate protective film main body 12 is preferably 0.1° or more and 1.4° or less, and more preferably 0.3° or more and 0.7° or less, in a plan view.
[0097] Specifically, the transport direction of the cut end 11 is the transport direction immediately after cutting by the cutting section 31, and is the direction of the arrow A1 (hereinafter referred to as the first transport direction A1). The transport direction of the polarizing plate protective film main body 12 is the transport direction immediately after cutting by the cutting section 31, and is the direction of the arrow A2 (hereinafter referred to as the second transport direction A2). The first transport direction A1 and the second transport direction A2 are directions in which they are separated from each other toward the downstream side. The angle α between the first transport direction A1 and the second transport direction A2 is 0.1° or more and 1.4° or less. In other words, the angle β between the end surface 11a of the cut end 11 on the polarizing plate protective film main body 12 side and the end surface 12a of the polarizing plate protective film main body 12 on the cut end 11 side is the same as the angle α in a plan view, and is 0.1° or more and 1.4° or less.
[0098] The first transport direction A1 corresponds to the transport direction of the cut end 11 existing in the range between a first point P1 of the cutting edge of the second circular blade 312 and a second point P2 of the cutting edge of the second circular blade 312. The second transport direction A2 corresponds to the transport direction of the polarizer protective film main body 12 existing in the range between the first point P1 and the second point P2. The end face 11a of the cut end 11 corresponds to the end face of the cut end 11 existing in the range between the first point P1 and the second point P2. The end face 12a of the polarizer protective film main body 12 corresponds to the end face of the polarizer protective film main body 12 existing in the range between the first point P1 and the second point P2.
[0099] The first point P1 is a point where the edge of the second circular blade 312 enters the groove 311a of the first circular blade 311 and starts to contact the polarizer protective film 10. The second point P2 is a point where the edge of the second circular blade 312 exits the groove 311a of the first circular blade 311 and ends to contact the polarizer protective film 10.
[0100] (Collection Division 50) 2, the collection section 50 is disposed downstream of the third transport section 23. The cut end portions 11 transported by the third transport section 23 are collected in the collection section 50. The cut end portions 11 collected in the collection section 50 are processed, for example, by being crushed.
[0101] (Polarizing plate protection film sending device 5) 1, the polarizing plate protective film feed device 5 feeds downstream the polarizing plate protective film 15 taken up by the winding device 4. The polarizing plate protective film feed device 5 is composed of, for example, a roller.
[0102] (Polarizing plate supply device 6) The polarizing plate supplying device 6 supplies the polarizing plate 16 manufactured by a device not shown in the figure. The polarizing plate supplying device 6 is composed of, for example, a roller.
[0103] (Laminating device 7) The laminating device 7 laminates the polarizing plate protective film 15 fed by the polarizing plate protective film feed device 5 and the polarizing plate 16 fed by the polarizing plate feed device 6 via the adhesive layer 102. At this time, the release layer 103 in the polarizing plate protective film 15 is peeled off from the adhesive layer 102. The laminating device 7 is composed of, for example, two opposing rollers. The polarizing plate protective film 15 and the polarizing plate 16 are laminated together to produce an optical laminate 17. The optical laminate 17 is taken up by an optical laminate take-up device 8.
[0104] (Optical laminate 17) Fig. 8 is a cross-sectional view of the optical laminate 17. As shown in Fig. 8, the optical laminate 17 has a polarizing plate 16 and a polarizing plate protective film 15 laminated on the polarizing plate 16. The polarizing plate protective film 15 includes a resin layer 101 and a pressure-sensitive adhesive layer 102 laminated on each other.
[0105] The adhesive layer 102 contacts the polarizing plate 16. The widthwise dimension of the adhesive layer 102 and the widthwise dimension of the resin layer 101 are the same. "Same" does not necessarily mean completely the same, but includes substantially the same. For example, when the absolute value of the difference in dimensions is 0.5 mm or less, they are considered to be the same. In other words, the widthwise end faces of the adhesive layer 102 and the widthwise end faces of the resin layer 101 are located on the same plane.
