Composition and heat storage material

A composition of water, ammonium chloride, and a second component with a eutectic temperature of -5.0°C or higher, optionally with a third component, addresses the performance issues of existing heat storage materials by stabilizing freezing and maintaining a low melting point, ensuring effective temperature maintenance in household refrigerators.

JP2024159598APending Publication Date: 2024-11-08INOAC TECHN CENT
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024067832
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-07-25
Filing Date
2024-04-18
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

The composition disclosed in Patent Document 1 for a heat storage material does not sufficiently meet the performance requirements for maintaining a temperature range around -15°C, particularly in applications such as keeping fresh and frozen foods and medical products cold.

Method used

A composition comprising water, ammonium chloride as a first component, and a second component with a eutectic temperature of -5.0°C or higher, optionally with a third component satisfying the relationship |a2-a3|<|a2-a1|, where a1, a2, and a3 are the maximum lengths of the crystal axes of the components, is used to enhance performance.

Benefits of technology

The composition achieves excellent performance by stabilizing freezing and maintaining a low melting point, preventing supercooling, and providing high latent heat, making it suitable for use in household refrigerators without specialized freezing equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024159598000001
    Figure 2024159598000001
  • Figure 2024159598000002
    Figure 2024159598000002
  • Figure 2024159598000003
    Figure 2024159598000003
Patent Text Reader

Abstract

To provide a composition with superior performance.SOLUTION: An aspect of this invention is a composition for heat storage material that comprises water, a first component, and a second component, where the first component is ammonium chloride and the second component is a compound with a eutectic point with water at -5.0°C or higher.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition and a heat storage material. [Background technology]

[0002] Phase change materials are one type of heat storage material that can maintain a certain temperature. Phase change materials are materials that can maintain a constant temperature by utilizing the latent heat generated when they change from a solid phase to a liquid phase.

[0003] Thermal storage materials are sometimes used to keep fresh foods, frozen foods, medical supplies (pharmaceuticals), etc., cool, and there are cases where they are required to maintain a temperature range of around -15°C.

[0004] As a heat storage material suitable for such a temperature range, Patent Document 1 discloses an aqueous solution of ammonium chloride and potassium chloride, which is capable of keeping things cold at -17.5°C. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2002-371269 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, the composition disclosed in Patent Document 1 does not fully satisfy the performance required when applied to a heat storage material.

[0007] Therefore, an object of the present invention is to provide a composition for a heat storage material having excellent performance.

[0008] The present inventors have conducted extensive research and found that the above problems can be solved by using a composition containing a specific component. [Means for solving the problem]

[0009] The first aspect of the present invention is comprising water, a first component, and a second component, the first component is ammonium chloride; The second component is a compound having a eutectic temperature with water of -5.0°C or higher. The present invention relates to a composition for a heat storage material.

[0010] A second aspect of the present invention is comprising water, a first component, a second component, and a third component; the first component is ammonium chloride; the second component is a compound having a eutectic temperature with water of −5.0° C. or higher, the third component is a compound other than the first component and the second component, The relationship between the maximum length a1 of the crystal axis of the first component, the maximum length a2 of the crystal axis of the second component, and the maximum length a3 of the crystal axis of the third component satisfies the following formula (1): The present invention relates to a composition for a heat storage material. (Equation 1) |a2-a3|<|a2-a1|

[0011] In the first and second embodiments, the second component preferably contains at least one selected from the group consisting of sulfates, nitrates, and carbonates. In the first and second embodiments, the second component is preferably potassium nitrate.

[0012] A third aspect of the present invention is The heat storage material comprises a container and a composition of a first form or a composition of a second form housed in the container.

[0013] A fourth aspect of the present invention is The food cooling device comprises a container and, contained within the container, the composition of the first form or the composition of the second form. Effect of the Invention

[0014] According to the present invention, there is provided a composition for a heat storage material having excellent performance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, when an upper limit value and a lower limit value are separately described, it is deemed that a numerical range combining any upper limit value and any lower limit value is substantially disclosed.

[0016] In the following, when a compound is described, its isomers are also described simultaneously.

[0017] In the following, unless otherwise specified, various measurements are carried out at room temperature (25° C.) and under normal pressure.

[0018] The components, properties / characteristics, applications, etc. of the composition will be specifically described below, but the present invention is not limited thereto.

[0019] <<Ingredients>> The composition according to the present disclosure preferably comprises water, a first component, and a second component. The composition may also contain other ingredients. Each component will be described below.

