Reflection adjustment film, optical member, and lens unit

The integration of a multilayer reflection adjustment film under a hydrophilic layer in lenses suppresses light reflection, enhancing visibility and durability by reducing optical defects.

JP2024158884AInactive Publication Date: 2024-11-08NIDEC CORP(JP) +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023074496
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Hydrophilic lenses reflect a portion of incident light, reducing visibility and causing optical defects like ghost and flare phenomena.

Method used

A reflection adjustment film with a multilayer structure of low and high refractive index layers is integrated under a hydrophilic layer to suppress light reflection, enhancing light transmission and durability.

Benefits of technology

The solution effectively reduces light reflection to less than 3%, minimizing optical defects and improving durability while maintaining hydrophilicity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024158884000001_ABST
    Figure 2024158884000001_ABST
Patent Text Reader

Abstract

To provide a reflection adjustment film, an optical member, and a lens unit capable of suppressing the reflection of incident light by a hydrophilic layer and an optical member.SOLUTION: A reflection adjustment film 30 is used for an optical member 100 having a hydrophilic layer 20 containing a plurality of photocatalyst particles. The reflection adjustment film 30 is arranged under the hydrophilic layer 20. The thickness of the reflection adjustment film 30 is at least 5 times greater than the thickness of the hydrophilic layer 20. The thickness of the reflection adjustment film 30 is preferably 20 nm or more and 2000 nm or less. The reflection adjustment film 30 preferably includes a low refractive index layer and a high refractive index layer. The photocatalyst particles are preferably titanium oxide particles.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a reflection control film, an optical member, and a lens unit. [Background technology]

[0002] Visibility is impaired by water droplets on window glass of buildings or automobiles exposed to outdoor weather. One solution to the problem of impaired visibility is to make the surface of the window glass hydrophilic. This makes it possible to turn the adhering water into a film, preventing the adhesion of water droplets and ensuring visibility on the window glass.

[0003] However, organic dirt caused by automobile exhaust gases or factory smoke easily adheres to the surface of hydrophilic members, causing water droplets to adhere to the surface, significantly reducing visibility.

[0004] In view of this, a hydrophilic lens including a glass substrate and a hydrophilic layer formed on the glass substrate has been disclosed (for example, Patent Document 1). In the hydrophilic lens of Patent Document 1, the hydrophilic layer contains a silicate material in which fine particles having photocatalytic activity are dispersed, the film thickness of the hydrophilic layer is 30 nm or less, the average particle diameter of the fine particles is 30 nm or less, and the arithmetic mean roughness Ra of the surface of the hydrophilic layer is 0.7 to 1.9 nm. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2018-77260 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, in the hydrophilic lens of Patent Document 1, a portion of the incident light is reflected rather than transmitted by optical members such as the hydrophilic layer and the glass substrate.

[0007] The present disclosure has been made in consideration of the above-mentioned problems, and has an object to provide a reflection adjustment film, an optical member, and a lens unit that can suppress reflection of incident light by a hydrophilic layer and an optical member. [Means for solving the problem]

[0008] The exemplary reflection adjustment film of the present disclosure is used in an optical component having a hydrophilic layer containing a plurality of photocatalytic particles. The reflection adjustment film is disposed under the hydrophilic layer. The thickness of the reflection adjustment film is 5 times or more the thickness of the hydrophilic layer.

[0009] An exemplary optical member of the present disclosure includes the reflection adjustment film, the translucent member, and the hydrophilic layer. The translucent member transmits light having a wavelength of 400 nm or more and 700 nm or less. The reflection adjustment film is disposed between the hydrophilic layer and the translucent member.

