Operation method of self-fluxing furnace

By calculating liquidus temperatures and adjusting the flow of smelting raw materials in a flash-smelting furnace, the method promotes efficient slag production and complete reactions, improving matte sedimentation and yield.

JP2024159128APending Publication Date: 2024-11-08SUMITOMO METAL MINING CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023074918
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing methods for operating flash-smelting furnaces do not effectively facilitate quick slag production within the reaction shaft, leading to incomplete reactions and unreacted copper concentrate and flux reaching the settler.

Method used

A method involving thermodynamic equilibrium calculations to determine the liquidus temperature of slag based on oxygen partial pressure, adjusting the flow of smelting raw materials to collide and react in a high-temperature region within the reaction shaft, and using dispersion cones and gas flow adjustments to promote mixing.

Benefits of technology

This approach enhances slag production efficiency, improves matte sedimentation, and increases matte yield by ensuring complete reactions within the reaction shaft.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159128000002
    Figure 2024159128000002
  • Figure 2024159128000003
    Figure 2024159128000003
  • Figure 2024159128000004
    Figure 2024159128000004
Patent Text Reader

Abstract

To provide an operation method of a self-fluxing furnace capable of efficiently realizing slag formation reaction in the self-fluxing furnace.SOLUTION: Provided is an operation method of a self-fluxing furnace that forms a matte and a slag by reacting with a reaction gas supplied into a reactor while refining raw materials, including a copper concentrate and a flux, supplied from a top of the reactor, fall toward a settler. The operation method of the self-fluxing furnace includes the following steps: performing thermodynamic equilibrium calculation using the composition of the slag assumed to be formed from the composition of the refining raw materials, and grasping a relation between an oxygen partial pressure and a liquidus temperature of the slag in the reactor; calculating, from the relation between the oxygen partial pressure and the liquidus temperature of the slag and oxygen partial pressures at one or more positions in the reactor obtained by measurement or calculation, liquidus temperatures at these positions; and adjusting the flow of the refining raw materials such that the refining raw materials flow in an area where an in-furnace temperature is higher than the liquidus temperature and promoting the collision of the copper concentrate and the flux in the area.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for operating a flash smelting furnace. [Background technology]

[0002] Copper sulfide concentrate (copper concentrate) is a powdered solid sulfide, etc., which is supplied as a smelting raw material to a flash smelting furnace (hereinafter referred to as a flash furnace), which is a type of smelting furnace, and is separated into two types of solutions, mainly matte and slag.

[0003] In the flash smelting furnace, copper concentrate, silica sand containing silicon dioxide, and auxiliary fuel such as heavy oil are blown into the reaction shaft together with reactive gas such as oxygen-enriched air delivered separately from a concentrate burner installed at the top of the reaction tower (reaction shaft). In the reaction shaft, the copper concentrate reacts with the reactive gas to produce two types of solutions (matte and slag), which fall in the form of droplets through the reaction shaft and are collected in a settler. In the settler, the matte and slag are separated into layers due to the difference in their specific gravities, and a matte layer and a slag layer are formed in that order from the bottom side of the settler.

[0004] In order to effectively separate the matte and slag in the settler, it is necessary to increase the fluidity of the slag and promote the settling of the matte, but it is difficult to obtain an optimal slag composition using copper concentrate alone.

[0005] In view of this, for example, a method has been proposed in which, when processing matte from copper concentrate in a flash smelting furnace, a flux such as silica stone, limestone, iron ore, or the like is added as a melting material together with the copper concentrate, and a eutectic composition is utilized to obtain slag at a temperature lower than the melting point of the oxide (see, for example, Patent Document 1).

[0006] In addition, in Patent Document 1, a blower nozzle for blowing a reactive gas is installed on the side wall of the reaction shaft, and the copper concentrate, flux, and reactive gas are mixed uniformly within the reaction shaft to cause the smelting raw materials to react.