[0020] <Water> In the composition, water functions as a solvent or a dispersion medium for the first component and the second component.

[0021] The water is not particularly limited, and may be pure water such as distilled water, ion-exchanged water, or RO (reverse osmosis) water, or ultrapure water.

[0022] The content of water in the composition can be adjusted taking into consideration the concentrations of other components, etc. The content of water is preferably, for example, 20.0% by mass or more, 30.0% by mass or more, 40.0% by mass or more, 50.0% by mass or more, 60.0% by mass or more, or 70.0% by mass or more, when the total amount of the composition is 100.0% by mass.

[0023] <First component> The first component is ammonium chloride.

[0024] The content M of the first component when the total amount of the composition is 100.0 mass% 1 is preferably 5.0 mass % or more, 8.0 mass % or more, or 10.0 mass % or more, and is preferably 30.0 mass % or less, 28.0 mass % or less, or 25.0 mass % or less.

[0025] <Second component> The second component is a compound (particularly, an inorganic salt) whose eutectic temperature with water is −5.0° C. or higher. The eutectic temperature of water and a compound is referred to as a known physical property shown in a phase diagram. The eutectic temperature of water and a compound can also be measured. The eutectic temperature of water and a compound can be measured, for example, by preparing a solution of eutectic concentration of water and the compound, and measuring the melting peak temperature according to differential scanning calorimetry (DSC) described later. Even if the eutectic concentration of water and the compound is unknown, it is possible to prepare aqueous solutions of different concentrations, measure each solution by DSC, and if a single melting peak is obtained, the eutectic temperature can be measured from the peak temperature.

[0026] The second component preferably has a eutectic temperature with water of -4.5°C or higher, -4.0°C or higher, -3.5°C or higher, or -3.0°C or higher, and preferably -1.0°C or lower, -1.5°C or lower, or -2.0°C or lower.

[0027] From another perspective, the eutectic temperature T 1 (-15.8°C) and the eutectic temperature T 2 and the difference (|T 1 -T 2 |) is preferably 11.0°C or more, 11.5°C or more, 12.0°C or more, or 12.5°C or more.

[0028] Specific examples of the second component include nickel sulfate (eutectic temperature: -4.15°C, eutectic latent heat: 259 J / g), magnesium sulfate (eutectic temperature: -3.9°C, eutectic latent heat: 264 J / g), sodium fluoride (eutectic temperature: -3.5°C, eutectic latent heat: 314 J / g), sodium hydroxide (eutectic temperature: -2.8°C, eutectic latent heat: 266 J / g), potassium nitrate (eutectic temperature: -2.8°C, eutectic latent heat: 296 J / g), sodium carbonate (eutectic temperature: -2.1°C, eutectic latent heat: 310 J / g), iron sulfate (eutectic temperature: -1.8°C, eutectic latent heat: 287 J / g), and copper sulfate (eutectic temperature: -1.6°C, eutectic latent heat: 291 J / g).

[0029] From the viewpoint of improving the stability of performance and safety, the second component preferably contains at least one selected from the group consisting of sulfates, nitrates and carbonates, and more preferably potassium nitrate.

[0030] A composition containing water, the first component, and the second component becomes a crystal nucleating agent by the precipitation of the second component when cooled to a low temperature, and the entire cold storage material is likely to freeze, so that supercooling is easily prevented (for example, it is likely to solidify even under cooling conditions of about -2°C from the melting point). In addition, when the first component and the second component are used in combination, a composition having a high latent heat is easily obtained. Furthermore, a composition containing water, the first component, and the second component is likely to become a homogeneous composition, so it is likely to solidify stably. More specifically, the composition according to the present disclosure can be a composition that can be expected to freeze in the freezer of a general household refrigerator (the average temperature inside the refrigerator is usually -18 to -20°C, etc.) (a composition that is easily frozen without using special freezing equipment).

[0031] The content M of the second component in the composition when the total amount of the composition is 100.0 mass% 2 is preferably 1.0 mass% or more, 2.0 mass% or more, 3.0 mass% or more, 4.0 mass% or more, or 5.0 mass% or more, and is preferably 30.0 mass% or less, 25.0 mass% or less, 20.0 mass% or less, or 15.0 mass% or less.

