Polarization plate having retardation layer and picture display unit equipped with the polarization plate having retardation layer

The polarizing plate with a retardation layer addresses cracking issues and maintains viewing angle characteristics by using a combination of liquid crystal and resin film layers, ensuring no cracks during bending tests and enhancing overall durability.

JP2024157969APending Publication Date: 2024-11-08NITTO DENKO CORP

Patent Information

Application Number
JP2023072674
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Conventional polarizing plates with retardation layers suffer from cracking during bending tests and compromise viewing angle characteristics due to the use of alignment solidified layers of liquid crystal compounds, particularly when subjected to inward bending with a small radius.

Method used

A polarizing plate design incorporating a first retardation layer made of a liquid crystal alignment solidified layer and a second retardation layer composed of a resin film with nz>nx=ny, separated by an adhesive layer, ensuring no cracks in the second layer during a bending test with a 1.5 mm radius and 50,000 bends, while maintaining excellent viewing angle characteristics.

Benefits of technology

The design achieves a thin polarizing plate with enhanced bending resistance and improved viewing angle performance by minimizing cracks and optimizing the retardation layer structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024157969000001_ABST
    Figure 2024157969000001_ABST
Patent Text Reader

Abstract

To provide a polarization plate having a retardation layer, being thin and excellent in flex resistance and visual field angle characteristics.SOLUTION: A polarization plate having a retardation layer includes: a polarization plate including a polarizer; a retardation layer including a first retardation layer being an oriented solidified layer of a liquid crystal compound and a second retardation layer being a resin film with a refractive index characteristic showing a relation of nz>nx=ny; and a first adhesion layer arranged between the first retardation layer and the second retardation layer. The number of cracks of the second retardation layer is 0 or less in an inward bending test of 50 thousand bends with bending radius R 1.5 mm.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polarizing plate with a retardation layer and an image display device having the polarizing plate with a retardation layer. [Background technology]

[0002] Image display devices, such as liquid crystal display devices and electroluminescence (EL) display devices (e.g., organic EL display devices, inorganic EL display devices), are rapidly becoming widespread. In these image display devices, retardation layer-attached polarizing plates are used for the purpose of improving display characteristics and preventing reflection. As a general retardation layer-attached polarizing plate, a retardation layer functioning as a λ / 4 plate is laminated so that its slow axis forms an angle of about 45° with respect to the absorption axis of the polarizer. In addition, from the viewpoint of viewing angle compensation, a retardation layer-attached polarizing plate in which a retardation layer exhibiting a refractive index characteristic of nz>nx=ny is further laminated on the opposite side of the retardation layer from the polarizer has also been proposed. In recent years, there has been an increasing demand for thinner image display devices, and an orientation-solidified layer of a liquid crystal compound is used as the retardation layer. In a retardation layer-attached polarizing plate having an orientation-solidified layer of a liquid crystal compound, cracks may occur in the retardation layer during a bending test. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2022-14611 Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention has been made to solve the above-mentioned problems in the conventional art, and a main object of the present invention is to provide a polarizing plate with a retardation layer which is thin and has excellent bending resistance and viewing angle characteristics. [Means for solving the problem]

[0005] 1. A polarizing plate with a retardation layer according to an embodiment of the present invention comprises: a polarizing plate including a polarizer; a retardation layer including a first retardation layer which is an alignment solidified layer of a liquid crystal compound; and a second retardation layer which is a resin film whose refractive index characteristics satisfy the relationship nz>nx=ny; and a first adhesive layer disposed between the first retardation layer and the second retardation layer, and the number of cracks in the second retardation layer in an inward bending test with a bending radius R of 1.5 mm and 50,000 bending cycles is 0 or less. 2. In the retardation layer-attached polarizing plate described in 1 above, the first retardation layer may be a single layer, have an in-plane retardation Re(550) of 100 nm to 190 nm, and satisfy Re(450) / Re(550)<1, and have an angle of 40° to 50° between a slow axis of the first retardation layer and an absorption axis of the polarizer. 3. In the retardation layer-attached polarizing plate described in 1 above, the first retardation layer may be a laminate of a liquid crystal compound alignment solidified layer A and a liquid crystal alignment solidified layer B, the alignment solidified layer A of the liquid crystal compound has Re(550) of 200 nm to 300 nm, the alignment solidified layer B of the liquid crystal compound has Re(550) of 100 nm to 200 nm, the angle between the slow axis of the alignment solidified layer A of the liquid crystal compound and the absorption axis of the polarizer is 14° to 20°, and the angle between the slow axis of the alignment solidified layer B of the liquid crystal compound and the absorption axis of the polarizer is 75° to 81°. 4. In the polarizing plate with a retardation layer described in 3 above, the alignment and fixed layer A of the liquid crystal compound, the first adhesive layer, the second retardation layer, and the alignment and fixed layer B of the liquid crystal compound may be laminated in this order. 5. In the retardation layer-attached polarizing plate according to any one of the above 1 to 4, the first retardation layer may have a thickness of 10 μm or less. 6. In the retardation layer-attached polarizing plate according to any one of the above 1 to 5, the second retardation layer may have a thickness of 10 μm or less. 7. In the retardation layer-attached polarizing plate according to any one of the above 1 to 6, the first adhesive layer may have a thickness of 7 μm or less. 8. In the retardation layer-attached polarizing plate according to any one of the above items 1 to 7, the second retardation layer may be made of a resin film containing a polymer exhibiting negative birefringence. 9. The retardation layer-attached polarizing plate according to any one of the above items 1 to 8 may further have a pressure-sensitive adhesive layer as the outermost layer, and the pressure-sensitive adhesive layer may have a storage modulus of 200 kPa or less. 10. In another aspect of the present invention, there is provided an image display device, which comprises the retardation layer-attached polarizing plate according to any one of 1 to 9 above. Effect of the Invention

[0006] According to an embodiment of the present invention, it is possible to provide a retardation layer-attached polarizing plate which is thin and has excellent bending resistance and viewing angle characteristics. [Brief description of the drawings]

[0007] [Figure 1] 1 is a schematic cross-sectional view of a retardation layer-attached polarizing plate according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view of a retardation layer-attached polarizing plate according to another embodiment of the present invention. [Diagram 3] 1 shows the measurement results of reflected luminance and reflected hue in the L*a*b* color space chromaticity diagram of retardation layer-attached polarizing plates of the examples of the present invention and the comparative examples. [Figure 4] 1A to 1C are diagrams illustrating a method for fixing a sample during a bending test in an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.

[0009] (Definition of terms and symbols) The definitions of terms and symbols used in this specification are as follows. (1) Refractive index (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the direction perpendicular to the slow axis in the plane (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-plane phase difference (Re) "Re(λ)" is the in-plane retardation measured with light of wavelength λ nm at 23° C. For example, "Re(550)" is the in-plane retardation measured with light of wavelength 550 nm at 23° C. Re(λ) is calculated by the formula: Re(λ)=(nx-ny)×d, where d(nm) is the thickness of the layer (film). (3) Retardation in the thickness direction (Rth) "Rth(λ)" is the retardation in the thickness direction measured with light of wavelength λ nm at 23° C. For example, "Rth(550)" is the retardation in the thickness direction measured with light of wavelength 550 nm at 23° C. Rth(λ) is calculated by the formula: Rth(λ)=(nx-nz)×d, where d(nm) is the thickness of the layer (film). (4) Nz coefficient The Nz coefficient is calculated by Nz=Rth / Re. (5)Angle When angles are referred to herein, the angles include both clockwise and counterclockwise angles relative to a reference direction, so for example, "45°" means ±45°.

