Lithium-ion rechargeable battery
The lithium-ion secondary battery design addresses high-rate deterioration by controlling lithium ion flow through adjusted porosities and spring constants in the electrode layers, ensuring balanced distribution and reduced concentration imbalances.
Patent Information
- Application Number
- JP2023073657
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2024-11-08
AI Technical Summary
Lithium-ion secondary batteries used in vehicles experience high-rate deterioration due to uneven lithium ion concentration during rapid charging and discharging, which existing technologies fail to adequately address.
The battery design includes an electrode body with positive and negative electrode composite layers having porosities higher than the separator, controlled by a separator with specific porosity and spring constant to manage lithium ion flow, thereby reducing concentration imbalances.
This configuration effectively suppresses high-rate deterioration by maintaining balanced lithium ion distribution and preventing concentration unevenness during charging and discharging.
Smart Images

Figure 2024158446000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a lithium ion secondary battery, and more particularly to a lithium ion secondary battery that suppresses high-rate degradation. [Background technology]
[0002] Lithium ion secondary batteries are lightweight and have a high energy density. In addition, because they have a high voltage and high output, they are also preferably used as high-output power sources for vehicles that perform high-rate charging and discharging. Such nonaqueous electrolyte secondary batteries include an electrode assembly having a storage element in which a positive electrode plate and a negative electrode plate are insulated by a separator. Such a separator is configured to facilitate the movement of lithium ions between the positive and negative electrodes.
[0003] Regarding the porosity of such an electrode body, for example, Patent Document 1 proposes the following configuration with the objective of suppressing precipitation of substances derived from charge carriers by providing a more preferable coating on the surface of the negative electrode active material. That is, a heat-resistant layer is provided between at least one of the positive and negative electrodes and the separator substrate to prevent internal short circuit due to thermal contraction of the separator substrate. Then, a nonaqueous electrolyte secondary battery is provided in which the porosity of the negative electrode mixture layer, the porosity of the separator substrate, and the porosity of the heat-resistant layer satisfy a predetermined relationship.
[0004] The invention, which focuses on such porosity, has the effect of suppressing the deposition of substances derived from charge carriers. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2014-120214 A Summary of the Invention [Problem to be solved by the invention]
[0006] In the case of a lithium-ion secondary battery for driving a vehicle mounted on an electric vehicle or a hybrid vehicle, when the battery is charged or discharged at a high rate due to rapid charging, rapid acceleration, or rapid deceleration, the electrolyte moves violently. If the non-aqueous electrolyte cannot move sufficiently in the cell battery, the concentration of the non-aqueous electrolyte becomes uneven. This can cause battery deterioration, known as "high-rate deterioration." The invention described in Patent Document 1 focuses on the porosity, but does not recognize such high-rate deterioration. For this reason, the invention described in Patent Document 1 cannot suppress high-rate deterioration.
[0007] When charging and discharging at a high rate, the lithium ion concentration in the electrode assembly may become biased due to the porosity of the positive electrode, negative electrode, and separator. The present inventors have found that such a bias in the lithium ion concentration is likely to cause high-rate deterioration.
[0008] The problem that the lithium ion secondary battery of the present invention aims to solve is to suppress high-rate degradation. [Means for solving the problem]
[0009] In order to solve the above problems, the lithium-ion secondary battery of the present invention comprises an electrode body in which a positive electrode plate having a positive electrode mixture layer and a negative electrode plate having a negative electrode mixture layer are stacked with a separator interposed therebetween, and is characterized in that the porosity PP of the positive electrode mixture layer and the porosity NP of the negative electrode mixture layer are set higher than the porosity SP of the separator.
[0010] It is desirable that the difference ΔP between the difference PPD between the porosity PP of the positive electrode mixture layer and the porosity SP of the separator and the difference NPD between the porosity NP of the negative electrode mixture layer and the porosity SP of the separator is 4% or less.
[0011] The difference PPD is preferably 2.00 to 6.59%. Moreover, it is preferable that the difference NPD is 3.96 to 7.86%. The porosity SP of the separator is desirably 42.15% or less and 39.54% or more.
[0012] The positive electrode mixture layer preferably has a porosity PP of 44.16% or more and 48.61% or less. The negative electrode mixture layer preferably has a porosity NP of 45.38% or more and 49.68% or less.
[0013] The density of the positive electrode mixture layer is 2.9 [g / cm 3 ] or less, 2.2[g / cm 3 ] or higher is desirable. The density of the negative electrode mixture layer is 1.2 [g / cm 3 ] or less, 0.9[g / cm 3 ] or higher is desirable.
[0014] The cell of the lithium ion secondary battery is pressed in the thickness direction by a load cell with a load of 9.8 [kN], and then the load of the load cell is set to 4.5 [kN]. The displacement at that time is D [mm]. The load of the load cell when the position of the load cell is fixed and left for 600 [seconds] is set to L [kN]. The spring constant C [kN / mm] of the cell is C = (9.8 - x) / D. It is desirable that C≦95.38 [kN / mm], C≧80.96 [kN / mm]. Effect of the Invention
[0015] According to the lithium ion secondary battery of the present invention, high-rate degradation can be suppressed. [Brief description of the drawings]
[0016] [Figure 1] 1 is a perspective view showing the outline of the configuration of a lithium-ion secondary battery 1 of the present embodiment. [Diagram 2] FIG. 2 is a schematic diagram showing the configuration of a wound electrode body. [Diagram 3] 2 is a schematic diagram showing the state of the lithium ion secondary battery of the present embodiment when no current is applied; FIG. [Figure 4]FIG. 2 is a schematic diagram showing the state of the lithium ion secondary battery during charging according to the embodiment. [Diagram 5] FIG. 2 is a schematic diagram showing the state of the lithium ion secondary battery during discharging according to the embodiment. [Figure 6] 1 is a table showing conditions and results of an experimental example. [Figure 7] 1 is a graph showing the relationship between the spring constant C and the high-rate characteristic index in an experiment. [Figure 8] FIG. 1 is a schematic diagram showing a state of a conventional lithium ion secondary battery when no current is applied. [Figure 9] FIG. 1 is a schematic diagram showing the state of a conventional lithium ion secondary battery during charging. [Figure 10] FIG. 1 is a schematic diagram showing the state of a conventional lithium ion secondary battery during discharging. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] (Outline of this embodiment) Hereinafter, the lithium ion secondary battery of the present invention will be described with reference to FIGS. 1 to 10, taking one embodiment of a lithium ion secondary battery 1 as an example.