[0032] Content of the first component M 1 The content of the second component M 2 Ratio (M 2 / M 1 ) is preferably 2.0 or less, 1.5 or less, 1.0 or less, 0.8 or less, 0.5 or less, or 0.4 or less, and is preferably 0.1 or more, 0.2 or more, or 0.3 or more.

[0033] <Other ingredients> The composition may contain known ingredients such as thickeners (gelling agents), gelling assistants, colorants (dyes, pigments), antibacterial agents, viscosity adjusters, supercooling inhibitors (e.g., ice nucleating bacteria, calcium carbonate, sodium sulfate, disodium hydrogen phosphate, borax, activated carbon, silver iodide, minerals, and other crystal nucleating agents), antifoaming agents, and organic solvents other than water.

[0034] When the composition contains a thickener (gelling agent), any conventionally known thickener can be used, such as polysaccharides, gelatin, polyacrylic acid (salt), polyacrylamide, polyvinyl alcohol, etc.

[0035] Examples of polysaccharides include cellulose derivatives such as carboxymethylcellulose (CMC), alginic acid, agar, etc. In addition, alginic acid, carboxymethylcellulose, etc. also include salt forms such as sodium salts.

[0036] The content of the thickener in the composition can be adjusted so that the composition has a predetermined viscosity, and is not particularly limited. For example, when the total amount of water, the first component, and the second component is 100.0 parts by mass, the content of the thickener in the composition is preferably 0.1 parts by mass or more, 0.5 parts by mass or more, or 1.0 parts by mass or more, and is preferably 10.0 parts by mass or less, or 5.0 parts by mass or less.

[0037] From the viewpoint of increasing the latent heat quantity, etc. of the composition, when the total amount of the composition is 100.0 mass%, the content of other components excluding the thickener is preferably 5.0 parts by mass or less, 3.0 parts by mass or less, 1.0 part by mass or less, 0.5 parts by mass or less, or 0.1 parts by mass or less.

[0038] <<Physical properties / properties>> <Thermal properties> The composition of the present disclosure may have a melting point of -15.0°C or lower, -15.5°C or lower, -16.0°C or lower, -16.5°C or lower, or -17.0°C or lower, and may be -18.0°C or higher.

[0039] Furthermore, the composition of the present disclosure may have a latent heat of 100 J / g or more, 150 J / g or more, 200 J / g or more, 250 J / g or more, or 275 J / g or more.

[0040] The melting point and latent heat of the composition are obtained by differential scanning calorimetry (DSC). Specifically, the following is performed. About 10 mg of the composition is placed in an aluminum pan for DSC measurement, heated to 25°C, cooled to -50°C at a rate of 1°C / min to solidify, and then heated back to 25°C at a rate of 1°C / min. The melting point and latent heat are obtained from the apex and area of ​​the peak that appears during the phase change. If the composition has multiple peaks (melting peaks), the temperature corresponding to the lowest peak position is taken as the melting point of the composition.

[0041] <Viscosity> The viscosity of the composition can be appropriately changed depending on the application, and is not particularly limited. When the composition contains a gel component, the viscosity of the composition can be 1.0 Pa·s or more, 2.0 Pa·s or more, 5.0 Pa·s or more, 10 Pa·s or more, 100 Pa·s or more, or 500 Pa·s or more. The upper limit of the viscosity of the composition is not particularly limited, but is, for example, 2000 Pa·s or less.

[0042] The viscosity of the composition is measured at 25° C. using a B-type rotational viscometer.

[0043] <<Applications>> The composition according to the present disclosure is preferably used for a heat storage material, a food cooling tool, or a medicine cooling tool. In other words, a preferred embodiment of the composition according to the present disclosure is a composition for a heat storage material, a food cooling tool, or a medicine cooling tool.

[0044] As an example of a specific method of using the composition according to the present disclosure, preferred examples of a heat storage material comprising the composition according to the present disclosure, and a food cooling tool and a medicine cooling tool comprising the composition according to the present disclosure will be described below.

[0045] <Heat storage material> The thermal storage material includes a container and a composition contained within the container.

[0046] The composition is as described above, and detailed description will be omitted. As described above, the composition may be gelled (containing a gel component). By using a gelled composition, leakage of the liquid material when the container is broken can be suppressed.

[0047] The material of the container may be flexible enough to be deformed in response to the phase changes (solidification and melting) of the composition.

[0048] The heat storage material may be a so-called soft type in which the container is made of a material that is easily deformed, such as a resin film or a metal film, or it may be a so-called hard type in which the container is made of a material that is less likely to deform, such as a thick resin material (e.g., a hollow molded body).