[0106] The widthwise dimension of the adhesive layer 102 and the widthwise dimension of the resin layer 101 are smaller than the widthwise dimension of the polarizing plate 16. In other words, the end face of the polarizing plate 16 in the widthwise direction is located on the outer side in the widthwise direction of the end face of the adhesive layer 102 and the end face of the resin layer 101 in the widthwise direction.
[0107] With the above-mentioned configuration, the width dimension of the adhesive layer 102 and the width dimension of the resin layer 101 are the same, so that the end of the resin layer 101 contacts the adhesive layer 102. This makes it possible to suppress moisture absorption deformation of the end of the resin layer 101 in the width direction, and to suppress peeling of the resin layer 101 from the adhesive layer 102 due to moisture absorption deformation. Therefore, defects of the polarizing plate protective film 15 can be reduced, and the yield of the optical laminate 16 can be improved.
[0108] [Method of manufacturing optical laminate] Next, one embodiment of a method for producing an optical laminate will be described with reference to FIGS.
[0109] First, a polarizing plate protective film (sheet-shaped polarizing plate protective film 10) including a resin layer 101 and an adhesive layer 102 laminated to each other is run between a first circular blade 311 that is rotated and a second circular blade 312 that is in contact with the first circular blade 311 and rotates together with the first circular blade 311, and an end 10a in the width direction of the polarizing plate protective film 10 is continuously sheared by the first circular blade 311 and the second circular blade 312. Hereinafter, this is referred to as the first step. Thereafter, the polarizing plate protective film 15 (polarizing plate protective film main body 12) whose end 10a has been sheared is bonded to a polarizing plate 16 to form an optical laminate 17. Hereinafter, this is referred to as the second step.
[0110] In the first step, the end 10a of the polarizing plate protective film 10 is sheared under a condition in which the relationship between the peripheral speed V1 of the first circular blade 311 and the running speed V3 of the polarizing plate protective film 10 satisfies V1≧1.05V3, and the relationship between the peripheral speed V2 of the second circular blade 312 and the running speed V3 of the polarizing plate protective film 10 satisfies V2≧1.05V3.
[0111] According to the above configuration, the end 10a of the polarizing plate protective film 10 is sheared in a state where V1 ≧ 1.05V3 and V2 ≧ 1.05V3 are satisfied, so that the speed difference between the circumferential speed V1 of the first circular blade 311 and the running speed V3 of the polarizing plate protective film 10 can be increased, and the speed difference between the circumferential speed V2 of the second circular blade 312 and the running speed V3 of the polarizing plate protective film 10 can be increased. This makes it possible to reduce the rotational resistance applied to the first circular blade 311 and the second circular blade 312 due to the adhesive layer 102 adhering to the first circular blade 311 and the second circular blade 312 when shearing the polarizing plate protective film 10. Therefore, the end 10a of the polarizing plate protective film 10 can be smoothly sheared, reducing cutting defects of the polarizing plate protective film 10 (polarizing plate protective film main body 12) and reducing defects (such as cutting chips and burrs) that occur on the cut surface of the polarizing plate protective film 10 (polarizing plate protective film main body 12).
[0112] Therefore, when bonding the polarizing plate protective film 15 (polarizing plate protective film main body 12) and the polarizing plate 16, defects (such as chips, glue chips, and cracks) that occur at the interface between the polarizing plate protective film 15 and the polarizing plate 16 can be reduced, and the yield of the optical laminate 17 can be improved.