[0010] An exemplary lens unit according to the present disclosure includes the optical member and an optical lens that transmits light having a wavelength of 400 nm or more and 700 nm or less, and the optical member is disposed on the opposite side of the optical lens in the traveling direction of the light. Effect of the Invention

[0011] According to the exemplary embodiment of the present disclosure, the reflection of incident light can be suppressed by the hydrophilic layer and the optical member. Cut. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a schematic diagram showing an example of an optical unit according to the present embodiment. [Diagram 2] FIG. 2 is a schematic diagram illustrating an example of an optical member according to the present embodiment. [Diagram 3] FIG. 3 shows the measurement results of the optical member according to Example 1 and the measurement results of the optical member according to Comparative Example 1. [Figure 4]FIG. 4 shows the measurement results of the optical member according to Example 1, the measurement results of the optical member according to Example 5, and the measurement results of the optical member according to Comparative Example 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the drawings, the same or corresponding parts are given the same reference symbols and the description will not be repeated. The dimensions, shapes, and size relationships between components in the drawings are not necessarily the same as the actual dimensions, shapes, and size relationships between components. In particular, the thickness ratios and curvatures of the reflection adjustment film, hydrophilic layer, and translucent member in the drawings may differ significantly from the actual ones.

[0014] In this specification, "thickness" refers to the length of an optical member in the optical axis direction. The "outside" of an optical member refers to the direction from the light-transmitting member to the hydrophilic layer. The "inside" of an optical member refers to the direction from the hydrophilic layer to the light-transmitting member.

[0015] The optical member according to this embodiment is suitable as an optical member used in, for example, an optical unit including one or more optical members (particularly, an optical unit used outdoors). The optical member according to this embodiment is particularly suitable as a lens for a lens unit of an in-vehicle camera for monitoring the surroundings of a vehicle. FIG. 1 is a schematic diagram showing an example of an optical unit according to this embodiment. As shown in FIG. 1, an optical unit 1000 includes an optical member 100. The optical unit is an example of a "lens unit".

[0016] The optical member according to this embodiment may be used in an optical unit (particularly an optical unit used outdoors) including the optical member 100 and an optical lens. The optical lens transmits light with a wavelength of 400 nm or more and 700 nm or less. The optical member 100 is disposed on the opposite side of the optical lens in the traveling direction of light.

[0017] The static contact angle of the surface of the optical member 100 with pure water is preferably 30.0° or less, more preferably 20.0° or less, and particularly preferably 10.0° or less. Hereinafter, the static contact angle with pure water may be referred to simply as "contact angle." Note that the contact angle of the surface of the optical member according to this embodiment is a value measured in an environment with a temperature of 23°C ± 3°C and a relative humidity of 50% ± 3%.

[0018] Moreover, the reflectance for light having a wavelength of 400 nm or more and 700 nm or less is 3% or less. The maximum reflectance of the optical member 100 for light having a wavelength of 400 nm or more and 700 nm or less is preferably 1.5% or less, more preferably 1.0% or less. The optical member 100 according to this embodiment can suppress the occurrence of image defects called ghost phenomenon and image defects called flare phenomenon as the above-mentioned maximum reflectance is lower. In particular, the occurrence of ghost phenomenon can be suppressed more effectively as the above-mentioned maximum reflectance is lower. When the above-mentioned maximum reflectance is 3.0% or less, the occurrence of ghost phenomenon can be suppressed. When the above-mentioned maximum reflectance is 1.0% or less, the occurrence of ghost phenomenon can be suppressed more effectively. Incidentally, light having a wavelength of 400 nm or more and 700 nm or less corresponds to light in the visible light region.

[0019] Hereinafter, an example of the optical member 100 according to this embodiment will be described with reference to Fig. 2. Fig. 2 is a schematic diagram showing an example of the optical member 100 according to this embodiment. The optical member 100 includes a light-transmitting member 10, a hydrophilic layer 20, and a reflection adjustment film 30.

[0020] <Translucent member> The light-transmitting member 10 has light-transmitting properties. That is, the light-transmitting member 10 transmits visible light. The light-transmitting member 10 may be transparent or translucent. The light-transmitting member 10 contains, for example, glass or synthetic resin as a main component.

[0021] The light-transmitting member 10 has a function as, for example, a lens (specifically, for example, a biconvex lens, a biconcave lens, a plano-convex lens, a plano-concave lens, a convex meniscus lens, or a concave meniscus lens). In this specification, when the light-transmitting member 10 is a lens, the lens surface of the light-transmitting member 10 may be spherical or aspherical. The radius of curvature of the lens surface of the light-transmitting member 10 is preferably 9 mm or more and 16 mm or less.

