Heat exchanger plate and heat exchanger comprising the same
Applying a fluorine-based film of 50 μm to 250 μm thickness on heat exchanger plates exposed to chromic acid solutions addresses corrosion issues, enhancing their durability and reducing replacement frequency.
Patent Information
- Application Number
- JP2023073774
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2024-11-08
AI Technical Summary
Heat exchanger plates exposed to chromic acid solutions corrode quickly due to temperature changes and flow rate variations, leading to frequent replacements, as existing acid-resistant films do not provide sufficient corrosion resistance.
A heat exchanger plate with a fluorine-based film of 50 μm to 250 μm thickness is applied to the surface of a metal base material, ensuring complete coverage and preventing contact with the chromic acid solution.
The fluorine-based film significantly extends the life of the heat exchanger plates by preventing corrosion, even under frequent temperature and flow rate changes, reducing the need for replacements.
Smart Images

Figure 2024158517000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a heat exchanger plate that is exposed to a chromic acid liquid, and a heat exchanger including the same. [Background technology]
[0002] A heat exchanger having an acid-resistant coating provided on the inner surface of a stainless steel tubular member in a refrigerant circuit has been disclosed (see, for example, Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] WO2020 / 040158 publication Summary of the Invention [Problem to be solved by the invention]
[0004] The heat exchanger may be provided in a plating device for chrome plating a base material. In this case, the heat exchanger heats a chromic acid solution, which is a strong acid, to about 50°C. The heat exchanger is provided with a plurality of metal heat exchanger plates, which are directly exposed to the chromic acid solution. For this reason, the heat exchanger plates exposed to the chromic acid solution are easily corroded by the chromic acid solution and are replaced at relatively short intervals due to corrosion. In particular, in an environment where the heating operation of the chromic acid solution by the heat exchanger is frequently turned on and off, the heat exchanger plate is subjected to a large load due to temperature changes and changes in the flow rate of the chromic acid solution. As a result, the deterioration of the heat exchanger plate becomes even faster, and frequent replacement of the heat exchanger plate is required. Therefore, it is considered to apply a corrosion prevention plating to the base material of the heat exchanger plate. However, even if a plating film is formed on the base material of the heat exchanger plate, sufficient corrosion resistance cannot be obtained. In addition, it cannot be said that Patent Document 1 takes into consideration the heat exchanger plate in an environment where it is exposed to a chromic acid solution, which is a strong acid solution.
[0005] In view of the above background, an object of the present invention is to extend the life of a heat exchanger plate exposed to a highly acidic chromic acid solution. [Means for solving the problem]
[0006] The present invention relates to the following heat exchanger plate and a heat exchanger including the same.
[0007] (1) A heat exchanger plate exposed to a chromic acid solution, A base material having a surface formed of metal; A fluorine-based coating having a thickness of 50 μm to 250 μm formed on the surface of the base material; A heat exchanger plate comprising:
[0008] (2) The heat exchanger plate according to (1) above, which is used to heat the chromic acid liquid to a temperature set in the range of 30°C to 60°C.
[0009] (3) A heat exchanger including a plurality of heat exchanger plates according to (1) or (2), A heat exchanger, wherein the heat exchanger plates are positioned by being pressed against each other in an arrangement direction of the heat exchanger plates. Effect of the Invention
[0010] According to the present invention, the life of heat exchanger plates exposed to highly acidic chromic acid solutions can be extended. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic diagram of a heat exchanger according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic front view of a heat exchanger plate. [Diagram 3]Fig. 3(A) is a schematic cross-sectional view of a comparative example showing a configuration in which the coating is less than 50 μm thick and the base material is not completely covered with the coating, and Fig. 3(B) is a schematic cross-sectional view of an enlarged portion of a heat exchanger plate having a coating thickness of 50 μm or more. [Figure 4] Fig. 4(A) is a graph showing the cumulative corrosion weight loss of Comparative Examples 1 to 8 and Invention Example 1. Fig. 4(B) is a graph showing the cumulative corrosion weight loss of Comparative Examples 9 and 10 and Invention Examples 2 to 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.
[0013] FIG. 1 is a schematic diagram of a heat exchanger 1 according to one embodiment of the present invention. The heat exchanger 1 of this embodiment is provided in a plating apparatus. The plating apparatus is an apparatus for forming a chromium plating film on the surface of an object to be plated, such as a roll. The heat exchanger 1 is a heater, and uses a medium such as steam to heat a chromium plating solution (chromic acid solution), which is a fluid to be heated, to a temperature set within a range of, for example, about 30°C to 60°C, for example, to 50°C. The chromium plating solution circulates between the heat exchanger 1 and a plating tank (not shown).
