Multilayer film, optical element, optical member, and optical device
The multilayer film configuration with antistatic and hard layers addresses the issues of foreign matter adhesion and scratch resistance in optical elements, ensuring effective optical performance and durability.
Patent Information
- Application Number
- JP2023075796
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-01
- Publication Date
- 2024-11-14
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing optical elements, such as lenses, suffer from foreign matter adhesion due to charging and lack sufficient scratch resistance, leading to decreased optical properties.
A multilayer film configuration with alternately laminated low and high refractive index layers, an antistatic layer, an oxygen-free layer, and a hard layer, which enhances scratch resistance while suppressing charge accumulation.
The solution effectively prevents foreign matter adhesion and improves scratch resistance, maintaining optical performance and integrity.
Smart Images

Figure 2024160605000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a multilayer film, an optical element, an optical member, and an optical device. [Background technology]
[0002] Conventionally, optical elements (e.g., lenses) mounted on cameras and the like have a multilayer film formed by stacking a plurality of dielectric layers. Since the multilayer film is easily charged, foreign matter such as dust adheres to the optical element. Based on this, Patent Document 1 proposes forming an antistatic layer having electrical conductivity on the multilayer film to suppress charging by dissipating electric charge from the surface of the optical element, thereby preventing the adhesion of foreign matter to the surface of the optical element. Patent Document 1 also discloses a glass article in which MgF2 or SiO2 is formed directly on a transparent conductive layer (ITO film (Indium Tin Oxide)) without introducing oxygen so as not to impair the antistatic function of the ITO film even in a high-temperature environment. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 3581783 Summary of the Invention [Problem to be solved by the invention]
[0004] However, Patent Document 1 cannot completely prevent adhesion of foreign matter to optical elements due to charging, and therefore it is necessary to physically remove the foreign matter. Also, in Patent Document 1, the outermost layer of the glass article does not have sufficient scratch resistance, so the outermost layer of the glass article may be scratched when removing the foreign matter, which may deteriorate the optical properties of the glass article.
[0005] Therefore, an object of the present invention is to improve scratch resistance while suppressing adhesion of objects. [Means for solving the problem]
[0006] In order to achieve the object of the present invention, a multilayer film according to one embodiment of the present invention has the following configuration: That is, the multilayer film is laminated on a substrate, and is characterized in that it comprises, from the substrate side, an alternately laminated low refractive index layer, a high refractive index layer having a refractive index higher than that of the low refractive index layer, and a hard layer, and an oxygen-free layer is formed immediately above an antistatic layer having a surface resistivity lower than that of the low refractive index layer and the hard layer among the layers constituting the multilayer film. Effect of the Invention
[0007] According to the present invention, it is possible to improve scratch resistance while suppressing adhesion of objects. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a cross-sectional view of an optical element according to the present invention. [Diagram 2] FIG. 11 is a cross-sectional view of a modified example of the optical element according to the present invention. [Diagram 3] FIG. 11 is a cross-sectional view of a modified example of the optical element according to the present invention. [Figure 4] FIG. 11 is a cross-sectional view of a modified example of the optical element according to the present invention. [Diagram 5] FIG. 11 is a cross-sectional view of a modified example of the optical element according to the present invention. [Figure 6] 4 shows the reflectance characteristics of the optical element according to the first embodiment. [Figure 7] 6 shows reflectance characteristics of the optical element according to Example 2. [Figure 8] 11 shows the reflectance characteristics of the optical element according to Example 3. [Figure 9] 13 shows the reflectance characteristics of the optical element according to Example 4. [Figure 10] 13 shows reflectance characteristics of the optical element according to Example 5. [Figure 11] 13 shows the reflectance characteristics of the optical element according to Example 6. [Figure 12] 4 shows the reflectance characteristics of the optical element according to Comparative Example 1. [Figure 13] 1A and 1B are diagrams showing configurations of an optical element and a conductive member according to the present invention. [Figure 14]1A and 1B are diagrams showing configurations of an optical element and a conductive member according to the present invention. [Figure 15] An optical unit and an optical device according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, the embodiments will be described in detail with reference to the attached drawings. Note that the following embodiments do not limit the invention according to the claims. Although the embodiments describe a number of features, not all of these features are essential to the invention, and the features may be combined in any manner. Furthermore, in the attached drawings, the same reference numbers are used for the same or similar configurations, and duplicated descriptions are omitted.
[0010] Example 1 The multilayer film includes a laminate having a high refractive index layer and a low refractive index layer, an antistatic layer, an oxygen-free layer, and a hard layer. The oxygen-free layer is laminated on the antistatic layer.
[0011] FIG. 1 is a cross-sectional view of an optical element according to the present invention.
[0012] <Multilayer film> The optical element 1 includes a substrate 2 and a multilayer film 9. The multilayer film 9 includes a laminate 5, an antistatic layer 6, an oxygen-free layer 7, and a hard layer 8. The laminate 5 includes one or more high refractive index layers 3 and one or more low refractive index layers 4. The optical element 1 will be described below with reference to FIG. 1.
[0013] (Low refractive index layer and high refractive index layer) The high refractive index layer 3 and the low refractive index layer 4 are films made of at least one of, for example, MgF2, SiO2, Al2O3, MgO, HfO2, ZrO2, La2Ti2O7 (LaTiO3), Si3N4, Ta2O5, Nb2O5, TiO2, etc. The high refractive index layer 3 and the low refractive index layer 4 may be layers made of a combination of the above materials, for example, a layer made of SiO2 and Al2O3, or a layer made of ZrO2 and TiO2.
[0014] Here, the high refractive index layer 3 and the low refractive index layer 4 are determined by comparing the refractive indexes of adjacent layers in the laminate 5. For example, when two layers are adjacent to each other in the laminate 5, the layer with the relatively high refractive index is determined as the high refractive index layer 3, and the layer with the relatively low refractive index is determined as the low refractive index layer 4. Note that the laminate 5 may also include an intermediate refractive index layer having a refractive index n3 lower than the refractive index n1 of the high refractive index layer 3 and higher than the refractive index n2 of the low refractive index layer 4.
[0015] The high refractive index layer 3 and the low refractive index layer 4 may be thin films made of materials that generate stress in different directions. For example, when the low refractive index layer 4 is a thin film made of SiO2 having compressive stress, the high refractive index layer 3 is TiO2 having tensile stress. This allows the laminate 5 to have opposing stresses and a large refractive index difference. If the refractive index difference (the difference between n1 and n2) is large, the number of layers of the high refractive index layer 3 and the low refractive index layer 4 and the film thickness of the laminate 5 can be reduced to obtain the desired spectral characteristics. This contributes to suppressing cracks in the multilayer film 9 and improving the productivity of manufacturing the multilayer film 9.