[0007] As another method for promoting the mixing of copper concentrate and flux in the reaction shaft, for example, there is a method of providing a dispersion cone on the auxiliary fuel burner of the concentrate burner. Also, a method has been proposed in which a concentrate dispersion regulator is fitted so as to be movable up and down, and the height position of the concentrate dispersion regulator is changed by moving a hanging bolt connected to the concentrate dispersion regulator up and down, thereby adjusting the wind speed of the reaction gas and burning the smelting raw material (for example, see Patent Document 2). [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Patent No. 5500115 [Patent Document 2] JP 2002-60859 A Summary of the Invention [Problem to be solved by the invention]

[0009] However, Patent Documents 1 and 2 do not disclose a specific method for obtaining slag in the reaction shaft as early as possible. In the methods of Patent Documents 1 and 2, slag cannot be sufficiently generated in the reaction shaft, and the copper concentrate and flux may reach the settler unreacted. In the process of producing matte from copper concentrate in a flash smelting furnace, it is desirable to efficiently realize the reaction between the copper concentrate and the flux in the reaction shaft and obtain slag as early as possible.

[0010] An object of one aspect of the present invention is to provide a method for operating a flash smelting furnace that can efficiently realize a slag formation reaction in the flash smelting furnace. [Means for solving the problem]

[0011] One aspect of a method for operating a flash melting furnace according to the present invention comprises: A method for operating a flash smelting furnace, in which a smelting raw material containing copper concentrate and flux, supplied from the top of a reaction tower, falls toward a settler located below the reaction tower and reacts with a reaction gas supplied into the reaction tower to produce matte and slag, comprising: A step of performing a thermodynamic equilibrium calculation using a composition of the slag assumed to be generated from the composition of the smelting raw material, and grasping a relationship between an oxygen partial pressure in the reaction tower and a liquidus temperature of the slag; calculating the liquidus temperature at one or more positions in the reaction tower from a relationship between the oxygen partial pressure and the liquidus temperature of the slag and the oxygen partial pressure at the positions obtained by measurement or calculation; The method for operating a flash smelting furnace includes adjusting a flow of the smelting raw material so that the smelting raw material flows into a region where the temperature inside the furnace is higher than the liquidus temperature, and promoting collision between the copper concentrate and the flux in the region. Effect of the Invention

[0012] One aspect of the method for operating a flash smelting furnace according to the present invention can efficiently realize a slag generating reaction in the flash smelting furnace. [Brief description of the drawings]

[0013] [Figure 1] 1 is a diagram showing a schematic configuration of a flash melting furnace to which a method for operating a flash melting furnace according to an embodiment of the present invention is applied; [Diagram 2] FIG. 2 is a diagram showing an example of the relationship between the oxygen partial pressure and the liquidus temperature of FeO and SiO2. [Diagram 3] FIG. 13 is a diagram showing the calculation results of the relationship between the oxygen partial pressure pO2 and the liquidus temperature of the slag in the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, the embodiments of the present invention will be described in detail. In order to facilitate understanding of the description, the same components in each drawing are given the same reference numerals, and duplicated descriptions will be omitted. In addition, the scale of each member in the drawings may differ from the actual scale. In this specification, "~" indicating a numerical range means that the numerical values ​​before and after it are included as the lower and upper limits, unless otherwise specified.

[0015] Before describing the method for operating a flash smelting furnace according to the embodiment of the present invention, the configuration of a flash smelting furnace (flash furnace) to which the method for operating a flash smelting furnace according to the embodiment of the present invention is applied will be described.

[0016] <Self-melting furnace> Fig. 1 is a diagram showing a schematic configuration of a flash smelting furnace to which a method of operating a flash smelting furnace according to the present embodiment is applied. As shown in Fig. 1, the flash smelting furnace 1 includes a reaction tower (reaction shaft) 10, a settler 20, and an exhaust flue 30. The flash smelting furnace 1 produces two types of solutions, slag and matte (copper content 60% to 65%), from copper concentrate (copper content 20% to 30%) and flux, which are smelting raw materials SP supplied to the reaction shaft 10, in the reaction shaft 10, and separates the slag and matte into layers in the settler 20 to recover matte with a high copper content.

