Optical laminate and article having the same

The optical laminate with a surface-modified silica filler and specific layer configurations addresses the lack of scratch and bending resistance in foldable displays, enhancing durability through improved adhesion and hardness.

JP2024159608AActive Publication Date: 2024-11-08DEXERIALS CORP

Patent Information

Application Number
JP2024069031
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-04-10
Filing Date
2024-04-22
Publication Date
2024-11-08
Estimated Expiration
2044-04-22

Smart Images

  • Figure 2024159608000001_ABST
    Figure 2024159608000001_ABST
Patent Text Reader

Abstract

To provide an optical laminate that can realize excellent abrasion resistance and further improves flex resistance.SOLUTION: An optical laminate 102 includes a transparent base material 11, a hard coat layer 12, an adhesive layer 13 made of a sputter film, an optical functional layer 14 in which a high refractive index layer made of the sputter film and a low refractive index layer having a lower refractive index than the high refractive index layer are laminated alternately, and an antifouling layer 15 in this order. The hard coat layer 12 contains a silica filler, and the optical laminate satisfies the following conditions 1 and 2. Condition 1: the ratio ((A) / (B)) between a Martens hardness (A) in a side of the optical laminate antifouling layer and a Martens hardness (B) in a side of the hard coat layer of the laminate having only the transparent base material and the hard coat layer is 3.6 or less. Condition 2: a contact angle difference for water between before friction and after friction in which a steel wool is reciprocated horizontally 200 times is 20° or less by using a friction testing machine using the steel wool conforming to JIS L0849.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical laminate and an article including the same, and in particular to an optical laminate used as an anti-reflection film suitable for displays that are used in a bent state, such as flexible displays, and an article including the same. [Background technology]

[0002] In recent years, mobile communication terminals such as smartphones and information devices such as notebook PCs equipped with foldable displays have been put on the market. In these displays, optical laminates such as anti-reflection films are sometimes used to reduce surface reflection. Optical laminates used in foldable displays are required to have higher durability against bending than non-foldable displays.

[0003] For example, Patent Document 1 proposes that in a hard coat film having a hard coat layer and an optical functional layer consisting of a sputtered film, the thickness ratio of the hard coat layer to the optical functional layer be set within a predetermined range to improve the bending resistance.

[0004] Furthermore, Patent Document 2 describes that bending resistance can be improved by making the hard coat layer and the antireflection layer out of resin. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2022-185597 A [Patent Document 2] JP 2020-74019 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, although Patent Document 1 aims to improve the abrasion resistance and bending resistance of the hard coat film, it does not evaluate the scratch resistance, and there is room for improvement. In addition, although Patent Document 2 also improves the bending resistance of the antireflection film, the antireflection layer is made of resin, and therefore the scratch resistance is poor.

[0007] The present invention has been made in consideration of the above problems, and aims to provide an optical laminate that can achieve excellent scratch resistance and further improves bending resistance, and an article including the same. [Means for solving the problem]

[0008] In order to solve the above problems, the present invention proposes the following means. [1] An optical laminate having, in this order, a transparent substrate, a hard coat layer, an adhesion layer made of a sputtered film, a high refractive index layer made of a sputtered film, and an optical functional layer in which a low refractive index layer having a refractive index lower than that of the high refractive index layer is alternately laminated, and an antifouling layer, The hard coat layer contains a silica filler, An optical laminate satisfying the following conditions 1 and 2. Condition 1: The ratio ((A) / (B)) of the Martens hardness (A) measured from the antifouling layer side of the optical laminate to the Martens hardness (B) measured from the hard coat layer side of a laminate having only the transparent substrate and the hard coat layer is 3.6 or less. Condition 2: Using a friction tester using steel wool conforming to JIS L0849, the steel wool is horizontally reciprocated 200 times, and the difference in the contact angle with water before and after friction is 20° or less.

[0009] [2] The optical laminate according to the above [1], wherein the silica filler is surface-modified with a functional group derived from a silane compound.

[0010] [3] The optical laminate according to the above [2], wherein the silane compound is one or more selected from a vinyl group-containing silane compound, a (meth)acryloyl group-containing silane compound, an amino group-containing silane compound, an isocyanate group-containing silane compound, an isocyanurate group-containing silane compound, an epoxy group-containing silane compound and a mercapto group-containing silane compound.

[0011] [4] The optical laminate according to the above [2], wherein the silane compound is a (meth)acryloyl group-containing silane compound.

[0012] [5] The hard coat layer contains a binder resin and a silica filler, The optical laminate according to the above [2], wherein the functional group derived from the silane compound has the same functional group as the binder resin.

[0013] [6] The binder resin contains a (meth)acrylate compound, The optical laminate according to the above-mentioned [5], wherein the functional group derived from the silane compound is a (meth)acryloyl group.

[0014] [7] The optical laminate according to the above [1], wherein the average particle size of the silica filler is 800 nm or less.

[0015] [8] The optical laminate according to the above [1], wherein the hard coat layer has a thickness of 0.5 μm or more and 100 μm or less.

[0016] [9] The optical laminate described in [1] above, in which, when the optical laminate is bent 180° so that the surface on which the antifouling layer is formed is on the outside, and a mandrel of the smallest diameter on which no cracks occur is used, the elongation S (%) of the optical functional layer calculated by the following formula (1) satisfies 1.3≦S. S(%)={(R2 / R1)-1}×100 ···(1) (where R2 is the distance from the axial center of the mandrel to the outer surface of the optical laminate, and R1 is the distance from the axial center of the mandrel to a virtual line indicating a position equivalent to 1 / 2 of the total thickness of the optical laminate.)

[0017]

[10] The optical laminate described in claim 9, wherein when the optical laminate is folded 180 degrees so that the surface on which the antifouling layer is formed is on the inside, the compression ratio C (%) of the optical functional layer calculated by the following formula (2) satisfies 4.5≦C when a mandrel of the smallest diameter that does not cause cracks is used. C(%)={1-(R3 / R1)}×100...(2) (wherein R3 is the distance from the axial center of the mandrel to the surface of the antifouling layer side of the optical laminate, and R1 is the distance from the axial center of the mandrel to an imaginary line indicating a position corresponding to 1 / 2 of the total thickness of the optical laminate.)

[0018]

[11] An article comprising the optical laminate according to any one of [1] to

[10] above. Effect of the Invention

[0019] According to the present invention, it is possible to provide an optical layered body that can realize excellent scratch resistance and further improved bending resistance, and an article including the optical layered body. [Brief description of the drawings]

[0020] [Figure 1] FIG. 2 is a cross-sectional view showing another example of the optical laminate of the present embodiment. [Diagram 2] FIG. 2 is a cross-sectional view showing another example of the optical laminate of the present embodiment. [Diagram 3] FIG. 2 is a schematic diagram for explaining an example of a manufacturing apparatus that can be used in the manufacturing method of the optical laminate of the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] Hereinafter, the present embodiment will be described in detail with reference to the drawings as appropriate. The drawings used in the following description may show characteristic parts in an enlarged scale for the sake of convenience in order to make the features of the present invention easier to understand, and the dimensional ratios of each component may differ from the actual ones. The materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited to them, and can be modified as appropriate within the scope of the effects.

[0022] [Optical laminate] FIG. 1 is a cross-sectional view showing another example of the optical laminate of the present embodiment. The optical laminate 102 shown in FIG. 1 is formed by laminating a transparent substrate 11, a hard coat layer 12, an adhesive layer 13, an optically functional layer 14, and an antifouling layer 15 in this order. The adhesion layer 13 is a layer that provides adhesion between the hard coat layer 12 and the optical functional layer 14 . The optical function layer 14 is a layer that exhibits an optical function. The optical function is a function that controls the properties of light, such as reflection, transmission, and refraction, and examples of the optical function include an anti-reflection function, a selective reflection function, and a lens function. The optical functional layer 14 preferably includes any one selected from an antireflection layer and a selective reflection layer. As the antireflection layer and the selective reflection layer, a known layer can be used. The antireflection layer and the selective reflection layer may be a single layer or a laminate of multiple layers.

[0023] FIG. 2 is a cross-sectional view showing another example of the optical laminate of the present embodiment. The optical laminate 101 shown in FIG. 2 is provided with an antireflection layer as the optical functional layer 14 in the optical laminate 102 shown in FIG. 1. The optical functional layer 14 (antireflection layer) is made of a laminate in which low refractive index layers 14b and high refractive index layers 14a are alternately laminated as shown in FIG. 1. The optical functional layer 14 shown in FIG. 1 is made of a hard coat layer 12, an adhesive layer 13, a high refractive index layer 14a, a low refractive index layer 14b, a high refractive index layer 14a, a low refractive index layer 14b, and an antifouling layer 15 laminated in this order from the transparent substrate 11 side. Therefore, the antifouling layer 15 is in contact with the low refractive index layer 14b of the optical functional layer 14.

[0024] The transparent substrate 11 may be formed of a transparent material capable of transmitting light in the visible light region. For example, a plastic film is preferably used as the transparent substrate 11. Specific examples of materials constituting the plastic film include polyester-based resins, acetate-based resins, polyethersulfone-based resins, polycarbonate-based resins, polyamide-based resins, polyimide-based resins, polyolefin-based resins, (meth)acrylic-based resins, polyvinyl chloride-based resins, polyvinylidene chloride-based resins, polystyrene-based resins, polyvinyl alcohol-based resins, polyarylate-based resins, and polyphenylene sulfide-based resins.

[0025] In the present invention, the term "transparent material" refers to a material having a transmittance of 80% or more for light in the wavelength range used, provided that the effect of the present invention is not impaired. In addition, in this embodiment, "(meth)acrylic" means methacryl and acrylic.

[0026] The transparent substrate 11 may contain a reinforcing material as long as the optical properties are not significantly impaired. Examples of the reinforcing material include cellulose nanofiber and nanosilica. In particular, polyester-based resins, acetate-based resins, polycarbonate-based resins, and polyolefin-based resins are preferably used as the reinforcing material. Specifically, a triacetyl cellulose (TAC) substrate is preferably used as the reinforcing material. The transparent substrate 11 may also be a glass film, which is an inorganic substrate.

[0027] When the plastic film is a TAC substrate, when the hard coat layer 12 is formed on one side of the plastic film, a permeation layer is formed in which a part of the components constituting the hard coat layer 12 permeates. As a result, the adhesion between the transparent substrate 11 and the hard coat layer 12 is improved, and the occurrence of interference fringes due to the difference in refractive index between the layers can be suppressed.