[0016] The laminate 5 preferably has 2 to 16 layers, and more preferably has 3 to 14 layers. In particular, in order to provide the multilayer film 9 with an anti-reflection function against light from visible light to near infrared light, the laminate 5 preferably has 7 to 14 layers. If the laminate 5 has a small number of layers, the multilayer film 9 has less freedom in designing, and therefore the multilayer film 9 cannot be provided with a sufficient anti-reflection function.
[0017] Furthermore, when the material of the substrate 2 is a resin substrate, an increase in the number of layers of the laminate 5 effectively suppresses deterioration of the resin substrate. When the resin substrate is exposed to oxygen and water vapor under a thermal load, yellowing occurs in the resin substrate. However, when the number of layers of the laminate 5 is large, even if there is a defect in a layer constituting the laminate 5, oxygen, water vapor, and the like can be prevented from reaching the resin substrate as long as there is no defect in the same region of the laminate 5. This makes it possible to suppress deterioration of the resin substrate. On the other hand, when the number of layers of the laminate 5 is too large, cracks are more likely to occur in the multilayer film 9.
[0018] The thickness of the laminate 5 is preferably 100 nm or more and 600 nm or less, more preferably 200 nm or more and 500 nm or less. If the thickness of the laminate 5 is small, the optical interference effect is unlikely to occur in the multilayer film 9, and therefore, the multilayer film 9 cannot be provided with a sufficient low reflection function. On the other hand, if the thickness of the multilayer film 9 is large, cracks occur in the multilayer film 9.
[0019] The thickness of each of the layers (high refractive index layer 3 and low refractive index layer 4) forming the laminate 5 is 150 nm or less. Since the stress of a thick layer is large, cracks are generated in the thick layer, and peeling occurs between the thick layer and the adjacent layer.
[0020] (Antistatic layer) The antistatic layer 6 is a film that is transparent in the visible light wavelength range so as not to impair the optical function (e.g., low reflection function) of the optical element 1. The antistatic layer 6 is a film that is transparent in the target wavelength range so as to suppress light absorption and increase transmittance. For example, the average light absorptance of the antistatic layer 6 in the target wavelength range is 10% or less, preferably 2% or less. In order to provide the optical element 1 with a sufficient antistatic function, it is preferable to reduce the surface resistivity of the antistatic layer 6. The antistatic layer 6 is a thin film made of, for example, indium tin oxide (ITO), titanium dioxide with niobium added (TNO), SnO2, or a material obtained by adding a metal or metal oxide to SnO2.
[0021] The antistatic layer 6 may be used as a substitute for the high refractive index layer 3 of the laminate 5. Alternatively, the high refractive index layer 3 may be composed of the same composition as the antistatic layer, and may be, for example, a thin film made of TNO. In particular, when the high refractive index layer 3 is a film made of TNO, the refractive index n1 of the high refractive index layer 3 is high, so that the refractive index difference between the high refractive index layer 3 and the low refractive index layer 4 becomes large. Here, even when at least one of the high refractive index layers 3 of the laminate 5 is replaced with the antistatic layer 6, a sufficient antireflection function can be imparted to the multilayer film 9.
[0022] Furthermore, at least one of the high refractive index layers 3 of the laminate 5 may be replaced with the antistatic layer 6, or all of the high refractive index layers 3 may be replaced with the antistatic layer 6. By replacing at least one of the high refractive index layers 3 of the laminate 5 with the antistatic layer 6, the antistatic function can be more effectively imparted to the multilayer film 9.
[0023] The antistatic layer 6 is a thin film made of ITO and TNO from the viewpoint of making the multilayer film 9 have a low surface resistivity. In addition, by changing the amount of Nb added and the film forming conditions, the refractive index of TNO can be changed to 2.3 to 2.6. The refractive index of TNO is high, comparable to that of TiO2. The antistatic layer 6 having a high refractive index can increase the refractive index difference between the antistatic layer 6 and the low refractive index layer 4. In other words, the optical interference effect can be effectively utilized, and therefore the multilayer film 9 can be endowed with an optical function (for example, an antireflection function).
[0024] The surface resistivity of the optical element 1 including the antistatic layer 6 is preferably 1.0×10 11 Ω / □ or less, more preferably 1.0×10 9 The surface resistivity of the antistatic layer 6 alone is 1.0×10 9 Ω / □ or less, more preferably 1.0×10 7 In this embodiment, the surface resistivities of the optical element 1 and the antistatic layer 6 were measured using a Hi-Resta-UX (manufactured by Mitsubishi Chemical Analytech Co., Ltd.) under the condition of an applied voltage of 100V.
[0025] The ITO, TNO, and SnO2-based antistatic layers 6 become n-type semiconductors that form donor levels due to the addition of additives (doping) and deviation from the stoichiometric composition due to oxygen deficiency. In addition, the antistatic layer 6 with many oxygen deficiencies has high conductivity and low surface resistivity (good conductivity). In order to provide the optical element 1 with a stable antistatic function, it is necessary to perform a process to prevent the antistatic layer 6 from being oxidized after the antistatic layer 6 is laminated on the laminate 5. Specifically, it is necessary to form the oxygen-free layer 7 immediately after the antistatic layer 6 is formed, which can be formed without introducing oxygen and does not contain oxygen as a chemical composition.
[0026] "Deposition without oxygen introduction" means a deposition method that can form a film without intentionally introducing oxygen. However, for example, oxygen released as outgas (volatile gas) from a deposition chamber or deposition material and oxygen atoms contained in water vapor are not included in the above oxygen.
[0027] "Does not contain oxygen as a chemical composition" means that it does not contain oxygen unintentionally contained during film formation, oxygen adsorbed to the film after film formation, oxygen atoms contained in water vapor, etc. Here, "unintentional inclusion of oxygen" means that the atomic ratio of oxygen in the oxygen-free layer 7 is 10 at % or less, 5 at % or less, or 1 at %.
[0028] In order to minimize contact of oxygen with the antistatic layer 6, the antistatic layer 6 is deposited on the laminate 5 under vacuum conditions. Immediately after deposition of the antistatic layer 6, the oxygen-free layer 7 is deposited on the antistatic layer 6 under the same vacuum conditions as above.
[0029] (oxygen-free layer) The oxygen-free layer 7 is a film made of an inorganic material from the viewpoints of the manufacturing process and adhesion with the hard layer 8. Examples of inorganic materials include MgF2, Si3N4, AlN, and DLC (diamond-like carbon). The oxygen-free layer 7 may be a film made of an organic material.
[0030] (Hard layer) The hard layer 8 is a layer formed on the oxygen-free layer 7. The hard layer 8 is, for example, a film made of an inorganic material from the viewpoint of improving the hardness of the multilayer film 9. Examples of inorganic materials include silicon nitride and its compounds, aluminum nitride, and DLC (diamond-like carbon).
