Production method of positive electrode active material, positive electrode active material, and lithium-ion secondary battery
By introducing a water-soluble polymer into the precursor of positive electrode active materials, the method reduces particle size and enhances battery performance by lowering resistance and improving energy density in lithium ion secondary batteries.
Patent Information
- Application Number
- JP2024138453
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2041-09-02
AI Technical Summary
Existing lithium ion secondary batteries face challenges in reducing battery resistance due to the large particle size of positive electrode active materials, which hinders optimal performance.
A method is developed to produce a positive electrode active material by introducing a water-soluble polymer into the interior of secondary particles during the precursor preparation, followed by firing and crushing, resulting in a composite oxide with a smaller particle size and reduced resistance.
The method achieves a positive electrode active material with a predetermined particle size, leading to lithium ion secondary batteries with lower resistance and improved energy density.
Smart Images

Figure 2024159833000001_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a method for manufacturing a positive electrode active material, a positive electrode active material, and a lithium ion secondary battery.
Background Art
[0002] In recent years, with the rapid spread of electronic devices such as personal computers and mobile phones, the development of batteries used as their power sources has been underway. Also, in the automotive industry, the development of batteries used in hybrid vehicles (HEV), plug-in hybrid vehicles (PHEV), or battery electric vehicles (BEV) has been underway. Among various batteries, lithium ion secondary batteries have the advantage of high energy density.
[0003] A lithium ion secondary battery generally has a positive electrode layer, a negative electrode layer, and an electrolyte layer disposed between the positive electrode layer and the negative electrode layer. As the positive electrode active material used in the positive electrode layer, composite oxides containing Li are known. For example, Patent Document 1 discloses a method for manufacturing a positive electrode active material for a lithium ion secondary battery including a lithium nickel composite oxide. Also, Patent Document 1 discloses improving the crushability of a fired body using organic compound particles.
[0004] Patent Document 2 discloses a positive electrode active material for a non-aqueous secondary battery composed of composite oxide particles represented by the general formula LiNi a Co b Mn c O2 (a + b + c = 1, 0 < a < 1, 0 < b < 1, 0 < c < 1). Also, Patent Document 3 discloses a precursor of a positive electrode active material for a lithium ion secondary battery. Also, Patent Document 4 discloses a positive electrode active material for a lithium ion secondary battery composed of secondary particles in which primary particles are aggregated. Also, Patent Document 5 discloses a positive electrode active material for a non-aqueous electrolyte secondary battery obtained by firing a nickel composite hydroxide with a lithium compound.
Prior Art Documents
Patent Documents
[0005] [Patent Document 1] JP 2020-113429 A [Patent Document 2] JP 2016-081800 A [Patent Document 3] JP 2020-177860 A [Patent Document 4] Patent Publication No. 2021-048071 [Patent Document 5] Patent Publication No. 2021-024764 Summary of the Invention [Problem to be solved by the invention]
[0006] In order to reduce the battery resistance, it is desirable to reduce the particle size of the positive electrode active material. The present disclosure has been made in view of the above-mentioned circumstances, and has as its main object to provide a method for producing a positive electrode active material capable of obtaining a positive electrode active material having a small particle size. [Means for solving the problem]
[0007] The present disclosure provides a method for producing a positive electrode active material containing a complex oxide, the method comprising: a preparation step of preparing a precursor containing Li and Me (Me is at least one of Ni, Co, Mn, Al, and Fe); and a calcination step of calcining the precursor to obtain the complex oxide, in which a water-soluble polymer is introduced into the interior of secondary particles constituting the precursor using a polymer-containing aqueous solution in which a water-soluble polymer is dissolved in the preparation step.
[0008] According to the present disclosure, by using a precursor in which a water-soluble polymer is introduced inside secondary particles, a positive electrode active material with a small particle size can be obtained.
[0009] In the above disclosure, the precursor may be a mixture having an Me compound containing the Me and a Li compound containing the Li, and at least one of the Me compound and the Li compound may be the secondary particles.