[0017] The smelting raw material refers to valuable minerals containing the target metal to be extracted, useless minerals (gangue), etc., and includes copper concentrate, flux, etc. In this embodiment, a case where the smelting raw material contains copper concentrate and flux will be described.

[0018] Copper concentrate is copper ore having a particle size of, for example, 1 μm to 300 μm, and is a powdered solid sulfide (Cu-Fe-S) containing copper, iron, and sulfur. Copper concentrate is oxidized by oxygen-enriched air in the flash smelting furnace 1 and contains iron oxide (FeOx), which is an Fe oxide. The Fe oxide contained in the copper concentrate may have the form of FeO, Fe3O4, Fe2O3, etc.

[0019] Fluxes are silica, limestone, iron ore, etc., and are used as welding materials.

[0020] Silica sand is a mineral whose main component is SiO2. Silica sand contains SiO2, etc. The composition of silica sand can be determined by chemical analysis and X-ray fluorescence analysis.

[0021] Matte is a mixture containing copper sulfide (Cu2S) and iron sulfide (FeS) as its main components, and is a solution containing a large amount of Cu.

[0022] Slag is a solution whose main component is silicate (2FeOx-SiO2) of iron oxide (FeOx), and contains a large amount of Fe.

[0023] The flash smelting furnace 1 supplies the smelting raw material SP, including copper concentrate and flux, into the reaction shaft 10.

[0024] The reaction shaft 10 is a hollow structure having a bottomed cylindrical top. The reaction shaft 10 is provided with a concentrate burner 11 at the top 10a. The number of the concentrate burners 11 may be one or more.

[0025] The concentrate burner 11 injects the smelting raw material SP, auxiliary fuel such as heavy oil, and a reaction gas RA such as oxygen-enriched air that is delivered separately into the reaction shaft 10 from the top 10a of the reaction shaft 10. The concentrate burner 11 can adjust the flow rate of the smelting raw material SP injected into the reaction shaft 10 by adjusting the flow rate of the reaction gas RA.

[0026] The concentrate burner 11 includes a concentrate chute 111 through which the raw material SP is supplied from the outside into the furnace, and an auxiliary fuel burner 112 is provided inside the concentrate chute 111. A concentrate dispersion regulator (not shown) may be provided inside the auxiliary fuel burner 112 so as to be movable in the vertical direction. A suspension bolt (not shown) may be provided on the outer periphery of the auxiliary fuel burner 112, and the concentrate dispersion regulator (not shown) may be configured to move in the vertical direction by moving the suspension bolt (not shown) in the vertical direction. The concentrate burner 11 may adjust the flow rate of the smelting raw material SP that is ejected and adjust the dispersion of the smelting raw material SP into the reaction shaft 10 by moving the concentrate dispersion regulator (not shown) in the vertical direction of the fuel burner and changing its height position.

[0027] The concentrate burner 11 may be provided at its tip with a dispersion cone 113 diverging downward, and the angle of the dispersion cone 113 may be adjusted. The concentrate burner 11 may adjust the degree of dispersion of the smelting raw material SP ejected from the concentrate burner 11 into the reaction shaft 10 by adjusting the angle of the dispersion cone 113. The angle of the dispersion cone 113 is not particularly limited, and may be any angle depending on the type, composition, flow rate, etc. of the smelting raw material SP.

[0028] Furthermore, the reaction shaft 10 may be provided with a gas supply nozzle 12 that supplies a gas such as an inert gas to the side wall 10b. The reaction shaft 10 may change the direction of the flow of the smelting raw material SP by blowing gas into the reaction shaft 10 from the vent or the inspection hole by the gas supply nozzle 12. The number of gas supply nozzles 12 may be one or more. When a plurality of gas supply nozzles 12 are provided, the plurality of gas supply nozzles 12 may be arranged above and below the side wall 10b, or may be arranged around the axis. The gas supply nozzle 12 may be provided so as to penetrate into the reaction shaft 10 through a vent or inspection hole provided in the side wall 10b. Examples of the inert gas include N2 gas, Ar gas, and the like. The gas supply nozzle 12 may be used as a blowing nozzle that blows the reaction gas.