[0031] 2 is a cross-sectional view of a modified example of the optical element according to the present invention. As shown in FIG. 2, the oxygen-free layer 7 has hardness and may also function as the hard layer 8.
[0032] 2, the optical element 1 includes a substrate 2 and a multilayer film 9. The multilayer film 9 includes a laminate 5, an antistatic layer 6, and a hard layer 8. The laminate 5 includes a high refractive index layer 3 and a low refractive index layer 4. The multilayer film 9 in FIG. 2 does not include an oxygen-free layer 7, unlike the multilayer film 9 in FIG. 1.
[0033] That is, the hard layer 8 may be a film made of the same material as the constituent material of the oxygen-free layer 7. For example, the hard layer 8 may be a film made of silicon nitride, a silicon nitride compound not containing oxygen, aluminum nitride, DLC, or the like.
[0034] The hard layer 8 prevents the optical element 1 from being scratched when a foreign object comes into contact with the optical element 1 and when a foreign object attached to the optical element 1 is physically wiped off. The hard layer 8 has high hardness in order to effectively prevent the optical element 1 from being scratched. The hardness of the hard layer 8 is measured by a hardness H IT It is expressed as:
[0035] Hardness of hard layer 8 H IT When the physical thickness of the hard layer 8 is 100 to 500 nm, the hardness is 14 GPa or more.
[0036] The physical film thickness of the hard layer 8 must be thick to some extent so that the hard layer 8 has a predetermined hardness. In the light transmission band applied to the multilayer film 9, the light absorption in the hard layer 8 is preferably small. Therefore, the hard layer 8 may preferably be a film made of silicon nitride and its compounds, and aluminum nitride. Further, from the viewpoints of hardness and optical properties, the hard layer 8 may more preferably be a film made of silicon nitride and its compounds.
[0037] Silicon nitride compounds include, for example, silicon oxynitride (SiO x N y : 0 < x < 2, 0 < y < 1.33), and silicon nitride compounds (SiM a O b N c : a < 1, 0 ≤ b, 0 < c) containing metal elements M such as Al, Ta, Y, and Mg. Here, the metal element M is a silicon nitride compound containing Al from the viewpoint of imparting an antireflection function to the multilayer film 9.
[0038] When the hard layer 8 is a film made of a silicon nitride compound containing Al, the hardness and transparency of the hard layer 8 are high, and the refractive index is lower than that of films made of other silicon nitride compounds and silicon nitride, so that it has an effect of suppressing surface reflection of the optical element 1.
[0039] When imparting an antireflection function to the multilayer film 9, the "optical film thickness" of the oxygen-free layer 7 and the hard layer 8 combined is preferably about λ / 4. Here, λ represents the center wavelength of the wavelength region imparting an antireflection function to the multilayer film 9. For example, when imparting an antireflection function to the multilayer film 9 in the visible light region (light wavelength 400 - 700 nm), λ = 550 nm. On the other hand, when imparting an antireflection function to the multilayer film 9 in the visible to near-infrared light region (400 nm - 1000 nm), λ = 700 nm.
[0040] Also, the "about λ / 4" of the optical film thickness indicates a range of 0.7 - 1.3λ / 4. When improving the hardness of the multilayer film 9, the optical film thickness is preferably 0.5 - 2 times the film thickness of the laminate 5. Specifically, the optical film thickness is preferably 50 - 1200 nm, more preferably 100 - 1000 nm.
[0041] Here, FIG. 3 is a cross-sectional view of a modified example of the optical element according to the present invention.
[0042] 3, the optical element 1 includes a substrate 2 and a multilayer film 9. The multilayer film 9 includes a laminate 5, an antistatic layer 6, an oxygen-free layer 7, a hard layer 8, and a gas barrier layer 10. The laminate 5 includes a high refractive index layer 3 and a low refractive index layer 4. The multilayer film 9 in FIG. 3 has a configuration in which the gas barrier layer 10 is added to the multilayer film 9 in FIG. 1.
[0043] (Gas barrier layer) 3 is formed on the oxygen-free layer 7 in order to prevent water vapor and oxygen from penetrating into the antistatic layer 6. The gas barrier layer 10 may be any layer that has low light absorption in the transmission band of the multilayer film 9. For example, SiO x (1≦x<2) and the film may be made of Al2O3.
[0044] The gas barrier layer 10 is provided between the oxygen-free layer 7 and the hard layer 8. The thickness of the gas barrier layer 10 is 6 nm or more. On the other hand, if the thickness of the gas barrier layer 10 is 6 nm or less, the gas barrier function of the gas barrier layer 10 may be reduced. When the multilayer film 9 is to have an anti-reflection function, the optical thickness including the oxygen-free layer 7, the hard layer 8, and the gas barrier layer 10 is preferably about 0.7 to 1.3λ / 4, where λ is the central wavelength.
[0045] Next, FIG. 4 is a cross-sectional view of a modified example of the optical element according to the present invention.
[0046] In Fig. 4, the optical element 1 includes a substrate 2 and a multilayer film 9. The multilayer film 9 includes a laminate 5, an antistatic layer 6, an oxygen-free layer 7, a hard layer 8, and a lubricating layer 11. The laminate 5 includes a high refractive index layer 3 and a low refractive index layer 4. The multilayer film 9 in Fig. 4 has a configuration in which a lubricating layer 11 is added to the multilayer film 9 in Fig. 1.
[0047] (lubricating layer) The lubricating layer 11 is a film formed on the hard layer 8 and made of a material with a small coefficient of friction. The refractive index of the lubricating layer 11 is preferably small when providing an anti-reflection function to the multilayer film 9. Materials with a small friction coefficient include, for example, fluoroalkyl ethers, fluorine-containing organic silicon compounds, tetrafluoroethylene, and fluorine compounds such as amorphous fluorine resins typified by CYTOP (manufactured by Asahi Glass Co., Ltd.).
[0048] Here, it is known that fluoroalkyl ether and fluorine-containing organic silicon compounds react with Si-OH (silanol group) to form a strong film. When forming the lubricating layer 11 using the above-mentioned fluorine-containing compounds, it is preferable to form SiO2 as an adhesion layer before forming the lubricating layer 11. In this case, the thickness of the adhesion layer made of SiO2 may be about several nm.
[0049] The thickness of the lubricating layer 11 is preferably 4 to 1000 nm, more preferably 5 to 100 nm, from the viewpoint of imparting an anti-reflection function to the multilayer film 9. If the thickness of the lubricating layer 11 is less than the above thickness, the lubricating layer 11 cannot exhibit a sufficient lubricating function. On the other hand, if the thickness of the lubricating layer 11 is more than the above thickness, ripples occur in the spectral characteristics of the multilayer film 9. The method of forming the lubricating layer 11 is dry coating, which is relatively easy to control the thin film thickness, from the viewpoint of preventing ripples in the spectral characteristics. Dry coating includes, for example, a vapor deposition method.