[0010] In the above disclosure, the preparation step includes a raw material solution preparation process in which a Me raw material containing Me is dissolved in a solvent to prepare a raw material solution, a precipitate preparation process in which a Me compound containing Me is prepared as a precipitate from the raw material solution, a washing process in which the Me compound is washed, and a mixing process in which the washed Me compound is mixed with the Li compound, and the water-soluble polymer may be introduced into the interior of the secondary particles using the polymer-containing aqueous solution in at least one of the raw material solution preparation process, the precipitate preparation process, the washing process, and the mixing process.
[0011] In the above disclosure, in the washing treatment, the Me compound may be washed away using the polymer-containing aqueous solution, thereby introducing the water-soluble polymer into the interior of the secondary particles.
[0012] In the above disclosure, the water-soluble polymer may include at least one of a cellulose derivative, a (meth)acrylic polymer, and a polyvinyl alcohol polymer.
[0013] In the above disclosure, the water-soluble polymer may include carboxymethylcellulose, and the concentration of the carboxymethylcellulose in the polymer-containing aqueous solution may be 0.5% by weight or more and 2.0% by weight or less.
[0014] In the above disclosure, the method for producing the positive electrode active material may include a crushing step of crushing the composite oxide after the firing step.
[0015] The present disclosure also provides a positive electrode active material containing a composite oxide, the composite oxide containing Li and Me (Me is at least one of Ni, Co, Mn, Al, and Fe), and a particle diameter of 10% cumulative from the fine particle side in a cumulative particle size distribution based on volume in the composite oxide is D 10 The cumulative 50% particle size is D 50 The cumulative 90% particle diameter is D 90 In this case, D 50 is 0.3 μm or more and 1.2 μm or less, (D 90 -D 10 ) / D 50 is 0.9 or more and 1.7 or less, and the residual Na concentration in the composite oxide is 0.010% by weight or more and 0.134% by weight or less.
[0016] According to the present disclosure, by having a predetermined particle size, a positive electrode active material can be obtained that makes it possible to obtain a battery with low resistance.
[0017] The present disclosure also provides a lithium ion secondary battery having a positive electrode layer, a negative electrode layer, and an electrolyte layer disposed between the positive electrode layer and the negative electrode layer, wherein the positive electrode layer contains the above-mentioned positive electrode active material.
[0018] According to the present disclosure, by using a specific positive electrode active material, a lithium ion secondary battery with low resistance can be obtained. Effect of the Invention
[0019] The method for producing a positive electrode active material according to the present disclosure has the effect of being able to obtain a positive electrode active material having a small particle size. [Brief description of the drawings]
[0020] [Figure 1] 1 is a flowchart illustrating a method for producing a positive electrode active material in the present disclosure. [Diagram 2] FIG. 2 is a schematic side view illustrating the firing step in the present disclosure. [Diagram 3]1 is a flowchart illustrating a preparation process according to the present disclosure. [Figure 4] FIG. 1 is a schematic cross-sectional view illustrating a lithium-ion secondary battery according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0021] The method for producing a positive electrode active material, the positive electrode active material, and the lithium ion secondary battery according to the present disclosure will be described in detail below.
[0022] A. Method for manufacturing positive electrode active material Fig. 1 is a flow chart illustrating a method for producing a positive electrode active material according to the present disclosure. In Fig. 1, first, a precursor containing Li and Me (Me is at least one of Ni, Co, Mn, Al, and Fe) is prepared (preparation step). In the preparation step, a water-soluble polymer is introduced into the interior of secondary particles constituting the precursor using a polymer-containing aqueous solution in which the water-soluble polymer is dissolved. Next, the precursor is fired to obtain a composite oxide (firing step). Next, the fired composite oxide is crushed (crushing step). This results in the positive electrode active material.
[0023] According to the present disclosure, a positive electrode active material having a small particle size can be obtained by using a precursor in which a water-soluble polymer is introduced inside the secondary particles. In addition, by using a positive electrode active material having a small particle size, the battery resistance is reduced. FIG. 2 is a schematic side view illustrating a firing process in the present disclosure. As shown in FIG. 2, the precursor before firing has secondary particles, and a water-soluble polymer (e.g., carboxymethyl cellulose, CMC) is introduced inside the secondary particles. During firing, the CMC decomposes, causing the structure of the secondary particles to collapse. As a result, a positive electrode active material (composite oxide) having a small particle size is obtained. Note that in FIG. 2, the cross section of the primary particles is expressed as a rectangle for convenience, but is not limited to a rectangle and includes other shapes such as a circle. The shape of the primary particles may be, for example, a rod shape or a sphere.