[0010] A. Overall structure of the polarizing plate with a retardation layer FIG. 1 is a schematic cross-sectional view of a polarizing plate with a retardation layer according to one embodiment of the present invention. The polarizing plate with a retardation layer 100 in the illustrated example has a retardation layer including a polarizing plate 10, a first retardation layer 20 which is an alignment solidified layer of a liquid crystal compound (hereinafter also referred to as a liquid crystal alignment solidified layer), a second retardation layer 40 which is a resin film whose refractive index characteristics show the relationship of nz>nx=ny, and a first adhesive layer 30 disposed between the first retardation layer and the second retardation layer, in this order from the viewing side. The retardation layer has a circular polarization function or an elliptical polarization function. In the illustrated example, the polarizing plate 10, the first retardation layer 20, the first adhesive layer 30, and the second retardation layer 40 are laminated in this order, but the polarizing plate 10, the second retardation layer 40, the first adhesive layer 30, and the first retardation layer 20 may be laminated in this order. The polarizing plate 10 typically includes a polarizer 11 and protective layers 12 and 13 arranged on both sides of the polarizer 11. The protective layer 13 may be omitted. For example, when the retardation layer (i.e., the retardation layer arranged on the polarizer side of the first retardation layer 20 or the second retardation layer 40) can also function as a protective layer, the protective layer 13 may be omitted. Each member constituting the retardation layer-attached polarizing plate may be laminated via any appropriate adhesive layer (not shown). Specific examples of the adhesive layer include an adhesive layer and a pressure-sensitive adhesive layer. Thus, the first adhesive layer may be a pressure-sensitive adhesive layer or an adhesive layer. The first retardation layer 20, which is a liquid crystal alignment solidified layer, may be a single layer or a laminate of two or more layers. FIG. 2 is a schematic cross-sectional view of a retardation layer-attached polarizing plate according to another embodiment of the present invention. In this illustrated example, the first retardation layer 20 is a laminate of a liquid crystal alignment solidified layer A21 and a liquid crystal alignment solidified layer B22. In a polarizing plate with a retardation layer having a liquid crystal alignment solidified layer and a retardation layer having a refractive index characteristic of nz>nx=ny, so-called a positive C plate, bending resistance may be a problem. In particular, in an inward bending test in which the polarizing plate is bent so that it faces inward, the layer on the outside is subjected to a greater load during bending, and cracks may occur in the positive C plate. Therefore, when a thin polarizing plate with a retardation layer is formed, it may be difficult to achieve both excellent bending resistance and viewing angle characteristics. The polarizing plate with a retardation layer according to an embodiment of the present invention includes a first retardation layer which is a liquid crystal alignment solidified layer and a second retardation layer which is a positive C plate of a resin film.This retardation layer-attached polarizing plate has a bending radius R of 1.5 mm and a number of cracks in the second retardation layer in an inward bending test of 50,000 times. With such a retardation layer-attached polarizing plate, a retardation layer-attached polarizing plate that is thin and has excellent bending resistance and viewing angle characteristics can be provided. In this specification, the inward bending test can be performed by the following method. <Inner bending test> The polarizing plate with a retardation layer is cut into a size of 10 cm x 5 cm so that the angle between the absorption axis of the polarizer and the long side is 135°. The cut polarizing plate with a retardation layer is attached to a resin film with a thickness of 20 μm (for example, Toyo Kohan Co., Ltd., product name: RV-20UB) via an adhesive layer with a thickness of 15 μm to prepare a measurement sample. This measurement sample is subjected to a continuous bending test using a bending tester (for example, Yuasa System Co., Ltd., product name "CL09 Type D01"). The measurement sample is fixed so that the resin film side is in contact with the bending tester, and is bent at 25°C (room temperature) with the viewing side protective layer facing inward. The bending radius of curvature is 1.5 mm, and the bending speed is 30 times / min. After bending the measurement sample 50,000 times, the presence or absence of cracks in the second retardation layer was visually checked, and if cracks were found, the cross section was further observed with a scanning electron microscope (SEM) to identify the layer in which the cracks had occurred.

[0011] In one embodiment, the retardation layer-attached polarizing plate 100 is preferably provided with a pressure-sensitive adhesive layer 50 on the outermost layer (for example, the surface of the second retardation layer 40 in FIG. 1 that is not in contact with the first adhesive layer 30), and can be attached to an image display device (substantially, an image display cell). For practical purposes, it is preferable that a release liner is temporarily attached to the surface of the pressure-sensitive adhesive layer 50 until the retardation layer-attached polarizing plate is used. By temporarily attaching the release liner, the pressure-sensitive adhesive layer is protected until actual use, and the retardation layer-attached polarizing plate can be rolled.

[0012] The thickness of the retardation layer-attached polarizing plate can be set to any appropriate value. In one embodiment, the total thickness of the retardation layer-attached polarizing plate is preferably 150 μm or less, more preferably 140 μm or less, even more preferably 120 μm or less, more preferably 100 μm or less, even more preferably 90 μm or less, and particularly preferably 85 μm or less. The total thickness of the retardation layer-attached polarizing plate can be, for example, 30 μm or more. The total thickness of the retardation layer-attached polarizing plate refers to the sum of the thicknesses of the polarizing plate, the retardation layer (the first retardation layer and the second retardation layer) and the adhesive layer for laminating them (that is, the total thickness of the retardation layer-attached polarizing plate does not include the thickness of the pressure-sensitive adhesive layer provided as the outermost layer and the release liner that can be temporarily attached to the surface of the pressure-sensitive adhesive layer).

[0013] The retardation layer-attached polarizing plate preferably has an average reflected luminance Y (Ave) measured at a polar angle θ of 50° of 0.8 or less, more preferably 0.75 or less. In addition, the difference ΔY between the maximum and minimum luminance values ​​measured at a polar angle θ of 50° is preferably 0.25 or less, more preferably 0.23 or less. * value and b * Δa calculated from the value using the following formula * b * The maximum value of Y(Ave), ΔY and Δa is preferably 9.0 or less, and more preferably 8.5 or less. * b * When the maximum value of Y(Ave), ΔY and Δa is within the above range, the viewing angle characteristic is excellent. * b * is measured using a display measurement system (e.g., Konica Minolta, product name "DMS505"). * a * b * Reflection luminance in color space L * Value and hue a * value, and b * It is calculated from the value by the following formula. In the following formula, A and B are L * a * b *In the color space chromaticity diagram, the azimuth angle represents the point where the hue is most distant at a polar angle of 50°, and is a value that is a multiple of 15 within the range of 0° to 345°. In this specification, the polar angle (θ) refers to the angle inclined from the Z axis to the XY plane direction, assuming that the surface of the retardation layer-attached polarizing plate is the X axis and the Y axis, and the axis perpendicular to the XY plane is the Z axis. In addition, the azimuth angle (φ) refers to the angle defined by setting the MD direction of the polarizing plate used in the retardation layer-attached polarizing plate as 0° and the MD direction of this polarizing plate and the measurement angle in the counterclockwise direction. Δa * b * =√(a * A- a * B ) 2 +(b * A -b * B ) 2

[0014] The components of the retardation layer-attached polarizing plate will be described in more detail below.

[0015] B. Polarizing plate B-1.Polarizer A polarizer is typically composed of a resin film containing a dichroic material (typically, iodine). As the resin film, any appropriate resin film that can be used as a polarizer can be adopted. The resin film is typically a polyvinyl alcohol resin (hereinafter, referred to as "PVA resin") film. The resin film may be a single-layer resin film or a laminate of two or more layers.

[0016] A specific example of a polarizer composed of a single-layer resin film is a PVA-based resin film that has been subjected to a dyeing treatment with iodine and a stretching treatment (typically, uniaxial stretching). The dyeing with iodine is performed, for example, by immersing the PVA-based resin film in an aqueous iodine solution. The stretching ratio of the uniaxial stretching is preferably 3 to 7 times. The stretching may be performed after the dyeing treatment or while dyeing. Alternatively, the film may be stretched and then dyed. If necessary, the PVA-based resin film is subjected to a swelling treatment, a crosslinking treatment, a washing treatment, a drying treatment, or the like. For example, by immersing the PVA-based resin film in water and washing it before dyeing, not only can dirt and antiblocking agents on the surface of the PVA-based resin film be washed off, but also the PVA-based resin film can be swelled to prevent uneven dyeing.