[0049] The heat storage material may be configured so that at least the composition is sealed in a container, and may be configured so that the composition can be removed or poured without destroying the container, for example by having an openable and closable lid, or may be configured so that the composition is difficult to remove without destroying the container.

[0050] The size and shape of the heat storage material can be appropriately changed depending on the application of the heat storage material.

[0051] The heat storage material may include components other than the container and the composition.

[0052] <Food cooling equipment and medicine cooling equipment> The food cooling device and the medicine cooling device include, for example, a container and a composition according to the present disclosure contained in the container.

[0053] The composition is as described above, and therefore a detailed description thereof will be omitted.

[0054] The container is, for example, a box-shaped article, and has a space inside the container that can accommodate an object to be kept cold, such as food. A composition storage section containing the composition according to the present disclosure is arranged on at least one or all of the inner side, inner bottom, and inner top surfaces of the container. The composition storage section may be configured to be removable from the container, or may be integrated with the container. The container usually has an opening and closing section, which is operated to be in a sealed state or an open state. The container is preferably made of a material having thermal insulation properties. The object to be kept cold, such as food or medicine, can be kept cold by storing the object to be kept cold in the space inside the container while the composition is solidified.

[0055] Examples of items to be kept cool by the food cooling equipment include frozen foods, ice cream, produce such as vegetables and fruits, and processed foods such as ham.

[0056] The items to be kept cool using the medicine cooling equipment include some medicines that require low temperature storage, such as blood, specimens, and vaccines.

[0057] <<Specific Forms of Composition>> As a preferred composition according to the present disclosure, a composition containing water, a first component, and a second component has been described above in detail. In the following, as a specific form of such a composition, a composition containing water, a first component, and a second component, and further containing a third component that is a specific component other than water, the first component, and the second component (a specific form of composition) will be described in detail.

[0058] The composition in a specific form may further contain other components as described above, in addition to water, the first component, the second component, and the third component.

[0059] The water, the first component, the second component and other components are as described above, and therefore their explanation will be omitted.

[0060] <Third component> The third component is a compound other than ammonium chloride, and has a eutectic temperature with water of less than -5.0°C.

[0061] The third component is preferably a compound in which the relationship between the maximum length a1 of the crystal axis of the first component, the maximum length a2 of the crystal axis of the second component, and the maximum length a3 of the crystal axis of the third component satisfies the following formula (1). (Equation 1) |a2-a3|<|a2-a1|

[0062] It is presumed that by further adding a third component satisfying the above formula (1) to a composition containing the first and second components, it becomes easier to obtain a composition with a lower melting point, and that the second component, which tends to precipitate in the initial stage of cooling, can also act as an effective nucleating agent for the third component, making nucleation more likely to occur, making it possible to adjust the melting point while maintaining a high nucleation rate for the entire composition.

[0063] In the above formula (1), the difference (|a2-a3|) between the maximum length a2 of the crystal axis of the second component and the maximum length a3 of the crystal axis of the third component is preferably 5.00 Å or less, 4.00 Å or less, 3.00 Å or less, or 2.50 Å or less.

[0064] From the viewpoint of further enhancing the above-mentioned effect, it is preferable that the maximum length a1 of the crystal axis of the first component, the maximum length a2 of the crystal axis of the second component, and the maximum length a3 of the crystal axis of the third component satisfy the following formula (2). (Formula 2) a1 <a3<a2

[0065] The third component is preferably a potassium halide, more preferably potassium chloride or potassium bromide, and particularly preferably potassium bromide. By using such a compound as the third component, it is possible to enhance the effect of preventing supercooling while maintaining the amount of latent heat. The eutectic temperature of potassium chloride with water is -11°C, and the eutectic temperature of potassium bromide with water is -12°C.

[0066] From another point of view, the third component is preferably urea or a urea derivative, and more preferably urea. The eutectic temperature of urea with water is −11.5° C. By using urea or a urea derivative as the third component, it is easy to further improve the performance of the heat storage material while maintaining the effects achieved by each component (first component, second component) in the composition.

[0067] Examples of urea derivatives include 1-methylurea, 1,3-dimethylurea, 2-imidazolidinone, 1,3-dimethyl-2-imidazolidinone, N,N'-dimethylpropyleneurea, tetramethylurea, 3-phenyl-1,1-dimethylurea, 3-(3,4-dichlorophenyl)-1,1-dimethylurea, 1,1'-(4-methyl-m-phenylene)-bis-(3,3'-dimethyl)urea, and phenyldimethylurea.

