Anode material, anode of secondary battery using said anode material, and method of manufacturing the same

By optimizing the ratio and density of Si-containing and graphite particles in the negative electrode material, the material addresses the volume change issue, enhancing the battery's capacity and cycle performance.

JP2024159006AActive Publication Date: 2024-11-08PRIME PLANET ENERGY & SOLUTIONS INC

Patent Information

Application Number
JP2023074714
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08
Estimated Expiration
2043-04-28

AI Technical Summary

Technical Problem

Si-containing particles in negative electrodes of secondary batteries experience significant volume changes during charging and discharging, leading to decreased filling properties and broken conductive paths, resulting in capacity deterioration and poor cycle characteristics when used with graphite particles.

Method used

A negative electrode material comprising Si-containing particles and graphite particles with a specific ratio of average particle diameters (1 to 8) and a mass ratio (10% to 60%) is formulated, achieving a density of 0.9 g/cm³ when uniaxially pressed, which enhances filling properties and suppresses capacity deterioration.

Benefits of technology

The configuration improves the resistance to capacity deterioration and maintains excellent cycle characteristics of secondary batteries, increasing their capacity and energy density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159006000001_ABST
    Figure 2024159006000001_ABST
Patent Text Reader

Abstract

To provide an anode material that contains Si-containing particles and graphite particles, and that is capable of suppressing capacity degradation when a secondary battery is repeatedly charged and discharged.SOLUTION: An anode material disclosed herein contains Si-containing particles and graphite particles. The ratio of the average particle size (D50) of the graphite particles to the average particle size (D50) of the Si-containing particles is 1 to 8. The mass ratio of the Si-containing particles to the total of the Si-containing particles and the graphite particles is 10 mass% to 60 mass%. When 1 g of the Si-containing particles is uniaxially pressed at 25°C and 60 MPa to form a tablet having a diameter of 20 mm, the density of the resulting molded body is 0.9 g / cm3 or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a negative electrode material. The present invention also relates to a negative electrode of a secondary battery using the negative electrode material. The present invention further relates to a method for producing the negative electrode of the secondary battery. [Background technology]

[0002] 2. Description of the Related Art In recent years, secondary batteries have been suitably used as portable power sources for personal computers, mobile terminals, and the like, and as power sources for driving vehicles such as electric vehicles (BEVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs), and the like.

[0003] In applications as a power source for driving vehicles, particularly BEVs, secondary batteries are desired to have a higher capacity from the viewpoint of extending the driving range of the vehicle. Si-containing particles are known as a high-capacity negative electrode active material, and it is known that the Si-containing particles can increase the capacity of secondary batteries (see, for example, Patent Document 1). Patent Document 1 discloses a technology in which Si-containing particles and graphite particles such as natural graphite are used in combination as a negative electrode active material. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-38862 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, while the Si-containing particles have a high capacity, they undergo a large volume change due to expansion / contraction when the secondary battery is charged and discharged. Therefore, when the Si-containing particles and the graphite particles are used in combination, particularly when the ratio of the Si-containing particles is large, the packing property of these particles decreases when the secondary battery is repeatedly charged and discharged, which may cause the conductive path to be broken, internal stress, etc. Therefore, when the Si-containing particles and the graphite particles are used in combination, there is a problem that the cycle characteristics of the secondary battery are reduced, specifically, there is a problem that the capacity deterioration is large when the secondary battery is repeatedly charged and discharged.

[0006] In view of the above circumstances, an object of the present invention is to provide a negative electrode material containing Si-containing particles and graphite particles, which is capable of suppressing capacity degradation when a secondary battery is repeatedly charged and discharged. [Means for solving the problem]

[0007] The negative electrode material disclosed herein contains Si-containing particles and graphite particles. The ratio of the average particle size (D50) of the graphite particles to the average particle size (D50) of the Si-containing particles is 1 to 8. The mass ratio of the Si-containing particles to the total of the Si-containing particles and the graphite particles is 10 mass% to 60 mass%. When 1 g of the Si-containing particles is uniaxially pressed at 60 MPa at 25°C to form into a tablet having a diameter of 20 mm, the density of the resulting molded body is 0.9 g / cm. 3 That's all.

[0008] According to this configuration, it is possible to provide a negative electrode material that contains Si-containing particles and graphite particles and that can suppress capacity degradation when a secondary battery is repeatedly charged and discharged.

[0009] From another aspect, the negative electrode of the secondary battery disclosed herein includes a negative electrode current collector and a negative electrode active material layer supported on the negative electrode current collector. The negative electrode active material layer contains the above-mentioned negative electrode material.

[0010] A negative electrode having such a configuration can provide the secondary battery with excellent resistance to capacity degradation when repeatedly charged and discharged.

[0011] From another aspect, a manufacturing method of a negative electrode of a secondary battery disclosed herein includes a step of applying a negative electrode paste containing the above-mentioned negative electrode material to a negative electrode current collector, a step of drying the applied negative electrode paste to form a negative electrode active material layer, and a step of pressing the negative electrode active material layer.

[0012] The negative electrode obtained by such a configuration can impart excellent resistance to capacity degradation to the secondary battery when repeatedly charged and discharged. [Brief description of the drawings]

[0013] [Figure 1] FIG. 2 is a schematic diagram of an example of a negative electrode material according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view illustrating a schematic configuration of a negative electrode of a secondary battery according to one embodiment of the present invention. [Diagram 3] FIG. 1 is a cross-sectional view showing a schematic configuration of a lithium ion secondary battery constructed using a negative electrode of a secondary battery according to one embodiment of the present invention. [Figure 4] 4 is a schematic exploded view showing the configuration of a wound electrode body of the lithium ion secondary battery of FIG. 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Matters not mentioned in this specification but necessary for carrying out the present invention can be understood as design matters for a person skilled in the art based on the prior art in the relevant field. The present invention can be carried out based on the contents disclosed in this specification and the technical common sense in the relevant field. In addition, in the following drawings, members and parts having the same function are described with the same reference numerals. Furthermore, the dimensional relationships (length, width, thickness, etc.) in each drawing do not reflect the actual dimensional relationships. In addition, the numerical range expressed as "A to B" in this specification includes A and B.