[0017] Specific examples of polarizers obtained using a laminate include a laminate of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, or a polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate. A polarizer obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate can be produced by, for example, applying a PVA-based resin solution to the resin substrate and drying the resin substrate to form a PVA-based resin layer on the resin substrate to obtain a laminate of the resin substrate and the PVA-based resin layer; stretching and dyeing the laminate to make the PVA-based resin layer into a polarizer. In this embodiment, a polyvinyl alcohol-based resin layer containing a halide and a polyvinyl alcohol-based resin is preferably formed on one side of the resin substrate. The stretching typically includes immersing the laminate in an aqueous boric acid solution to stretch it. Furthermore, the stretching may further include, as necessary, stretching the laminate in air at a high temperature (for example, 95° C. or higher) before stretching in the aqueous boric acid solution. In addition, in this embodiment, the laminate is preferably subjected to a drying shrinkage treatment in which the laminate is heated while being transported in the longitudinal direction to shrink the laminate by 2% or more in the width direction. Typically, the manufacturing method of this embodiment includes subjecting the laminate to an air-assisted stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment in this order. By introducing the auxiliary stretching, even when PVA is applied onto a thermoplastic resin, it is possible to increase the crystallinity of the PVA, and to achieve high optical properties. At the same time, by increasing the orientation of the PVA in advance, problems such as a decrease in the orientation or dissolution of the PVA when immersed in water in the subsequent dyeing and stretching steps can be prevented, and high optical properties can be achieved. Furthermore, when the PVA-based resin layer is immersed in a liquid, the orientation disorder and the decrease in the orientation of the polyvinyl alcohol molecules can be suppressed compared to when the PVA-based resin layer does not contain a halide. This can improve the optical properties of a polarizer obtained through a treatment process in which the laminate is immersed in a liquid, such as a dyeing treatment and an underwater stretching treatment. Furthermore, the optical properties can be improved by shrinking the laminate in the width direction by the drying shrinkage treatment.The obtained laminate of resin substrate / polarizer may be used as it is (i.e., the resin substrate may be used as a protective layer for the polarizer), or the resin substrate may be peeled off from the laminate of resin substrate / polarizer, and any suitable protective layer may be laminated on the peeled surface depending on the purpose. Details of the method for producing such a polarizer are described in, for example, JP-A-2012-73580 (Patent No. 5414738) and Japanese Patent No. 6470455. The entire disclosures of these publications are incorporated herein by reference.

[0018] The thickness of the polarizer is preferably 1 μm to 30 μm, more preferably 1 μm to 25 μm, even more preferably 1 μm to 15 μm, still more preferably 1 μm to 10 μm, particularly preferably 1 μm to 8 μm, and most preferably 2 μm to 5 μm. When the thickness of the polarizer is within the above range, the retardation layer-attached polarizing plate can be made thinner.

[0019] The polarizer preferably exhibits absorption dichroism at any wavelength of 380 nm to 780 nm. The single transmittance Ts of the polarizer is preferably 40% to 48%, more preferably 41% to 46%. The degree of polarization P of the polarizer is preferably 97.0% or more, more preferably 99.0% or more, and even more preferably 99.9% or more. The single transmittance is typically a Y value measured using an ultraviolet-visible spectrophotometer and subjected to luminosity correction. The degree of polarization is typically calculated by the following formula based on the parallel transmittance Tp and crossed transmittance Tc measured using an ultraviolet-visible spectrophotometer and subjected to luminosity correction. Degree of polarization (%)={(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100

[0020] B-2.Protective layer The protective layers 12 and 13 are formed of any suitable film that can be used as a protective layer for a polarizer. Specific examples of materials that are the main components of the films include cellulose-based resins such as triacetyl cellulose (TAC), and transparent resins such as polyesters, polyvinyl alcohols, polycarbonates, polyamides, polyimides, polyethersulfones, polysulfones, polystyrenes, polynorbornenes, polyolefins, (meth)acrylics, and acetates. Other examples include thermosetting resins or ultraviolet-curing resins such as (meth)acrylics, urethanes, (meth)acrylic urethanes, epoxys, and silicones. Other examples include glassy polymers such as siloxane polymers. Polymer films described in JP 2001-343529 A (WO01 / 37007) can also be used. The material for this film may be, for example, a resin composition containing a thermoplastic resin having a substituted or unsubstituted imide group in the side chain, and a thermoplastic resin having a substituted or unsubstituted phenyl group and a nitrile group in the side chain, such as a resin composition containing an alternating copolymer of isobutene and N-methylmaleimide, and an acrylonitrile-styrene copolymer. The polymer film may be, for example, an extrusion molded product of the above resin composition.

[0021] The polarizing plate with a retardation layer is typically placed on the viewing side of an image display device, and the protective layer 12 is typically placed on the viewing side. Therefore, the protective layer 12 may be subjected to surface treatment such as hard coat treatment, anti-reflection treatment, anti-sticking treatment, and anti-glare treatment, as necessary.

[0022] The thickness of the protective layer is preferably 10 μm to 50 μm, and more preferably 10 μm to 30 μm. When a surface treatment is applied, the thickness of the outer protective layer (protective layer 12) includes the thickness of the surface treatment layer.

[0023] C. Retardation layer The retardation layer includes a first retardation layer which is a liquid crystal alignment solidified layer, and a second retardation layer which is a resin film whose refractive index characteristic shows the relationship of nz>nx=ny. If the retardation layer includes a first retardation layer which is a liquid crystal alignment solidified layer, and a second retardation layer which is a resin film whose refractive index characteristic shows the relationship of nz>nx=ny, that is, a positive C plate, a retardation layer-attached polarizing plate which is thin and has excellent bending resistance and viewing angle characteristics can be provided. As described above, the retardation layer only needs to include a first retardation layer and a second retardation layer, and may be laminated in the order of a polarizing plate, a first retardation layer, a first adhesive layer, and a second retardation layer, or may be laminated in the order of a polarizing plate, a second retardation layer, a first adhesive layer, and a first retardation layer. In one embodiment, the first retardation layer may be a laminate of a liquid crystal alignment solidified layer A and a liquid crystal alignment solidified layer B. In this embodiment, the second retardation layer may be disposed between the liquid crystal alignment solidified layer A and the liquid crystal alignment solidified layer B. For example, the polarizing plate, the liquid crystal alignment solidified layer A, the second retardation layer, and the liquid crystal alignment solidified layer B may be laminated in this order. Preferably, the liquid crystal alignment solidified layer may be disposed on the viewing side of the retardation layer-attached polarizing plate. If the liquid crystal alignment solidified layer is on the viewing side, the viewing angle characteristics may be further improved.

[0024] C-1. First retardation layer The first retardation layer is a liquid crystal alignment solidified layer. The first retardation layer can function as a λ / 4 plate. The first retardation layer may be a single layer or a laminate of two or more layers. The first retardation layer may further include an alignment layer and / or a substrate.

[0025] C-1-1. First retardation layer which is a single layer In one embodiment, the first retardation layer is a single layer. The first retardation layer preferably has Re(550) of 100 nm to 190 nm, Re(450) / Re(550) of the retardation layer is <1, and the angle between the slow axis of the first retardation layer and the absorption axis of the polarizer is 40° to 50°. The in-plane retardation Re(550) of the first retardation layer is preferably 100 nm to 190 nm, more preferably 110 nm to 170 nm, and further preferably 130 nm to 160 nm.

[0026] In this embodiment, the Nz coefficient of the first retardation layer is preferably 0.9 to 1.5, and more preferably 0.9 to 1.3. By satisfying such a relationship, when the obtained retardation layer-attached polarizing plate is used in an image display device, a very excellent reflection hue can be achieved.

[0027] The thickness of the first retardation layer is preferably 10 μm or less, more preferably 0.5 μm to 10 μm, further preferably 0.5 μm to 7 μm, and particularly preferably 1 μm to 5 μm.

[0028] The first retardation layer preferably exhibits inverse dispersion wavelength characteristics. In this case, Re(550) / Re(650) is preferably greater than 1, more preferably greater than 1 and less than 1.2, and even more preferably 1.01 to 1.15. The first retardation layer preferably has Re(450) / Re(550) less than 1, more preferably 0.8 or more and less than 1, and even more preferably 0.8 or more and 0.95 or less. With this configuration, it is possible to realize very excellent antireflection characteristics.

[0029] In this embodiment, the angle between the slow axis of the first retardation layer and the absorption axis of the polarizer is preferably 40° to 50°, more preferably 42° to 48°, and even more preferably about 45°. If the angle is in this range, by using a λ / 4 plate as the first retardation layer, a retardation layer-attached polarizing plate having very excellent circular polarization properties (resulting in very excellent antireflection properties) can be obtained.

[0030] As described above, the first retardation layer is preferably an alignment solidified layer of a liquid crystal compound. By using a liquid crystal compound, the difference between nx and ny of the obtained retardation layer can be significantly increased compared to non-liquid crystal materials, so the thickness of the retardation layer for obtaining a desired in-plane retardation can be significantly reduced. As a result, the retardation layer-attached polarizing plate can be further thinned.

[0031] The retardation layer, which is an alignment solidification layer of a liquid crystal compound, can be formed using a composition containing a polymerizable liquid crystal compound. In this specification, the polymerizable liquid crystal compound contained in the composition refers to a compound having a polymerizable group and having liquid crystal properties. The polymerizable group means a group involved in a polymerization reaction, and is preferably a photopolymerizable group. Here, the photopolymerizable group refers to a group that can be involved in a polymerization reaction by an active radical or an acid generated from a photopolymerization initiator.

