Low reflection laminate, low reflection treatment agent, and method for producing low reflection laminate

The low-reflection laminate with controlled refractive indices and layers addresses the environmental and performance issues of existing technologies by using non-fluorine solvents, achieving low reflectivity, scratch resistance, and abrasion resistance on diverse substrates.

JP2024158203APending Publication Date: 2024-11-08HONNY CHEM
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023073194
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing antireflection and antifouling technologies for displays are costly, environmentally harmful due to the use of fluorine-based solvents, and lack an optimal balance of low reflectivity, scratch resistance, and abrasion resistance, with complex manufacturing processes.

Method used

A low-reflection laminate comprising a base material layer, a first anti-reflection layer made from a cured hydrolyzed condensate oligomer of an epoxy group-containing silane coupling agent or alkoxy titanium compound, and a second anti-reflection layer made from a hydrolyzed condensate oligomer of an alkoxysilane compound, with controlled refractive indices and thicknesses, applied using environmentally friendly alcohol or glycol solvents.

Benefits of technology

The laminate achieves a balanced performance in low reflectivity, scratch resistance, and abrasion resistance with a simple layer structure, while reducing environmental impact through the use of non-fluorine-based solvents and enabling application on various substrates like glass and resin.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158203000001_ABST
    Figure 2024158203000001_ABST
Patent Text Reader

Abstract

To provide a low reflection laminate that is substantially free of fluorine-based solvents, contributes to reduced environmental load, offers superior manufacturability, and features an excellent combination of low reflectivity, scratch resistance, wear resistance, and fouling prevention despite having a simple layer structure, a low reflection treatment agent for preparing the low reflection laminate, and a method for producing the low reflection laminate.MEANS FOR SOLVING THE PROBLEM: A low reflection laminate includes at least a specific substrate layer, a specific first anti-reflection layer, and a specific second anti-reflection layer, which are laminated adjacently in this order. The first anti-reflection layer has a refractive index of 1.6-1.9, the second anti-reflection layer has a refractive index of 1.2-1.5, and the difference in refractive index between the first anti-reflection layer and the second anti-reflection layer is 0.2-0.5. The first anti-reflection layer has a thickness of 50-200 nm and the second anti-reflection layer has a thickness of 50-200 nm. The surface hardness of the low reflection laminate on the second anti-reflection layer side is 6 H or higher as measured by the pencil hardness test, and the minimum reflectance at wavelengths of 380-780 nm is 0.5-2%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a low-reflection laminate that has a small environmental load, excellent manufacturability, and a simple layer structure while having an excellent balance of low reflectivity, scratch resistance, abrasion resistance, and stain resistance; a low-reflection treatment agent that has a small environmental load for producing the low-reflection laminate; and a method for producing the low-reflection laminate. [Background technology]

[0002] 2. Description of the Related Art Displays for personal computers and the like are generally provided with an anti-reflection layer and an anti-fouling layer to prevent light reflection and staining. Anti-reflection layer and anti-fouling layer Anti-reflection is generally formed by first performing an anti-glare treatment on the glass by etching or the like, then forming an anti-reflection layer by forming multiple layers of SiO2 or Nb2O5 by sputtering, and then forming an anti-fouling layer by spraying a fluorine-based compound or the like. Since sputtering is carried out under vacuum conditions, the equipment costs are high and the productivity is low. Some antireflection layers contain nanoparticles to reduce the refractive index, but nanoparticles are expensive and have the problem of reducing the hardness of the layer (Patent Documents 1 to 6). Antifouling layers are generally formed on an antiglare treatment layer or an antireflection layer by spraying a treatment agent that contains a fluorine-based silane coupling agent to adhere to the substrate and to impart water repellency. However, since fluorine-based silane coupling agents are poorly soluble in general solvents, they must be diluted with a fluorine-based solvent before use, which places a heavy burden on the environment and is very expensive (Patent Documents 7 to 10). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2012-220556 A [Patent Document 2] Japanese Patent Application Publication No. 06-344489 [Patent Document 3] JP 2013-109169 A [Patent Document 4] Patent No. 6858860 [Patent Document 5] Patent No. 3930884 [Patent Document 6] JP 2018-097379 A [Patent Document 7] Patent No. 3449070 [Patent Document 8] Patent No. 5655215 [Patent Document 9] Patent No. 3876961 [Patent Document 10] International Publication No. 2006-046643 Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention aims to provide a low-reflection laminate that does not contain a fluorine compound, has a small environmental impact, is excellent in manufacturability, and has a simple layer structure while having an excellent balance of low reflectivity, scratch resistance, abrasion resistance, and stain resistance; a low-reflection treatment agent for producing the low-reflection laminate that does not substantially contain a fluorine-based solvent; and a method for producing the low-reflection laminate. [Means for solving the problem]

[0005] As a result of extensive investigations, the inventors have found that the above-mentioned object can be achieved by a low-reflection laminate comprising at least a specific substrate layer, a specific first antireflection layer, and a specific second antireflection layer laminated adjacent to each other in this order, in which the first antireflection layer and the second antireflection layer have specific refractive indexes, layer thicknesses, hardness, and minimum reflectance.