[0015] In this specification, the term "secondary battery" refers to an electricity storage device that can be repeatedly charged and discharged. In addition, in this specification, the term "lithium ion secondary battery" refers to a secondary battery that uses lithium ions as a charge carrier and realizes charging and discharging by the transfer of charge associated with the lithium ions between the positive and negative electrodes.

[0016] The negative electrode material according to the present embodiment contains Si-containing particles and graphite particles. The ratio of the average particle diameter D50 of the graphite particles to the average particle diameter D50 of the Si-containing particles is 1 to 8. The mass ratio of the Si-containing particles to the total of the Si-containing particles and the graphite particles is 10 mass% to 60 mass%. When 1 g of the Si-containing particles is uniaxially pressed at 60 MPa at 25°C to form a tablet having a diameter of 20 mm, the density of the resulting molded body is 0.9 g / cm. 3 That's all.

[0017] Fig. 1 is a schematic diagram showing a case where an example of the negative electrode material according to the present embodiment is used in a negative electrode. In the example shown in Fig. 1, the negative electrode material 10 contains graphite particles 12 and Si-containing particles 14. In the example shown in Fig. 1, the graphite particles 12 and the Si-containing particles 14 are mixed. The negative electrode material 10 is filled and arranged on a negative electrode current collector 62.

[0018] The graphite constituting the graphite particles 12 may be natural graphite or artificial graphite, or may be amorphous carbon-coated graphite in which graphite is coated with an amorphous carbon material.

[0019] 1, particles of a Si-C composite material are used as the Si-containing particles 14. The Si-containing particles 14 have carbon domains 14a and Si-containing domains 14b. The Si-containing domains 14b are dispersed in the carbon domains 14a, and thus the carbon domains 14a form a matrix.

[0020] The carbon domain 14a is, for example, a carbonized material of a carbon precursor (eg, petroleum pitch, coal pitch, phenolic resin, etc.); graphite, or the like.

[0021] The Si-containing domain 14b contains Si, and is, for example, Si, Si oxide (SiO x The Si-containing domain 14b is preferably made of Si and Si oxide (SiO x ) The Si-containing domains 14b may be fine particles. The number of the Si-containing domains 14b in the Si-containing particle 14 is not limited to that shown in the figure.

[0022] The average particle diameter of the Si-containing domains 14b is, for example, 50 nm or less, and may be 5 nm to 50 nm. The "average particle diameter of the Si-containing domains 14b" can be obtained as follows. First, a sample for scanning transmission electron microscope (STEM) observation of the negative electrode material 10 is prepared. For example, a negative electrode active material layer including the negative electrode material 10 is processed with FIB (focused ion beam) to prepare a sample for STEM observation. Then, the sample is subjected to elemental analysis by EDX element mapping, and then a BF image (bright field image) and a HAADF image (high angle scattering annular dark field image) are obtained. The diameter of the Si-containing domains 14b can be obtained from the contrast and shape obtained from the BF image and the HAADF image. The diameters of 10 or more arbitrarily selected Si-containing domains 14b are obtained, and the average value is defined as the "average particle diameter of the Si-containing domains 14b" here.

[0023] The Si content in the Si-containing particles 14 is not particularly limited. From the viewpoint of a higher capacity of the secondary battery, the Si content in the Si-containing particles 14 is preferably 20 mass% or more, more preferably 30 mass% or more, and further preferably 40 mass% or more. From the viewpoint of suppressing an excessive volume change of the Si-containing particles 14, the Si content in the Si-containing particles 14 is preferably 60 mass% or less, more preferably 50 mass% or less. In addition, the oxygen (O) content in the Si-containing particles 14 is not particularly limited, but is preferably 10 mass% or less. The Si content and O content in the Si-containing particles 14 can be determined by analysis based on high-frequency inductively coupled plasma (ICP) emission spectroscopy.

[0024] The Si-containing particles 14 are, for example, particles containing Si dispersed inside a carbon material; particles containing Si embedded in the pores of porous graphite granulated into a spherical shape; and the like.

[0025] The Si-containing particles 14 can be obtained according to a known method. For example, the particles can be obtained by mixing fine particles of Si, Si oxide, etc. with the carbon precursor, followed by carbonization and spheroidization. Alternatively, the particles can be obtained by mixing spherically granulated porous graphite with fine particles of Si, Si oxide, etc. in a dispersion medium, drying, and disposing the fine particles in the pores of the porous graphite.

[0026] However, the Si-containing particles 14 are not limited to those shown in the figures. The Si-containing particles may be carbon particles with fine particles containing Si attached to the surface; particles containing Si with fine carbon particles attached to the surface; etc. As shown in the figures, in the Si-C composite material, when the carbon domains 14a serve as a matrix and a plurality of Si-containing domains 14b are dispersed in the carbon domains 14a, the carbon domains 14a are advantageous in that they can reduce the volume change caused by the expansion / contraction of the Si-containing domains 14b. In addition, the Si-containing particles may be composited with elements other than carbon, or may be metal Si particles, Si oxide particles, etc. that are not composited with other elements.

[0027] In this embodiment, when 1 g of the Si-containing particle 14 is uniaxially pressed at 25° C. and 60 MPa to form a tablet having a diameter of 20 mm, the density of the resulting compact is 0.9 g / cm 3 The higher the density of the compact, the higher the packing of the particles. When 1 g of conventionally used Si-containing particles is molded in the same manner, the density of the compact is usually 0.9 / cm 3Therefore, in this embodiment, the Si-containing particles 14 having a higher packing property than the conventionally used Si-containing particles are used. By using the Si-containing particles 14 having such a higher packing property together with the graphite particles 12 at a specific content ratio and controlling the ratio of the average particle diameter (D50) of the Si-containing particles 14 to the graphite particles 12 within a specific range, it is possible to suppress the capacity degradation when the secondary battery is repeatedly charged and discharged.