[0032] The liquid crystallinity may be expressed as thermotropic or lyotropic. The liquid crystal phase may be structured as nematic liquid crystal or smectic liquid crystal. From the viewpoint of ease of production, the liquid crystallinity is preferably thermotropic nematic liquid crystal.

[0033] C-1-2. First retardation layer as a laminate In one embodiment, the first retardation layer is a laminate of a liquid crystal compound alignment solidified layer A and a liquid crystal alignment solidified layer B. In this embodiment, for example, either the liquid crystal alignment solidified layer A or the liquid crystal alignment solidified layer B may function as a λ / 4 plate, and the other may function as a λ / 2 plate. For example, when the liquid crystal alignment solidified layer A functions as a λ / 2 plate and the liquid crystal alignment solidified layer B functions as a λ / 4 plate, the Re(550) of the liquid crystal alignment solidified layer A is preferably 200 nm to 300 nm, more preferably 230 nm to 290 nm, even more preferably 240 nm to 280 nm, and particularly preferably 250 nm to 270 nm; the Re(550) of the liquid crystal alignment solidified layer B is preferably 100 nm to 200 nm, more preferably 105 nm to 180 nm, even more preferably 110 nm to 160 nm, and particularly preferably 115 nm to 140 nm. The angle between the slow axis of the liquid crystal alignment solidified layer A and the absorption axis of the polarizer is preferably 10° to 25°, more preferably 14° to 20°. The angle between the slow axis of the liquid crystal alignment solidified layer B and the absorption axis of the polarizer is preferably 70° to 85°, more preferably 75° to 81°.

[0034] The thickness of the liquid crystal alignment solidified layer A can be adjusted so that the desired in-plane retardation of the λ / 2 plate is obtained; the thickness of the liquid crystal alignment solidified layer B can be adjusted so that the desired in-plane retardation of the λ / 4 plate is obtained. Preferably, the total thickness of the liquid crystal alignment solidified layer A and the liquid crystal alignment solidified layer B (i.e., the thickness of the first retardation layer, which is a laminate) is 10 μm or less. The thickness of the liquid crystal alignment solidified layer A can be, for example, 2 μm to 3 μm; the thickness of the liquid crystal alignment solidified layer B can be, for example, 1 μm to 2 μm. By using a liquid crystal compound, the difference between nx and ny of the obtained retardation layer can be significantly increased compared to non-liquid crystal materials, so that the thickness of the retardation layer for obtaining a desired in-plane retardation can be significantly reduced. Note that the case where the liquid crystal alignment solidified layer A functions as a λ / 2 plate and the liquid crystal alignment solidified layer B functions as a λ / 4 plate has been described, but the liquid crystal alignment solidified layer A may be a λ / 4 plate and the liquid crystal alignment solidified layer B may be a λ / 2 plate. Alternatively, the angle between the slow axis of the liquid crystal alignment solidified layer A and the absorption axis of the polarizer may be 75° to 81°, and the angle between the slow axis of the liquid crystal alignment solidified layer B and the absorption axis of the polarizer may be 14° to 20°.

[0035] When the retardation layer is a liquid crystal alignment solidified layer, in this embodiment, typically, rod-shaped liquid crystal compounds are aligned in the slow axis direction of the retardation layer (homogeneous alignment).Specific examples of liquid crystal compounds and details of the method for forming the liquid crystal alignment solidified layer are described in, for example, JP-A-2006-163343 and JP-A-2006-178389.The descriptions in these publications are incorporated herein by reference.

[0036] C-2. Second retardation layer The second retardation layer is a resin film that is a so-called positive C plate whose refractive index characteristics show the relationship nz>nx=ny. If the second retardation layer is a positive C plate, it is possible to effectively prevent reflection in an oblique direction, and the anti-reflection function can be made to have a wide viewing angle. The thickness direction retardation Rth(550) of the second retardation layer is preferably -20nm to -300nm, more preferably -30nm to -250nm, further preferably -40nm to -200nm, and particularly preferably -50nm to -150nm. Here, "nx=ny" includes not only the case where nx and ny are strictly equal, but also the case where nx and ny are substantially equal. That is, the in-plane retardation Re(550) of the second retardation layer can be less than 10nm.

[0037] The second retardation layer preferably has a puncture elastic modulus of 50 g / mm or more, more preferably 52 g / mm or more, and even more preferably 55 g / mm or more. The puncture elastic modulus of the second retardation layer is, for example, 200 g / mm or less. If the puncture elastic modulus of the second retardation layer is within the above range, the bending resistance of the retardation layer-attached polarizing plate can be further improved. In this specification, the puncture elastic modulus refers to a value obtained by dividing the force (g) just before the retardation film breaks (or tears) when a needle (puncture tool) is pierced perpendicularly to the main surface of the retardation film (the second retardation layer) by the strain (mm) at that time. As the needle, one with a tip diameter of 1 mmφ and 0.5R can be used. The needle piercing speed can be 0.33 cm / sec. The puncture elastic modulus is measured by sandwiching the retardation film between two plates with a circular hole with a diameter of 15 mm or less through which the needle can pass. The puncture modulus can be measured in an environment at a temperature of 23°C. For example, the puncture modulus of five retardation films can be measured, and the average value can be used as the puncture modulus of the retardation film. Commercially available devices can be used to measure the puncture modulus. Examples of commercially available devices include a handy compression tester "KES-G5 Needle Penetration Force Measurement Specification" manufactured by Kato Tech Co., Ltd. and a small tabletop tester "EZ Test" manufactured by Shimadzu Corporation.

[0038] The thickness of the second retardation layer can be set to any appropriate thickness. The thickness of the second retardation layer is preferably 10 μm or less, more preferably 2 μm to 10 μm, and further preferably 2 μm to 7 μm. If the thickness of the second retardation layer is within the above range, it can contribute to making the retardation layer-attached polarizing plate thinner.

[0039] The second retardation layer is a resin film made of any suitable resin. It is preferably made of a resin film containing a polymer exhibiting negative birefringence. Here, "exhibiting negative birefringence" means that when a polymer is oriented by stretching or the like, the refractive index in the stretching direction becomes relatively small. In other words, it means that the refractive index in the direction perpendicular to the stretching direction becomes large. If it is made of a resin film containing a polymer exhibiting negative birefringence, a retardation layer-attached polarizing plate with even better bending resistance can be provided.

[0040] Examples of polymers that exhibit negative birefringence include polymers in which a chemical bond or functional group with large polarization anisotropy, such as an aromatic ring and / or a carbonyl group, is introduced into the side chain. Specific examples include acrylic resins, styrene resins, and maleimide resins. Only one type of polymer exhibiting negative birefringence may be used, or two or more types may be used in combination.

[0041] The acrylic resin can be obtained, for example, by addition polymerization of an acrylate monomer. Examples of the acrylic resin include polymethyl methacrylate (PMMA), polybutyl methacrylate, and polycyclohexyl methacrylate.

[0042] The styrene resin can be obtained, for example, by addition polymerization of a styrene monomer, such as styrene, α-methylstyrene, o-methylstyrene, p-methylstyrene, p-chlorostyrene, p-nitrostyrene, p-aminostyrene, p-carboxystyrene, p-phenylstyrene, 2,5-dichlorostyrene, and pt-butylstyrene.

[0043] The maleimide resin can be obtained, for example, by addition polymerization of a maleimide monomer. Examples of maleimide monomers include N-ethylmaleimide, N-cyclohexylmaleimide, N-phenylmaleimide, N-(2-methylphenyl)maleimide, N-(2-ethylphenyl)maleimide, N-(2-propylphenyl)maleimide, N-(2-isopropylphenyl)maleimide, N-(2,6-dimethylphenyl)maleimide, N-(2,6-dipropylphenyl)maleimide, N-(2,6-diisopropylphenyl)maleimide, N-(2-methyl-6-ethylphenyl)maleimide, N-(2-chlorophenyl)maleimide, N-(2,6-dichlorophenyl)maleimide, N-(2-bromophenyl)maleimide, N-(2,6-dibromophenyl)maleimide, N-(2-biphenyl)maleimide, and N-(2-cyanophenyl)maleimide. The maleimide monomer can be obtained, for example, from Tokyo Chemical Industry Co., Ltd.