[0028] The transparent substrate 11 may be a film having optical and / or physical functions. Examples of films having optical and / or physical functions include a polarizing plate, a retardation compensation film, a heat ray blocking film, a transparent conductive film, a brightness improving film, and a barrier improving film.

[0029] The thickness of the transparent substrate 11 is not particularly limited, but is preferably, for example, 25 μm or more, and more preferably, 40 μm or more. When the transparent substrate 11 has a thickness of 25 μm or more, the rigidity of the substrate itself is ensured, and wrinkles are unlikely to occur even when stress is applied to the optical laminate 10. In addition, when the transparent substrate 11 has a thickness of 25 μm or more, wrinkles are unlikely to occur even when the hard coat layer 12 is continuously formed on the transparent substrate 11, and there are fewer manufacturing concerns, which is preferable. When the transparent substrate 11 has a thickness of 40 μm or more, wrinkles are even less likely to occur, which is preferable.

[0030] When the production is performed in a roll, the thickness of the transparent substrate 11 is preferably 1000 μm or less, and more preferably 600 μm or less. When the thickness of the transparent substrate 11 is 1000 μm or less, the optical laminate 10 during production and the optical laminate 10 after production can be easily wound into a roll shape, and the optical laminate 10 can be produced efficiently. Furthermore, when the thickness of the transparent substrate 11 is 1000 μm or less, the optical laminate 10 can be made thinner and lighter. When the thickness of the transparent substrate 11 is 600 μm or less, the optical laminate 10 can be produced more efficiently and can be made even thinner and lighter, which is preferable.

[0031] The surface of the transparent substrate 11 may be previously subjected to an etching treatment such as sputtering, corona discharge, ultraviolet irradiation, electron beam irradiation, conversion, oxidation, and / or an undercoat treatment. By previously performing these treatments, it is possible to improve the adhesion with the hard coat layer 12 formed on the transparent substrate 11. In addition, before forming the hard coat layer 12 on the transparent substrate 11, it is also preferable to remove dust and clean the surface of the transparent substrate 11 by subjecting the surface of the transparent substrate 11 to solvent cleaning, ultrasonic cleaning, or the like, as necessary.

[0032] The hard coat layer 12 contains a binder resin and a filler as essential components, and may contain other components such as a dispersant as optional components. A known binder resin can be used. The filler is contained in the binder resin to the extent that the transparency is not impaired. The filler may be made of an organic material, an inorganic material, or a combination of an organic material and an inorganic material, but from the viewpoint of hardness and flex resistance, an inorganic material is preferred, silica particles made of silica are more preferred, and surface-modified silica particles are particularly preferred.

[0033] The binder resin used in the hard coat layer 12 is preferably transparent, and examples of the binder resin that can be used include ionizing radiation curable resins that are cured by ultraviolet light or electron beams, thermoplastic resins, and thermosetting resins.

[0034] Examples of the ionizing radiation curable resin used as the binder resin of the hard coat layer 12 include ethyl (meth)acrylate, ethylhexyl (meth)acrylate, styrene, methylstyrene, and N-vinylpyrrolidone. Examples of the compound that is an ionizing radiation curable resin having two or more unsaturated bonds include trimethylolpropane tri(meth)acrylate, tripropylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,6-hexanediol di(meth)acrylate, dipentaerythritol hexa ... Examples of the polyfunctional compounds include erythritol penta(meth)acrylate, tripentaerythritol octa(meth)acrylate, tetrapentaerythritol deca(meth)acrylate, isocyanuric acid tri(meth)acrylate, isocyanuric acid di(meth)acrylate, polyester tri(meth)acrylate, polyester di(meth)acrylate, bisphenol di(meth)acrylate, diglycerin tetra(meth)acrylate, adamantyl di(meth)acrylate, isobornyl di(meth)acrylate, dicyclopentane di(meth)acrylate, tricyclodecane di(meth)acrylate, and ditrimethylolpropane tetra(meth)acrylate. Among them, pentaerythritol triacrylate (PETA), dipentaerythritol hexaacrylate (DPHA), and pentaerythritol tetraacrylate (PETTA) are preferably used. Incidentally, "(meth)acrylate" refers to methacrylate and acrylate. In addition, as the ionizing radiation curable resin, the above-mentioned compounds modified with PO (propylene oxide), EO (ethylene oxide), CL (caprolactone), etc. can also be used. In addition, urethane (meth)acrylate oligomers, epoxy (meth)acrylate oligomers, etc. can also be used from the viewpoint of film formation of the hard coat layer and adjustment of viscoelasticity.

[0035] Examples of the thermoplastic resin used for the binder resin of the hard coat layer 12 include styrene-based resins, (meth)acrylic resins, vinyl acetate-based resins, vinyl ether-based resins, halogen-containing resins, alicyclic olefin-based resins, polycarbonate-based resins, polyester-based resins, polyamide-based resins, cellulose derivatives, silicone-based resins, and rubber or elastomers. The thermoplastic resin is preferably non-crystalline and soluble in an organic solvent (particularly a common solvent capable of dissolving a plurality of polymers and curable compounds). In particular, from the viewpoint of transparency and weather resistance, styrene-based resins, (meth)acrylic resins, alicyclic olefin-based resins, polyester-based resins, cellulose derivatives (cellulose esters, etc.), and the like are preferred.

[0036] The hard coat layer 12 contains, for example, a binder resin and silica particles as a filler. The silica particles preferably contain silica particles that have been surface-modified in advance. Specific examples of the silane compound include vinyl group-containing silane compounds, (meth)acryloyl group-containing silane compounds, amino group-containing silane compounds, isocyanate group-containing silane compounds, isocyanurate group-containing silane compounds, epoxy group-containing silane compounds, and mercapto group-containing silane compounds. These may be used alone or in combination. The silane compound is appropriately selected according to the type of binder resin, and when the binder resin contains a functional group, a silane compound having the same functional group as the binder resin is preferred. For example, when the binder resin contains a (meth)acrylate compound as an ionizing radiation curable resin, the silane compound is preferably a (meth)acryloyl group-containing alkoxysilane compound. Note that "(meth)acrylate" refers to methacrylate and / or acrylate. In the present invention, methacrylate and acrylate are treated as the same thing in terms of reaction mechanism. The silane compound used for surface modification preferably has an alkoxysilyl group or a silanol group at its terminal, since this improves bonding with the hydroxyl groups present on the surface of the silica particles. By previously surface-modifying the silica particles, the dispersibility in the binder resin is improved, and the reaction between the surface treatment agent used for the surface modification and the binder resin causes the silica particles to bond more firmly to the binder resin, thereby improving the hardness of the optical laminate. These silica particles may be exposed on the surface of the hard coat layer 12 on the optical functional layer 14 side. In this case, the hard coat layer 12 and the optical functional layer 14 are bonded more strongly via the adhesion layer 13. Examples of the method for exposing the silica particles include glow treatment described later, and in this case, the surface modification of the exposed silica surface is removed. The filler is exposed on the surface of the hard coat layer, and the surface modification is removed at that time, which generates an electrostatic attraction between the hydroxyl groups on the filler surface and the adhesion layer 13 described below, thereby further improving adhesion. The exposed filler also contributes to improving adhesion by acting as an anchor to bite into the adhesion layer 13. The improvement in flex resistance is caused by a combination of the bonding with the binder resin due to the surface modification of the silica surface described above and the interaction between the silica and the adhesion layer.

[0037] The average particle size of the filler in the hard coat layer 12 is, for example, 800 nm or less, preferably 780 nm or less, and more preferably 100 nm or less. When the particle size of the filler is within this range, the haze value of the entire optical laminate 10 is 2% or less. The optical laminate 10 having a haze of 2% or less has high transparency and serves as a so-called clear type antireflection film.

[0038] The surface of the hard coat layer 12 is preferably subjected to, for example, glow discharge treatment, plasma treatment, ion etching, alkali treatment, etc. Among these, it is preferable to use the glow discharge treatment because it allows treatment over a large area. The intensity of the glow discharge treatment is, for example, 100 W / m2 in terms of electrode power density. 2 ~11000W / m 2 It can be done at 1600W / m 2 ~7000W / m 2 It is preferable to do so in the following manner. By performing a glow discharge treatment on the surface of the hard coat layer 12, the surface of the hard coat layer 12 is roughened at the nano level, and substances with weak binding strength present on the surface of the hard coat layer 12 are removed. As a result, the adhesion between the hard coat layer 12 and the adhesion layer 13 formed on the hard coat layer 12 is improved. In addition, there is also an effect of exposing silica particles from the hard coat layer 12. In addition, although increasing the strength during the discharge treatment tends to improve the flex resistance described below, the effect plateaus when the discharge strength exceeds a certain level, and excessive glow discharge strength also leads to deterioration of the resin constituting the hard coat layer, so it is preferable to perform the glow discharge treatment at a discharge strength within the above-mentioned range.

[0039] In addition, when an anti-glare type optical laminate is to be obtained, the average particle diameter of the filler of the hard coat layer 12 may be, for example, 0.5 μm or more. As a filler of this size, for example, organic fine particles such as acrylic resin are preferably used. When the particle diameter of the filler is within this range, the haze value of the entire optical laminate 10 exceeds 2%. An optical laminate 10 with a haze of more than 2% has anti-glare properties and becomes a so-called anti-glare (AG) type anti-reflection film. In this case, too, the average particle diameter of the filler is preferably 10 μm or less, more preferably 5 μm or less, and particularly preferably 3 μm or less. As the filler contained in the hard coat layer 12, various reinforcing materials can be used within a range that does not impair the optical properties in order to impart toughness to the hard coat layer 12. Examples of reinforcing materials include cellulose nanofibers.

[0040] The thickness of the hard coat layer 12 is not particularly limited, but is preferably 0.5 μm or more, and more preferably 1 μm or more. The thickness of the hard coat layer 12 is preferably 100 μm or less. When the thickness of the hard coat layer 12 is 0.5 μm or more, sufficient hardness is obtained, so that scratches during production are unlikely to occur. Furthermore, when the thickness of the hard coat layer 12 is 100 μm or less, the optical laminate 10 can be made thinner and lighter. Furthermore, when the thickness of the hard coat layer 12 is 100 μm or less, microcracks in the hard coat layer 12 that occur when the optical laminate 10 is bent during production are unlikely to occur, and productivity is good.

[0041] The hard coat layer 12 may be a single layer or a laminate of multiple layers. The hard coat layer 12 may further be provided with known functions such as ultraviolet absorbing performance, antistatic performance, refractive index adjusting function, and hardness adjusting function. Furthermore, the function imparted to the hard coat layer 12 may be imparted to a single hard coat layer, or may be imparted to a plurality of separate layers.