[0022] <Hydrophilic layer> The hydrophilic layer 20 covers the light-transmitting member 10. Specifically, the hydrophilic layer 20 is disposed on the reflection adjustment film 30. The hydrophilic layer 20 has hydrophilic properties.

[0023] The thickness of the hydrophilic layer 20 is preferably 20 nm or more and 200 nm or less, more preferably 30 nm or more and 100 nm or less. If the thickness of the hydrophilic layer 20 is less than 20 nm, the function of restoring hydrophilicity tends to be insufficient. If the thickness of the hydrophilic layer 20 is more than 200 nm, the transmittance of visible light tends to be insufficient.

[0024] In the present specification, the "thickness" may be determined using a stylus-type step gauge. Specifically, a sharp needle is traced over the surface to measure the step between areas with and without a layer (film). The step is measured at three arbitrary locations, and the average value of the step differences at the three locations is taken as the "thickness."

[0025] The hydrophilic layer 20 contains a plurality of photocatalyst particles. The photocatalyst particles have a photocatalytic function. For example, when the optical member 100 is used for a long period of time, dirt adheres to the optical member 100, reducing the hydrophilic function. When the optical member 100 is irradiated with ultraviolet light (sunlight), the dirt is broken down and the hydrophilic function can be restored. The optical member 100 according to this embodiment exhibits a high hydrophilicity when exposed to ultraviolet light of 1 mW / cm when the contact angle exceeds 30.0°. 2It is preferable that the contact angle becomes 30.0° or less by irradiating the hydrophilic layer 20 with a UV-ray source for 6 hours. Examples of photocatalyst particles include particles of titanium oxide, strontium titanate, zinc oxide, silicon carbide, gallium phosphate, cadmium sulfide, cadmium selenide, and molybdenum trisulfide, but titanium oxide particles are preferable in terms of photocatalytic function. Specifically, the photocatalyst particles are, for example, primary or secondary particles of titanium dioxide. In detail, it is preferable that the hydrophilic layer 20 contains secondary particles formed by agglomeration of a plurality of primary particles of titanium dioxide.

[0026] Examples of titanium dioxide include anatase type titanium dioxide, rutile type titanium dioxide, and brookite type titanium dioxide. From the viewpoint of photocatalytic activity, anatase type titanium dioxide is preferable.

[0027] It is preferable that the hydrophilic layer 20 further contains tetraethoxysilane and silicon dioxide, so that the abrasion resistance of the optical member 100 is further improved.

[0028] <Reflection adjustment film> The reflection adjustment film 30 is disposed under the hydrophilic layer 20. The reflection adjustment film 30 covers the light-transmitting member 10. The reflection adjustment film 30 is disposed between the light-transmitting member 10 and the hydrophilic layer 20. The reflection adjustment film 30 suppresses reflection of light.

[0029] The reflection adjustment film 30 has a multi-layer structure. Specifically, the reflection adjustment film 30 includes low-refractive index layers and high-refractive index layers alternately stacked along the thickness direction (optical axis direction). The refractive indices of the low-refractive index layers and the high-refractive index layers are not limited as long as the combination allows the reflection adjustment film 30 to exhibit an anti-reflection effect. The refractive index of the low-refractive index layer is, for example, 1.80 or less. The refractive index of the high-refractive index layer is, for example, more than 1.80.

[0030] The refractive index of the low refractive index layer may be less than that of the high refractive index layer. For example, the refractive index of the low refractive index layer is preferably 1.30 or more and 1.80 or less, more preferably 1.40 or more and 1.60 or less. By making the refractive index of the low refractive index layer 1.30 or more and 1.80 or less, the reflectance of the optical member 100 is further reduced. The low refractive index layer preferably contains, for example, SiO2, Al2O3, or MgF2, and more preferably contains SiO2.

[0031] The refractive index of the high refractive index layer may be higher than that of the low refractive index layer. For example, the refractive index of the high refractive index layer is preferably 1.80 or more and 3.00 or less, more preferably 2.00 or more and 2.80 or less. By having the refractive index of the high refractive index layer be 1.80 or more and 3.00 or less, the reflectance of the optical member 100 is further reduced. The high refractive index layer preferably contains, for example, Si3N4, ZrO2, TiO2, Ti3O5, Ta2O5, In2O3, CeO2 and Nb2O5, and more preferably contains Si3N4.

