Positive electrode active material and method for manufacturing positive electrode active material

A layered rock salt crystal structured positive electrode active material with specific surface and inner layer compositions addresses conductivity and structural stability issues in lithium ion secondary batteries, improving discharge capacity and safety.

JP2024160775APending Publication Date: 2024-11-15SEMICON ENERGY LAB CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023076117
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-02
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Lithium ion secondary batteries face challenges in discharge capacity, cycle characteristics, reliability, safety, and conductivity, particularly in low-temperature environments, due to changes in the positive electrode active material's crystal structure and hindered lithium ion insertion and extraction.

Method used

A positive electrode active material with a layered rock salt crystal structure, containing lithium cobalt oxide or cobalt-lithium nickelate, is developed with crack portions having specific surface and inner wall surface layers enriched with aluminum and titanium or nickel, respectively, to enhance conductivity and stabilize the crystal structure.

Benefits of technology

The proposed active material improves lithium ion conductivity, maintains discharge capacity in low-temperature environments, and prevents structural collapse during charging and discharging cycles, enhancing battery safety and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024160775000001_ABST
    Figure 2024160775000001_ABST
Patent Text Reader

Abstract

To provide a positive electrode active material of which discharge capacity in a charge-discharge cycle is prevented from dropping, and a secondary battery using the positive electrode active material.SOLUTION: The positive electrode active material has a crystal structure of a layered rock salt type belonging to a space group R-3m. The positive electrode active material has a cobaltic acid lithium having a crack part. The cobaltic acid lithium has a surface layer part and an inner wall surface layer part including the surface of the inner wall of the crack part. The surface layer part has aluminum and nickel. The inner wall surface layer part has aluminum and does not substantially have nickel.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] One embodiment of the present invention relates to an object, a method, or a manufacturing method. Alternatively, the present invention relates to a process, a machine, a manufacture, or a composition of matter. One embodiment of the present invention relates to a power storage device including a secondary battery, a semiconductor device, a display device, a light-emitting device, a lighting device, an electronic device, or a manufacturing method thereof.

[0002] In this specification, the term "electronic device" refers to any device having a power storage device, and an electro-optical device having a power storage device, an information terminal device having a power storage device, and the like are all classified as electronic devices. [Background technology]

[0003] In recent years, various types of power storage devices, such as lithium-ion secondary batteries, lithium-ion capacitors, and air batteries, have been actively developed. In particular, the demand for high-output, high-energy-density lithium-ion secondary batteries has rapidly expanded in conjunction with the development of the semiconductor industry, and they have become indispensable in modern society as a repeatedly rechargeable energy source, as they are used in portable information terminals, such as mobile phones, smartphones, and notebook computers, portable music players, digital cameras, medical equipment, and next-generation clean energy automobiles, such as hybrid vehicles (HVs), electric vehicles (EVs), and plug-in hybrid vehicles (PHVs).

[0004] Lithium ion secondary batteries are required to have high capacity density, high performance, and safety in various operating environments.

[0005] Patent Documents 1 and 2 disclose methods for producing electrodes that can increase the capacity density of secondary batteries. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] WO2020 / 128699 Brochure [Patent Document 2] WO2022 / 172118 Brochure Summary of the Invention [Problem to be solved by the invention]

[0007] Lithium ion secondary batteries have room for improvement in various aspects, such as discharge capacity, cycle characteristics, reliability, safety, and cost. For example, in order to suppress changes in the crystal structure of the surface of the positive electrode active material, the surface of the positive electrode active material may be coated with an inactive oxide, but this coating may reduce the electrical conductivity and inhibit the insertion and desorption of lithium. If the electrical conductivity is reduced and / or the insertion and desorption of lithium ions is inhibited, there is a concern that the characteristics of the secondary battery may be reduced, such as a reduction in rate characteristics and a reduction in charge and discharge capacity in a low-temperature environment.

[0008] In view of the above, an object of one embodiment of the present invention is to provide a positive electrode active material that can be used in a lithium ion secondary battery and has improved conductivity and / or facilitates insertion and desorption of lithium ions. Another object is to provide a positive electrode active material or a composite oxide in which a decrease in discharge capacity in a low-temperature environment is suppressed. Another object is to provide a positive electrode active material or a composite oxide in which a decrease in discharge capacity in a charge and discharge cycle is suppressed. Another object is to provide a positive electrode active material or a composite oxide whose crystal structure is not easily destroyed even after repeated charge and discharge. Another object is to provide a positive electrode active material or a composite oxide with a large discharge capacity. Another object is to provide a secondary battery or a vehicle with high safety or reliability.

[0009] Another object of one embodiment of the present invention is to provide a positive electrode active material, a composite oxide, a power storage device, or a manufacturing method thereof.

[0010] Note that the description of these problems does not preclude the existence of other problems. Note that one embodiment of the present invention does not necessarily solve all of these problems. Note that it is possible to extract problems other than these from the description of the specification, drawings, and claims. [Means for solving the problem]

[0011] One aspect of the present invention is a positive electrode active material having a layered rock salt type crystal structure belonging to space group R-3m, the positive electrode active material has lithium cobalt oxide, the lithium cobalt oxide has a crack portion, the lithium cobalt oxide has a surface layer portion and an inner wall surface layer portion including the surface of the inner wall of the crack portion, the surface layer portion has aluminum and nickel, and the inner wall surface layer portion has aluminum. Note that it is preferable that the inner wall surface layer portion is substantially free of nickel.

[0012] Alternatively, one embodiment of the present invention is a positive electrode active material having a layered rock salt type crystal structure belonging to space group R-3m, the positive electrode active material has cobalt-lithium nickel oxide, the cobalt-lithium nickel oxide has a crack portion, the cobalt-lithium nickel oxide has a surface layer portion and an inner wall surface layer portion including the surface of the inner wall of the crack portion, the surface layer portion has aluminum and titanium, and the inner wall surface layer portion has aluminum. Note that it is preferable that the inner wall surface layer portion is substantially free of titanium.

[0013] Alternatively, one embodiment of the present invention is a positive electrode active material having a layered rock salt type crystal structure belonging to space group R-3m, the positive electrode active material has nickel-cobalt-manganese lithium, the nickel-cobalt-manganese lithium has a crack part, the nickel-cobalt-manganese lithium has a surface layer part and an inner wall surface layer part including the surface of the inner wall of the crack part, the surface layer part has aluminum and titanium, and the inner wall surface layer part has aluminum. Note that it is preferable that the inner wall surface layer part does not substantially contain titanium.

[0014] One embodiment of the present invention is a method for producing a positive electrode active material, comprising: a first step of mixing a composite oxide having a layered rock-salt crystal structure belonging to the space group R-3m, a solid material, and a liquid material to produce a mixture; and a second step of heating the mixture, in which the solid material contains nickel and the liquid material contains aluminum.

[0015] In the above, the solid material includes one of nickel oxide and nickel hydroxide, and the liquid material includes one of an aluminum alkoxide solution, an aluminum acetylacetonate solution, an aluminum lactate solution, and an aluminum phthalocyanine solution.

[0016] Alternatively, one embodiment of the present invention is a method for producing a positive electrode active material, comprising: a first step of mixing a composite oxide having a layered rock-salt crystal structure belonging to the space group R-3m, a solid material, and a liquid material to produce a mixture; and a second step of heating the mixture, in which the solid material contains titanium and the liquid material contains aluminum.

[0017] In the above, the solid material includes any one of lithium titanate, titanium oxide, and titanium hydroxide, and the liquid material includes any one of an aluminum alkoxide solution, an aluminum acetylacetonate solution, an aluminum lactate solution, and an aluminum phthalocyanine solution.

[0018] In any one of the above methods for producing a positive electrode active material, the particle size of the solid material is such that D50 (median diameter) obtained by particle size distribution measurement is 1 μm or more and 5 μm or less.

[0019] Alternatively, one embodiment of the present invention is a method for producing a positive electrode active material, comprising: a first step of mixing a composite oxide having a layered rock-salt crystal structure belonging to the space group R-3m, a first solid material, a second solid material, and a liquid material to produce a mixture; and a second step of heating the mixture, in which the first solid material contains nickel, the second solid material contains titanium, and the liquid material contains aluminum.

[0020] In the above, the first solid material includes one of nickel oxide and nickel hydroxide, the second solid material includes one of lithium titanate, titanium oxide and titanium hydroxide, and the liquid material includes one of an aluminum alkoxide solution, an aluminum acetylacetonate solution, an aluminum lactate solution and an aluminum phthalocyanine solution.

[0021] In any one of the above methods for producing a positive electrode active material, the particle diameter of the first solid material is such that D50 (median diameter) obtained by particle size distribution measurement is 1 μm or more and 5 μm or less, and the particle diameter of the second solid material is such that D50 (median diameter) obtained by particle size distribution measurement is 1 μm or more and 5 μm or less. Effect of the Invention

[0022] According to one embodiment of the present invention, it is possible to provide a positive electrode active material that can be used in a lithium ion secondary battery and has improved electrical conductivity and / or facilitated insertion and desorption of lithium ions. Alternatively, it is possible to provide a positive electrode active material or composite oxide that can be used in a lithium ion secondary battery and in which a decrease in discharge capacity in a low-temperature environment is suppressed. Alternatively, it is possible to provide a positive electrode active material or composite oxide in which a decrease in discharge capacity during charge and discharge cycles is suppressed. Alternatively, it is possible to provide a positive electrode active material or composite oxide whose crystal structure is unlikely to collapse even after repeated charge and discharge. Alternatively, it is possible to provide a positive electrode active material or composite oxide with a large discharge capacity. Alternatively, it is possible to provide a secondary battery or vehicle with high safety or reliability.

[0023] According to one embodiment of the present invention, a positive electrode active material, a composite oxide, a power storage device, or a manufacturing method thereof can be provided.

[0024] Note that the description of these effects does not preclude the existence of other effects. Note that one embodiment of the present invention does not necessarily have all of these effects. Note that effects other than these will become apparent from the description in the specification, drawings, claims, etc., and it is possible to extract effects other than these from the description in the specification, drawings, claims, etc. [Brief description of the drawings]

[0025] [Figure 1] Fig. 1(A) is a schematic diagram of a cross-sectional structure of a positive electrode active material, and Fig. 1(B) and Fig. 1(C) are diagrams illustrating the distribution of an additive element in the positive electrode active material. [Diagram 2] 2(A) and 2(B) are diagrams illustrating the distribution of additive elements in the positive electrode active material. [Diagram 3] FIG. 3 is a diagram illustrating a method for producing a positive electrode active material. [Figure 4] 4(A) and 4(B) are diagrams illustrating the step of adding an additive element. [Diagram 5] FIG. 5 is a diagram illustrating a method for producing a positive electrode active material. [Figure 6] 6(A) and 6(B) are SEM (scanning electron microscope) images illustrating an example of a crack. [Figure 7] FIG. 7 is a diagram illustrating a method for producing a positive electrode active material. [Figure 8] FIG. 8 is a diagram illustrating a method for producing a positive electrode active material. [Figure 9] FIG. 9 is a diagram illustrating a method for producing a positive electrode active material. [Figure 10] FIG. 10 is a diagram illustrating a method for producing a positive electrode active material. [Figure 11] FIG. 11 is a diagram illustrating a method for producing a positive electrode active material. [Figure 12] FIG. 12 is a diagram illustrating a method for producing a positive electrode active material. [Figure 13] FIG. 13 is a diagram illustrating a method for producing a positive electrode active material. [Figure 14]FIG. 14 is a diagram illustrating a method for producing a positive electrode active material. [Figure 15] FIG. 15 is a diagram showing the external appearance of a secondary battery. [Figure 16] 16A to 16C are diagrams illustrating a method for manufacturing a secondary battery. [Figure 17] 17A to 17H are diagrams illustrating examples of electronic devices. [Figure 18] 18A to 18D are diagrams illustrating examples of electronic devices. [Figure 19] 19A to 19C are diagrams illustrating examples of electronic devices. [Figure 20] 20(A) to 20(C) are diagrams illustrating an example of a vehicle. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] In the following, examples of embodiments of the present invention will be described with reference to the drawings, etc. However, the present invention should not be interpreted as being limited to the following examples. The embodiments of the present invention can be modified without departing from the spirit of the present invention.

[0027] In this specification, the space group is expressed using the short notation of the international notation (or Hermann-Mauguin notation). The crystal plane and crystal direction are expressed using Miller indices. In crystallography, the space group, crystal plane, and crystal direction are expressed by adding a superscript bar to the number, but in this specification, due to format restrictions, instead of adding a bar above the number, a - (minus sign) may be added before the number. In addition, individual directions indicating directions within a crystal are expressed with [ ], collective directions indicating all equivalent directions are expressed with < >, individual planes indicating crystal planes are expressed with ( ), and collective planes with equivalent symmetry are expressed with {}. In addition, trigonal crystals expressed by the space group R-3m are generally sometimes expressed as a composite hexagonal lattice of hexagonal crystals for ease of understanding the structure. In addition, not only (hkl) but also (hkil) may be used as Miller indices. Here, i is -(h+k). In this specification, the crystal planes of the space group R-3m are expressed as a composite hexagonal lattice unless otherwise specified.

[0028] In this specification and the like, the term "particle" does not necessarily refer to only spherical shapes (cross-sectional shape being circular), and the cross-sectional shape of each particle may be an ellipse, a rectangle, a trapezoid, a triangle, a square with rounded corners, an asymmetric shape, or the like, and further each particle may be an irregular shape.

[0029] The theoretical capacity of a positive electrode active material refers to the amount of electricity when all of the lithium that can be inserted and removed from the positive electrode active material is removed. For example, the theoretical capacity of LiCoO2 is 274mAh / g, that of LiNiO2 is 275mAh / g, and that of LiMn2O4 is 148mAh / g.

[0030] In addition, the amount of lithium remaining in the positive electrode active material that can be inserted or removed can be determined by the x in the composition formula, for example, Li x The charge capacity is expressed as x in MO2 (where M is one or more selected from cobalt, nickel, and manganese). In the case of a positive electrode active material in a secondary battery, x = (theoretical capacity - charging capacity) / theoretical capacity. For example, when a secondary battery using LiMO2 as the positive electrode active material is charged at 219.2 mAh / g, Li 0.2 We can say MO2 or x=0.2. Lix When x in MO2 is small, for example, it means 0.1 < x ≤ 0.24. Also, when indicating to what extent the lithium desorbed from the positive electrode active material is with respect to the theoretical capacity, it may be shown as the depth of charge. In this specification and the like, the depth of charge = 1 - x.

[0031] For example, when appropriately synthesized lithium cobaltate before being used in the positive electrode approximately satisfies the stoichiometric ratio, it is LiCoO2 and x = 1. Also, the lithium cobaltate contained in the secondary battery after the discharge is completed may also be said to be LiCoO2 and x = 1. Here, the completion of the discharge means, for example, a state where the voltage becomes 3.0 V or 2.5 V or less at a current of 100 mA / g or less.

[0032] Li x The charge capacity and / or discharge capacity used for calculating x in MO2 are preferably measured under conditions where there is no or little influence of short circuit and / or decomposition of the electrolyte solution, etc. For example, the data of the secondary battery in which a rapid change in capacity regarded as a short circuit has occurred should not be used for calculating x.

[0033] Also, the space group of the crystal structure is identified by XRD, electron beam diffraction, neutron beam diffraction, etc. Therefore, in this specification and the like, the terms belonging to a certain space group, being of a certain space group, or being a certain space group can be paraphrased as being identified as a certain space group.

[0034] Also, if the arrangement of anions is roughly close to cubic close-packed, it can be considered as cubic close-packed. The arrangement of anions in cubic close-packed refers to a state in which the second layer of anions is arranged above the gaps of the anions packed in the first layer, and the third layer of anions is arranged directly above the gaps of the second layer of anions, but not directly above the anions in the first layer. Therefore, the anions do not have to be strictly cubic lattices. Also, since real crystals always have defects, the analysis results do not necessarily have to be as theoretically correct. For example, in the electron diffraction pattern or FFT (fast Fourier transform) pattern of a TEM image, etc., spots may appear at positions slightly different from the theoretical positions. For example, if the orientation with respect to the theoretical positions is 5 degrees or less, or 2.5 degrees or less, it can be said to have a cubic close-packed structure.

[0035] The distribution of a certain element refers to a region in which the element is continuously detected in a certain continuous analytical method without being a noise region. The region in which the element is continuously detected in a non-noise region can also be referred to as a region in which the element is always detected when the analysis is performed multiple times.

[0036] Furthermore, a positive electrode active material to which an additive element that improves electrical conductivity and / or an additive element that stabilizes the crystal structure has been added may be referred to as a composite oxide, a positive electrode material, a positive electrode material, a positive electrode material for secondary batteries, etc.

[0037] In addition, when describing the characteristics of individual particles of the positive electrode active material in the following embodiments, etc., it is not necessary that all particles have that characteristic. For example, if 50% or more, preferably 70% or more, and more preferably 90% or more of three or more randomly selected particles of the positive electrode active material have that characteristic, it can be said that there is a sufficient effect of improving the characteristics of the positive electrode active material and the secondary battery having it.

[0038] As the charging voltage of a secondary battery increases, the voltage of the positive electrode generally increases. The positive electrode active material of one embodiment of the present invention has a stable crystal structure even at high voltages. Since the crystal structure of the positive electrode active material is stable in a charged state, it is possible to suppress a decrease in charge / discharge capacity due to repeated charging and discharging.

[0039] Unless otherwise specified, the materials (positive electrode active material, negative electrode active material, electrolyte, separator, etc.) of the secondary battery are described in the state before degradation. The decrease in discharge capacity due to aging and burn-in treatments during the secondary battery manufacturing stage is not called degradation. For example, when a lithium-ion secondary cell and a lithium-ion secondary battery pack (hereinafter referred to as a lithium-ion secondary battery) have a discharge capacity of 97% or more of the rated capacity, it can be said to be in the state before degradation. The rated capacity of lithium-ion secondary batteries for portable devices complies with JIS C 8711:2019. For other lithium-ion secondary batteries, the rated capacity complies with not only the above JIS standard but also with each JIS, IEC standard, etc. for electric vehicle propulsion and industrial use.

[0040] In this specification, the state of the materials in a secondary battery before deterioration is referred to as an initial product or initial state, and the state after deterioration (the state when the secondary battery has a discharge capacity less than 97% of the rated capacity) may be referred to as a product in use or in use state, or a used product or used state.

[0041] (Embodiment 1) In this embodiment, a positive electrode active material 100 of one embodiment of the present invention will be described with reference to FIGS.

[0042] <Cathode active material> Fig. 1(A) is a schematic diagram of a cross-sectional structure of a positive electrode active material 100 according to one embodiment of the present invention. Fig. 1(B) and Fig. 1(C) are schematic diagrams of element concentration distributions in a cross section of the positive electrode active material 100, as measured by STEM (scanning transmission electron microscope)-EDX (energy dispersive X-ray spectroscopy) line analysis.

[0043] 1A shows a cross-sectional structure of a positive electrode active material 100 having a crack portion 106. However, the positive electrode active material 100 of one embodiment of the present invention may include not only the positive electrode active material 100 having the crack portion 106, but also the positive electrode active material 100 without the crack portion 106. In addition, the proportion of the number of particles of the positive electrode active material 100 having the crack portion 106 to the total number of particles of the positive electrode active material 100 is preferably small.

[0044] 1A, the positive electrode active material 100 has a surface layer portion 100a and an interior portion 100b. Moreover, the positive electrode active material 100 having a crack portion 106 has an inner wall surface layer portion 100c in the crack portion 106.