[0068] The content M of the third component in the composition when the total amount of the composition is 100.0 mass% 3 is preferably 1.0 mass% or more, 2.0 mass% or more, 5.0 mass% or more, 8.0 mass% or more, or 10.0 mass% or more, and is preferably 40.0 mass% or less, 35.0 mass% or less, 30.0 mass% or less, 25.0 mass% or less, or 20.0 mass% or less.

[0069] Content of the first component M 1 The content of the third component M 3 Ratio (M 3 / M 1) is preferably 2.0 or less, 1.8 or less, 1.6 or less, 1.4 or less, or 1.2 or less, and is preferably 0.1 or more, 0.2 or more, 0.5 or more, 0.8 or more, or 1.0 or more.

[0070] The preferred contents of water, the first component, the second component, and other components in the composition are as described above. 1 and the content of the second component M 2 and the content of the third component M 3 By M 2 ≦M 1 ≦M 3 It is preferable that the following is satisfied.

[0071] The composition of this specific embodiment may have a melting point at a lower temperature. More specifically, the melting point of the composition of this specific embodiment may be -16.0°C or lower, -18.0°C or lower, -19.0°C or lower, or -20.0°C or lower, or may be -25.0°C or higher, -24.0°C or higher, or -22.0°C or higher. Since the composition of this specific embodiment is easily prevented from being supercooled, even if it has a melting point at such a low temperature, it can be sufficiently frozen even in a -25.0°C environment.

[0072] Other configurations of the composition of this specific embodiment (such as latent heat amount, viscosity, uses, and application to heat storage materials, food cooling devices, and medicine cooling devices) are as described above.

[0073] The composition of this particular form is not limited to the above. Another composition of this particular embodiment may be, for example, a composition including a first component which is ammonium chloride, a second component which is a compound other than urea or a urea derivative and has a eutectic temperature with water of −5.0° C. or higher, and a third component which is urea or a urea derivative. When the composition contains urea or a urea derivative, the configuration for further enhancing the effect derived from urea or a urea derivative is as follows. The content M of the third component in the composition when the total amount of the composition is 100.0 mass% 3is preferably 1.0 mass% or more, 2.0 mass% or more, 5.0 mass% or more, or 8.0 mass% or more, and is preferably 40.0 mass% or less, 30.0 mass% or less, 25.0 mass% or less, 20.0 mass% or less, or 18.0 mass% or less. Content of the first component M 1 The content of the third component M 3 Ratio (M 3 / M 1 ) is preferably 2.0 or less, 1.6 or less, 1.4 or less, or 1.1 or less, and is preferably 0.1 or more, 0.3 or more, 0.4 or more, 0.5 or more, or 0.6 or more. Content of the first component M 1 and the content of the second component M 2 and the content of the third component M 3 By M 2 ≦M 3 ≦M 1 It is preferable that the following is satisfied. The melting point of the composition can be -18.0°C or lower, -19.0°C or lower, -20.0°C or lower, or -21.0°C or lower, and can be -25.0°C or higher, -24.0°C or higher, or -23.0°C or higher. The first component, the second component, the other components, the preferred contents of each component, and other configurations are as described above. EXAMPLES

[0074] The composition (heat storage material composition) will be specifically described below with reference to examples, but the present invention is not limited to the following.

[0075] <<<First embodiment>>> <<Preparation of composition>> The compositions according to Examples 1 to 5 and Comparative Examples 1 to 3 were obtained by mixing and stirring the raw materials shown in Table 1 in the amounts (parts by mass) shown in Table 1. Note that KCl has a eutectic temperature with water of -11°C.

[0076] <<Evaluation>> <Melting point and latent heat> The melting point and latent heat of each composition were measured by the above-mentioned differential scanning calorimetry. The measurement results for each item are shown in Table 1.

[0077] <Freezing test> The composition was left to stand in a -20°C low-temperature bath for 5 hours, and it was confirmed whether freezing occurred (whether heat of solidification occurred or not). Cases where freezing occurred were marked with "O", and cases where freezing did not occur were marked with "-".

[0078] [Table 1]

[0079] From the above results, it can be seen that the compositions according to each example are capable of stably solidifying even under cooling conditions of -20°C for 5 hours, and therefore have excellent supercooling prevention performance, sufficiently low melting points, and sufficiently high latent heats.