[0024] As described above, Patent Document 1 discloses that organic compound particles are used to improve the crushability of the fired body. However, the organic compound particles, which are solid, cannot penetrate into the interior of the secondary particles. Therefore, the structure of the secondary particles is not destroyed and is maintained. In particular,
[0089] of Patent Document 1 clearly states that the secondary particles themselves are not destroyed. In contrast, in the present disclosure, a water-soluble polymer is actively introduced into the interior of the secondary particles, thereby destroying the structure of the secondary particles during firing. This results in a positive electrode active material with a small particle size.
[0025] 1. Preparation process The preparation step in the present disclosure is a step of preparing a precursor containing Li and Me (Me is at least one of Ni, Co, Mn, Al, and Fe). In addition, in the preparation step, a water-soluble polymer is introduced into the interior of the secondary particles constituting the precursor using a polymer-containing aqueous solution in which the water-soluble polymer is dissolved. That is, the water-soluble polymer is introduced into the interior of the secondary particles constituting the precursor.
[0026] In the present disclosure, "secondary particles constituting the precursor" refers to secondary particles corresponding to at least one compound among one or more compounds constituting the entire precursor. Also, "secondary particles" refers to particles formed by agglomeration of primary particles. Also, "inside of secondary particles" refers to voids existing between the agglomerated primary particles.
[0027] The precursor may also be a mixture containing an Me compound containing Me and an Li compound containing Li. In this case, it is preferable that at least one of the Me compound and the Li compound is a secondary particle. A water-soluble polymer may be introduced into the inside of the Me compound that is a secondary particle. A water-soluble polymer may also be introduced into the inside of the Li compound that is a secondary particle.
[0028] The Me compound is not particularly limited as long as it contains Me and can synthesize a desired composite oxide by firing. Examples of the Me compound include hydroxides containing Me and oxides containing Me. The precursor may contain only one type of Me compound, or may contain two or more types of Me compounds. For example, when the precursor contains Ni, Co, and Mn as Me, an example of one type of Me compound is a single compound containing Ni, Co, and Mn. On the other hand, an example of two or more types of Me compounds is a mixture of a Ni compound, a Co compound, and a Mn compound.
[0029] The Li compound is not particularly limited as long as it contains Li and can be used to synthesize a desired composite oxide by firing. Examples of Li compounds include lithium carbonate, lithium hydroxide, lithium nitrate, and lithium acetate.
[0030] In the preparation step, the water-soluble polymer is introduced into the inside of the secondary particles constituting the precursor using a polymer-containing aqueous solution in which the water-soluble polymer is dissolved. The polymer-containing aqueous solution contains a water-soluble polymer and water. Examples of the water-soluble polymer include cellulose derivatives such as carboxymethyl cellulose; (meth)acrylic polymers such as polyacrylic acid and polymethacrylic acid; and polyvinyl alcohol polymers such as polyvinyl alcohol and polyvinyl alcohol derivatives. The decomposition temperature of the water-soluble polymer is, for example, 600° C. or less, and may be 500° C. or less. On the other hand, the decomposition temperature of the water-soluble polymer is, for example, 120° C. or more, and may be 200° C. or more. The decomposition temperature of the water-soluble polymer refers to the temperature at which the water-soluble polymer is thermally decomposed. The weight-average molecular weight of the water-soluble polymer is, for example, 1000 or more, and may be 10,000 or more.
[0031] The concentration of the water-soluble polymer in the polymer-containing aqueous solution is not particularly limited, but is, for example, 0.1% by weight or more and 5% by weight or less. When the polymer-containing aqueous solution contains carboxymethylcellulose as the water-soluble polymer, the concentration of carboxymethylcellulose in the polymer-containing aqueous solution is, for example, 0.5% by weight or more. The concentration is, for example, 2.0% by weight or less, and may be 1.5% by weight or less. The viscosity of the polymer-containing aqueous solution is, for example, 100 Pa·s or less, and preferably 80 Pa·s or less.