[0018] <Porosity P[%]> Prior to the description, the "porosity P [%]" in this embodiment will be defined. The "porosity P [%]" is a measure that represents the ratio of the volume (capacity) of spaces such as interparticle voids and pores to the total volume. Since the porosity P [%] generally has a correlation with the water permeability coefficient, in this embodiment, the porosity PP [%] of the positive electrode mixture layer 32, the porosity NP [%] of the negative electrode mixture layer 22, and the porosity SP [%] of the separator 4 are calculated based on the ratio of the volume (capacity) of the lithium ion Li + In the present embodiment, the porosity P [%] is used as an index showing the efficiency of the flow of the porous material. Generally, the term "porosity [%]" is used for a porous material such as the separator 4, but since both terms have the same definition, the term "porosity P [%]" will be used in the present embodiment.
[0019] The porosity P [%] can be measured, for example, by the immersion method, in which a porous sample is immersed in a liquid with good wetting properties and the pores are saturated with the liquid. Alternatively, an optical method can be used to determine the material area and the area of visible pores through microscopic observation of the sample cross section. Furthermore, it can be measured by the mercury intrusion method, in which mercury, which has a strong surface tension, is forced into minute pores, and the amount of intrusion is measured against the amount of pressure applied from the outside to determine the distribution of pore diameters and pore volume.
[0020] <Previous issues> As described in the prior art, when a conventional lithium-ion secondary battery 101 for driving an automobile is charged and discharged at a high rate, the lithium ion Li + If the electrolyte cannot move sufficiently in the cell battery, the lithium ions Li in the non-aqueous electrolyte 13 will move violently. + The concentration of lithium ion Li + If there is unevenness in the concentration of , the internal resistance will increase overall. 2 The unevenness of the lithium ion layer can also cause the precipitation of metallic Li. + It is known that battery deterioration, known as "high rate deterioration," occurs due to unevenness in the concentration of
[0021] Fig. 8 is a schematic diagram showing the state of a conventional lithium ion secondary battery 101 when no current is applied. As with the lithium ion secondary battery 1 shown in Fig. 2, the electrode body 12 of the lithium ion secondary battery 101 has a positive electrode plate 3 and a negative electrode plate 2 facing each other with a separator 104 interposed therebetween. A non-aqueous electrolyte 13 is filled between the positive electrode plate 3 and the negative electrode plate 2, so that lithium ions Li + When power is off, the lithium-ion Li + Since it is not electrically attracted to either the positive electrode plate 3 or the negative electrode plate 2, it does not move.
[0022] 9 is a schematic diagram showing the state of a conventional lithium ion secondary battery 101 during charging. When the lithium ion secondary battery 101 is charged, electrons flow from the negative electrode connection portion 21a of the negative electrode plate 2 to the negative electrode current collector 21. Electrons are supplied from the negative electrode current collector 21 to the negative electrode active material 23. As a result, lithium ions Li + is attracted to the negative electrode active material 23.
[0023] At this time, the conventional separator 104 is + The porosity SP [%] is sufficient so as not to impede the smooth movement of lithium ions Li + can easily move from the positive electrode plate 3 side to the negative electrode plate 2 side.
[0024] On the other hand, the negative electrode mixture layer 22 of the negative electrode plate 2 contains a sufficient amount of the negative electrode active material 23 to increase the battery capacity, and therefore the porosity PP [%] is lower than that of the separator 104. For this reason, lithium ions Li + As the concentration of lithium ions Li increases, + This causes unevenness in the density of the image, which in turn causes the problem of high-rate degradation.
[0025] FIG. 10 is a schematic diagram showing the state of a conventional lithium ion secondary battery 101 during discharge. When the lithium ion secondary battery 101 is discharged, electrons flow from the positive electrode connection portion 31a of the positive electrode plate 3 to the positive electrode current collector 31. Electrons are supplied from the positive electrode current collector 31 to the positive electrode active material 33. As a result, lithium ions Li + is attracted to the positive electrode active material 33.
[0026] At this time, the conventional separator 104 is + The porosity SP [%] is sufficient so as not to inhibit the movement of lithium ions Li + could easily move from the negative electrode plate 2 side to the positive electrode plate 3 side.
[0027] On the other hand, the positive electrode mixture layer 32 of the positive electrode plate 3 contains a sufficient amount of positive electrode active material 33 to increase the battery capacity, and therefore the porosity PP [%] is lower than that of the separator 104. For this reason, lithium ions Li + As the concentration of lithium ions Li increases, + This causes unevenness in the concentration of , which in turn causes the problem of high-rate degradation occurring easily during discharging, just as during charging.
[0028] <Features of this embodiment> Therefore, in the lithium ion secondary battery 1 of this embodiment, the inventors deliberately set the porosity SP [%] of the separator 4 lower than the porosity PP [%] of the positive electrode mixture layer 32 and the porosity NP [%] of the negative electrode mixture layer 22, contrary to the conventional technical common sense of those skilled in the art. + However, this makes it difficult for lithium ions Li + The rate of movement of lithium ions Li in the entire nonaqueous electrolyte 13 is determined by the separator 4. + Therefore, the distribution of lithium ions Li in the nonaqueous electrolyte 13 is averaged. + As a result, deterioration at high rates is less likely to occur.
[0029] 3 is a schematic diagram showing the state of the lithium ion secondary battery 1 of this embodiment when no current is applied. As shown in FIG. 2, the electrode body 12 of the lithium ion secondary battery 1 has a positive electrode plate 3 and a negative electrode plate 2 facing each other with a separator 4 interposed therebetween. A nonaqueous electrolyte 13 is filled between the positive electrode plate 3 and the negative electrode plate 2, so that lithium ions Li + When power is off, the lithium-ion Li + does not move because it is not electrically attracted to either the positive electrode plate 3 or the negative electrode plate 2. In this state, the battery is the same as the conventional lithium ion secondary battery 101.
[0030] 4 is a schematic diagram showing the state of the lithium ion secondary battery 1 during charging according to this embodiment. When the lithium ion secondary battery 1 is charged, electrons flow from the negative electrode connection portion 21a of the negative electrode plate 2 to the negative electrode current collector 21. Electrons are supplied from the negative electrode current collector 21 to the negative electrode active material 23. As a result, lithium ions Li + is attracted to the negative electrode active material 23.
[0031] At this time, the separator 4 of this embodiment is deliberately made of lithium ions Li + The porosity SP [%] is low so as to inhibit the movement of lithium ions Li + cannot easily move from the positive electrode plate 3 side to the negative electrode plate 2 side.
[0032] On the other hand, the negative electrode mixture layer 22 of the negative electrode plate 2 needs a sufficient amount of negative electrode active material 23 to increase the battery capacity, but the porosity PP [%] is adjusted to be higher than that of the separator 4. For this reason, during charging, the separator 4 does not absorb excessive lithium ions Li + Since the movement of lithium ions Li is suppressed, the lithium ions Li are distributed throughout the nonaqueous electrolyte solution 13 on the surface of the negative electrode mixture layer 22. + Therefore, the concentration of lithium ion Li + Therefore, the so-called high-rate deterioration can be suppressed.