[0029] The average temperature inside the reaction shaft 10 is set to, for example, about 1300° C. In the reaction shaft 10, the copper concentrate is burned while falling inside the reaction shaft 10, and melted and oxidized, thereby producing two types of solutions (matte and slag) and sulfurous acid gas.

[0030] The settler 20 is provided below the reaction shaft 10, and one end of the settler 20 (left side in FIG. 1) is connected to the lower part of the reaction shaft 10. The settler 20 collects matte and slag generated in the reaction shaft 10 inside. In the settler 20, the matte and slag are separated into layers due to the difference in specific gravity between the matte and slag, and in the settler 20, a matte layer and a slag layer are formed in this order from the bottom side of the settler 20. The settler 20 has, on its side, one or more slag holes 21 as an outlet for removing slag, and one or more matte holes 22 as an outlet for removing matte.

[0031] The flue gas duct 30 is formed in a cylindrical shape, with one end connected to the top of the other end side (right side in Figure 1) of the settler 20 and the other end connected to the boiler 31, and supplies high-temperature sulfur dioxide gas generated in the reaction shaft 10 to the boiler 31.

[0032] The electric slag furnace 40 collects the slag discharged from the settler 20 through the slag hole 21, and separates and collects trace amounts of matte contained in the slag.

[0033] In the flash smelting furnace 1, copper concentrate is blown into the reaction shaft 10 from the top 10a of the reaction shaft 10 by the concentrate burner 11 together with silica sand, auxiliary fuel such as heavy oil, and reaction gas RA such as oxygen-enriched air delivered separately. The copper concentrate blown into the reaction shaft 10 is heated by the combustion heat of the fuel, the sensible heat of the reaction gas, and the radiant heat in the furnace wall of the reaction shaft 10, and the sulfur content in the raw material for smelting reacts with the reaction gas instantaneously and burns. The combustion heat generated by the combustion of the sulfur content in the raw material for smelting causes the dissolution and oxidation of the copper concentrate particles (copper concentrate particles) in the raw material for smelting, and two types of solutions (matte (Cu2S-FeS) and slag (FeOx-SiO2)) and sulfurous acid gas are generated mainly by the reactions shown in the following formulas (1) and (2). CuFeS2+O2→Cu2S-FeS+FeOx+SO2···(1) FeOx+SiO2→FeOx-SiO2···(2)

[0034] The matte and slag generated in the reaction shaft 10 fall in the form of droplets into the settler 20 and are collected in the settler 20. At this time, droplets consisting of matte and slag (matte and slag droplets) repeatedly collide in the reaction shaft 10, increasing their particle size as they fall. In the settler 20, the matte and slag are separated into layers due to the difference in their specific gravities, and a matte layer and a slag layer are formed in this order at the bottom of the settler 20.

[0035] An appropriate amount of matte in the settler 20 is extracted from the matte hole 22 in response to a request from a converter (not shown) to which the matte is to be transported, and the slag in the settler 20 is appropriately discharged from the slag hole 21. The slag discharged from the slag hole 21 is introduced into an electric slag furnace 40, where it is heated and maintained by heat transfer caused by the passage of electricity through an electrode 41. A portion of the matte in the flash furnace slag layer does not settle to the bottom of the settler 20 but is discharged together with the slag, and further settles to the bottom of the furnace during the residence time in the electric slag furnace 40, forming a matte layer and a slag layer in the electric slag furnace 40 as well. The matte in the electric slag furnace 40 is recovered, and only the slag containing a small amount of copper is discharged from a discharge port 42 to the outside of the furnace.

[0036] In this manner, in the flash smelting furnace 1, the copper concentrate is separated into slag and matte, and the copper content in the recovered matte is set to, for example, 60% to 65%.

[0037] In addition, high-temperature sulfur dioxide gas generated in the reaction shaft 10 is discharged through a settler 20 and an exhaust flue 30 and cooled in a boiler 31.