[0014] The chromium plating solution is a strong acid solution whose main components are chromic anhydride and sulfuric acid. The chromium plating solution used for trivalent chromium plating is a strong acid solution with a pH of about 2.0 to 4.0, and the chromium plating solution used for hexavalent chromium plating is an even stronger acid solution with a pH of 1.0 or less. Note that other chromic acid solutions may be used instead of the chromium plating solution.
[0015] The heat exchanger 1 includes a box-shaped case 2 (only a portion of which is shown in FIG. 1), a plurality of heat exchanger plates 10 housed in the case 2 and exposed to a chrome plating solution, and a medium pipe 3 and a chrome plating solution pipe 4 extending from the inside to the outside of the case 2.
[0016] The heat exchanger plates 10 are arranged in a predetermined arrangement direction. For example, the upper and lower parts of the heat exchanger plates 10 are fixed to each other using fixing members such as male and female screw members (not shown), and are pressed against each other in the arrangement direction of the heat exchanger plates 10 to position them. Two adjacent heat exchanger plates 10 may be in direct contact with each other, or may face each other with a spacer (not shown) sandwiched therebetween. By fixing the heat exchanger plates 10 to each other, an axial force along the arrangement direction (left and right direction in FIG. 1) is applied to the parts of each heat exchanger plate 10 that are fastened by the fixing members. Each heat exchanger plate 10 has the same configuration.
[0017] FIG. 2 is a schematic front view of the heat exchanger plate 10. As shown in FIG. 2, the heat exchanger plate 10 has an uneven shape formed on the surface, and is configured to have a larger contact area with the chrome plating solution to ensure heat exchange performance. The specific shape of the unevenness on the surface of the heat exchanger plate 10 is not limited. The heat exchanger plate 10 has, for example, four through holes 10a, 10b, 10c, and 10d formed therein. The through holes 10a and 10b are through holes through which the medium pipe 3 is passed, for example. The through holes 10c and 10d are through holes through which the chrome plating solution pipe 4 is passed, or through which the chrome plating solution passes between the case 2 and the space partitioned by the multiple heat exchanger plates 10. The medium pipe 3 is connected to a steam generator or a condenser, not shown. The chrome plating solution pipe 4 is connected to a plating tank, not shown.
[0018] Fig. 3(A) is a schematic cross-sectional view of a comparative example showing a configuration in which the thickness t' of the coating 12' is less than 50 µm and the base material 11' is not completely covered by the coating 12'. Fig. 3(B) is a schematic cross-sectional view in which a part of a heat exchanger plate 10 in which the thickness t of the coating 12 is 50 µm or more is enlarged.
[0019] As shown in FIG. 2 and FIG. 3(B), the heat exchanger plate 10 includes a base material 11 and a coating 12 formed on the entire surface 11a of the base material 11.
[0020] The base material 11 is formed of a material having excellent thermal conductivity, and is composed of metal or the like. The base material 11 is made of metal from the viewpoint of thermal conductivity, and is easily corroded when exposed to a chrome plating acid solution. Examples of the base material 11 include steel materials such as stainless steel and carbon steel. Examples of stainless steel include SUS316, SUS316L, and SUS430. Examples of carbon steel include rolled steel materials for general structure such as SS400, and carbon steel materials for machine structure such as S45C. In this embodiment, the base material 11 is SUS316. The plate thickness of the base material 11 is about 0.2 mm to 1.0 mm, and in this embodiment, it is 0.5 mm.
[0021] The coating 12 is formed on the surface 11a (outer surface) of the base material 11, and covers the entire surface 11a of the base material 11 without any gaps, thereby preventing the base material 11 from coming into contact with the chrome plating solution. The coating 12 is made of a material with excellent chemical resistance, thereby suppressing corrosion of the base material 11. The coating 12 is a fluorine-based coating. Examples of materials (fluorine resins) for the fluorine-based coating include fluorine resins such as PFA (perfluoroalkoxyalkane), PTFE (polytetrafluoroethylene), FEP (tetrafluoroethylene-hexafluoropropylene copolymer), ETFE (ethylene-tetrafluoroethylene copolymer), PCTFE (polychlorotrifluoroethylene), ECTFE (ethylene-chlorotrifluoroethylene copolymer), and PVDF (polyvinylidene fluoride). Other examples include materials in which fluorine resins are mixed with heat-resistant resins such as epoxy resins, PAI (polyamideimide) resins, and PES (polyethersulfone) resins, and fluorine rubber.