[0045] 1(A) shows a state after an additive element is added to a crack that occurred before the step of adding the additive element in the manufacturing process of the positive electrode active material 100. Since the crack occurred before the step of adding the additive element, the inner wall surface layer 100c of the crack portion 106 can contain the additive element described later.

[0046] On the other hand, in the manufacturing process of the positive electrode active material 100, cracks may occur even after the process of adding the additive element. The cracked portion that occurs after the process of adding the additive element cannot have the inner wall surface layer portion 100c. Therefore, the positive electrode active material 100 may be not only a positive electrode active material having the crack portion 106 shown in FIG. 1(A), but also a positive electrode active material having the surface layer portion 100a and not having the inner wall surface layer portion 100c. The manufacturing process of the positive electrode active material 100 will be described in detail later.

[0047] In this specification and the like, the surface layer 100a of the positive electrode active material 100 refers to, for example, a region within 50 nm from the surface toward the inside, more preferably within 35 nm from the surface toward the inside, even more preferably within 20 nm from the surface toward the inside, and most preferably within 10 nm perpendicular or approximately perpendicular from the surface toward the inside. Note that approximately perpendicular is defined as an angle of 80° or more and 100° or less.

[0048] In this specification and the like, the inner wall surface portion 100c of the positive electrode active material 100 refers to, for example, a region in the crack portion 106 that is within 50 nm from the inner wall surface of the crack portion 106 toward the inside, more preferably within 35 nm from the inner wall surface toward the inside, even more preferably within 20 nm from the inner wall surface toward the inside, and most preferably within 10 nm perpendicular or approximately perpendicular from the inner wall surface toward the inside.

[0049] The region deeper than the surface layer 100a of the positive electrode active material and the region deeper than the inner wall surface layer 100c are referred to as the interior 100b, which is synonymous with the interior region or core.

[0050] The surface of the positive electrode active material 100 and the inner wall surface of the crack portion 106 refer to the surface of the composite oxide including the surface layer portion 100a and the interior portion 100b. Therefore, aluminum oxide (AlO X (X is an arbitrary number)) and other metal oxides attached thereto, carbonates chemically adsorbed after the preparation of the positive electrode active material, hydroxyl groups, and the like are not included in the positive electrode active material 100. The attached metal oxide refers to, for example, a metal oxide whose crystal structure does not match that of the interior 100b.

[0051] In addition, the positive electrode active material 100 does not include the electrolyte, organic solvent, binder, conductive material, or compounds derived from these that are attached to the positive electrode active material 100.

[0052] Although not shown, the positive electrode active material 100 may have a crystal grain boundary. The crystal grain boundary refers to, for example, a portion where particles of the positive electrode active material 100 are adhered to each other, a portion where the crystal orientation changes inside the positive electrode active material 100, that is, a portion where the repetition of bright and dark lines in a STEM image or the like becomes discontinuous, a portion containing many crystal defects, a portion where the crystal structure is disordered, and the like. The crystal defect refers to a defect that can be observed in a cross-sectional TEM (transmission electron microscope) or a cross-sectional STEM image, that is, a structure in which other atoms have entered between lattices, a cavity, and the like. The crystal grain boundary can be said to be one of the plane defects. The vicinity of the crystal grain boundary refers to a region within 10 nm from the crystal grain boundary.

[0053] [Contained elements] The positive electrode active material 100 includes lithium, a transition metal M, oxygen, and an additive element that improves electrical conductivity. It is preferable that the positive electrode active material 100 further includes an additive element that stabilizes the crystal structure. The additive element that improves electrical conductivity and the additive element that stabilizes the crystal structure may be simply called an additive element. The transition metal M is one or more selected from cobalt, nickel, manganese, and iron. The positive electrode active material 100 may have, for example, a layered rock salt type crystal structure. More specifically, the positive electrode active material 100 may have lithium cobalt oxide (LCO), lithium cobalt nickel oxide (LCNO), lithium nickel cobalt manganate (NCM), and lithium nickel cobalt aluminum oxide (NCA), each of which has a layered rock salt type crystal structure.

[0054] The positive electrode active material 100 can be said to be a composite oxide (LiMO2) of lithium and a transition metal M having a layered rock-salt crystal structure to which an additive element is added. In this case, however, the positive electrode active material 100 of one embodiment of the present invention may have a distribution or crystal structure of the additive element described below. Therefore, the composition is not strictly limited to Li:M:O=1:1:2 (atomic ratio).

[0055] The additive element that improves the electrical conductivity is preferably dissolved in the surface layer 100a of the positive electrode active material 100. The additive element that stabilizes the crystal structure is preferably dissolved in the surface layer 100a of the positive electrode active material 100 and the inner wall surface layer 100c of the crack portion 106.

[0056] Therefore, for example, when STEM-EDX line analysis is performed in the depth direction in the surface layer portion 100a and the inner wall surface layer portion 100c, the depth at which the amount of these added elements detected increases is preferably located deeper than the depth at which the amount of transition metal M detected increases, i.e., toward the inside of the positive electrode active material 100.

[0057] The additive element for improving the conductivity of the positive electrode active material 100 may be an element that is not only highly conductive as a single element but also highly conductive when it is made into a compound, for example, an oxide. A compound having high conductivity means that the electrical conductivity (literature value) of the compound is higher than the electrical conductivity (literature value) of the material in the inside 100b of the positive electrode active material 100. Specifically, either nickel or titanium or both of them can be used. By containing these additive elements, it is expected that the impedance of the surface layer 100a of the positive electrode active material 100 will be reduced. Nickel oxide and titanium oxide have semiconducting properties.

[0058] As an additive element for stabilizing the crystal structure, it is preferable to use one or more elements selected from aluminum, magnesium, fluorine, zirconium, iron, manganese, chromium, arsenic, zinc, silicon, sulfur, phosphorus, boron, bromine, and beryllium.

[0059] [distribution] The positive electrode active material 100 preferably has the above-mentioned additive element in the surface layer portion 100a and the inner wall surface layer portion 100c of the crack portion 106. In addition, it is more preferable that the positive electrode active material 100 has a plurality of additive elements.

[0060] Moreover, it is preferable that the surface layer portion 100a has a higher concentration of one or more selected from the additive elements than the inner portion 100b. Alternatively, it is preferable that the surface layer portion 100a has a larger detected amount of one or more selected from the additive elements than the inner portion 100b. It is also preferable that the surface layer portion 100a has a concentration gradient of one or more selected from the additive elements contained in the positive electrode active material 100.

[0061] In addition, it is preferable that the concentration of one or more selected from the additive elements is higher in the inner wall surface layer portion 100c than in the interior 100b. Alternatively, it is preferable that the detection amount of one or more selected from the additive elements is higher in the inner wall surface layer portion 100c than in the interior 100b. It is also preferable that the one or more selected from the additive elements contained in the positive electrode active material 100 have a concentration gradient in the inner wall surface layer portion 100c.

[0062] In addition, when the positive electrode active material 100 has a layered rock salt type crystal structure of space group R-3m, the surface layer portion 100a has an edge region and a basal region. (001) in FIG. 1(A) indicates the (001) plane of LiMO2. Here, the edge region has a surface exposed in a direction intersecting with the (001) plane (also called a surface other than the (001) orientation), and the edge region is a region within 50 nm from the surface toward the inside, more preferably within 35 nm from the surface toward the inside, even more preferably within 20 nm from the surface toward the inside, and most preferably within 10 nm perpendicular or approximately perpendicular from the surface toward the inside. Here, "intersect" means that the angle between the perpendicular to the first face (the (001) face) and the normal to the second face (the surface of the positive electrode active material 100) is 10 degrees or more and 90 degrees or less, more preferably 30 degrees or more and 90 degrees or less, and even more preferably 50 degrees or more and 90 degrees or less.

[0063] The basal region has a surface parallel to the (001) plane (also referred to as a (001)-oriented surface), and is a region within 50 nm from the surface toward the inside, more preferably within 35 nm from the surface toward the inside, even more preferably within 20 nm from the surface toward the inside, and most preferably within 10 nm perpendicular or approximately perpendicular from the surface toward the inside. Note that "parallel" here means that the angle between the perpendicular to the first surface (the (001) plane) and the normal to the second surface (the surface of the positive electrode active material 100) is 0 degrees or more and less than 10 degrees, preferably 0 degrees or more and 5 degrees or less, more preferably 0 degrees or more and 2.5 degrees or less.

[0064] Furthermore, the distribution of the additive element may differ between the edge region and the basal region of the positive electrode active material 100.

[0065] The distribution of the positive electrode active material 100 may differ depending on the added element. For example, the depth of the peak of the detection amount in the surface layer from the surface or a reference point in EDX ray analysis described later may differ depending on the added element. The peak of the detection amount here refers to the maximum value of the detection amount at the surface layer 100a or 50 nm or less from the surface. The peak of the detection amount refers to the maximum value of the detection amount at the inner wall surface layer 100c or 50 nm or less from the inner wall surface. The detection amount refers to, for example, the count in EDX ray analysis.

[0066] FIG. 1(B) is a schematic diagram of element concentration distribution when STEM-EDX ray analysis is performed from the outside (A) to the inside (B) of the positive electrode active material 100 in a region including the surface layer 100a of the positive electrode active material 100. In the graph of the schematic diagram, the horizontal axis indicates distance, and the vertical axis indicates the concentration of the added element. The vertical axis of the graph can also be shown as the count number of characteristic X-rays of the added element. Measurement from the outside to the inside of the positive electrode active material 100 is also called measurement in the depth direction, and the arrows A to B in FIG. 1(A) are an example of the depth direction of the surface layer 100a. The surface layer 100a at the position indicated by the arrows A to B in FIG. 1(A) is an edge region.

[0067] FIG. 1(B) shows a preferred distribution of each additive element when the positive electrode active material 100 has one or both of nickel and titanium as an additive element for improving conductivity and aluminum as an additive element for stabilizing the crystal structure. Of the additive elements, nickel (Ni) and titanium (Ti) are preferably higher in concentration in the positive electrode active material 100 on the outer side (side A) than in the positive electrode active material 100 on the inner side (side B), as shown by the curves labeled "Ni, Ti" in FIG. 1(B). Alternatively, it is preferred that the detected amount (count number) of nickel (Ni) and titanium (Ti) in the positive electrode active material 100 on the outer side (side A) is greater than the detected amount in the positive electrode active material 100 on the inner side (side B). Furthermore, it is preferred that nickel (Ni) and titanium (Ti) have a peak of the detected amount in a region closer to the surface of the surface layer portion 100a. For example, it is preferred that nickel (Ni) and titanium (Ti) have a peak of the detected amount on the surface or within 3 nm from the reference point.

[0068] By distributing either or both of nickel and titanium as described above, the impedance in the surface layer portion 100a of the positive electrode active material 100 can be reduced. When the positive electrode active material 100 is used in a battery, it is expected to have the effect of improving the charge / discharge rate and the charge / discharge characteristics at low temperatures.

[0069] Also, it is preferable that aluminum has a concentration peak on the inner side of nickel and titanium, as shown by the curve marked "Al" in FIG. 1(B). Alternatively, it is preferable that aluminum has a detection amount peak on the inner side of nickel and titanium. As shown in FIG. 1(B), the distributions of nickel and titanium and aluminum may overlap, but there may be almost no overlapping area. The detection amount peak of aluminum may be present in the surface layer portion 100a, or may be deeper than the surface layer portion 100a. For example, it is preferable that the peak is present on the surface, or in a region of 5 nm to 30 nm from the reference point toward the inside.

[0070] [aluminum] The distribution of aluminum as described above can further stabilize the layered rock-salt crystal structure of the positive electrode active material 100. For example, it is expected that the change from the layered rock-salt crystal structure to a spinel crystal structure in the surface layer 100a of the positive electrode active material 100 can be suppressed.

[0071] On the other hand, an excess of aluminum may adversely affect the insertion and extraction of lithium.

[0072] Therefore, it is preferable that the amount of aluminum contained in the entire positive electrode active material 100 is appropriate. For example, the number of aluminum atoms contained in the entire positive electrode active material 100 is preferably 0.05% to 4% of the number of atoms of the transition metal M (all of the elements contained in the positive electrode active material 100 among cobalt, nickel, manganese, and iron) contained in the entire positive electrode active material 100, preferably 0.1% to 2% and more preferably 0.3% to 1.5%. Alternatively, 0.05% to 2% is preferable. Alternatively, 0.1% to 4% is preferable. The amount contained in the entire positive electrode active material 100 may be, for example, a value obtained by performing elemental analysis of the entire positive electrode active material 100 using GD-MS, ICP-MS, or the like, or may be based on the value of the composition of raw materials in the process of producing the positive electrode active material 100.

[0073] FIG. 1(C) is a schematic diagram of element concentration distribution when STEM-EDX ray analysis is performed from the outside (C) to the inside (D) of the positive electrode active material 100 in a region including the inner wall surface layer portion 100c of the positive electrode active material 100. In the graph of the schematic diagram, the horizontal axis indicates distance, and the vertical axis indicates the concentration of the added element. The vertical axis of the graph can also be shown as the count number of characteristic X-rays of the added element. Measurement from the outside to the inside of the positive electrode active material 100 is also called measurement in the depth direction, and the arrows from C to D in FIG. 1(A) are an example of the depth direction of the inner wall surface layer portion 100c. When the positive electrode active material 100 has a layered rock salt type crystal structure of space group R-3m, cracks are likely to occur on the (001) plane, but cracks may occur on planes other than the (001) plane.

[0074] Unlike FIG. 1(B), FIG. 1(C) does not include a curve labeled "Ni, Ti." This shows a preferred distribution of additive elements in the positive electrode active material 100, in which the inner wall surface layer 100c of the crack portion 106 is substantially free of nickel and titanium, which are additive elements that improve electrical conductivity. In addition, aluminum, which is an additive element that stabilizes the crystal structure, is preferably distributed in the same manner as aluminum in FIG. 1(B), as shown by the curve labeled "Al" in FIG. 1(C).

[0075] However, the aluminum distribution in the surface layer portion 100a and the aluminum distribution in the inner wall surface layer portion 100c do not necessarily need to be the same, and may be different. For example, the aluminum concentration in the surface layer portion 100a may be higher than the aluminum concentration in the inner wall surface layer portion 100c, or the aluminum concentration in the surface layer portion 100a may be lower than the aluminum concentration in the inner wall surface layer portion 100c. In addition, the distance from the surface of the aluminum concentration peak in the surface layer portion 100a may be different from the distance from the inner wall surface of the aluminum concentration peak in the inner wall surface layer portion 100c.

[0076] As described above, by having aluminum but not nickel or titanium in the inner wall surface layer portion 100c, when the positive electrode active material 100 is used in a battery, it is possible to increase the impedance in the inner wall surface layer portion 100c and suppress the charge / discharge reaction in the crack portion 106. The above-described distribution of the additive elements in the inner wall surface layer portion 100c is preferable because it is possible to suppress the increase in deterioration of the battery caused by the volume change of the positive electrode active material 100 due to the charge / discharge reaction in the crack portion 106, specifically, the insertion / removal of lithium ions on the inner wall surface of the crack portion 106.

[0077] In this specification, "substantially free of a certain element" refers to a case where the characteristic X-ray energy spectrum of the element is not detected in cross-sectional STEM-EDX analysis. Also, a case where the characteristic X-ray energy spectrum of the element is not detected is also referred to as the element being below the detection limit in STEM-EDX analysis.

[0078] 2(A) and 2(B) show a preferred distribution of additive elements when magnesium is included as an additive element for stabilizing the crystal structure in addition to the configuration shown in FIG. 1(B) and FIG. 1(C). Of the additive elements, magnesium (Mg), nickel (Ni) and titanium (Ti) are preferably higher in concentration in the positive electrode active material 100 on the outer side (side A) than in the positive electrode active material 100 on the inner side (side B), as shown by the curves labeled "Mg, Ni, Ti" in FIG. 2(A). Alternatively, it is preferred that the detected amount of magnesium (Mg), nickel (Ni) and titanium (Ti) in the positive electrode active material 100 on the outer side (side A) is greater than the detected amount in the positive electrode active material 100 on the inner side (side B). Furthermore, it is preferred that magnesium (Mg), nickel (Ni) and titanium (Ti) have a peak of detected amount in a region closer to the surface of the surface layer portion 100a. For example, it is preferred that the detected amount peak is on the surface or within 3 nm from the reference point.

[0079] Moreover, it is preferable that the distributions of magnesium and nickel overlap in the surface layer portion 100a. The peaks of the detected amounts of magnesium and nickel may be at the same depth, or the peak of magnesium may be closer to the surface, or the peak of nickel may be closer to the surface. The difference in depth between the peak of the detected amount of nickel and the peak of the detected amount of magnesium is preferably within 3 nm, and more preferably within 1 nm. It is also preferable that the half-width of the detected amount is narrow.

[0080] Similarly, it is preferable that the distributions of magnesium and titanium overlap in the surface layer portion 100a. The peaks of the detected amounts of magnesium and titanium may be at the same depth, or the peak of magnesium may be closer to the surface, or the peak of titanium may be closer to the surface. The difference in depth between the peak of the detected amount of titanium and the peak of the detected amount of magnesium is preferably within 3 nm, and more preferably within 1 nm. It is also preferable that the half-width of the detected amount is narrow.

[0081] In other words, it is preferable that the distributions of magnesium, nickel, and titanium overlap in the surface layer portion 100a. The difference in depth between the peak of the detected amount of titanium, the peak of the detected amount of nickel, and the peak of the detected amount of magnesium is preferably within 3 nm, and more preferably within 1 nm. In addition, it is preferable that the half-width of the detected amount is narrow.

[0082] However, similarly to the explanation in FIG. 1(C), as shown in FIG. 2(B), in the positive electrode active material 100, it is preferable that the inner wall surface layer 100c of the crack portion 106 is substantially free of nickel and titanium, which are additive elements that improve electrical conductivity, and that the positive electrode active material 100 has magnesium (Mg) and aluminum (Al), which are additive elements that stabilize the crystal structure.

[0083] The effects of the added elements in the positive electrode active material 100 other than those described above will be described below.

[0084] [Fluorine] Fluorine, an additive element that stabilizes the crystal structure, is a monovalent anion, and when part of the oxygen is replaced by fluorine in the surface layer portion 100a and the inner wall surface layer portion 100c, the lithium desorption energy is reduced. This is because the redox potential of the cobalt ion accompanying lithium desorption differs depending on the presence or absence of fluorine. In other words, when there is no fluorine, the cobalt ion changes from trivalent to tetravalent with lithium desorption. On the other hand, when there is fluorine, the cobalt ion changes from divalent to trivalent with lithium desorption. The redox potential of the cobalt ion is different between the two. Therefore, when part of the oxygen is replaced by fluorine in the surface layer portion 100a and the inner wall surface layer portion 100c of the positive electrode active material 100, it can be said that desorption and insertion of lithium ions near the fluorine can occur smoothly. Therefore, when the positive electrode active material 100 is used in a secondary battery, the charge / discharge characteristics, large current characteristics, etc. can be improved. In addition, the presence of fluorine in the surface layer portion 100a and the inner wall surface layer portion 100c, which have a surface that is in contact with the electrolyte, or the attachment of fluoride to the surface, can suppress excessive reaction between the positive electrode active material 100 and the electrolyte, and can effectively improve corrosion resistance to hydrofluoric acid.

[0085] In addition, when the melting point of the fluoride, such as lithium fluoride, is lower than that of the other additive element sources, it can function as a flux (also called a fluxing agent) that lowers the melting point of the other additive element sources. When the fluoride contains LiF and MgF2, since the eutectic point of LiF and MgF2 is around 742°C, it is preferable to set the heating temperature to 742°C or higher in the heating step after mixing the additive elements.