[0028] The density of the molded body is preferably 0.95 g / cm 3 More preferably, it is 1.0 g / cm 3 On the other hand, the upper limit of the density of the molded body is 2.3 g / cm 3 Below 2.0g / cm 3 Below 1.8g / cm 3 or less than 1.5g / cm 3 It may be the following:

[0029] The density of the green body can be determined by weighing out 1 g of the Si-containing particles 14 into a mold having a diameter of 20 mm in a temperature environment of 25° C., applying a press pressure in one axial direction (i.e., a direction perpendicular to the radial direction) until a tablet-shaped green body is obtained, and measuring the bulk density of the green body. The density of the green body can be easily measured, for example, by using an automatic powder resistivity measuring system (e.g., “MCP-PD600” manufactured by Nitto Seiko Analytech Co., Ltd.) and a probe having a diameter of 20 mm (corresponding to a mold).

[0030] The density of the compact is affected by the circularity of the Si-containing particles 14. When the circularity of the Si-containing particles 14 is increased, the density of the compact tends to increase. Therefore, when the circularity of the Si-containing particles 14 is set to 0.85 to 1 (particularly 0.90 to 1), the density of the compact becomes 0.9 g / cm 3or more. In this specification, "circularity" refers to the ratio of the perimeter of a perfect circle having the same area as the projected area of ​​the particle to the perimeter of the projected image of the particle (i.e., circularity = perimeter of a perfect circle having the same area as the projected area of ​​the particle / perimeter of the projected image of the particle). Therefore, the closer the circularity is to 1, the closer the projected image of the particle is to a perfect circle, and the closer the particle is to a perfect sphere. The circularity can be determined, for example, by using a commercially available static automatic image analyzer to determine the circularity of 100 or more particles and calculating the average value.

[0031] Furthermore, the particle size of the Si-containing particles 14 also affects the density of the compact. When the average particle size of the Si-containing particles 14 is set to 2 μm to 10 μm (particularly, 5 μm to 10 μm), the density of the compact is 0.9 g / cm 3 The true density of the Si-containing particles 14 also affects the density of the compact. Therefore, by adjusting the composition of the Si-containing particles 14 (the content ratio of the constituent elements), the density of the compact can be finely adjusted.

[0032] There is no particular limitation on the circularity of the graphite particles 12. As the graphite particles 12, spheroidized graphite particles are preferred, and therefore the circularity of the graphite particles 12 is preferably 0.85 to 1, more preferably 0.88 to 1, and further preferably 0.90 to 1.

[0033] The ratio of the average particle diameter (D50) of the graphite particles 12 to the average particle diameter (D50) of the Si-containing particles 14 (D50 of the graphite-containing particles / D50 of the Si-containing particles) is 1 to 8. If the ratio (D50 of the graphite-containing particles / D50 of the Si-containing particles) is less than 1, the packing property is reduced due to the expansion / contraction of the Si-containing particles 14 during charging / discharging of the secondary battery, and the effect of improving the cycle characteristics of the secondary battery cannot be obtained. On the other hand, if the ratio (D50 of the graphite-containing particles / D50 of the Si-containing particles) exceeds 8, the dispersibility of the graphite particles 12 is reduced, and the aggregation of the Si-containing particles 14 occurs, which reduces the packing property. As a result, the effect of improving the cycle characteristics of the secondary battery cannot be obtained. The ratio (D50 of the graphite-containing particles / D50 of the Si-containing particles) is preferably 1.0 to 5.0, more preferably 1.2 to 3.0, and even more preferably 1.4 to 2.5.

[0034] In this specification, the term "average particle size (D50)" refers to the median size (D50), which is the particle size corresponding to a cumulative frequency of 50 volume % from the fine particle side with a small particle size in the volume-based particle size distribution based on the laser diffraction / scattering method. The average particle size (D50) can be determined using a commercially available laser diffraction / scattering type particle size distribution measuring device, etc.

[0035] The average particle diameter (D50) of the graphite particles 12 is not particularly limited as long as the ratio (D50 of the graphite-containing particles / D50 of the Si-containing particles) is 1 to 8. The average particle diameter (D50) of the graphite particles 12 is preferably 5 μm to 25 μm, more preferably 10 μm to 23 μm, and further preferably 12 μm to 20 μm.

[0036] The average particle diameter (D50) of the Si-containing particles 14 is not particularly limited as long as the ratio (D50 of graphite-containing particles / D50 of Si-containing particles) is 1 to 8. The average particle diameter (D50) of the Si-containing particles 14 is preferably 2 μm to 10 μm, more preferably 4 μm to 10 μm, and further preferably 6 μm to 9 μm.

[0037] The mass ratio of the Si-containing particles 14 to the total of the Si-containing particles 14 and the graphite particles 12 is 10 mass% to 60 mass%. If the mass ratio of the Si-containing particles 14 is less than 10 mass%, the capacity of the secondary battery is insufficient. If the mass ratio of the Si-containing particles 14 exceeds 60 mass%, the effect of the volume change of the Si-containing particles 14 becomes large, and the effect of suppressing capacity deterioration when the secondary battery is repeatedly charged and discharged becomes insufficient. The mass ratio of the Si-containing particles 14 is preferably 15 mass% to 55 mass%, and more preferably 20 mass% to 50 mass%.

[0038] The negative electrode material 10 can be obtained by mixing the Si-containing particles 14 and the graphite particles 12 according to a known method.

[0039] The negative electrode material 10 may further contain materials used in the negative electrode of a secondary battery, such as a binder and a conductive material.

[0040] According to the negative electrode material 10 of this embodiment, it is possible to suppress the capacity deterioration when the secondary battery is repeatedly charged and discharged. That is, when a negative electrode is produced using the negative electrode material 10 of this embodiment and a secondary battery is produced using this negative electrode, the secondary battery has excellent resistance to capacity deterioration when repeatedly charged and discharged, and therefore has excellent cycle characteristics. In addition, since the negative electrode material 10 of this embodiment contains Si, the secondary battery can have a high capacity. Furthermore, since the negative electrode material 10 of this embodiment contains Si-containing particles 14 with high packing property, the packing property of the negative electrode active material layer can be increased, and the energy density of the secondary battery can be increased.