[0050] When the lubricating layer 11 containing a fluorine-containing compound such as fluoroalkyl ether is formed by a vapor deposition method, the thickness of the lubricating layer 11 may be 4 to 20 nm. If the thickness of the lubricating layer 11 is less than the above thickness, the lubricating layer 11 having sufficient lubricating performance over a long period of time cannot be obtained. On the other hand, if the thickness of the lubricating layer 11 is more than the above thickness, light scattering is likely to occur in the lubricating layer 11.
[0051] Next, FIG. 5 is a cross-sectional view of a modified example of the optical element according to the present invention.
[0052] 5, the optical element 1 includes a substrate 2 and a multilayer film 9. The multilayer film 9 includes a laminate 5, an antistatic layer 6, an oxygen-free layer 7, a hard layer 8, and a conductive film 12. The laminate 5 includes a high refractive index layer 3 and a low refractive index layer 4. The multilayer film 9 in FIG. 5 has a configuration in which a conductive film 12 is added to the multilayer film 9 in FIG. 1.
[0053] (Conductive film) The conductive film 12 is a film provided between the substrate 2 and the laminate 5, and is, for example, an ITO film or a thin metal film. The conductive film 12 is a film for actively dissipating the electric charge accumulated in the optical element 1 from the optical element 1, and has good electrical conductivity. The surface resistivity of the conductive film 12 is, for example, 1.0×10 2 It is less than Ω / □.
[0054] In particular, the conductive film 12 may be an ITO film having high transparency in the visible light wavelength range so as not to impair the anti-reflection function of the multilayer film 9. The surface resistivity of the conductive film 12 is measured by Loresta GP (manufactured by Mitsubishi Chemical Analytech Co., Ltd.). Furthermore, by bringing the conductive film 12 into contact with a conductive member (not shown), electric charge can be discharged from the optical element 1.
[0055] In order not to impair the anti-reflection function of the multilayer film 9, the conductive film 12 is sandwiched between the substrate 2 and the multilayer film 9. Furthermore, it is preferable that the conductive film 12 is formed on the substrate 2 so that the bottom area of the conductive film 12 is larger than the bottom area of the multilayer film 9. The contact between the region where the conductive film 12 contacts the substrate 2 and the conductive member 13 makes it possible to effectively prevent charging of the optical element 1.
[0056] (substrate) The substrate 2 is a substrate that is transparent in a predetermined light wavelength region and is made of any material. Here, the predetermined light wavelength region refers to, for example, visible light wavelengths (400 to 700 nm). Transparency refers to a transmittance of 80% or more in the target wavelength region.
[0057] The substrate 2 may be a substrate made of, for example, inorganic materials such as glass and quartz, or various synthetic resins such as polyester, norbornene, polyether, acrylic, styrene, PET (polyethylene terephthalate), PES (polyethersulfone), polysulfone, PEN (polyethylene naphthalate), PC (polycarbonate), and polyimide.
[0058] The substrate 2 is required to have high heat resistance from the viewpoint of the environment in which the optical components are used. Therefore, the substrate 2 is a glass substrate from the viewpoint of ensuring high heat resistance. On the other hand, a synthetic resin substrate is flexible, light, and has good processability compared to a substrate made of an inorganic material such as glass. However, a synthetic resin substrate is prone to deformation due to thermal stress and changes in characteristics due to moisture. In addition, a synthetic resin substrate may have polarization characteristics depending on the manufacturing method.
[0059] For this reason, when a synthetic resin substrate is used as the substrate 2, high heat resistance (high glass transition temperature T g ), low water absorption, and low birefringence are preferably used. Synthetic resins that satisfy the above characteristics are norbornene-based, etc. Furthermore, the substrate 2 may be a substrate made of an organic-inorganic hybrid material, such as a substrate having a silsesquioxane skeleton, as required.
[0060] To improve rigidity and ease of handling, the thickness of the substrate 2 is preferably 0.1 to 30 mm, more preferably 0.4 to 20 mm. When the thickness of the substrate 2 is greater than or equal to the above and a synthetic resin substrate is used as the substrate 2, retardation due to birefringence may become large.
[0061] The substrate 2 may be a substrate that has light absorption properties in a specific wavelength range (for example, near-infrared range) due to dyes, pigments, metal ions, and the like.
[0062] The substrate 2 may be radiation-resistant glass. Examples of radiation-resistant glass include glass materials to which CeO2 (cerium oxide) or the like is added, such as glass materials manufactured by Ohara Corporation (S-BAL35R, S-BSL7R, S-BSM22R, PBM2R, and PBM8R) and glass materials manufactured by Sumita Optical Glass Co., Ltd. (NBSF1, NBLaK9, NBBK7, NBSK4, NBF2, and NBSK10).
[0063] The radiation-resistant substrate 2 includes synthetic quartz. Alternatively, a glass substrate having an absorption characteristic in the infrared region and having a radiation-resistant function, such as BS-12 (manufactured by Matsunami Glass Industry Co., Ltd.), may be used as the substrate 2.
[0064] <Method of manufacturing optical elements> The following describes a method for manufacturing the optical element 1. The optical element 1 is manufactured by depositing the laminate 5, the antistatic layer 6, the oxygen-free layer 7, and the hard layer 8 in this order on the substrate 2 using a vapor phase deposition method. Here, the method for manufacturing the optical element 1 using an ion plating method, which is one of the vapor phase deposition methods, will be described, but is not limited to this.
[0065] The manufacturing method of the optical element 1 may be various known methods, such as other PVD (Physical Vapor Deposition) methods such as ion-assisted method, vacuum deposition method, and sputtering method, CVD (Chemical Vapor Deposition) method, and ALD (Atomic Layer Deposition) method.
[0066] First, the substrate 2 is set in a deposition jig consisting of a deposition mask and a holder. An evaporation dome is attached so that the deposition surface of the substrate 2 faces the deposition source. When a resin substrate is used for the substrate 2, it is advisable to perform an annealing treatment in advance to remove residual stress during deposition and moisture adsorbed by the substrate 2.
[0067] (Deposition of high refractive index layer) Next, the deposition dome is inserted into the deposition chamber, and the deposition chamber is evacuated. The deposition chamber is evacuated to a desired vacuum level (e.g., 1.0×10-3 After the pressure reaches 1000 bar (Pa), the starting material of the high refractive index layer 3 filled in the crucible is heated by an electron beam, and the evaporated particles are deposited on the substrate 2. In this way, the high refractive index layer 3 is formed on the substrate 2.
[0068] At this time, the deposition particles are positively charged by passing through a plasma atmosphere generated by a high-frequency power supply between the evaporation source and the deposition dome. Meanwhile, a negative charge is applied to the deposition dome, and the deposition particles having a large kinetic energy reach the substrate 2. As a result, a dense film is formed on the substrate 2. The gases that form the plasma are Ar, O2, N2, etc. When an oxide film is formed on the substrate 2, the gases that form the plasma are Ar and O2.