[0042] The adhesion layer 13 is a layer formed to improve adhesion between the transparent substrate 11 or the hard coat layer 12, which is an organic film, and the optical functional layer 14, which is an inorganic film. In the optical laminate 10 shown in FIG. 2, the adhesion layer 13 is provided between the hard coat layer 12 and the optical functional layer 14. The adhesion layer 13 has a function of adhering the hard coat layer 12 and the optical functional layer 14. The adhesion layer 13 is preferably made of a metal oxide or metal in an oxygen-deficient state. The metal oxide in an oxygen-deficient state refers to a metal oxide in a state in which the number of oxygen is deficient compared to the stoichiometric composition. Examples of the metal oxide in an oxygen-deficient state include SiOx, AlOx, TiOx, ZrOx, CeOx, MgOx, ZnOx, TaOx, SbOx, SnOx, and MnOx. Examples of the metal include Si, Al, Ti, Zr, Ce, Mg, Zn, Ta, Sb, Sn, Mn, and In. The adhesion layer 13 may be, for example, SiOx, where x is more than 0 and less than 2.0. The adhesion layer may be formed from a mixture of multiple types of metals or metal oxides. From the viewpoint of maintaining transparency and adhesion with the optical functional layer and obtaining good optical characteristics, the thickness of the adhesive layer is preferably more than 0 nm and not more than 20 nm, and particularly preferably 1 nm or more and 10 nm or less.

[0043] The optical functional layer 14 is a laminate that exhibits an anti-reflection function. The optical functional layer 14 shown in Fig. 2 is a laminate of four layers in total, in which high refractive index layers 14a and low refractive index layers 14b are alternately laminated in this order from the adhesive layer 13 side. The number of the high refractive index layers 14a and the low refractive index layers 14b is not particularly limited, and the number of the high refractive index layers 14a and the low refractive index layers 14b can be any number.

[0044] 2, the optical functional layer 14 is made of a laminate in which low refractive index layers 14b and high refractive index layers 14a are alternately laminated, so that the light incident from the antifouling layer 15 side interferes with each other through the optical functional layer 14, thereby reducing the intensity of the reflected light and providing an antireflection function. Therefore, an antireflection function is obtained that prevents the light incident from the antifouling layer 15 side from being reflected in one direction.

[0045] The low refractive index layer 14b contains, for example, a metal oxide. The low refractive index layer 14b may contain an oxide of Si from the viewpoints of availability and cost, and is preferably a layer mainly composed of SiO2 (oxide of Si) or the like. The SiO2 single layer film is colorless and transparent. In this embodiment, the main component of the low refractive index layer 14b means a component contained in the low refractive index layer 14b at 50 mass % or more. When the low refractive index layer 14b is a layer mainly composed of an oxide of Si, it may contain less than 50 mass% of another element. The content of the element other than the oxide of Si is preferably 10% or less. As the other element, for example, Na may be contained for the purpose of improving durability, Zr, Al or N for the purpose of improving hardness, and Zr, Al for the purpose of improving alkali resistance.

[0046] The refractive index of the low refractive index layer 14b is preferably 1.20 to 1.60, and more preferably 1.30 to 1.50. Examples of the dielectric material used for the low refractive index layer 14b include magnesium fluoride (MgF2, refractive index 1.38).

[0047] The refractive index of the high refractive index layer 14a is preferably 2.00 to 2.60, and more preferably 2.10 to 2.45. Examples of dielectric materials used for the high refractive index layer 14a include niobium pentoxide (Nb2O5, refractive index 2.33), titanium oxide (TiO2, refractive index 2.33 to 2.55), tungsten oxide (WO3, refractive index 2.2), cerium oxide (CeO2, refractive index 2.2), tantalum pentoxide (Ta2O5, refractive index 2.16), zinc oxide (ZnO, refractive index 2.1), indium tin oxide (ITO, refractive index 2.06), and zirconium oxide (ZrO2, refractive index 2.2). If it is desired to impart conductive properties to the high refractive index layer 14a, for example, ITO, indium zinc oxide (IZO) can be selected.

[0048] In the optical function layer 14, it is preferable to use, for example, a layer made of niobium pentoxide (Nb2O5, refractive index 2.33) as the high refractive index layer 14a and a layer made of SiO2 as the low refractive index layer 14b.

[0049] The thickness of the low refractive index layer 14b may be in the range of 1 nm to 200 nm, and is appropriately selected depending on the wavelength range in which the anti-reflection function is required. The thickness of the high refractive index layer 14a may be, for example, 1 nm or more and 200 nm or less, and is appropriately selected depending on the wavelength range in which the anti-reflection function is required. The thicknesses of the high refractive index layer 14a and the low refractive index layer 14b can be appropriately selected depending on the design of the optical function layer 14. For example, from the adhesive layer 13 side, the layers may be a high refractive index layer 14a of 5 to 50 nm, a low refractive index layer 14b of 10 to 80 nm, a high refractive index layer 14a of 20 to 200 nm, and a low refractive index layer 14b of 50 to 200 nm.

[0050] Of the layers constituting the optical functional layer 14, a low refractive index layer 14b is disposed on the side of the antifouling layer 15. When the low refractive index layer 14b of the optical functional layer 14 is in contact with the antifouling layer 15, the antireflection performance of the optical functional layer 14 is improved, which is preferable.

[0051] The antifouling layer 15 is formed on the outermost surface of the optical functional layer 14 and prevents the optical functional layer 14 from being soiled. Furthermore, when the antifouling layer 15 is applied to a touch panel or the like, it suppresses wear of the optical functional layer 14 due to its abrasion resistance. The antifouling layer 15 of this embodiment is made of a vapor-deposited film formed by vapor-depositing an antifouling material. In this embodiment, the antifouling layer 15 is formed by vacuum-depositing a fluorine-based organic compound as the antifouling material on one surface of the low refractive index layer 14b constituting the optical functional layer 14. In this embodiment, since the antifouling material contains a fluorine-based organic compound, the optical laminate 10 has even better abrasion resistance and alkali resistance.

[0052] A compound consisting of a fluorine-modified organic group and a reactive silyl group (e.g., alkoxysilane) is preferably used as the fluorine-based organic compound constituting the antifouling layer 15. Examples of commercially available products include Optool DSX (manufactured by Daikin Corporation) and KY-100 series (manufactured by Shin-Etsu Chemical Co., Ltd.).

[0053] When a compound consisting of a fluorine-modified organic group and a reactive silyl group (e.g., alkoxysilane) is used as the fluorine-based organic compound constituting the antifouling layer 15, and a layer consisting of SiO2 is used as the low refractive index layer 14b of the optical functional layer 14 in contact with the antifouling layer 15, a siloxane bond is formed between the silanol group, which is the skeleton of the fluorine-based organic compound, and the SiO2. This results in good adhesion between the optical functional layer 14 and the antifouling layer 15, which is preferable.

[0054] The optical thickness of the antifouling layer 15 may be in the range of 1 nm or more and 20 nm or less, and is preferably in the range of 3 nm or more and 10 nm or less. When the thickness of the antifouling layer 15 is 1 nm or more, the abrasion resistance can be sufficiently ensured when the optical laminate 10 is applied to a touch panel or the like. When the thickness of the antifouling layer 15 is 3 nm or more, the liquid resistance and the like of the optical laminate 10 are improved. When the thickness of the antifouling layer 15 is 20 nm or less, the time required for vapor deposition is short, and the optical laminate 10 can be efficiently manufactured.

[0055] In the optical laminate 10, 102 configured as described above, the ratio ((A) / (B)) of the Martens hardness (A) measured from the antifouling layer 15 side of the optical laminate 10, 102 to the Martens hardness measured from the hard coat layer 12 side of a laminate having only the transparent substrate 11 and the hard coat layer 12 is 3.6 or less (condition 1). Moreover, the ratio ((A) / (B)) is preferably 3.5 or less, more preferably 3.4 or less. When the ratio ((A) / (B)) is 3.6 or less, the difference in hardness between the hard coat layer surface and the antifouling layer surface is small, thereby suppressing deformation, and as a result, excellent scratch resistance can be realized and bending resistance can be further improved.

[0056] In addition, in the optical laminate 10, 102 configured as described above, a contact angle difference with water before and after rubbing in which the steel wool is horizontally reciprocated 200 times using a friction tester using steel wool conforming to JIS L0849 is 20° or less (condition 2). If the optical laminate 10, 102 has a high hardness, the contact angle difference becomes 20° or less, and excellent scratch resistance can be realized.

[0057] In the optical laminate 10, 102 configured as described above, when the optical laminate 10, 102 is bent 180° so that the surface on which the antifouling layer 15 is formed is on the outside, the elongation S (%) of the optical functional layer 14 calculated by the following formula (1) when using a mandrel with the smallest diameter at which no cracks occur preferably satisfies 1.3≦S. This allows the bending resistance of the optical laminate 10, 102 to be further improved. S = {(R2 / R1)-1} × 100 (1) (where R2 is the distance from the axial center of the mandrel to the outer surface of the optical laminate, and R1 is the distance from the axial center of the mandrel to a virtual line indicating a position corresponding to 1 / 2 of the total thickness of the optical laminate.)

[0058] Furthermore, in the optical laminate 10, 102, when the optical laminate 10, 102 is folded 180° so that the surface on which the antifouling layer 15 is formed is on the inside, the compression ratio C (%) of the optical functional layer 14 calculated by the following formula (2) when a mandrel of the smallest diameter that does not cause cracks is used preferably satisfies 4.5≦C, and more preferably satisfies 5≦C. This allows the bending resistance of the optical laminate 10, 102 to be further improved. C(%)={1-(R3 / R1)}×100 ···(2) (wherein R3 is the distance from the axial center of the mandrel to the surface of the antifouling layer side of the optical laminate, and R1 is the distance from the axial center of the mandrel to an imaginary line indicating a position corresponding to 1 / 2 of the total thickness of the optical laminate.)

[0059] Furthermore, the optical functional layer 14 preferably satisfies both the above range of the elongation percentage S (%) and the above range of the compression percentage C (%). That is, in the optical laminate 10, 102, when the optical laminate 10, 102 is folded 180° so that the surface on which the antifouling layer 15 is formed is on the outside, the elongation percentage S (%) of the optical functional layer 14 calculated by the following formula (1) satisfies 1.3≦S when a mandrel of the smallest diameter at which no cracks are generated is used, and when the optical laminate 10, 102 is folded 180° so that the surface on which the antifouling layer 15 is formed is on the inside, the compression percentage C (%) of the optical functional layer 14 calculated by the above formula (2) satisfies 4.5≦C. This can further improve the bending resistance of the optical laminate 10, 102.