[0044] In addition polymerization, the birefringence characteristics of the resulting resin can also be controlled by substituting side chains after polymerization, or by carrying out maleimidization or grafting reactions.

[0045] The polymer exhibiting negative birefringence may be copolymerized with other monomers. By copolymerizing other monomers, brittleness, moldability, and heat resistance can be improved. Examples of the other monomers include olefins such as ethylene, propylene, 1-butene, 1,3-butadiene, 2-methyl-1-butene, 2-methyl-1-pentene, and 1-hexene; acrylonitrile; (meth)acrylates such as methyl acrylate and methyl methacrylate; maleic anhydride; and vinyl esters such as vinyl acetate.

[0046] When the polymer exhibiting negative birefringence is a copolymer of the styrene monomer and the other monomer, the blending ratio of the styrene monomer is preferably 50 mol% to 80 mol%. When the polymer exhibiting negative birefringence is a copolymer of the maleimide monomer and the other monomer, the blending ratio of the maleimide monomer is preferably 2 mol% to 50 mol%. By blending in such a range, a resin film excellent in toughness and moldability can be obtained.

[0047] As the polymer exhibiting negative birefringence, preferably, styrene-maleic anhydride copolymer, styrene-acrylonitrile copolymer, styrene-(meth)acrylate copolymer, styrene-maleimide copolymer, vinyl ester-maleimide copolymer, olefin-maleimide copolymer, etc. are used. These may be used alone or in combination of two or more. These polymers exhibit high negative birefringence and may have excellent heat resistance. These polymers are available, for example, from Nova Chemical Japan, Arakawa Chemical Industries, Ltd., etc.

[0048] As the polymer exhibiting negative birefringence, a polymer having a repeating unit represented by the following general formula (I) is preferably used. Such a polymer exhibits a higher negative birefringence and can have excellent heat resistance and mechanical strength. Such a polymer can be obtained, for example, by using an N-phenyl-substituted maleimide in which a phenyl group having a substituent at least at the ortho position is introduced as the N-substituent of the maleimide monomer as the starting material. [ka]

[0049] In the above general formula (I), R 1 ~R 5 each independently represents a hydrogen atom, a halogen atom, a carboxylic acid, a carboxylate, a hydroxyl group, a nitro group, or a linear or branched alkyl or alkoxy group having 1 to 8 carbon atoms (provided that R 1 and R5 is not a hydrogen atom at the same time), R 6 and R 7 represents a hydrogen atom or a linear or branched alkyl or alkoxy group having 1 to 8 carbon atoms, and n represents an integer of 2 or more.

[0050] The polymer exhibiting negative birefringence is not limited to the above, and for example, a cyclic olefin copolymer as disclosed in JP-A-2005-350544 can be used. Furthermore, a composition containing a polymer and inorganic fine particles as disclosed in JP-A-2005-156862, JP-A-2005-227427, etc. can also be suitably used. Furthermore, these can be modified by copolymerization, branching, crosslinking, molecular end modification (or sealing), stereoregular modification, etc. before use. The descriptions in these publications can be incorporated herein by reference.

[0051] The second retardation layer can be obtained by molding a resin composition further containing a polymer exhibiting negative birefringence and any suitable additive. Specific examples of the additive include a plasticizer, a heat stabilizer, a light stabilizer, a lubricant, an antioxidant, an ultraviolet absorber, a flame retardant, a colorant, an antistatic agent, a compatibilizer, a crosslinking agent, and a thickener. The type and content of the additive can be appropriately set according to the purpose. The content of the additive is typically about 3 parts by weight to 10 parts by weight with respect to 100 parts by weight of the total solid content of the resin composition. If the content of the additive is excessively large, the transparency of the polymer film may be impaired or the additive may bleed out from the surface of the polymer film.

[0052] Any suitable molding method can be adopted as the molding method of the second retardation layer. For example, compression molding, transfer molding, injection molding, extrusion molding, blow molding, powder molding, FRP molding, solvent casting, etc. can be mentioned. Among these, extrusion molding and solvent casting are preferably used. This is because a retardation film having high smoothness and good optical uniformity can be obtained. Specifically, the extrusion molding method is a method in which a resin composition containing the above-mentioned thermoplastic resin, plasticizer, additives, etc. is heated and melted, and this is extruded into a thin film on the surface of a casting roll by a T-die or the like, and cooled to form a film. The solvent casting method is a method in which a concentrated solution (dope) in which the above-mentioned resin composition is dissolved in a solvent is degassed, and cast into a thin film uniformly on the surface of a metallic endless belt or a rotating drum, or a plastic substrate, etc., and the solvent is evaporated to form a film. The molding conditions can be appropriately set according to the composition and type of the resin used, the molding method, etc.

[0053] D. First Adhesive Layer The first retardation layer and the second retardation layer may be laminated via a first adhesive layer. As described above, in one embodiment, the second retardation layer may be disposed between the liquid crystal alignment solidified layer A and the liquid crystal alignment solidified layer B. In this embodiment, the liquid crystal alignment solidified layer A and the second retardation layer may be laminated via a first adhesive layer, the liquid crystal alignment solidified layer B and the second retardation layer may be laminated via a first adhesive layer, and both the liquid crystal alignment solidified layer A and the second retardation layer, and the liquid crystal alignment solidified layer B and the second retardation layer may be laminated via a first adhesive layer. The first adhesive layer may be an adhesive layer or a pressure-sensitive adhesive layer. The thickness of the first adhesive layer is preferably 7 μm or less, more preferably 5 μm or less. The thickness of the first adhesive layer is, for example, 0.5 μm or more. If the thickness of the first adhesive layer is within the above range, the first retardation layer and the second retardation layer can be sufficiently adhered to each other, which may contribute to a thinner film. When the adhesive layer is an adhesive layer, any suitable adhesive can be used. For example, an ultraviolet-curing adhesive can be used. When the adhesive layer is an adhesive layer, any suitable adhesive can be used. Specific examples of adhesives include acrylic adhesives, rubber adhesives, silicone adhesives, polyester adhesives, urethane adhesives, epoxy adhesives, and polyether adhesives. By adjusting the type, number, combination, and compounding ratio of monomers forming the base resin of the adhesive, as well as the compounding amount of the crosslinking agent, reaction temperature, reaction time, etc., an adhesive having desired properties according to the purpose can be prepared. The base resin of the adhesive may be used alone or in combination of two or more. From the viewpoints of transparency, processability, durability, etc., an acrylic adhesive (acrylic adhesive composition) is preferred.

[0054] The acrylic adhesive may preferably contain a silane coupling agent and / or a crosslinking agent. Examples of the silane coupling agent include an epoxy group-containing silane coupling agent. Examples of the crosslinking agent include an isocyanate-based crosslinking agent and a peroxide-based crosslinking agent. Furthermore, the acrylic adhesive composition may contain an antioxidant and / or a conductive agent. Details of the adhesive layer or the acrylic adhesive composition are described in, for example, JP 2006-183022 A, JP 2015-199942 A, JP 2018-053114 A, JP 2016-190996 A, and WO 2018 / 008712 A, and the descriptions in these publications are incorporated herein by reference.

[0055] E. Adhesive layer Any suitable adhesive can be used as the adhesive constituting the adhesive layer (adhesive layer between the retardation layer-attached polarizing plate and the image display device) provided as the outermost layer. Examples of the adhesive include rubber-based adhesives, acrylic-based adhesives, silicone-based adhesives, urethane-based adhesives, vinyl alkyl ether-based adhesives, polyvinyl alcohol-based adhesives, polyvinyl pyrrolidone-based adhesives, polyacrylamide-based adhesives, and cellulose-based adhesives. Among these adhesives, those that are excellent in optical transparency, exhibit adhesive properties such as appropriate wettability, cohesion, and adhesion, and are excellent in weather resistance and heat resistance are preferably used. Acrylic-based adhesives are preferably used as those that exhibit such characteristics. In addition, the adhesives exemplified in the above section D may be used as the adhesive.

[0056] The pressure-sensitive adhesive layer has a storage modulus of preferably 200 kPa or less, more preferably 10 kPa to 150 kPa, and even more preferably 10 kPa to 50 kPa at 23° C. If the pressure-sensitive adhesive layer has a storage modulus of within the above range at 23° C., a retardation layer-attached polarizing plate that is thin and has excellent bending resistance can be provided. The storage modulus at 23° C. can be measured by a dynamic viscoelasticity measuring device.