[0006] That is, the present invention is characterized in the following points. 1. A low-reflection laminate in which at least a substrate layer, a first antireflection layer, and a second antireflection layer are laminated adjacent to each other in this order, the substrate layer is made of a metal, a metal oxide or a resin; the first antireflective layer is made of a cured product of a hydrolysis-condensation product oligomer (A1), The hydrolysis condensation product oligomer (A1) is a hydrolysis condensation product oligomer of an epoxy group-containing silane coupling agent (B1) and / or an alkoxytitanium compound (C1), the second antireflective layer is made of a cured product of a hydrolysis-condensation product oligomer (A2), The hydrolysis condensation product oligomer (A2) is a hydrolysis condensation product oligomer of an alkoxysilane-based compound (D2), The alkoxysilane compound (D2) contains a tetraalkoxysilane compound (E2), the first antireflection layer has a refractive index of 1.6 to 1.9, the second antireflection layer has a refractive index of 1.2 to 1.5, and the difference in refractive index between the first antireflection layer and the second antireflection layer is 0.2 to 0.5; The first anti-reflective layer has a thickness of 50 to 250 nm, and the second anti-reflective layer has a thickness of 50 to 250 nm. The surface hardness of the low reflection laminate on the second antireflection layer side is 6H or more according to JIS K5600-5-4:1999, and the minimum reflectance at a wavelength of 380 to 780 nm is 0.5 to 2%. A low reflection laminate. 2. The low reflection laminate according to the above item 1, wherein the first antireflection layer further contains titanium oxide fine particles (F1) for controlling the refractive index, and has a refractive index of 1.6 to 1.9. 3. The alkoxysilane compound (D2) further contains a fluorine-containing silane coupling agent compound (G2), In the alkoxysilane compound (D2), the mass ratio of the tetraalkoxysilane compound (E2) to the fluorine-containing silane coupling agent compound (G2) is 1 / 1 to 1000 / 1. 3. The low reflection laminate according to 1 or 2 above. 4. The low reflection laminate according to any one of the above items 1 to 3, wherein the hydrolysis condensate oligomer (A2) is substantially free of fluorine and is soluble in an alcohol-based solvent and / or a glycol-based solvent. 5. The low reflection laminate according to any one of the above items 1 to 4, wherein the surface of the base layer is antiglare treated and has a surface roughness Ra of 0.5 to 20 nm. 6. The substrate layer is made of a metal oxide or a resin, The surface roughness Ra of the second anti-reflective layer is 0.5 to 20 nm, The haze of the low reflection laminate is 0.3 to 10%. 7. The low reflection laminate according to any one of the above items 1 to 6. 7. A low reflection treatment agent 1 for forming a first anti-reflection layer contained in the low reflection laminate according to any one of 1 to 6 above, The low reflection treatment agent 1 contains a hydrolysis condensation product oligomer (A1), The hydrolysis condensation product oligomer (A1) is a hydrolysis condensation product oligomer of an epoxy group-containing silane coupling agent (B1) and / or an alkoxytitanium compound (C1), and is soluble in a solvent (H1); The solvent (H1) contains an alcohol-based solvent and / or a glycol-based solvent, The content of the hydrolysis-condensation product oligomer (A1) in the low reflection treatment agent 1 is 5 to 80 mass %, The refractive index of the layer obtained by heat-curing the low reflection treatment agent 1 is 1.6 to 1.9. The low reflection treatment agent 1 is characterized by the above. 8. The low reflection treatment agent 1 according to the above item 7, further comprising 5 to 80 mass % of titanium oxide fine particles (F1) for controlling the refractive index. 9. A low reflection treatment agent 2 for forming a second anti-reflection layer contained in the low reflection laminate described in any one of 1 to 6 above, The low reflection treatment agent 2 contains a hydrolysis condensation product oligomer (A2) and a solvent (H2), The hydrolysis condensation product oligomer (A2) is a hydrolysis condensation product oligomer of an alkoxysilane-based compound (D2) and is soluble in a solvent (H2); The alkoxysilane compound (D2) contains a tetraalkoxysilane compound (E2), The solvent (H2) contains an alcohol-based solvent and / or a glycol-based solvent, The content of the hydrolysis-condensation product oligomer (A2) in the low reflection treatment agent 2 is 5 to 80 mass %, The refractive index of the layer obtained by heat-curing the low reflection treatment agent 2 is 1.2 to 1.5. The low reflection treatment agent 2 is characterized by the above. 10. The alkoxysilane compound (D2) further contains a fluorine-containing silane coupling agent compound (G2), a mass ratio of the tetraalkoxysilane compound (E2) to the fluorine-containing silane coupling agent compound (G2) is 1 / 1 to 1000 / 1; The solvent (H2) does not substantially contain a fluorine-based solvent. 10. The low reflection treatment agent 2 according to the above item 9. 11. A method for producing a low reflection laminate according to any one of 1 to 5 above, The production method includes the following steps 1 and 2 in this order, adjusting the refractive index of the first antireflective layer to 1.6 to 1.9, the refractive index of the second antireflective layer to 1.2 to 1.5, and a difference in refractive index between the first and second antireflective layers to 0.2 to 0.5; The minimum reflectance at a wavelength of 380 to 780 nm on the second antireflection layer side surface of the low reflection laminate is adjusted to 0.5 to 2%, Step 1: forming a first anti-reflective layer on a substrate layer; Base material layer temperature: 10~40℃, Coating method of the low reflection treatment agent 1 for the first anti-reflection layer: spray coating, spin coating, or roll coating; Drying and heat curing conditions for the first anti-reflective layer: 80 to 200°C, 1 to 120 minutes, Thickness of the first anti-reflective layer: 50 to 250 nm, Step 2: forming a second anti-reflective layer on the first anti-reflective layer; Base material layer temperature: 10~40℃, Coating method of low reflection treatment agent 2 for the second anti-reflection layer: spray coating, spin coating, or roll coating; Drying and heat curing conditions for the second anti-reflective layer: 80 to 200°C, 1 to 120 minutes, Thickness of the second anti-reflective layer: 50 to 250 nm, The low reflection treatment agent 1 for the first anti-reflection layer is the following low reflection treatment agent 1a or low reflection treatment agent 1b, Low-reflection treatment agent 1a: A low-reflection treatment agent containing a hydrolysis condensate oligomer (A1), the hydrolysis condensate oligomer (A1) being a hydrolysis condensate oligomer of an epoxy group-containing silane coupling agent (B1) and / or an alkoxytitanium compound (C1) and soluble in a solvent (H1), the solvent (H1) containing an alcohol-based solvent and / or a glycol-based solvent, the content of the hydrolysis condensate oligomer (A1) in the low-reflection treatment agent 1a being 5 to 80 mass %; Low-reflection treatment agent 1b: A low-reflection treatment agent comprising a hydrolysis condensate oligomer (A1), the hydrolysis condensate oligomer (A1) being a hydrolysis condensate oligomer of an epoxy group-containing silane coupling agent (B1) and / or an alkoxy titanium compound (C1), soluble in a solvent (H1), the solvent (H1) comprising an alcohol-based solvent and / or a glycol-based solvent, the content of the hydrolysis condensate oligomer (A1) in the low-reflection treatment agent 1b being 5 to 80% by mass, and further comprising titanium oxide fine particles (F1) for controlling the refractive index in an amount of 5 to 80% by mass in the low-reflection treatment agent 1b; A method for producing a second anti-reflection layer, comprising the steps of: Low-reflection treatment agent 2a: A low-reflection treatment agent containing a hydrolysis condensate oligomer (A2), the hydrolysis condensate oligomer (A2) being a hydrolysis condensate oligomer of an alkoxysilane-based compound (D2) and soluble in a solvent (H2), the alkoxysilane-based compound (D2) containing a tetraalkoxysilane-based compound (E2), the solvent (H2) containing an alcohol-based solvent and / or a glycol-based solvent, and the content of the hydrolysis condensate oligomer (A2) in the low-reflection treatment agent 2a being 1 to 80 mass%; Low-reflection treatment agent 2b: A low-reflection treatment agent comprising a hydrolysis condensate oligomer (A2), the hydrolysis condensate oligomer (A2) being a hydrolysis condensate oligomer of an alkoxysilane-based compound (D2) and soluble in a solvent (H2), the alkoxysilane-based compound (D2) comprising a tetraalkoxysilane-based compound (E2), the solvent (H2) comprising an alcohol-based solvent and / or a glycol-based solvent and substantially no fluorine-based solvent, the content of the hydrolysis condensate oligomer (A2) in the low-reflection treatment agent 2a being 1 to 80 mass%, the alkoxysilane-based compound (D2) further comprising a fluorine-containing silane coupling agent-based compound (G2), and the mass ratio of the tetraalkoxysilane-based compound (E2) / fluorine-containing silane coupling agent-based compound (G2) being 1 / 1 to 1000 / 1. 12. A method for producing a low reflection laminate according to the above 6, The production method includes the following steps 1 and 2 in this order, adjusting the refractive index of the first antireflective layer to 1.5 to 1.9, the refractive index of the second antireflective layer to 1.2 to 1.5, and the difference in refractive index between the first and second antireflective layers to 0.2 to 0.4, adjusting the surface roughness Ra of the second antireflective layer to 0.5 to 20 nm, and adjusting the haze of the low-reflection laminate to 0.5 to 10%, The minimum reflectance at a wavelength of 380 to 780 nm on the second antireflection layer side surface of the low reflection laminate is adjusted to 0.5 to 2%, Step 1: forming a first anti-reflective layer on a substrate layer; Base material layer temperature: 10~40℃, Coating method of the low reflection treatment agent 1 for the first anti-reflection layer: spray coating, spin coating, or roll coating; Drying and heat curing conditions for the first anti-reflective layer: 80 to 200°C, 30 to 120 minutes, Thickness of the first anti-reflective layer: 50 to 250 nm, Step 2: forming a second anti-reflective layer on the first anti-reflective layer; Base material layer temperature: 10~40℃, Coating method of low reflection treatment agent 2 for the second anti-reflection layer: spray coating, spin coating, or roll coating; Drying and heat curing conditions for the second anti-reflective layer: 80 to 200°C, 30 to 120 minutes, Thickness of the second anti-reflective layer: 50 to 250 nm, The low reflection treatment agent 1 for the first anti-reflection layer is the following low reflection treatment agent 1a or low reflection treatment agent 1b, Low-reflection treatment agent 1a: A low-reflection treatment agent containing a hydrolysis condensate oligomer (A1), the hydrolysis condensate oligomer (A1) being a hydrolysis condensate oligomer of an epoxy group-containing silane coupling agent (B1) and / or an alkoxytitanium compound (C1) and soluble in a solvent (H1), the solvent (H1) containing an alcohol-based solvent and / or a glycol-based solvent, the content of the hydrolysis condensate oligomer (A1) in the low-reflection treatment agent 1a being 5 to 80 mass %; Low-reflection treatment agent 1b: A low-reflection treatment agent comprising a hydrolysis condensate oligomer (A1), the hydrolysis condensate oligomer (A1) being a hydrolysis condensate oligomer of an epoxy group-containing silane coupling agent (B1) and / or an alkoxy titanium compound (C1), soluble in a solvent (H1), the solvent (H1) comprising an alcohol-based solvent and / or a glycol-based solvent, the content of the hydrolysis condensate oligomer (A1) in the low-reflection treatment agent 1b being 1 to 80% by mass, and further comprising titanium oxide fine particles (F1) for controlling the refractive index in an amount of 1 to 80% by mass in the low-reflection treatment agent 1b; A method for producing a second anti-reflection layer, comprising the steps of: Low-reflection treatment agent 2a: A low-reflection treatment agent containing a hydrolysis condensate oligomer (A2), the hydrolysis condensate oligomer (A2) being a hydrolysis condensate oligomer of an alkoxysilane-based compound (D2) and soluble in a solvent (H2), the alkoxysilane-based compound (D2) containing a tetraalkoxysilane-based compound (E2), the solvent (H2) containing an alcohol-based solvent and / or a glycol-based solvent, and the content of the hydrolysis condensate oligomer (A2) in the low-reflection treatment agent 2a being 1 to 80 mass%; Low-reflection treatment agent 2b: A low-reflection treatment agent comprising a hydrolysis condensate oligomer (A2), the hydrolysis condensate oligomer (A2) being a hydrolysis condensate oligomer of an alkoxysilane-based compound (D2) and soluble in a solvent (H2), the alkoxysilane-based compound (D2) comprising a tetraalkoxysilane-based compound (E2), the solvent (H2) comprising an alcohol-based solvent and / or a glycol-based solvent, the content of the hydrolysis condensate oligomer (A2) in the low-reflection treatment agent 2a being 1 to 80 mass%, the alkoxysilane-based compound (D2) further comprising a fluorine-containing silane coupling agent-based compound (G2), the mass ratio of the tetraalkoxysilane-based compound (E2) / the fluorine-containing silane coupling agent-based compound (G2) being 1 / 1 to 1000 / 1, and the solvent (H2) comprising substantially no fluorine-based solvent. 13. In the step 2, the coating method of the low reflection treatment agent 2 is spray coating; The low reflection treatment agent 2 is applied under the following application conditions: The surface roughness Ra of the second anti-reflective layer is adjusted to 0.5 to 20 nm. 13. The method according to claim 12, Coating conditions of low reflection treatment agent 2 for second anti-reflection layer Nozzle diameter: 0.1 to 10 mm Atomization pressure: 150~700kPa Discharge amount: 0.5~20ml / min Spray distance: 10~200mm Head speed: 50~500mm / sec Pitch: 0.5~10mm Effect of the Invention