[0069] Here, before forming the first layer on the substrate 2, an ion bombardment treatment is performed to remove dirt from the substrate 2 and to improve the surface activity. This can improve the adhesion between the substrate 2 and the first layer. When the first layer (high refractive index layer 3) formed on the substrate 2 reaches a predetermined film thickness, the heating of the starting material by the electron beam is stopped. By forming the high refractive index layer 3 on the substrate 2 as the first layer, the refractive index difference between the substrate 2 and the high refractive index layer 3 can be effectively utilized.
[0070] (Deposition of low refractive index layer) The low refractive index layer 4 is formed on the high refractive index layer 3 by the same film formation method as that for the high refractive index layer 3. After a predetermined number of high refractive index layers 3 and low refractive index layers 4 are alternately formed on the substrate 2, the process proceeds to the formation of the antistatic layer 6.
[0071] (Deposition of antistatic layer) The antistatic layer 6 is formed on the laminate 5 by the same film formation method as for the above-mentioned layers. However, since the antistatic function and optical properties of the antistatic layer 6 are easily affected by oxygen deficiency, it is necessary to adjust the oxygen mixture ratio in the gas for generating plasma.
[0072] (Deposition of oxygen-free layer) The oxygen-free layer 7 is deposited on the antistatic layer 6 by the same deposition method as the above layers. However, when the oxygen-free layer 7 is deposited by the ion plating method, O2 is not used as the gas for generating plasma. In other words, Ar and N2 gases can be used as the gas for generating plasma. The oxygen-free layer 7 may also be deposited without generating plasma. After the oxygen-free layer 7 is deposited, the process proceeds to depositing the hard layer 8.
[0073] (Deposition of hard layer) The hard layer 8 is formed on the antistatic layer 6, the oxygen-free layer 7, or the gas barrier layer 10 by the same film formation method as for the above layers. For example, the hard layer 8 may be made of SiAl a O b N c When depositing SiAl on any of the above layers, the plasma may be generated by a gas mixture of Ar, O2, and N2, for example. The ratio of oxygen and nitrogen in the deposition material is adjusted in advance, and SiAl a O b N c During the deposition of the hard layer 8, a plasma of Ar and O2 may be generated, or a plasma of Ar and N2 may be generated. The deposition conditions may be adjusted so that the composition of the finally obtained hard layer 8 is a predetermined composition.
[0074] (Gas barrier layer formation) When the multilayer film 9 includes the gas barrier layer 10, the gas barrier layer 10 is sandwiched between the oxygen-free layer 7 and the hard layer 8. The gas barrier layer 10 is deposited on the oxygen-free layer 7 by the same deposition method as for the above layers.
[0075] (Deposition of lubricant layer) When the multilayer film 9 includes the lubricating layer 11, the lubricating layer 11 is formed by a resistance heating method on the hard layer 8. As the lubricating layer 11, a fluorine-containing compound such as a fluoroalkyl ether can be used.
[0076] The fluorine-containing compound can be impregnated into a metal support such as steel wool and deposited by vapor deposition. In this case, when the fluorine-containing compound is heated as a deposition material by an electron beam, the chemical bond of the fluorine-containing compound is broken and decomposed. Therefore, it is preferable to form a film of the fluorine-containing compound by indirectly heating the fluorine-containing compound by resistance heating.
[0077] The adhesion between the lubricating layer 11 and the hard layer 8 can be improved by a SiO2 film. For example, after a SiO2 film of several nm to several tens of nm is formed on the hard layer 8, the lubricating layer 11 may be formed on the SiO2 film.
[0078] (Deposition of conductive film) When the optical element 1 includes a conductive film 12, the conductive film 12 can be formed on the substrate 2 by the same film formation method as for the above-mentioned layers before the laminate 5 is formed. It is preferable to use a film formation mask for the film formation tool that has a larger opening than the other layers so that the deposition area of the conductive film 12 is larger than that of the other layers. In other words, the conductive film 12 is formed in a separate process from the other layers. The laminate 5, the antistatic layer 6, the oxygen-free layer 7, and the hard layer 8 are formed on the substrate 2 on which the conductive film 12 has been formed in advance.
[0079] In addition, when the oxygen-free layer 7 is formed by a sputtering method (so-called metal mode sputtering) in which metal film formation and oxidation and nitridation are successively performed, "film formation without introducing oxygen" means that oxygen is not introduced into the gas used for the oxidation and nitridation processes in the metal mode sputtering.
[0080] After the formation of the antistatic layer 6 or the multilayer film 9, a process for lowering the surface resistivity may be added. Since the antistatic layer 6 is an n-type semiconductor, the electrical conductivity (i.e., antistatic performance) of the antistatic layer 6 can be improved by improving the crystallinity of the antistatic layer 6 or by causing oxygen deficiency. For example, after the formation of the antistatic layer 6 or the multilayer film 9, the crystallinity of the antistatic layer 6 can be improved by applying a heat load.
[0081] Furthermore, annealing in a H2 reducing atmosphere improves the electrical conductivity of the antistatic layer 6. Although the details of this mechanism are unclear, it is speculated that the electrical conductivity of the antistatic layer 6 is improved by promoting oxygen deficiency in the antistatic layer 6. Note that, since H2 is a very small gas molecule, it contributes to oxygen deficiency in the antistatic layer 6 by passing through the oxygen-free layer 7, the gas barrier layer 10, or the hard layer 8 formed on the antistatic layer 6, or a combination of these layers.
[0082] However, when a fluorine-containing compound is formed as the lubricating layer 11 on the hard layer 8, the fluorine-containing compound may be thermally decomposed by the heat load and annealing in an H2 reducing atmosphere for improving the crystallinity of the antistatic layer 6. Therefore, the lubricating layer 11 is formed on the hard layer 8 after the heat load treatment and H2 reducing treatment are performed.
[0083] The optical element 1 has a multilayer film 9 formed on one surface of the substrate 2, but may have a multilayer film 9 formed on each of both surfaces (upper and lower) of the substrate 2. Furthermore, the optical element 1 may have a multilayer film 9 that does not include the antistatic layer 6 and the hard layer 8, with or without an optical functional film that cuts infrared rays, ultraviolet rays, visible light, etc. as a general antireflection film function.
[0084] <Example 1> Table 1 shows the configuration of the optical element according to the first embodiment.