[0032] The method of introducing a water-soluble polymer into the inside of the secondary particles constituting the precursor using a polymer-containing aqueous solution is not particularly limited. For example, a method of contacting the polymer-containing aqueous solution with the secondary particles constituting the precursor, penetrating the polymer-containing aqueous solution into the inside of the secondary particles constituting the precursor, and then drying the solution to remove the moisture contained in the polymer-containing aqueous solution can be mentioned. In addition, the timing of introducing the water-soluble polymer is not particularly limited. For example, after mixing the Me compound and the Li compound, the polymer-containing aqueous solution can be added, and then the mixture can be dried to introduce the water-soluble polymer into the mixture. In addition, before mixing the Me compound and the Li compound, the water-soluble polymer can be introduced into at least one of the Me compound and the Li compound. In addition, the water-soluble polymer can be introduced during the preparation of the Me compound.
[0033] FIG. 3 is a flow chart illustrating a preparation process in the present disclosure. In FIG. 3, first, a Me raw material containing Me is dissolved in a solvent to prepare a raw material solution (raw material solution preparation process). For example, an inorganic salt containing Ni, an inorganic salt containing Co, and an inorganic salt containing Mn are dissolved in water to obtain a raw material solution. Next, a Me compound is prepared as a precipitate from the raw material solution (precipitate preparation process). For example, the raw material solution is neutralized to obtain a precipitate of the Me compound. Next, the Me compound is filtered and washed (washing process). Next, the washed Me compound is mixed with a Li compound (mixing process). This results in a precursor being obtained.
[0034] In the raw solution preparation process, a Me raw material containing Me is dissolved in a solvent to prepare a raw solution. Examples of the Me raw material include salts containing Me. Examples of such salts include sulfates, nitrates, and chlorides. Examples of the solvent include water. In the present disclosure, a water-soluble polymer may be introduced in the raw solution preparation process. For example, when dissolving the Me raw material in a solvent, a water-soluble polymer may be added at the same time, or a polymer-containing aqueous solution in which a water-soluble polymer is dissolved may be added.
[0035] In the precipitate preparation process, a Me compound containing Me is prepared as a precipitate from the raw solution. The method for obtaining a precipitate of the Me compound is not particularly limited, and a general crystallization method can be used. Examples of the crystallization method include neutralization and concentration. For example, when the raw solution is acidic, an alkaline solution is added to obtain the Me compound. Examples of the alkaline solution include a sodium hydroxide aqueous solution, a calcium hydroxide aqueous solution, and a potassium hydroxide solution. The Me compound is preferably a hydroxide. On the other hand, when the raw solution is alkaline, an acidic solution is added to obtain the Me compound. A complexing agent may be added to the raw solution. Examples of the complexing agent include an ammonia aqueous solution. In the present disclosure, a water-soluble polymer may be introduced in the precipitate preparation process. For example, a water-soluble polymer may be added before or after neutralizing the raw solution, or a polymer-containing aqueous solution in which a water-soluble polymer is dissolved may be added simultaneously when neutralizing the raw solution.
[0036] In the cleaning process, the Me compound is cleaned using a cleaning solution. The cleaning solution may be, for example, water. In the present disclosure, a water-soluble polymer may be introduced in the cleaning process. For example, a polymer-containing aqueous solution in which a water-soluble polymer is dissolved may be used as the cleaning solution.
[0037] In the mixing process, the washed Me compound and the Li compound are mixed. The Li compound is as described above. In the present disclosure, a water-soluble polymer may be introduced in the mixing process. For example, when the Me compound and the Li compound are mixed, a polymer-containing aqueous solution in which a water-soluble polymer is dissolved may be added.
[0038] The shape of the precursor is not particularly limited, and may be a powder or a molded body.