[0007] The low reflection laminate of the present invention has a simple layer structure and yet has an excellent balance of low reflectivity, scratch resistance, and abrasion resistance. In addition, the low-reflection treatment agent of the present invention can be applied by a simple method to transparent substrates other than glass, such as resins, and does not substantially contain fluorine-based solvents, so that the environmental impact is small and the low-reflection laminate can be produced by simple equipment and methods. [Brief description of the drawings]

[0008] [Figure 1] 1 is a cross-sectional view of a low reflection laminate of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The low reflection laminate and the low reflection treatment agent of the present invention will be described in more detail below. Specific examples will be given, but the present invention is not limited thereto.

[0010] 1. Low-reflection laminate The low-reflection laminate of the present invention is a low-reflection laminate having at least a base layer, a first antireflection layer, and a second antireflection layer laminated adjacent to each other in this order, and has excellent transparency and antireflection properties. In order for the low reflective laminate of the present invention to have excellent transparency, the haze of the low reflective laminate is preferably from 0.3 to 10%, and more preferably from 0.3 to 5.0%.

[0011] The excellent antireflection property of the low reflection laminate of the present invention is caused by the refractive index difference between the first and second antireflection layers, and in order to have excellent antireflection property, the refractive index difference between the first and second antireflection layers is preferably 0.2 to 0.5, and more preferably 0.2 to 0.4. If the refractive index difference is smaller than the above range, the antireflection property is likely to be inferior, and if the refractive index difference is larger than the above range, the transparency is likely to be inferior.

[0012] The minimum reflectance at a wavelength of 380 to 780 nm on the second antireflection layer side surface of the low reflection laminate of the present invention is preferably 0.5 to 2%, more preferably 0.5 to 1.5%. It is difficult to obtain a minimum reflectance lower than the above range, and a minimum reflectance higher than the above range is likely to result in poor antireflection properties.

[0013] 1-1. About the base layer The substrate layer is an object to be coated with the anti-glare treatment agent of the present invention. The substrate layer is preferably made of a metal, a metal oxide or a resin, and in order for the low reflection laminate to have transparency, it is more preferably made of a highly transparent metal oxide or resin, and even more preferably a transparent metal oxide such as soda glass.

[0014] Specific examples of the metal contained in the substrate layer include stainless steel, aluminum, copper, zinc alloy, etc. Among these, stainless steel is preferable. The metal oxide contained in the substrate layer may be ceramic, glass, or the like. Examples of the substrate that uses glass include a glass plate and a glass cloth. Specific examples of the resin contained in the substrate layer include PMMA, PC, PET, etc. Among these, PMMA is preferable.

[0015] The thickness of the substrate layer is not particularly limited, but is preferably 0.1 to 5.0 mm. The surface of the base layer may be subjected to an antiglare treatment (AG treatment), and the surface roughness Ra is preferably 0.5 to 20 nm as a result of the antiglare treatment. In order to set the haze of the low reflection laminate to 0.3 to 10%, the haze of the base layer is preferably 0.3 to 10%.

[0016] 1-2. First anti-reflective layer The first anti-reflection layer is a layer formed from a low reflection treatment agent 1, and is preferably made of a cured product of a hydrolysis condensation product oligomer (A1), and may further contain titanium oxide fine particles (F1) to control the refractive index. When titanium oxide particles (F1) are contained, the content of titanium oxide particles (F1) in the first antireflective layer is preferably 5 to 95 mass %, more preferably 10 to 90 mass %. If the content is less than the above range and the layer is thin, the effect of containing titanium oxide particles (F1) is not easily obtained, whereas if the content is more than the above range, the film formability is easily deteriorated.

[0017] The refractive index of the first antireflective layer is preferably from 1.6 to 1.9, and more preferably from 1.6 to 1.8. The thickness of the first antireflective layer is preferably 50 to 250 nm, more preferably 70 to 200 nm. If the thickness is thinner than the above range, the effect of providing the first antireflective layer is less likely to be obtained, whereas if the thickness is thicker than the above range, the reflectance is likely to increase.

[0018] 1-3. Second anti-reflective layer The second anti-reflection layer is a layer formed from a low reflection treatment agent 2, and is preferably made of a cured product of a hydrolysis condensation product oligomer (A2), and may further contain a hydrolysis condensation product of an alkoxytitanium compound (C2) or titanium oxide fine particles (F2) in order to control the refractive index.

[0019] The refractive index of the second antireflective layer is preferably from 1.2 to 1.5, and more preferably from 1.3 to 1.5.

[0020] The thickness of the second anti-reflective layer is preferably 50 to 20050 to 250 nm, and more preferably 70 to 200 nm. If the thickness is thinner than the above range, the effect of providing the second anti-reflective layer is less likely to be obtained, whereas if the thickness is thicker than the above range, the reflectance is likely to increase. The surface roughness Ra of the second antireflective layer is preferably 0.5 to 20 nm, more preferably 0.5 to 15 nm. It is difficult to obtain an Ra smaller than the above range, and if it is larger than the above range, the haze tends to increase.

[0021] In addition, the second anti-reflective layer has a high hardness and can therefore function as a scratch-resistant layer. The surface hardness of the second antireflective layer is preferably 6H or more when measured in accordance with JIS K5600-5-4 "Scratch hardness (pencil method)".

[0022] Furthermore, the second antireflective layer exhibits water repellency and can function as an antifouling layer by containing a fluorine-containing silane coupling agent compound (G2) in the hydrolysis condensation product oligomer (A2). The contact angle of the surface of the second antireflective layer with water is preferably 100 degrees or more, and more preferably 105 degrees or more.

[0023] 2. About Anti-Reflection Treatment Agent 1 The low reflection treatment agent 1 is a treatment agent for forming a first antireflection layer included in the low reflection laminate. The low reflection treatment agent 1 contains a hydrolysis condensation oligomer (A1) and a solvent (H1), and may further contain titanium oxide fine particles (F1) to control the refractive index. Furthermore, it may further contain an acid or base catalyst (J1) to promote the hydrolysis condensation reaction. In addition, the low reflection treatment agent 1 may contain, as necessary, a wetting agent, a viscous material (thickener), a surface adjustment material, a coloring material (pigment, dye), an antistatic material, a conductivity imparting agent, an antibacterial and antiviral material, a filler such as hollow, chain-like, or porous solid silica particles, metal fine particles, etc., within a range that does not adversely affect the characteristics of the low reflection laminate.

[0024] The low reflection treatment agent 1 preferably has excellent storage stability. For example, when stored at 40°C for 3 months in a stationary state, it is preferable that there is no change in appearance and the increase in molecular weight is 0 to 100%, and more preferably 0 to 50%.

[0025] 2-1. Hydrolysis condensation product oligomer (A1) The hydrolysis condensation product oligomer (A1) is a hydrolysis condensation product oligomer of the epoxy group-containing silane coupling agent (B1) and / or the alkoxytitanium compound (C1), and is soluble in the solvent (H1). The content of the hydrolysis condensate oligomer (A1) in the low reflection treatment agent 1 is preferably from 1 to 80% by mass, more preferably from 2 to 40% by mass.

[0026] 2-2. Epoxy group-containing silane coupling agent (B1) The epoxy group-containing silane coupling agent (B1) is a silane compound having an epoxy group and an alkoxy group. The alkoxy group undergoes hydrolysis and dehydration condensation to form a crosslinked structure, and the epoxy group has the effect of increasing the refractive index.

[0027] Specific examples of the epoxy group-containing silane coupling agent (B1) include monomers or oligomers such as 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethylmethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 8-glycidoxyoctyltrimethoxysilane. Among these, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, or oligomers thereof are preferred. In the present invention, the above compounds can be used alone or in combination of two or more as the epoxy group-containing silane coupling agent (B1).