[0085] The optical element 1 is a laminate 5 in which a high refractive index layer 3 (TNO layer) and a low refractive index layer 4 (SiO2 layer) are alternately laminated on a radiation-resistant glass substrate 2 (S-BSL7R, manufactured by Ohara Corporation), an antistatic layer 6 (TNO layer), an oxygen-free layer 7 (MgF2 layer), a hard layer 8 (SiAl a O b N cIt has a multilayer film 9 on which a layer (a < 1, 0 < b, 0 < c) is formed. When TNO is used for both the high refractive index layer 3 and the antistatic layer 6 (when the compositions of the high refractive index layer 3 and the antistatic layer 6 are the same), due to the film formation conditions and variations, the surface resistivity of the high refractive index layer 3 (TNO layer) closest to the substrate 2 becomes smaller than the surface resistivity of the antistatic layer 6 (TNO layer). On the other hand, the surface resistivity of the high refractive index layer 3 (TNO layer) other than the high refractive index layer 3 (TNO layer) closest to the substrate 2 is higher than that of the antistatic layer 6 (TNO layer). In this specification, when the compositions of the high refractive index layer 3 and the antistatic layer 6 (for example, TNO) are the same as in Example 1, the magnitude relationship of the surface resistivity between the high refractive index layer 3 and the antistatic layer 6 described above can be applied. Also, when the compositions of the high refractive index layer 3 and the antistatic layer 6 are not the same, the surface resistivity of the antistatic layer 6 is smaller than the surface resistivity of the high refractive index layer 3.
[0086] The optical element 1 has a multilayer film 9 having an antireflection function for the visible to near-infrared region. With the center wavelength λ = 700 nm, the total optical film thickness of the oxygen-free layer 7 (MgF2 layer) and the hard layer 8 (SiAl a O b N c layer) is 0.726λ / 4.
[0087] Note that the refractive index of the hard layer 8 is 1.750 at λ = 700 nm. The film thickness of the hard layer 8 is 10 nm or more, for example, 20.7 nm, so that the hard layer 8 has scratch resistance.
[0088] Here, FIG. 6 shows the reflectance characteristics of the optical element according to Example 1. The horizontal axis in FIG. 6 is Wavelength (nm), and the vertical axis is Reflectance (%). The optical element 1 has the reflectance characteristics shown in FIG. 6.
[0089]
Table 1
[0090] <Example 2> Table 2 shows the configuration of the optical element according to Example 2.
[0091] The optical element 1 has a multilayer film 9 formed by alternately laminating a high refractive index layer 3 (TNO layer) and a low refractive index layer 4 (SiO2 layer) on a glass substrate 2 (S-BSL7R, manufactured by Ohara Corporation) having a radiation resistance function, an antistatic layer 6 (TNO layer), an oxygen-free layer 7 (MgF2 layer), and a hard layer 8 (SiAl a O b N c (a<1, 0<b, 0<c)). That is, the optical element 1 has a multilayer film 9 in which the high refractive index layer 3 and the antistatic layer 6 are made of TNO layers.
[0092] The optical element 1 has a multilayer film 9 having an antireflection function for the visible to near-infrared region. With the center wavelength λ = 700 nm, the total optical film thickness of the oxygen-free layer 7 (MgF2 layer) and the hard layer 8 (SiAl a O b N c layer) is 0.727λ / 4.
[0093] Note that the refractive index of the hard layer 8 is 1.750 at λ = 700 nm. The film thickness of the hard layer 8 is 10 nm or more, for example, 21.6 nm, so that the hard layer 8 has scratch resistance.
[0094] Here, FIG. 7 shows the reflectance characteristics of the optical element according to Example 2. The horizontal axis of FIG. 7 is Wavelength (nm), and the vertical axis is Reflectance (%). The optical element 1 has the reflectance characteristics shown in FIG. 7.
[0095] [Table 2]
[0096] <Example 3> Table 3 shows the configuration of the optical element according to Example 3.
[0097] The optical element 1 has a multilayer film 9 formed by depositing a stack 5 in which a high refractive index layer 3 (Si3N4 layer) and a low refractive index layer 4 (SiO2 layer) are alternately laminated, an antistatic layer 6 (TNO layer), and a hard layer 8 (Si3N4 layer) having the function of an oxygen-free layer 7 on a glass substrate 2 (BS-12, manufactured by Matsunami Glass Industry Co., Ltd.) having a radiation resistance function.
[0098] The physical film thickness of the hard layer 8 having the function of the oxygen-free layer 7 is 400 nm, which is about 1.74 times the physical film thickness of the stack 5.
[0099] Here, FIG. 8 shows the reflectance characteristics of the optical element according to Example 3. The horizontal axis in FIG. 8 is Wavelength (nm), and the vertical axis is Reflectance (%). The optical element 1 has the reflectance characteristics shown in FIG. 8.
[0100]
Table 3
[0101] <Example 4> Table 4 shows the configuration of the optical element according to Example 4.
[0102] The optical element 1 has a multilayer film 9 formed by depositing a stack 5 in which a high refractive index layer 3 (TiO2 layer) and a low refractive index layer 4 (SiO2 layer) are alternately laminated, an antistatic layer 6 (TNO layer), an oxygen-free layer 7 (MgF2 layer), a gas barrier layer 10 (Al2O3 layer), and a hard layer 8 (SiAl a O b N c layer (a<1, 0<b, 0<c)) on a resin substrate 2 (COP cycloolefin polymer, manufactured by Nippon Zeon Co., Ltd.) having a plate thickness of 100 μm.
[0103] Here, the film thickness of the gas barrier layer 10 is set to 8 nm so as not to affect the optical characteristics of the optical element 1.
[0104] The optical element 1 has a multilayer film 9 with an antireflection function for the visible light range. Assuming the center wavelength λ = 550 nm, the total optical film thickness of the oxygen-free layer 7, the gas barrier layer 10, and the hard layer 8 is 0.970λ / 4.
[0105] The refractive index of the hard layer 8 is 1.765 at λ = 550 nm. To ensure that the hard layer 8 has scratch resistance, the film thickness of the hard layer 8 is 10 nm or more, for example, 11 nm.
[0106] Here, FIG. 9 shows the reflectance characteristics of the optical element according to Example 4. The horizontal axis in FIG. 9 is Wavelength (nm), and the vertical axis is Reflectance (%). The optical element 1 has the reflectance characteristics shown in FIG. 9.
[0107]
Table 4
[0108] <Example 5> Table 5 shows the configuration of the optical element according to Example 5.
[0109] The optical element 1 has a multilayer film 9 formed by alternately laminating a high refractive index layer 3 (TNO layer) and a low refractive index layer 4 (SiO2 layer) on a glass lens substrate 2 (D263Teco, manufactured by SCHOTT), an antistatic layer 6 (TNO layer), an oxygen-free layer 7 (MgF2 layer), a hard layer 8 (SiAl a O b N c layer (a<1, 0<b, 0<c)), an adhesion layer of about 6 nm (SiO2 layer), and a lubricating layer 11 (a fluoroalkyl ether layer (SC-100, manufactured by Canon Optron). That is, the optical element 1 has a multilayer film 9 in which the high refractive index layer 3 and the antistatic layer 6 are made of TNO layers.