[0039] 2. Firing process The calcination step in the present disclosure is a step of calcining the precursor to obtain the composite oxide. The calcination temperature in the calcination step is not particularly limited as long as the desired composite oxide can be obtained. The calcination temperature is preferably a temperature equal to or higher than the decomposition temperature of the water-soluble polymer. The calcination temperature is, for example, 500°C or higher, may be 700°C or higher, or may be 900°C or higher. On the other hand, the calcination temperature is, for example, 1500°C or lower. The calcination time is, for example, 1 hour or more, and may be 5 hours or more. On the other hand, the calcination time is, for example, 30 hours or less.
[0040] The atmosphere during firing may be, for example, an oxygen-containing atmosphere. Examples of the oxygen-containing atmosphere include an atmospheric pressure atmosphere and an atmosphere in which oxygen gas is added to an inert gas. Examples of the firing method include a method using a furnace such as a muffle furnace.
[0041] 3.Crushing process The crushing step in the present disclosure is a step of crushing the composite oxide after the firing step. By carrying out the crushing step, the sintered necking between secondary particles is crushed. In the crushing step, the structure of the secondary particles themselves is usually not destroyed. As a method for crushing the composite oxide, for example, a method of applying mechanical energy can be mentioned, and a specific example is a jet mill. In addition, the crushing conditions are appropriately adjusted so as to obtain the positive electrode active material described later.
[0042] 4.Cathode active material The positive electrode active material in the present disclosure includes a composite oxide containing Li and Me (Me is at least one of Ni, Co, Mn, Al, and Fe).
[0043] The composite oxide may contain at least Ni as Me. Similarly, the composite oxide may contain at least Co as Me. Similarly, the composite oxide may contain at least Mn as Me. Also, the composite oxide may contain at least one of Ni, Co, and Mn as Me. Similarly, the composite oxide may contain at least one of Ni, Co, and Al as Me. Also, the composite oxide may contain at least one of Ni, Co, and Mn as Me. X Contains Me X A part of Me is at least one of Al and Fe. Y may be substituted with.
[0044] In the case of composite oxides, the particle size of the cumulative 10% from the fine particle side in the cumulative particle size distribution based on volume is D 10 The cumulative 50% particle size is D 50 The cumulative 90% particle diameter is D 90 Let us assume that. D 50 is, for example, 0.3 μm or more, may be 0.4 μm or more, or may be 0.5 μm or more. 50 If D is too small, the particles tend to aggregate. 50 is, for example, 1.2 μm or less, and may be 1.1 μm or less.
[0045] Also, (D 90 -D 10 ) / D 50 is an index showing the spread of the particle size distribution. (D 90 -D 10 ) / D 50 is, for example, 0.9 or more, and may be 1.0 or more. 90 -D 10 ) / D 50 is, for example, 1.7 or less, and may be 1.5 or less. (D 90 -D 10 ) / D50 When the thickness is within the predetermined range, the filling rate of the positive electrode active material in the positive electrode layer is improved.
[0046] It is preferable that the composite oxide has a high bulk density, because this improves the energy density per volume. The bulk density of the composite oxide is, for example, 1.8 g / cm 3 More than 2.1g / cm 3 The bulk density of the composite oxide may be, for example, 3.0 g / cm 3 Less than or equal to 2.5 g / cm 3 It may be the following.
[0047] The composite oxide may contain Na residues. For example, when a sodium salt of a polymer is used as the water-soluble polymer, Na residues are generated in the composite oxide after firing. The residual Na concentration in the composite oxide is, for example, 0.010% by weight or more, may be 0.020% by weight or more, or may be 0.030% by weight or more. On the other hand, the residual Na concentration in the composite oxide is, for example, 0.134% by weight or less, and may be 0.100% by weight or less.
[0048] The composite oxide in the present disclosure preferably has a crystalline phase. Examples of the crystalline phase include a layered rock salt type crystalline phase and a spinel type crystalline phase. In addition, the present disclosure can provide a positive electrode active material obtained by the above-mentioned method for producing a positive electrode active material.
[0049] B. Positive electrode active material The positive electrode active material according to the present disclosure is a positive electrode active material containing a composite oxide, the composite oxide containing Li and Me (Me is at least one of Ni, Co, Mn, Al, and Fe), and the composite oxide having a particle diameter of 10% cumulative from the fine particle side in a cumulative particle size distribution based on volume, which is D 10 The cumulative 50% particle size is D 50 The cumulative 90% particle diameter is D 90 In this case, D 50 is 0.3 or more and 1.2 or less, (D 90 -D 10 ) / D50 is 0.9 or more and 1.7 or less, and the residual Na concentration in the composite oxide is 0.01% by weight or more and 0.1% by weight or less.