[0038] <How to operate a flash melting furnace> The method of operating a flash smelting furnace according to the present embodiment will be described. The method of operating a flash smelting furnace according to the present embodiment will be described when applied to a flash smelting furnace 1 shown in Fig. 1. Note that, although the smelting raw material SP is copper concentrate and flux, it may contain substances other than copper concentrate and flux.

[0039] In the method of operating the flash smelting furnace according to this embodiment, copper concentrate and flux are fed from the top of the reaction shaft 10 .

[0040] The supply amounts of copper concentrate and flux may be ascertained from a flow meter (not shown) or the like provided in a supply means (not shown) that supplies copper concentrate and flux to the reaction shaft 10 .

[0041] Copper concentrate and flux supplied from the top of the reaction shaft 10 fall toward the settler 20 located below the reaction shaft 10 and react with the reaction gas supplied into the reaction shaft 10 to produce matte and slag.

[0042] A thermodynamic equilibrium calculation is performed using the composition of slag assumed to be generated from the composition of the smelting raw material SP consisting of copper concentrate and flux, and the relationship between the oxygen partial pressure and the liquidus temperature of the slag in the reaction shaft 10 is grasped (process of grasping the liquidus temperature of the slag corresponding to the oxygen partial pressure).

[0043] The reaction progress is assumed based on the composition of the copper concentrate and flux that constitute the smelting raw material SP that is supplied to the reaction shaft 10, and the composition of the matte and slag generated from the copper concentrate and flux is calculated. Using the composition of the generated slag, the oxygen partial pressure of the gas phase and solution (matte or slag) in the reaction shaft 10 is set to 1×10 -10 Thermodynamic equilibrium calculations are performed for oxygen partial pressures ranging from 0 to 1, and the liquidus temperature of the slag corresponding to each oxygen partial pressure is calculated.

[0044] The thermodynamic equilibrium calculation may be performed by evaluating the stable phase at each temperature and oxygen partial pressure using a spreadsheet software or the like using the Gibbs energy equation, or by utilizing commercially available thermodynamic equilibrium calculation software. The spreadsheet software may be any commonly available spreadsheet software. Examples of commercially available thermodynamic equilibrium calculation software include FactSage, Thermo-Calc, and HSC Chemistry.

[0045] Next, the liquidus temperature at one or more positions in the reaction shaft 10 is calculated from the relationship between the oxygen partial pressure and the liquidus temperature of the slag and the oxygen partial pressure at that position obtained by measurement or calculation (a step of calculating the liquidus temperature of the slag corresponding to the oxygen partial pressure).

[0046] First, the oxygen partial pressure and the furnace temperature at each position in the reaction shaft 10 are obtained.

[0047] Specific locations for grasping the oxygen partial pressure and the temperature inside the furnace include inside the reaction shaft where the collision and reaction of the copper concentrate and the silica sand proceeds, and the portion of the settler 20 directly below the reaction shaft 10.

[0048] The oxygen partial pressure and the temperature inside the furnace may be grasped, for example, by inserting an oxygen probe using an oxide-based solid electrolyte and a thermocouple through an inspection hatch provided in the side wall of the flash smelting furnace 1 during operation to grasp the oxygen partial pressure and the temperature inside the furnace, or by calculating the oxygen partial pressure and the temperature inside the furnace through a simulation using thermal fluid analysis software, etc. Examples of thermal fluid analysis software include Fluent, ANSYS CFX, OpenFOAM, etc.

[0049] Next, the flow of the smelting raw material SP is adjusted so that the smelting raw material SP flows into a region (high temperature region) where the temperature inside the furnace is higher than the liquidus temperature, and collision between the copper concentrate that constitutes the smelting raw material SP and the flux is promoted in the high temperature region (collision promotion process).

[0050] The liquidus temperature of the slag at each position in the flash smelting furnace 1 is calculated from the oxygen partial pressure obtained at each position in the flash smelting furnace 1 and the relationship between the oxygen partial pressure and the liquidus temperature obtained by thermodynamic equilibrium calculation. The obtained liquidus temperature of the slag is compared with the in-furnace temperature obtained at the same position to understand the magnitude relationship between them. Collision between the copper concentrate and the flux is promoted at a position where the in-furnace temperature is equal to or higher than the liquidus temperature of the slag.