[0060] The above elongation percentages are values ​​when the substrate is PET and the thickness is 50 μm, and these values ​​may vary if the thickness is reduced.

[0061] In the optical laminate 10, 102 configured as described above, when the thickness of the hard coat layer of the optical laminate is 5 μm, the optical laminate 10, 102 is folded 180° so that the surface on which the anti-fouling layer 15 is formed is on the outside. The diameter of the mandrel is gradually replaced with one that is smaller, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which the first crack was discovered is preferably 4.0φmm or less, more preferably 3.5φmm or less, and even more preferably 3.0φmm or less.

[0062] Furthermore, when the thickness of the hard coat layer of the optical laminate is 5 μm, and the optical laminate 10, 102 is folded 180° so that the surface on which the anti-fouling layer 15 is formed is on the inside, the diameter of the mandrel is gradually replaced with one that is smaller, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which the first crack was discovered is preferably 1.1φmm or less, and more preferably less than 1.0φmm.

[0063] Furthermore, when the thickness of the hard coat layer of the optical laminate is 5 μm, it is more preferable that when the optical laminate 10, 102 is bent 180° so that the surface on which the anti-fouling layer 15 is formed is on the outside, the diameter of the mandrel is gradually replaced with a smaller one, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which a crack was first discovered is 4.0 φmm or less, and that when the optical laminate 10, 102 is bent 180° so that the surface on which the anti-fouling layer 15 is formed is on the inside, the diameter of the mandrel is gradually replaced with a smaller one, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which a crack was first discovered is 1.1 φmm or less.

[0064] In the optical laminate 10, 102 configured as described above, when the thickness of the hard coat layer of the optical laminate is 10 μm, the optical laminate 10, 102 is folded 180° so that the surface on which the anti-fouling layer 15 is formed is on the outside. The diameter of the mandrel is gradually replaced with one that is smaller, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which the first crack was discovered is preferably 4.0φmm or less, more preferably 3.5φmm or less, and even more preferably 3.0φmm or less.

[0065] Furthermore, when the thickness of the hard coat layer of the optical laminate is 10 μm, and the optical laminate 10, 102 is folded 180° so that the surface on which the anti-fouling layer 15 is formed is on the inside, the diameter of the mandrel is gradually replaced with one that is smaller, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which the first crack was discovered is preferably 1.4φmm or less, and more preferably 1.2φmm or less.

[0066] Furthermore, when the thickness of the hard coat layer of the optical laminate is 10 μm, it is more preferable that when the optical laminate 10, 102 is bent 180° so that the surface on which the anti-fouling layer 15 is formed is on the outside, the diameter of the mandrel is gradually changed to smaller ones, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which a crack was first discovered is 4.0 φmm or less, and that when the optical laminate 10, 102 is bent 180° so that the surface on which the anti-fouling layer 15 is formed is on the inside, the diameter of the mandrel is gradually changed to smaller ones, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which a crack was first discovered is 1.4 φmm or less.

[0067] In the optical laminate 10, 102 configured as described above, when the thickness of the hard coat layer of the optical laminate is 2 μm, the optical laminate 10, 102 is folded 180° so that the surface on which the anti-fouling layer 15 is formed is on the outside. The diameter of the mandrel is gradually replaced with one that is smaller, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which the first crack was discovered is preferably 4.0φmm or less, more preferably 3.5φmm or less, and even more preferably 3.0φmm or less.

[0068] Furthermore, when the thickness of the hard coat layer of the optical laminate is 2 μm, and the optical laminate 10, 102 is folded 180° so that the surface on which the anti-fouling layer 15 is formed is on the inside, the diameter of the mandrel is gradually replaced with one that is smaller, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which the first crack was discovered is preferably 1.1φmm or less, and more preferably less than 1.0φmm.

[0069] Furthermore, when the thickness of the hard coat layer of the optical laminate is 2 μm, it is more preferable that when the optical laminate 10, 102 is bent 180° so that the surface on which the anti-fouling layer 15 is formed is on the outside, the diameter of the mandrel is gradually replaced with a smaller one, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which a crack was first discovered is 4.0 φmm or less, and that when the optical laminate 10, 102 is bent 180° so that the surface on which the anti-fouling layer 15 is formed is on the inside, the diameter of the mandrel is gradually replaced with a smaller one, and the diameter of the mandrel that is 0.2 mm larger than the diameter of the mandrel at which a crack was first discovered is 1.1 φmm or less.

[0070] The mandrel diameter is calculated by cutting out three identical samples, measuring them, and averaging the three measurements.

[0071] [Method of manufacturing optical laminate] The optical laminate 10 of this embodiment shown in FIG. 2 can be produced, for example, by the method described below. In this embodiment, as an example of a method for producing the optical laminate 10, a case in which the optical laminate 10 is produced using the transparent base material 11 wound in a roll shape will be described. First, the transparent substrate 11 wound in a roll shape is unwound. Then, a slurry containing a material to be the hard coat layer 12 is applied onto the transparent substrate 11 by a known method, and cured by a known method corresponding to the material to be the hard coat layer 12. The slurry used may be, for example, a composition containing a binder resin and silica particles as a filler, and this composition is applied onto the transparent substrate 11 and then cured. In this way, the hard coat layer 12 is formed on the transparent substrate 11 (hard coat layer forming step). The above composition may contain one or more additives such as a polymerization initiator and a leveling agent as necessary. As the polymerization initiator, for example, a photopolymerization initiator is used. Then, the transparent substrate 11 on which the hard coat layer 12 is formed is wound into a roll shape by a known method.

[0072] Next, an adhesion layer forming step of forming an adhesion layer 13 on the hard coat layer 12 and an optical function layer forming step of forming an optical function layer 14 are performed. Then, an antifouling layer forming step of forming an antifouling layer 15 on the optical function layer 14 is performed. In this embodiment, it is preferable to perform a first surface treatment step of treating the surface of the hard coat layer 12 before the optical function layer forming step, and then perform the adhesion layer forming step and the optical function layer forming step. Also, in this embodiment, it is preferable to perform a second surface treatment step of treating the surface of the optical function layer 14 after the optical function layer forming step, and then perform the antifouling layer forming step.

[0073] In the manufacturing method of the optical laminate 10 of this embodiment, the first surface treatment step, the adhesion layer forming step, the optical functional layer forming step, the second surface treatment step, and the antifouling layer forming step are preferably performed successively while the optical laminate in the middle of manufacture is maintained under reduced pressure. When the first surface treatment step, the adhesion layer forming step, the optical functional layer forming step, the second surface treatment step, and the antifouling layer forming step are performed successively while the optical laminate in the middle of manufacture is maintained under reduced pressure, for example, a device equipped with a thin film forming device described in Patent Document 4 can be used as a sputtering device.

[0074] A specific example of a production apparatus that can be used in the method for producing the optical laminate of this embodiment is a production apparatus 20 shown in FIG. The manufacturing apparatus 20 shown in Fig. 3 includes a roll unwinding device 4, a pretreatment device 2A, a sputtering device 1, a pretreatment device 2B, a vapor deposition device 3, and a roll winding device 5. As shown in Fig. 3, these devices 4, 2A, 1, 2B, 3, and 5 are connected in this order. The manufacturing apparatus 20 shown in Fig. 3 is a roll-to-roll type manufacturing apparatus that unwinds a substrate from a roll, passes the substrate through connected devices (pretreatment device 2A, sputtering device 1, pretreatment device 2B, and vapor deposition device 3 in Fig. 3) in succession, and then winds the substrate, thereby continuously forming multiple layers on the substrate.

[0075] When the optical laminate 10 is manufactured using a roll-to-roll manufacturing device, the conveying speed (line speed) of the optical laminate 10 during the manufacturing process can be appropriately set. The conveying speed is, for example, preferably 0.5 to 20 m / min, and more preferably 0.5 to 10 m / min.

[0076] <Roll unwinding device> The roll unwinding device 4 shown in Fig. 3 has a chamber 34 inside which a predetermined reduced pressure atmosphere is maintained, one or more vacuum pumps 21 (one in Fig. 3) that exhaust gas from within the chamber 34 to create a reduced pressure atmosphere, and an unwinding roll 23 and a guide roll 22 installed within the chamber 34. As shown in Fig. 3, the chamber 34 is connected to the chamber 31 of the sputtering apparatus 1 via a pretreatment device 2A. The transparent substrate 11 having the hard coat layer 12 formed on the surface thereof is wound around the unwinding roll 23. The unwinding roll 23 supplies the transparent substrate 11 having the hard coat layer 12 formed on the surface thereof to the pretreatment device 2A at a predetermined transport speed.

[0077] <Pretreatment device 2A> The pretreatment device 2A shown in Fig. 3 has a chamber 32 with a predetermined reduced pressure atmosphere inside, a can roll 26, a plurality of (two in Fig. 3) guide rolls 22, and a plasma discharge device 42. As shown in Fig. 3, the can roll 26, the guide roll 22, and the plasma discharge device 42 are installed in the chamber 32. As shown in Fig. 3, the chamber 32 is connected to the chamber 31 of the sputtering device 1.

[0078] The can roll 26 and the guide roll 22 transport the transparent substrate 11 on which the hard coat layer 12 has been formed, which has been sent from the roll unwinding device 4, at a predetermined transport speed, and send the transparent substrate 11 with the surface of the hard coat layer 12 treated thereon to the sputtering device 1. As shown in Fig. 3, the plasma discharge device 42 is disposed facing the outer peripheral surface of the can roll 26 at a predetermined distance. The plasma discharge device 42 ionizes the gas by glow discharge. The gas is preferably inexpensive and inert and does not affect the optical properties, and examples of the gas that can be used include argon gas, oxygen gas, nitrogen gas, and helium gas. In this embodiment, it is preferable to use argon gas or oxygen gas as the gas.

[0079] <Sputtering equipment> The sputtering apparatus 1 shown in Fig. 3 includes a chamber 31 with a predetermined reduced pressure atmosphere inside, one or more vacuum pumps 21 (two in Fig. 3) that exhaust gas from the chamber 31 to create a reduced pressure atmosphere, a film-forming roll 25, a plurality of guide rolls 22 (two in Fig. 4), and a plurality of film-forming units 41 (four in the example shown in Fig. 3). As shown in Fig. 3, the film-forming roll 25, the guide roll 22, and the film-forming units 41 are installed in the chamber 31. As shown in Fig. 3, the chamber 31 is connected to a chamber 32 of a pretreatment device 2B.