[0032] The refractive indices of the low refractive index layer and the high refractive index layer described above are merely examples and are not limited thereto. The refractive indices of the low refractive index layer and the high refractive index layer may be set to values ​​optimal for the refractive index of the light-transmitting member 10.

[0033] The thickness of the reflection adjustment film 30 is 5 times or more the thickness of the hydrophilic layer 20. The thickness of the reflection adjustment film 30 is preferably 100 times or less the thickness of the hydrophilic layer 20 from the viewpoint of productivity. That is, the thickness of the reflection adjustment film 30 is preferably 5 times or more and 100 times or less the thickness of the hydrophilic layer 20. The total film thickness of the reflection adjustment film 30 is preferably 20 nm or more and 2000 nm or less, and more preferably 200 nm or more and 750 nm or less. If the total film thickness of the reflection adjustment film 30 is less than 20 nm, there is a tendency that sufficient anti-reflection effect cannot be obtained. If the total film thickness of the reflection adjustment film 30 exceeds 2000 nm, it takes a long time to form the film, and the productivity of the optical member 100 tends to decrease. In addition, if the total film thickness exceeds 2000 nm, there is a tendency that the production cost of the optical member 100 increases.

[0034] The thickness of one low refractive index layer is, for example, from 5.0 nm to 200.0 nm, and the thickness of one high refractive index layer is, for example, from 5.0 nm to 200.0 nm.

[0035] The total number of low refractive index layers and high refractive index layers is usually an odd number, but may be an even number.

[0036] 1 and 2, in this embodiment, the thickness of the reflection adjustment film 30 is five times or more the thickness of the hydrophilic layer 20, and therefore it is possible to suppress reflection of incident light by the hydrophilic layer 20 and the translucent member 10. Specifically, by including the reflection adjustment film 30, the optical member 100 suppresses reflection of light attempting to enter the translucent member 10 from the reflection adjustment film 30 by the surface on the reflection adjustment film 30 side.

[0037] Furthermore, the reflection adjustment film 30 has low refractive index layers and high refractive index layers alternately stacked along the thickness direction (optical axis direction), so that a multilayer film interference effect can be obtained.

[0038] Moreover, it is preferable that the Vickers hardness of the reflection adjustment film 30 is 400 HV or more. As a result, it is possible to improve the durability of the reflection adjustment film 30. As a result, it is possible to improve the durability of the optical member 100. A coating layer may be disposed on the reflection adjustment film 30. The coating layer may contain titanium oxide particles.

[0039] <Method of manufacturing optical members> An example of a method for manufacturing the optical member 100 according to this embodiment will be described below. The method for manufacturing the optical member 100 includes a preparation step, a reflection adjustment film formation step, a coating step, and a drying step.

[0040] <Preparation steps> First, prepare a light-transmitting member 10. The light-transmitting member 10 contains, for example, glass or synthetic resin as a main component.

[0041] <Reflection adjustment film formation step> A low refractive index material is prepared. The low refractive index material preferably contains, for example, SiO2, Al2O3, or MgF2, and more preferably contains SiO2. The content of SiO2 in the low refractive index material is preferably 95 mass% or more. The method for forming the low refractive index material is preferably deposition or sputtering.

[0042] A high refractive index material is prepared. The high refractive index material preferably contains, for example, Si3N4, ZrO2, TiO2, Ti3O5, Ta2O5, In2O3, CeO2, and Nb2O5, and more preferably contains Si3N4. The content of Si3N4 in the high refractive index material is preferably 95 mass% or more. The method for forming the high refractive index material is preferably deposition or sputtering.

[0043] The low refractive index layers and the high refractive index layers are alternately laminated. The total number of the low refractive index layers and the high refractive index layers is usually an odd number. However, the total number of the low refractive index layers and the high refractive index layers may be an even number.

[0044] <Application step> A hydrophilic material is applied. The hydrophilic material contains a plurality of primary particles of photocatalyst particles. The average particle size of the primary particles of the photocatalyst particles is preferably 5 nm or more and 20 nm or less.