[0022] Among these fluororesins, PFA has good fluidity at temperatures equal to or higher than its melting point (approximately 310°C), and can spread more tightly on the base material 11 when the fluororesin film 12 is formed on the base material 11. This makes it possible to prevent breaks in the film 12 from occurring on the base material 11, and more reliably prevents the chrome plating solution from reaching the base material 11 through the breaks. PTFE has strong chemical resistance and is less corroded by the chrome plating solution. FEP has a lower melting point and continuous use temperature than PTFE, while having the same chemical resistance as PTFE. As a result, like PFA, FEP can spread more tightly on the base material 11 when the fluororesin film is formed on the base material 11. ETFE has good fluidity at temperatures equal to or higher than its melting point (approximately 270°C), and can spread more tightly on the base material 11 when the fluororesin film is formed on the base material 11. Materials made by mixing fluororesin with heat-resistant resins such as PCTFE, ECTFE, PVDF, epoxy resin, PAI resin, and PES resin, and fluororubber have strong chemical resistance and are less corroded by chrome plating solutions. As described above, from the viewpoint of moldability, it is preferable to use PFA, FEP, and ETFE as the coating material for fluororesins, and PFA is particularly preferable.
[0023] The thickness t of the fluororesin coating 12 is set to 50 μm to 250 μm. The coating 12 is formed, for example, by heating the fluororesin that is the material of the coating 12 to a melting point or higher to make it fluid, and exposing the fluidized fluororesin to the base material 11. At this time, the fluororesin is formed on the base material 11 at a thickness of several tens of μm at a time. Therefore, when the thickness t is to be greater than the thickness that can be formed at one time, a coating is first formed on the base material 11, and after this coating is fixed to the base material 11, the fluidized fluororesin is further layered on the coating fixed to the base material 11. By repeating this operation, the coating 12 of the desired thickness t can be formed.
[0024] The comparative example in FIG. 3(A) typically illustrates a configuration in which the film formation operation is performed twice to form the coating 12 with a two-layer structure, while the embodiment in FIG. 3(B) typically illustrates a configuration in which the film formation operation is performed four times to form the coating 12 with a four-layer structure.
[0025] As shown in FIG. 3(A), in the heat exchanger plate 10', if the thickness t' of the coating 12' is less than the above-mentioned lower limit, the coating 12' cannot be formed evenly over the entire surface 11a' of the base material 11', and minute through holes 12a' are present in the coating 12'. Therefore, the chromium plating solution passes through the through holes 12a' to reach the surface 11a' of the base material 11', and the base material 11' is eroded by the chromium plating solution, resulting in a corroded portion 13'. If the thickness t' is less than the above-mentioned lower limit, some of the multiple minute holes 12b formed in each film formation operation are formed at the overlapping portions of the base material 11' in a plan view, resulting in a portion of the base material 11' that is not covered by the coating 12'. As described above, this portion is eroded and corroded by the chromium plating solution.
[0026] On the other hand, as shown in the present embodiment in FIG. 3(B), when the thickness t of the coating 12 is equal to or greater than the above-mentioned lower limit, the coating 12 can be formed evenly over the entire surface 11a of the base material 11, and the coating 12 can be formed without through holes penetrating in the thickness direction of the coating 12. Therefore, the chrome plating solution does not reach the surface 11a of the base material 11, and the base material 11 is not eroded or corroded by the chrome plating solution. When the thickness t is equal to or greater than the above-mentioned lower limit, the multiple microholes 12b formed in each film formation operation are not formed in overlapping areas of the base material 11 in a plan view, and no part of the base material 11 is not covered by the coating 12. That is, the entire surface 11a of the base material 11 is covered by the coating 12 without any gaps even microscopically.
[0027] On the other hand, if the thickness t of the coating 12 exceeds the above upper limit, it becomes difficult to form the coating 12 on the base material 11 in terms of manufacturing. As described above, the coating 12 is formed on the base material 11 by, for example, repeating the coating operation multiple times. However, as the number of times of the coating operation increases, air bubbles are generated in the coating material during the coating operation, and these air bubbles cause the above-mentioned through holes 12a to be generated. In addition, the coating 12, which has a lower thermal conductivity than the base material 11, becomes too thick, and the efficiency of heat conduction from the medium (steam) to the chrome plating solution by the heat exchanger plate 10 decreases. For this reason, when the heat exchanger plate 10 of this embodiment is adopted instead of a heat exchanger plate made of only the base material 11 and not having the coating 12 formed thereon, it becomes necessary to increase the number of heat exchanger plates 10. Furthermore, if the thickness t of the coating 12 exceeds the above upper limit, when an axial force (a force pressing the heat exchanger plates 10 together) that fastens the heat exchanger plates 10 together with a fixing member (not shown) acts on a part of the heat exchanger plates 10, a load that distorts the coating 12 acts on the boundary between the part of the heat exchanger plate 10 to which the axial force acts and the part to which it does not act. For this reason, if the coating 12 is too thick, there is a risk that the coating 12 will crack at the above boundary.