[0033] 5 is a schematic diagram showing the state of the lithium ion secondary battery 1 during discharge according to this embodiment. When the lithium ion secondary battery 1 is discharged, electrons flow from the positive electrode connection portion 31a of the positive electrode plate 3 to the positive electrode current collector 31. Electrons are supplied from the positive electrode current collector 31 to the positive electrode active material 33. As a result, the lithium ions Li + is attracted to the positive electrode active material 33.
[0034] At this time, the separator 4 of this embodiment is deliberately made of lithium ions Li + The porosity SP [%] is limited to prevent the movement of lithium ions Li +cannot easily move from the negative electrode plate 2 side to the positive electrode plate 3 side.
[0035] On the other hand, it is desirable that the positive electrode mixture layer 32 of the positive electrode plate 3 contains a sufficient amount of positive electrode active material 33 in order to increase the battery capacity. However, the porosity PP [%] is adjusted to be higher than that of the separator 4. For this reason, during discharge, the separator 4 disperses lithium ions Li + Since the movement of lithium ions Li is suppressed, the lithium ions Li are released from the surface of the positive electrode mixture layer 32. + Therefore, the concentration of lithium ions Li in the entire nonaqueous electrolyte solution 13 does not increase excessively. + In this case, the high-rate degradation can be effectively suppressed.
[0036] <Configuration of this embodiment> The configuration of the lithium ion secondary battery 1 of this embodiment will be described in detail below.
[0037] (Configuration of lithium-ion secondary battery 1) First, an example of the overall configuration of the lithium ion secondary battery 1, which is the premise of this embodiment, and the configuration of the separator 4 will be briefly described.
[0038] FIG. 1 is a perspective view showing an outline of the configuration of a lithium ion secondary battery 1 of this embodiment. As shown in FIG. 1, the lithium ion secondary battery 1 is configured as a cell battery. The lithium ion secondary battery 1 includes a rectangular parallelepiped battery case 11 having an opening on the upper side. An electrode body 12 is housed inside the battery case 11. A nonaqueous electrolyte 13 is filled into the battery case 11 through a filling hole. The battery case 11 is made of a metal such as an aluminum alloy, and forms a sealed battery container. The lithium ion secondary battery 1 also includes a positive electrode external terminal 14 and a negative electrode external terminal 15 used for charging and discharging power. The shapes of the positive electrode external terminal 14 and the negative electrode external terminal 15 are not limited to those shown in FIG. 1.
[0039] <Electrode body 12> 2 is a schematic diagram showing the configuration of a wound electrode assembly 12. The electrode assembly 12 is formed by winding a large number of negative electrode plates 2 and positive electrode plates 3, with separators 4 arranged between them, flatly. The negative electrode plates 2 have a negative electrode composite layer 22 formed on a negative electrode current collector 21 that serves as a base material. A negative electrode connection part 21a where the negative electrode composite layer 22 is not formed and the negative electrode current collector 21 is exposed is provided on one end side in a width direction W (winding axis direction) perpendicular to the winding direction (winding direction L).
[0040] <Layer structure of electrode body 12> As shown in FIG. 2, the basic configuration of an electrode assembly 12 of a lithium ion secondary battery 1 includes a negative electrode plate 2, a positive electrode plate 3, and a separator 4.
[0041] The negative electrode plate 2 includes a negative electrode mixture layer 22 on both sides of a negative electrode current collector 21 serving as a negative electrode base material. One end of the negative electrode current collector 21 is a negative electrode connection portion 21a where the metal is exposed. The positive electrode plate 3 includes a positive electrode mixture layer 32 on both sides of a positive electrode current collector 31 serving as a positive electrode base material. The other end of the positive electrode current collector 31 is a positive electrode connection portion 31a where the metal is exposed.
[0042] The negative electrode plate 2 and the positive electrode plate 3 are stacked with a separator 4 interposed therebetween to form a laminate. This laminate is wound in the longitudinal direction around a winding axis, and formed into a flat wound electrode body 12.
[0043] <Nonaqueous electrolyte 13> As shown in FIG. 1, the nonaqueous electrolyte 13 is filled in a battery container formed by a battery case 11. The nonaqueous electrolyte 13 of the lithium ion secondary battery 1 is a composition in which a lithium salt is dissolved in an organic solvent. Examples of the lithium salt that can be used include LiClO4, LiPF6, LiAsF6, LiBF4, and LiSO3CF3. Examples of the organic solvent include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, and trifluoropropylene carbonate (F.PC), chain carbonates such as diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and dipropyl carbonate (DPC), ether compounds such as tetrahydrofuran (TFH), 2-methyltetrahydrofuran (2-MeTHF), and dimethoxyethane, sulfur compounds such as ethyl methyl sulfone and butane sultone, and phosphorus compounds such as triethyl phosphate and trioctyl phosphate. One or a mixture of two or more of these may be used as the nonaqueous electrolyte 13. The composition of the nonaqueous electrolyte 13 is not limited to these.
[0044] <Components of electrode body 12> Next, the negative electrode plate 2, the positive electrode plate 3, and the separator 4, which are the components that make up the electrode assembly 12, will be described.
[0045] In this embodiment, the "average diameter" refers to the median diameter (D 50 Average particle size (50% volume average particle size) refers to the average particle size in the range of approximately 1 μm or more, which can be determined by the laser diffraction / light scattering method. In addition, average particle size in the range of approximately 1 μm or less can be determined by the dynamic light scattering (DLS) method. The average particle size based on the DLS method can be measured in accordance with JIS Z 8828:2013.
[0046] <Negative electrode plate 2> The negative electrode plate 2 is constituted by forming a negative electrode mixture layer 22 on both sides of a negative electrode current collector 21, which is a negative electrode base material. In this embodiment, the negative electrode current collector 21 is made of Cu foil. The negative electrode current collector 21 serves as a base as an aggregate for the negative electrode mixture layer 22, and also has a function as a current collecting member that collects electricity from the negative electrode mixture layer 22. In this embodiment, the negative electrode active material 23 is a material capable of absorbing and releasing lithium ions, and a powdered carbon material made of graphite or the like is used.
[0047] The negative electrode plate 2 is formed, for example, by kneading the negative electrode active material 23, a solvent, and a binding material (binder), and applying the kneaded negative electrode mixture paste to the negative electrode current collector 21 and drying it to form the negative electrode mixture layer 22.
[0048] <Positive electrode plate 3> As shown in FIG. 2, the positive electrode plate 3 is composed of a positive electrode current collector 31 and a positive electrode mixture layer 32 applied thereto.