[0086] <Method of producing positive electrode active material> An example of a method for manufacturing the positive electrode active material 100 of one embodiment of the present invention will be described with reference to FIGS.

[0087] The method of adding the additive element is important for producing the positive electrode active material 100 having the distribution of the additive element as described in Figures 1 and 2. A specific example of a method for producing the positive electrode active material 100 having the distribution of the additive element as described in Figures 1 and 2 is shown below.

[0088] [Method 1 for preparing positive electrode active material] As an example of the positive electrode active material 100 having the distribution of the additive elements described in Fig. 1(A), Fig. 2(A) and Fig. 2(B), a method for producing the positive electrode active material 100A will be described. The positive electrode active material 100A is a lithium cobalt oxide having either or both of nickel and titanium as additive elements for improving electrical conductivity in the surface layer portion 100a, and aluminum as an additive element for stabilizing the crystal structure. The positive electrode active material 100A is a lithium cobalt oxide having aluminum as an additive element for stabilizing the crystal structure in the inner wall surface layer portion 100c of the crack portion 106, and substantially no nickel or titanium as additive elements for improving electrical conductivity.

[0089] As an example of a method for producing the positive electrode active material 100A, a method for producing the positive electrode active material 100A-1 will be described with reference to FIGS.

[0090] <Step S11> In step S11 shown in FIG. 3, a lithium source (Li source) and a cobalt source (Co source) are prepared as starting materials, that is, lithium and transition metal materials, respectively.

[0091] As the lithium source, it is preferable to use a compound containing lithium, such as lithium carbonate, lithium hydroxide, lithium nitrate, lithium fluoride, etc. It is preferable that the lithium source has high purity, and for example, it is preferable to use a material with a purity of 99.99% or more.

[0092] As the cobalt source, it is preferable to use a compound containing cobalt, for example, cobalt oxide such as tricobalt tetroxide, cobalt hydroxide, or the like.

[0093] The cobalt source is preferably of high purity, for example, a material with a purity of 3N (99.9%) or more, preferably 4N (99.99%) or more, more preferably 4N5 (99.995%) or more, and even more preferably 5N (99.999%) or more may be used. By using a material of high purity, impurities in the positive electrode active material can be controlled. As a result, the capacity of the secondary battery is increased and / or the reliability of the secondary battery is improved.

[0094] In addition, it is preferable that the cobalt source has high crystallinity, for example, single crystal grains. The crystallinity of the cobalt source can be evaluated using TEM images, STEM images, HAADF-STEM (high angle annular dark-field scanning transmission electron microscope) images, ABF-STEM (annular bright-field scanning transmission electron microscope) images, etc., or by X-ray diffraction (XRD), electron beam diffraction, neutron beam diffraction, etc. The above-mentioned methods for evaluating crystallinity can be applied not only to the evaluation of cobalt sources, but also to the evaluation of other crystallinity.

[0095] <Step S12> Next, in step S12 shown in FIG. 3, the lithium source and the cobalt source are pulverized and mixed to prepare a mixed material. The pulverization and mixing can be performed in a dry or wet manner. The wet method is preferable because it can be crushed into smaller pieces. When performing the wet method, a solvent is prepared. As the solvent, ketones such as acetone, alcohols such as ethanol and isopropanol, ether, dioxane, acetonitrile, N-methyl-2-pyrrolidone (NMP), etc. can be used. It is more preferable to use an aprotic solvent that does not easily react with lithium. In the method 1 for preparing the positive electrode active material, dehydrated acetone with a purity of 99.5% or more is used. It is preferable to mix the lithium source and the cobalt source in dehydrated acetone with a purity of 99.5% or more, in which the moisture content is suppressed to 10 ppm or less, and then pulverize and mix. By using dehydrated acetone with the above-mentioned purity, it is possible to reduce impurities that may be mixed in.

[0096] A ball mill, a bead mill, or the like can be used as a means for pulverization and mixing. When using a ball mill, aluminum oxide balls or zirconium oxide balls are preferably used as pulverization media. Zirconium oxide balls are preferred because they emit less impurities. When using a ball mill, a bead mill, or the like, the peripheral speed is preferably set to 100 mm / s or more and 2000 mm / s or less in order to suppress contamination from the media. In the positive electrode active material preparation method 1, the peripheral speed is set to 838 mm / s (rotation speed 400 rpm, ball mill diameter 40 mm).

[0097] <Step S13> Next, in step S13 shown in FIG. 3, the mixed material is heated. The heating is preferably performed at 800°C or more and 1100°C or less, more preferably at 900°C or more and 1000°C or less, and even more preferably at about 950°C. If the temperature is too low, the decomposition and melting of the lithium source and the cobalt source may be insufficient. On the other hand, if the temperature is too high, defects may occur due to lithium transpiration from the lithium source and / or cobalt being excessively reduced. For example, cobalt may change from trivalent to divalent, inducing oxygen defects, etc.

[0098] If the heating time is too short, lithium cobalt oxide will not be synthesized, but if it is too long, productivity will decrease. For example, the heating time is preferably 1 hour or more and 100 hours or less, and more preferably 2 hours or more and 20 hours or less.

[0099] The rate of temperature rise depends on the heating temperature reached, but it is recommended to set it to between 80°C / h and 250°C / h. For example, if heating at 1000°C for 10 hours, the rate of temperature rise should be 200°C / h.

[0100] The heating is preferably performed in an atmosphere with little water, such as dry air, for example, an atmosphere with a dew point of -50° C. or less, more preferably an atmosphere with a dew point of -80° C. or less. In the method 1 for producing a positive electrode active material, the heating is performed in an atmosphere with a dew point of -93° C. In order to suppress impurities that may be mixed into the material, the impurity concentrations of CH4, CO, CO2, and H2 in the heating atmosphere should each be 5 ppb (parts per billion) or less.

[0101] The heating atmosphere is preferably an atmosphere containing oxygen. For example, there is a method of continuously introducing dry air into the reaction chamber. In this case, the flow rate of the dry air is preferably 10 L / min. The method of continuously introducing oxygen into the reaction chamber and having oxygen flow through the reaction chamber is called flow.

[0102] When the heating atmosphere is an atmosphere containing oxygen, a method that does not allow oxygen to flow may be used. For example, the reaction chamber may be depressurized and then filled with oxygen (or purged) to prevent the oxygen from entering or leaving the reaction chamber. For example, the reaction chamber may be depressurized to -970 hPa and then filled with oxygen to 50 hPa.

[0103] After heating, the material may be naturally cooled, but it is preferable that the time required for the material to cool from the specified temperature to room temperature is within a range of 10 to 50 hours. However, cooling to room temperature is not always necessary, and it is sufficient to cool the material to a temperature that is acceptable for the next step.

[0104] The heating in this step may be performed using a rotary kiln or a roller hearth kiln. Heating using a rotary kiln may be performed while stirring in either a continuous or batch type.

[0105] The crucible used for heating is preferably an aluminum oxide crucible. An aluminum oxide crucible is a material that does not easily release impurities. In the positive electrode active material production method 1, an aluminum oxide crucible with a purity of 99.9% is used. It is preferable to place a lid on the crucible when heating. This can prevent the material from volatilizing.

[0106] In addition, it is preferable to use a crucible that has been used multiple times rather than a new one. In this specification, a new crucible refers to one that has undergone the process of putting in and heating materials containing lithium, transition metal M, and / or additive elements two or less times. In addition, a crucible that has been used multiple times refers to one that has undergone the process of putting in and heating materials containing lithium, transition metal M, and / or additive elements three or more times. This is because when a new crucible is used, there is a risk that some of the materials, including lithium fluoride, may be absorbed, diffused, moved, and / or attached to the sheath during heating. If some of the materials are lost due to these reasons, there is a growing concern that the distribution of elements in the surface layer of the positive electrode active material will not be within a preferred range. On the other hand, this risk is less likely with a crucible that has been used multiple times.

[0107] After the heating is completed, the material may be crushed and sieved as necessary. When recovering the heated material, the material may be transferred from the crucible to a mortar and then recovered. It is preferable to use an aluminum oxide mortar for the mortar. The aluminum oxide mortar is made of a material that does not easily release impurities. Specifically, an aluminum oxide mortar with a purity of 90% or more, preferably 99% or more, is used. Note that the same heating conditions as those in step S13 can be applied to the heating steps described below other than step S13.

[0108] <Step S14> By the above process, lithium cobalt oxide (LCO) can be synthesized as shown in step S14 in FIG.

[0109] <Step S15> Next, the lithium cobalt oxide is heated in step S15 shown in Fig. 3. Since this is the first heating of the lithium cobalt oxide, the heating in step S15 may be called initial heating. Or, since it is heating before step S33 described below, it may be called preheating or pretreatment.

[0110] As described above, the initial heating causes lithium to be desorbed from a part of the surface layer 100a of the lithium cobalt oxide. It is also expected to have the effect of increasing the crystallinity of the interior 100b. The lithium source and / or cobalt source prepared in step S11 etc. may contain impurities. The initial heating makes it possible to reduce the impurities in the lithium cobalt oxide completed in step S14.

[0111] Furthermore, the initial heating has the effect of smoothing the surface of the lithium cobalt oxide. A smooth surface means that there are few irregularities, the composite oxide is generally rounded, and the corners are rounded. Furthermore, a state in which there is little foreign matter adhering to the surface is called smooth. Foreign matter is thought to be the cause of irregularities, so it is preferable that it does not adhere to the surface.

[0112] For this initial heating, it is not necessary to prepare a lithium source, a source of an additive element, or a material that functions as a flux.

[0113] If the heating time of this step is too short, sufficient effect is not obtained, but if it is too long, productivity decreases. For example, the heating conditions can be selected from those described in step S13. In addition to the heating conditions, the heating temperature of this step should be lower than the temperature of step S13 in order to maintain the crystal structure of the complex oxide. Furthermore, the heating time of this step should be shorter than the time of step S13 in order to maintain the crystal structure of the complex oxide. For example, heating should be performed at a temperature of 700°C to 1000°C for 2 hours to 20 hours.

[0114] The effect of enhancing the crystallinity of the inner portion 100b is, for example, the effect of mitigating distortion, displacement, and the like resulting from a shrinkage difference or the like possessed by the lithium cobalt oxide produced in step S13.

[0115] The heating in step S13 may cause a temperature difference between the surface and the inside of the lithium cobalt oxide. The temperature difference may induce a shrinkage difference. It is also considered that the temperature difference causes the shrinkage difference because the fluidity of the surface and the inside is different. The energy related to the shrinkage difference gives the lithium cobalt oxide a difference in internal stress. The internal stress difference is also called strain, and the energy is sometimes called strain energy. The internal stress is removed by the initial heating in step S15, or in other words, the strain energy is considered to be homogenized by the initial heating in step S15. When the strain energy is homogenized, the strain of the lithium cobalt oxide is relaxed. As a result, the surface of the lithium cobalt oxide may become smooth. This is also called the surface being improved. In other words, it is considered that the shrinkage difference caused in the lithium cobalt oxide is relaxed after step S15, and the surface of the composite oxide becomes smooth.

[0116] Furthermore, the shrinkage difference may cause microscopic deviations, such as crystal deviations, in the lithium cobalt oxide. In order to reduce such deviations, it is advisable to carry out this step. Through this step, it is possible to equalize the deviations in the composite oxide. When the deviations are equalized, the surface of the composite oxide may become smooth. This is also referred to as the alignment of crystal grains. In other words, it is believed that through step S15, deviations of crystals and the like that have occurred in the composite oxide are alleviated, and the surface of the composite oxide becomes smooth.

[0117] When lithium cobalt oxide, which has a smooth surface, is used as the positive electrode active material, deterioration during charging and discharging as a secondary battery is reduced and cracking of the positive electrode active material can be prevented.

[0118] Note that lithium cobalt oxide synthesized in advance may be used in step S14. In this case, steps S11 to S13 can be omitted. By carrying out step S15 on lithium cobalt oxide synthesized in advance, lithium cobalt oxide with a smooth surface can be obtained.

[0119] Next, as shown in steps S21 to S53, it is preferable to add an additive element to the lithium cobalt oxide. In the method for producing a positive electrode active material described in the positive electrode active material production method 1, the additive element is added in a plurality of steps, so that the additive element added first in the flow shown in Fig. 3 is described as A1, and the additive element added second time is described as A2. The steps for preparing a source of the additive element A1 used for adding the additive element A1 will be described using steps S21 to S23.

[0120] <Step S21> 3, a source of an additive element A1 (A1 source) to be added to lithium cobalt oxide is prepared. A lithium source may be prepared together with the A1 source.

[0121] As the additional element A1, one or more elements selected from magnesium, fluorine, zirconium, iron, manganese, chromium, arsenic, zinc, silicon, sulfur, phosphorus, boron, bromine, and beryllium can be used.

[0122] When magnesium is selected as the additive element, the source of the additive element can be called a magnesium source (Mg source). As the magnesium source, magnesium fluoride, magnesium oxide, magnesium hydroxide, magnesium carbonate, etc. can be used. In addition, a plurality of the above-mentioned magnesium sources may be used.

[0123] When fluorine is selected as the additive element, the additive element source can be called a fluorine source (F source). As the fluorine source, for example, lithium fluoride (LiF), magnesium fluoride (MgF2), aluminum fluoride (AlF3), zirconium fluoride (ZrF4), vanadium fluoride (VF5), manganese fluoride, iron fluoride, chromium fluoride, niobium fluoride, zinc fluoride (ZnF2), calcium fluoride (CaF2), sodium fluoride (NaF), potassium fluoride (KF), barium fluoride (BaF2), cerium fluoride (CeF3, CeF4), lanthanum fluoride (LaF3), or sodium aluminum hexafluoride (Na3AlF6) can be used. Among them, lithium fluoride is preferable because it has a relatively low melting point of 848°C and is easily melted in the heating process described below.

[0124] Magnesium fluoride can be used as both the fluorine source and the magnesium source, and lithium fluoride can be used as the lithium source. Another lithium source that can be used in step S21 is lithium carbonate.

[0125] The fluorine source may be a gas, such as fluorine (F2), carbon fluoride, sulfur fluoride, oxygen fluoride (OF2, O2F2, O3F2, O4F2, O5F2, O6F2, O2F), or nitrogen trifluoride (NF3), which may be mixed into the atmosphere in the heating step described below. A plurality of the above-mentioned fluorine sources may be used.

[0126] In the method 1 for preparing the positive electrode active material described in FIG. 3, magnesium and fluorine are used as the additive element A1. Lithium fluoride (LiF) is prepared as the fluorine source, and magnesium fluoride (MgF2) is prepared as the fluorine source and magnesium source. When lithium fluoride and magnesium fluoride are mixed at about LiF:MgF2=65:35 (molar ratio), the effect of lowering the melting point is maximized. On the other hand, if the amount of lithium fluoride is large, there is a concern that the lithium becomes excessive and the cycle characteristics deteriorate. Therefore, the molar ratio of lithium fluoride and magnesium fluoride is preferably LiF:MgF2=x:1 (0≦x≦1.9), more preferably LiF:MgF2=x:1 (0.1≦x≦0.5), and even more preferably LiF:MgF2=x:1 (x=0.33 or nearby). In this specification, etc., the term "nearby" refers to a value that is greater than 0.9 times and less than 1.1 times the value.

[0127] <Step S22> Next, in step S22 shown in Fig. 3, the magnesium source and the fluorine source are pulverized and mixed. This step can be carried out under conditions selected from the pulverization and mixing conditions described in step S12.

[0128] <Step S23> Next, in step S23 shown in Fig. 3, the above-mentioned crushed and mixed materials are collected to obtain the A1 source. Note that the A1 source shown in step S23 has a plurality of starting materials and can be called a mixture.

[0129] The particle size of the mixture is preferably D50 (median diameter) 600 nm to 10 μm, more preferably 1 μm to 5 μm. Even when a single material is used as the additive element source, the D50 (median diameter) is preferably 600 nm to 10 μm, more preferably 1 μm to 5 μm.

[0130] When such a finely powdered mixture (including the case where only one kind of additive element is included) is mixed with lithium cobalt oxide in a later step, the mixture can be easily attached uniformly to the surface of the lithium cobalt oxide particles. If the mixture is attached uniformly to the surface of the lithium cobalt oxide particles, it is preferable because the additive element can be easily distributed or diffused uniformly in the surface layer portion 100a of the composite oxide after heating.

[0131] <Step S31> 3, lithium cobalt oxide and the Al source are mixed together. The ratio of the number of cobalt atoms Co in the lithium cobalt oxide to the number of magnesium atoms Mg in the Al source is preferably Co:Mg=100:y (0.1≦y≦6), and more preferably M:Mg=100:y (0.3≦y≦3).

[0132] The mixing in step S31 is preferably performed under milder conditions than the mixing in step S12 in order not to destroy the shape of the lithium cobalt oxide particles. For example, the mixing is preferably performed under conditions of a lower rotation speed or shorter time than in step S12. It can also be said that the dry method is a milder condition than the wet method. For example, a ball mill, a bead mill, etc. can be used for mixing. When using a ball mill, it is preferable to use zirconium oxide balls as the media.

[0133] In the positive electrode active material preparation method 1, the materials are mixed in a ball mill using zirconium oxide balls with a diameter of 1 mm at 150 rpm for 1 hour in a dry room with a dew point of -100°C or higher and -10°C or lower.

[0134] <Step S32> 3, the mixed material is collected to obtain a mixture 901. When collecting the material, it may be crushed and then sieved, if necessary.

[0135] <Step S33> Next, in step S33 shown in FIG. 3, the mixture 901 is heated. The heating conditions can be selected from those described in step S13. The heating time is preferably 2 hours or more. At this time, the pressure inside the furnace may be higher than atmospheric pressure in order to increase the oxygen partial pressure of the heating atmosphere. This is because if the oxygen partial pressure of the heating atmosphere is insufficient, cobalt, etc. will be reduced, and lithium cobalt oxide, etc. may not be able to maintain the layered rock salt type crystal structure.

[0136] Here, a supplementary note on the heating temperature will be provided. The lower limit of the heating temperature in step S33 must be equal to or higher than the temperature at which the reaction between the lithium cobalt oxide and the additive element source proceeds. The temperature at which the reaction proceeds may be any temperature at which interdiffusion of elements contained in the lithium cobalt oxide and the additive element source occurs, and may be lower than the melting temperatures of these materials. An oxide will be used as an example to explain the melting temperature T m 0.757 times (Tammann temperature T d ) solid-phase diffusion occurs. Therefore, the heating temperature in step S33 should be 650° C. or higher.

[0137] Of course, the reaction proceeds more easily if the temperature is equal to or higher than the melting temperature of one or more of the materials contained in the mixture 901. For example, when LiF and MgF2 are contained as the additive element source, the eutectic point of LiF and MgF2 is around 742°C, so that the lower limit of the heating temperature in step S33 is preferably set to 742°C or higher.

[0138] In addition, a mixture 903 obtained by mixing LiCoO2:LiF:MgF2=100:0.33:1 (molar ratio) shows an endothermic peak at about 830° C. in differential scanning calorimetry (DSC measurement). Therefore, the lower limit of the heating temperature is more preferably 830° C. or higher.

[0139] A higher heating temperature is preferable because the reaction proceeds more easily, the heating time is shorter, and the productivity is high.

[0140] The upper limit of the heating temperature is set to be lower than the decomposition temperature (1130°C) of lithium cobalt oxide. At temperatures close to the decomposition temperature, there is a concern that lithium cobalt oxide may decompose, albeit in a small amount. Therefore, the temperature is preferably 1000°C or lower, more preferably 950°C or lower, and even more preferably 900°C or lower.