[0041] Therefore, from another aspect, the negative electrode according to the present embodiment includes a negative electrode current collector and a negative electrode active material layer supported by the negative electrode current collector. The negative electrode active material layer contains the negative electrode material according to the above-mentioned embodiment. Such a negative electrode can impart excellent resistance to capacity degradation when repeatedly charged and discharged to the secondary battery. In addition, such a negative electrode can increase the capacity of the secondary battery. Furthermore, such a negative electrode can increase the energy density of the secondary battery.

[0042] The negative electrode according to this embodiment will be specifically described with reference to Fig. 2. Fig. 2 is a cross-sectional view showing a schematic example of a negative electrode 60 according to this embodiment, and is a cross-sectional view taken along the thickness direction and the width direction. The negative electrode 60 according to this embodiment shown in Fig. 2 is a negative electrode for a lithium ion secondary battery.

[0043] As shown in the figure, the negative electrode 60 includes a negative electrode current collector 62 and a negative electrode active material layer 64 supported by the negative electrode current collector 62. In other words, the negative electrode 60 includes the negative electrode current collector 62 and the negative electrode active material layer 64 provided on the negative electrode current collector 62. The negative electrode active material layer 64 may be provided on only one side of the negative electrode current collector 62, or may be provided on both sides of the negative electrode current collector 62 as in the illustrated example. The negative electrode active material layer 64 is preferably provided on both sides of the negative electrode current collector 62.

[0044] As shown in the illustrated example, a negative electrode active material layer non-forming portion 62a where no negative electrode active material layer 64 is provided may be provided at one end in the width direction of the negative electrode 60. In the negative electrode active material layer non-forming portion 62a, the negative electrode current collector 62 is exposed, and the negative electrode active material layer non-forming portion 62a can function as a current collector. However, the configuration for collecting current from the negative electrode 60 is not limited to this.

[0045] In the illustrated example, the shape of the negative electrode collector 62 is a foil (or sheet), but is not limited thereto. The negative electrode collector 62 may have various forms such as a rod, a plate, a mesh, etc. As with conventional lithium ion secondary batteries, the material of the negative electrode collector 62 may be a metal with good electrical conductivity (e.g., copper, nickel, titanium, stainless steel, etc.), and among these, copper is preferable. Copper foil is particularly preferable as the negative electrode collector 62.

[0046] The dimensions of the negative electrode current collector 62 are not particularly limited and may be appropriately determined depending on the battery design. When a copper foil is used as the negative electrode current collector 62, the thickness is not particularly limited, but is, for example, 5 μm or more and 35 μm or less, and preferably 6 μm or more and 20 μm or less.

[0047] The negative electrode active material layer 64 contains a negative electrode active material, and the negative electrode material 10 according to the above-described embodiment is used as this negative electrode active material. Thus, the negative electrode active material layer 64 contains the negative electrode material 10 according to the above-described embodiment.

[0048] The negative electrode active material layer 64 may contain components other than the negative electrode active material, examples of which include a binder and a conductive material. Examples of the binder that can be used include styrene butadiene rubber (SBR), carboxymethyl cellulose (CMC), polyacrylic acid (PAA), polyvinylidene fluoride (PVDF), and the like. CMC also functions as a thickener. Examples of the conductive material include carbon nanotubes (CNTs). When CNTs are used as the conductive material, the negative electrode active material layer 64 may contain a dispersant for CNTs.

[0049] The content of the negative electrode active material in the negative electrode active material layer 64 (i.e., relative to the total mass of the negative electrode active material layer 64) is preferably 90 mass% or more, and more preferably 95 mass% or more. The content of the binder in the negative electrode active material layer is preferably 0.1 mass% to 8 mass% or less, and more preferably 0.5 mass% to 5 mass% or less. The content of the conductive material in the negative electrode active material layer 64 is preferably 0.01 mass% to 3 mass% or less, and more preferably 0.05 mass% to 1 mass% or less.

[0050] The thickness of the negative electrode active material layer 64 is not particularly limited, but is, for example, not less than 10 μm and not more than 400 μm, and preferably not less than 20 μm and not more than 300 μm.

[0051] The density of the negative electrode active material layer 64 is not particularly limited, but is, for example, 0.9 g / cm 3 or more, preferably 1.1 g / cm 3 More preferably, it is 1.2 g / cm 3 On the other hand, the density of the negative electrode active material layer 64 is, for example, 2.3 g / cm 3 Less than or equal to 2.0 g / cm 3 It may be the following:

[0052] The negative electrode 60 may include members other than the negative electrode current collector 62 and the negative electrode active material layer 64. For example, an insulating layer (not shown) adjacent to the negative electrode active material layer 64 may be provided on the negative electrode active material layer non-forming portion 62a. The insulating layer contains, for example, an insulating inorganic filler or the like.

[0053] The negative electrode 60 can be suitably manufactured by a manufacturing method including a step of applying a negative electrode paste containing the negative electrode material according to the above-described embodiment to the negative electrode current collector 62 (hereinafter also referred to as a "coating step"), a step of drying the applied negative electrode paste to form a negative electrode active material layer 64 (hereinafter also referred to as a "drying step"), and a step of pressing the negative electrode active material layer 64 (hereinafter also referred to as a pressing step).

[0054] The coating process can be carried out according to a known method, except for using the negative electrode material according to the above embodiment. Specifically, for example, the negative electrode material according to the above embodiment and optional components (e.g., binder, conductive material, etc.) are mixed with a dispersion medium (e.g., water) using a known mixer, stirrer, etc. to prepare a negative electrode paste.

[0055] In this specification, the term "paste" refers to a mixture in which a part or all of the solid content is dispersed in a dispersion medium, and includes so-called "slurry", "ink", and the like.