[0049] <Positive electrode current collector 31> A positive electrode mixture layer 32 is formed on both sides of a positive electrode current collector 31, which is a positive electrode base material, to form a positive electrode plate 3. In this embodiment, the positive electrode current collector 31 is made of aluminum foil. The positive electrode current collector 31 serves as a base for the aggregate of the positive electrode mixture layer 32, and also functions as a current collecting member that collects electricity from the positive electrode mixture layer 32.
[0050] Although the positive electrode base material constituting the positive electrode current collector 31 is exemplified by aluminum foil, it may be made of, for example, a conductive material made of a metal having good conductivity. As the conductive material, for example, a material containing aluminum or a material containing an aluminum alloy may be used. The configuration of the positive electrode current collector 31 is not limited to this.
[0051] <Positive electrode mixture layer 32> Positive electrode mixture layer 32 is formed by applying a positive electrode mixture paste to positive electrode current collector 31 and drying it. Positive electrode mixture layer 32 contains, in addition to positive electrode active material 33, additives such as a conductive material, a binding material (binder), and a dispersant.
[0052] <Composition of Positive Electrode Active Material 33> The particles of the positive electrode active material 33 contain a lithium transition metal oxide having a layered crystal structure, without being limited to those exemplified in the embodiment. The lithium transition metal oxide contains one or more predetermined transition metal elements in addition to Li. The transition metal element contained in the lithium transition metal oxide is preferably at least one of Ni, Co, and Mn. A suitable example of the lithium transition metal oxide is a lithium transition metal oxide containing all of Ni, Co, and Mn.
[0053] The positive electrode active material 33 may additionally contain one or more elements in addition to a transition metal element (i.e., at least one of Ni, Co, and Mn). Examples of the additional element of the positive electrode active material 33 include any element belonging to Group 1 (alkali metals such as sodium), Group 2 (alkaline earth metals such as magnesium and calcium), Group 4 (transition metals such as titanium and zirconium), Group 6 (transition metals such as chromium and tungsten), Group 8 (transition metals such as iron), Group 13 (metalloid element boron or metals such as aluminum), and Group 17 (halogens such as fluorine) of the periodic table.
[0054] <Binding material (binder)> The binder may be, for example, polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), polyacrylic acid, polyacrylate, or the like.
[0055] (Characteristic configuration of the lithium-ion secondary battery 1 according to the present embodiment) The basic configuration of the lithium ion secondary battery 1 of this embodiment includes an electrode body 12 in which a positive electrode plate 3 having a positive electrode mixture layer 32 and a negative electrode plate 2 having a negative electrode mixture layer 22 are stacked with a separator 4 interposed therebetween. The porosity PP of the positive electrode mixture layer 32 and the porosity NP of the negative electrode mixture layer 22 are both set higher than the porosity SP of the separator 4.
[0056] With this configuration, the lithium ion Li +The movement of lithium ions Li is rate-determined by the separator 4. That is, by setting the porosity PP of the positive electrode mixture layer 32 and the porosity NP of the negative electrode mixture layer 22 higher than the porosity SP of the separator 4, + The flow of lithium ions Li is governed by the flow speed in the separator 4. + It can suppress the movement of lithium ions (Li + It is possible to suppress the concentration bias.
[0057] <Porosity SP of separator 4> In this embodiment, the porosity SP of the separator 4 is adjusted to 42.15% or less. This is because, if the porosity SP is 42.15% or less, lithium ions Li + This is because it is possible to suppress the flow of lithium ions Li+ in the non-aqueous electrolyte solution 13 and thereby suppress the uneven distribution of lithium ions Li+ in the non-aqueous electrolyte solution 13.
[0058] The porosity SP of the separator 4 is preferably 39.54% or more. This is because the porosity SP of 39.54% or more prevents excessive lithium ion Li + This is to avoid impeding the passage of
[0059] <Porosity PP of Positive Electrode Mixture Layer 32> In this embodiment, the porosity PP of the positive electrode mixture layer 32 is adjusted to 44.16% or more. When the porosity PP is 44.16% or more, lithium ions Li + It is possible to effectively suppress the bias of the
[0060] It is preferable that the porosity PP of the positive electrode mixture layer 32 is 48.61% or less. This is because by setting the porosity PP to 48.61% or less, the battery capacity is not reduced more than necessary.
[0061] The density of the positive electrode mixture layer 32 is 2.9 [g / cm 3 The density of the positive electrode mixture layer 32 is 2.9 [g / cm 3 ] or less, a sufficient void ratio as described above can be ensured. The density of the positive electrode mixture layer 32 is 2.2 [g / cm 3 The density of the positive electrode mixture layer 32 is adjusted to 2.2 [g / cm 3 ] or more, sufficient battery capacity can be ensured.
[0062] <Porosity NP of negative electrode mixture layer 22> In this embodiment, the porosity NP of the negative electrode mixture layer 22 is adjusted to 45.38% or more. When the porosity NP is 45.38% or more, the lithium ion Li + It is possible to effectively suppress the bias of the
[0063] It is desirable that the porosity NP of the negative electrode mixture layer 22 is 49.68% or less. If the porosity NP of the negative electrode mixture layer 22 is 49.68% or less, a sufficient battery capacity can be achieved.
[0064] The density of the negative electrode mixture layer 22 is 1.2 [g / cm 3 The density of the negative electrode mixture layer 22 is 1.2 [g / cm 3 ] or less, sufficient porosity NP can be ensured. The density of the negative electrode mixture layer 22 is 0.9 [g / cm 3 The density of the negative electrode mixture layer 22 is adjusted to 0.9 [g / cm 3 ] or more will ensure sufficient capacity.
[0065] <Spring constant C of battery cell> First, the "spring constant C [kN / mm]" of the battery cell in this embodiment will be described. The "spring constant C [kN / mm]" in this embodiment is measured by the following procedure. First, the cell of the lithium ion secondary battery 1 on the stage is pressed in the thickness direction with a load of 9.8 [kN] by the load cell. Then, the load of the load cell is reduced to 4.5 [kN]. Then, the cell that was pressed with the load of 9.8 [kN] and crushed together with the electrode body 12 becomes thick again by the elastic force. The displacement at that time is defined as D [mm]. Then, the position of the load cell is fixed at this position and left for 600 [seconds]. Then, mainly due to the spring back of the electrode body 12 over time, the cell pushes back the load cell, and the load of the load cell whose position is fixed increases. The load of the load cell at this time is defined as L [kN]. Here, the spring constant C of the cell can be calculated by C=(9.8-x) / D. In the cell of the lithium ion secondary battery 1 of this embodiment, the strength is adjusted so as to satisfy C≦95.38 [kN / mm].