[0028] 2-3. Alkoxytitanium compounds (C1) The alkoxytitanium compound (C1) is a titanium compound having an alkoxy group. The alkoxy group can undergo hydrolysis and dehydration condensation to form a crosslinked structure.

[0029] Specific examples of the alkoxy titanium compound (C1) include tetraisopropyl titanate, tetra-n-butyl titanate, butyl titanate dimer, tetraoctyl titanate, titanium acetylacetonate, titanium tetraacetylacetonate, titanium ethylacetoacetate, dodecylbenzenesulfonic acid titanium compound, phosphate titanium complex, titanium octylene glycolate, titanium ethylacetoacetate, titanium lactate ammonium salt, titanium lactate, etc., or may be a compound synthesized with an oligomer or an organic monomer. Among these, tetra-n-butyl titanate or a compound similar thereto is preferred. In the present invention, the above compounds can be used alone or in combination of two or more as the alkoxytitanium compound (C1).

[0030] 2-4. Titanium oxide particles (F1) The titanium oxide fine particles (F1) are a component added to control the refractive index. In order for the low reflection laminate to have sufficient transparency, the particle size distribution of the titanium oxide fine particles (F1) is such that the number average primary particle diameter is preferably 1 to 50 nm, more preferably 1 to 30 nm, and the maximum particle diameter is preferably 50 to 100 nm, more preferably 50 to 80 nm.

[0031] 2-5. Acid or base catalyst (J1) The acid or base catalyst (J1) is a component that promotes the hydrolysis reaction and dehydration condensation reaction of the epoxy group-containing silane coupling agent (B1), the alkoxytitanium compound (C1), and the hydrolysis condensate oligomer (A1). The content of the acid or base catalyst (J1) in the low reflection treatment agent 1 is preferably 0.05 to 10 mass %, more preferably 0.1 to 5.0 mass %. If it is less than the above range, the promotion effect is likely to be insufficient, and if it is more than the above range, it is likely to be difficult to ensure uniform reaction progress.

[0032] Specific examples of the acid catalyst include hydrochloric acid, sulfuric acid, nitric acid, p-toluenesulfonic acid, benzenesulfonic acid, 10-camphorsulfonic acid, formic acid, oxalic acid, acetic acid, monochloroacetic acid, dichloroacetic acid, trichloroacetic acid, and lactic acid. Specific examples of the base catalyst include triethyleneamine, dimethylaminoethanol, and aqueous ammonia. Of these, nitric acid is preferred. In the present invention, the above compounds can be used alone or in combination of two or more as the acid or base catalyst (J1).

[0033] 2-6. Solvent (H1) The solvent (H1) is not particularly limited as long as it can dissolve the hydrolysis condensation product oligomer (A1) and disperse the titanium oxide fine particles (F1), but it is preferable that the solvent (H1) contains an alcohol-based solvent and / or a glycol-based solvent, and is preferably a non-fluorine-based solvent.

[0034] Specific examples of alcohol-based solvents include methanol (carbon number 1, boiling point 65°C), ethanol (carbon number 2, boiling point 78°C), normal propanol (carbon number 3, boiling point 97°C), isopropyl alcohol (carbon number 3, boiling point 82°C), tertiary butanol (carbon number 4, boiling point 82°C), normal butanol (carbon number 4, boiling point 118°C), isobutanol (carbon number 4, boiling point 108°C), and secondary butanol. Examples of such alcohols include ethanol (carbon number: 4, boiling point: 100° C.), 1-pentanol (carbon number: 5, boiling point: 138° C.), 2-methyl-1-butanol (carbon number: 5, boiling point: 128° C.), 3-methyl-1-butanol (carbon number: 5, boiling point: 131° C.), 2-pentanol (carbon number: 5, boiling point: 119° C.), 1-ethyl-1-propanol (carbon number: 5, boiling point: 116° C.), and 2-methyl-2-butanol (carbon number: 5, boiling point: 102° C.). Among these, ethanol and normal butanol are preferred.

[0035] Specific examples of glycol-based solvents include alkylene glycols and alkylene glycol ethers. Specific examples of alkylene glycols include ethylene glycol (carbon number 2, boiling point 197°C), propylene glycol (carbon number 3, boiling point 189°C), butylene glycol (carbon number 4, boiling point 207°C), hexylene glycol (carbon number 6, boiling point 197°C), and octylene glycol (carbon number 8, boiling point 175°C).

[0036] Specific examples of alkylene glycol ethers include ethylene glycol monomethyl ether (carbon number 3, boiling point 124°C), ethylene glycol monoethyl ether (carbon number 4, boiling point 135°C), ethylene glycol diethyl ether (carbon number 6, boiling point 121°C), ethylene glycol monoisopropyl ether (carbon number 5, boiling point 141°C), ethylene glycol monobutyl ether (carbon number 6, boiling point 171°C), propylene glycol monomethyl ether (carbon number 4, boiling point 120°C), propylene glycol monoethyl ether (carbon number 5, boiling point 132°C), propylene glycol mono-normal propyl ether (carbon number 6, boiling point 149°C), and propylene glycol mono-normal butyl ether (carbon number 7, boiling point 171°C). Among these, propylene glycol monomethyl ether is preferred. In the present invention, the above compounds can be used alone or in combination of two or more as the solvent (H1).

[0037] 2-6. Manufacturing method of low reflection treatment agent 1 The low reflection treatment agent 1 of the present invention can be prepared, for example, by the following method. 1) Preparation of silane compound solution An epoxy group-containing silane coupling agent (B1) and an alkoxytitanium compound (C1) are dissolved in a solvent (H1) to obtain a silane compound solution. 2) Preparation of catalyst solution Also, an acid or base catalyst (J1) is added dropwise to the solvent (H1) and mixed to obtain a catalyst solution. 3) Preparation of low reflection treatment agent 1 The catalyst solution obtained above is added dropwise to the silane compound solution obtained above while stirring and mixing to produce a hydrolysis condensation oligomer (A1). The temperature of the mixture is preferably adjusted to between 10 and 60° C. in order to suppress the hydrolysis condensation reaction.

[0038] Here, if necessary, a titanium oxide fine particle (F1) / solvent (H1) dispersion may be added to the reaction liquid and mixed by stirring. The obtained reaction liquid is diluted with a solvent (H1) to a concentration and viscosity according to a desired coating method and coating conditions to obtain a low reflection treatment agent 1. The low reflection treatment agent 1 may be filtered, for example, with a filter having a mesh size of 0.5 to 2 μm.

[0039] When using a solvent that evaporates slowly, it is effective to mix a large amount of a solvent with a low boiling point or to reduce the spray discharge amount, coating speed, atomization pressure, etc. To speed up the evaporation, the substrate may be preheated to about 100°C.

[0040] 3. About low reflection treatment agent 2 The low reflection treatment agent 2 is a treatment agent for forming the second antireflection layer contained in the low reflection laminate of the present invention. The low reflection treatment agent 2 contains a hydrolysis condensation oligomer (A2) and a solvent (H2), and may further contain an acid or base catalyst (J2) to promote the hydrolysis condensation reaction. In addition, the low reflection treatment agent 2 may contain, as necessary, a wetting agent, a viscous material (thickener), a surface adjustment material, a coloring material (pigment, dye), an antistatic material, a conductivity imparting agent, an antibacterial and antiviral material, a filler such as hollow, chain-like, or porous solid silica particles, metal fine particles, etc., within a range that does not adversely affect the characteristics of the low reflection laminate.

[0041] The low reflection treatment agent 2 preferably has excellent storage stability. For example, when stored at 40°C for 3 months in a stationary state, it is preferable that there is no change in appearance and the increase in molecular weight is 0 to 100%, and more preferably 0 to 50%.

[0042] 3-1. Hydrolysis condensation product oligomer (A2) The hydrolysis condensation oligomer (A2) is a hydrolysis condensation oligomer of an alkoxysilane compound (D2), and is soluble in a solvent (H2) containing substantially no fluorine. The content of the hydrolysis condensate oligomer (A2) in the low reflection treatment agent 2 is preferably from 1 to 80 mass %, more preferably from 2 to 40 mass %.

[0043] 3-2. Alkoxysilane compounds (D2) The alkoxysilane compound (D2) contains a tetraalkoxysilane compound (E2), and may further contain a fluorine-containing silane coupling agent compound (G2) as necessary to enhance water repellency, etc. The fluorine-containing silane coupling agent compound (G2) is poorly compatible with other organic components such as resins and solvents, but by forming a hydrolysis condensation oligomer with the tetraalkoxysilane compound (E2), it becomes compatible with other organic components such as resins and solvents.