[0045] The hydrophilic material preferably further contains a solvent. The solvent is preferably an aqueous solvent. The aqueous solvent contains water and an additive. Examples of the additive include an organic acid, an alcohol compound, or ammonia. Examples of the organic acid include nitric acid, formic acid, acetic acid, propionic acid, succinic acid, citric acid, or malic acid. Examples of the alcohol compound include methanol, ethanol, isopropyl alcohol, n-propyl alcohol, or butanol.

[0046] The content of the solvent in the hydrophilic material is preferably 50.0% by mass or more and 99.9% by mass or less. By having the content of the solvent be 50.0% by mass or more and 99.9% by mass or less, coating can be easily performed.

[0047] The method of applying the hydrophilic material is preferably a wet process. Examples of the wet process include spin coating, roll coating, bar coating, dip coating, spray coating, or a combination of two or more of these (e.g., dip spin coating). Examples of the wet process include spin coating, dip coating, or dip spin coating.

[0048] <Drying step> The hydrophilic material is dried to produce the hydrophilic layer 20. The hydrophilic layer 20 preferably contains secondary particles formed by agglomeration of a plurality of primary particles of the photocatalyst particles.

[0049] It is preferable to heat-treat the coated hydrophilic material. Heat treatment promotes the removal of the solvent in the hydrophilic material. Heating conditions can be, for example, a treatment temperature of 60°C to 200°C and a treatment time of 10 minutes to 2 hours.

[0050] It is preferable that the method for producing the optical member 100 further includes a coating material application step.

[0051] The above describes the embodiments of the present disclosure with reference to the drawings. However, the above embodiments are merely examples of the present disclosure, and the present disclosure is not limited to the above embodiments, and can be implemented in various aspects without departing from the gist of the present disclosure. The drawings are mainly schematic illustrations of each component for ease of understanding, and the thickness, length, number, etc. of each component shown in the drawings are different from the actual ones due to the convenience of drawing. In addition, the material, shape, dimensions, etc. of each component shown in the above embodiments are only examples and are not particularly limited, and various modifications are possible within a range that does not substantially deviate from the effects of the present disclosure. The configuration of the embodiment may be appropriately modified within a range that does not exceed the technical idea of ​​the present disclosure. In addition, the embodiments may be implemented in combination within a possible range.

[0052] The present technology can also adopt the following configuration.

[0053] (1) Used in an optical member having a hydrophilic layer containing a plurality of photocatalyst particles, A reflection adjustment film disposed under the hydrophilic layer, A reflection adjustment film, the thickness of which is 5 times or more the thickness of the hydrophilic layer.

[0054] (2) The reflection adjustment film according to (1), wherein the thickness of the reflection adjustment film is 20 nm or more and 2000 nm or less.

[0055] (3) The reflection adjustment film according to (1) or (2), wherein the reflection adjustment film comprises a low refractive index layer and a high refractive index layer.

[0056] (4) A reflection adjustment film according to any one of (1) to (3), a light-transmitting member that transmits light having a wavelength of 400 nm or more and 700 nm or less; The hydrophilic layer. Equipped with The reflection adjustment film is disposed between the hydrophilic layer and the light-transmitting member.

[0057] (5) The optical member according to (4), wherein the photocatalyst particles are titanium oxide particles.

[0058] (6) The optical member according to (4) or (5), wherein the reflection adjustment film has a Vickers hardness of 400 HV or more.

[0059] (7) An optical member according to any one of (4) to (6), an optical lens that transmits light having a wavelength of 400 nm or more and 700 nm or less; Equipped with The optical member is disposed on the opposite side of the optical lens in the traveling direction of the light. EXAMPLES

[0060] The present invention will be described in more detail below using examples, but the present invention is not limited to the scope of the examples.

[0061] <Manufacturing of optical components> Optical members according to Examples 1 to 10 and optical members according to Comparative Examples 1 to 6 were manufactured.