[0028] The lower limit of the thickness t of the coating 12 is preferably 50 μm, 75 μm, 100 μm, or 150 μm. The upper limit of the thickness t is preferably 300 μm, 250 μm, or 200 μm. The thickness t of the coating 12 may be, for example, 50 μm to 250 μm, or preferably 100 μm to 200 μm.
[0029] As described above, according to this embodiment, by forming a fluorine-based coating having a thickness t of 50 μm to 250 μm on the surface 11a of the base material 11, the surface 11a can be covered with the coating 12 without any gaps. Therefore, the chromium plating solution is reliably prevented from contacting the base material 11, and corrosion of the base material 11 can be prevented for a long period of time.
[0030] Furthermore, even when the heat exchanger 1 is a heater that heats a chrome plating solution, the use of the coating 12 formed from a fluororesin having excellent heat resistance can more reliably suppress corrosion of the heat exchanger plate 10.
[0031] Furthermore, even if multiple heat exchanger plates 10 are positioned by being pressed against each other, the thickness t of the coating 12 is not too large, so that the coating 12 is prevented from cracking due to the above-mentioned pressing force.
[0032] The embodiment of the present invention has been described above. However, the present invention is not limited to the above embodiment. Various modifications of the present invention are possible within the scope of the claims.
[0033] In the above embodiment, the heat exchanger 1 is used as a heater, but it may also be used as a cooler. EXAMPLES
[0034] (Preparation of Comparative Examples 1 to 8 and Invention Example 1) As the base materials, rectangular plates of SUS316 and SUS316L were prepared. Comparative Example 1 was made of SUS316 and no coating was formed. Comparative Example 2 was made of SUS316L and no coating was formed.
[0035] For Comparative Examples 3 to 8 and Invention Example 1, coatings shown in Table 1 below were formed on the surface of the base material SUS316. In Table 1, the "Type of Coating" column lists the details of the coating. The "Characteristics of Coating" column lists the main characteristics of the coating. The "Film Thickness" column lists the thickness of the coating. If there is a range for the thickness, it means that the thickness is within the range listed. The "Coating Method" column lists the method for forming the coating. The "Processing Temperature" column shows the temperature of the coating material when the coating is formed.
[0036] [Table 1]
[0037] (Experimental and Evaluation Methods) For each of Comparative Examples 1 to 8 and Example 1 of the invention, a corrosion resistance test was conducted by immersing the plate in a tank of chrome plating solution (pH 0.12) maintained at approximately 80°C by a heater. The chrome plating solution is mainly composed of sulfuric acid and chromic anhydride. Since the heat exchanger plate is actually used at approximately 60°C or less, the corrosion resistance test was accelerated by heating the plate to 80°C. In the corrosion resistance test, the weight of each of Comparative Examples 1 to 8 and Example 1 of the invention was measured on a scale four times every week from the start of immersion, and the weight loss per unit area due to corrosion from before the test was calculated as the cumulative corrosion weight loss. In Comparative Examples 6 and 8, the cumulative corrosion weight loss increased rapidly, so the test was completed in two weeks.
[0038] The "Evaluation" column shows the evaluation results for each of Comparative Examples 1 to 8 and Invention Example 1. The cumulative corrosion weight loss after 4 weeks from the start of the test was 100 g / m 2 In addition, the cumulative corrosion loss after 4 weeks from the start of the test was 10 g / m 2 The following cases were rated as .