[0044] The mass ratio of the tetraalkoxysilane compound (E2) / fluorine-containing silane coupling agent compound (G2) is preferably 1 / 1 to 1000 / 1, more preferably 4 / 1 to 50 / 1. If it is smaller than the above range, the hardness is likely to be inferior, and if it is larger than the above range, the water contact angle is likely to be inferior.

[0045] 3-3. Tetraalkoxysilane compounds (E2) The tetraalkoxysilane compound (E2) is a silane compound having four alkoxy groups. The alkoxy group undergoes hydrolysis and dehydration condensation to form a crosslinked structure.

[0046] Specific examples of the tetraalkoxysilane compound (E2) include tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, tetrabutoxysilane, and oligomers thereof. Among these, tetraethoxysilane and its oligomers are preferred. In the present invention, the above compounds can be used alone or in combination of two or more as the tetraalkoxysilane compound (E2).

[0047] 3-4. Fluorine-containing silane coupling agent compounds (G2) The fluorine-containing silane coupling agent compound (G2) is a silane compound having a functional group capable of reacting with an organic component, a fluorine group and an alkoxy group. The functional group capable of reacting with an organic component has the effect of adjusting the refractive index.

[0048] Specific examples of the fluorine-containing silane coupling agent compound (G2) include trifluoropropyltrimethoxysilane, dimethoxy(methyl)(3,3,3-trifluoropropyl)silane, trimethoxy(1H,1H,2H,2H-perfluorohexyl)silane, triethoxy(1H,1H,2H,2H-perfluorohexyl)silane, trimethoxy(1H,1H,2H,2H-perfluoro-n-octyl)silane, triethoxy(1H,1H,2H,2H-perfluoro-n-octyl)silane, triethoxy[5,5,6,6,7,7,7-heptafluoro-4,4-bis(trifluoromethyl)heptyl]silane, trimethoxy(1H,1H,2H,2H-heptadecafluorodecyl)silane, and triethoxy-1H,1H,2H,2H-heptadecafluorodecylsilane. Among these, trimethoxy(1H,1H,2H,2H-perfluoro-n-octyl)silane and triethoxy(1H,1H,2H,2H-perfluoro-n-octyl)silane are preferable. In the present invention, the above compounds can be used alone or in combination of two or more as the fluorine-containing silane coupling agent compound (G2).

[0049] 3-5. Acid or base catalyst (J2) The acid or base catalyst (J2) is a component that promotes the hydrolysis reaction and dehydration condensation reaction of the alkoxysilane compound (D2) and the hydrolysis condensate oligomer (A2). The content of the acid or base catalyst (J2) in the low reflection treatment agent 2 is preferably 0.05 to 10 mass %, more preferably 0.1 to 5.0 mass %. If the content is less than the above range, the promotion effect is likely to be insufficient, and if the content is more than the above range, it is likely to be difficult to ensure uniform reaction progress.

[0050] Specific examples of the acid catalyst include hydrochloric acid, sulfuric acid, nitric acid, p-toluenesulfonic acid, benzenesulfonic acid, 10-camphorsulfonic acid, formic acid, oxalic acid, acetic acid, monochloroacetic acid, dichloroacetic acid, trichloroacetic acid, and lactic acid. Specific examples of the base catalyst include triethyleneamine, dimethylaminoethanol, and aqueous ammonia. Of these, nitric acid is preferred. In the present invention, the above compounds can be used alone or in combination of two or more as the acid or base catalyst (J2).

[0051] 3-6. Solvent (H2) The solvent (H2) is not particularly limited as long as it can dissolve the hydrolysis condensate oligomer (A2) and the acid or base catalyst (J2). However, it is preferable that the solvent (H2) does not substantially contain a fluorine-based solvent and contains an alcohol-based solvent and / or a glycol-based solvent.

[0052] Specific examples of alcohol-based solvents include methanol (carbon number 1, boiling point 65°C), ethanol (carbon number 2, boiling point 78°C), normal propanol (carbon number 3, boiling point 97°C), isopropyl alcohol (carbon number 3, boiling point 82°C), tertiary butanol (carbon number 4, boiling point 82°C), normal butanol (carbon number 4, boiling point 118°C), isobutanol (carbon number 4, boiling point 108°C), and secondary butanol. Examples of the alcohol include ethanol (carbon number: 4, boiling point: 100° C.), 1-pentanol (carbon number: 5, boiling point: 138° C.), 2-methyl-1-butanol (carbon number: 5, boiling point: 128° C.), 3-methyl-1-butanol (carbon number: 5, boiling point: 131° C.), 2-pentanol (carbon number: 5, boiling point: 119° C.), 1-ethyl-1-propanol (carbon number: 5, boiling point: 116° C.), and 2-methyl-2-butanol (carbon number: 5, boiling point: 102° C.). Among these, ethanol is preferred. Regarding the selection of the solvent, one or more of these can be used in combination, taking into consideration the stability and drying property of the liquid.

[0053] Specific examples of glycol-based solvents include alkylene glycols and alkylene glycol ethers. Specific examples of alkylene glycols include ethylene glycol (carbon number: 2, boiling point: 197° C.), propylene glycol (carbon number: 3, boiling point: 189° C.), butylene glycol (carbon number: 4, boiling point: 207° C.), hexylene glycol (carbon number: 6, boiling point: 197° C.), and octylene glycol (carbon number: 8, boiling point: 175° C.). Specific examples of alkylene glycol ethers include ethylene glycol monomethyl ether (carbon number: 3, boiling point: 124° C.), ethylene glycol monoethyl ether (carbon number: 4, boiling point: 135° C.), and ethylene glycol ether (carbon number: 1, 135° C.). Examples of the propylene glycol monoethyl ether include propylene glycol monoethyl ether (carbon number: 6, boiling point: 121° C.), ethylene glycol monoisopropyl ether (carbon number: 5, boiling point: 141° C.), ethylene glycol monobutyl ether (carbon number: 6, boiling point: 171° C.), propylene glycol monomethyl ether (carbon number: 4, boiling point: 120° C.), propylene glycol monoethyl ether (carbon number: 5, boiling point: 132° C.), propylene glycol mono-normal propyl ether (carbon number: 6, boiling point: 149° C.), and propylene glycol mono-normal butyl ether (carbon number: 7, boiling point: 171° C.). Among these, propylene glycol monomethyl ether is preferred. In the present invention, the above compounds can be used alone or in combination of two or more as the solvent (H2).

[0054] 3-7. Manufacturing method of low reflection treatment agent 2 The low reflection treatment agent 2 of the present invention can be prepared, for example, by the following method. 1) Preparation of silane compound solution An alkoxysilane compound (D2) is dissolved in a solvent (H2) to obtain a silane compound solution. 2) Preparation of catalyst solution Also, an acid or base catalyst (J2) is added dropwise to the solvent (H2) and mixed to obtain a catalyst solution. 3) Preparation of low reflection treatment agent 2 The catalyst solution obtained above is added dropwise to the silane compound solution obtained above while stirring and mixing to produce a hydrolysis condensation oligomer (A2). The temperature of the mixture is preferably adjusted to between 10 and 60° C. in order to suppress the hydrolysis condensation reaction. The obtained reaction liquid is diluted with a solvent (H2) to a concentration and viscosity according to a desired coating method and coating conditions to obtain a low reflection treatment agent 2. The low reflection treatment agent 2 may be filtered, for example, with a filter having a mesh size of 0.5 to 2 μm.

[0055] 4. Manufacturing method of low reflection laminate The low reflective laminate of the present invention can be produced by a production method including the following steps 1 and 2 in this order.

[0056] Step 1: forming a first anti-reflective layer on a substrate layer; Base material layer temperature: 10~40℃, Coating method of the low reflection treatment agent 1 for the first anti-reflection layer: spray coating, spin coating, or roll coating; Drying and heat curing conditions for the first anti-reflective layer: 80 to 200°C, 1 to 120 minutes, Thickness of the first anti-reflective layer: 50 to 250 nm,

[0057] Step 2: forming a second anti-reflective layer on the first anti-reflective layer; Base material layer temperature: 10~40℃, Coating method of low reflection treatment agent 2 for the second anti-reflection layer: spray coating, spin coating, or roll coating; Drying and heat curing conditions for the second anti-reflective layer: 80 to 200°C, 1 to 120 minutes, Thickness of the second anti-reflective layer: 50 to 250 nm,

[0058] By adjusting the compositions of the low reflection treatment agents 1 and 2 and the process conditions of steps 1 and 2, it is possible to adjust the refractive index of the first antireflection layer to 1.6 to 1.9, the refractive index of the second antireflection layer to 1.2 to 1.5, the difference in refractive index between the first and second antireflection layers to 0.2 to 0.5, preferably 0.2 to 0.4, the surface roughness Ra of the second antireflection layer to 0.5 to 20 nm, the haze of the low reflection laminate to 0.5 to 10%, and the minimum reflectance at a wavelength of 380 to 780 nm on the second antireflection layer side surface of the low reflection laminate to 0.5 to 2%, thereby imparting antireflection property, high hardness, water repellency, abrasion resistance, and the like to the low reflection laminate.