[0066] The spring constant C of the cell is set to 95.38 [kN / mm] or less for the following reason. When charging and discharging at a high rate, the thickness of the negative electrode mixture layer 22 changes in the lithium ion secondary battery 1. At this time, if the spring constant C is large, that is, if the electrode body 12 is hard, the nonaqueous electrolyte 13 cannot be stored inside the electrode body 12, and the lithium ions Li inside the electrode body 12 are dispersed due to the inflow and outflow of the nonaqueous electrolyte 13 to and from the outside of the electrode body 12. + On the other hand, if the spring constant C is 95.38 [kN / mm] or less, the electrode body 12 is flexible, the non-aqueous electrolyte 13 can be stored inside the electrode body 12, and a sudden inflow and outflow of the non-aqueous electrolyte 13 to the outside can be suppressed. + It is possible to suppress unevenness in density, which contributes to solving the problem of this embodiment, namely, suppressing high-rate deterioration.
[0067] It is preferable that the spring constant C is 84.96 kN / mm or more. If the spring constant C is 84.96 kN / mm or more, the cell can be made sufficiently hard. As a result, the stability of the battery module in which the cells are stacked in the thickness direction and the battery pack made of the battery module can be increased.
[0068] <Difference ΔP> The "difference ΔP" in this embodiment (also referred to as PPD-NPD porosity difference ΔP) will be described. The "difference ΔP" in this embodiment is calculated by the following procedure. First, the difference between the porosity PP of the positive electrode mixture layer 32 and the porosity SP of the separator 4 is defined as the PP-SP porosity difference PPD. Also, the difference between the porosity NP of the negative electrode mixture layer 22 and the porosity SP of the separator 4 is defined as the negative electrode porosity difference NPD. Then, the difference between the PP-SP porosity difference PPD and the NP-SP porosity difference NPD is defined as the difference ΔP. Here, the difference ΔP is calculated by: Difference ΔP = (PP-SP porosity difference PPD) - (NP-SP porosity difference NPD) =(Porosity PP-Porosity SP)-(Porosity NP-Porosity SP) = porosity PP - porosity NP That is, the difference ΔP is the difference between the porosity PP of the positive electrode mixture layer 32 and the porosity NP of the negative electrode mixture layer 22. If the difference ΔP is 0, it means that the porosity PP and the porosity NP are equal. In this embodiment, this difference ΔP is adjusted to be less than 4%. If this difference ΔP is less than 4% it is possible to make the difference in the porosity between the positive electrode mixture layer 32 and the separator 4 and the difference in the porosity between the negative electrode mixture layer 22 and the separator 4 nearly equal. With this configuration, the lithium ion Li is well balanced both during charging and discharging. + Suppresses the bias of lithium ion Li + Therefore, the high-rate degradation of the lithium-ion secondary battery 1 as a whole can be effectively suppressed.
[0069] <Method of manufacturing separator 4> An example of a method for producing the separator 4 having the above-mentioned characteristics will be described below. Note that the method for producing the lithium ion secondary battery 1 of the present invention is not limited to this embodiment.
[0070] The separator 4 is made of a thin film of polyolefin such as polyethylene (PE) or polypropylene (PP). In this embodiment, the separator 4 has a three-layer structure in which a positive electrode sheet and a negative electrode sheet made of PP are attached to both sides of a PE core sheet.
[0071] Each sheet is formed into a porous long piece, and is drawn out from a roll in the longitudinal direction and stretched in the longitudinal direction. It is also stretched in the direction perpendicular to the longitudinal direction. This biaxial stretching process expands the voids in the direction perpendicular to the longitudinal direction. The voids in the PP positive electrode sheet and negative electrode sheet on both sides of the PE core sheet can be adjusted in the stretching process to adjust the void ratio P [%]. Of course, the separator 4 can also be constructed as a single layer.
[0072] <Method of manufacturing the positive electrode plate 3> The positive electrode mixture layer 32 of the positive electrode plate 3 is manufactured by the following method. First, the positive electrode active material 33 and conductive material 34 to be mixed in the positive electrode mixture paste constituting the positive electrode mixture layer 32, as well as the binder, organic solvent, and additives, are kneaded together. At this time, the porosity PP [%] also changes depending on the type of conductive material 34 selected. In this embodiment, the conductive material 34 is selected from among those having a specific surface area BET of 150 to 300 [m 2 / g] of carbon nanotubes and carbon nanofibers are used. These form an effective conductive network even in small amounts, which can increase the porosity PP [%].
[0073] In addition, the porosity PP [%] is adjusted by adjusting the pressing pressure / speed after coating the positive electrode composite paste to control the density and thickness of the positive electrode composite layer 32. In this embodiment, the pressing pressure is 50 to 196 [kN], and the pressing speed is 6 to 60 [m / min].
[0074] <Method of Manufacturing Negative Electrode Plate 2> The negative electrode mixture layer 22 of the negative electrode plate 2 is manufactured by the following method. First, the negative electrode active material 23 and the conductive material 34 to be mixed in the negative electrode mixture paste constituting the negative electrode mixture layer 22, as well as the binder, organic solvent, and additives, are kneaded. At this time, the negative electrode mixture layer 22 of the negative electrode plate 2 is made into a slurry having a certain degree of blackness (amount of fine powder is controlled) by applying a shear force to a slurry containing graphite, a binder (SBR, SAR, etc.), and a thickener (CMC, etc.). The pressing pressure / speed after coating of the negative electrode mixture paste is adjusted to adjust the thickness and density of the negative electrode mixture layer 22 to adjust the porosity NP [%]. In this embodiment, the pressing pressure is 50 to 196 [kN], and the pressing speed is 6 to 60 [m / min].
[0075] (Experimental Example) <Experimental conditions> In the experiment, first, the porosity PP of positive electrode mixture layer 32, the porosity NP of negative electrode mixture layer 22, and the porosity SP of separator 4 of each test piece were measured.
[0076] "High-rate characteristics" were evaluated by the "high-rate degradation resistance increase rate [%]." The "high-rate degradation resistance increase rate [%]" is the increase rate [%] of internal resistance (CD-IR) after a charge-discharge cycle test in which charging and discharging at a large current (tens of amperes or more) is repeated for a certain period of time.
[0077] As a result of the experiment, the standard for "high rate characteristics" was 1.124 or less. This "high rate characteristics" was expressed as a "high rate characteristics index HI", with a standard of 1.000 when the high rate characteristics is 1.124. This "high rate characteristics index HI" made it possible to easily compare high rate characteristics.
[0078] “PP-SP porosity difference PPD” is a value indicating the difference between the porosity PP of positive electrode mixture layer 32 and the porosity SP of separator 4. “NP-SP porosity difference NPD” is a value indicating the difference between the porosity NP of negative electrode mixture layer 22 and the porosity SP of separator 4.
[0079] The "PPD-NPD porosity difference ΔP" is further a value indicating the "difference" between the "PP-SP porosity difference PPD" and the "NP-SP porosity difference NPD". If the spring constant C [kN / mm] is too high, the electrode body 12 becomes too stiff and it becomes difficult to store the nonaqueous electrolyte 13, which tends to cause high-rate deterioration. On the other hand, if the spring constant C [kN / mm] is too low, the stability decreases when the cells are stacked.