[0141] Considering these, the heating temperature in step S33 is preferably 650°C to 1130°C, more preferably 650°C to 1000°C, even more preferably 650°C to 950°C, and even more preferably 650°C to 900°C. Also, it is preferably 742°C to 1130°C, more preferably 742°C to 1000°C, even more preferably 742°C to 950°C, and even more preferably 742°C to 900°C. Also, it is preferably 800°C to 1100°C, 830°C to 1130°C, more preferably 830°C to 1000°C, even more preferably 830°C to 950°C, and even more preferably 830°C to 900°C. The heating temperature in step S33 is preferably higher than that in step S13.

[0142] Furthermore, when the mixture 901 is heated, it is preferable to control the partial pressure of fluorine or fluoride resulting from the fluorine source or the like within an appropriate range.

[0143] In the preparation method described in Preparation Method 1 of the Positive Electrode Active Material, some materials, for example LiF, which is a fluorine source, may function as a flux. This function allows the heating temperature to be lowered below the decomposition temperature of lithium cobalt oxide, for example, to between 742°C and 950°C, and additive elements such as magnesium can be distributed in the surface layer to prepare a positive electrode active material with good characteristics.

[0144] However, since LiF has a lower specific gravity in a gaseous state than oxygen, LiF may volatilize or sublime when heated, and if it volatilizes, the amount of LiF in the mixture 903 will decrease. This weakens its function as a flux. Therefore, it is necessary to heat while suppressing the volatilization of LiF. Even if LiF is not used as a fluorine source, etc., Li on the LiCoO2 surface may react with F of the fluorine source to produce LiF, which may then volatilize. Therefore, even if a fluoride with a higher melting point than LiF is used, it is necessary to suppress the volatilization in the same way.

[0145] Therefore, it is preferable to heat the mixture 901 in an atmosphere containing LiF, that is, to heat the mixture 901 in a state where the partial pressure of LiF is high in the heating furnace. By such heating, the volatilization of LiF in the mixture 901 can be suppressed.

[0146] The heating in this step is preferably performed so as not to cause adhesion between particles of the mixture 901. If the particles of the mixture 901 adhere to each other during heating, the contact area with oxygen in the atmosphere decreases, and the route along which the additive element (e.g., fluorine) diffuses is blocked, which may result in poor distribution of the additive element (e.g., magnesium and fluorine) in the surface layer.

[0147] It is also believed that if an additive element (e.g., fluorine) is uniformly distributed in the surface layer, a smooth positive electrode active material with few irregularities can be obtained. Therefore, in order to maintain the smooth surface or to make it even smoother after the heating in step S15 in this process, it is better for the particles of mixture 901 not to stick together.

[0148] In addition, when heating is performed using a rotary kiln, it is preferable to control the flow rate of the oxygen-containing atmosphere in the kiln. For example, it is preferable to reduce the flow rate of the oxygen-containing atmosphere, or to first purge the atmosphere and not flow the atmosphere after introducing the oxygen atmosphere into the kiln. If oxygen is flowed, the fluorine source may evaporate, which is not preferable in terms of maintaining the smoothness of the surface.

[0149] When heating is performed using a roller hearth kiln, the mixture 901 can be heated in an atmosphere containing LiF, for example, by placing a lid on a container containing the mixture 901.

[0150] Regarding the heating time, the heating time varies depending on conditions such as the heating temperature, the size and composition of the lithium cobalt oxide in step S14, etc. When the lithium cobalt oxide is small, a lower temperature or a shorter heating time may be more preferable than when the lithium cobalt oxide is large.

[0151] When the median diameter (D50) of the lithium cobalt oxide in step S14 of Fig. 3 is about 12 µm, the heating temperature is preferably, for example, 650°C or more and 950°C or less. The heating time is preferably, for example, 3 hours or more and 60 hours or less, more preferably 10 hours or more and 30 hours or less, and further preferably about 20 hours. The temperature reduction time after heating is preferably, for example, 10 hours or more and 50 hours or less.

[0152] On the other hand, when the median diameter (D50) of the lithium cobalt oxide in step S14 is about 7 μm, the heating temperature is preferably, for example, 650° C. to 950° C. The heating time is preferably, for example, 1 hour to 10 hours, more preferably about 5 hours. The cooling time after heating is preferably, for example, 10 hours to 50 hours.

[0153] <Step S34> Next, in step S34 shown in FIG. 3, the heated material is recovered and crushed as necessary to obtain composite oxide 902.

[0154] Next, an additive element A2 source (A2 source) is added in steps S41 to S53 shown in Fig. 3. The steps of preparing the A2 source used to add the additive element A2 will be described with reference to steps S41 to S43.

[0155] As the additive element A2, the additive element for improving the electrical conductivity and the additive element for stabilizing the crystal structure described in [Additive element] are used. In the method 1 for producing the positive electrode active material described in Fig. 3, nickel is used as the additive element for improving the electrical conductivity, and aluminum is used as the additive element for stabilizing the crystal structure.

[0156] As the additive element source used for adding the additive element, the additive element source used for adding the additive element that improves the electrical conductivity is preferably solid. Also, the additive element source used for adding the additive element that stabilizes the crystal structure is preferably liquid. That is, in the manufacturing method 1 of the positive electrode active material described in FIG. 3, the nickel source (Ni source) used for adding nickel is preferably solid, and the aluminum source (Al source) used for adding aluminum is preferably liquid.

[0157] 1A to 2B, in the positive electrode active material 100 of one embodiment of the present invention, the distribution of the added element is different between the surface layer portion 100a and the inner wall surface layer portion 100c of the crack portion 106. In order to manufacture the positive electrode active material 100 having such characteristics, for example, as the nickel source (Ni source), a nickel source 91 having a shape that can be in contact with the surface of the composite oxide 902 and cannot be in contact with the inner wall surface of the crack portion 106, as shown in FIG.

[0158] In other words, the opening width W of the crack portion 106A of the composite oxide 902, which becomes the crack portion 106 after the preparation of the positive electrode active material 100, is C The particle diameter W of the nickel source 91 is N It is preferable to use a solid material containing nickel, which has a large resistance.

[0159] 4(B), the aluminum source (Al source) 92 may be an aluminum source 92 that can contact the surface of the composite oxide 902 and can contact the inner wall surface of the crack portion 106. In other words, a liquid material containing aluminum may be used.

[0160] In the positive electrode active material preparation method 1 described in FIG. 3, nickel and aluminum are added in the same step, so that the nickel source 91 and the aluminum source 92 are preferably in contact with the composite oxide 902, for example, in a state as shown in FIG. 5.

[0161] <Step S41> As described above, in step S41, a liquid aluminum source (Al source) and a solid nickel source (Ni source) are prepared.

[0162] As the liquid aluminum source, liquid materials such as an aluminum alkoxide solution, an aluminum acetylacetonate solution, an aluminum lactate solution, an aluminum phthalocyanine solution, or the like can be used.

[0163] As the aluminum alkoxide contained in the aluminum alkoxide solution, aluminum isopropoxide, trimethoxyaluminum, triethoxyaluminum, tri-n-propoxyaluminum, tri-i-propoxyaluminum, tri-n-butoxyaluminum, tri-i-butoxyaluminum, tri-sec-butoxyaluminum, tri-t-butoxyaluminum, etc. can be used. As the solvent for dissolving the aluminum alkoxide, methanol, ethanol, propanol, 2-propanol, butanol, 2-butanol, etc. can be used. Although the alkoxide group of the aluminum alkoxide and the alcohol used as the solvent may be different in type, it is preferable that they are the same type.

[0164] As the solid nickel source, solid materials such as nickel oxide and nickel hydroxide can be used.

[0165] In the positive electrode active material preparation method 1 described with reference to FIG. 3, an aluminum isopropoxide solution in which aluminum isopropoxide is dissolved in isopropoxide is used as the aluminum source, and nickel hydroxide is used as the nickel source.

[0166] <Step S42> As shown in step S42 of FIG. 3, the nickel source can be pulverized to adjust the particle size of the nickel source. In addition, although not shown, the pulverized nickel source can be classified by a classifier to obtain a nickel source having a particle diameter of 1000 nm. C The nickel source having the following particle size may be removed. Note that the conditions for pulverizing the nickel source can refer to the conditions in step S12.

[0167] As described above, the size of the nickel source is set to the opening width W of the crack portion 106A of the composite oxide 902. C It is preferable that the average particle size of the nickel source is larger than 100 μm. Here, FIG. 6(A) is an SEM image showing an example of a crack in lithium cobalt oxide, and FIG. 6(B) is an SEM image showing an enlarged portion of FIG. 6(A). In FIG. 6(B), the portion indicated by the arrow is a crack, and the opening width of the crack is about 500 nm at the widest portion. On the other hand, if the particles of the nickel source are too large, the uniformity when adding nickel to the surface layer portion 100a may decrease. Therefore, the particle size of the nickel source is preferably 500 nm or more and 10 μm or less, more preferably 1 μm or more and 8 μm or less, and even more preferably 1 μm or more and 5 μm or less, in terms of D50 (median diameter) obtained by particle size distribution measurement.

[0168] Particle size can be measured by a particle size distribution meter (laser diffraction type particle size distribution measuring device) using the laser diffraction / scattering method. D50 is the particle size when the integrated amount in the integrated particle amount curve of the particle size distribution measurement result is 50%. D10 is the particle size when the integrated amount in the integrated particle amount curve of the particle size distribution measurement result is 10%. D90 is the particle size when the integrated amount in the integrated particle amount curve of the particle size distribution measurement result is 90%.

[0169] The measurement of particle size is not limited to laser diffraction particle size distribution measurement, and the major axis of the particle cross section may be measured by analysis such as SEM or TEM. For example, as a method for measuring D50 by analysis such as SEM or TEM, 20 or more particles are measured, an integrated particle amount curve is created, and the particle diameter when the integrated amount is 50% is taken as D50.

[0170] <Step S43> The above-mentioned liquid aluminum source and solid nickel source can be used as a source of the additional element A2 (A2 source).

[0171] <Step S51> 3, the composite oxide 902 and the A2 source are mixed to prepare a mixed solution. A stirrer or the like may be used for mixing.

[0172] <Step S52> When an aluminum isopropoxide solution is used as the aluminum source, the above mixture is stirred in an atmosphere containing water vapor. This treatment causes the H2O in the atmosphere and the aluminum isopropoxide to undergo hydrolysis and polycondensation reactions. Then, a gel-like layer containing aluminum is formed on the surface of the lithium cobalt oxide particles containing magnesium and fluorine.

[0173] Stirring can be performed, for example, with a magnetic stirrer. The stirring time may be long enough for the water in the atmosphere and the aluminum isopropoxide to undergo hydrolysis and polycondensation reactions, and may be performed, for example, for 4 hours at 25°C and 90% RH (relative humidity).

[0174] <Step S53> The precipitate is collected from the mixed solution after the above treatment. The collection method can be filtration, centrifugation, drying, etc. In the positive electrode active material production method 1, the precipitate is collected by filtration. A paper filter is used for filtration, and the residue is washed with the same alcohol as the solvent in which the aluminum alkoxide was dissolved.

[0175] <Step S54> Next, the collected residue is dried. In the positive electrode active material preparation method 1, the residue is dried in vacuum at 70° C. for 1 hour.

[0176] <Step S55> 3, the dried material is collected to obtain a mixture 903. When collected, the material may be crushed and then sieved, if necessary.

[0177] <Step S56> 3, the mixture 903 is heated. The description of step S33 can be referred to for the heating conditions, and for example, the mixture may be heated at 850° C. for 10 hours in an oxygen-containing atmosphere.

[0178] <Step S57> Next, in step S57 shown in FIG. 3, the heated material is collected and crushed as necessary to obtain the positive electrode active material 100A-1. At this time, it is preferable to further sieve the collected particles. Through the above steps, the positive electrode active material 100A-1, which is an example of the positive electrode active material 100 of one embodiment of the present invention, can be produced. The positive electrode active material 100A-1 can be said to be lithium cobalt oxide having aluminum and nickel on the surface layer portion 100a and aluminum on the inner wall surface layer portion 100c of the crack portion 106. The positive electrode active material 100A-1 can also be said to be lithium cobalt oxide having magnesium, aluminum, and nickel on the surface layer portion 100a and magnesium and aluminum on the inner wall surface layer portion 100c of the crack portion 106.

[0179] Positive electrode active material 100A-1 according to one embodiment of the present invention has a smooth surface, and may be more resistant to physical shocks such as those caused by pressure than positive electrode active materials that do not have a smooth surface.

[0180] [Method 2 for preparing positive electrode active material] A method for producing a positive electrode active material 100A-2 will be described as an example of the positive electrode active material 100A, which is different from the positive electrode active material 100A-1 described above. The method for producing the positive electrode active material 100A-2 will be described with reference to FIG.

[0181] The manufacturing method shown in Fig. 7 is the same as the manufacturing method shown in Fig. 3 except for the steps S41 to S43. The steps S41 to S43 will be described below.

[0182] In the positive electrode active material preparation method 2 described in FIG. 7, titanium and aluminum are added in the same process, so that the titanium source (Ti source) and the aluminum source (Al source) may be brought into contact with the composite oxide 902 under conditions in which the nickel source 91 in FIG. 5 is replaced with the titanium source, for example.

[0183] <Step S41> In the second method for producing a positive electrode active material described with reference to FIG. 7, in step S41, a liquid aluminum source (Al source) and a solid titanium source (Ti source) are prepared.

[0184] As the solid titanium source, a solid material such as lithium titanate, titanium oxide, titanium hydroxide, etc. can be used.

[0185] As the liquid aluminum source, the liquid material described in the description of step S41 in FIG. 3 can be used.

[0186] In the second method for producing a positive electrode active material described in FIG. 7, an aluminum isopropoxide solution in which aluminum isopropoxide is dissolved in isopropoxide is used as the aluminum source, and lithium titanate is used as the titanium source.

[0187] <Step S42> As shown in step S42 of FIG. 7, the titanium source can be pulverized to adjust the particle size of the titanium source. In addition, although not shown, the pulverized titanium source can be classified by a classifier to obtain a titanium source having a particle diameter of 1000 nm. C The titanium source particles having the following particle sizes may be removed. Note that the conditions for pulverizing the titanium source can be referred to as the conditions for step S12 in FIG.

[0188] The particle size of the titanium source is preferably such that D50 (median diameter) obtained by particle size distribution measurement is 500 nm or more and 10 μm or less, more preferably 1 μm or more and 8 μm or less, and even more preferably 1 μm or more and 5 μm or less.

[0189] <Step S43> The above-mentioned liquid aluminum source and solid titanium source can be used as a source of the additional element A2 (A2 source).

[0190] 7, the positive electrode active material 100A-2 can be obtained in step S57. The positive electrode active material 100A-2 can be referred to as lithium cobalt oxide having aluminum and titanium in the surface layer portion 100a and having aluminum in the inner wall surface layer portion 100c of the crack portion 106. The positive electrode active material 100A-2 can be referred to as lithium cobalt oxide having magnesium, aluminum, and titanium in the surface layer portion 100a and having magnesium and aluminum in the inner wall surface layer portion 100c of the crack portion 106.

[0191] [Method 3 for preparing positive electrode active material] A method for producing a positive electrode active material 100A-3 will be described as an example of a positive electrode active material 100A different from the above-described positive electrode active material 100A-1 etc. The method for producing the positive electrode active material 100A-3 will be described with reference to FIG.

[0192] The manufacturing method shown in Fig. 8 is the same as the manufacturing method shown in Fig. 3 except for the steps S41 to S43. The steps S41 to S43 will be described below.

[0193] In the positive electrode active material preparation method 3 described in FIG. 8, nickel, titanium, and aluminum are added in the same step. Therefore, the nickel source (Ni source), titanium source (Ti source), and aluminum source (Al source) may be in contact with the composite oxide 902 under conditions in which, for example, some of the particles of the nickel source 91 in FIG. 5 are replaced with the titanium source.

[0194] <Step S41> In the third method for producing a positive electrode active material described with reference to FIG. 8, in step S41, a liquid aluminum source (Al source), a solid nickel source (Ni source), and a solid titanium source (Ti source) are prepared.

[0195] As the solid nickel source, the solid material shown in the description of step S41 in Fig. 3 can be used. As the solid titanium source, the solid material shown in the description of step S41 in Fig. 7 can be used.

[0196] As the liquid aluminum source, the liquid material described in the description of step S41 in FIG. 3 can be used.

[0197] In the method 2 for preparing a positive electrode active material described in FIG. 7, an aluminum isopropoxide solution in which aluminum isopropoxide is dissolved in a solvent, isopropoxide, is used as the aluminum source, nickel hydroxide is used as the nickel source, and lithium titanate is used as the titanium source.

[0198] <Step S42> As shown in step S42 of FIG. 7, the nickel source and the titanium source can be pulverized to adjust the particle size of the nickel source and the titanium source. In addition, although not shown, the pulverized nickel source and the titanium source can be classified by a classifier to obtain a W C The nickel source and titanium source having the following particle sizes may be removed. Note that the conditions for pulverizing the nickel source and titanium source can refer to the conditions in step S12 in FIG.

[0199] <Step S43> The above-mentioned liquid aluminum source, solid nickel source, and solid titanium source can be used as a source of the additional element A2 (A2 source).

[0200] By such a preparation method, the positive electrode active material 100A-3 can be obtained in step S57 of Fig. 8. The positive electrode active material 100A-3 can be said to be lithium cobalt oxide having aluminum, nickel, and titanium in the surface layer portion 100a, and having aluminum in the inner wall surface layer portion 100c of the crack portion 106. The positive electrode active material 100A-3 can also be said to be lithium cobalt oxide having magnesium, aluminum, nickel, and titanium in the surface layer portion 100a, and having magnesium and aluminum in the inner wall surface layer portion 100c of the crack portion 106.

[0201] [Method 4 for preparing positive electrode active material] A method for producing a positive electrode active material 100A-4 will be described as an example of a positive electrode active material 100A different from the above-described positive electrode active material 100A-1 etc. The method for producing the positive electrode active material 100A-4 will be described with reference to FIG.

[0202] The production method shown in Fig. 9 is the same as the production method shown in Fig. 3, except that step S15 is not performed. Thus, in producing positive electrode active material 100A, the initial heating in step S15 does not necessarily have to be performed.

[0203] By such a preparation method, the positive electrode active material 100A-4 can be obtained in step S57 of Fig. 9. The positive electrode active material 100A-4 can be said to be lithium cobalt oxide having aluminum and nickel in the surface layer portion 100a and having aluminum in the inner wall surface layer portion 100c of the crack portion 106. The positive electrode active material 100A-4 can be said to be lithium cobalt oxide having magnesium, aluminum, and nickel in the surface layer portion 100a and having magnesium and aluminum in the inner wall surface layer portion 100c of the crack portion 106.

[0204] Although not shown, similarly to the above, the method for producing positive electrode active material 100A-2 described in Fig. 7 may be modified so as to not perform step S15. Similarly, the method for producing positive electrode active material 100A-3 described in Fig. 8 may be modified so as to not perform step S15.

[0205] [Method 5 for preparing positive electrode active material] A method for producing a positive electrode active material 100A-5 will be described as an example of a positive electrode active material 100A different from the above-described positive electrode active material 100A-1 etc. The method for producing the positive electrode active material 100A-5 will be described with reference to FIG.

[0206] The preparation method shown in Fig. 10 is the same as the preparation method shown in Fig. 3 except that steps S15 to S34 are not performed. In this manner, in preparation of the positive electrode active material 100A, the initial heating in step S15 does not necessarily have to be performed. In addition, in preparation of the positive electrode active material 100A, the addition of the additive element A1 does not necessarily have to be performed.