[0059] When adjusting the refractive index of the first antireflective layer to 1.6 to 1.9, the refractive index of the second antireflective layer to 1.2 to 1.5, the difference in refractive index between the first and second antireflective layers to 0.2 to 0.5, and the minimum reflectance at a wavelength of 380 to 780 nm on the surface of the low-reflection laminate facing the second antireflective layer to 0.5 to 2%, the drying and heat-curing conditions for the first antireflective layer and the second antireflective layer are preferably 80 to 200° C. and 1 to 120 minutes.

[0060] In the case where the refractive index of the first antireflective layer is adjusted to 1.6 to 1.9, the refractive index of the second antireflective layer is adjusted to 1.2 to 1.5, the difference in refractive index between the first and second antireflective layers is adjusted to 0.2 to 0.5, the surface roughness Ra of the second antireflective layer is adjusted to 0.5 to 20 nm, the haze of the low-reflective laminate is adjusted to 0.5 to 10%, and the minimum reflectance at a wavelength of 380 to 780 nm on the surface of the low-reflective laminate facing the second antireflective layer is adjusted to 0.5 to 2%, the drying and heat-curing conditions for the first antireflective layer and the second antireflective layer are preferably 80 to 200° C. and 1 to 120 minutes.

[0061] Also, for example, it is possible to adjust the minimum reflectance by adjusting the refractive index difference, and it is possible to adjust the wavelength for which reflection is to be suppressed by adjusting the film thickness.

[0062] The application of the low-reflection treatment agent 1 and the low-reflection treatment agent 2 may be performed by any of spray coating, spin coating, roll coating, and dip coating. However, spray coating is preferred because it is highly productive, easy to adjust the appearance and film thickness, and environmentally friendly.

[0063] As the conditions for spray coating, for example, the following are preferable. Nozzle diameter: 0.1 to 10 mm, more preferably 0.1 to 2.0 mm Atomization pressure: 150~700kPa Discharge amount: 0.5~20ml / min Spray distance: 10~200mm Head speed: 50~500mm / sec Pitch: 0.5~10mm

[0064] When the surface roughness Ra of the second antireflective layer is adjusted to 0.5 to 20 nm using the low reflection treatment agent 2, the nozzle diameter is particularly preferably 0.1 to 2.0 mm. EXAMPLES

[0065] <Ingredients> Tetraalkoxysilane compound 1: Silicate 40 manufactured by Tama Chemicals Co., Ltd. A mixture of ethyl polysilicate and tetraethoxysilane. Ethyl polysilicate 60-70% by mass. · Epoxy group-containing silane coupling agent hydrolysis condensate oligomer 1: KR-517 manufactured by Shin-Etsu Chemical Co., Ltd. Epoxy group-containing trialkoxyl silane oligomer. Fluorine-containing silane coupling agent compound 1: Trimethoxy(1H,1H,2H,2H-perfluoro-n-octyl)silane. · Alkoxy titanium compound hydrolysis condensate oligomer solution 1: Orgatics PC-200 manufactured by Matsumoto Fine Chemical Co., Ltd. Organotitanium compound solid content 31%. Titanium oxide dispersion 1: TKS-202 manufactured by Teika Co., Ltd. TiO2 content 33% by mass, water solvent. Hollow silica dispersion 1: Sururia 1110 manufactured by JGC Catalysts and Chemicals. Hollow silica content 20% by mass, isopropyl alcohol solvent. · PGM1: Propylene glycol monomethyl ether. Degreased glass 1: A soda glass plate degreased with an alkaline detergent. 50 mm x 100 mm x 2 m thick. A commercially available soda glass plate was cleaned with a glass detergent solution (Semiclean LGL, Yokohama Resin Industries Co., Ltd.), then rinsed with water three times, water droplets on the surface were removed with an air blower, and the plate was dried in a dryer at 50°C for at least 5 minutes. · AG degreased glass 1: Obtained by subjecting the surface of degreased glass 1 to AG (Anti-Glare) treatment by etching. Surface roughness Ra 0.01 to 0.2 μm.

[0066] [Example 1] (Preparation of low reflection treatment agent 1 for first anti-reflection layer) The following ingredients were mixed to obtain an epoxy group-containing silane coupling agent hydrolysis condensate oligomer 1 / ethanol solution. Epoxy group-containing silane coupling agent hydrolysis condensate oligomer 1 4 parts by mass Ethanol 0.5 parts by weight Next, the following was mixed to obtain a nitric acid solution: 10% nitric acid aqueous solution 0.4 parts by mass Water 2.0 parts by mass Ethanol 0.5 parts by weight

[0067] Then, the nitric acid solution obtained above was added dropwise to the epoxy group-containing silane coupling agent hydrolysis condensate oligomer 1 / ethanol solution obtained above, and the mixture was stirred and mixed at 40° C. for 1.5 hours.

[0068] Next, the following was further added and mixed with stirring to obtain a low reflection treatment agent 1 for the first anti-reflection layer. PGM1 65 parts by mass Water 22.6 parts by mass Titanium oxide dispersion 1 5.0 parts by weight

[0069] (Preparation of low reflection treatment agent 2 for second anti-reflection layer) The following was mixed to obtain a tetraalkoxysilane compound 1 / ethanol solution. Tetraalkoxysilane compound 1 8 parts by mass Ethanol 1.5 parts by mass

[0070] Next, the following was mixed to obtain a nitric acid solution: 10% nitric acid aqueous solution 1.0 parts by mass Water 4.0 parts by mass Ethanol 1.5 parts by mass

[0071] The nitric acid solution obtained above was added dropwise to the tetraalkoxysilane compound 1 / ethanol solution obtained above, and the mixture was stirred and mixed at 40° C. for 1.5 hours.

[0072] (Formation of the first anti-reflective layer) The low-reflection treatment agent 1 obtained above was spin-coated at 2000 rpm using a precision coating machine manufactured by Apiros Co., Ltd. onto one side of degreased glass 1 at 20°C, and then dried and heat-cured at 150°C for 30 minutes to form a first anti-reflection layer having a thickness of 100 nm.

[0073] (Formation of second anti-reflective layer) Next, the low reflection treatment agent 2 obtained above was spin-coated on the first anti-reflection layer at a rotation speed of 2000 rpm using a precision coating machine manufactured by Apiros Co., Ltd., and dried and heat-cured at 150°C for 30 minutes to form a second anti-reflection layer having a thickness of 100 nm. Various evaluations were then carried out.

[0074] [Examples 2 to 7, 9 to 11] According to the description in Tables 1 and 2, the low reflection treatment agent 1 and the low reflection treatment agent 2 were prepared in the same manner as in Example 1, and the first anti-reflection layer and the second anti-reflection layer were formed to prepare a low reflection laminate. Then, various evaluations were carried out in the same manner as in Example 1.

[0075] [Example 8] The low reflection treatment agent 1 obtained above was spray-coated on one side of degreased glass 1 at 20°C under the following conditions using a precision coating machine manufactured by Apiros Co., Ltd., and then heated and dried at 100°C for 30 minutes to form a first antireflection layer with a thickness of 100 nm, thereby obtaining a low reflection laminate. Various evaluations were then carried out in the same manner as in Example 1. Nozzle diameter: 1.2mm Atomization pressure: 400kPa Discharge amount: 4.0ml / min Spray distance: 60mm Head speed: 500mm / sec Pitch: 7.0mm

[0076] Next, the low-reflection treatment agent 2 obtained above was spray-coated on the first anti-reflection layer using a precision coating machine manufactured by Apiros Co., Ltd. under the following conditions, and then heated and baked at 100°C for 30 minutes to form a second anti-reflection layer having a thickness of 100 nm. Nozzle diameter: 1.2mm Atomization pressure: 400kPa Discharge amount: 4.0ml / min Spray distance: 60mm Head speed: 500mm / sec Pitch: 7.0mm

[0077] [Comparative Examples 1 to 8] According to the description in Tables 3 and 4, the low reflection treatment agent 1 or the low reflection treatment agent 2 was prepared, and the first anti-reflection layer or the second anti-reflection layer was formed to prepare a laminate in the same manner as in Example 1. Then, various evaluations were carried out in the same manner as in Example 1.

[0078] <Evaluation items> [Appearance of low-reflective laminate] The appearance of the produced low reflection laminate was visually observed for the presence or absence of abnormalities. The symbols in the table have the following meanings. 〇: No abnormalities ×: Abnormal

[0079] [Surface hardness] The surface hardness of the first and second anti-reflective layers of the low reflection laminate was measured in accordance with JIS K5600-5-4:1999 "Scratch hardness (pencil method)". A hardness of 6H or more was considered acceptable.