[0057] F. Image display device The retardation layer-attached polarizing plate described in the above items A to E can be applied to an image display device. Therefore, the embodiment of the present invention includes an image display device using such a retardation layer-attached polarizing plate. Representative examples of image display devices include liquid crystal display devices and electroluminescence (EL) display devices (e.g., organic EL display devices, inorganic EL display devices). The image display device according to the embodiment of the present invention includes the retardation layer-attached polarizing plate described in the above items A to E on the viewing side. The retardation layer-attached polarizing plate is laminated so that the retardation layer is on the image display cell (e.g., liquid crystal cell, organic EL cell, inorganic EL cell) side (so that the polarizer is on the viewing side). EXAMPLES

[0058] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring each property are as follows. In the examples and comparative examples, "parts" and "%" are by weight unless otherwise specified.

[0059] (1) Thickness The thickness of 10 μm or less was measured using an interference film thickness meter (manufactured by Otsuka Electronics, product name "MCPD-3000"), and the thickness of more than 10 μm was measured using a digital micrometer (manufactured by Anritsu, product name "KC-351C").

[0060] (2) Puncture elastic modulus The puncture modulus of elasticity was measured for the retardation layer obtained in Production Example 4. A needle was attached to a handy compression tester (product name: KES-G5 needle penetration force measurement specification) manufactured by Kato Tech Co., Ltd. The needle was pierced vertically into the main surface of the retardation layer fixed between two plates with a circular hole of 11 mm in diameter, and the force (g) just before the layer broke was divided by the strain (mm) at that time to calculate the value. This operation was performed for each of the five retardation layers (samples for puncture test), and the average value was taken as the puncture modulus of elasticity of the retardation layer. The needle used had a tip diameter of 1 mmφ and 0.5R. The needle was pierced at a speed of 0.33 cm / sec.

[0061] (3) Reflection brightness and reflection hue The retardation layer-attached polarizing plates obtained in the examples and comparative examples were measured using a display measurement system (Konica Minolta, product name "DMS505") * a * b * Reflection luminance in color space L * Value and hue a * value, and b * The value was obtained. In this case, the surface of the retardation layer-attached polarizing plate is the X-axis and the Y-axis, and the axis perpendicular to the XY plane is the Z-axis. The angle tilted from the Z-axis to the XY plane direction is the polar angle (θ), the MD direction of the polarizing plate used in the retardation layer-attached polarizing plate is set to 0°, and the measurement angle defined between the MD direction of this polarizing plate and the counterclockwise direction is the azimuth angle (φ). Figure 3 shows the L of the retardation layer-attached polarizing plate of the embodiment and the comparative example of the present invention. * a * b * The results are shown in the measurement of reflected luminance and reflected hue based on a color space chromaticity diagram. For each example and comparative example, the average value Y (Ave) of the reflected luminance measured at a polar angle θ of 50° was calculated. If Y (Ave) is 0.8 or less, the viewing angle characteristics are excellent. In addition, the difference ΔY between the maximum and minimum values ​​of the luminance measured at a polar angle θ of 50° was calculated. If ΔY is 0.25 or less, the viewing angle characteristics are excellent. * value and b * From the value, Δa * b * The maximum value of Δa was calculated. * b * If the value is 9.0 or less, the viewing angle characteristics are excellent. * a * b * In a color space chromaticity diagram, these represent the azimuth angles of the points at which hues are furthest apart at a polar angle of 50°, and are values ​​that are multiples of 15 within the range of 0° to 345°. Δa * b * =√(a * A- a * B ) 2 +(b * A-b * B ) 2

[0062] (4) Flexibility The polarizing plate with retardation layer obtained in the examples and comparative examples was attached to a resin film (manufactured by Toyo Kohan Co., Ltd., product name: RV-20UB) having a thickness of 20 μm, and cut into a size of 10 cm × 5 cm so that the angle between the absorption axis of the polarizer and the long side was 135°, and used as a measurement sample. This measurement sample was subjected to a continuous bending test using a bending tester (manufactured by Yuasa System Co., Ltd., product name "CL09 Type D01"). FIG. 4 is a schematic diagram for explaining a method of fixing a sample during a bending test in an example of the present invention. As shown in FIG. 4, the measurement sample was fixed with double-sided tape so that the resin film side of the measurement sample and the fixed part of the bending tester were in contact with each other, and then the measurement was performed. The bending was performed at 25° C. (room temperature) with the viewing side protective layer facing inward. The bending radius of curvature was 1.5 mm, and the bending speed was 30 times / min. The presence or absence of cracks after bending the sample 10,000 times, 30,000 times, and 50,000 times was visually observed. If there were zero or fewer cracks, the sample was rated as ◯ (good), and if there were one or more cracks, the sample was rated as × (bad).

[0063] [Production Example 1: Preparation of polarizing plate] 1. Preparation of Polarizer A polyvinyl alcohol film having an average polymerization degree of 2,400, a saponification degree of 99.9 mol%, and a thickness of 45 μm was prepared. The polyvinyl alcohol film was stretched 2.2 times in the conveying direction while swelling by immersing in a swelling bath (water bath) at 20 ° C. between rolls with different peripheral speed ratios (swelling step), and then stretched 3.3 times in the conveying direction based on the original polyvinyl alcohol film (polyvinyl alcohol film not stretched at all in the conveying direction) while dyeing by immersing in a dyeing bath (aqueous solution with an iodine concentration of 0.1 wt % and a potassium iodide concentration of 0.9 wt %) at 30 ° C. (dyeing step). Next, the dyed polyvinyl alcohol film was immersed in a crosslinking bath (aqueous solution with a boric acid concentration of 3.0 wt % and a potassium iodide concentration of 3.0 wt %) at 40 ° C. for 28 seconds to stretch 3.6 times in the conveying direction based on the original polyvinyl alcohol film (crosslinking step). The obtained polyvinyl alcohol film was then immersed in a 61°C stretching bath (aqueous solution with a boric acid concentration of 4.0% by weight and a potassium iodide concentration of 5.0% by weight) for 60 seconds to stretch the film to 6.0 times the original polyvinyl alcohol film in the conveying direction (stretching step), and then immersed in a 20°C washing bath (aqueous solution with a potassium iodide concentration of 2.0% by weight) for 10 seconds (washing step). The washed polyvinyl alcohol film was dried at 40°C for 30 seconds to produce a polarizer. The polarizer had a thickness of 18 μm.

[0064] 2. Preparation of Polarizing Plates As the adhesive, an aqueous solution containing a polyvinyl alcohol resin containing an acetoacetyl group (average polymerization degree 1,200, saponification degree 98.5 mol%, acetoacetylation degree 5 mol%) and methylolmelamine in a weight ratio of 3:1 was used. Using this adhesive, a 30 μm thick transparent protective film (manufactured by Nippon Shokubai) made of a (meth)acrylic resin (modified acrylic polymer having a lactone ring structure) was laminated as a protective layer on one side (display element side) of the polarizer obtained above, and a 49 μm thick transparent protective film made of a triacetyl cellulose film (manufactured by Fuji Film, product name "TJ40UL") with HC was laminated as a protective layer on the other side (viewing side) using a roll laminator, and then heated and dried in an oven (temperature 90°C, time 10 minutes) to produce a polarizing plate in which the transparent protective film was laminated on both sides of the polarizer. The single transmittance of the obtained polarizer was 41.7%, and the polarization degree was 99.9%.