[0062] <Example 1> <Preparation steps> A lens ("TAFD-5G" manufactured by HOYA Corporation, composition: glass, diameter 12.9 mm, refractive index: 1.835) was prepared as a light-transmitting member. One surface of the lens was a convex surface (radius of curvature 12 mm) and the other surface was a concave surface (radius of curvature 3.07 mm).

[0063] <Reflection adjustment film formation step> A low refractive index material containing SiO2 and a high refractive index material containing Si3N4 were alternately laminated. The total number of low refractive index layers and high refractive index layers was 11, and a reflection adjustment film of Example 1 having a thickness of 579 nm was formed.

[0064] <Application step> A hydrophilic material according to Example 1 containing titanium dioxide particles and silicon dioxide was prepared.

[0065] A hydrophilic material was applied onto the reflection adjustment film. Specifically, 60 μL of the hydrophilic material was dropped onto the optical axis of the light-transmitting member. Next, the light-transmitting member was rotated at a rotation speed of 5000 rpm using a spin coater ("MS-B100" manufactured by Mikasa Co., Ltd.). At this time, the rotation axis was aligned with the optical axis of the light-transmitting member.

[0066] <Drying step> A heat treatment was carried out at 90° C. for 30 minutes to form a hydrophilic layer having a thickness of 30 nm. The thickness of the reflection adjustment film was 19 times that of the hydrophilic layer.

[0067] <Example 2> In the <reflection adjustment film forming step> of Example 1, the total number of low and high refractive index layers was 11, and a reflection adjustment film having a thickness of 579 nm was formed, but instead, the total number of low and high refractive index layers was 13, and a reflection adjustment film having a thickness of 415 nm according to Example 2 was formed. The thickness of the reflection adjustment film was 14 times the thickness of the hydrophilic layer.

[0068] <Example 3> In the <reflection adjustment film forming step> of Example 1, the total number of low and high refractive index layers was 11, and a reflection adjustment film having a thickness of 579 nm was formed, but instead, the total number of low and high refractive index layers was 9, and a reflection adjustment film having a thickness of 388 nm according to Example 3 was formed. The thickness of the reflection adjustment film was 13 times the thickness of the hydrophilic layer.

[0069] <Example 4> In the <reflection adjustment film formation step> of Example 1, the total number of low and high refractive index layers was 11, and a reflection adjustment film having a thickness of 579 nm was formed, but instead, the total number of low and high refractive index layers was 7, and a reflection adjustment film having a thickness of 324 nm according to Example 4 was formed. The thickness of the reflection adjustment film was 11 times the thickness of the hydrophilic layer.

[0070] <Example 5> In the <reflection adjustment film formation step> of Example 1, the total number of low and high refractive index layers was 11, and a reflection adjustment film having a thickness of 579 nm was formed, but instead, the total number of low and high refractive index layers was 5, and a reflection adjustment film having a thickness of 196 nm was formed according to Example 5. The thickness of the reflection adjustment film was 7 times the thickness of the hydrophilic layer.

[0071] <Example 6> In the <reflection adjustment film forming step> of Example 1, the total number of low and high refractive index layers was 11, and a reflection adjustment film having a thickness of 579 nm was formed, but instead, the total number of low and high refractive index layers was 17, and a reflection adjustment film having a thickness of 749 nm according to Example 6 was formed. The thickness of the reflection adjustment film was 25 times the thickness of the hydrophilic layer.

[0072] <Comparative Example 1> In the <reflection adjustment film forming step> of Example 1, the total number of low refractive index layers and high refractive index layers was 11, and instead of forming a reflection adjustment film with a thickness of 579 nm, no reflection adjustment film was formed.

[0073] <Comparative Example 2> In the <reflection adjustment film forming step> of Example 1, the total number of low and high refractive index layers was 11, and instead of forming a reflection adjustment film with a thickness of 579 nm, the total number of low and high refractive index layers was 5, and a reflection adjustment film with a thickness of 115 nm according to Comparative Example 2 was formed. Note that the thickness of the reflection adjustment film was four times the thickness of the hydrophilic layer.