[0056] The coating step can be performed by applying the negative electrode paste onto the negative electrode current collector 62 using a coating device such as a gravure coater, a comma coater, a slit coater, or a die coater.

[0057] The drying step can be carried out according to a known method. Specifically, for example, the dispersion medium is removed from the negative electrode current collector 62 on which the negative electrode paste is applied, using a drying device such as a drying oven, to form the negative electrode active material layer 64. This allows the drying step to be carried out. The drying temperature and drying time may be appropriately determined according to the solid content concentration of the negative electrode paste, and are not particularly limited. The drying temperature is, for example, 60°C or higher and 200°C or lower, and preferably 70°C or higher and 150°C or lower. The drying time is, for example, 10 seconds or higher and 30 minutes or lower, and preferably 30 seconds or higher and 10 minutes or lower.

[0058] The pressing step can be carried out according to a known method. Specifically, the pressing step can be carried out by applying pressure to the negative electrode active material layer 64 formed above using a roller press or the like. The pressing step can densely pack the graphite particles 12 and the Si-containing particles 14 contained in the negative electrode material 10. In this way, the negative electrode 60 is obtained.

[0059] The negative electrode 60 can be used in a secondary battery according to a known method. A secondary battery typically includes a positive electrode, a negative electrode, and an electrolyte, and the negative electrode is the above-mentioned negative electrode 60. A configuration example of a secondary battery using the negative electrode 60 will be described in detail below with reference to Figs. 3 and 4. The configuration example is a flat prismatic lithium ion secondary battery having a flat wound electrode body and a flat battery case.

[0060] The lithium ion secondary battery 100 shown in FIG. 3 is a sealed lithium ion secondary battery 100 constructed by housing a flat wound electrode body 20 and a nonaqueous electrolyte (not shown) in a flat rectangular battery case (i.e., an outer container) 30. The battery case 30 is provided with a positive electrode terminal 42 and a negative electrode terminal 44 for external connection, and a thin-walled safety valve 36 that is set to release the internal pressure when the internal pressure of the battery case 30 rises to a predetermined level or higher. The battery case 30 is also provided with an injection port (not shown) for injecting the nonaqueous electrolyte. The positive electrode terminal 42 is electrically connected to a positive electrode current collector plate 42a. The negative electrode terminal 44 is electrically connected to a negative electrode current collector plate 44a. The material of the battery case 30 is, for example, a lightweight metal material with good thermal conductivity, such as aluminum.

[0061] As shown in Fig. 3 and Fig. 4, the wound electrode body 20 has a configuration in which a positive electrode sheet 50 and a negative electrode sheet 60 are overlapped with two long separator sheets 70 interposed therebetween and wound in the longitudinal direction. The positive electrode sheet 50 has a configuration in which a positive electrode active material layer 54 is formed along the longitudinal direction on one or both sides (both sides here) of a long positive electrode current collector 52. The negative electrode sheet 60 has a configuration in which a negative electrode active material layer 64 is formed along the longitudinal direction on one or both sides (both sides here) of a long negative electrode current collector 62. The positive electrode active material layer-free portion 52a (i.e., a portion where the positive electrode active material layer 54 is not formed and the positive electrode current collector 52 is exposed) and the negative electrode active material layer-free portion 62a (i.e., a portion where the negative electrode active material layer 64 is not formed and the negative electrode current collector 62 is exposed) are formed so as to protrude outward from both ends in the winding axis direction (i.e., the sheet width direction perpendicular to the longitudinal direction) of the wound electrode body 20. The positive electrode active material layer-free portion 52a and the negative electrode active material layer-free portion 62a are joined to the positive electrode current collector 42a and the negative electrode current collector 44a, respectively.

[0062] The positive electrode current collector 52 constituting the positive electrode sheet 50 may be a known positive electrode current collector used in lithium ion secondary batteries, and examples thereof include a sheet or foil made of a metal having good electrical conductivity (e.g., aluminum, nickel, titanium, stainless steel, etc.). The positive electrode current collector 52 is preferably aluminum foil.

[0063] The dimensions of the positive electrode current collector 52 are not particularly limited and may be appropriately determined depending on the battery design. When an aluminum foil is used as the positive electrode current collector 52, the thickness is not particularly limited, but is, for example, 5 μm or more and 35 μm or less, and preferably 7 μm or more and 20 μm or less.

[0064] The positive electrode active material layer 54 contains a positive electrode active material. As the positive electrode active material, a positive electrode active material having a known composition used in a lithium ion secondary battery may be used. Specifically, for example, as the positive electrode active material, a lithium composite oxide, a lithium transition metal phosphate compound, or the like may be used. The crystal structure of the positive electrode active material is not particularly limited, and may be a layered structure, a spinel structure, an olivine structure, or the like.

[0065] The lithium composite oxide is preferably a lithium transition metal composite oxide containing at least one of Ni, Co, and Mn as a transition metal element, and specific examples thereof include lithium nickel-based composite oxides, lithium cobalt-based composite oxides, lithium manganese-based composite oxides, lithium nickel manganese-based composite oxides, lithium nickel cobalt manganese-based composite oxides, lithium nickel cobalt aluminum-based composite oxides, and lithium iron nickel manganese-based composite oxides.

[0066] In this specification, the term "lithium nickel cobalt manganese composite oxide" includes oxides containing Li, Ni, Co, Mn, and O as constituent elements, as well as oxides containing one or more additional elements other than those. Examples of such additional elements include transition metal elements and typical metal elements such as Mg, Ca, Al, Ti, V, Cr, Y, Zr, Nb, Mo, Hf, Ta, W, Na, Fe, Zn, and Sn. The additional element may be a semimetal element such as B, C, Si, or P, or a nonmetal element such as S, F, Cl, Br, or I. This also applies to the above-mentioned lithium nickel composite oxide, lithium cobalt composite oxide, lithium manganese composite oxide, lithium nickel manganese composite oxide, lithium nickel cobalt aluminum composite oxide, and lithium iron nickel manganese composite oxide.