[0050] According to the present disclosure, the positive electrode active material has a predetermined particle size, and thus it is possible to obtain a battery with low resistance. Details of the positive electrode active material in the present disclosure are the same as those described in "A. Positive electrode active material" above. The positive electrode active material in the present disclosure is used in a battery.
[0051] C. Lithium-ion secondary battery Fig. 4 is a schematic cross-sectional view illustrating a lithium ion secondary battery according to the present disclosure. The lithium ion secondary battery 10 shown in Fig. 4 includes a positive electrode layer 1, a negative electrode layer 2, an electrolyte layer 3 disposed between the positive electrode layer 1 and the negative electrode layer 20, a positive electrode current collector 4 that collects current from the positive electrode layer 1, and a negative electrode current collector 5 that collects current from the negative electrode layer 2. The positive electrode layer 1 contains the positive electrode active material described above in "B. Positive electrode active material".
[0052] According to the present disclosure, by using a specific positive electrode active material, a lithium ion secondary battery with low resistance can be obtained.
[0053] The positive electrode layer contains at least a positive electrode active material. The positive electrode active material is the same as that described in "B. Positive electrode active material". The positive electrode layer may contain at least one of an electrolyte, a conductive material, and a binder, as necessary. The electrolyte will be described in detail later. Examples of the conductive material include carbon materials. Examples of the carbon material include particulate carbon materials such as acetylene black (AB) and ketjen black (KB), and fibrous carbon materials such as carbon fibers, carbon nanotubes (CNT), and carbon nanofibers (CNF). Examples of the binder include fluorine-containing binders such as polyvinylidene fluoride (PVDF) and polytetrafluoroethylene (PTFE). The thickness of the positive electrode layer is, for example, 0.1 μm or more and 1000 μm or less.
[0054] The negative electrode layer contains at least a negative electrode active material. Examples of the negative electrode active material include Li-based active materials such as metallic lithium and lithium alloys; carbon-based active materials such as graphite and hard carbon; oxide-based active materials such as lithium titanate; and Si-based active materials such as simple Si, Si alloys, and silicon oxide. The negative electrode layer may contain at least one of an electrolyte, a conductive material, and a binder, as necessary. These materials are as described above. The thickness of the negative electrode layer is, for example, 0.1 μm or more and 1000 μm or less.
[0055] The electrolyte layer includes at least an electrolyte. Examples of the electrolyte include a liquid electrolyte (electrolytic solution), a gel electrolyte, and a solid electrolyte. The electrolyte includes, for example, a lithium salt and a solvent. Examples of the lithium salt include inorganic lithium salts such as LiPF6, LiBF4, LiClO4, and LiAsF6; and organic lithium salts such as LiCF3SO3, LiN(SO2CF3)2, LiN(SO2C2F5)2, and LiC(SO2CF3)3. Examples of the solvent include ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC).
[0056] The gel electrolyte is usually obtained by adding a polymer to an electrolytic solution. Examples of the polymer include polyethylene oxide and polypropylene oxide. Examples of the solid electrolyte include organic solid electrolytes such as polymer electrolytes; and inorganic solid electrolytes such as sulfide solid electrolytes and oxide solid electrolytes. The thickness of the electrolyte layer is, for example, 0.1 μm or more and 1000 μm or less. The electrolyte layer may have a separator.
[0057] Examples of applications of the lithium ion secondary battery in the present disclosure include power sources for vehicles such as hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), electric vehicle (BEVs), gasoline-powered automobiles, diesel-powered automobiles, etc. The lithium ion secondary battery in the present disclosure may also be used as a power source for moving objects other than vehicles (for example, railways, ships, and aircraft), and may also be used as a power source for electrical appliances such as information processing devices.