[0113] Preferably, in the first step, the edge 10a of the polarizing plate protective film 10 is sheared in a state where the relationship between the circumferential speed V1 of the first circular blade 311 and the running speed V3 of the polarizing plate protective film satisfies 1.2V3 ≧ V1 ≧ 1.05V3. This satisfies V1 ≧ 1.05V3, so that as described above, it is possible to reduce cutting defects of the polarizing plate protective film 10 (polarizing plate protective film main body 12) and improve the yield of the optical laminate 17. In addition, since 1.2V3 ≧ V1 is satisfied, it is possible to prevent the speed difference between the circumferential speed V1 of the first circular blade 311 and the running speed V3 of the sheet-like polarizing plate protective film 10 from becoming excessive. Therefore, it is possible to reduce the occurrence of scratches on the polarizing plate protective film 15 (polarizing plate protective film main body 12) caused by the first circular blade 311 sliding against the polarizing plate protective film 10.
[0114] Preferably, in the first step, the end 10a of the polarizing plate protective film 10 is sheared in a state where the relationship between the circumferential speed V2 of the second circular blade 312 and the running speed V3 of the polarizing plate protective film satisfies 1.2V3 ≧ V2 ≧ 1.05V3. This satisfies V2 ≧ 1.05V3, so that as described above, it is possible to reduce cutting defects of the polarizing plate protective film 10 (polarizing plate protective film main body 12) and improve the yield of the optical laminate 17. In addition, since 1.2V3 ≧ V2 is satisfied, it is possible to prevent the speed difference between the circumferential speed V2 of the second circular blade 312 and the running speed V3 of the sheet-like polarizing plate protective film 10 from becoming excessive. Therefore, it is possible to reduce the occurrence of scratches on the polarizing plate protective film 15 (polarizing plate protective film main body 12) caused by the second circular blade 312 sliding against the polarizing plate protective film 10.
[0115] Preferably, in the first step, the edge 10a of the polarizing plate protective film 10 is sheared in a state in which the peripheral speed V1 of the first circular blade 311 and the peripheral speed V2 of the second circular blade 312 are the same. This makes it easier to control the peripheral speed V1 of the first circular blade 311 and the peripheral speed V2 of the second circular blade 312. Here, the peripheral speeds V1 and V2 being the same does not necessarily mean that they are completely the same, but also includes that they are substantially the same. For example, when the absolute value of the difference between the peripheral speeds V1 and V2 is 0.1 m / min or less, they are considered to be the same.
[0116] Preferably, as shown in Fig. 4, the thickness of the adhesive layer 102 of the polarizing plate protective film 10 is 10 μm or more and 40 μm or less. According to this, when the thickness of the adhesive layer 102 is 10 μm or more, the adhesive layer 102 adheres to the first circular blade 311 and the second circular blade 312 when the polarizing plate protective film 10 is sheared, and the rotation resistance applied to the first circular blade 311 and the second circular blade 312 may be large due to the adhesive layer 102 adhering to the first circular blade 311 and the second circular blade 312. However, as described above, since V1 ≥ 1.05V3 is satisfied and V2 ≥ 1.05V3 is satisfied, the cutting failure of the polarizing plate protective film 10 can be reduced and the yield of the optical laminate 17 can be improved. In addition, since the thickness of the adhesive layer 102 is 40 μm or less, for example, when the polarizing plate protective film 10 is finally peeled off from the optical laminate 17, the polarizing plate protective film 10 can be easily peeled off from the optical laminate 17.
[0117] Preferably, as shown in Fig. 4, the relationship between the width W1 of the polarizing plate protection film (polarizing plate protection film main body 12) after shearing and the width W0 of the polarizing plate protection film 10 before shearing satisfies W0>W1≧0.95W0. According to this, the end portion 10a to be sheared has a narrow width. As described above, since V1≧1.05V3 and V2≧1.05V3 are satisfied, the end portion 10a of the polarizing plate protection film 10 can be smoothly sheared.