[0207] In the method for producing the positive electrode active material 100A-5 shown in FIG. 10, in the mixing in step S51, LiCoO2 in step S14 and a source of the additive element A2 are mixed.

[0208] By such a production method, the positive electrode active material 100A-5 can be obtained in step S57 of Fig. 10. The positive electrode active material 100A-5 can be said to be lithium cobalt oxide having aluminum and nickel in the surface layer portion 100a and having aluminum in the inner wall surface layer portion 100c of the crack portion 106.

[0209] Although not shown, similarly to the above, the method for producing the positive electrode active material 100A-2 described in Fig. 7 may be a method for producing the positive electrode active material 100A-2 without performing steps S15 to S34. Similarly, the method for producing the positive electrode active material 100A-3 described in Fig. 8 may be a method for producing the positive electrode active material 100A-3 without performing steps S15 to S34.

[0210] [Method 6 for preparing positive electrode active material] As an example of the positive electrode active material 100 having the distribution of the additive elements described in Figures 1(A), 2(A), and 2(B), a method for producing the positive electrode active material 100B will be described. The positive electrode active material 100B is a lithium cobalt-nickel oxide (LCNO) having titanium as an additive element for improving electrical conductivity in the surface layer portion 100a and aluminum as an additive element for stabilizing the crystal structure. The positive electrode active material 100B is also a lithium cobalt-nickel oxide having aluminum as an additive element for stabilizing the crystal structure in the inner wall surface layer portion 100c of the crack portion 106 and substantially no titanium as an additive element for improving electrical conductivity.

[0211] As an example of a method for producing positive electrode active material 100B, a method for producing positive electrode active material 100B-1 will be described with reference to FIG.

[0212] The manufacturing method shown in Fig. 11 is the same as the manufacturing method shown in Fig. 11 except for the steps S11 to S14. The steps S11 to S14 will be described below.

[0213] <Step S11> In step S11 shown in FIG. 11, a lithium source (Li source), a cobalt source (Co source), and a nickel source (Ni source) are prepared as starting materials, ie, lithium and transition metal materials, respectively.

[0214] As the lithium source, the material described in step S11 of FIG. 3 may be used.

[0215] As the cobalt source, the material described in step S11 of FIG. 3 may be used.

[0216] As the nickel source, nickel oxide, nickel hydroxide, etc. can be used.

[0217] <Step S12> Next, in step S12 shown in Fig. 11, the lithium source, the cobalt source, and the nickel source are pulverized and mixed to prepare a mixed material. The pulverization and mixing method may be the same as that described in step S12 of Fig. 3.

[0218] The mixed amounts of the cobalt source and nickel source used as transition metal materials may be such that, when the total of the number of cobalt atoms in the cobalt source and the number of nickel atoms in the nickel source is taken as 100%, the number of nickel atoms in the nickel source is 5% to 25%. The number of nickel atoms in the nickel source is preferably 5% to 20%, more preferably 5% to 15%, and even more preferably 5% to 10%.

[0219] <Step S13> Next, the mixed material is heated in step S13 shown in Fig. 11. The heating conditions can be seen from the conditions in step S13 in Fig. 3.

[0220] <Step S14> By the above process, lithium cobalt-nickel oxide (LCNO) can be synthesized as shown in step S14 in FIG.

[0221] By such a preparation method, the positive electrode active material 100B-1 can be obtained in step S57 of Fig. 11. The positive electrode active material 100B-1 can be referred to as lithium cobalt-nickel oxide having aluminum and titanium on the surface layer portion 100a and having aluminum on the inner wall surface layer portion 100c of the crack portion 106. The positive electrode active material 100B-1 can also be referred to as lithium cobalt-nickel oxide having magnesium, aluminum, and titanium on the surface layer portion 100a and having magnesium and aluminum on the inner wall surface layer portion 100c of the crack portion 106.

[0222] [Method 7 for preparing positive electrode active material] A method for producing a positive electrode active material 100B-2, which is an example of the positive electrode active material 100B different from the positive electrode active material 100B-1 described above, will be described below. The method for producing the positive electrode active material 100B-2 will be described with reference to FIG.

[0223] The production method shown in Fig. 12 is the same as the production method shown in Fig. 11 except that step S15 is not performed. Thus, in producing positive electrode active material 100B, the initial heating in step S15 does not necessarily have to be performed.

[0224] By such a preparation method, the positive electrode active material 100B-2 can be obtained in step S57 of Fig. 12. The positive electrode active material 100B-2 can be referred to as lithium cobalt-nickel oxide having aluminum and titanium on the surface layer portion 100a and having aluminum on the inner wall surface layer portion 100c of the crack portion 106. The positive electrode active material 100B-2 can also be referred to as lithium cobalt-nickel oxide having magnesium, aluminum, and titanium on the surface layer portion 100a and having magnesium and aluminum on the inner wall surface layer portion 100c of the crack portion 106.

[0225] [Method 8 for preparing positive electrode active material] A method for producing a positive electrode active material 100B-3 will be described as an example of the positive electrode active material 100B, which is different from the above-described positive electrode active material 100B-1, etc. The method for producing the positive electrode active material 100B-3 will be described with reference to FIG.

[0226] The fabrication method shown in Fig. 13 is the same as the fabrication method shown in Fig. 11 except that steps S15 to S34 are not performed. In this manner, in fabricating the positive electrode active material 100B, the initial heating in step S15 does not necessarily have to be performed. Also, in fabricating the positive electrode active material 100B, the addition of the additive element A1 does not necessarily have to be performed.

[0227] In the method for producing the positive electrode active material 100B-3 shown in FIG. 13, in the mixing in step S51, LiCoO2 in step S14 and the source of the additive element A2 are mixed.

[0228] By such a production method, positive electrode active material 100B-3 can be obtained in step S57 of Fig. 13. Positive electrode active material 100B-3 can be said to be lithium cobalt-nickel oxide having aluminum and titanium in surface layer portion 100a and aluminum in inner wall surface layer portion 100c of crack portion 106.

[0229] [Method 9 for preparing positive electrode active material] As an example of the positive electrode active material 100 having the distribution of the additive elements described in Fig. 1(A), Fig. 2(A) and Fig. 2(B), a method for producing the positive electrode active material 100C will be described. The positive electrode active material 100C is a nickel-cobalt-manganese lithium oxide (NCM) having titanium as an additive element for improving electrical conductivity in the surface layer portion 100a and aluminum as an additive element for stabilizing the crystal structure. The positive electrode active material 100C is also a nickel-cobalt-manganese lithium oxide having aluminum as an additive element for stabilizing the crystal structure in the inner wall surface layer portion 100c of the crack portion 106 and substantially no titanium as an additive element for improving electrical conductivity.

[0230] Lithium nickel-cobalt-manganese oxide has a layered rock-salt crystal structure with space group R-3m. The composition of lithium nickel-cobalt-manganese oxide is LiNi x Co y Mn zWhen represented by O2 (x > 0, y > 0, z > 0, 0.8 < x + y + z < 1.2), x, y, and z preferably satisfy x:y:z = 8:1:1 or values in the vicinity thereof. Or x, y, and z preferably satisfy x:y:z = 9:0.5:0.5 or values in the vicinity thereof. That is, it is preferable that the nickel content ratio satisfies x > 2(y + z). Also, as a composition with a high nickel content ratio, x, y, and z preferably satisfy x:y:z = 6:2:2 or values in the vicinity thereof. Or x, y, and z preferably satisfy x:y:z = 5:2:3 or values in the vicinity thereof. However, the composition of the positive electrode active material 100C is not particularly limited, and those in which x, y, and z satisfy x:y:z = 1:1:1 or values in the vicinity thereof may be used. Or those in which x, y, and z satisfy x:y:z = 1:4:1 or values in the vicinity thereof may be used. In this specification and the like, the vicinity values in the composition refer to the range that becomes the composition when the significant figure is one digit. At this time, the digits below the significant figure are rounded off. For example, x:y:z = 4.6:2.3:3.1 can be said to be values in the vicinity of x:y:z = 5:2:3.

[0231] The particles of the positive electrode active material 100C are preferably primary particles (single particles). Or, when the particles of the positive electrode active material 100C are secondary particles, the number of primary particles contained in the secondary particles is preferably small. For example, it is preferably 2 or more and 20 or less, more preferably 2 or more and 15 or less, more preferably 2 or more and 10 or less, more preferably 2 or more and 5 or less, and even more preferably 2.

[0232] The particles of the positive electrode active material 100C are produced by using an aqueous solution that becomes a nickel source, a cobalt source, and a manganese source, mixing nickel-cobalt-manganese hydroxide obtained by a coprecipitation method with lithium hydroxide, performing a first heat treatment, and then further mixing with lithium hydroxide and performing a second heat treatment.

[0233] In the above-mentioned second heat treatment, titanium can be added as an additive element for improving electrical conductivity, and aluminum can be added as an additive element for stabilizing the crystal structure in the same process. The element added in this second heat treatment is called additive element X, and the material used to add additive element X is called additive element X source (X source).

[0234] As an example of a method for producing the positive electrode active material 100C, a method for producing a positive electrode active material 100C-1 will be described with reference to FIG.

[0235] <Step S111> 14, first, a transition metal M source, i.e., a nickel source (Ni source), a cobalt source (Co source), and a manganese source (Mn source) are prepared. It is preferable that the mixture ratio of nickel, cobalt, and manganese is within a range that allows the product to have a layered rock-salt type crystal structure.

[0236] In particular, a positive electrode active material containing a large amount of nickel as the transition metal M is preferable because the raw material may be cheaper than a material containing a large amount of cobalt, and the charge / discharge capacity per weight may increase. For example, nickel among the transition metals M is preferably more than 25 atomic %, more preferably 60 atomic % or more, and even more preferably 80 atomic % or more. However, if the proportion of nickel is too high, chemical stability and heat resistance may decrease. Therefore, nickel among the transition metals M is preferably 95 atomic % or less.

[0237] A secondary battery having cobalt as the transition metal M of the positive electrode active material is preferable because it has a high average discharge voltage and cobalt contributes to stabilizing the layered rock salt structure, making it a highly reliable secondary battery. However, since cobalt is more expensive than nickel and manganese and is unstable, if the proportion of cobalt is too high, the cost of manufacturing the secondary battery may increase. Therefore, for example, it is preferable that cobalt among the transition metals M is 2.5 atomic % or more and 34 atomic % or less.

[0238] A positive electrode active material having manganese as the transition metal M is preferable because it improves heat resistance and chemical stability. However, if the ratio of manganese is too high, the discharge voltage and discharge capacity tend to decrease. Therefore, for example, it is preferable that manganese in the transition metal M is 2.5 atomic % or more and 34 atomic % or less.

[0239] The transition metal M source is prepared as an aqueous solution of a compound containing the transition metal M. An aqueous solution of a nickel salt can be used as the nickel source. For example, nickel sulfate, nickel chloride, nickel nitrate, or hydrates thereof can be used as the nickel salt. Nickel acetate or other nickel organic acid salts, or hydrates thereof can also be used. An aqueous solution of a nickel alkoxide or an organic nickel complex can also be used as the nickel source. In this specification and the like, an organic acid salt refers to a compound of an organic acid such as acetic acid, citric acid, oxalic acid, formic acid, or butyric acid with a metal.

[0240] Similarly, the cobalt source may be an aqueous solution of a cobalt salt. Examples of the cobalt salt include cobalt sulfate, cobalt chloride, cobalt nitrate, and hydrates thereof. Organic acid salts of cobalt, such as cobalt acetate, and hydrates thereof may also be used. The cobalt source may be an aqueous solution of a cobalt alkoxide or an organic cobalt complex.

[0241] Similarly, the manganese source may be an aqueous solution of a manganese salt. The manganese salt may be, for example, an aqueous solution of manganese sulfate, manganese chloride, manganese nitrate, or a hydrate thereof. An organic acid salt of manganese, such as manganese acetate, or a hydrate thereof may also be used. The manganese source may be an aqueous solution of a manganese alkoxide or an organic manganese complex.

[0242] In the 9th method for preparing the positive electrode active material, an aqueous solution of nickel sulfate, cobalt sulfate, and manganese sulfate dissolved in pure water is prepared as a transition metal M source.

[0243] <Step S113> Also, as shown in step S113 of FIG. 14, a chelating agent may be prepared. Examples of the chelating agent include glycine, oxine, 1-nitroso-2-naphthol, 2-mercaptobenzothiazole, and EDTA (ethylenediaminetetraacetic acid). A plurality of types selected from glycine, oxine, 1-nitroso-2-naphthol, and 2-mercaptobenzothiazole may be used. At least one of these is dissolved in pure water and used as a chelating aqueous solution. The chelating agent is a complexing agent that creates a chelating compound, and is preferable to a general complexing agent. Of course, a complexing agent may be used instead of a chelating agent, and ammonia water may be used as the complexing agent. The use of a chelating aqueous solution is preferable because it can suppress the unnecessary generation of crystal nuclei and promote growth. When the generation of unnecessary nuclei is suppressed, the generation of fine particles is suppressed, and therefore a composite hydroxide with a good particle size distribution can be obtained. In addition, when ammonia is used in the alkaline solution, an ammonia salt may be generated. In addition, the use of a chelating aqueous solution can delay the acid-base reaction, and the reaction proceeds gradually, resulting in secondary particles that are close to spherical. Glycine has the effect of maintaining a constant pH value at or near a pH value of 9 or more and 10 or less, and it is preferable to use an aqueous glycine solution as the aqueous chelate solution since this makes it easier to control the pH in the reaction tank when obtaining the composite hydroxide 98. In the aqueous solution containing a transition metal and glycine, the glycine concentration is preferably 0.05 mol / L or more and 0.3 mol / L or less, and more preferably 0.07 mol / L or more and 0.32 mol / L or less.

[0244] <Step S114> Next, in step S114 of FIG. 14, a transition metal M source and a chelating agent are mixed to prepare an acid solution.

[0245] <Step S121> Next, in step S121 of Fig. 14, an alkaline solution is prepared. As the alkaline solution, for example, an aqueous solution containing sodium hydroxide, potassium hydroxide, lithium hydroxide, or ammonia can be used. This aqueous solution is preferably prepared using pure water. Alternatively, the aqueous solution may be prepared by dissolving a plurality of types selected from sodium hydroxide, potassium hydroxide, lithium hydroxide, and ammonia in pure water.

[0246] The pure water preferably used for the transition metal M source and the alkaline solution is water having a resistivity of 1 MΩ·cm or more, more preferably 10 MΩ·cm or more, and even more preferably 15 MΩ·cm or more. Water satisfying the above resistivity has high purity and contains very few impurities.

[0247] <Step S122> As shown in step S122 of FIG. 14, it is preferable to prepare water in the reaction tank. This water may be an aqueous solution of a chelating agent, but it is more preferable to use pure water. The use of pure water promotes nucleation, and allows the production of composite hydroxides with small particle sizes. The water prepared in the reaction tank can be called a filling liquid or an adjustment liquid for the reaction tank. When using an aqueous chelating solution, the description of step S113 can be referred to.

[0248] <Step S131> 14, the acid solution and the alkaline solution are mixed and reacted with each other, which can be called a co-precipitation reaction, a neutralization reaction, or an acid-base reaction.

[0249] During the coprecipitation reaction in step S131, it is preferable to adjust the pH of the reaction system to be 9.0 or more and 13.0 or less.

[0250] For example, when an alkaline solution is placed in a reaction tank and an acid solution is added to the reaction tank, it is advisable to maintain the pH of the aqueous solution in the reaction tank within the above-mentioned range. The same applies when an acid solution is placed in a reaction tank and an alkaline solution is added. It is preferable to set the acid solution delivery speed to 0.1 mL / min or less, as this makes it easier to control the pH conditions. A pump is provided in the tank that stores the acid solution, and the acid solution can be added to the reaction tank through a tube by using the pump. The amount of acid solution added, i.e., the amount of solution delivered, can be controlled by the pump.

[0251] The alkaline solution is added so as to keep the pH of the aqueous solution in the reaction tank constant. The reaction tank includes a reaction vessel and the like.

[0252] The aqueous solution may be stirred in the reaction tank using a stirring means. The stirring means may have a stirrer or stirring blades. Between two and six stirring blades may be provided. For example, when using four stirring blades, they may be arranged in a cross shape when viewed from above. The rotation speed of the stirring means may be between 800 rpm and 1200 rpm. Baffle plates may also be provided in the reaction tank to change the stirring direction and flow rate. The provision of baffle plates improves the mixing efficiency, allowing the synthesis of more uniform composite hydroxide particles.

[0253] The temperature of the reaction vessel is preferably adjusted to be 50° C. or higher and 90° C. or lower. The addition of the alkaline solution or acid solution should be started after the reaction vessel has reached the appropriate temperature.

[0254] The inside of the reaction vessel should be kept in an inert atmosphere. In this case, nitrogen or argon can be used as the inert atmosphere. When using a nitrogen atmosphere, nitrogen gas should be introduced at a flow rate of 0.5 L / min to 2 L / min.

[0255] The reactor may also be equipped with a reflux condenser, which allows nitrogen gas to be vented from the reactor and water vapor to be returned to the reactor.

[0256] By the above coprecipitation reaction, a composite hydroxide 98 containing the transition metal M is precipitated.

[0257] <Step S132> In order to recover the composite hydroxide 98, it is preferable to perform filtration as shown in step S132 of Fig. 14. The filtration is preferably suction filtration. During the filtration, the reaction product precipitated in the reaction tank may be washed with pure water, and then filtered using an organic solvent (e.g., acetone, etc.).

[0258] <Step S133> As shown in step S133 of Fig. 14, the composite hydroxide 98 after filtration may be dried. For example, it may be dried under vacuum at 60°C to 200°C for 0.5 hours to 20 hours. For example, it may be dried for 12 hours.

[0259] In this manner, a composite hydroxide 98 containing the transition metal M can be obtained. In this specification and the like, the composite hydroxide 98 refers to a hydroxide of a plurality of metals. The composite hydroxide 98 can be said to be a precursor of a positive electrode active material.

[0260] <Step S141> Next, in step S141 of Fig. 14, a lithium source is prepared. In the process for producing particles of the positive electrode active material, the step of adding the lithium source is performed multiple times, so in step S141, an amount of lithium prepared is less than the final amount. For example, when the sum of the atoms of nickel, cobalt, and manganese is 1, the number of lithium atoms can be 0.5 to 0.9 (atomic ratio), and it is more preferable to set it to 0.7 (atomic ratio). Note that the entire amount of the lithium source may be added in one step S141.

[0261] The lithium source may be, for example, lithium hydroxide, lithium carbonate, or lithium nitrate. In particular, it is preferable to use a material with a low melting point among lithium compounds, such as lithium hydroxide (melting point 462°C). A positive electrode active material with a high proportion of nickel is more susceptible to cation mixing than lithium cobalt oxide, etc., so heating in step S43, etc., must be performed at a low temperature. For this reason, it is preferable to use a material with a low melting point.

[0262] In addition, the smaller the particle size of the lithium source, the better the reaction will proceed. For example, a lithium source pulverized using a fluidized bed jet mill can be used. The particle size here refers to the median diameter.

[0263] <Step S142> Next, in step S142 of FIG. 14, the composite hydroxide 98 and the lithium source are mixed. The mixing can be performed by a dry method or a wet method. For example, a ball mill, a bead mill, or a kneader can be used for mixing. When using a ball mill, it is preferable to use zirconia balls as the media. Furthermore, when using a ball mill or a bead mill, it is preferable to set the peripheral speed to 100 mm / sec or more and 2000 mm / sec or less in order to suppress contamination from the media or materials. The composite hydroxide 98 and the lithium compound may be pulverized at the same time as mixing.