[0067] Examples of the lithium transition metal phosphate compound include lithium iron phosphate (LiFePO4), lithium manganese phosphate (LiMnPO4), and lithium manganese iron phosphate.

[0068] These positive electrode active materials may be used alone or in combination of two or more. As the positive electrode active material, lithium nickel cobalt manganese based composite oxide is particularly preferable because of its excellent properties such as initial resistance characteristics.

[0069] The average particle diameter (D50) of the positive electrode active material is not particularly limited, but is, for example, 0.05 μm or more and 25 μm or less, preferably 1 μm or more and 20 μm or less, and more preferably 3 μm or more and 15 μm or less.

[0070] The positive electrode active material layer 54 may contain components other than the positive electrode active material, such as trilithium phosphate, a conductive material, a binder, etc. As the conductive material, for example, carbon black such as acetylene black (AB), carbon fibers such as vapor grown carbon fiber (VGCF) and carbon nanotubes (CNT), and other carbon materials (e.g., graphite, etc.) can be suitably used. As the binder, for example, polyvinylidene fluoride (PVdF) can be used.

[0071] The content of the positive electrode active material in the positive electrode active material layer 54 (i.e., the content of the positive electrode active material relative to the total mass of the positive electrode active material layer 54) is not particularly limited, but is preferably 70 mass% or more, more preferably 80 mass% or more, and even more preferably 85 mass% or more and 99 mass% or less. The content of the trilithium phosphate in the positive electrode active material layer 54 is not particularly limited, but is preferably 0.1 mass% or more and 15 mass% or less, and more preferably 0.2 mass% or more and 10 mass% or less. The content of the conductive material in the positive electrode active material layer 54 is not particularly limited, but is preferably 0.1 mass% or more and 20 mass% or less, and more preferably 0.3 mass% or more and 15 mass% or less. The content of the binder in the positive electrode active material layer 54 is not particularly limited, but is preferably 0.4 mass% or more and 15 mass% or less, and more preferably 0.5 mass% or more and 10 mass% or less.

[0072] The thickness of the positive electrode active material layer 54 per side is not particularly limited, but is usually 10 μm or more, and preferably 20 μm or more. On the other hand, the thickness is usually 400 μm or less, and preferably 300 μm or less.

[0073] The negative electrode sheet 60 is a negative electrode 60 using the above-mentioned negative electrode material 10 as a negative electrode active material.

[0074] The separator 70 may be a porous sheet (film) made of a resin such as polyethylene (PE), polypropylene (PP), polyester, cellulose, or polyamide. Such a porous sheet may have a single-layer structure or a laminated structure of two or more layers (for example, a three-layer structure in which a PP layer is laminated on both sides of a PE layer). A heat-resistant layer (HRL) may be provided on the surface of the separator 70.

[0075] The thickness of the separator 70 is not particularly limited, but is, for example, 5 μm to 50 μm, and preferably 10 μm to 30 μm. The air permeability of the separator 70 obtained by the Gurley test method is not particularly limited, but is preferably 350 sec / 100 cc or less.

[0076] The non-aqueous electrolyte typically contains a non-aqueous solvent and a supporting salt (electrolyte salt). As the non-aqueous solvent, organic solvents such as carbonates, ethers, esters, nitriles, sulfones, and lactones, which are used in electrolytes of general lithium ion secondary batteries, can be used without any particular limitation. Among them, carbonates are preferable, and specific examples thereof include ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), monofluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), monofluoromethyl difluoromethyl carbonate (F-DMC), and trifluorodimethyl carbonate (TFDMC). Such non-aqueous solvents can be used alone or in appropriate combination of two or more. As an example, the non-aqueous solvent is composed of only carbonates. As another example, non-aqueous solvents include carbonates and esters, such as methyl acetate.

[0077] As the supporting salt, for example, a lithium salt such as LiPF6, LiBF4, lithium bis(fluorosulfonyl)imide (LiFSI) (preferably LiPF6) can be suitably used. The concentration of the supporting salt is preferably 0.7 mol / L or more and 1.3 mol / L or less.

[0078] The nonaqueous electrolyte may contain various additives other than the above-mentioned components, such as film-forming agents such as vinylene carbonate (VC) and oxalate complexes; gas generating agents such as biphenyl (BP) and cyclohexylbenzene (CHB); and thickeners, as long as the effects of the present invention are not significantly impaired.

[0079] The lithium ion secondary battery 100 is suppressed from deteriorating in capacity when repeatedly charged and discharged, and has a high capacity. The lithium ion secondary battery 100 can be used for various applications. Suitable applications include a driving power source mounted on vehicles such as electric vehicles (BEVs), hybrid vehicles (HEVs), and plug-in hybrid vehicles (PHEVs). The lithium ion secondary battery 100 can also be used as a storage battery for small power storage devices and the like. The lithium ion secondary battery 100 can also be used in the form of a battery pack in which a plurality of lithium ion secondary batteries 100 are typically connected in series and / or parallel.

[0080] The above describes, as an example, a rectangular lithium ion secondary battery 100 equipped with a flat wound electrode assembly 20. However, the lithium ion secondary battery can also be configured as a lithium ion secondary battery equipped with a laminated electrode assembly (i.e., an electrode assembly in which multiple positive electrodes and multiple negative electrodes are alternately laminated). The lithium ion secondary battery can also be configured as a cylindrical lithium ion secondary battery, a laminated case type lithium ion secondary battery, etc.

[0081] Furthermore, the lithium ion secondary battery 100 can also be constructed as an all-solid-state lithium ion secondary battery using a solid electrolyte instead of a non-aqueous electrolyte according to known methods.

[0082] Furthermore, although the negative electrode 60 according to this embodiment is suitable for use as a negative electrode for a lithium ion secondary battery, it can also be used as a negative electrode for other secondary batteries, and the other secondary batteries can be constructed according to known methods.

[0083] Examples of the present invention will be described in detail below, but it is not intended that the present invention be limited to those shown in these examples.

[0084] <Preparation of negative electrode material> Example 1 Particles of a Si-C composite material having an average particle size (D50) of 8 μm, a Si content of 40 mass %, and a circularity of 0.98 were prepared as Si-containing particles.