[0051] The flow of the smelting feedstock SP may be adjusted during or after the supply of the copper concentrate and flux.

[0052] The high temperature region is a region where the temperature inside the furnace is higher than the liquidus temperature, and therefore the slag generated when the copper concentrate collides with the flux is considered to melt entirely. The temperature of the high temperature region is a value that varies depending on the composition of the copper concentrate and flux constituting the smelting material SP and the oxygen partial pressure, and may be changed, for example, to 1100°C to 1500°C. There may be only one high temperature region in the reaction shaft 10, or there may be multiple high temperature regions.

[0053] The flow direction of the raw material SP may be changed in any way so that the raw material SP flows into the high temperature region. Examples of the method for changing the flow direction of the raw material SP include a method for blowing in an inert gas or other gas from a vent or access hole provided in the side wall of the reaction shaft 10, and a method for providing a dispersion cone (not shown) at the tip of the concentrate burner 11 and adjusting the flow rate of the raw material SP and the angle of the dispersion cone.

[0054] When a method of injecting gas from a vent or inspection hole provided on the side wall of the reaction shaft 10 is used, the direction of the flow of the smelting raw material SP in the reaction shaft 10 can be changed by injecting gas into the reaction shaft 10 from the vent or inspection hole, so that the smelting raw material SP is caused to flow into a high-temperature region, which makes it easy to promote collisions between the copper concentrate and the flux.

[0055] When a method is used in which a dispersion cone 113 is provided at the tip of the concentrate burner 11 and the flow rate of the smelting raw material SP and the angle of the dispersion cone 113 are adjusted, the smelting raw material SP with its adjusted flow rate collides with the dispersion cone 113, thereby adjusting the flow direction of the smelting raw material SP and the degree of dispersion of the smelting raw material SP into the reaction shaft 10. This makes it possible to change the direction of the flow of the smelting raw material SP ejected into the reaction shaft 10, and therefore the trajectory of the fall of the smelting raw material SP can be easily adjusted so that the copper concentrate and the flux collide in the high temperature region.

[0056] As shown in Fig. 2, the liquidus temperature (the temperature at which the entire amount becomes liquid) of slag such as FeO-SiO2 generated in the reaction shaft 10 decreases with a decrease in the oxygen partial pressure, and the reaction proceeds easily. Therefore, if the liquidus temperature of the slag is calculated from the oxygen partial pressure at each position in the reaction shaft 10 and the temperature inside the reaction shaft 10 is set in a high temperature region to promote the collision between the copper concentrate and the flux, the reaction between the copper concentrate and the flux can be efficiently promoted. Therefore, slag is efficiently formed in the reaction shaft 10.

[0057] The method for operating a flash smelting furnace according to this embodiment includes a step of determining the liquidus temperature of the slag corresponding to the oxygen partial pressure, a step of calculating the liquidus temperature of the slag corresponding to the oxygen partial pressure, and a collision promotion step, in which the flow direction of the raw material SP is adjusted so that the raw material SP flows in a high-temperature region in the reaction shaft 10, and collision between the copper concentrate contained in the raw material SP and the flux in the high-temperature region is promoted. As a result, the method for operating a flash smelting furnace according to this embodiment can efficiently carry out a slag generation reaction in the reaction shaft 10.

[0058] Since the fluidity of the slag varies depending on the amount of slag generated by the collision of the smelting raw materials with the flux in the reaction shaft 10, it is important to drop the reaction shaft 10 in such a way that the collision of the smelting raw materials with the flux in the reaction shaft 10 is promoted so that slag with a low melting point and low viscosity is generated.