[0080] [Minimum reflectance] The side of the base layer of the low reflection laminate was painted black, and black tape was attached to prevent light from passing through the low reflection laminate. The reflectance of the surface on the first anti-reflection layer and second anti-reflection layer side was measured using an ultraviolet-visible spectrophotometer (UV-2600, manufactured by Shimadzu Corporation). A reflectance of 2.0% or less was considered to be acceptable.

[0081] [Haze of low-reflective laminate] The haze value of the produced low reflection laminate was measured in accordance with JIS K7136:2000 using a haze meter NDH7000 (manufactured by Nippon Denshoku Industries Co., Ltd.) A haze value of 10% or less was considered to be acceptable.

[0082] [Surface roughness Ra] The surface roughness Ra of the side surfaces of the first and second antireflection layers of the produced low reflection laminate was measured using a laser microscope LEXT OLS4100 (manufactured by Olympus Corporation). A roughness of 20 nm or less was considered to be acceptable.

[0083] [Contact angle] The contact angle with water on the surfaces of the first and second antireflective layers of the produced low reflection laminate was measured using PCA-11 (manufactured by Kyowa Interface Science Co., Ltd.) in accordance with JIS R3257. A value of 100 degrees or more was considered to be acceptable. The antifouling layer was subjected to the following abrasion treatment, and then the contact angle with water was measured in the same manner. A passing grade was 100 degrees or above. Abrasive material: Steel wool #0000 Load: 10gf Load area: 2.25cm 2 Travel width: 40mm Speed: 100mm / sec

[0084] [Refractive index] The low-reflection treatment agent 1 was spin-coated onto a soda glass plate (refractive index 1.53), dried at 150°C for 30 minutes, and heat-cured to form a 100 nm treatment layer. The refractive index was measured using a high-speed automatic ellipsometer DVA-36L3 (manufactured by Mizojiri Optical Co., Ltd.) to obtain the refractive index of the first anti-reflection layer. The same procedure was carried out using low reflection treatment agent 2 to obtain the refractive index of the second anti-reflection layer. Each layer was judged to pass the following criteria: Refractive index of the first anti-reflective layer: 1.6 to 1.9 Refractive index of the second anti-reflective layer: 1.2 to 1.5 Difference in refractive index between the first anti-reflective layer and the second anti-reflective layer: 0.2 to 0.5

[0085] [Storage stability of low reflection treatment agent] The low reflection treatment agent 1 and the low reflection treatment agent 2 were stored at 40° C. for 3 months in a stationary state, and the storage stability was evaluated. The symbols in the table have the following meanings. ○: No change in molecular weight or appearance ○△: Molecular weight increased by 50%, but there was no change in appearance △: Molecular weight increased by 100%, with slight change in appearance ×: Molecular weight increased by 150%, and there was a change in appearance

[0086] [Table 1]

[0087] [Table 2]

[0088] [Table 3]

[0089] [Table 4]

[0090] <Summary of results> The low-reflection laminates of all the Examples exhibited an excellent balance of surface hardness, low reflectance, and low haze, whereas the laminates of the Comparative Examples exhibited poor surface hardness and / or low reflectance. [Industrial Applicability]

[0091] The low-reflection treatment agent of the present invention can be used for transparent glass or resin used in displays, showcases, partitions, etc. for personal computers, etc., and the low-reflection laminate of the present invention can be used for displays, showcases, partitions, etc. for personal computers, etc. [Explanation of symbols]

[0092] 1. Low reflection laminate 2 Base material layer 3 first anti-reflection layer, 4 Second anti-reflection layer

Claims

1. A low-reflection laminate including at least a base layer, a first antireflection layer, and a second antireflection layer laminated adjacent to each other in this order, the substrate layer is made of a metal, a metal oxide or a resin; the first antireflective layer is made of a cured product of a hydrolysis-condensation product oligomer (A1), The hydrolysis condensation product oligomer (A1) is a hydrolysis condensation product oligomer of an epoxy group-containing silane coupling agent (B1) and / or an alkoxytitanium compound (C1), the second antireflective layer is made of a cured product of a hydrolysis-condensation product oligomer (A2), The hydrolysis condensation product oligomer (A2) is a hydrolysis condensation product oligomer of an alkoxysilane-based compound (D2), The alkoxysilane compound (D2) contains a tetraalkoxysilane compound (E2), the first antireflective layer has a refractive index of 1.6 to 1.9, the second antireflective layer has a refractive index of 1.2 to 1.5, and the difference in refractive index between the first antireflective layer and the second antireflective layer is 0.2 to 0.5; The first anti-reflective layer has a thickness of 50 to 250 nm, and the second anti-reflective layer has a thickness of 50 to 250 nm. The surface hardness of the low reflection laminate on the second anti-reflection layer side is 6H or more according to JIS K5600-5-4:1999, and the minimum reflectance at wavelengths of 380 to 780 nm is 0.5 to 2%. A low reflection laminate.

2. 2. The low reflection laminate according to claim 1, wherein the first anti-reflection layer further contains titanium oxide fine particles (F1) for controlling the refractive index, and has a refractive index of 1.6 to 1.

9.

3. The alkoxysilane compound (D2) further contains a fluorine-containing silane coupling agent compound (G2), In the alkoxysilane compound (D2), the mass ratio of the tetraalkoxysilane compound (E2) to the fluorine-containing silane coupling agent compound (G2) is 1 / 1 to 1000 / 1. The low reflection laminate according to claim 1 .

4. 2. The low reflection laminate according to claim 1, wherein the hydrolysis condensate oligomer (A2) is substantially free of fluorine and is soluble in an alcohol-based solvent and / or a glycol-based solvent.

5. 2. The low reflection laminate according to claim 1, wherein the surface of the base layer is antiglare treated and has a surface roughness Ra of 0.5 to 20 nm.

6. The substrate layer is made of a metal oxide or a resin, the surface roughness Ra of the second anti-reflective layer is 0.5 to 20 nm; The haze of the low reflection laminate is 0.3 to 10%. The low reflection laminate according to claim 1 .

7. A low reflection treatment agent 1 for forming a first anti-reflection layer contained in the low reflection laminate according to claim 1, The low reflection treatment agent 1 contains a hydrolysis condensation product oligomer (A1), The hydrolysis condensate oligomer (A1) is a hydrolysis condensate oligomer of an epoxy group-containing silane coupling agent (B1) and / or an alkoxytitanium compound (C1), and is soluble in a solvent (H1); The solvent (H1) contains an alcohol-based solvent and / or a glycol-based solvent, The content of the hydrolysis-condensation product oligomer (A1) in the low reflection treatment agent 1 is 5 to 80 mass %, The refractive index of the layer obtained by heat-curing the low reflection treatment agent 1 is 1.6 to 1.

9. The low reflection treatment agent 1 is characterized by the above.

8. The low reflection treatment agent 1 according to claim 7, further comprising 5 to 80 mass % of titanium oxide fine particles (F1) for controlling the refractive index.

9. A low reflection treatment agent 2 for forming a second anti-reflection layer contained in the low reflection laminate according to claim 1, The low reflection treatment agent 2 contains a hydrolysis condensation product oligomer (A2) and a solvent (H2), The hydrolysis condensation product oligomer (A2) is a hydrolysis condensation product oligomer of an alkoxysilane-based compound (D2) and is soluble in a solvent (H2); The alkoxysilane compound (D2) contains a tetraalkoxysilane compound (E2), The solvent (H2) contains an alcohol-based solvent and / or a glycol-based solvent, The content of the hydrolysis-condensation product oligomer (A2) in the low reflection treatment agent 2 is 5 to 80 mass %, The refractive index of the layer obtained by heat-curing the low reflection treatment agent 2 is 1.2 to 1.

5. The low reflection treatment agent 2 is characterized by the above.

10. The alkoxysilane compound (D2) further contains a fluorine-containing silane coupling agent compound (G2), The mass ratio of the tetraalkoxysilane compound (E2) to the fluorine-containing silane coupling agent compound (G2) is 1 / 1 to 1000 / 1; The solvent (H2) does not substantially contain a fluorine-based solvent.