[0080] The film-forming roll 25 and the guide roll 22 transport the transparent substrate 11 having the surface-treated hard coat layer 12 formed thereon, which has been sent from the pre-processing device 2A, at a predetermined transport speed, and supply the transparent substrate 11 having the adhesion layer 13 and the optical functional layer 14 formed on the hard coat layer 12 to the pre-processing device 2B. In the sputtering apparatus 1 shown in FIG. 3, an adhesion layer 13 is laminated by sputtering on the hard coat layer 12 of the transparent substrate 11 running on a film-forming roll 25, and a high refractive index layer 14a and a low refractive index layer 14b are alternately laminated on top of the adhesion layer 13 to form an optically functional layer 14.

[0081] As shown in FIG. 3, the film forming unit 41 is disposed facing the outer peripheral surface of the film forming roll 25 at a predetermined interval, and a plurality of film forming units 41 are provided so as to surround the film forming roll 25. The number of film forming units 41 is determined according to the total number of laminations of the adhesive layer 13 and the high refractive index layer 14a and the low refractive index layer 14b forming the optical functional layer 14. When it is difficult to ensure the distance between adjacent film forming units 41 because the total number of laminations of the adhesive layer 13 and the high refractive index layer 14a and the low refractive index layer 14b forming the optical functional layer 14 is large, a plurality of film forming rolls 25 may be provided in the chamber 31, and the film forming unit 41 may be disposed around each film forming roll 25. When a plurality of film forming rolls 25 are provided, a guide roll 22 may be further provided as necessary. A plurality of chambers 31 provided with the film forming rolls 25 and the film forming units 41 may be connected. In addition, the diameter of the film forming roll 25 may be appropriately changed in order to easily ensure the distance between adjacent film forming units 41.

[0082] A predetermined target (not shown) is installed in each film forming section 41. A voltage is applied to the target by a known structure. In this embodiment, a gas supply section (not shown) that supplies a predetermined reactive gas and a carrier gas to the target at a predetermined flow rate, and a known magnetic field generating source (not shown) that forms a magnetic field on the surface of the target are provided near the target.

[0083] The target material and the type and flow rate of the reactive gas are appropriately determined according to the composition of the adhesion layer 13, the high refractive index layer 14a, and the low refractive index layer 14b formed on the transparent substrate 11 by passing between the film forming unit 41 and the film forming roll 25. For example, when forming a layer made of SiO2, Si is used as the target and O2 is used as the reactive gas. Also, for example, when forming a layer made of Nb2O5, Nb is used as the target and O2 is used as the reactive gas. The low refractive index layer 14b is preferably formed at a vacuum degree of less than 0.5 Pa, and the high refractive index layer 14a is preferably formed at a vacuum degree of less than 1.0 Pa. When these layers are formed at the vacuum degree, the optical function layer 14 becomes dense, the water vapor transmission rate decreases, and the durability and the like improve.

[0084] In this embodiment, from the viewpoint of increasing the film formation speed, it is preferable to use magnetron sputtering as the sputtering method. The sputtering method is not limited to magnetron sputtering, and a two-pole sputtering method using plasma generated by direct current glow discharge or high frequency, or a three-pole sputtering method with an additional hot cathode may also be used.

[0085] The sputtering apparatus 1 includes an optical monitor (not shown) as a measurement unit that measures optical characteristics after forming each layer that becomes the adhesive layer 13 and the optical functional layer 14. This makes it possible to confirm the quality of the formed adhesive layer 13 and optical functional layer 14. When the sputtering apparatus 1 has, for example, two or more chambers, it is preferable to install an optical monitor in each chamber.

[0086] An example of the optical monitor (not shown) is one that measures the optical characteristics in the width direction of the adhesive layer 13 and the optical functional layer 14 formed on the hard coat layer 12 using an optical head capable of scanning in the width direction. When such an optical monitor is provided, for example, the peak wavelength of reflectance is measured as the optical characteristic, and the optical thickness distribution in the width direction of the adhesive layer 13 and the optical functional layer 14 can be measured by converting it into an optical thickness. By measuring the optical characteristics using the optical monitor, it is possible to form an optical laminate 10 including an adhesive layer 13 and an optical functional layer 14 having optimal optical characteristics while adjusting the sputtering conditions in real time.

[0087] <Pretreatment device 2B> The pretreatment device 2B shown in Fig. 3 has a chamber 32 with a predetermined reduced pressure atmosphere inside, a can roll 26, a plurality of (two in Fig. 3) guide rolls 22, and a plasma discharge device 42. As shown in Fig. 3, the can roll 26, the guide roll 22, and the plasma discharge device 42 are installed in the chamber 32. As shown in Fig. 3, the chamber 32 is connected to a chamber 33 of the deposition device 3.

[0088] The can roll 26 and the guide roll 22 transport the transparent substrate 11, on which each layer up to the optical functional layer 14 has been formed, sent from the sputtering device 1 at a predetermined transport speed, and send the transparent substrate 11, on which the surface of the optical functional layer 14 has been treated, to the deposition device 3. As the plasma discharge device 42, for example, the same device as the pretreatment device 2A can be used.

[0089] <Vapor deposition equipment> The deposition apparatus 3 shown in Fig. 4 includes a chamber 33 having a predetermined reduced pressure atmosphere inside, one or more vacuum pumps 21 (one in Fig. 3) that exhaust gas from the chamber 33 to create a reduced pressure atmosphere, a plurality of guide rolls 22 (four in Fig. 3), a deposition source 43, and a heating device 53. As shown in Fig. 3, the guide roll 22 and the deposition source 43 are installed in the chamber 33. The chamber 33 is connected to a chamber 35 of a roll winding device 5.

[0090] The vapor deposition source 43 is disposed opposite to the transparent substrate 11 having the treated surface of the optical functional layer 14, which is transported approximately horizontally between two adjacent guide rolls 22. The vapor deposition source 43 supplies evaporated gas made of a material that will become the antifouling layer 15 onto the optical functional layer 14. The orientation of the vapor deposition source 43 can be set arbitrarily. The heating device 53 heats the material that will become the antifouling layer 15 to the vapor pressure temperature. The heating device 53 may be one that uses a resistance heating method, a heater heating method, an induction heating method, an electron beam method, or the like. In the resistance heating method, a container that contains the antifouling material that will become the antifouling layer 15 is used as a resistor and electrically heated. In the heater heating method, the container is heated by a heater arranged on the outer periphery of the container. In the induction heating method, the container or the antifouling material is heated by electromagnetic induction from an induction coil installed externally.

[0091] The deposition apparatus 3 shown in FIG. 3 includes a guide plate (not shown) for guiding the deposition material evaporated from the deposition source 43 to a predetermined position, a thickness gauge (not shown) for observing the thickness of the antifouling layer 15 formed by deposition, a vacuum pressure gauge (not shown) for measuring the pressure inside the chamber 33, and a power supply (not shown). The guide plate may have any shape as long as it can guide the evaporated deposition material to a desired position. If the guide plate is not necessary, it does not have to be provided. As the vacuum pressure gauge, for example, an ion gauge can be used. The power supply device may be, for example, a high frequency power supply.

[0092] <Roll winding device> The roll winding device 5 shown in Figure 3 has a chamber 35 inside which a predetermined reduced pressure atmosphere is maintained, one or more vacuum pumps 21 (one in Figure 3) that evacuate the gas inside the chamber 35 to create a reduced pressure atmosphere, and a winding roll 24 and a guide roll 22 installed inside the chamber 35. The transparent substrate 11 (optical laminate 10) having each layer formed on its surface up to the antifouling layer 15 is wound around the winding roll 24. The winding roll 24 and the guide roll 22 wind up the optical laminate 10 at a predetermined winding speed. If necessary, a carrier film may also be used.

[0093] 4 may be equipped with a dry pump, an oil rotary pump, a turbo molecular pump, an oil diffusion pump, a cryopump, a sputter ion pump, a getter pump, etc. The vacuum pump 21 may be appropriately selected or used in combination to create a desired reduced pressure state in each of the chambers 31, 32, 33, 34, and 35.

[0094] The vacuum pump 21 may be installed at any position and in any number in the manufacturing apparatus 20 as long as it can maintain both the chamber 31 of the sputtering apparatus 1 and the chamber 33 of the deposition apparatus 3 in a desired reduced pressure state. In the manufacturing apparatus 20 shown in FIG. 3, the roll unwinding apparatus 4, the pretreatment apparatus 2A, the sputtering apparatus 1, the pretreatment apparatus 2B, the deposition apparatus 3, and the roll winding apparatus 5 are connected. For this reason, the vacuum pump 21 may be installed in each of the chambers 31, 32, 33, 34, and 35, or may be installed in only some of the chambers 31, 32, 33, 34, and 35 as long as it can maintain both the chamber 31 of the sputtering apparatus 1 and the chamber 33 of the deposition apparatus 3 in a desired reduced pressure state.

[0095] Next, a method will be described in which the first surface treatment step, the adhesion layer formation step, the optical functional layer formation step, the second surface treatment step, and the antifouling layer formation step are successively performed using the manufacturing apparatus 20 shown in FIG. 3 while maintaining the optical laminate 10 in the middle of production under reduced pressure. First, the unwinding roll 23 around which the transparent substrate 11 having the hard coat layer 12 formed on its surface is wound is placed in the chamber 34 of the roll unwinding device 4. Then, the unwinding roll 23 and the guide roll 22 are rotated to send the transparent substrate 11 having the hard coat layer 12 formed on its surface to the pretreatment device 2A at a predetermined transport speed.

[0096] Next, in the chamber 32 of the pretreatment device 2A, a first surface treatment step is performed as a pretreatment for the surface on which the adhesion layer 13 and the optical functional layer 14 are to be formed. In this embodiment, the first surface treatment step is performed on the transparent substrate 11 on which the hard coat layer 12 is formed. In the first surface treatment step, the can roll 26 and the guide roll 22 are rotated to transport the transparent substrate 11 on which the hard coat layer 12 is formed at a predetermined transport speed, while treating the surface of the hard coat layer 12 running on the can roll 26.

[0097] Examples of methods that can be used for treating the surface of the hard coat layer 12 include glow discharge treatment, plasma treatment, ion etching, and alkali treatment. As described above, among these, it is preferable to use the glow discharge treatment because it allows treatment over a large area.