[0074] <Comparative Example 3> In the <coating step> of Example 1, a hydrophilic layer having a thickness of 30 nm was formed, and in the <reflection adjustment film forming step>, the total number of low and high refractive index layers was 11, and a reflection adjustment film having a thickness of 579 nm was formed, but in the <coating step>, a hydrophilic layer having a thickness of 40 nm was formed, and in the <reflection adjustment film forming step>, the total number of low and high refractive index layers was 5, and a reflection adjustment film having a thickness of 108 nm was formed according to Comparative Example 3. The thickness of the reflection adjustment film was three times that of the hydrophilic layer.

[0075] <Example 7> In the <coating step> of Example 1, a hydrophilic layer having a thickness of 30 nm was formed, and in the <reflection adjustment film forming step>, the total number of low and high refractive index layers was 11, and a reflection adjustment film having a thickness of 579 nm was formed, but in the <coating step>, a hydrophilic layer having a thickness of 50 nm was formed, and in the <reflection adjustment film forming step>, the total number of low and high refractive index layers was 17, and a reflection adjustment film having a thickness of 745 nm was formed according to Example 7. The thickness of the reflection adjustment film was 15 times the thickness of the hydrophilic layer.

[0076] <Example 8> In the <coating step> of Example 1, a hydrophilic layer having a thickness of 30 nm was formed, and in the <reflection adjustment film forming step>, the total number of low and high refractive index layers was 11, and a reflection adjustment film having a thickness of 579 nm was formed, but in the <coating step>, a hydrophilic layer having a thickness of 50 nm was formed, and in the <reflection adjustment film forming step>, the total number of low and high refractive index layers was 11, and a reflection adjustment film having a thickness of 558 nm was formed according to Example 8. The thickness of the reflection adjustment film was 11 times the thickness of the hydrophilic layer.

[0077] <Example 9> In the <coating step> of Example 1, a hydrophilic layer having a thickness of 30 nm is formed, and in the <reflection adjustment film forming step>, the total number of low refractive index layers and high refractive index layers is 11 layers, and the thickness Instead of forming a reflection adjustment film of 579 nm, a hydrophilic layer of 50 nm was formed in the <coating step>, and the total number of low refractive index layers and high refractive index layers was 7 in the <reflection adjustment film forming step>, forming a reflection adjustment film of 289 nm according to Example 9. The thickness of the reflection adjustment film was 6 times the thickness of the hydrophilic layer.

[0078] <Comparative Example 4> In the <coating step> of Example 1, a hydrophilic layer having a thickness of 30 nm was formed, and in the <reflection adjustment film forming step>, the total number of low and high refractive index layers was 11, and a reflection adjustment film having a thickness of 579 nm was formed, but in the <coating step>, a hydrophilic layer having a thickness of 50 nm was formed, and in the <reflection adjustment film forming step>, the total number of low and high refractive index layers was 5, and a reflection adjustment film having a thickness of 100 nm was formed according to Comparative Example 4. The thickness of the reflection adjustment film was twice as thick as the thickness of the hydrophilic layer.

[0079] <Comparative Example 5> In the <coating step> of Example 1, a hydrophilic layer having a thickness of 30 nm was formed, and in the <reflection adjustment film forming step>, the total number of low and high refractive index layers was 11, and a reflection adjustment film having a thickness of 579 nm was formed, but in the <coating step>, a hydrophilic layer having a thickness of 50 nm was formed, and in the <reflection adjustment film forming step>, the total number of low and high refractive index layers was 5, and a reflection adjustment film having a thickness of 181 nm was formed according to Comparative Example 5. The thickness of the reflection adjustment film was four times that of the hydrophilic layer.

[0080] <Example 10> In the <coating step> of Example 1, a hydrophilic layer having a thickness of 30 nm was formed, and in the <reflection adjustment film forming step>, the total number of low and high refractive index layers was 11, and a reflection adjustment film having a thickness of 579 nm was formed, but in the <coating step>, a hydrophilic layer having a thickness of 100 nm was formed, and in the <reflection adjustment film forming step>, the total number of low and high refractive index layers was 17, and a reflection adjustment film having a thickness of 656 nm was formed according to Example 10. The thickness of the reflection adjustment film was 7 times the thickness of the hydrophilic layer.