10. The low reflection treatment agent 2 according to claim 9.

11. A method for producing the low reflection laminate according to any one of claims 1 to 5, The production method includes the following steps 1 and 2 in this order, adjusting the refractive index of the first antireflective layer to 1.6 to 1.9, adjusting the refractive index of the second antireflective layer to 1.2 to 1.5, and adjusting the difference in refractive index between the first antireflective layer and the second antireflective layer to 0.2 to 0.5: The minimum reflectance at a wavelength of 380 to 780 nm on the second antireflection layer side surface of the low reflection laminate is adjusted to 0.5 to 2%; Step 1: forming a first anti-reflective layer on a substrate layer; Base material layer temperature: 10 to 40°C, Coating method of the low reflection treatment agent 1 for the first anti-reflection layer: spray coating, spin coating, or roll coating; Drying and heat curing conditions for the first anti-reflective layer: 80 to 200° C., 1 to 120 minutes, Thickness of the first anti-reflective layer: 50 to 250 nm, Step 2: forming a second anti-reflective layer on the first anti-reflective layer; Base material layer temperature: 10 to 40°C, Coating method of the low reflection treatment agent 2 for the second anti-reflection layer: spray coating, spin coating, or roll coating; Drying and heat curing conditions for the second anti-reflective layer: 80 to 200° C., 1 to 120 minutes, Thickness of second anti-reflective layer: 50 to 250 nm, The low reflection treatment agent 1 for the first anti-reflection layer is the following low reflection treatment agent 1a or low reflection treatment agent 1b, Low-reflection treatment agent 1a: A low-reflection treatment agent comprising a hydrolysis condensate oligomer (A1), the hydrolysis condensate oligomer (A1) being an epoxy group-containing silane coupling agent (B1) and / or an alkoxy titanium compound (C1) and soluble in a solvent (H1), the solvent (H1) comprising an alcohol-based solvent and / or a glycol-based solvent, the content of the hydrolysis condensate oligomer (A1) in the low-reflection treatment agent 1a being 5 to 80 mass %; Low reflection treatment agent 1b: A low reflection treatment agent comprising a hydrolysis condensate oligomer (A1), the hydrolysis condensate oligomer (A1) being a hydrolysis condensate oligomer of an epoxy group-containing silane coupling agent (B1) and / or an alkoxy titanium compound (C1), soluble in a solvent (H1), the solvent (H1) containing an alcohol-based solvent and / or a glycol-based solvent, the content of the hydrolysis condensate oligomer (A1) in the low reflection treatment agent 1b being 5 to 80 mass%, and further comprising titanium oxide fine particles (F1) for controlling the refractive index in an amount of 5 to 80 mass% in the low reflection treatment agent 1b; A method for producing a second anti-reflective layer, comprising the steps of: Low-reflection treatment agent 2a: A low-reflection treatment agent comprising a hydrolysis condensate oligomer (A2), the hydrolysis condensate oligomer (A2) being a hydrolysis condensate oligomer of an alkoxysilane-based compound (D2) and soluble in a solvent (H2), the alkoxysilane-based compound (D2) comprising a tetraalkoxysilane-based compound (E2), the solvent (H2) comprising an alcohol-based solvent and / or a glycol-based solvent, and the content of the hydrolysis condensate oligomer (A2) in the low-reflection treatment agent 2a being 1 to 80 mass%; Low reflection treatment agent 2b: A low reflection treatment agent comprising a hydrolysis condensate oligomer (A2), the hydrolysis condensate oligomer (A2) being a hydrolysis condensate oligomer of an alkoxysilane-based compound (D2) and soluble in a solvent (H2), the alkoxysilane-based compound (D2) comprising a tetraalkoxysilane-based compound (E2), the solvent (H2) comprising an alcohol-based solvent and / or a glycol-based solvent and substantially no fluorine-based solvent, the content of the hydrolysis condensate oligomer (A2) in the low reflection treatment agent 2a being 1 to 80 mass%, the alkoxysilane-based compound (D2) further comprising a fluorine-containing silane coupling agent-based compound (G2), and the mass ratio of the tetraalkoxysilane-based compound (E2) / fluorine-containing silane coupling agent-based compound (G2) being 1 / 1 to 1000 / 1.

12. A method for producing the low reflection laminate according to claim 6, The production method includes the following steps 1 and 2 in this order, adjusting the refractive index of the first antireflective layer to 1.6 to 1.9, the refractive index of the second antireflective layer to 1.2 to 1.5, and the difference in refractive index between the first and second antireflective layers to 0.2 to 0.4, adjusting the surface roughness Ra of the second antireflective layer to 0.5 to 20 nm, and adjusting the haze of the low-reflection laminate to 0.5 to 10%, The minimum reflectance at a wavelength of 380 to 780 nm on the second antireflection layer side surface of the low reflection laminate is adjusted to 0.5 to 2%, Step 1: forming a first anti-reflective layer on a substrate layer; Base material layer temperature: 10 to 40°C, Coating method of the low reflection treatment agent 1 for the first anti-reflection layer: spray coating, spin coating, or roll coating; Drying and heat curing conditions for the first anti-reflective layer: 80 to 200° C., 30 to 120 minutes, Thickness of the first anti-reflective layer: 50 to 250 nm, Step 2: forming a second anti-reflective layer on the first anti-reflective layer; Base material layer temperature: 10 to 40°C, Coating method of the low reflection treatment agent 2 for the second anti-reflection layer: spray coating, spin coating, or roll coating; Drying and heat curing conditions for the second anti-reflective layer: 80 to 200° C., 30 to 120 minutes, Thickness of second anti-reflective layer: 50 to 250 nm, The low reflection treatment agent 1 for the first anti-reflection layer is the following low reflection treatment agent 1a or low reflection treatment agent 1b, Low reflection treatment agent 1a: Contains a hydrolysis condensation product oligomer (A1), which is a hydrolysis condensation product oligomer of an epoxy group-containing silane coupling agent (B1) and / or an alkoxy titanium compound (C1), and is soluble in a solvent (H1); A low-reflection treatment agent, wherein the solvent (H1) contains an alcohol-based solvent and / or a glycol-based solvent, and the content of the hydrolysis-condensate oligomer (A1) in the low-reflection treatment agent 1a is 5 to 80 mass %. Low-reflection treatment agent 1b: A low-reflection treatment agent comprising a hydrolysis condensate oligomer (A1), the hydrolysis condensate oligomer (A1) being a hydrolysis condensate oligomer of an epoxy group-containing silane coupling agent (B1) and / or an alkoxy titanium compound (C1), soluble in a solvent (H1), the solvent (H1) comprising an alcohol-based solvent and / or a glycol-based solvent, the content of the hydrolysis condensate oligomer (A1) in the low-reflection treatment agent 1b being 1 to 80% by mass, and further comprising titanium oxide fine particles (F1) for controlling the refractive index in an amount of 1 to 80% by mass in the low-reflection treatment agent 1b; A method for producing a second anti-reflective layer, comprising the steps of: Low-reflection treatment agent 2a: A low-reflection treatment agent comprising a hydrolysis condensate oligomer (A2), the hydrolysis condensate oligomer (A2) being a hydrolysis condensate oligomer of an alkoxysilane-based compound (D2) and soluble in a solvent (H2), the alkoxysilane-based compound (D2) comprising a tetraalkoxysilane-based compound (E2), the solvent (H2) comprising an alcohol-based solvent and / or a glycol-based solvent, and the content of the hydrolysis condensate oligomer (A2) in the low-reflection treatment agent 2a being 1 to 80 mass%; Low reflection treatment agent 2b: A low reflection treatment agent comprising a hydrolysis condensate oligomer (A2), the hydrolysis condensate oligomer (A2) being a hydrolysis condensate oligomer of an alkoxysilane-based compound (D2) and soluble in a solvent (H2), the alkoxysilane-based compound (D2) comprising a tetraalkoxysilane-based compound (E2), the solvent (H2) comprising an alcohol-based solvent and / or a glycol-based solvent, the content of the hydrolysis condensate oligomer (A2) in the low reflection treatment agent 2a being 1 to 80 mass%, the alkoxysilane-based compound (D2) further comprising a fluorine-containing silane coupling agent-based compound (G2), the mass ratio of the tetraalkoxysilane-based compound (E2) / the fluorine-containing silane coupling agent-based compound (G2) being 1 / 1 to 1000 / 1, and the solvent (H2) substantially not comprising a fluorine-based solvent.

13. In the step 2, the coating method of the low reflection treatment agent 2 is spray coating, The low reflection treatment agent 2 is applied under the following application conditions: The surface roughness Ra of the second anti-reflective layer is adjusted to 0.5 to 20 nm. The method according to claim 12, Coating conditions of low reflection treatment agent 2 for second anti-reflection layer Nozzle diameter: 5 to 100 mm Atomization pressure: 150 to 700 kPa Discharge amount: 0.5-20ml / min Spray distance: 10-200mm Head speed: 50 to 500 mm / sec Pitch: 0.5 to 10 mm

Citation Information

Patent Citations

  • Manufacturing device for cement tile

    JP1981055215A

  • Coating for forming antistatic high refractive index film, transparent laminate having antistatic antireflective film and cathode rays tube

    JP1994344489A

  • Antireflection film, composition for forming high refractive layer of the antireflection film, and display for outdoor installation

    JP2012220556A

  • Antireflection member

    JP2013109169A

  • Method of manufacturing Anti-glare, Anti-reflection member

    JP2018097379A