[0058] The present disclosure is not limited to the above-described embodiment. The above-described embodiment is merely an example, and any configuration that is substantially the same as the technical idea described in the claims of the present disclosure and that exhibits similar effects is included in the technical scope of the present disclosure. EXAMPLES
[0059] [Example 1] NiSO4, CoSO4, and MnSO4 were prepared as Me raw materials and dissolved in ion-exchanged water to prepare a raw material solution (concentration: 30% by weight). The molar ratio of Ni, Co, and Mn in the raw material solution was Ni:Co:Mn=1:1:1.
[0060] Next, a certain amount of NH3 aqueous solution (complexing agent) was placed in the reaction vessel, and the atmosphere was replaced with nitrogen while stirring with a stirrer. NaOH was added to the reaction vessel to adjust the pH to alkaline. While controlling the pH inside the reaction vessel at a constant level with NaOH, the raw material solution and NH3 aqueous solution were dropped to precipitate Me compounds (secondary particles of hydroxide).
[0061] Next, the solution containing the Me compound was filtered, and the residue (Me compound) remaining on the filter paper was washed with a polymer-containing aqueous solution in which carboxymethylcellulose sodium salt (CMC-Na) was dissolved at a concentration of 0.5 wt%. The solution was then dried at 120°C for 16 hours to evaporate the water. This introduced CMC into the interior of the Me compound.
[0062] Next, the Me compound with CMC introduced and the Li compound (Li2CO3) were mixed in a mortar. The resulting mixture was fired at 1000°C for 10 hours in a muffle furnace to obtain a composite oxide. The resulting composite oxide was crushed using a jet mill to obtain a positive electrode active material.
[0063] [Example 2] A positive electrode active material was obtained in the same manner as in Example 1, except that the CMC concentration in the polymer-containing aqueous solution was changed to 1.0% by weight.
[0064] [Example 3] A positive electrode active material was obtained in the same manner as in Example 1, except that the CMC concentration in the polymer-containing aqueous solution was changed to 1.5% by weight.
[0065] [Example 4] A positive electrode active material was obtained in the same manner as in Example 1, except that the CMC concentration in the polymer-containing aqueous solution was changed to 2.0% by weight.
[0066] [Comparative Example 1] A positive electrode active material was obtained in the same manner as in Example 1, except that the CMC concentration in the polymer-containing aqueous solution was changed to 0% by weight.
[0067] [evaluation] (Particle size distribution measurement) Particle size distribution measurement was carried out on the positive electrode active materials obtained in Examples 1 to 4 and Comparative Example 1. For the measurement, a laser diffraction / scattering type particle size distribution measurement device (MT3000, Microtrack Bell Corporation) was used to measure the particle diameter D 10 , cumulative 50% particle diameter D 50 , and cumulative 90% particle diameter D 90 The results are shown in Table 1.
[0068] (bulk density measurement) Bulk density measurements were performed on the positive electrode active materials obtained in Examples 1 to 4 and Comparative Example 1. For the measurements, a powder property evaluation device (Powder Tester PT-X, Hosokawa Micron Corporation) was used, with a tap stroke of 3 mm, 200 taps, and a speed of 100 taps / min. The results are shown in Table 1.
[0069] (Residual Na measurement) The amount of residual Na was measured for the positive electrode active materials obtained in Examples 1 to 4 and Comparative Example 1. For the measurement, an ICP emission spectrometer (ICPE-9800, Shimadzu Corporation) was used. The results are shown in Table 1.
[0070] (Initial resistance measurement) Batteries were produced using the positive electrode active materials obtained in Examples 1 to 4 and Comparative Example 1, and the initial resistance of the batteries was measured. The method of producing the batteries is as follows. First, the obtained positive electrode active material, a conductive material (acetylene black), and a binder (polyvinylidene fluoride) were weighed in a weight ratio of positive electrode active material:conductive material:binder=88:10:2, and mixed. A dispersion medium was added to the obtained mixture, and the mixture was stirred to obtain a positive electrode slurry. The obtained positive electrode slurry was applied onto a positive electrode current collector using a film applicator (with a film thickness adjustment function, All Good Co., Ltd.), and then dried at 80°C for 5 minutes. As a result, a positive electrode structure having a positive electrode current collector and a positive electrode layer was obtained.