[0065] [Production Example 2: First Retardation Layer 1] 55 parts by weight of the compound represented by formula (I), 25 parts by weight of the compound represented by formula (II), and 20 parts by weight of the compound represented by formula (III) were added to 400 parts by weight of cyclopentanone (CPN), and then heated to 60°C and stirred to dissolve. Then, the solution of the above-mentioned compound was returned to room temperature, and 3 parts by weight of Irgacure 907 (manufactured by BASF Japan Ltd.), 0.2 parts by weight of Megafac F-554 (manufactured by DIC Corporation), and 0.1 parts by weight of p-methoxyphenol (MEHQ) were added to the solution of the above-mentioned compound, and further stirred. The solution after stirring was transparent and uniform. The obtained solution was filtered through a 0.20 μm membrane filter to obtain a polymerizable composition. Also, a polyimide solution for an alignment film was applied to a glass substrate having a thickness of 0.7 mm by spin coating, and a coating film was obtained by drying at 100° C. for 10 minutes and then baking at 200° C. for 60 minutes. The obtained coating film was subjected to a rubbing treatment using a commercially available rubbing device to form an alignment film. Next, the polymerizable composition obtained above was applied to the substrate (substantially the alignment film) by spin coating, and dried at 100° C. for 2 minutes. After the obtained coating film was cooled to room temperature, it was heated with a high-pressure mercury lamp at 30 mW / cm2 The film was irradiated with ultraviolet light at an intensity of 100 nm for 30 seconds to obtain a retardation layer (thickness 2.7 μm) which is an alignment solidified layer of the liquid crystal compound. The in-plane retardation Re(550) of the retardation layer was 149 nm. The retardation layer also had a Re(450) / Re(550) of 0.851, which showed reverse dispersion wavelength characteristics. The retardation layer can function as a λ / 4 plate. [ka] [ka]

[0066] [Production Example 3: Preparation of the first retardation layer 2] A liquid crystal composition (coating liquid) was prepared by dissolving 10 g of a polymerizable liquid crystal exhibiting a nematic liquid crystal phase (manufactured by BASF: product name "Paliocolor LC242", represented by the following formula) and 3 g of a photopolymerization initiator for the polymerizable liquid crystal compound (manufactured by BASF: product name "Irgacure 907") in 40 g of toluene. [ka] The surface of a PET film (thickness 38 μm) was rubbed with a rubbing cloth and subjected to an alignment treatment. The direction of the alignment treatment was set to be 15° from the viewing side with respect to the direction of the absorption axis of the polarizer when it was attached to the polarizing plate. The above liquid crystal coating liquid was applied to this alignment-treated surface with a bar coater, and the liquid crystal compound was aligned by heating and drying at 90° C. for 2 minutes. The liquid crystal layer thus formed was then irradiated with 100 mJ / cm 2 using a metal halide lamp. 2 The liquid crystal layer was cured by irradiating the liquid crystal with light, thereby forming a liquid crystal alignment solidified layer A on the PET film. The liquid crystal alignment solidified layer A had a thickness of 2.2 μm and an in-plane retardation Re(550) of 245 nm. Furthermore, the liquid crystal alignment solidified layer A had a refractive index distribution of nx>ny=nz. A liquid crystal alignment layer B was formed on a PET film in the same manner as above, except that the coating thickness was changed and the alignment treatment direction was set to a 75° direction relative to the absorption axis direction of the polarizer when viewed from the viewing side. The liquid crystal alignment layer B had a thickness of 1.1 μm and an in-plane retardation Re(550) of 120 nm. Furthermore, the liquid crystal alignment layer B had a refractive index distribution of nx>ny=nz.

[0067] [Production Example 4: Preparation of second retardation layer 1] In an autoclave equipped with a stirrer, a cooling tube, a nitrogen inlet tube, and a thermometer, 48 parts by weight of hydroxypropyl methylcellulose (manufactured by Shin-Etsu Chemical, trade name: Metolose 60SH-50), 15601 parts by weight of distilled water, 8161 parts by weight of diisopropyl fumarate, 240 parts by weight of 3-ethyl-3-oxetanylmethyl acrylate, and 45 parts by weight of t-butyl peroxypivalate, a polymerization initiator, were placed, and after nitrogen bubbling for 1 hour, the mixture was kept at 49°C for 24 hours while stirring to carry out radical suspension polymerization. The mixture was then cooled to room temperature, and the suspension containing the produced polymer particles was centrifuged. The obtained polymer was washed twice with distilled water and twice with methanol, and then dried under reduced pressure. The obtained fumarate ester resin was dissolved in a toluene-methyl ethyl ketone mixed solution (toluene / methyl ethyl ketone, 50% by weight / 50% by weight) to prepare a 20% solution. Furthermore, 5 parts by weight of tributyl trimellitate was added as a plasticizer to 100 parts by weight of the fumaric acid ester resin to prepare a dope. A biaxially stretched film (thickness 75 μm) of polyester (polyethylene-terephthalate / isophthalate copolymer) was used as the support film. The prepared dope was applied to the support film so that the film thickness after drying was 5 μm, and dried at 140° C. The coating film (positive C plate) after drying had an in-plane retardation Re(550)≒0 nm and Rth(550)=-75 nm. The puncture modulus T of the obtained retardation film was 57.2 g / mm.

[0068] [Production Example 5: Preparation of Adhesive 1] A monomer mixture containing 91.5 parts by weight of butyl acrylate, 3 parts by weight of acrylic acid, 0.5 parts by weight of 4-hydroxybutyl acrylate, and 5 parts by weight of acryloylmorpholine was charged into a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser. Next, 0.1 parts by weight of 2,2'-azobisisobutyronitrile as a polymerization initiator was charged together with 100 parts by weight of ethyl acetate for 100 parts by weight of this monomer mixture, and nitrogen gas was introduced while gently stirring to replace the atmosphere with nitrogen. The liquid temperature in the flask was kept at about 55°C, and a polymerization reaction was carried out for 8 hours to prepare a solution of an acrylic polymer with a weight average molecular weight (Mw) of 2.5 million. Per 100 parts by weight of the solid content of the obtained acrylic polymer solution, 0.2 parts by weight of an isocyanate crosslinking agent (Coronate L, manufactured by Nippon Polyurethane Industry Co., Ltd., an adduct of trimethylolpropane and tolylene diisocyanate), 0.3 parts by weight of benzoyl peroxide (Niper BMT, manufactured by Nippon Oil & Fats Co., Ltd.), and 0.1 parts by weight of a silane coupling agent (product name: KBM403, manufactured by Shin-Etsu Chemical Co., Ltd.) were mixed to prepare a solution of an acrylic adhesive composition (solid content 11%) (adhesive 1).

[0069] [Production Example 6: Preparation of Adhesive 2] A monomer mixture containing 99 parts by weight of butyl acrylate (BA) and 1 part by weight of 4-hydroxybutyl acrylate (HBA) was charged into a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a cooler. Furthermore, 0.1 parts by weight of 2,2'-azobisisobutyronitrile as a polymerization initiator was charged together with ethyl acetate for 100 parts by weight of the monomer mixture (solid content), and nitrogen gas was introduced while gently stirring to replace the atmosphere with nitrogen. The liquid temperature in the flask was kept at about 55°C and a polymerization reaction was carried out for 7 hours. Ethyl acetate was then added to the resulting reaction liquid to prepare a solution of a (meth)acrylic polymer with a weight average molecular weight of 1.6 million, with a solid content concentration of 30%. An acrylic adhesive composition (adhesive 2) was prepared by blending 100 parts by weight of the solid content of the obtained (meth)acrylic polymer solution with 0.1 part by weight of an isocyanate crosslinking agent (product name: Takenate D110N, trimethylolpropane xylylene diisocyanate, manufactured by Mitsui Chemicals, Inc.), 0.3 part by weight of a peroxide crosslinking agent, benzoyl peroxide (product name: Niper BMT, manufactured by Nippon Oil & Fats Co., Ltd.), and 0.1 part by weight of a silane coupling agent (product name: KBM403, manufactured by Shin-Etsu Chemical Co., Ltd.).

[0070] [Example 1] The first retardation layer obtained in Production Example 2 was attached to the protective layer made of the (meth)acrylic resin film of the polarizing plate obtained in Production Example 1 via an acrylic adhesive (thickness 15 μm). At this time, the absorption axis of the polarizer and the slow axis of the first retardation film were attached so as to form an angle of 45°. Next, the first retardation layer and the second retardation layer obtained in Production Example 4 were laminated via an adhesive layer (thickness of adhesive layer 5 μm) formed using adhesive 1, and a retardation layer-attached polarizing plate (thickness: 80 μm) having a configuration of protective layer (HC layer / TAC film) / adhesive layer / polarizer / adhesive layer / protective layer (transparent protective film made of (meth)acrylic resin) / acrylic adhesive layer / first retardation layer / first adhesive layer (adhesive layer formed using adhesive 1) / second retardation layer was obtained. Thereafter, the adhesive 2 was applied to the surface of the second retardation layer not in contact with the first retardation layer to form an adhesive layer (thickness 15 μm), and a retardation layer-attached polarizing plate having an adhesive layer was obtained. The obtained retardation layer-attached polarizing plate was subjected to the above-mentioned evaluation. The results are shown in Table 1.