[0081] <Comparative Example 6> In the <coating step> of Example 1, a hydrophilic layer having a thickness of 30 nm was formed, and in the <reflection adjustment film forming step>, the total number of low and high refractive index layers was 11, and a reflection adjustment film having a thickness of 579 nm was formed, but in the <coating step>, a hydrophilic layer having a thickness of 100 nm was formed, and in the <reflection adjustment film forming step>, the total number of low and high refractive index layers was 5, and a reflection adjustment film having a thickness of 70 nm was formed according to Comparative Example 6. The thickness of the reflection adjustment film relative to the thickness of the hydrophilic layer was 0.7 times.

[0082] <Evaluation> The reflectance and productivity were evaluated by the following methods for the optical members according to Examples 1 to 10 and the optical members according to Comparative Examples 1 to 6. The measurement results are shown in the following Tables 1 to 4. All measurements were performed in an environment with a temperature of 23°C ± 3°C and a relative humidity of 50% ± 3%.

[0083] <Reflectance> A reflectance measuring device (Olympus Corporation, "USPM-RU") was used to measure the maximum reflectance of the optical members for light with a wavelength of 400 nm or more and 700 nm or less. The angle of incidence of the incident light was set to 0 degrees. The maximum reflectance of the optical members was evaluated according to the following criteria. The evaluation results are shown in Tables 1 to 4. Furthermore, the measurement results of the optical members according to Example 1 and Comparative Example 1 are shown in FIG. 3. Furthermore, the measurement results of the optical members according to Example 1, Example 5, and Comparative Example 4 are shown in FIG. 4.

[0084] ○: 1.0% or less △: More than 1.0% but less than 3.0% ×: More than 3.0%

[0085] <Productivity> The working time for the <reflection adjustment film formation step> was measured. The evaluation results are shown in Tables 1 to 4.

[0086] 〇: Less than 1 hour △: More than 1 hour and less than 2 hours ×: Over 2 hours

[0087] [Table 1]

[0088] [Table 2]

[0089] [Table 3]

[0090] [Table 4]

[0091] The optical members according to Comparative Example 1 to Comparative Example 6 had a reflectance of more than 3% for light having a wavelength of 400 nm or more and 700 nm or less. In contrast, the optical members according to Examples 1 to 10 had a reflectance of 3% or less for light having a wavelength of 400 nm or more and 700 nm or less. In particular, the optical members according to Examples 1 to 5 and Examples 7 to 10 had good productivity. [Explanation of symbols]

[0092] 10...Translucent member 20...Hydrophilic layer 30...Reflection adjustment film 60...Covering layer 100 Optical components

Claims

1. The present invention is used in an optical member having a hydrophilic layer including a plurality of photocatalyst particles, A reflection adjustment film disposed under the hydrophilic layer, A reflection adjustment film, the thickness of which is 5 times or more the thickness of the hydrophilic layer.

2. The reflection adjustment film according to claim 1 , wherein the thickness of the reflection adjustment film is 20 nm or more and 2000 nm or less.

3. The reflection adjustment film according to claim 1 , comprising a low refractive index layer and a high refractive index layer.

4. The reflection adjustment film according to claim 1 ; a light-transmitting member that transmits light having a wavelength of 400 nm or more and 700 nm or less; The hydrophilic layer. Equipped with The reflection adjustment film is disposed between the hydrophilic layer and the light-transmitting member.

5. The optical member according to claim 4 , wherein the photocatalyst particles are titanium oxide particles.

6. The optical member according to claim 4 , wherein the reflection adjustment film has a Vickers hardness of 400 HV or more.

7. The optical member according to claim 4 ; an optical lens that transmits light having a wavelength of 400 nm or more and 700 nm or less; Equipped with The optical member is disposed on the opposite side of the optical lens in the traveling direction of the light.

8. a light-transmitting member that transmits light having a wavelength of 400 nm or more and 700 nm or less; A hydrophilic layer containing a plurality of photocatalyst particles; a reflection adjustment film disposed between the hydrophilic layer and the light-transmitting member; Equipped with The optical member has a reflectance of 3% or less for light with a wavelength of 400 nm or more and 700 nm or less.

Citation Information

Patent Citations

  • Hydrophilic lens

    JP2018077260A