[0080] <Experiment evaluation criteria> The evaluation criteria for the experiment was the "high rate characteristic index HI." <Conditions and results of Examples 1 to 6 and Comparative Examples 1 to 6> In Example 1, the porosity PP of the positive electrode mixture layer 32 is 44.16%; the porosity NP of the negative electrode mixture layer 22 is 47.41%; and the porosity SP of the separator 4 is 41.49%. The high rate characteristic is 1.07, which is converted to a high rate characteristic index HI of 1.05.
[0081] The PP-SP porosity difference PPD, which is the difference between the porosity PP of positive electrode mixture layer 32 and the porosity SP of separator 4, is 2.67%. The NP-SP porosity difference NPD, which is the difference between the porosity NP of negative electrode mixture layer 22 and the porosity SP of separator 4, is 5.92%.
[0082] The PPD-NPD porosity difference ΔP, which is the difference between the PP-SP porosity difference PPD and the NP-SP porosity difference NPD, is 3.24%. The spring constant C at this time was 85.42 [kN / mm].
[0083] In Example 2, the porosity PP of the positive electrode mixture layer 32 is 44.16%; the porosity NP of the negative electrode mixture layer 22 is 47.41%; and the porosity SP of the separator 4 is 42.15%. The high rate characteristic is 1.08, and the high rate characteristic index HI is 1.04. The PP-SP porosity difference PPD is 2.01%; and the NP-SP porosity difference NPD is 5.26%. The PPD-NPD porosity difference ΔP is 3.24%. The spring constant C at this time was 84.96 kN / mm.
[0084] In Example 3, the porosity PP of the positive electrode mixture layer 32 is 43.42%; the porosity NP of the negative electrode mixture layer 22 is 45.38%; and the porosity SP of the separator 4 is 41.42%. The high rate characteristic is 1.08, and the high rate characteristic index HI is 1.04. The PP-SP porosity difference PPD is 2.00%; the NP-SP porosity difference NPD is 3.96%. The PPD-NPD porosity difference ΔP is 1.96%. The spring constant C at this time was 91.48 kN / mm.
[0085] In Example 4, the porosity PP of the positive electrode mixture layer 32 is 44.16%; the porosity NP of the negative electrode mixture layer 22 is 46.16%; and the porosity SP of the separator 4 is 39.88%. The high rate characteristic is 1.10, and the high rate characteristic index HI is 1.02. The PP-SP porosity difference PPD is 4.29%; and the NP-SP porosity difference NPD is 6.28%. The PPD-NPD porosity difference ΔP is 2.00%. The spring constant C at this time was 92.38 kN / mm.
[0086] In Example 5, the porosity PP of the positive electrode mixture layer 32 is 44.16%; the porosity NP of the negative electrode mixture layer 22 is 46.16%; and the porosity SP of the separator 4 is 39.54%. The high rate characteristic is 1.11, and the high rate characteristic index HI is 1.01. The PP-SP porosity difference PPD is 4.63%; and the NP-SP porosity difference NPD is 6.63%. The PPD-NPD porosity difference ΔP is 2.00%. The spring constant C at this time was 95.38 kN / mm.
[0087] In Example 6, the porosity PP of the positive electrode mixture layer 32 is 48.61%; the porosity NP of the negative electrode mixture layer 22 is 49.88%; and the porosity SP of the separator 4 is 42.02%. The high rate characteristic is 1.11, and the high rate characteristic index HI is 1.01. The PP-SP porosity difference PPD is 6.59%; and the NP-SP porosity difference NPD is 7.86%. The PPD-NPD porosity difference ΔP is 1.26%. The spring constant C at this time was 86.41 kN / mm.
[0088] In Comparative Example 1, the porosity PP of the positive electrode mixture layer 32 is 38.05%; the porosity NP of the negative electrode mixture layer 22 is 48.04%; and the porosity SP of the separator 4 is 41.64%. The high rate characteristic is 1.16, and the high rate characteristic index HI is 0.97. The PP-SP porosity difference PPD is -3.59%; and the NP-SP porosity difference NPD is 6.41%. The PPD-NPD porosity difference ΔP is 9.99%. The spring constant C at this time was 94.00 kN / mm.
[0089] In Comparative Example 2, the porosity PP of the positive electrode mixture layer 32 is 43.99%; the porosity NP of the negative electrode mixture layer 22 is 39.58%; and the porosity SP of the separator 4 is 41.05%. The high rate characteristic is 1.15, and the high rate characteristic index HI is 0.98. The PP-SP porosity difference PPD is 2.94%; and the NP-SP porosity difference NPD is -1.47%. The PPD-NPD porosity difference ΔP is 4.41%. The spring constant C at this time was 92.83 kN / mm.
[0090] In Comparative Example 3, the porosity PP of the positive electrode mixture layer 32 is 44.45%; the porosity NP of the negative electrode mixture layer 22 is 47.39%; and the porosity SP of the separator 4 is 48.15%. The high rate characteristic is 1.17, and the high rate characteristic index HI is 0.96. The PP-SP porosity difference PPD is -3.70%; and the NP-SP porosity difference NPD is -0.76%. The PPD-NPD porosity difference ΔP is 2.94%. The spring constant C at this time was 88.80 kN / mm.
[0091] In Comparative Example 4, the porosity PP of the positive electrode mixture layer 32 is 45.04%; the porosity NP of the negative electrode mixture layer 22 is 45.38%; and the porosity SP of the separator 4 is 46.41%. The high rate characteristic is 1.17, and the high rate characteristic index HI is 0.96. The PP-SP porosity difference PPD is -1.37%; and the NP-SP porosity difference NPD is -1.02%. The PPD-NPD porosity difference ΔP is 0.34%. The spring constant C at this time was 87.93 kN / mm.
[0092] In Comparative Example 5, the porosity PP of the positive electrode mixture layer 32 is 46.04%; the porosity NP of the negative electrode mixture layer 22 is 46.12%; and the porosity SP of the separator 4 is 49.30%. The high rate characteristic is 1.34, and the high rate characteristic index HI is 0.84. The PP-SP porosity difference PPD is -3.26%; and the NP-SP porosity difference NPD is -3.18%. The PPD-NPD porosity difference ΔP is 0.08%. The spring constant C at this time was 98.48 kN / mm.
[0093] <Summary of the experiment> High rate characteristic index HI The above experiments lead to the following. The present invention is first evaluated by the high-rate performance index HI. In the table shown in Fig. 6, Examples 1 to 3 marked with ● all had particularly good results with a high-rate performance index HI of 1.05 to 1.04. Examples 4 to 6 marked with ◯ all had the next best high-rate performance index HI of 1.02 to 1.01.