[0085] The density of the compact was measured by the method described below when 1 g of the Si-containing particles was pressed uniaxially at 25°C and 60 MPa to form a tablet with a diameter of 20 mm. The value of the density of the compact was 1.3 g / cm 3 .

[0086] Graphite particles with an average particle diameter (D50) of 18 μm were prepared. The negative electrode material of Example 1 was obtained by mixing the graphite particles and the Si-containing particles at a mass ratio of 60:40.

[0087] [Examples 2 to 3 and Comparative Examples 1 to 3] Particles of an Si-C composite material having an average particle diameter (D50), Si content, and circularity shown in Table 1 were prepared as the Si-containing particles. The density of the compact was measured by the method described below when 1 g of the Si-containing particles was pressed uniaxially at 25°C and 60 MPa to form a tablet with a diameter of 20 mm. The density of the compact is shown in Table 1.

[0088] Also, graphite particles having an average particle diameter (D50) shown in Table 1 were prepared. The negative electrode materials of Examples 2 to 3 and Comparative Examples 1 to 3 were obtained by mixing the graphite particles and the Si-containing particles at a mass ratio of 60:40. In each example and each comparative example, the average particle diameter (D50) of the Si-containing particles and the graphite particles, the Si content in the Si-containing particles, and the circularity of the Si-containing particles were determined by the following methods.

[0089] [Measurement of the average particle diameter (D50) of Si-containing particles and graphite particles] Using a commercially available laser diffraction particle size distribution analyzer, the particle size distribution measurements of the Si-containing particles and the graphite particles were performed based on volume, respectively, and the particle diameter corresponding to a cumulative frequency of 50% by volume from the side of the fine particles with a small particle diameter was determined as the average particle diameter (D50) of the Si-containing particles and the graphite particles.

[0090] [Measurement of the Si content of Si-containing particles] Using a commercially available ICP analyzer, the Si content in the Si-containing particles was determined as mass%.

[0091] <Measurement of Circularity of Si-Containing Particles> Using a commercially available image-based particle size distribution measuring device, the circularity of Si-containing particles was determined as the perimeter of a perfect circle having the same area as the projected area of the particles / the perimeter of the particle projection image.

[0092] <Measurement of Density of Formed Body of Si-Containing Particles> 1 g of Si-containing particles was weighed as a powder measurement sample and set on a probe (diameter 20 mm) of an automatic powder resistance measurement system "MCP-PD600" (manufactured by Nitto Seiko Analytic Co., Ltd.). At 25°C, using this automatic powder resistance measurement system, the load and displacement when pressurized in a uniaxial direction were measured. Based on this, the bulk density of the formed body at a pressure of 60 MPa was determined.

[0093] <Fabrication of Negative Electrode and Lithium-Ion Secondary Battery for Evaluation> As binders, carboxymethyl cellulose (CMC), polyacrylic acid (PAA), and styrene-butadiene rubber (SBR) were prepared. Also, a dispersion of single-walled carbon nanotubes (SWCNT) as a conductive material was prepared. The negative electrode material, CMC, and PAA of each example and each comparative example were dry-blended using a planetary mixer. The obtained mixture, the SWCNT dispersion, and the dispersion medium were kneaded using a planetary mixer. To this, SBR and further the dispersion medium were added and uniformly mixed to prepare a negative electrode paste. In the negative electrode paste, the mass ratio of negative electrode material:CMC:PAA:SBR:SWCNT was 100:1:1:1.5:0.1.

[0094] The prepared negative electrode paste was applied to the surface of a copper foil with a thickness of 10 μm and dried to form a negative electrode active material layer. After roll-pressing the negative electrode active material layer, the obtained sheet was processed into a predetermined size to obtain a negative electrode sheet.

[0095] LiNi as the positive electrode active material powder 1 / 3 Co 1 / 3 Mn 1 / 3O2 (NCM), acetylene black (AB) as a conductive material, and polyvinylidene fluoride (PVdF) as a binder were mixed with N-methylpyrrolidone (NMP) in a mass ratio of NCM:AB:PVdF = 100:1:1 to prepare a positive electrode paste. This paste was applied to the surface of an aluminum foil with a thickness of 15 μm and dried to form a positive electrode active material layer. After the positive electrode active material layer was roll-pressed, the resulting sheet was processed to a predetermined size to obtain a positive electrode sheet.

[0096] A separator made of porous polyolefin was prepared. A lead was attached to each of the negative electrode sheet and the positive electrode sheet prepared above, and the sheets were laminated with a separator interposed therebetween to prepare an electrode body. This was housed in a case made of an aluminum laminate film together with a non-aqueous electrolyte. The non-aqueous electrolyte was a mixed solvent containing ethylene carbonate (EC), fluoroethylene carbonate (FEC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of 15:5:40:40, in which LiPF6 was dissolved as a supporting salt at a concentration of 1.0 mol / L. The case was then sealed to obtain a lithium ion secondary battery for evaluation.

[0097] <Cycle characteristic evaluation> Each of the lithium ion secondary batteries for evaluation prepared above was placed in an environment of 25° C. Each of the lithium ion secondary batteries for evaluation was charged at a constant current of 0.4 C to 4.2 V, and then charged at a constant voltage until the current value reached 0.1 C. Next, each of the lithium ion secondary batteries for evaluation was discharged at a constant current of 0.4 C to 2.5 V. The discharge capacity at this time was measured to obtain the initial capacity.

[0098] The above charge / discharge cycle was repeated 200 times. The discharge capacity after 200 cycles was determined in the same manner as the initial capacity. As an index of cycle characteristics, the capacity retention rate (%) was calculated by (discharge capacity after 200 charge / discharge cycles / initial capacity)×100. The results are shown in Table 1.