[0118] Preferably, as shown in FIG. 3, in the first step, the cut end 11 and the polarizing plate protective film (polarizing plate protective film main body 12) after shearing are transported downstream, and the angle α between the first transport direction A1 of the cut end 11 and the second transport direction A2 of the polarizing plate protective film (polarizing plate protective film main body 12) after shearing is 0.1° or more and 1.4° or less, more preferably 0.3° or more and 0.7° or less. According to this, since the angle with the transport direction is 0.1° or more, it is possible to suppress the cut end 11 from interfering with the second circular blade 312 or the first circular blade 311. Therefore, it is possible to suppress the vibration of the polarizing plate protective film (polarizing plate protective film main body 12) caused by the cut end 11 contacting the second circular blade 312 or the first circular blade 311. In addition, since the angle with the transport direction is 1.4° or less, it is possible to suppress the generation of a force that tears the cut end 11 from the polarizing plate protective film 10 to the outside in the width direction. Therefore, it is possible to prevent the cut surface of the polarizing plate protective film (polarizing plate protective film body 12) from becoming rough.
[0119] Preferably, as shown in FIG. 8, in the optical laminate 17 produced in the second step, the adhesive layer 102 contacts the polarizing plate 16, the width dimension of the adhesive layer 102 is the same as the width dimension of the resin layer 101, and the width dimension of the adhesive layer 102 is smaller than the width dimension of the polarizing plate 16. According to this, since the width dimension of the adhesive layer 102 is the same as the width dimension of the resin layer 101, the end of the resin layer 101 in the width direction contacts the adhesive layer 102. This can suppress moisture absorption deformation of the end of the resin layer 101 and suppress peeling of the resin layer 101 from the adhesive layer 102 due to moisture absorption deformation. Therefore, defects of the polarizing plate protective film 15 can be reduced, and the yield of the optical laminate 17 can be improved.
[0120] The present disclosure is not limited to the above-described embodiment, and the design can be modified without departing from the scope of the present disclosure. For example, the method for producing an optical laminate of the present disclosure is not limited to being realized by the production apparatus 1 shown in Figs. 1, 2, and 3, and may be realized by other different apparatuses.
[0121] <Example> Next, an example will be described. The peripheral speed V1 of the first circular blade 311 and the running speed V3 of the sheet-like polarizing plate protective film 10 were variously changed to shear the end portion 10a of the sheet-like polarizing plate protective film 10, and the number and ratio of defects in the sheet-like polarizing plate protective film 10 were measured. The measurement results are shown in Table 1.
[0122] [Table 1] TIFF2024157266000003.tif36147
[0123] As shown in Table 1, the defects of the polarizing plate protective film refer to defects (such as chips and burrs) that occur on the cut surface of the sheet-shaped polarizing plate protective film 10 (polarizing plate protective film body 12) after the end 10a of the sheet-shaped polarizing plate protective film 10 is sheared. The number of defects refers to the number of defects in a predetermined range of the polarizing plate protective film (polarizing plate protective film body 12) after shearing. The predetermined range is a range of 1 cm in the width direction (direction B) and 5 m in the longitudinal direction (direction A) from the end face (reference number 12a in FIG. 3) of the polarizing plate protective film after cutting. The defect ratio refers to the ratio of the number of defects when the number of defects in Comparative Example 1, which has the largest number of defects, is set to 100%. The peripheral speed V2 of the second circular blade 312 is the same as the peripheral speed V1 of the first circular blade 311, and V1 / V2 is also the same as V1 / V3.
[0124] Based on Table 1, the relationship between the peripheral speed V1 of the first circular blade 311 and the defect ratio of the polarizer protective film is shown in the graph of Fig. 9. In Fig. 9, the horizontal axis represents the peripheral speed V1 of the first circular blade 311, and the vertical axis represents the defect ratio of the polarizer protective film.
[0125] 9, in Comparative Examples 1, 2, and 3, V1 / V3 was smaller than 1.05, i.e., V1<1.05V3, and the number of defects was large and the defect ratio was high. In contrast, in Example 1, V1 / V3 was larger than 1.05, i.e., V1≧1.05V3, and the number of defects was small and the defect ratio was low. In each of Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3, the angle between the first transport direction of the cut end and the second transport direction of the polarizing plate protective film after shearing was 0.3°.