[0098] Next, an adhesion layer forming step and an optical functional layer forming step are performed in the chamber 31 of the sputtering device 1. Specifically, the adhesion layer 13 and the optical functional layer 14 are formed on the hard coat layer 12 running on the film formation roll 25 while the transparent substrate 11 on which the hard coat layer 12 has been formed is transported at a predetermined transport speed by rotating the film formation roll 25 and the guide roll 22.

[0099] In this embodiment, the adhesive layer 13 is formed by sputtering while changing the material of the target placed in each film forming section 41 or the type and flow rate of the reactive gas supplied from the gas supply section, and the high refractive index layer 14a and the low refractive index layer 14b are alternately laminated thereon. That is, the adhesive layer forming process and the optical function layer forming process are performed continuously in the sputtering apparatus 1. In this way, the adhesive layer 13 and the optical function layer 14, which is an anti-reflection layer, are formed. The high refractive index layer 14a and the low refractive index layer 14b are formed under conditions of a predetermined vacuum level or less. Specifically, the high refractive index layer 14a is formed at a vacuum level of less than 1.0 Pa, and the low refractive index layer 14b is formed at a vacuum level of less than 0.5 Pa.

[0100] When a SiOx film is formed as the adhesion layer 13, it is preferable to form it by reactive sputtering using a silicon target in a mixed gas atmosphere of oxygen gas and argon gas. When the adhesive layer 13, the high refractive index layer 14a, and the low refractive index layer 14b are successively laminated by sputtering, the target material may be changed when forming the adhesive layer 13, the high refractive index layer 14a, and the low refractive index layer 14b. Alternatively, for example, one type of material may be used as the target, and a layer made of the target material and a layer made of an oxide of the target material may be alternately formed by changing the flow rate of oxygen (reactive gas) during sputtering to form the adhesive layer 13, the high refractive index layer 14a, and the low refractive index layer 14b.

[0101] The pressure during sputtering to form the adhesion layer 13 and the optical functional layer 14 varies depending on the metal to be sputtered, but may be 2 Pa or less, preferably 1 Pa or less, more preferably 0.6 Pa or less, and particularly preferably 0.2 Pa or less. When the pressure during sputtering is reduced to 1 Pa or less, the mean free path of the film-forming molecules becomes longer, and the film-forming molecules are laminated while maintaining their high energy, resulting in a denser and better film quality. It is preferable that the pressure during sputtering of the high refractive index layer and the low refractive index layer be different. This is because the mean free path differs for each film-forming type. By changing the pressure for each film-forming type, a denser film can be formed.

[0102] Thereafter, the transparent substrate 11 having the adhesion layer 13 and the optical functional layer 14 formed on the hard coat layer 12 is sent to the pretreatment device 2B by the rotation of the film-forming roll 25 and the guide roll 22. Next, in the chamber 32 of the pretreatment device 2B, a second surface treatment step is performed as a pretreatment for the surface on which the antifouling layer 15 is to be formed. In this embodiment, the transparent substrate 11 on which the optical functional layer 14 has been formed, obtained by the optical functional layer forming step, is continuously subjected to the second surface treatment step while being maintained under reduced pressure without being exposed to the air. In the second surface treatment process, the can roll 26 and the guide roll 22 are rotated to transport the transparent substrate 11, on which each layer up to the optical functional layer 14 has been formed, at a predetermined transport speed, while a discharge treatment is performed on the surface of the optical functional layer 14 running on the can roll 26.

[0103] Examples of methods that can be used for treating the surface of the optical functional layer 14 include glow discharge treatment, plasma treatment, ion etching, and alkali treatment. Among these, it is preferable to use the glow discharge treatment because it allows treatment over a large area.

[0104] When the surface of the optical functional layer 14 is subjected to a discharge treatment, the surface of the optical functional layer 14 is etched, and the surface state of the optical functional layer 14 changes. The surface state of the optical functional layer 14 is expressed by the surface roughness Ra or the average length of the elements RSm. For example, in the case of a clear type anti-reflective film in which the haze of the optical functional layer 14 is 2.0 or less, the surface state of the optical functional layer 14 is easily defined by the surface roughness Ra. Also, for example, in the case of an AG type anti-reflective film in which the haze of the optical functional layer 14 is more than 2.0, the surface state of the optical functional layer 14 is easily defined by the average length of the elements RSm. The surface roughness Ra and the average length of the elements RSm are measured in accordance with JIS B0601 (ISO4287).

[0105] Thereafter, the transparent substrate 11 with the surface of the optical functional layer 14 treated is sent to the deposition device 3 by the rotation of the can roll 26 and the guide roll 22 . Next, an antifouling layer forming step is performed in the chamber 33 of the deposition device 3. In this embodiment, the transparent substrate 11 having the treated surface of the optical functional layer 14 obtained by the second surface treatment step is continuously subjected to the antifouling layer forming step while being maintained under reduced pressure without being exposed to the air. In the antifouling layer forming process, the guide roll 22 is rotated to transport the transparent substrate 11 having the treated surface of the optical functional layer 14 at a predetermined transport speed, while the deposition source 43 is deposited on the surface of the optical functional layer 14.

[0106] In this embodiment, for example, an antifouling material made of a fluorine-based organic compound that becomes the antifouling layer 15 is heated to a vapor pressure temperature by a heating device 53, and the resulting evaporated gas is supplied from a deposition source 43 in a reduced pressure environment and adhered to the optical functional layer 14 whose surface has been treated, thereby forming the antifouling layer 15 by vacuum deposition. The pressure during vacuum deposition of the antifouling layer 15 is, for example, preferably 0.05 Pa or less, more preferably 0.01 Pa or less, and particularly preferably 0.001 Pa or less. When the pressure during vacuum deposition is a reduced pressure of 0.05 Pa or less, the mean free path of the film-forming molecules is long and the deposition energy is high, so that a denser and better antifouling layer 15 can be obtained.

[0107] By the above method, an optical laminate 10 is obtained in which an antifouling layer 15 is formed by vacuum deposition on the adhesion layer 13 and the optical functional layer 14 formed by sputtering. The antifouling layer 15 after film formation preferably has an initial fluorine content of 0.03 or more as measured by X-ray fluorescence analysis (XRF).

[0108] Thereafter, the transparent substrate 11 (optical laminate 10) on which each layer up to the antifouling layer 15 has been formed is sent to a roll winding device 5 by the rotation of the guide roll 22. Then, in the chamber 35 of the roll winding device 5 , the optical laminate 10 is wound around the winding roll 24 by the rotation of the winding roll 24 and the guide roll 22 .

[0109] In this embodiment, it is preferable to perform the optical functional layer forming step and the antifouling layer forming step continuously under reduced pressure. In particular, as in the manufacturing method of this embodiment using the manufacturing apparatus 20 shown in FIG. 3, when the optical laminate 10 is continuously manufactured as a wound body by a roll-to-roll method, it is more preferable to perform the optical functional layer forming step and the antifouling layer forming step continuously in-line while maintaining a reduced pressure state. In-line means that the antifouling layer forming step is performed without exposing the optical functional layer 14 formed in the optical functional layer forming step to the air. By performing the optical functional layer forming step and the antifouling layer forming step continuously under reduced pressure, it is possible to suppress the generation of a natural oxide film on the optical functional layer 14 formed in the optical functional layer forming step before forming the antifouling layer 15. In addition, it is possible to prevent contamination such as foreign matter when winding the roll from adhering to the optical functional layer 14 and inhibiting the adhesion between the optical functional layer 14 and the antifouling layer 15. Therefore, compared to the case where, after the optical functional layer formation step, the transparent substrate 11 on which each layer up to the optical functional layer 14 has been formed is removed from the chamber under reduced pressure, and then placed back in the chamber to perform the anti-fouling layer formation step under reduced pressure, an optical laminate having good adhesion between the optical functional layer 14 and the anti-fouling layer 15 and excellent transparency can be obtained.

[0110] In addition, since the antifouling layer 15 of the optical laminate 10 of this embodiment is a vapor deposition film, it has high abrasion resistance compared to, for example, an antifouling film formed by a coating method. This is presumed to be due to the following reasons. That is, in the antifouling film formed by the coating method, voids due to the solvent contained in the paint exist. In contrast, there are no voids due to the solvent in the vapor deposition film. For this reason, it is presumed that the vapor deposition film has a high density and has high abrasion resistance and alkali resistance compared to the antifouling film formed by the coating method.

[0111] The method for producing the optical laminate 10 of this embodiment includes an adhesion layer forming step of forming an adhesion layer 13, an optical functional layer forming step of forming an optical functional layer 14 by alternately laminating high refractive index layers 14a and low refractive index layers 14b, a second surface treatment step of treating the surface of the optical functional layer 14, and an antifouling layer forming step of forming an antifouling layer 15 on the surface-treated optical functional layer 14. Therefore, the adhesion between the optical functional layer 14 and the antifouling layer 15 formed on the optical functional layer 14 is good, and the abrasion resistance and alkali resistance are further improved.

[0112] In this embodiment, when the first surface treatment step, the optical functional layer formation step, the second surface treatment step, and the antifouling layer formation step are performed successively while maintaining the optical laminate in the middle of production under reduced pressure, the reduced pressure conditions in the chambers of, for example, the sputtering apparatus and the deposition apparatus may be different as long as they do not interfere with each production step.

[0113] In this embodiment, it is preferable to measure the film formation results over time using a measuring device in one or more of the adhesion layer formation process, the optical functional layer formation process, and the antifouling layer formation process, and feed back the results to the conditions of the subsequent manufacturing process. This makes it easier to optimize the characteristics of the entire optical laminate, and makes it possible to make the characteristics of the optical laminate uniform within the plane. In addition, the measuring device can also be used to feed back the manufacturing conditions in the same process. In this case, the layer formed in that process has uniform and stable characteristics.

[0114] In this embodiment, the second surface treatment step is performed between the optical functional layer forming step and the antifouling layer forming step, but the second surface treatment step may be performed as necessary, and may not be performed. Even if the second surface treatment step is not performed, it is preferable to perform the optical functional layer forming step and the antifouling layer forming step continuously under reduced pressure.

[0115] In the manufacturing method of the present embodiment, the optical functional layer is formed under conditions of a predetermined vacuum degree or less. Therefore, the optical functional layer 14 becomes dense, the water vapor transmission rate decreases, and the abrasion resistance and alkali resistance improve. Furthermore, the thickness of the antifouling layer is a predetermined thickness or more, so that sufficient scratch resistance and alkali resistance can be ensured.