[0094] On the other hand, Comparative Examples 1 and 2, indicated by ▲, had a high rate performance index HI of 0.97 to 0.98, which was somewhat low. Furthermore, Comparative Examples 3 to 5, indicated by △, had a high rate performance index of 0.84 to 0.96, which was found to have been significantly deteriorated.
[0095] -Porosity SP, porosity PP, and porosity NP First, a common condition among Examples 1 to 6 is that the porosity PP of the positive electrode mixture layer 32 and the porosity NP of the negative electrode mixture layer 22 are set higher than the porosity SP of the separator 4. On the other hand, in Comparative Examples 1 to 5, the porosity PP of the positive electrode mixture layer 32 and the porosity NP of the negative electrode mixture layer 22 are set lower than the porosity SP of the separator 4. For this reason, as analyzed by the present inventors, it is derived that setting the porosity PP of the positive electrode mixture layer 32 and the porosity NP of the negative electrode mixture layer 22 higher than the porosity SP of the separator 4 is a condition for suppressing high-rate degradation.
[0096] Porosity of the positive electrode mixture layer 32 PP It was found that when the porosity PP of the positive electrode mixture layer 32 in Examples 1 to 6 was in the range of 44.16 to 48.61%, the high rate characteristic index was good, and the porosity PP of the positive electrode mixture layer 32 was preferably in the range of 44.16 to 48.61%.
[0097] Porosity NP of the negative electrode mixture layer 22 It was found that the high rate characteristic index was good when the porosity PP of the negative electrode mixture layer 22 in Examples 1 to 6 was in the range of 45.38 to 49.68%, and the porosity PP of the positive electrode mixture layer 32 was preferably in the range of 45.38 to 49.68%.
[0098] Separator 4 porosity SP It was found that the separators 4 in Examples 1 to 6 had good high rate characteristic indexes when the porosity SP was in the range of 39.54 to 42.15% and that the porosity SP of the separator 4 was preferably in the range of 39.54 to 42.15%.
[0099] ·Difference ΔP It was found that in Examples 1 to 6, the difference ΔP was in the range of 1.26 to 3.24% and the high rate characteristic index was good, and the difference ΔP was preferably in the range of 1.26 to 3.24%.
[0100] Spring constant C The spring constants C [kN / mm] of Examples 1 to 6 were in the range of 84.96 to 95.38 [kN / mm]. It was found that the spring constant C is preferably in the range of 84.96 to 95.38 [kN / mm].
[0101] (Action of this embodiment) The lithium ion secondary battery 1 of this embodiment has the following function. As shown in FIG. 4, when the lithium ion secondary battery 1 is charged, electrons are supplied from the negative electrode current collector 21 to the negative electrode active material 23. Then, the lithium ions Li + is attracted to the negative electrode active material 23.
[0102] At this time, the separator 4 of this embodiment is deliberately made of lithium ions Li + The porosity SP [%] is low so as to inhibit the movement of lithium ions Li + The lithium ions Li cannot easily move from the positive electrode plate 3 to the negative electrode plate 2. + The movement of lithium ions Li is rate-determined by the separator 4. + Since the movement of lithium ions Li is suppressed, the lithium ions Li are distributed throughout the nonaqueous electrolyte solution 13 on the surface of the negative electrode mixture layer 22. + Therefore, the concentration of lithium ion Li + Therefore, the so-called high-rate deterioration can be suppressed.
[0103] As shown in FIG. 5, during discharge, the separator 4 also transports lithium ions Li + Since the movement of lithium ions Li is suppressed, the lithium ions Li are released from the surface of the positive electrode mixture layer 32. + Therefore, the concentration of lithium ions Li in the entire nonaqueous electrolyte solution 13 does not increase excessively. + In this case, the high-rate degradation can be effectively suppressed.
[0104] In the lithium ion secondary battery 1 of this embodiment, the lithium ions Li are well balanced both during charging and discharging. + Lithium ion Li + Furthermore, by appropriately adjusting the spring constant C, the lithium ion Li in the nonaqueous electrolyte 13 can be prevented from being biased. + As a result, high-rate deterioration of the lithium-ion secondary battery 1 can be suppressed even during high-rate charging and discharging.
[0105] (Effects of this embodiment) (1) The lithium ion secondary battery of the present embodiment has the effect of suppressing high-rate degradation.
[0106] (2) The porosity PP of the positive electrode mixture layer 32 and the porosity NP of the negative electrode mixture layer 22 are set higher than the porosity SP of the separator 4. For this reason, the lithium ions Li + This has the effect of suppressing bias in the
[0107] (3) The difference ΔP between the PP-SP porosity difference PPD between the porosity PP of the positive electrode mixture layer 32 and the porosity SP of the separator 4 and the NP-SP porosity difference NPD between the porosity NP of the negative electrode mixture layer 22 and the porosity SP of the separator 4 is set to 4% or less. + Lithium ion Li + This has the effect of enabling the distribution of
[0108] (4) The PP-SP porosity difference PPD is set to 2.00 to 6.59%. Therefore, the lithium ions Li are distributed in a well-balanced manner in the positive electrode plate 3. + Lithium ion Li + This has the effect of enabling the distribution of
[0109] (5) The NP-SP porosity difference NPD is set to 3.96 to 7.86%. Therefore, lithium ions Li are distributed in a well-balanced manner in the negative electrode plate 2. + Lithium ion Li + This has the effect of enabling the distribution of
[0110] (6) The porosity SP of the separator 4 is set to 42.15% or less. Therefore, the lithium ion Li + This has the effect of suppressing bias in the (7) The porosity SP of the separator 4 is set to 39.54% or more. This allows the lithium ions Li to flow smoothly through the negative electrode plate 2. + This has the effect of enabling the distribution of
[0111] (8) The porosity PP is set to 44.16% or more. Therefore, the positive electrode plate 3 is charged with lithium ions Li + This has the effect of suppressing bias in the (9) The porosity PP is set to 48.61% or less, which has the effect of ensuring sufficient battery capacity.
[0112] (10) The porosity NP is set to 45.38% or more. Therefore, the lithium ion Li + This has the effect of suppressing bias in the (11) The porosity NP is set to 49.68% or less, which has the effect of ensuring sufficient battery capacity.
[0113] (12) The density of the positive electrode mixture layer 32 is set to 2.9 [g / cm 3 This has the effect of providing a sufficient porosity in positive electrode mixture layer 32. (13) The density of the positive electrode mixture layer 32 is set to 2.2 [g / cm 3 This has the effect of providing a sufficient battery capacity.
[0114] (14) The density of the negative electrode mixture layer 22 is set to 1.2 [g / cm3 This has the effect of providing a sufficient porosity in negative electrode mixture layer 22. (15) The density of the negative electrode mixture layer 22 is set to 0.9 [g / cm 3 This has the effect of providing a sufficient battery capacity.