[0059] By using the method for operating a flash smelting furnace according to the present embodiment, it is possible to efficiently produce slag with a low melting point and low viscosity from the copper concentrate and the flux by promoting collision between the smelting raw material and the flux in the reaction shaft 10, and it is possible to promote subsequent collision between the reacted molten bodies. As a result, it is possible to operate the flash smelting furnace 1 so as to reduce the amount of copper concentrate and flux recovered in the settler 20 without reacting in the reaction shaft 10, and to increase the particle size of the matte to enhance the settling property of the matte, thereby increasing the amount of matte recovered.

[0060] In the method for operating a flash melting furnace according to this embodiment, the temperature of the high temperature region can be set to 1100°C to 1500°C.

[0061] In the method for operating the flash smelting furnace according to the present embodiment, the flow direction of the smelting raw material SP can be changed by blowing in gas from a vent or access hole provided in the side wall of the reaction shaft 10. In the method for operating the flash smelting furnace according to the present embodiment, the flow direction of the smelting raw material SP is changed, so that the smelting raw material SP flows in a high-temperature region, promoting the agitation of the flows of the copper concentrate and flux, and making collisions more likely to occur.

[0062] In the method of operating a flash smelting furnace according to the present embodiment, a dispersion cone 113 is provided at the tip of the concentrate burner 11, and the flow rate of the smelting raw material SP and the angle of the dispersion cone 113 can be adjusted. In the method of operating a flash smelting furnace according to the present embodiment, the smelting raw material SP whose flow rate has been adjusted is collided with the dispersion cone 113 in the concentrate burner 11, thereby adjusting the dispersion state of the smelting raw material SP ejected from the concentrate burner 11 and changing the direction of the flow of the smelting raw material SP. Therefore, in the method of operating a flash smelting furnace according to the present embodiment, the smelting raw material SP can be made to flow into the high temperature region. Therefore, in the method of operating a flash smelting furnace according to the present embodiment, the trajectory of the fall of the smelting raw material SP can be adjusted so that the collision between the copper concentrate and the flux is promoted in the high temperature region, so that the slag generation reaction is further improved and slag generation can be more reliably performed.

[0063] As described above, the method for operating a flash smelting furnace according to this embodiment can efficiently generate slag in the reaction shaft 10, thereby increasing the fluidity of the slag and promoting the settling of the matte, thereby improving the yield of the matte. Therefore, the method for operating a flash smelting furnace according to this embodiment can be effectively used for prior examination of equipment improvements for the flash smelting furnace 1, investigation of the effects of changes in the operating conditions of the flash smelting furnace 1, and the type of smelting raw material supplied to the flash smelting furnace 1, etc.

[0064] Although the embodiment has been described above, the above embodiment is presented as an example, and the present invention is not limited to the above embodiment. The above embodiment can be implemented in various other forms, and various combinations, omissions, substitutions, modifications, etc. can be made without departing from the gist of the invention. These embodiments and their modifications are included in the scope and gist of the invention, and are included in the scope of the invention and its equivalents described in the claims. EXAMPLES

[0065] The present embodiment will be described in more detail below with reference to examples, although the present embodiment is not limited to the following examples.

[0066] <Example> [Slag production] Slags 1 to 4 having the compositions shown in Table 1 were produced.

[0067] [Table 1]

[0068] [Measurement of liquidus temperature] Using the prepared slags 1 to 4, the slag liquidus temperature (unit: °C) was calculated using the thermodynamic equilibrium calculation software FactSage 8.2 when the oxygen partial pressure pO2 (unit: atm) in the furnace was changed. The relationship between the calculated oxygen partial pressure pO2 and the slag liquidus temperature is shown in Figure 3. In Figure 3, the oxygen partial pressure pO2 is shown in logarithm (log).

[0069] As shown in Figure 3, the oxygen partial pressure pO2 is 1×10 -6 If the temperature is below 1350° C., the liquidus temperature can be set to about 1350° C. Therefore, when producing slag from smelting raw materials containing copper concentrate and flux, it can be said that slag can be produced efficiently by supplying the copper concentrate and flux so that they flow in a region where the temperature is 1350° C. or higher (high temperature region) and promoting collision between the copper concentrate and the flux.