[0110] The optical element 1 has a multilayer film 9 with an antireflection function for the visible light range. Assuming the center wavelength λ = 550 nm, the total optical film thickness of the oxygen-free layer 7 and the hard layer 8 is 0.896λ / 4.
[0111] Note that the refractive index of the hard layer 8 is 1.765 at 550 nm. The film thickness of the hard layer 8 is 10 nm or more, for example, 10 nm, so that the hard layer 8 has scratch resistance.
[0112] Here, in order to improve the adhesion between the hard layer 8 and the lubricating layer 11, the SiO2 layer formed between these layers is 6 nm, so that it does not substantially affect the optical properties of the multilayer film 9. The lubricating layer 11 made of fluoroalkyl ether has a film thickness of 14 nm so that light scattering does not occur.
[0113] Here, FIG. 10 shows the reflectance characteristics of the optical element according to Example 5. The horizontal axis in FIG. 10 is Wavelength (nm), and the vertical axis is Reflectance (%). The optical element 1 has the reflectance characteristics shown in FIG. 10.
[0114]
Table 5
[0115] <Example 6> Table 6 shows the configuration of the optical element according to Example 6.
[0116] The optical element 1 has a multilayer film 9 formed by alternately laminating a conductive film 12 (ITO layer), a low refractive index layer 4 (SiO2 layer), and a high refractive index layer 3 (TNO layer) on a radiation-resistant glass substrate 2 (S-BSL7R, manufactured by Ohara), an antistatic layer 6 (TNO layer), an oxygen-free layer 7 (MgF2 layer), and a hard layer 8 (SiAl a O b N c layer (a < 1, 0 < b, 0 < c)).
[0117] The conductive film 12 is formed to actively release the charge of the optical element 1 to the outside. The surface resistivity of the conductive film 12 is 9.91 Ω / square. Further, the deposition area of the conductive film 12 is formed to be larger than those of the laminate 5, the antistatic layer 6, and the oxygen-free layer 7.
[0118] The optical element 1 has a multilayer film 9 having an anti-reflection film for the visible light region. When the central wavelength λ is 550 nm, the total optical thickness of the oxygen-free layer 7 and the hard layer 8 is 0.872λ / 4.
[0119] The refractive index of the hard layer 8 is 1.765 at 550 nm. In order for the hard layer 8 to have scratch resistance, the film thickness of the hard layer 8 is 10 nm or more, for example, 13.2 nm.
[0120] 11 shows the reflectance characteristics of the optical element according to Example 6. The horizontal axis of Fig. 11 is wavelength (nm) and the vertical axis is reflectance (%). The optical element 1 has the reflectance characteristics shown in Fig. 11.
[0121] [Table 6]
[0122] Comparative Example 1 Table 7 shows the configuration of the optical element according to Comparative Example 1.
[0123] The optical element 1 has a multilayer film 9 formed on a glass substrate 2 (D263Teco, manufactured by SCHOTT), which includes a laminate 5 in which high refractive index layers 3 (TiO2 layers) and low refractive index layers 4 (SiO2 layers) are alternately laminated, an antistatic layer 6 (TNO layer), and an oxygen-free layer 7 (MgF2 layer). Here, the oxygen-free layer 7 has an anti-reflection function. The optical thickness of the oxygen-free layer 7 is 0.268λ / 4, assuming λ=550 nm.
[0124] 12 shows the reflectance characteristics of the optical element according to Comparative Example 1. The horizontal axis of Fig. 12 is wavelength (nm) and the vertical axis is reflectance (%). The optical element 1 has the reflectance characteristics shown in Fig. 12.
[0125] [Table 7]
[0126] According to the results of performance evaluation of Examples 1 to 6 and Comparative Example 1, the optical members maintain a transmittance of 80% or more in the visible light wavelength region. Moreover, according to the results of evaluation of the reflectance of the optical member of Example 1, the reflectance is 1.5% or less in the visible light wavelength region. Shows.
[0127] (Wear test) The abrasion test was carried out as follows. Samples were prepared by cutting the optical elements 1 of Examples 1 to 6 and Comparative Example 1 into pieces measuring 25 mm long x 25 mm wide. The upper surface of the multilayer film 9 of each sample was abraded with cotton 30 times. The abrasion speed was 50 mm / s.
[0128] (Antistatic property confirmation test) Next, 0.5 g of Kanto loam (7 types) was spread on the multilayer film 9, and the optical element 1 was placed at an angle of 90° and gently vibrated. The evaluation criteria for the antistatic properties were as follows: ○: 0 to 100 Kanto loam particles adhering to optical element 1 △: 101 to 500 Kanto loam particles attached to optical element 1 ×: 501 or more Kanto loam particles adhered to optical element 1
[0129] (Scratch resistance verification test) Furthermore, without removing the Kanto loam adhering to the optical element 1, an abrasion test was carried out using Silbon paper to check for the presence or absence of scratches on the optical element 1. The load was 500 g, and the abrasion speed was 50 mm / s, with 100 reciprocations.
[0130] (Test Results) As a result of carrying out a wear test, an antistatic confirmation test, and a scratch resistance confirmation test, the optical elements of Examples 1 to 6 had a well-balanced performance of surface resistivity, antistatic property, and scratch resistance because they had an antistatic layer with low surface resistivity and a hard layer. Note that, although the antistatic property of Example 3 was lower than those of Examples 1, 2, and 4 to 6, the antistatic property was within a range that would not be problematic in practical use. On the other hand, the optical element of Comparative Example 1 had antistatic property but no scratch resistance.
[0131] FIG. 13 is a diagram showing the configuration of an optical element and a conductive member according to the present invention.
[0132] The optical element 1 is fixed so that at least a part of the antistatic layer 6 is in contact with the conductive member 13. The conductive member 13 also contacts other conductive members such as the housing (lens barrel 21) and functions to release the charge of the optical element 1 to the housing side. By having the above-mentioned configuration, the optical element 1 can further enhance the antistatic effect, thereby suppressing the adhesion of foreign matter. The conductive member 13 may be made of metal or a material in which known conductive members 13 are dispersed in resin.
[0133] FIG. 14 is a diagram showing the configuration of an optical element and a conductive member according to the present invention.
[0134] When the optical element 1 has a conductive film 12 as in Example 6, at least a part of the conductive film 12 of the optical element 1 may be in contact with the conductive member 13. In this case, a part of the antistatic layer 6 may or may not be in contact with the conductive member 13.
[0135] 13 and 14, the optical element 1 is in contact with the conductive member 13 of the frame, but this is not necessarily the case and the metal wire may be disposed in contact with the antistatic layer 6 or the conductive film 12. The conductive member 13 may also function as a lens barrel.
[0136] FIG. 15 shows an optical unit and an optical device according to the present invention.