[0039] FIG. 4(A) is a graph showing the cumulative corrosion weight loss of Comparative Examples 1 to 8 and Example 1 of the invention. FIG. 4(A) shows the trend line of the cumulative corrosion weight loss measured every week for Comparative Examples 1 to 8 and Example 1 of the invention. As shown in Table 1 and FIG. 4(A), in Comparative Examples 1 to 8, weight loss due to corrosion of the base material clearly occurred over time, and in Comparative Examples 3 to 8, the base material could not be isolated from the chrome plating solution by the coating, resulting in the need to replace the heat exchanger plate early. More specifically, it was found that the base material had no resistance in Comparative Examples 1 and 2. In Comparative Examples 3 to 5, the coating had no resistance to the chrome plating solution, resulting in damage to the coating itself. In Comparative Example 6, the fluororesin coating had minute through-holes, which allowed the chrome plating solution to reach the base material through the through-holes, resulting in corrosion of the base material by the chrome plating solution. In Comparative Examples 7 and 8, the ceramic coating had voids, which allowed the chromium plating solution to penetrate the ceramic coating and reach the base material, resulting in corrosion of the base material by the chromium plating solution. On the other hand, in Invention Example 1, the coating was formed to a sufficient thickness, so that the micropores generated during coating formation did not become through-holes, and the coating completely covered the base material. Therefore, regardless of the passage of time, the coating prevented the chromium plating solution from reaching the base material, and no weight loss occurred in the base material, proving that replacement of the heat exchanger plate is unnecessary for a long period of time.
[0040] (Preparation of Comparative Examples 9 and 10 and Invention Examples 2 to 4) A rectangular plate of SS400 carbon steel was prepared as the base material. In both Comparative Examples 9 and 10 and Examples 2 to 4 of the invention, PFA, a fluororesin, was formed on the surface of the base material. The coating was made into a multi-layer coating by repeating a process of immersing the base material in molten PFA multiple times. Then, for each of Comparative Examples 9 and 10 and Examples 2 to 4 of the invention, the thickness of the coating was adjusted by cutting the PFA. The thicknesses of the coatings in Comparative Examples 9 and 10 and Examples 2 to 4 of the invention are as follows. The thicknesses of the coatings were measured with a thickness meter (SWT9200 manufactured by Sanko Electronics Laboratory). For each of Comparative Examples 9 and 10 and Examples 2 to 4 of the invention, the thickness of the coating was measured at one point selected from each of nine equal areas when viewed from one side, and the average value of these measurements was taken as the thickness of the coating. The thicknesses of the coatings are as follows.
[0041] Comparative Example 9: 5μm Comparative example 10: 25μm Invention example 2: 50μm Invention example 3: 75μm Invention example 4: 150μm
[0042] (Evaluation method) Corrosion resistance tests and evaluations were conducted under the same conditions as Comparative Examples 1 to 8 and Invention Example 1. FIG. 4(B) is a graph that shows a schematic of the cumulative corrosion weight loss of Comparative Examples 9 and 10 and Invention Examples 2 to 4. FIG. 4(B) shows the trend line of the cumulative corrosion weight loss measured every week for Comparative Examples 9 and 10 and Invention Examples 2 to 4. The results are shown in FIG. 4(B) and Table 2.
[0043] [Table 2]
[0044] In Comparative Examples 9 and 10, the fluororesin coating had minute through-holes, which allowed the chromium plating solution to reach the base material, resulting in corrosion of the base material by the chromium plating solution. Comparative Example 10 showed a smaller increase in cumulative corrosion weight loss, but it was demonstrated that the heat exchanger plate needed to be replaced in a relatively short period of time. On the other hand, in Inventive Examples 2 to 4, the coating was formed with a sufficient thickness, so that the minute holes generated during coating formation did not become through-holes, and the coating completely covered the base material. Therefore, regardless of the passage of time, the chromium plating solution was prevented by the coating and did not reach the base material, and weight loss did not occur in the base material, demonstrating that replacement of the heat exchanger plate was not necessary for a long period of time. In particular, it is clear from Table 2 that Inventive Examples 3 and 4 showed extremely low cumulative corrosion weight loss even four weeks after the start of the test. [Industrial Applicability]
[0045] The present invention is widely applicable to heat exchanger plates and heat exchangers. [Explanation of symbols]
[0046] 1 heat exchanger 10 Heat exchanger plate 11 Base material 11a surface 12. Membrane
Claims
1. A heat exchanger plate exposed to a chromic acid solution, comprising: A base material having a surface formed of metal; A fluorine-based coating having a thickness of 50 μm to 250 μm formed on the surface of the base material; A heat exchanger plate comprising:
2. The heat exchanger plate according to claim 1, which is used to heat the chromic acid liquid to a set temperature in the range of 30°C to 60°C.
3. A heat exchanger comprising a plurality of heat exchanger plates according to claim 1 or 2, A heat exchanger, wherein the heat exchanger plates are positioned by being pressed against each other in an arrangement direction of the heat exchanger plates.
Citation Information
Patent Citations
Refrigeration cycle device
WO2020040158A1