[0264] <Step S143> Next, the mixture of composite hydroxide 98 and the lithium source is heated. To distinguish from other heating steps, in Fig. 14, step S143 may be referred to as the first heating, step S153 as the second heating, and step S155 as the third heating.

[0265] The firing equipment for these heating processes can be an electric furnace or a rotary kiln. The crucible, scabbard, setter, and container used during heating are preferably made of materials that do not easily release impurities. For example, it is recommended to use a crucible made of aluminum oxide with a purity of 99.9%. It is also preferable to heat these containers with their lids on.

[0266] The heating temperature in step S143 is preferably 400° C. to 750° C., more preferably 650° C. to 750° C. The heating time in step S143 is preferably 1 hour to 30 hours, more preferably 2 hours to 20 hours.

[0267] The heating is preferably performed in an atmosphere containing oxygen, or a so-called dry air containing oxygen with little water (for example, a dew point of -50°C or less, more preferably a dew point of -80°C or less).

[0268] <Step S144> Moreover, it is preferable to have a crushing step after heating as step S144. Crushing can be performed, for example, in a mortar. Furthermore, classification can be performed using a sieve. By having the crushing step, the particle size and / or shape of the positive electrode active material 100A2 can be made more uniform. Through the above steps, a composite oxide 99 is obtained. The composite oxide 99 can also be called nickel-cobalt-lithium manganese oxide (NCM).

[0269] <Step S145> Next, in step S145 of manufacturing method 9 of the positive electrode active material described with reference to FIG. 14, a liquid aluminum source (Al source) and a solid titanium source (Ti source) are prepared.

[0270] As the solid titanium source, the solid material shown in the description of step S41 in FIG. 7 can be used.

[0271] As the liquid aluminum source, the liquid material described in the description of step S41 in FIG. 3 can be used.

[0272] In method 9 for producing a positive electrode active material, which will be described with reference to FIG. 14, an aluminum isopropoxide solution in which aluminum isopropoxide is dissolved in isopropoxide is used as the aluminum source, and lithium titanate is used as the titanium source.

[0273] <Step S146> As shown in step S146 of FIG. 14, the titanium source can be pulverized to adjust the particle size of the titanium source. In addition, although not shown, the pulverized titanium source can be classified by a classifier to obtain a titanium source having a particle diameter of 100 nm or less. C The titanium source particles having the following particle sizes may be removed. Note that the conditions for pulverizing the titanium source can be referred to as the conditions for step S12 in FIG.

[0274] <Step S147> The above-mentioned liquid aluminum source and solid titanium source can be used as a source of the additive element X (X source).

[0275] <Step S151> Next, in step S151, a lithium source is prepared. At this time, an amount that will be the final amount of lithium in combination with step S141 is prepared. For example, in step S141, when the sum of the atomic numbers of nickel, cobalt, and manganese is set to 1, if the atomic number of lithium is set to 0.7 (atomic number ratio), it is preferable to prepare, for example, 0.31 (atomic number ratio) in step S151. Here, the final amount of lithium atoms when the sum of the atomic numbers of nickel, cobalt, and manganese is set to 1 is set to 1.01, but one embodiment of the present invention is not limited to this. When the sum of the atomic numbers of nickel, cobalt, and manganese is set to 1, the final amount of lithium is preferably 0.95 to 1.25, and more preferably 1.00 to 1.05. For anything other than the amount to be prepared, the description of step S141 can be referred to.

[0276] 14, a method is described in which the lithium source is added twice in steps S141 and S151 and heated, but this is not a limitation of one embodiment of the present invention. The entire amount of the lithium source may be added once in step S141, or the lithium source may be added three or more times and heated.

[0277] <Step S152> Next, the composite oxide 99 obtained in step S144, the source of the additive element X (X source), and the lithium source are mixed together to prepare a mixed solution. A stirrer or the like may be used for mixing.

[0278] <Step S153> When an aluminum isopropoxide solution is used as the aluminum source, the above mixture is stirred in an atmosphere containing water vapor. This treatment causes the H2O in the atmosphere and the aluminum isopropoxide to undergo hydrolysis and polycondensation reactions. Then, a gel-like layer containing aluminum is formed on the surface of the lithium cobalt oxide particles containing magnesium and fluorine.

[0279] Stirring can be performed, for example, with a magnetic stirrer. The stirring time may be long enough for the water in the atmosphere and the aluminum isopropoxide to undergo hydrolysis and polycondensation reactions, and may be performed, for example, for 4 hours at 25°C and 90% RH (relative humidity).

[0280] <Step S154> The precipitate is collected from the mixed solution after the above treatment. The collection method can be filtration, centrifugation, drying, etc. In the positive electrode active material production method 1, the precipitate is collected by filtration. A paper filter is used for filtration, and the residue is washed with the same alcohol as the solvent in which the aluminum alkoxide was dissolved.

[0281] <Step S155> Next, the collected residue is dried. In the positive electrode active material preparation method 9, the residue is dried in a vacuum at 70° C. for 1 hour. The material collected as described above may be crushed and then sieved as necessary during collection.

[0282] <Step S156> Next, the material collected in step S155 is heated. The heating in step S156 is preferably performed at a sufficiently high temperature to increase the crystallite size of the positive electrode active material 100C-1, although the range may differ depending on the composition of the transition metal M.

[0283] When the proportion of nickel in the transition metal M is high, for example 70% or more, the heating temperature in step S156 is preferably 750°C or more, more preferably 800°C or more, and even more preferably 850°C or more. On the other hand, if the heating temperature is too high, there is a risk that the transition metal M such as nickel may be reduced to a divalent state. Therefore, for example, the heating temperature is preferably 950°C or less, more preferably 920°C or less, and even more preferably 900°C or less.

[0284] When the proportion of nickel in the transition metal M is 40% or more and 60% or less, for example, 900° C. or more is preferable, 950° C. or more is more preferable, and about 970° C. is more preferable. On the other hand, if the temperature is too high, there is a risk of the same disadvantages as described above occurring, so 1020° C. or less is preferable, and 990° C. or less is more preferable. For other heating conditions, see the description of step S143.

[0285] It is also preferable to have a crushing step after the heating as step S157. For the crushing, see the description of step S144.

[0286] By such a preparation method, the positive electrode active material 100C-1 can be obtained in step S158 of Fig. 14. The positive electrode active material 100C-1 can be referred to as lithium nickel-cobalt-manganese oxide having aluminum and titanium on the surface layer portion 100a and having aluminum on the inner wall surface layer portion 100c of the crack portion 106. The positive electrode active material 100C-1 can also be referred to as lithium nickel-cobalt-manganese oxide having aluminum and titanium on the surface layer portion 100a and having aluminum on the inner wall surface layer portion 100c of the crack portion 106.

[0287] This embodiment mode can be used in appropriate combination with other embodiment modes.

[0288] (Embodiment 2) In this embodiment, an example of a secondary battery of one embodiment of the present invention will be described with reference to FIGS.

[0289] <Example of secondary battery configuration> The following description will be given taking as an example a secondary battery shown in FIG. 15 in which a positive electrode, a negative electrode, and an electrolyte are enclosed in an exterior body.

[0290] [Positive electrode] The positive electrode includes a positive electrode active material layer and a positive electrode current collector. The positive electrode active material layer includes a positive electrode active material, and may include a conductive material (synonymous with a conductive additive) and a binder. The positive electrode active material is prepared by the method described in the above embodiment.

[0291] The positive electrode active material described in the above embodiment may be mixed with another positive electrode active material.

[0292] Other examples of the positive electrode active material include composite oxides having an olivine type crystal structure, a layered rock salt type crystal structure, or a spinel type crystal structure, such as LiFePO4, LiFeO2, LiNiO2, LiMn2O4, V2O5, Cr2O5, and MnO2.

[0293] In addition, as another positive electrode active material, it is preferable to mix a lithium-containing material having a spinel-type crystal structure containing manganese such as LiMn2O4 with lithium nickelate (LiNiO2 or LiNi 1-x M x O2(0 < x < 1)(M = Co, Al, etc.)). By adopting such a configuration, the characteristics of the secondary battery can be improved.

[0294] <Conductive material> The conductive material, also called a conductivity-imparting agent or a conductive auxiliary agent, is a carbon material. By attaching the conductive material between a plurality of active materials, the plurality of active materials are electrically connected to each other, enhancing the conductivity. Note that the term "attachment" does not only refer to the physical adhesion between the active material and the conductive material, but also includes cases where a covalent bond occurs, cases where bonding occurs by van der Waals forces, cases where a part of the surface of the active material is covered by the conductive material, cases where the conductive material fits into the surface irregularities of the active material, and cases where they are electrically connected even if they are not in contact with each other.

[0295] Active material layers such as the positive electrode active material layer and the negative electrode active material layer preferably have a conductive material.

[0296] As the conductive material, for example, any one or two or more of carbon blacks such as acetylene black and furnace black, graphites such as artificial graphite and natural graphite, carbon fibers such as carbon nanofibers and carbon nanotubes, and graphene compounds can be used.

[0297] As the carbon fiber, for example, carbon fibers such as mesophase pitch-based carbon fibers and isotropic pitch-based carbon fibers can be used. Also, as the carbon fiber, carbon nanofibers or carbon nanotubes can be used. Carbon nanotubes can be produced, for example, by a vapor phase growth method.

[0298] In the present specification and the like, the graphene compound includes graphene, multi-layer graphene, multi-graphene, graphene oxide, multi-layer graphene oxide, multi-graphene oxide, reduced graphene oxide, reduced multi-layer graphene oxide, reduced multi-graphene oxide, graphene quantum dots, and the like. The graphene compound has carbon, has a shape such as a plate shape or a sheet shape, and has a two-dimensional structure formed by six-membered carbon rings. The two-dimensional structure formed by six-membered carbon rings may be called a carbon sheet. The graphene compound may have a functional group. In addition, the graphene compound preferably has a curved shape. In addition, the graphene compound may be rolled up like a carbon nanofiber.

[0299] In this specification and the like, graphene oxide refers to a material that contains carbon and oxygen, has a sheet-like shape, and has a functional group, in particular, an epoxy group, a carboxy group, or a hydroxy group.

[0300] In the present specification and the like, reduced graphene oxide refers to a graphene oxide having a sheet-like shape and a two-dimensional structure formed of six-membered carbon rings, which contains carbon and oxygen. Although reduced graphene oxide functions as a single sheet, multiple sheets may be stacked. Reduced graphene oxide preferably has a portion in which the carbon concentration is greater than 80 atomic % and the oxygen concentration is 2 atomic % to 15 atomic %. By setting such carbon and oxygen concentrations, it can function as a conductive material with high conductivity even in a small amount. In addition, reduced graphene oxide preferably has an intensity ratio G / D of G band to D band in Raman spectrum of 1 or more. Reduced graphene oxide with such an intensity ratio can function as a conductive material with high conductivity even in a small amount.

[0301] The graphene compound may have excellent electrical properties such as high electrical conductivity, and excellent physical properties such as high flexibility and high mechanical strength. The graphene compound may have a sheet-like shape. The graphene compound may have a curved surface, enabling surface contact with low contact resistance. In addition, even if the graphene compound is thin, it may have very high electrical conductivity, and a small amount of the graphene compound may efficiently form a conductive path in the active material layer. Therefore, by using the graphene compound as a conductive material, the contact area between the active material and the conductive material can be increased. The graphene compound may cover 80% or more of the area of ​​the active material. It is preferable that the graphene compound is wrapped around at least a part of the active material particles. It is also preferable that the graphene compound is overlapped on at least a part of the active material particles. It is also preferable that the shape of the graphene compound matches at least a part of the shape of the active material particles. The shape of the active material particles refers to, for example, the unevenness of a single active material particle or the unevenness formed by a plurality of active material particles. It is also preferable that the graphene compound surrounds at least a part of the active material particles. The graphene compound may have holes.

[0302] When using active material particles having a small particle size, for example, active material particles having a size of 1 μm or less, the specific surface area of ​​the active material particles is large, and more conductive paths connecting the active material particles are required. In such a case, it is preferable to use a graphene compound that can efficiently form conductive paths even in a small amount.

[0303] Because of the above-mentioned properties, it is particularly effective to use a graphene compound as a conductive material for secondary batteries that require rapid charging and rapid discharging. For example, secondary batteries for two-wheeled or four-wheeled vehicles and secondary batteries for drones may require rapid charging and rapid discharging characteristics. Rapid charging and discharging may also be required for mobile electronic devices. Rapid charging and discharging refers to charging and discharging at 200 mA / g, 400 mA / g, or 1000 mA / g or more per weight of the positive electrode active material.

[0304] The multiple graphenes or graphene compounds are formed so as to partially cover the multiple granular positive electrode active material particles or to be attached to surfaces of the multiple granular positive electrode active material particles, and therefore are preferably in surface contact with each other.

[0305] Here, a mesh-like graphene compound sheet (hereinafter referred to as a graphene compound net or graphene net) can be formed by bonding multiple graphenes or graphene compounds together. When an active material is covered with a graphene net, the graphene net can also function as a binder that bonds the active materials together. Therefore, the amount of binder can be reduced or no binder can be used, and the ratio of the active material to the electrode volume and electrode weight can be improved. That is, the discharge capacity of the secondary battery can be increased.

[0306] In addition, a material used in forming the graphene compound may be mixed with the graphene compound and used in the active material layer 200. For example, particles used as a catalyst in forming the graphene compound may be mixed with the graphene compound. Examples of catalysts used in forming the graphene compound include silicon oxide (SiO2, SiO x (x<2)), aluminum oxide, iron, nickel, ruthenium, iridium, platinum, copper, germanium, etc. The particles preferably have a median diameter (D50) of 1 μm or less, more preferably 100 nm or less.

[0307] The content of the conductive material relative to the total amount of the active material layer is preferably 1 wt % or more and 10 wt % or less, and more preferably 1 wt % or more and 5 wt % or less.

[0308] Unlike granular conductive materials such as carbon black, which are in point contact with the active material, the graphene compound allows for surface contact with low contact resistance, and therefore can improve the electrical conductivity between the granular active material and the graphene compound with a smaller amount than that of a normal conductive material. This allows the ratio of the active material in the active material layer to be increased, thereby increasing the discharge capacity of the battery.

[0309] Particulate carbon-containing compounds such as carbon black and graphite, or fibrous carbon-containing compounds such as carbon nanotubes, tend to enter microspaces. Microspaces refer to, for example, regions between a plurality of active materials. By using a combination of a carbon-containing compound that tends to enter microspaces and a sheet-like carbon-containing compound such as graphene that can impart conductivity across a plurality of particles, the density of the electrode can be increased and an excellent conductive path can be formed. The battery obtained by the manufacturing method of one embodiment of the present invention has a high capacity density and can be stable, and is effective as an in-vehicle battery.

[0310] [Binder] As the binder, it is preferable to use a rubber material such as styrene-butadiene rubber (SBR), styrene-isoprene-styrene rubber, acrylonitrile-butadiene rubber, butadiene rubber, ethylene-propylene-diene copolymer, etc. Also, as the binder, fluororubber can be used.

[0311] In addition, it is preferable to use, for example, a water-soluble polymer as the binder. For example, polysaccharides can be used as the water-soluble polymer. For the polysaccharides, one or more of cellulose derivatives such as carboxymethyl cellulose (CMC), methyl cellulose, ethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, regenerated cellulose, and starch can be used. It is even more preferable to use these water-soluble polymers in combination with the above-mentioned rubber material.

[0312] Alternatively, it is preferable to use materials such as polystyrene, polymethyl acrylate, polymethyl methacrylate (polymethyl methacrylate, PMMA), sodium polyacrylate, polyvinyl alcohol (PVA), polyethylene oxide (PEO), polypropylene oxide, polyimide, polyvinyl chloride, polytetrafluoroethylene, polyethylene, polypropylene, polyisobutylene, polyethylene terephthalate, nylon, polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), ethylene propylene diene polymer, polyvinyl acetate, and nitrocellulose as the binder.

[0313] The binder may be a combination of two or more of the above.

[0314] [Current collector] As the current collector, a material having high electrical conductivity, such as metals such as stainless steel, gold, platinum, aluminum, and titanium, and alloys thereof, can be used. In addition, it is preferable that the material used for the positive electrode current collector does not dissolve at the potential of the positive electrode. In addition, an aluminum alloy to which an element that improves heat resistance, such as silicon, titanium, neodymium, scandium, or molybdenum, is added can be used. In addition, it may be formed of a metal element that reacts with silicon to form a silicide. Examples of the metal element that reacts with silicon to form a silicide include zirconium, titanium, hafnium, vanadium, niobium, tantalum, chromium, molybdenum, tungsten, cobalt, and nickel. The current collector can be appropriately used in the form of a foil, plate, sheet, net, punched metal, or expanded metal. It is preferable to use a current collector having a thickness of 5 μm or more and 30 μm or less.

[0315] [Negative electrode] The negative electrode includes a negative electrode active material layer and a negative electrode current collector. The negative electrode active material layer may include a conductive material and a binder.

[0316] [Negative electrode active material] As the negative electrode active material, for example, an alloy-based material and / or a carbon-based material can be used.

[0317] As the negative electrode active material, an element capable of carrying out a charge / discharge reaction by alloying / dealloying reaction with lithium can be used. For example, a material containing one or more elements selected from silicon, tin, gallium, aluminum, germanium, lead, antimony, bismuth, silver, zinc, cadmium, indium, etc. can be used. Such elements have a larger charge / discharge capacity than carbon, and silicon in particular has a high theoretical capacity of 4200mAh / g. For this reason, it is preferable to use silicon as the negative electrode active material. Compounds containing these elements may also be used. For example, SiO, Mg2Si, Mg2Ge, SnO, SnO2, Mg2Sn, SnS2, V2Sn3, FeSn2, CoSn2, Ni3Sn2, Cu6Sn5, Ag3Sn, Ag3Sb, Ni2MnSb, CeSb3, LaSn3, La3Co2Sn7, CoSb3, InSb, SbSn, etc. Here, elements capable of carrying out charge / discharge reactions through alloying / dealloying reactions with lithium, and compounds containing such elements, are sometimes referred to as alloying materials.

[0318] In this specification, SiO refers to, for example, silicon monoxide. Alternatively, SiO x Here, x preferably has a value of 1 or close to 1. For example, x is preferably 0.2 or more and 1.5 or less, more preferably 0.3 or more and 1.2 or less, or preferably 0.2 or more and 1.2 or less, or preferably 0.3 or more and 1.5 or less.

[0319] As the carbon-based material, graphite, easily graphitizable carbon (soft carbon), non-graphitizable carbon (hard carbon), carbon nanotubes, graphene, carbon black, and the like may be used.

[0320] Examples of graphite include artificial graphite and natural graphite. Examples of artificial graphite include mesocarbon microbeads (MCMB), coke-based artificial graphite, and pitch-based artificial graphite. Here, as the artificial graphite, spherical graphite having a spherical shape can be used. For example, MCMB may have a spherical shape, which is preferable. In addition, it is relatively easy to reduce the surface area of ​​MCMB, which may be preferable. Examples of natural graphite include flake graphite and spheroidized natural graphite.

[0321] When lithium ions are inserted into graphite (when lithium-graphite intercalation compounds are formed), graphite exhibits a low potential similar to that of lithium metal (0.05 V to 0.3 V vs. Li / Li + ) This allows lithium-ion secondary batteries to exhibit high operating voltages. Furthermore, graphite is preferred because it has the advantages of relatively high charge / discharge capacity per unit volume, relatively small volume expansion, low cost, and high safety compared to lithium metal.