[0080] Hereinafter, another embodiment of the composition (heat storage material composition) will be described in detail.

[0081] <<<Second embodiment>>> <<Preparation of composition>> The compositions according to Examples 6 to 15 and Comparative Example 4 were obtained by mixing and stirring the raw materials shown in Table 2 in the amounts (parts by mass) shown in Table 2. The maximum length (a1) of the crystal axis of ammonium chloride was 3.87 Å, the maximum length (a2) of the crystal axis of potassium nitrate was 9.17 Å, and the maximum length (a3) ​​of the crystal axis of potassium bromide was 6.6 Å, satisfying the relationship |a2-a3|<|a2-a1|.

[0082] <<Evaluation>> <Melting point and latent heat> The melting point and latent heat of each composition were measured by the above-mentioned differential scanning calorimetry. The measurement results for each item are shown in Table 2.

[0083] <Freezing test> The composition was allowed to stand in a low-temperature bath at -25°C for 20 hours, and it was confirmed whether freezing occurred (whether heat of solidification occurred or not). For each Example and Comparative Example, the case where freezing occurred was marked with "◯", and the case where freezing did not occur was marked with "-".

[0084] [Table 2]

[0085] In addition, the freezing completion time (the time from the start of the freezing test to the end of the period during which the temperature of the composition is kept constant due to phase change in the freezing test) was measured for Examples 12, 14, and 15, and was 452 minutes for Example 12, 390 minutes for Example 14, and 317 minutes for Example 15.

[0086] From the above results, it can be seen that the compositions according to each example have a melting point of around -20 to -22°C, but can be stably solidified under cooling conditions of -25°C for 20 hours, and therefore have excellent supercooling prevention performance, a sufficiently low melting point, and a sufficiently high latent heat.

[0087] <<<Third Example>>> <<Preparation of composition>> The compositions according to Examples 16 to 22 were obtained by mixing and stirring the raw materials shown in Table 3 in the amounts (parts by mass) shown in Table 3. The maximum length (a1) of the crystal axis of ammonium chloride was 3.87 Å, the maximum length (a2) of the crystal axis of potassium nitrate was 9.17 Å, and the maximum length (a3) ​​of the crystal axis of urea was 4.73 Å, satisfying the relationship |a2-a3|<|a2-a1|.

[0088] <<Evaluation>> <Melting point and latent heat> The melting point and latent heat of each composition were measured by the above-mentioned differential scanning calorimetry. The measurement results for each item are shown in Table 3.

[0089] <Freezing test> The composition was allowed to stand in a low-temperature bath at -25°C for 20 hours, and it was confirmed whether freezing occurred (whether heat of solidification occurred or not). For each Example, the case where freezing occurred was marked with "◯", and the case where freezing did not occur was marked with "-".

[0090] [Table 3]

[0091] From the above results, it can be seen that the compositions according to each example have a melting point of around -21 to -23°C, but can be stably solidified under cooling conditions of -25°C for 20 hours, and therefore have excellent supercooling prevention performance, a sufficiently low melting point, and a sufficiently high latent heat. [Industrial Applicability]

[0092] The composition of the present invention has excellent properties and is therefore applicable to various uses such as heat storage materials, food cooling devices, and medicine cooling devices.

Claims

1. comprising water, a first component, and a second component; the first component is ammonium chloride; The second component is a compound having a eutectic temperature with water of −5.0° C. or higher. A composition for heat storage material, comprising:

2. comprising water, a first component, a second component, and a third component; the first component is ammonium chloride; the second component is a compound having a eutectic temperature with water of −5.0° C. or higher, the third component is a compound other than the first component and the second component, The relationship between the maximum length a1 of the crystal axis of the first component, the maximum length a2 of the crystal axis of the second component, and the maximum length a3 of the crystal axis of the third component satisfies the following formula (1): A composition for heat storage material comprising: (Formula 1) |a2-a3|<|a2-a1|

3. The composition according to claim 1 or 2, wherein the second component comprises at least one selected from the group consisting of sulfates, nitrates, and carbonates.

4. The composition of claim 3 wherein said second component is potassium nitrate.

5. A heat storage material comprising a container and the composition according to claim 1 or 2 housed in the container.

6. A food cooling device comprising a container and the composition according to claim 1 or 2 contained in the container.

Citation Information

Patent Citations

  • Mixed low-temperature insulating material

    JP2002371269A