[0116] In this embodiment, an example has been described in which the optical laminate 10 is continuously manufactured by a roll-to-roll method using a manufacturing apparatus 20 shown in FIG. 3, which is equipped with a pre-processing device 2A, a sputtering device 1, a pre-processing device 2B, a vapor deposition device 3, a roll unwinding device 4, and a roll winding device 5. However, the manufacturing apparatus for manufacturing the optical laminate 10 is not limited to the manufacturing apparatus 20 shown in FIG. 3. For example, a manufacturing apparatus may be used that does not include pretreatment apparatus 2A and pretreatment apparatus 2B, and that has roll unwinding apparatus 4, sputtering apparatus 1, vapor deposition apparatus 3, and roll winding apparatus 5 connected in this order.

[0117] The manufacturing apparatus 20 shown in FIG. 3 may be provided with a pretreatment chamber (not shown) between the chamber 33 of the vapor deposition apparatus 3 and the chamber 32 of the pretreatment apparatus 2B for cleaning the surface of the optical functional layer 14 on which the antifouling layer 15 is to be formed. The manufacturing apparatus 20 shown in FIG. 3 may be provided with a post-treatment chamber (not shown) between the chamber 33 of the vapor deposition apparatus 3 and the chamber 35 of the roll winding apparatus 5 for cooling and / or inspecting the transparent substrate 11 on which each layer up to the antifouling layer 15 has been formed.

[0118] 3, a hard coat layer forming device for forming a hard coat layer 12 on the surface of the transparent substrate 11 may be provided between the roll unwinding device 4 and the sputtering device 1. In this case, not only the optical functional layer 14 and the antifouling layer 15 but also the hard coat layer 12 can be continuously produced by the roll-to-roll method, which is preferable.

[0119] In this embodiment, an example has been described in which the optical functional layer formation process is performed using a sputtering device and the anti-fouling layer formation process is performed using a vapor deposition device. However, if the second surface treatment process is not performed, the optical functional layer formation process and the anti-fouling layer formation process may be performed in the same device (within one chamber).

[0120] In the optical laminate 10 of this embodiment, various layers may be provided as necessary on the surface of the transparent substrate opposite to the surface on which the optical functional layer or the like is formed. For example, a pressure-sensitive adhesive layer used for adhesion to other members may be provided. In addition, other optical films may be provided via this pressure-sensitive adhesive layer. Examples of other optical films include films that function as polarizing films, retardation compensation films, 1 / 2 wavelength plates, and 1 / 4 wavelength plates.

[0121] In addition, a layer having functions such as antireflection, selective reflection, antiglare, polarization, phase difference compensation, viewing angle compensation or expansion, light guiding, diffusion, brightness improvement, hue adjustment, and electrical conductivity may be formed directly on the opposing surface of the transparent substrate. The optical laminate may have a smooth shape, or may have a nano-order uneven structure that exhibits a moth-eye or anti-glare function. It may also have a geometric shape of micro to millimeter order such as a lens or prism. The shape can be formed by, for example, a combination of photolithography and etching, shape transfer, heat pressing, or the like. In this embodiment, since the film is formed by deposition or the like, even if the substrate has an uneven shape, the uneven shape can be maintained.

[0122] The article of the present embodiment is, for example, a liquid crystal display panel, an organic EL display panel, etc., in which the above-mentioned optical laminate 10 is provided on the display surface of an image display unit. This makes it possible to impart high abrasion resistance and alkali resistance to, for example, the touch panel display unit of a smartphone or an operating device, and to realize an image display device having excellent durability and suitable for practical use.

[0123] Furthermore, the article is not limited to image display devices, and may be any article to which the optical laminate 10 can be applied, such as window glass or goggles having the optical laminate of this embodiment provided on the surface, the light receiving surface of a solar cell, a smartphone screen or a display such as a notebook PC, information input terminals, tablet terminals, AR (augmented reality) devices, VR (virtual reality) devices, electronic display boards, glass table surfaces, gaming machines, operation support devices such as aircraft and trains, navigation systems, instrument panels, and the surface of optical sensors.

[0124] Although the embodiment of the present invention has been described above, this embodiment is presented as an example and is not intended to limit the scope of the invention. This embodiment can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the gist of the invention. These embodiments and their modifications are included in the scope of the invention and its equivalents described in the claims, as well as the scope and gist of the invention. For example, instead of the hard coat layer 12, an anti-glare layer may be formed, or an arbitrary functional layer such as a soft coat layer having flexibility may be added as necessary. These layers may be laminated. EXAMPLES

[0125] Examples of the present invention will be described below. Note that the optical laminates produced in the following examples and comparative examples are examples that function as anti-reflection films, and the gist of the present invention is not limited to these.

[0126] <Preparation of composition for hard coat layer> First, a photocurable composition 1 was prepared, in which the content of silica particles (filler) having an average particle size of 50 nm was 28 mass % relative to the total solid content of the composition. As shown in Table 1, composition 1 was prepared by dissolving acrylate (binder resin), silica particles, and a photopolymerization initiator in a solvent, and further adding a leveling agent.

[0127] [Table 1]

[0128] CN968: Hexafunctional aliphatic urethane acrylate having a polyester backbone SR610: Polyethylene glycol diacrylate, average molecular weight of the polyethylene glycol chain 600 PGM-AC-4130Y: Silica sol surface-modified with a methacryloyl group-containing silane compound, dispersion medium propylene glycol monomethyl ether Ominirad 184: 1-Hydroxy-cyclohexyl-phenyl-ketone

[0129] (Example 1) A 50-μm-thick PET film was used as the transparent substrate. After applying Composition 1 onto this PET film using a bar coater, Composition 1 was photopolymerized to form a 5-μm-thick hard coat layer on the transparent substrate.

[0130] Next, the surface of the hard coat layer was surface-treated by glow discharge treatment with an electrode power density of 5500 W / m 2 Subsequently, on the hard coat layer, using an Si target and an Nb target as sputtering targets and a mixed gas of Ar gas and O2 gas, an adhesion layer and an optical functional layer were continuously formed by reactive sputtering. That is, on the hard coat layer, an adhesion layer made of Si oxide (SiOx, 0 < x < 2) that may have oxygen deficiency with a thickness of 3 nm, a first high refractive index material layer made of Nb2O5 with a thickness of 10 nm, a first low refractive index material layer made of SiO2 with a thickness of 26 nm, a second high refractive index material layer made of Nb2O5 with a thickness of 110 nm, and a second low refractive index material layer made of SiO2 with a thickness of 85 nm were formed in this order.

[0131] Next, a 3 nm-thick antifouling layer made of an alkoxysilane compound having a perfluoropolyether group (KY1903-1, Shin-Etsu Chemical Co., Ltd.) was formed by deposition on the SiO2 film of the topmost layer of the optical functional layer at a pressure of 0.01 Pa in the deposition chamber, a deposition temperature of 230°C, and a retention time of 7.2 s to produce an optical laminate (anti-reflection film) of the example.

[0132] Example 2 The electrode power density during glow discharge treatment was 5500W / m 2 to 1100 W / m 2 An optical layered body was obtained in the same manner as in Example 1, except for changing the above.

[0133] Example 3 The electrode power density for glow discharge treatment is 5500W / m 2 to 6600 W / m 2 An optical layered body was obtained in the same manner as in Example 1, except for changing the above.

[0134] Example 4 An optical layered body was obtained in the same manner as in Example 1, except that the thickness of the hard coat layer formed on the transparent substrate was 2 μm.

[0135] Example 5 An optical layered body was obtained in the same manner as in Example 1, except that the composition for the hard coat layer was changed to Composition 2.

[0136] Example 6 An optical layered body was obtained in the same manner as in Example 1, except that the composition for the hard coat layer was changed to Composition 3.

[0137] Example 7 An optical laminate was obtained in the same manner as in Example 1, except that a 23 μm thick PET film was used as the transparent substrate instead of the 50 μm thick PET film.

[0138] Example 8 An optical layered body was obtained in the same manner as in Example 1, except that the thickness of the hard coat layer formed on the transparent substrate was 10 μm.

[0139] Example 9 The electrode power density during glow discharge treatment was 5500W / m 2 to 3300 W / m 2 An optical layered body was obtained in the same manner as in Example 8, except for changing the above.

[0140] Example 10 The electrode power density during glow discharge treatment was 5500W / m 2 to 1100 W / m 2 An optical layered body was obtained in the same manner as in Example 8, except for changing the above.

[0141] Example 11 The electrode power density during glow discharge treatment was 5500W / m 2 from 550 W / m 2 An optical layered body was obtained in the same manner as in Example 8, except for changing the above.

[0142] Comparative Example 1 The composition 1 for forming the hard coat layer was changed to the composition 4 shown in Table 1, and the electrode power density during the glow discharge treatment was 5000 W / m 2 An optical layered body was obtained in the same manner as in Example 1, except that the above-mentioned was changed.

[0143] Comparative Example 2 The thickness of the hard coat layer formed on the transparent substrate was set to 10 μm, and the electrode power density during glow discharge treatment was set to 5000 W / m 2 to 1100 W / m 2 An optical layered body was obtained in the same manner as in Comparative Example 1, except for changing the above.

[0144] Next, the optical layered bodies obtained in Examples 1 to 11 and Comparative Examples 1 and 2 were measured and evaluated by the following methods.

[0145] <Bending test> As a sample, an optical laminate was cut into a size of 1 cm x 15 cm. It was confirmed that the optical laminate had no cracks on the cut surface. A 5.0 mm mandrel was set in a bending tester capable of setting a mandrel. The optical laminate described above was set in this tester so that the surface on which the antifouling layer was formed was bent outward. The tester was then bent over 2 seconds to bend the optical laminate 180° and held for 10 seconds. The presence or absence of cracks in the antifouling layer was then confirmed visually and with an optical microscope. The above procedure was repeated, changing the mandrel diameter to a smaller one every 0.2 mm, until abnormalities such as cracks were found on the surface of the anti-fouling layer side of the optical laminate both visually and under an optical microscope, and the test result of the bending test was determined to be the mandrel diameter (φmm) that was 0.2 mm larger than the diameter of the mandrel where the first crack was found. Similarly, measurements were also taken when the optical laminate was set in the above-mentioned testing machine so that the surface on which the anti-fouling layer was formed was bent inward, and the mandrel diameter (φmm) that was 0.2 mm larger than the mandrel diameter at which the first crack was discovered was recorded as the test result of the bending test.