[0070] In addition, a thermal fluid analysis was performed in the flash melting furnace using the thermal fluid analysis software FLUENT. The results showed that the temperature in the reaction shaft was 1349°C and the oxygen partial pressure was 3.24×10 -8 A position was found where the calculated result was obtained. This position can be said to be a position included in the high temperature region. The calculation was performed again by adjusting the dispersion cone angle and the supply gas flow rate to the concentrate burner so that the trajectories of the copper concentrate and flux intersect at this position. As a result, it was confirmed that the amount of unreacted material in the slag tends to decrease. Therefore, it can be said that slag can be generated efficiently by adjusting the copper concentrate and flux to flow to the above-mentioned position.

[0071] The aspects of the embodiment of the present invention are as follows, for example. <1> A method for operating a flash smelting furnace, in which a smelting raw material containing copper concentrate and flux, supplied from the top of a reaction tower, falls toward a settler located below the reaction tower and reacts with a reaction gas supplied into the reaction tower to produce matte and slag, comprising: A step of performing a thermodynamic equilibrium calculation using a composition of the slag assumed to be generated from the composition of the smelting raw material, and grasping a relationship between an oxygen partial pressure in the reaction tower and a liquidus temperature of the slag; calculating the liquidus temperature at one or more positions in the reaction tower from a relationship between the oxygen partial pressure and the liquidus temperature of the slag and the oxygen partial pressure at the positions obtained by measurement or calculation; A method for operating a flash smelting furnace, comprising adjusting a flow of the smelting raw material so that the smelting raw material flows into a region in which the temperature inside the furnace is higher than the liquidus temperature, and promoting collision of the copper concentrate with the flux in the region. <2> A vent or an inspection port is provided in the side wall of the reaction tower, Gas is blown in through the vent or the access hole to change the direction of the flow of the smelting material. <1> A method for operating the flash melting furnace described in claim 1. <3> a dispersion cone is provided at the tip of a concentrate burner provided at the top of the reaction tower; The flow rate of the smelting raw material ejected from the concentrate burner and the angle of the dispersion cone are adjusted to adjust the dispersion of the smelting raw material in the reaction tower and change the direction of the flow of the smelting raw material. <1> or <2> A method for operating the flash melting furnace described in claim 1. [Explanation of symbols]

[0072] 1 Flash-melting furnace 10 Reaction tower (reaction shaft) 11 Concentrate burner 20 Settler 30 Flue flue 40 Electric smelting furnace

Claims

1. A method for operating a flash smelting furnace, in which a smelting raw material containing copper concentrate and flux, supplied from the top of a reaction tower, falls toward a settler located below the reaction tower and reacts with a reaction gas supplied into the reaction tower to produce matte and slag, comprising: A step of performing a thermodynamic equilibrium calculation using a composition of the slag assumed to be generated from the composition of the smelting raw material, and grasping a relationship between an oxygen partial pressure in the reaction tower and a liquidus temperature of the slag; calculating the liquidus temperature at one or more positions in the reaction tower from a relationship between the oxygen partial pressure and the liquidus temperature of the slag and the oxygen partial pressure at the positions obtained by measurement or calculation; A method for operating a flash smelting furnace, comprising adjusting a flow of the smelting raw material so that the smelting raw material flows into a region in which the temperature inside the furnace is higher than the liquidus temperature, and promoting collision of the copper concentrate with the flux in the region.

2. A vent or an inspection port is provided in the side wall of the reaction tower, 2. The method for operating a flash smelting furnace according to claim 1, further comprising the step of blowing gas through said vent hole or said access hole to change the direction of the flow of said smelting raw material.

3. a dispersion cone is provided at the tip of a concentrate burner provided at the top of the reaction tower; 2. The method for operating a flash smelting furnace according to claim 1, further comprising adjusting a flow rate of the smelting raw material ejected from the concentrate burner and an angle of the dispersion cone to adjust a degree of dispersion of the smelting raw material in the reaction tower and change a direction of the flow of the smelting raw material.

Citation Information

Patent Citations

  • Steam iron

    JP1980000115A

  • Burner for concentrate

    JP2002060859A