[0071] [Example 2] The liquid crystal alignment solidified layer A and the liquid crystal alignment solidified layer B obtained in Manufacturing Example 3 were transferred (laminated) in this order so that the angle between the absorption axis of the polarizer and the slow axis of the liquid crystal alignment solidified layer A was 19°, and the angle between the absorption axis of the polarizer and the slow axis of the liquid crystal alignment solidified layer B was 81°. The liquid crystal alignment solidified layer A and the liquid crystal alignment solidified layer B were laminated via an acrylic adhesive (thickness 5 μm). Next, an adhesive layer (thickness 5 μm) formed using adhesive 1 was transferred to the liquid crystal alignment solidified layer B, and the second retardation layer obtained in Manufacturing Example 4 was laminated, to obtain a retardation layer laminate of liquid crystal alignment solidified layer A / adhesive layer / liquid crystal alignment solidified layer B / first adhesive layer (adhesive layer formed using adhesive 1) / second retardation layer. Next, the surface of the liquid crystal alignment solidified layer A side of the retardation layer laminate obtained above was laminated to the protective layer made of the (meth)acrylic resin film of the polarizing plate obtained in Production Example 1 via an acrylic adhesive (thickness 15 μm), and a retardation layer-attached polarizing plate (thickness: 81 μm) having a configuration of protective layer (HC layer / TAC film) / adhesive layer / polarizer / adhesive layer / protective layer (transparent protective film made of (meth)acrylic resin) / acrylic adhesive layer / first retardation layer (liquid crystal alignment solidified layer A / adhesive layer / liquid crystal alignment solidified layer B) / first adhesive layer / second retardation layer was obtained. Then, adhesive 2 was applied to the surface of the second retardation layer that was not in contact with the first retardation layer to form an adhesive layer (thickness 15 μm), and a retardation layer-attached polarizing plate having an adhesive layer was obtained. The obtained retardation layer-attached polarizing plate was subjected to the above evaluation. The results are shown in Table 1.

[0072] [Example 3] The liquid crystal alignment solidified layer A and the liquid crystal alignment solidified layer B obtained in Manufacturing Example 3 were laminated with the second retardation layer and the liquid crystal alignment solidified layer B obtained in Manufacturing Example 4, each via an acrylic adhesive (thickness 5 μm), so that the angle between the absorption axis of the polarizer and the slow axis of the liquid crystal alignment solidified layer A was 19°, and the angle between the absorption axis of the polarizer and the slow axis of the liquid crystal alignment solidified layer B was 81°, thereby obtaining a retardation layer laminate of liquid crystal alignment solidified layer A / adhesive layer / second retardation layer / adhesive layer / liquid crystal alignment solidified layer B. A retardation layer-attached polarizing plate (thickness: 81 μm) having a configuration of protective layer (HC layer / TAC film) / adhesive layer / polarizer / adhesive layer / protective layer (transparent protective film made of (meth)acrylic resin) / acrylic adhesive layer / liquid crystal alignment solidified layer A / adhesive layer / second retardation layer / adhesive layer / liquid crystal alignment solidified layer B was obtained in the same manner as in Example 2, except that this retardation layer laminate was used and a protective layer made of a (meth)acrylic resin film and a liquid crystal alignment solidified layer A of the retardation layer laminate were laminated. Thereafter, adhesive 2 was applied to the surface of the liquid crystal alignment solidified layer B that was not in contact with the second retardation layer to form an adhesive layer (thickness 15 μm), and a retardation layer-attached polarizing plate having an adhesive layer was obtained. The obtained retardation layer-attached polarizing plate was subjected to the above-mentioned evaluation. The results are shown in Table 1.

[0073] Comparative Example 1 A polarizing plate with a retardation layer was obtained in the same manner as in Example 1, except that the second retardation layer was not laminated. The obtained polarizing plate with a retardation layer (thickness: 73 μm) was subjected to the above evaluation. The results are shown in Table 1.

[0074] Comparative Example 2 A polarizing plate with a retardation layer (thickness 70 μm excluding the outermost adhesive layer) was produced in the same manner as in Example 1, except that a film ("MCP-N(100)" manufactured by Dai Nippon Printing Co., Ltd.) having a homeotropic alignment liquid crystal layer (thickness: 3 μm, refractive index characteristics showing the relationship nz>nx=ny) was laminated as the second retardation layer. The results are shown in Table 1.

[0075] Comparative Example 3 A polarizing plate with a retardation layer (thickness excluding the outermost adhesive layer: 73 μm) was obtained in the same manner as in Example 2, except that the second retardation layer was not laminated. The obtained polarizing plate with a retardation layer was subjected to the above-mentioned evaluation. The results are shown in Table 1.

[0076] Comparative Example 4 A polarizing plate with a retardation layer (thickness 76 μm excluding the outermost adhesive layer) was produced in the same manner as in Example 2, except that a film ("MCP-N(100)" manufactured by Dai Nippon Printing Co., Ltd.) having a homeotropic alignment liquid crystal layer (thickness: 3 μm, refractive index characteristics showing the relationship nz>nx=ny) was laminated as the second retardation layer. The results are shown in Table 1.

[0077] [Table 1]

[0078] [evaluation] As is clear from Table 1, the retardation layer-attached polarizing plates of the examples of the present invention were thin and had excellent viewing angle characteristics and bending resistance. [Industrial Applicability]

[0079] The retardation layer-attached polarizing plate according to the embodiment of the present invention can be suitably used in image display devices such as liquid crystal display devices, organic EL display devices, and inorganic EL display devices, and can also be suitably used in vehicle-mounted image display devices. [Explanation of symbols]

[0080] 10 Polarizing plate 11 Polarizer 12 Protective layer 13 Protective layer 20 First retardation layer 30 First adhesive layer 40 Second retardation layer 50 Adhesive layer 100 Polarizing plate with retardation layer

Claims

1. a polarizing plate including a polarizer; a retardation layer including a first retardation layer which is an alignment solidified layer of a liquid crystal compound, and a second retardation layer which is a resin film having a refractive index characteristic that satisfies the relationship nz>nx=ny; and a first adhesive layer disposed between the first retardation layer and the second retardation layer, A polarizing plate with a retardation layer, in which the number of cracks in the second retardation layer is 0 or less in an inward bending test with a bending radius R of 1.5 mm and 50,000 bending cycles.

2. The first retardation layer is a single layer, The in-plane retardation Re(550) is 100 nm to 190 nm and satisfies Re(450) / Re(550)<1; 2. The polarizing plate with a retardation layer according to claim 1, wherein an angle between a slow axis of the first retardation layer and an absorption axis of the polarizer is 40° to 50°.

3. the first retardation layer is a laminate of a liquid crystal compound alignment and solidified layer A and a liquid crystal alignment and solidified layer B, The Re(550) of the alignment / solidified layer A of the liquid crystal compound is 200 nm to 300 nm, and the Re(550) of the alignment / solidified layer B of the liquid crystal compound is 100 nm to 200 nm, the angle between the slow axis of the alignment solidified layer A of the liquid crystal compound and the absorption axis of the polarizer is 14° to 20°; 2. The polarizing plate with a retardation layer according to claim 1, wherein the angle between the slow axis of the aligned and solidified layer B of the liquid crystal compound and the absorption axis of the polarizer is from 75° to 81°.

4. 4. The retardation layer-attached polarizing plate according to claim 3, wherein the alignment and solidification layer A of the liquid crystal compound, the first adhesive layer, the second retardation layer, and the alignment and solidification layer B of the liquid crystal compound are laminated in this order.

5. 2. The polarizing plate with a retardation layer according to claim 1, wherein the first retardation layer has a thickness of 10 μm or less.

6. 2. The polarizing plate with a retardation layer according to claim 1, wherein the second retardation layer has a thickness of 10 μm or less.

7. The polarizing plate with a retardation layer according to claim 1 , wherein the first adhesive layer has a thickness of 7 μm or less.

8. 2. The polarizing plate with a retardation layer according to claim 1, wherein the second retardation layer is made of a resin film containing a polymer exhibiting negative birefringence.

9. 2. The retardation layer-attached polarizing plate according to claim 1, further comprising a pressure-sensitive adhesive layer as an outermost layer, the pressure-sensitive adhesive layer having a storage modulus of 200 kPa or less.

10. An image display device comprising the retardation layer-attached polarizing plate according to claim 1 .

Citation Information

Patent Citations

  • Control device for vehicular headlight, control method for vehicular headlight, and vehicular headlight system

    JP2022014611A

Cited By

  • Optical laminate, method for manufacturing optical film piece, and method for manufacturing display system

    WO2026191554A1