[0071] Next, the negative electrode active material (natural graphite) and the binder (SBR and CMC) were mixed, and a dispersion medium was added to the obtained mixture and stirred to obtain a negative electrode slurry. The obtained negative electrode slurry was applied onto a negative electrode current collector using a film applicator, and then dried at 80°C for 5 minutes. This resulted in a negative electrode structure having a negative electrode current collector and a negative electrode layer.
[0072] The positive electrode layer of the positive electrode structure and the negative electrode layer of the negative electrode structure were placed opposite each other with a separator interposed between them, wound, and an electrolyte was injected to obtain a battery. The electrolyte used was a mixed solvent containing EC, DMC, and EMC in a volume ratio of EC:DMC:EMC=3:4:3, with LiPF6 dissolved to a concentration of 1M.
[0073] The obtained battery was charged to 4.1 V and then discharged to 3.0 V. It was then charged to 3.7 V and left to stand at 60° C. for 9 hours. Thereafter, the charging resistance at 3.7 V and 1 C for 10 seconds was measured at −10° C. and taken as the initial resistance. The results are shown in Table 1. The initial resistance was calculated as a relative value when Comparative Example 1 was taken as 100%.
[0074] (Dispersibility of active material) Positive electrode layers were prepared in the same manner as above using the positive electrode active materials obtained in Examples 1 to 4 and Comparative Example 1. The cross sections of the obtained positive electrode layers were observed with a scanning electron microscope (SEM) to evaluate the dispersibility of the positive electrode active materials in the positive electrode layers. The dispersibility of the positive electrode active materials was calculated according to the following formula using images (1 μm×1 μm) obtained by dividing a cross-sectional image (1000 times, 20 μm×100 μm) of the positive electrode layer into 20 parts.
[0075]
number
[0076] In the above formula, σ 2 is the dispersibility of the positive electrode active material, n is the number of divisions (n=20), and X i is the volume of the positive electrode active material in the i-th image, and X ave is the average of each volume of the positive electrode active material.
[0077] [Table 1]
[0078] As shown in Table 1, in Examples 1 to 4, the D of the positive electrode active material was higher than that in Comparative Example 1. 50In particular, in Examples 2 and 3, D 50 In addition, in Examples 1 to 4, compared with Comparative Example 1, (D 90 -D 10 ) / D 50 It was suggested that this contributes to improving the filling rate of the positive electrode active material in the positive electrode layer. 90 -D 10 ) / D 50 was significantly high. Moreover, it was confirmed that Examples 1 to 4 had a higher bulk density than Comparative Example 1, which contributed to an improvement in the energy density per volume. In particular, Examples 1 to 3 had a significantly high bulk density. Moreover, Na residues due to CMC-Na were confirmed in Examples 1 to 4. Moreover, in Example 3, the dispersibility of the positive electrode active material was significantly high. Moreover, Examples 1 to 4 had a lower initial resistance than Comparative Example 1, which confirmed an improvement in the battery performance. In particular, Examples 1 to 3 had a significantly lower initial resistance. [Explanation of symbols]
[0079] 1 ... Positive electrode layer 2 ... Negative electrode layer 3...electrolyte layer 4...Positive electrode current collector 5...Negative electrode current collector 10...Lithium-ion secondary battery
Claims
[Claim 1] A method for producing a positive electrode active material containing a composite oxide, comprising the steps of: A preparation step of preparing a precursor containing Li and Me (Me is at least one of Ni, Co, Mn, Al, and Fe); A calcination step of calcining the precursor to obtain the composite oxide, a water-soluble polymer is introduced into the interior of secondary particles constituting the precursor by using a polymer-containing aqueous solution in which a water-soluble polymer is dissolved in the preparation step.
Citation Information
Patent Citations
Electrode active material manufacturing method
JP2013089454A
Positive electrode active material for nonaqueous secondary battery and manufacturing method thereof, and secondary battery
JP2016081800A
Method for producing positive electrode active material for lithium ion secondary battery
JP2020047584A
Production method of positive electrode active material, positive electrode active material, and lithium-ion secondary battery
JP2023036133A
Manufacturing method of cathode active material for lithium ion secondary battery and molding
JP2020113429A