[0322] In addition, titanium dioxide (TiO2), lithium titanium oxide (Li4Ti5O 12 ), lithium-graphite intercalation compound (Li x C6), niobium pentoxide (Nb2O5), tungsten oxide (WO2), molybdenum oxide (MoO2), and other oxides can be used.

[0323] In addition, the negative electrode active material is Li3N-type Li, a complex nitride of lithium and transition metals. 3-x M x N (M=Co, Ni, Cu) can be used. For example, Li 2.6 Co 0.4 N3 has a large charge / discharge capacity (900mAh / g, 1890mAh / cm 3 ) and is preferred.

[0324] When a composite nitride of lithium and a transition metal is used, lithium ions are contained in the negative electrode active material, and therefore it is preferable to combine it with a material that does not contain lithium ions, such as V2O5 or Cr3O8, as the positive electrode active material. Even when a material that contains lithium ions is used as the positive electrode active material, the composite nitride of lithium and a transition metal can be used as the negative electrode active material by first removing the lithium ions contained in the positive electrode active material.

[0325] In addition, materials that undergo a conversion reaction can also be used as the negative electrode active material. For example, transition metal oxides that do not form an alloy with lithium, such as cobalt oxide (CoO), nickel oxide (NiO), and iron oxide (FeO), can be used as the negative electrode active material. Further examples of materials that undergo a conversion reaction include oxides such as Fe2O3, CuO, Cu2O, RuO2, and Cr2O3, and CoS 0.89 Examples of such oxides include sulfides such as NiS and CuS, nitrides such as Zn3N2, Cu3N and Ge3N4, phosphides such as NiP2, FeP2 and CoP3, and fluorides such as FeF3 and BiF3.

[0326] As the conductive material and binder that can be contained in the negative electrode active material layer, materials similar to the conductive material and binder that can be contained in the positive electrode active material layer can be used.

[0327] [Negative electrode current collector] The negative electrode current collector may be made of the same material as the positive electrode current collector, but it is preferable that the negative electrode current collector is made of a material that does not form an alloy with carrier ions such as lithium.

[0328] [Electrolyte] As one form of the electrolyte, an electrolyte solution having a solvent and an electrolyte dissolved in the solvent can be used. The electrolyte solution has a solvent and a lithium salt. As the solvent of the electrolyte solution, an aprotic organic solvent is preferable, and for example, one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, chloroethylene carbonate, vinylene carbonate, γ-butyrolactone, γ-valerolactone, dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl formate, methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, 1,3-dioxane, 1,4-dioxane, dimethoxyethane (DME), dimethyl sulfoxide, diethyl ether, methyl diglyme, acetonitrile, benzonitrile, tetrahydrofuran, sulfolane, sultone, etc., or two or more of these can be used in any combination and ratio.

[0329] When the electrolyte contains ethylene carbonate (EC) and diethyl carbonate (DEC), the volume ratio of ethylene carbonate and diethyl carbonate can be x:100-x (where 20≦x≦40) when the total content of ethylene carbonate and diethyl carbonate is 100 vol%. More specifically, a mixed organic solvent containing EC and DEC in a volume ratio of EC:DEC=30:70 can be used.

[0330] Also, when using a mixed organic solvent containing ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) as the electrolyte, when the total content of ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate is 100 vol%, a mixed organic solvent with a volume ratio of ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate of x:y:100 - x - y (where 5 ≤ x ≤ 35 and 0 < y < 65) can be used. More specifically, a mixed organic solvent containing EC, EMC, and DMC in a volume ratio of EC:EMC:DMC = 30:35:35 can be used.

[0331] Furthermore, as the electrolyte, a mixed organic solvent containing a cyclic fluorinated carbonate (which may also be referred to as a fluorinated cyclic carbonate) or a linear fluorinated carbonate (which may also be referred to as a fluorinated linear carbonate) can be used. Further, it is preferable that the above mixed organic solvent contains both a cyclic fluorinated carbonate and a linear fluorinated carbonate. Both the cyclic fluorinated carbonate and the linear fluorinated carbonate have an electron-withdrawing substituent, which is preferable as it lowers the solvation energy of lithium ions. Therefore, both the cyclic fluorinated carbonate and the linear fluorinated carbonate are suitable for the electrolyte, and these mixed organic solvents are suitable.

[0332] As the cyclic fluorinated carbonate, for example, fluoroethylene carbonate (fluoroethylene carbonate, FEC, F1EC), difluoroethylene carbonate (DFEC, F2EC), trifluoroethylene carbonate (F3EC), or tetrafluoroethylene carbonate (F4EC) can be used. Note that DFEC has isomers such as cis-4,5 and trans-4,5. Since any of the cyclic fluorinated carbonates has an electron-withdrawing substituent, it is considered that the solvation energy of lithium ions is low. In FEC, the electron-withdrawing substituent is the F group.

[0333] Methyl 3,3,3-trifluoropropionate is an example of a fluorinated chain carbonate. The abbreviation for methyl 3,3,3-trifluoropropionate is "MTFP." In MTFP, the electron-withdrawing substituent is the CF3 group.

[0334] FEC is one of the cyclic carbonates and has a high relative dielectric constant, so when used in an organic solvent, it has the effect of promoting the dissociation of lithium salts. Furthermore, since FEC has a substituent that exhibits electron-withdrawing properties, it is easy to bind with lithium ions by Coulomb force or the like. Specifically, since the solvation energy of lithium ions in FEC is smaller than that of ethylene carbonate (EC), which does not have a substituent that exhibits electron-withdrawing properties, it can be said that FEC is easy to form solvation with lithium ions. Furthermore, FEC is thought to have a deep highest occupied molecular orbital (HOMO) level, and if the HOMO level is deep, it is difficult to oxidize and the oxidation resistance is improved. On the other hand, there is a concern that FEC has a high viscosity. Therefore, it is recommended to use a mixed organic solvent containing not only FEC but also MTFP in the electrolyte. MTFP is one of the chain carbonates, and it is possible to have the effect of lowering the viscosity of the electrolyte or maintaining the viscosity at room temperature (typically 25°C) even at low temperatures (typically 0°C). Furthermore, since MTFP has a smaller solvation energy than methyl propionate (abbreviated as "MP"), which does not have an electron-withdrawing substituent, it may form a solvate with lithium ions when used in an electrolyte.

[0335] It is preferable to mix FEC having such physical properties and MTFP in a mixed organic solvent so that the volume ratio is x:100-x (where 5≦x≦30, preferably 10≦x≦20), assuming the total content of the mixed organic solvent containing MTFP as 100 vol%. In other words, it is preferable to mix MTFP in a larger amount than FEC in the mixed organic solvent.

[0336] In addition, by using one or more ionic liquids (room-temperature molten salts) that are flame-retardant and non-volatile as a solvent for the electrolyte, even if the internal temperature of the secondary battery rises due to an internal short circuit or overcharging, etc., the secondary battery can be prevented from exploding and / or catching fire. The ionic liquid is composed of a cation and an anion, and includes an organic cation and an anion. Examples of the organic cation used in the electrolyte include aliphatic onium cations such as quaternary ammonium cations, tertiary sulfonium cations, and quaternary phosphonium cations, and aromatic cations such as imidazolium cations and pyridinium cations. Examples of the anion used in the electrolyte include monovalent amide anions, monovalent methide anions, fluorosulfonate anions, perfluoroalkylsulfonate anions, tetrafluoroborate anions, perfluoroalkylborate anions, hexafluorophosphate anions, and perfluoroalkylphosphate anions.

[0337] [Lithium salt] Examples of the lithium salt (also called electrolyte) dissolved in the above-mentioned solvent include LiPF6, LiClO4, LiAsF6, LiBF4, LiAlCl4, LiSCN, LiBr, LiI, Li2SO4, Li2B 10 Cl 10 , Li2B 12 Cl 12 Lithium salts such as LiCF3SO3, LiC4F9SO3, LiC(CF3SO2)3, LiC(C2F5SO2)3, LiN(CF3SO2)2, LiN(C4F9SO2)(CF3SO2), LiN(C2F5SO2)2, etc. can be used alone or in any combination and ratio of two or more of these. The lithium salt should be 0.5 mol / L or more and 3.0 mol / L or less relative to the solvent. The use of fluorides such as LiPF6 and LiBF4 improves the safety of lithium-ion secondary batteries.

[0338] The above-mentioned electrolyte is preferably a highly purified electrolyte with a low content of granular waste or elements other than the constituent elements of the electrolyte (hereinafter, simply referred to as "impurities"). Specifically, the weight ratio of impurities to the electrolyte is 1 wt% or less, preferably 0.1 wt% or less, and more preferably 0.01 wt% or less.

[0339] [Additives] The electrolyte may contain an additive. The additive can suppress the reactive decomposition of the electrolyte that may occur on the positive electrode surface or the negative electrode surface when the secondary battery is operated at high voltage and / or high temperature. For example, vinylene carbonate (VC), propane sultone (PS), tert-butylbenzene (TBB), fluoroethylene carbonate (FEC), and lithium bis(oxalate)borate (LiBOB) can be used as the additive. LiBOB is particularly preferred because it is easy to form a good coating. VC or FEC is preferred because it can form a good coating on the negative electrode during aging or charging in the early stages of use of the secondary battery, thereby improving the cycle characteristics.

[0340] As the additive, any one or more of dinitrile compounds can be used. Specific examples of the dinitrile compound include succinonitrile, glutaronitrile, adiponitrile (ADN), and ethylene glycol bis(propionitrile) ether (EGBE).

[0341] Further, fluorobenzene may be added to the organic solvent. The concentration of the additive may be, for example, 0.1 wt% or more and 5 wt% or less with respect to the entire electrolyte. PS or EGBE is preferable because it can form a good coating on the positive electrode during charging and discharging, thereby improving cycle characteristics. FB is preferable because it improves the wettability of the organic solvent to the positive electrode and the negative electrode. Dinitrile compounds are preferable because the nitrile groups are oriented to the positive electrode and the negative electrode, inhibiting the oxidative decomposition of the organic solvent, thereby improving the high voltage resistance. Furthermore, dinitrile compounds are preferable because they can prevent the dissolution of copper during overdischarge when a current collector having copper is used for the negative electrode. Considering the use of secondary batteries at high voltages, it is preferable to add a nitrile compound.

[0342] [Gel electrolyte] As the gel electrolyte, a polymer gel in which a polymer is swollen with an electrolytic solution may be used. By using a polymer gel electrolyte, a semi-solid electrolyte layer can be provided, and safety against leakage and the like can be improved. In addition, it is possible to make the secondary battery thinner and lighter.

[0343] Examples of the polymer that can be gelled include silicone gel, acrylic gel, acrylonitrile gel, polyethylene oxide gel, polypropylene oxide gel, and fluorine-based polymer gel.

[0344] Examples of the polymer that can be used include polymers having a polyalkylene oxide structure such as polyethylene oxide (PEO), PVDF, polyacrylonitrile, and copolymers containing these. For example, PVDF-HFP, which is a copolymer of PVDF and hexafluoropropylene (HFP), can be used. The polymer that is formed may have a porous shape.

[0345] [Solid electrolyte] Instead of the electrolyte, a solid electrolyte containing an inorganic material such as a sulfide or oxide, or a solid electrolyte containing a polymer material such as a PEO (polyethylene oxide) can be used. When a solid electrolyte is used, the installation of a separator and / or spacer becomes unnecessary. In addition, since the entire battery can be solidified, there is no risk of leakage, and safety is dramatically improved.

[0346] [Separator] The secondary battery preferably has a separator. The separator may be made of, for example, paper, nonwoven fabric, glass fiber, ceramics, or synthetic fibers such as nylon (polyamide), vinylon (polyvinyl alcohol fiber), polyester, acrylic, polyolefin, or polyurethane. The separator is preferably processed into an envelope shape and disposed so as to encase either the positive electrode or the negative electrode.

[0347] The separator may have a multi-layer structure. For example, an organic material film such as polypropylene or polyethylene may be coated with a ceramic material, a fluorine material, a polyamide material, or a mixture of these. As the ceramic material, for example, aluminum oxide particles or silicon oxide particles may be used. As the fluorine material, for example, PVDF or polytetrafluoroethylene may be used. As the polyamide material, for example, nylon or aramid (meta-aramid or para-aramid) may be used.

[0348] Coating with ceramic materials improves oxidation resistance, suppressing the deterioration of the separator during high-voltage charging and improving the reliability of the secondary battery. Coating with fluorine-based materials also improves adhesion between the separator and electrodes, improving output characteristics. Coating with polyamide-based materials, especially aramid, improves heat resistance, improving the safety of the secondary battery.

[0349] For example, both sides of a polypropylene film may be coated with a mixture of aluminum oxide and aramid.Alternatively, the surface of the polypropylene film that contacts the positive electrode may be coated with a mixture of aluminum oxide and aramid, and the surface that contacts the negative electrode may be coated with a fluorine-based material.

[0350] By using a separator with a multi-layer structure, the safety of the secondary battery can be maintained even if the overall thickness of the separator is thin, and therefore the discharge capacity per volume of the secondary battery can be increased.

[0351] [Exterior body] The exterior body of the secondary battery can be made of, for example, a metal material such as aluminum and / or a resin material. Also, a film-shaped exterior body can be used. As the film, for example, a three-layer structure film can be used in which a thin metal film having excellent flexibility such as aluminum, stainless steel, copper, nickel, etc. is provided on a film made of a material such as polyethylene, polypropylene, polycarbonate, ionomer, polyamide, etc., and an insulating synthetic resin film such as a polyamide-based resin, polyester-based resin, etc. is further provided on the thin metal film as the outer surface of the exterior body.

[0352] <Laminated secondary battery and its manufacturing method> An example of an external view of a laminated secondary battery 500 is shown in Fig. 15 and Fig. 16. Fig. 15 and Fig. 16 have a positive electrode 503, a negative electrode 506, a separator 507, an exterior body 509, a positive electrode lead electrode 510, and a negative electrode lead electrode 511. If the laminated secondary battery has a flexible structure, and is mounted in an electronic device having at least a part having flexibility, the secondary battery can also be bent in accordance with the deformation of the electronic device. An example of a method for manufacturing the laminated secondary battery will be described with reference to Figs. 16(A) to 16(C).

[0353] First, the negative electrode 506, the separator 507, and the positive electrode 503 are laminated. FIG. 16(B) shows the laminated negative electrode 506, the separator 507, and the positive electrode 503. Here, an example is shown in which five pairs of negative electrodes and four pairs of positive electrodes are used. Next, the tab regions of the positive electrodes 503 are bonded to each other, and the positive electrode lead electrode 510 is bonded to the tab region of the outermost positive electrode. For example, ultrasonic welding or the like may be used for the bonding. Similarly, the tab regions of the negative electrodes 506 are bonded to each other, and the negative electrode lead electrode 511 is bonded to the tab region of the outermost negative electrode.

[0354] Next, the negative electrode 506 , the separator 507 and the positive electrode 503 are placed on the exterior body 509 .

[0355] Next, as shown in Fig. 16(C), exterior body 509 is folded at the portion indicated by the dashed line. After that, the outer periphery of exterior body 509 is joined. For the joining, for example, thermocompression bonding or the like may be used. At this time, a region (hereinafter referred to as an inlet) that is not joined is provided in a part (or one side) of exterior body 509 so that an electrolyte can be introduced later.

[0356] Next, an electrolyte (not shown) is introduced into the inside of the exterior body 509 through an inlet provided in the exterior body 509. The introduction of the electrolyte is preferably performed under a reduced pressure atmosphere or an inert atmosphere. Finally, the inlet is joined. In this manner, the laminate type secondary battery 500 can be produced.

[0357] By using the positive electrode active material described in the above embodiment for the positive electrode 503, the secondary battery 500 can have a high discharge capacity and excellent cycle characteristics.

[0358] This embodiment mode can be used in appropriate combination with other embodiment modes.

[0359] (Embodiment 3) In this embodiment, an example in which a secondary battery which is one embodiment of the present invention is mounted on an electronic device will be described with reference to FIGS.

[0360] 17A to 17G show examples of electronic devices to which the secondary battery having the positive electrode active material described in the above embodiment is mounted. Examples of electronic devices to which the secondary battery is applied include television devices (also called televisions or television receivers), monitors for computers, digital cameras, digital video cameras, digital photo frames, mobile phones (also called mobile phones or mobile phone devices), portable game machines, personal digital assistants, audio playback devices, and large game machines such as pachinko machines.

[0361] Furthermore, a secondary battery having a flexible shape can be incorporated along the curved surfaces of the inner or outer walls of a house or building, or the interior or exterior of an automobile.

[0362] 17A shows an example of a mobile phone. A mobile phone 7400 includes a display portion 7402 built into a housing 7401, operation buttons 7403, an external connection port 7404, a speaker 7405, a microphone 7406, and the like. Note that the mobile phone 7400 includes a secondary battery 7407. By using the secondary battery of one embodiment of the present invention as the secondary battery 7407, a lightweight mobile phone with a long life can be provided.

[0363] FIG. 17B shows a state in which the mobile phone 7400 is bent. When the mobile phone 7400 is deformed by an external force and bent as a whole, the secondary battery 7407 provided inside is also bent. FIG. 17C shows the bent state of the secondary battery 7407 at that time. The secondary battery 7407 is a thin storage battery. The secondary battery 7407 is fixed in a bent state. The secondary battery 7407 has a lead electrode electrically connected to a current collector. For example, the current collector is a copper foil, and a part of the current collector is alloyed with gallium to improve adhesion with the active material layer in contact with the current collector, so that the secondary battery 7407 has a high reliability when bent.

[0364] FIG. 17D shows an example of a bangle-type display device. The portable display device 7100 includes a housing 7101, a display unit 7102, an operation button 7103, and a secondary battery 7104. FIG. 17E shows a bent state of the secondary battery 7104. When the secondary battery 7104 is worn on a user's arm in a bent state, the housing is deformed, and the curvature of the secondary battery 7104 changes in part or in whole. Note that the degree of bending at any point of the curve expressed by the value of the radius of the corresponding circle is called the radius of curvature, and the reciprocal of the radius of curvature is called the curvature. Specifically, the housing or the main surface of the secondary battery 7104 changes in part or in whole when the radius of curvature is in the range of 40 mm to 150 mm. High reliability can be maintained if the radius of curvature of the main surface of the secondary battery 7104 is in the range of 40 mm to 150 mm. By using the secondary battery of one embodiment of the present invention as the secondary battery 7104, a lightweight portable display device with a long life can be provided.

[0365] 17F shows an example of a wristwatch-type portable information terminal. A portable information terminal 7200 includes a housing 7201, a display portion 7202, a band 7203, a buckle 7204, operation buttons 7205, an input / output terminal 7206, and the like.

[0366] The portable information terminal 7200 can execute various applications such as mobile telephone, e-mail, document browsing and creation, music playback, Internet communication, and computer games.

[0367] The display surface of the display portion 7202 is curved, and display can be performed along the curved display surface. The display portion 7202 is also provided with a touch sensor, and can be operated by touching the screen with a finger, a stylus, or the like. For example, an application can be started by touching an icon 7207 displayed on the display portion 7202.

[0368] The operation button 7205 can have various functions, such as time setting, power on / off operation, wireless communication on / off operation, silent mode activation / cancellation, power saving mode activation / cancellation, etc. For example, the function of the operation button 7205 can be freely set by an operating system built into the mobile information terminal 7200.