[0115] (16) The cell of the lithium ion secondary battery 1 was pressed in the thickness direction with a load cell of 9.8 [kN], and then the load of the load cell was set to 4.5 [kN]. The displacement at that time was set to D [mm], and the load of the load cell when the position of the load cell was fixed and left for 600 [seconds] was set to L [kN]. When the spring constant C [kN / mm] of the cell is C = (9.8-x) / D, C ≦ 95.38 [kN / mm]. This has the effect of making it difficult for uneven concentration of the nonaqueous electrolyte 13 to occur during charging and discharging.
[0116] (17) The spring constant C is set to C≧80.96 [kN / mm]. This has the effect of increasing stability when the lithium-ion secondary battery 1 cells are stacked or assembled into a battery pack.
[0117] (18) While adjusting the spring constant C, the porosity PP of the positive electrode mixture layer 32 and the porosity NP of the negative electrode mixture layer 22 are set higher than the porosity SP of the separator 4. This increases the degree of freedom in setting the values of both, resulting in an effect of improving productivity.
[0118] (Modification) The above embodiment is an example of the present invention, and the present invention can be modified as follows.
[0119] Porosity P [%] and density [g / cm 3 The manufacturing methods such as the preparation of the above-mentioned compound are merely illustrative examples, and the practice of the present invention is not limited thereto. In this embodiment, the lithium ion secondary battery 1, which is a plate-shaped cell battery for vehicle use, is exemplified as an example of a non-aqueous electrolyte secondary battery, but the present invention is not limited to this, and other shapes such as a cylindrical shape and other uses such as stationary use are also possible. The electrode body 12 is also not limited to a flat wound type, and may be a laminate of rectangular plate-shaped electrodes. The shapes of the positive electrode external terminal 14 and the negative electrode external terminal 15 are also not limited.
[0120] The drawings are schematic diagrams used to explain the present embodiment, and numbers may be omitted or dimensional balance may be exaggerated for ease of viewing, so the drawings are not limited to these.
[0121] The various numerical values and ranges in the embodiments are merely examples and can be optimized and implemented by those skilled in the art. The compositions and material properties of the positive electrode mixture layer 32 and the negative electrode mixture layer 22 are merely examples of the present invention and can be optimized by those skilled in the art.
[0122] The present embodiment is one embodiment of the present invention, and it goes without saying that those skilled in the art can add, delete, or modify the configuration without being limited to the embodiment, as long as it does not deviate from the scope of the claims. [Explanation of symbols]
[0123] P[%]…Porosity PP [%]…Porosity (of the positive electrode composite layer) NP [%]…Porosity (of negative electrode composite layer) SP [%]...(separator) porosity HI...High rate characteristic index PPD[%]…(=PP-SP) Positive electrode porosity difference NPD[%]…(=NP-SP) negative electrode porosity difference ΔP[%]…(=PPD-NPD porosity difference) difference C [kN / mm]…Spring constant 1, 101...Lithium-ion secondary battery (cell) 11…Battery case 12...Electrode body 13...Nonaqueous electrolyte 14…Positive external terminal 15...Negative external terminal 2...Negative electrode plate 21...Negative electrode current collector 21a...Negative electrode connection part 22...Negative electrode composite material layer 23...Negative electrode active material 3…Positive electrode plate 31...Positive electrode current collector 31a…Positive electrode connection part 32...Positive electrode mixture layer 33...Cathode active material 34...Conductive material 4, 104…Separator
Claims
1. The battery includes an electrode assembly in which a positive electrode plate having a positive electrode mixture layer and a negative electrode plate having a negative electrode mixture layer are stacked with a separator interposed therebetween; A lithium ion secondary battery comprising: a positive electrode mixture layer having a porosity PP and a negative electrode mixture layer having a porosity NP that is higher than a porosity SP of the separator.
2. The lithium ion secondary battery according to claim 1, characterized in that a difference ΔP between a difference PPD between the porosity PP of the positive electrode mixture layer and the porosity SP of the separator and a difference NPD between the porosity NP of the negative electrode mixture layer and the porosity SP of the separator is 4% or less.
3. 3. The lithium ion secondary battery according to claim 2, wherein the difference PPD is 2.00 to 6.59%.
4. 3. The lithium ion secondary battery according to claim 2, wherein the difference NPD is 3.96 to 7.86%.
5. 2. The lithium ion secondary battery according to claim 1, wherein the separator has a porosity SP of 42.15% or less.
6. 6. The lithium ion secondary battery according to claim 5, wherein the separator has a porosity SP of 39.54% or more.
7. 2. The lithium ion secondary battery according to claim 1, wherein the positive electrode mixture layer has a porosity PP of 44.16% or more.
8. 8. The lithium ion secondary battery according to claim 7, wherein the positive electrode mixture layer has a porosity PP of 48.61% or less.
9. 2. The lithium ion secondary battery according to claim 1, wherein the negative electrode mixture layer has a porosity NP of 45.38% or more.
10. 10. The lithium ion secondary battery according to claim 9, wherein the negative electrode mixture layer has a porosity NP of 49.68% or less.
11. The density of the positive electrode mixture layer is 2.9 [g / cm 3 2. The lithium ion secondary battery according to claim 1, wherein the capacitance is equal to or less than 1.
12. The density of the positive electrode mixture layer is 2.2 [g / cm 3 12. The lithium ion secondary battery according to claim 11, wherein the capacitance is equal to or greater than 1.
13. The density of the negative electrode mixture layer is 1.2 [g / cm 3 2. The lithium ion secondary battery according to claim 1, wherein the capacitance is equal to or less than 1.
14. The density of the negative electrode mixture layer is 0.9 [g / cm 3 14. The lithium ion secondary battery according to claim 13, wherein the capacitance is equal to or greater than 1.
15. The lithium ion secondary battery according to claim 1, characterized in that, when a cell of the lithium ion secondary battery is pressed in a thickness direction by a load cell with a load of 9.8 [kN], and then the load of the load cell is set to 4.5 [kN], the displacement amount at that time is denoted as D [mm], the load of the load cell when the position of the load cell is fixed and left for 600 [seconds] is denoted as L [kN], and the spring constant C [kN / mm] of the cell is C = (9.8 - x) / D, C ≦ 95.38 [kN / mm].
16. 16. The lithium ion secondary battery according to claim 15, wherein the spring constant C satisfies C≧80.96 [kN / mm].
Citation Information
Patent Citations
Nonaqueous electrolyte secondary battery
JP2001223029A
Nonaqueous electrolyte secondary battery
JP2015167065A
Lithium ion secondary battery
JP2017111894A
Non-aqueous electrolyte secondary battery
JP2021153014A
Nonaqueous electrolyte secondary battery
JP2014120214A