[0099] [Table 1]

[0100] From the results in Table 1, it is clear that the ratio of the average particle size (D50) of the graphite particles to the average particle size (D50) of the Si-containing particles is 1 to 8, the mass ratio of the Si-containing particles to the total of the Si-containing particles and the graphite particles is 10 mass% to 60 mass%, and when 1 g of the Si-containing particles is pressed uniaxially at 25°C and 60 MPa to form a tablet having a diameter of 20 mm, the density of the resulting molded body is 0.9 g / cm 3 It can be seen that the capacity retention rate after 200 charge / discharge cycles is significantly high when the negative electrode material disclosed herein is above this level, and therefore it can be seen that the capacity degradation caused by repeated charge / discharge of the secondary battery can be suppressed.

[0101] Although the specific examples of the present invention have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and changes of the specific examples exemplified above.

[0102] That is, the negative electrode material, the negative electrode of a secondary battery, and the method for producing the same disclosed herein are the following items [1] to [8]. [1] A negative electrode material containing Si-containing particles and graphite particles, a ratio of an average particle size (D50) of the graphite particles to an average particle size (D50) of the Si-containing particles is 1 to 8; a mass ratio of the Si-containing particles to the total of the Si-containing particles and the graphite particles is 10 mass% to 60 mass%, When 1 g of the Si-containing particles is pressed uniaxially at 25° C. and 60 MPa to form a tablet having a diameter of 20 mm, the density of the resulting molded body is 0.9 g / cm 3 That's it for the negative electrode material. [2] The negative electrode material according to item [1], wherein the Si-containing particles have an average particle size (D50) of 2 μm to 10 μm, and the graphite particles have an average particle size (D50) of 5 μm to 25 μm. [3] The negative electrode material according to item [1] or [2], wherein the ratio of the average particle size (D50) of the graphite particles to the average particle size (D50) of the Si-containing particles is 1.2 to 3.0. [4] The negative electrode material according to any one of items [1] to [3], wherein a mass ratio of the Si-containing particles to a total of the Si-containing particles and the graphite particles is 20 mass% to 50 mass%. [5] The negative electrode material according to any one of items [1] to [4], wherein the Si-containing particles are particles of a Si-C composite material in which Si-containing domains are dispersed in a carbon matrix. [6] The negative electrode material according to item [5], wherein the Si content in the Si-containing particles is 20% by mass or more and 60% by mass or less. [7] A negative electrode current collector; a negative electrode active material layer supported on the negative electrode current collector; A negative electrode of a secondary battery comprising: The negative electrode active material layer contains the negative electrode material according to any one of items [1] to [6]. [8] A step of applying a negative electrode paste containing the negative electrode material according to any one of items [1] to [6] to a negative electrode current collector; drying the applied negative electrode paste to form a negative electrode active material layer; pressing the negative electrode active material layer; A method for manufacturing a negative electrode of a secondary battery, comprising the steps of: [Explanation of symbols]

[0103] 10. Anode materials 12 Graphite particles 14 Si-containing particles 14a Carbon domain 14b Si-containing domain 20 Wound electrode body 30 Battery case 36 Safety valve 42 Positive terminal 42a Positive current collector 44 Negative terminal 44a Negative current collector plate 50 Positive electrode sheet (positive electrode) 52 Positive electrode current collector 52a Portion where positive electrode active material layer is not formed 54 Cathode active material layer 60 Negative electrode sheet (negative electrode) 62 Negative electrode current collector 62a Part where negative electrode active material layer is not formed 64 Negative electrode active material layer 70 Separator sheet (separator) 100 Lithium-ion secondary battery

Claims

1. A negative electrode material containing Si-containing particles and graphite particles, a ratio of an average particle size (D50) of the graphite particles to an average particle size (D50) of the Si-containing particles is 1 to 8; a mass ratio of the Si-containing particles to a total of the Si-containing particles and the graphite particles is 10 mass% to 60 mass%; When 1 g of the Si-containing particles is pressed uniaxially at 25° C. and 60 MPa to form a tablet having a diameter of 20 mm, the density of the resulting molded body is 0.9 g / cm 3 That's it for the negative electrode material.

2. 2. The negative electrode material according to claim 1, wherein the Si-containing particles have an average particle size (D50) of 2 μm to 10 μm, and the graphite particles have an average particle size (D50) of 5 μm to 25 μm.

3. 2. The negative electrode material according to claim 1, wherein the ratio of the average particle size (D50) of the graphite particles to the average particle size (D50) of the Si-containing particles is 1.2 to 3.

0.

4. 2. The negative electrode material according to claim 1, wherein a mass ratio of the Si-containing particles to a total of the Si-containing particles and the graphite particles is 20 mass% to 50 mass%.

5. 2. The negative electrode material of claim 1, wherein the Si-containing particles are particles of a Si-C composite having Si-containing domains dispersed in a carbon matrix.

6. The negative electrode material according to claim 5 , wherein the Si-containing particle has a Si content of 20% by mass or more and 60% by mass or less.

7. A negative electrode current collector; a negative electrode active material layer supported on the negative electrode current collector; A negative electrode of a secondary battery comprising: The negative electrode of a secondary battery, wherein the negative electrode active material layer contains the negative electrode material according to claim 1 .

8. A step of applying a negative electrode paste containing the negative electrode material according to claim 1 to a negative electrode current collector; drying the applied negative electrode paste to form a negative electrode active material layer; pressing the negative electrode active material layer; A method for manufacturing a negative electrode of a secondary battery, comprising the steps of:

Citation Information

Patent Citations

  • Carbon material for nonaqueous secondary battery negative electrode, negative electrode for nonaqueous secondary battery and nonaqueous secondary battery

    JP2015164127A

  • Negative electrode for nonaqueous-electrolyte secondary battery, and nonaqueous-electrolyte secondary battery

    WO2021172005A1

  • Preparation of silicon composite material, and negative electrode plate containing same

    WO2022135096A1

  • Carbon material for nonaqueous secondary battery negative electrode, negative electrode for nonaqueous secondary battery using the same, and nonaqueous secondary battery

    JP2015038862A

Cited By

  • Negative electrode plate and manufacturing method for non-aqueous electrolyte secondary batteries

    CN123120620A