[0126] Therefore, it was confirmed that by shearing the end 10a of the polarizing plate protective film 10 while satisfying V1≧1.05V3 and V2≧1.05V3, cutting defects of the polarizing plate protective film 10 (polarizing plate protective film main body 12) are reduced, and defects (such as cutting chips and burrs) occurring on the cut surface of the polarizing plate protective film 10 (polarizing plate protective film main body 12) are reduced.
[0127] The present disclosure includes the following aspects. <1> a first step of running a polarizing plate protective film including a resin layer and a pressure-sensitive adhesive layer laminated to each other between a first circular blade that is rotated and a second circular blade that is in contact with the first circular blade and rotates together with the first circular blade, thereby continuously shearing the widthwise end of the polarizing plate protective film with the second circular blade and the first circular blade; a second step of bonding the polarizing plate protective film with the edge portion sheared to a polarizing plate to form an optical laminate; Equipped with A method for producing an optical laminate, wherein in the first step, the end of the polarizing plate protection film is sheared in a state in which the relationship between the peripheral speed V1 of the first circular blade and the running speed V3 of the polarizing plate protection film satisfies V1≧1.05V3, and the relationship between the peripheral speed V2 of the second circular blade and the running speed V3 of the polarizing plate protection film satisfies V2≧1.05V3. <2> In the first step, the edge of the polarizing plate protective film is sheared in a state in which the relationship between the peripheral speed V1 of the first circular blade and the running speed V3 of the polarizing plate protective film satisfies 1.2V3≧V1≧1.05V3. <1> A method for producing the optical laminate described in claim 1. <3> In the first step, the edge of the polarizing plate protective film is sheared in a state in which the peripheral speed V1 of the first circular blade and the peripheral speed V2 of the second circular blade are the same. <1> or <2> A method for producing the optical laminate described in claim 1. <4> The thickness of the pressure-sensitive adhesive layer is 10 μm or more and 40 μm or less. <1> from <3> 13. A method for producing an optical laminate according to claim 12. <5> The relationship between the width W1 of the polarizing plate protective film after shearing and the width W0 of the polarizing plate protective film before shearing satisfies W0>W1≧0.95W0. <1> from <4> 13. A method for producing an optical laminate according to claim 12. <6> In the first step, the sheared end portion and the polarizing plate protective film after shearing are transported downstream, and an angle between a transport direction of the sheared end portion and a transport direction of the polarizing plate protective film after shearing is 0.1° or more and 1.4° or less. <1> from <5> 13. A method for producing an optical laminate according to claim 12. <7> In the optical laminate, the pressure-sensitive adhesive layer is in contact with the polarizing plate, The width direction dimension of the pressure-sensitive adhesive layer and the width direction dimension of the resin layer are the same, the width direction dimension of the pressure-sensitive adhesive layer and the width direction dimension of the resin layer are smaller than the width direction dimension of the polarizing plate; <1> from <6> 13. A method for producing an optical laminate according to claim 12. <8> A polarizing plate; a polarizing plate protective film laminated on the polarizing plate; Equipped with The polarizing plate protective film includes a resin layer and a pressure-sensitive adhesive layer laminated together, the pressure-sensitive adhesive layer is in contact with the polarizing plate, The width direction dimension of the pressure-sensitive adhesive layer and the width direction dimension of the resin layer are the same, an optical laminate, wherein the width direction dimension of the pressure-sensitive adhesive layer and the width direction dimension of the resin layer are smaller than the width direction dimension of the polarizing plate. [Explanation of symbols]