[0146] In addition, the theoretical elongation percentage S (%) of the optical functional layer was calculated when a mandrel with the smallest diameter at which no cracks were generated was used. The elongation percentage S was calculated as follows. S(%)={(R2 / R1)-1}×100 (where R2 is the distance from the axial center of the mandrel to the outer surface of the optical laminate, and R1 is the distance from the axial center of the mandrel to an imaginary line indicating a position corresponding to 1 / 2 of the total thickness of the optical laminate.)

[0147] In addition, when the surface on which the antifouling layer was formed was folded inward, the theoretical compression ratio C (%) of the optical functional layer was calculated using the mandrel with the smallest diameter at which no cracks occurred. The compression ratio C was calculated as follows. C(%)={1-(R3 / R1)}×100 (wherein R3 is the distance from the axial center of the mandrel to the surface of the antifouling layer side of the optical laminate, and R1 is the distance from the axial center of the mandrel to an imaginary line indicating a position corresponding to 1 / 2 of the total thickness of the optical laminate.)

[0148] Three samples were prepared for each measurement, and each value was calculated as the average of the three measurements. The smallest mandrel diameter was 1.0φmm, and 1.0φmm was used for measuring the elongation rate, but since no cracks were observed, the result of the bending test was less than 1.0φmm.

[0149] <Martens hardness> Compositions 1 to 4 were used to prepare laminates (samples) each having a hard coat layer formed on a transparent substrate. For the optical laminates obtained in Examples 1 to 11 and Comparative Examples 1 and 2, the Martens hardness of the antifouling layer side of the optical laminate was measured. For the laminates in which only the hard coat layer was formed, the Martens hardness of the hard coat layer side of the laminate was measured. For the measurement, a microcompression tester (Elionix, ENT-NEXUS, measuring indenter: Berkovich indenter) was used in accordance with ISO14577-1. For the optical laminates, the hardness was measured at an indentation depth of 50 nm, and for the laminates in which only the hard coat layer was formed, the hardness was measured when indented to a depth of 1 / 10 of the thickness of the hard coat layer. The Martens hardness of the optical laminate measured above was designated as (A), and the Martens hardness of the laminate in which only the hard coat layer was formed on the transparent substrate was designated as (B), and the ratio (A) / (B) was calculated. The results are shown in Table 2.

[0150] Moreover, the optical layered bodies obtained in Examples 1 to 11 and Comparative Examples 1 and 2 were measured and evaluated by the following methods.

[0151] <Contact angle measurement test for pure water> Measurements were performed using an automatic contact angle meter DM-700 (manufactured by Kyowa Interface Science Co., Ltd.) by the ellipse fitting method under the following conditions: Pure water was placed in a glass syringe, a stainless steel needle was attached to the tip, and the pure water was dropped onto the optical laminate (test piece). Amount of pure water dispensed: 2.0μL Measurement temperature: 25℃ Pure water was dropped onto the laminate (sample), and the contact angle after 4 seconds was measured at any 6 points on the surface of the test piece, and the average value was taken as the pure water contact angle.

[0152] <Steel wool sliding test> Using a friction tester type I conforming to JIS L0849, a friction body was caused to move back and forth horizontally along the surface of the optical laminate (test piece) to obtain a test piece. Steel wool (Bonstar Corporation #0000) was used as the friction material. The test settings were a load of 1000g / cm 2 The sliding distance was 50 mm, the sliding speed was 60 rpm (1 reciprocation / sec), and the number of sliding cycles was 200 (100 reciprocations). After sliding, the sample was subjected to a test similar to the above-mentioned contact angle measurement test for pure water, and the difference in contact angle before and after the test was determined. The results are shown in Table 3.

[0153] [Table 2]

[0154] [Table 3]

[0155] From the results of Table 2, in all of Examples 1 to 7, the ratio ((A) / (B)) of the Martens hardness (A) of the antifouling layer side of the optical laminate to the Martens hardness (B) of the hard coat layer side of the laminate having only a transparent substrate and a hard coat layer is 3.6 or less, so it was found that the bending resistance can be further improved while realizing excellent hardness. In particular, it was found that the silica particles contained in the hard coat layer are surface-modified with methacryloyl groups derived from a methacryloyl group-containing silane compound, and the methacryloyl groups are more firmly bonded to the acrylate (binder resin), and as a result, the hardness of the optical laminate is improved. Furthermore, it was found that the methacryloyl groups on the silica particle surface further improve the adhesion between the hard coat layer and the adhesive layer, and between the optical functional layer via the adhesive layer, and the bending resistance is further improved. Furthermore, in all of Examples 1 to 7, the difference in contact angle with water before and after rubbing, in which the steel wool was moved back and forth horizontally 200 times, was 20° or less. It is believed that the silica particles contained in the hard coat layer are surface-modified with methacryloyl groups derived from a methacryloyl group-containing silane compound, and the methacryloyl groups are more firmly bonded to the acrylate (binder resin). As a result, it was found that the hardness of the optical laminate was improved and excellent scratch resistance could be achieved.

[0156] Furthermore, from the results of Table 3, in all of Examples 8 to 11, similar to Examples 1 to 7, the difference in contact angle with water before and after rubbing in which steel wool was horizontally reciprocated 200 times was 20° or less, and it was found that the hardness of the optical laminate was improved and excellent scratch resistance could be realized. In addition, the ratio ((A) / (B)) of the Martens hardness (A) of the antifouling layer side of the optical laminate to the Martens hardness (B) of the hard coat layer side of the laminate having only the transparent substrate and the hard coat layer was 3.6 or less, and it was found that the bending resistance could be further improved while excellent hardness was realized.

[0157] On the other hand, in Comparative Example 1, when a hard coat layer was formed using composition 4 containing silica particles that had not been surface-modified, the ratio ((A) / (B)) was 3.71, and the hardness of the laminate was low. In addition, the elongation rate S (outer bending) was 1.22, and the compression rate C (inner bending) was 4.4, and the flex resistance was poor.

[0158] In Comparative Example 2, when a hard coat layer was formed using Composition 2 containing silica particles that had not been surface-modified, the contact angle difference was 23.6°, indicating a decrease in scratch resistance. In addition, the elongation rate S (outer bending) was 1.29, and the compression rate C (inner bending) was 3.63, indicating poor flex resistance. [Explanation of symbols]

[0159] 10, 102...Optical laminate 11...Transparent base material 12...Hard coat layer 13...Adhesion layer 14...Optical functional layer 14a...High refractive index layer 14b...Low refractive index layer 15...Anti-stain layer 20…Manufacturing equipment 1...Sputtering equipment 2A, 2B...Pretreatment equipment 3...Vapor deposition equipment 4…Roll unwinding device 5…Roll winding device 20…Manufacturing equipment 21…Vacuum pump 22...Guide roll 23…Unwinding roll 24…Winding roll 25...Deposition roll 26…Canroll 31, 32, 33, 34, 35…Chambers 41...Film forming section 42...Plasma discharge device 43...evaporation source 53...Heating device

Claims

1. An optical laminate having, in this order, a transparent substrate, a hard coat layer, an adhesion layer made of a sputtered film, a high refractive index layer made of a sputtered film, and an optical functional layer in which a low refractive index layer having a refractive index lower than that of the high refractive index layer is alternately laminated, and an antifouling layer, The hard coat layer contains a silica filler, An optical laminate satisfying the following conditions 1 and 2. Condition 1: The ratio ((A) / (B)) of the Martens hardness (A) measured from the antifouling layer side of the optical laminate to the Martens hardness (B) measured from the hard coat layer side of a laminate having only the entire transparent substrate and the hard coat layer is 3.6 or less. Condition 2: Using a friction tester using steel wool conforming to JIS L0849, the steel wool is horizontally reciprocated 200 times, and the difference in contact angle with water before and after friction is 20° or less.

2. The optical laminate according to claim 1 , wherein the silica filler is surface-modified with a functional group derived from a silane compound.

3. The optical laminate according to claim 2, wherein the silane compound is one or more selected from the group consisting of vinyl group-containing silane compounds, (meth)acryloyl group-containing silane compounds, amino group-containing silane compounds, isocyanate group-containing silane compounds, isocyanurate group-containing silane compounds, epoxy group-containing silane compounds and mercapto group-containing silane compounds.

4. The optical laminate according to claim 2 , wherein the silane compound is a (meth)acryloyl group-containing silane compound.

5. the hard coat layer contains a binder resin and a silica filler, The optical laminate according to claim 2 , wherein the functional group derived from the silane compound has the same functional group as the binder resin.

6. The binder resin contains a (meth)acrylate compound, The optical laminate according to claim 5 , wherein the functional group derived from the silane compound is a (meth)acryloyl group.

7. The optical laminate according to claim 1 , wherein the average particle size of the silica filler is 800 nm or less.

8. The optical laminate according to claim 1 , wherein the hard coat layer has a thickness of 0.5 μm or more and 100 μm or less.

9. 2. The optical laminate according to claim 1, wherein when the optical laminate is folded 180° so that the surface on which the antifouling layer is formed is on the outside, and a mandrel of the smallest diameter on which no cracks occur is used, the elongation S (%) of the optical functional layer calculated by the following formula (1) satisfies 1.3≦S. S(%)={(R2 / R1)-1}×100...(1) (wherein R2 is the distance from the axial center of the mandrel to the outer surface of the optical laminate, and R1 is the distance from the axial center of the mandrel to a virtual line indicating a position corresponding to 1 / 2 of the total thickness of the optical laminate.)

10. 10. The optical laminate according to claim 9, wherein when the optical laminate is folded 180° so that the surface on which the antifouling layer is formed is on the inside, a compression ratio C (%) of the optical functional layer calculated by the following formula (2) satisfies 4.5≦C when a mandrel of the smallest diameter at which no cracks occur is used. C (%) = {1-(R3 / R1)}×100...(2) (wherein R3 is the distance from the axial center of the mandrel to the surface of the antifouling layer side of the optical laminate, and R1 is the distance from the axial center of the mandrel to a virtual line indicating a position corresponding to 1 / 2 of the total thickness of the optical laminate.)

11. An article comprising the optical laminate according to any one of claims 1 to 10.

Citation Information

Patent Citations

  • Laminated thin film and manufacturing method therefor

    JP2016224443A

  • Antireflection film

    JP2019164255A

  • Photocurable hard coat composition for plastic substrates and hard coat film

    JP2019214670A

  • Hard coat resin and hard coat film

    JP2021134303A

  • Optical laminate body, object, and method for manufacturing optical laminate body

    JP2022007992A

Cited By

  • Optical laminate, article, and method for manufacturing optical laminate

    WO2026168317A1