[0137] (optical device) The optical device 32 includes an optical unit 31 including a lens barrel 21, lenses 22 to 25, and an aperture 26, a protective filter 29, a cover glass 27, an imaging element 28, and a foreign matter removal mechanism 30.
[0138] (Optical unit) The light incident on the optical unit 31 is collected by the lenses 22 to 25 and the like on the image pickup element 28, which is made up of a CCD and a CMOS sensor. The light collected on the image pickup element 28 is converted into an electric signal and imaged as necessary. Here, at least one of the lens 22 and the protective filter 29 mounted on the optical unit 31 is the optical element 1 of the present invention. In other words, the lens 22 or the protective filter 29, which is closest to the subject, has antistatic properties and scratch resistance.
[0139] The diaphragm 26 has a function of preventing unnecessary light from entering the imaging element 28, and may be provided between each lens, or may be provided only in some of the spaces between the lenses. When the optical unit 31 is used under severe temperature conditions, such as in an in-vehicle camera or a surveillance camera, the diaphragm 26 is preferably an diaphragm made of a metal substrate. The metal diaphragm 26 is, for example, a metal plate blackened by anodization, or a metal substrate on which a film having a light absorbing function is formed by deposition or the like.
[0140] The protective filter 29 is a filter provided to protect the optical unit 31 from dirt and damage, and has optical functions such as AR (anti-reflection) function, UV cut, IR cut, and visible light cut.
[0141] The cover glass 27 is provided to prevent foreign matter from adhering to the imaging element 28, and is, for example, a glass material or a quartz substrate. The cover glass 27 may have a near-infrared cut function. When imaging the light incident on the imaging element 28, the sensitivity of the imaging element 28 in the near-infrared region may cause a difference from the color visible to the human eye. In such a case, an infrared cut film or the like may be formed on the cover glass 27 to prevent light in the near-infrared region from being incident on the imaging element 28.
[0142] The infrared cut film utilizes the light interference effect obtained by alternately laminating low refractive index layers and high refractive index layers, for example. The cover glass 27 may be infrared absorbing glass that is kneaded with metal ions that have absorption in the near infrared region.
[0143] The foreign matter removal mechanism 30 is a mechanism for physically removing foreign matter adhering to the optical element. The foreign matter removal mechanism 30 may be made of any of rubber, metal, and ceramics, such as a so-called wiper (a mechanism for wiping off dirt and impurities).
[0144] 15 is an example of an optical device according to the present invention, and does not necessarily have to include all of the components shown in the figure. In FIG. 15, the optical unit 31 is configured with four lenses, but the number of lenses may be three or less, or five or more.
[0145] Furthermore, the optical unit 31 does not necessarily have to be a lens unit, and may be an optical unit including an anti-reflection protective film and a phase film of a liquid crystal display device, etc. For example, at least one of the optical element 1, the optical unit 31, and the optical device 32 of the present invention can be applied to the windshield of a driving body of a space probe or the like and an optical sensor attached to the driving body.
[0146] The application environments of the optical element 1, optical unit 31, and optical device 32 of the present invention include, for example, the moon and planets. Fine sand (regolith) exists on the surfaces of celestial bodies such as the moon and planets. Furthermore, on the moon, which has almost no atmosphere, the regolith is electrically charged. If this regolith adheres to the windshield or optical sensor of a probe, it will block visibility. If the regolith is physically removed from the optical element, the optical element will be damaged by the frictional force of the regolith particles.
[0147] The optical element of the present invention has antistatic properties and scratch resistance, and therefore can suppress adhesion of regolith. Even if regolith adheres to the optical element, the amount of regolith that adheres is less than that of the conventional optical element, so that the optical element is less likely to be scratched even if the regolith that adheres to the optical element is removed by a physical method. This makes it possible to provide an optical device that can maintain good visibility and good sensor sensitivity for a long period of time.
[0148] As another application, a solar power generation panel having a power generation layer on the surface of which is provided the optical element of the present invention can suppress adhesion of foreign matter and scratches, and therefore can generate stable power for a long period of time.
[0149] The invention is not limited to the above-described embodiments, and various modifications and variations are possible without departing from the spirit and scope of the invention. Accordingly, the following claims are appended to apprise the public of the scope of the invention. [Explanation of symbols]
[0150] 1 Optical elements 2. Board 3 High refractive index layer 4. Low refractive index layer 5. Laminate 6 Antistatic layer 7 Oxygen-free layer 8 hard layer 9 Optical multilayer film 10 Gas barrier layer 11 Lubricating layer 12 Conductive film 13 Conductive materials 21 Lens barrel 22~25 Lens 26 Aperture 27 Coverslip 28 Image sensor 29 Protective Filters 30 Foreign object removal mechanism 31 Optical Unit 32 Optical equipment
Claims
1. A multilayer film laminated on a substrate, a low refractive index layer and a high refractive index layer having a refractive index higher than that of the low refractive index layer, which are alternately stacked; a hard layer, in this order from the substrate side; an oxygen-free layer is formed immediately on an antistatic layer having a surface resistivity lower than that of the low refractive index layer and the hard layer among the layers constituting the multilayer film; A multilayer film characterized by:
2. At least one of the high refractive index layers is the antistatic layer. The multilayer film according to claim 1 .
3. The antistatic layer is provided on the low refractive index layer and the high refractive index layer which are alternately stacked. The multilayer film according to claim 1 .
4. The hard layer is the oxygen-free layer. The multilayer film according to claim 1 .
5. The oxygen-free layer is made of MgF 2 , Si 3 N 4 and DLC, The multilayer film according to claim 1 .
6. The hard layer is made of Si 3 N 4 , SiO x N y (0<x<2, 0<y<1.33), and SiM a O b N c (M: metal element, a<1, 0≦b, 0<c) The multilayer film according to claim 1 .
7. The antistatic layer is a thin film made of TNO. The multilayer film according to claim 1 .
8. a gas barrier layer having the highest gas barrier property is provided between the antistatic layer and the hard layer; The multilayer film according to claim 1 .
9. A lubricating layer having minimal friction is provided directly on the hard layer. The multilayer film according to claim 1 .
10. a conductive film formed between the substrate and the multilayer film such that at least a portion of the conductive film is in contact with the multilayer film; The multilayer film according to claim 1 .
11. The substrate is a glass having a radiation-resistant function; The multilayer film according to claim 1 .
12. The substrate; The multilayer film according to claim 10, An optical element characterized by:
13. The optical element according to claim 12 is held by a conductive member, At least a part of the multilayer film or the conductive film is in contact with the conductive member. An optical member characterized by:
14. an optical element having the substrate and the multilayer film according to any one of claims 1 to 11; and an image pickup element that captures an image of the light transmitted through the optical element.
1. An optical device comprising:
Citation Information
Patent Citations
Glass article coated with conductive antireflection film
JP3581783B2