[0369] The mobile information terminal 7200 can also perform short-distance wireless communication according to a communication standard. For example, the mobile information terminal 7200 can communicate with a wireless headset to enable hands-free calling.

[0370] The portable information terminal 7200 also includes an input / output terminal 7206, and can directly exchange data with another information terminal via a connector. Charging can also be performed via the input / output terminal 7206. Note that charging may be performed by wireless power supply without using the input / output terminal 7206.

[0371] A display portion 7202 of a portable information terminal 7200 includes the secondary battery of one embodiment of the present invention. By using the secondary battery of one embodiment of the present invention, a portable information terminal that is lightweight and has a long life can be provided. For example, the secondary battery 7104 shown in FIG. 17E can be incorporated in a curved state inside a housing 7201 or in a bendable state inside a band 7203.

[0372] The portable information terminal 7200 preferably has a sensor. For example, it is preferable that a fingerprint sensor, a pulse sensor, a human body sensor such as a body temperature sensor, a touch sensor, a pressure sensor, an acceleration sensor, or the like is mounted as the sensor.

[0373] 17G illustrates an example of an armband-type display device. The display device 7300 includes a display portion 7304 and a secondary battery of one embodiment of the present invention. The display device 7300 can also include a touch sensor in the display portion 7304 and can function as a portable information terminal.

[0374] The display surface of the display portion 7304 is curved, and display can be performed along the curved display surface. In addition, the display device 7300 can change the display state by short-range wireless communication according to a communication standard.

[0375] The display device 7300 also includes an input / output terminal, and can directly exchange data with other information terminals via a connector. Charging can also be performed via the input / output terminal. Note that charging may be performed by wireless power supply without using the input / output terminal.

[0376] By using the secondary battery of one embodiment of the present invention as a secondary battery included in the display device 7300, a lightweight display device with a long lifetime can be provided.

[0377] In addition, an example in which the secondary battery having good cycle characteristics described in the above embodiment is mounted on an electronic device will be described with reference to FIGS.

[0378] By using the secondary battery of one embodiment of the present invention as a secondary battery in daily electronic devices, products that are lightweight and have a long life can be provided. For example, daily electronic devices include electric toothbrushes, electric shavers, and electric beauty devices. For the secondary battery of these products, a stick-shaped secondary battery that is small, lightweight, and has a large discharge capacity is desired in consideration of ease of holding by users.

[0379] FIG. 17(H) is a perspective view of a device also called a tobacco-receiving smoking device (electronic cigarette). In FIG. 17(H), the electronic cigarette 7500 is composed of an atomizer 7501 including a heating element, a secondary battery 7504 that supplies power to the atomizer, and a cartridge 7502 including a liquid supply bottle, a sensor, and the like. To enhance safety, a protection circuit that prevents overcharging and / or overdischarging of the secondary battery 7504 may be electrically connected to the secondary battery 7504. The secondary battery 7504 shown in FIG. 17(H) has an external terminal so that it can be connected to a charging device. Since the secondary battery 7504 is the tip part when held, it is desirable that the total length is short and the weight is light. Since the secondary battery of one embodiment of the present invention has a high discharge capacity and good cycle characteristics, a small and lightweight electronic cigarette 7500 that can be used for a long period of time can be provided.

[0380] Fig. 18(A) shows an example of a wearable device. The wearable device uses a secondary battery as a power source. In addition, when a user uses the device in daily life or outdoors, in order to improve splash-proof performance, water resistance, or dust resistance, there is a demand for a wearable device that can be charged wirelessly as well as by wire with an exposed connector.

[0381] For example, the secondary battery according to one embodiment of the present invention can be mounted on a glasses-type device 4000 as shown in FIG. 18A. The glasses-type device 4000 includes a frame 4000a and a display unit 4000b. By mounting a secondary battery on temples of the curved frame 4000a, the glasses-type device 4000 can be lightweight, well-balanced in weight, and has a long continuous use time. By providing the secondary battery according to one embodiment of the present invention, a configuration that can accommodate space saving associated with a smaller housing can be realized.

[0382] Furthermore, the secondary battery according to one embodiment of the present invention can be mounted on the headset type device 4001. The headset type device 4001 has at least a microphone unit 4001a, a flexible pipe 4001b, and an earphone unit 4001c. The secondary battery can be provided in the flexible pipe 4001b and / or the earphone unit 4001c. By providing the secondary battery according to one embodiment of the present invention, a configuration that can accommodate space saving associated with a miniaturized housing can be realized.

[0383] Furthermore, the secondary battery according to one embodiment of the present invention can be mounted on a device 4002 that can be directly attached to the body. A secondary battery 4002b can be provided in a thin housing 4002a of the device 4002. By providing the secondary battery according to one embodiment of the present invention, a configuration that can accommodate space saving due to miniaturization of the housing can be realized.

[0384] Furthermore, the secondary battery according to one embodiment of the present invention can be mounted on a device 4003 that can be attached to clothing. A secondary battery 4003b can be provided in a thin housing 4003a of the device 4003. By providing the secondary battery according to one embodiment of the present invention, a configuration that can accommodate space saving due to miniaturization of the housing can be realized.

[0385] Furthermore, the secondary battery according to one embodiment of the present invention can be mounted on the belt type device 4006. The belt type device 4006 has a belt portion 4006a and a wireless power receiving portion 4006b, and a secondary battery can be mounted inside the belt portion 4006a. By providing the secondary battery according to one embodiment of the present invention, a configuration that can accommodate space saving associated with miniaturization of the housing can be realized.

[0386] Furthermore, the secondary battery according to one embodiment of the present invention can be mounted on the wristwatch device 4005. The wristwatch device 4005 has a display portion 4005a and a belt portion 4005b, and the secondary battery can be provided on the display portion 4005a or the belt portion 4005b. By providing the secondary battery according to one embodiment of the present invention, a configuration that can accommodate space saving due to miniaturization of the housing can be realized.

[0387] The display unit 4005a can display not only the time, but also various other information such as incoming e-mails and phone calls.

[0388] In addition, since the wristwatch type device 4005 is a wearable device that is directly wrapped around the arm, it may be equipped with sensors that measure the user's pulse, blood pressure, etc. Data on the user's amount of exercise and health can be accumulated to manage the user's health.

[0389] FIG. 18B shows a perspective view of the wristwatch type device 4005 removed from the wrist.

[0390] 18C shows a side view of the display portion 4005. FIG. 18C shows a state in which a secondary battery 913 is built in the display portion 4005. The secondary battery 913 is the secondary battery described in Embodiment 2. The secondary battery 913 is provided at a position overlapping with the display portion 4005a, and is small and lightweight.

[0391] 18(D) shows an example of a wireless earphone. Here, the wireless earphone is illustrated having a pair of main bodies 4100a and 4100b, but this does not necessarily have to be a pair.

[0392] The main bodies 4100a and 4100b each have a driver unit 4101, an antenna 4102, and a secondary battery 4103. They may also have a display unit 4104. They also preferably have a substrate on which a circuit such as a wireless IC is mounted, a charging terminal, and the like. They may also have a microphone.

[0393] The case 4110 has a secondary battery 4111. It is preferable that the case 4110 also has a board on which circuits such as a wireless IC and a charge control IC are mounted, and a charging terminal. It may also have a display unit, buttons, and the like.

[0394] The main units 4100a and 4100b can wirelessly communicate with other electronic devices such as smartphones. This allows the main units 4100a and 4100b to play back audio data sent from other electronic devices. If the main units 4100a and 4100b have a microphone, the audio captured by the microphone can be sent to the other electronic device, and the audio data processed by the electronic device can be sent back to the main units 4100a and 4100b for playback. This allows the main units 4100a and 4100b to be used as a translator, for example.

[0395] In addition, the secondary battery 4103 in the main body 4100a can be charged from the secondary battery 4111 in the case 4110. The coin-type secondary battery, the cylindrical secondary battery, or the like described in the previous embodiments can be used as the secondary battery 4111 and the secondary battery 4103. A secondary battery using the positive electrode active material 100 obtained in Embodiment 1 as a positive electrode has a high energy density, and by using the secondary battery 4103 and the secondary battery 4111, a configuration that can accommodate space saving associated with miniaturization of wireless earphones can be realized.

[0396] 19A shows an example of a cleaning robot. The cleaning robot 6300 has a display unit 6302 arranged on the top surface of a housing 6301, a plurality of cameras 6303 arranged on the side surface, a brush 6304, an operation button 6305, a secondary battery 6306, various sensors, and the like. Although not shown, the cleaning robot 6300 is provided with tires, a suction port, and the like. The cleaning robot 6300 can move by itself, detect dust 6310, and suck up the dust from a suction port arranged on the bottom surface.

[0397] For example, the cleaning robot 6300 can analyze an image captured by the camera 6303 and determine the presence or absence of an obstacle such as a wall, furniture, or a step. When an object that may become entangled in the brush 6304, such as a wire, is detected by image analysis, the rotation of the brush 6304 can be stopped. The cleaning robot 6300 includes a secondary battery 6306 according to one embodiment of the present invention and a semiconductor device or electronic component therein. By using the secondary battery 6306 according to one embodiment of the present invention in the cleaning robot 6300, the cleaning robot 6300 can be an electronic device with long operating time and high reliability.

[0398] Fig. 19(B) shows an example of a robot. The robot 6400 shown in Fig. 19(B) includes a secondary battery 6409, an illuminance sensor 6401, a microphone 6402, an upper camera 6403, a speaker 6404, a display unit 6405, a lower camera 6406, an obstacle sensor 6407, a moving mechanism 6408, a computing device, and the like.

[0399] The microphone 6402 has a function of detecting the user's voice, environmental sounds, etc. The speaker 6404 has a function of emitting sound. The robot 6400 can communicate with the user using the microphone 6402 and the speaker 6404.

[0400] The display unit 6405 has a function of displaying various information. The robot 6400 can display information desired by the user on the display unit 6405. The display unit 6405 may be equipped with a touch panel. The display unit 6405 may also be a removable information terminal, and by installing it in a fixed position on the robot 6400, charging and data transfer are possible.

[0401] The upper camera 6403 and the lower camera 6406 have a function of capturing images of the surroundings of the robot 6400. In addition, the obstacle sensor 6407 can detect the presence or absence of an obstacle in the moving direction when the robot 6400 moves forward using the moving mechanism 6408. The robot 6400 can recognize the surrounding environment and move safely using the upper camera 6403, the lower camera 6406, and the obstacle sensor 6407.

[0402] The robot 6400 includes a secondary battery 6409 according to one embodiment of the present invention and a semiconductor device or an electronic component inside the robot 6400. By using the secondary battery according to one embodiment of the present invention in the robot 6400, the robot 6400 can be a highly reliable electronic device with a long operating time.

[0403] Fig. 19C shows an example of an aircraft. An aircraft 6500 shown in Fig. 19C includes a propeller 6501, a camera 6502, a secondary battery 6503, and the like, and has a function of flying autonomously.

[0404] For example, image data captured by the camera 6502 is stored in the electronic component 6504. The electronic component 6504 can analyze the image data and detect the presence or absence of an obstacle when moving. The electronic component 6504 can estimate the remaining battery charge from a change in the power storage capacity of the secondary battery 6503. The flying object 6500 includes therein the secondary battery 6503 according to one embodiment of the present invention. By using the secondary battery according to one embodiment of the present invention in the flying object 6500, the flying object 6500 can be an electronic device with a long operating time and high reliability.

[0405] This embodiment mode can be implemented in appropriate combination with other embodiment modes.

[0406] (Embodiment 4) In this embodiment, an example is described in which a secondary battery including the positive electrode active material of one embodiment of the present invention is mounted on a vehicle.

[0407] By installing secondary batteries in vehicles, next-generation clean energy vehicles such as hybrid vehicles (HVs), electric vehicles (EVs), and plug-in hybrid vehicles (PHVs) can be realized.

[0408] FIG. 20 illustrates an example of a vehicle using a secondary battery according to one embodiment of the present invention. An automobile 8400 illustrated in FIG. 20A is an electric automobile using an electric motor as a power source for running. Alternatively, the automobile 8400 is a hybrid automobile that can use an electric motor and an engine as a power source for running. By using one embodiment of the present invention, a vehicle with a long cruising distance can be realized. In addition, the automobile 8400 has a secondary battery. For example, secondary battery modules can be arranged on the floor of the vehicle. The secondary battery can not only drive the electric motor 8406 but also supply power to light-emitting devices such as a headlight 8401 and a room light (not shown).

[0409] The secondary battery can also supply power to display devices such as a speedometer and a tachometer included in the automobile 8400. The secondary battery can also supply power to semiconductor devices such as a navigation system included in the automobile 8400.

[0410] The automobile 8500 shown in FIG. 20(B) can charge the secondary battery of the automobile 8500 by receiving power supply from an external charging facility by a plug-in method and / or a non-contact power supply method. FIG. 20(B) shows a state in which a secondary battery 8024 mounted on the automobile 8500 is being charged from a ground-mounted charging device 8021 via a cable 8022. When charging, the charging method and connector standards may be appropriately performed by a predetermined method such as CHAdeMO (registered trademark) or combo. The charging device 8021 may be a charging station installed in a commercial facility or a home power source. For example, the secondary battery 8024 mounted on the automobile 8500 can be charged by an external power supply using plug-in technology. Charging can be performed by converting AC power to DC power via a conversion device such as an ACDC converter.

[0411] Although not shown, a power receiving device may be mounted on a vehicle, and charging may be performed by supplying power contactlessly from a ground power transmitting device. In the case of this contactless power supply method, by incorporating a power transmitting device in the road and / or an exterior wall, charging may be performed not only while the vehicle is stopped but also while it is moving. This contactless power supply method may also be used to transmit and receive power between vehicles. Furthermore, a solar cell may be provided on the exterior of the vehicle, and a secondary battery may be charged while the vehicle is stopped and / or moving. For such contactless power supply, an electromagnetic induction method and / or a magnetic field resonance method may be used.

[0412] 20C is an example of a two-wheeled vehicle using the secondary battery of one embodiment of the present invention. A scooter 8600 shown in FIG. 20C includes a secondary battery 8602, a side mirror 8601, and a turn signal light 8603. The secondary battery 8602 can supply electricity to the turn signal light 8603.

[0413] 20(C) is capable of storing a secondary battery 8602 in the under-seat storage 8604. Even if the under-seat storage 8604 is small, the secondary battery 8602 can be stored in the under-seat storage 8604. The secondary battery 8602 is removable, and when charging, the secondary battery 8602 can be carried indoors, charged, and stored before riding.

[0414] According to one aspect of the present invention, the cycle characteristics of the secondary battery are improved, and the discharge capacity of the secondary battery can be increased. Therefore, the secondary battery itself can be made small and lightweight. If the secondary battery itself can be made small and lightweight, it contributes to reducing the weight of the vehicle, and the cruising distance can be improved. In addition, the secondary battery mounted on the vehicle can be used as a power supply source other than the vehicle. In this case, for example, it is possible to avoid using a commercial power source during peak power demand. If it is possible to avoid using a commercial power source during peak power demand, it is possible to contribute to energy conservation and reduction of carbon dioxide emissions. In addition, if the cycle characteristics are good, the secondary battery can be used for a long period of time, and the amount of rare metals used, including cobalt, can be reduced.

[0415] This embodiment mode can be implemented in appropriate combination with other embodiment modes. [Explanation of symbols]

[0416] 91 Nickel Source 92 Aluminum Source 98 Complex hydroxides 99 Complex oxides 100 Cathode active material 100a Surface layer 100b internal 100c Inner wall surface layer 106 Crack

Claims

1. A positive electrode active material having a layered rock salt type crystal structure belonging to the space group R-3m, The positive electrode active material includes lithium cobalt oxide, The lithium cobalt oxide has a crack portion, The lithium cobalt oxide has a surface layer portion and an inner wall surface layer portion including a surface of an inner wall of the crack portion, the surface layer portion comprises aluminum and nickel, The positive electrode active material, wherein the inner wall surface portion comprises aluminum.

2. In claim 1, The positive electrode active material, wherein the inner wall surface portion is substantially free of nickel.

3. A positive electrode active material having a layered rock salt type crystal structure belonging to the space group R-3m, The positive electrode active material comprises lithium cobalt-nickel oxide, The cobalt-nickel lithium oxide has a crack portion, The lithium cobalt-nickel oxide has a surface layer portion and an inner wall surface layer portion including a surface of an inner wall of the crack portion, the surface layer portion includes aluminum and titanium, The positive electrode active material, wherein the inner wall surface portion comprises aluminum.

4. In claim 3, The positive electrode active material, wherein the inner wall surface portion is substantially free of titanium.

5. A positive electrode active material having a layered rock salt type crystal structure belonging to the space group R-3m, The positive electrode active material comprises lithium nickel-cobalt-manganese oxide, The nickel-cobalt-manganese lithium oxide has a crack portion, The nickel-cobalt-manganese lithium oxide has a surface layer portion and an inner wall surface layer portion including a surface of an inner wall of the crack portion, the surface layer portion includes aluminum and titanium, The positive electrode active material, wherein the inner wall surface portion comprises aluminum.

6. In claim 5, The positive electrode active material, wherein the inner wall surface portion is substantially free of titanium.

7. A first step of mixing a composite oxide having a layered rock salt type crystal structure belonging to the space group R-3m, a solid material, and a liquid material to prepare a mixture; a second step of heating the mixture; the solid material comprises nickel; The method for producing a positive electrode active material, wherein the liquid material contains aluminum.

8. In claim 7, the solid material comprises one of nickel oxide and nickel hydroxide; The method for producing a positive electrode active material, wherein the liquid material comprises any one of an aluminum alkoxide solution, an aluminum acetylacetonate solution, an aluminum lactate solution, and an aluminum phthalocyanine solution.

9. A first step of mixing a composite oxide having a layered rock salt type crystal structure belonging to the space group R-3m, a solid material, and a liquid material to prepare a mixture; a second step of heating the mixture; the solid material comprises titanium; The method for producing a positive electrode active material, wherein the liquid material contains aluminum.

10. In claim 9, the solid material comprises one of lithium titanate, titanium oxide, and titanium hydroxide; The method for producing a positive electrode active material, wherein the liquid material has any one of an aluminum alkoxide solution, an aluminum acetylacetonate solution, an aluminum lactate solution, and an aluminum phthalocyanine solution.

11. A first step of mixing a composite oxide having a layered rock salt type crystal structure belonging to the space group R-3m, a first solid material, a second solid material, and a liquid material to prepare a mixture; a second step of heating the mixture; the first solid material comprises nickel; the second solid material comprises titanium; The method for producing a positive electrode active material, wherein the liquid material contains aluminum.

12. In claim 11, the first solid material comprises one of nickel oxide and nickel hydroxide; the second solid material comprises one of lithium titanate, titanium oxide, and titanium hydroxide; The method for producing a positive electrode active material, wherein the liquid material has any one of an aluminum alkoxide solution, an aluminum acetylacetonate solution, an aluminum lactate solution, and an aluminum phthalocyanine solution.

13. In any one of claims 7 to 10, The method for producing a positive electrode active material, wherein the particle size of the solid material is such that D50 (median diameter) obtained by particle size distribution measurement is 1 μm or more and 5 μm or less.

14. In claims 11 and 12, The particle size of the first solid material is such that D50 (median diameter) obtained by particle size distribution measurement is 1 μm or more and 5 μm or less, The method for producing a positive electrode active material, wherein the particle size of the second solid material has a D50 (median diameter) obtained by particle size distribution measurement of 1 μm or more and 5 μm or less.

Citation Information

Patent Citations

  • Positive electrode active material and secondary battery

    WO2020128699A1

  • Method for manufacturing electrode

    WO2022172118A1