[0128] 1. Polarizing plate protection film manufacturing equipment 2. Production equipment 3 End Processing Equipment 4 Winding device 5. Polarizing plate protection film delivery device 6 Polarizing plate supply device 7 Laminating device 8. Optical laminate winding device 9. Optical laminate manufacturing equipment 10. Sheet-shaped polarizing plate protection film 101 Resin layer 102 Adhesive layer 103 Peeling layer 10a end 11 Cut end 11a End face 12 Polarizing plate protection film body 12a End face 15 Polarizing plate protection film 16 Polarizing plate 17 Optical laminate 21, 22, 23 First, second, and third conveying sections 31 Cut section 311 First round blade 311a Groove 312 2nd round blade 50 Collection Department 60 Cutting section adjustment mechanism 61 First speed sensor 62 Second speed sensor 63 3rd speed sensor 65 Control device A Conveying direction A1 First conveying direction A2 Second conveying direction α Angle between the first conveying direction and the second conveying direction β Angle between the edge of the cut end and the edge of the polarizing plate protective film body
Claims
1. a first step of running a polarizing plate protective film including a resin layer and a pressure-sensitive adhesive layer laminated to each other between a first circular blade that is rotated and a second circular blade that is in contact with the first circular blade and rotates together with the first circular blade, thereby continuously shearing an end portion of the polarizing plate protective film in the width direction with the second circular blade and the first circular blade; a second step of bonding the polarizing plate protective film with the edge portion sheared to a polarizing plate to form an optical laminate; Equipped with A method for producing an optical laminate, wherein in the first step, the end of the polarizing plate protective film is sheared in a state in which the relationship between the peripheral speed V1 of the first circular blade and the running speed V3 of the polarizing plate protective film satisfies V1≧1.05V3, and the relationship between the peripheral speed V2 of the second circular blade and the running speed V3 of the polarizing plate protective film satisfies V2≧1.05V3.
2. 2. The method for producing an optical laminate according to claim 1, wherein in the first step, the end of the polarizing plate protective film is sheared in a state in which the relationship between the peripheral speed V1 of the first circular blade and the running speed V3 of the polarizing plate protective film satisfies 1.2V3≧V1≧1.05V3.
3. 3. The method for producing an optical laminate according to claim 1, wherein in the first step, the end of the polarizing plate protective film is sheared in a state in which a peripheral speed V1 of the first circular blade and a peripheral speed V2 of the second circular blade are the same.
4. The method for producing an optical laminate according to claim 1 or 2, wherein the pressure-sensitive adhesive layer has a thickness of 10 μm or more and 40 μm or less.
5. The method for producing an optical laminate according to claim 1 or 2, wherein a relationship between a width W1 of the polarizing plate protective film after shearing and a width W0 of the polarizing plate protective film before shearing satisfies W0>W1≧0.95W0.
6. 3. The method for producing an optical laminate according to claim 1 or 2, wherein in the first step, the sheared end and the polarizing plate protective film after shearing are each transported downstream, and an angle between the transport direction of the sheared end and the transport direction of the polarizing plate protective film after shearing is 0.1° or more and 1.4° or less.
7. In the optical laminate, the pressure-sensitive adhesive layer is in contact with the polarizing plate, The width direction dimension of the pressure-sensitive adhesive layer and the width direction dimension of the resin layer are the same, The method for producing an optical laminate according to claim 1 , wherein a width dimension of the pressure-sensitive adhesive layer and a width dimension of the resin layer are smaller than a width dimension of the polarizing plate.
8. A polarizing plate; a polarizing plate protective film laminated on the polarizing plate; Equipped with The polarizing plate protective film includes a resin layer and a pressure-sensitive adhesive layer laminated together, the pressure-sensitive adhesive layer is in contact with the polarizing plate, The width direction dimension of the pressure-sensitive adhesive layer and the width direction dimension of the resin layer are the same, an optical laminate, wherein the width direction dimension of the pressure-sensitive adhesive layer and the width direction dimension of the resin layer are smaller than the width direction dimension of the polarizing plate.